Membrane electrolysis method for aqueous lithium salt solution

JP2024151485A5Active Publication Date: 2024-11-08ASAKA RIKEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023064855
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-11-08
Estimated Expiration
2043-04-12

AI Technical Summary

Benefits of technology

【0009】 本発明は、高い効率を示す膜電解工程を含み、水酸化リチウムが電解膜中及び表面に発生し難い、リチウム塩水溶液の膜電解方法を提供する。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a method for recovering lithium from an aqueous lithium salt solution, the method including a membrane electrolysis step with high efficiency, making lithium hydroxide less likely to form in and on the electrolytic membrane.SOLUTION: This membrane electrolysis method for an aqueous lithium salt solution includes: a negative electrode chamber charging step for charging at least one selected from the group consisting of a first aqueous lithium hydroxide solution having a lithium hydroxide concentration of 10 mass% or less and water into a negative electrode chamber of a membrane electrolysis apparatus; and a membrane electrolysis step for performing membrane electrolysis until the lithium hydroxide concentration in the negative electrode chamber reaches a predetermined concentration. The negative electrode chamber charging step and the membrane electrolysis step are preferably repeated sequentially.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for membrane electrolysis of an aqueous lithium salt solution. [Background technology]

[0002] 2. Description of the Related Art In recent years, with the widespread use of lithium ion batteries, methods have been considered for recovering valuable metals such as cobalt, nickel, manganese, and lithium from discarded lithium ion batteries and reusing them as materials for the lithium ion batteries.

[0003] Cited Document 1 discloses a system for recovering lithium from waste lithium-ion batteries, the system including the steps of: dissolving active material powder obtained by pretreating waste lithium-ion batteries in a mineral acid to obtain an acid solution of the active material containing at least lithium; separating at least one metal other than lithium from the acid solution to which lithium hydroxide has been added by solvent extraction to obtain a first aqueous lithium salt solution as a residual solution of the solvent extraction; and performing membrane electrolysis of the first aqueous lithium salt solution using an ion exchange membrane to obtain an aqueous lithium hydroxide solution, an acid, and a second aqueous lithium salt solution that is more dilute than the first aqueous lithium salt solution. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7060899 Summary of the Invention [Problem to be solved by the invention]

[0005] In the membrane electrolysis of lithium hydroxide aqueous solution, the higher the lithium hydroxide concentration in the catholyte in the cathode chamber of the membrane electrolysis device, the easier it is for hydroxide ions to migrate to the anode chamber, and the lower the membrane electrolysis efficiency. Furthermore, lithium hydroxide is easily precipitated in and on the electrolytic membrane. An electrolytic membrane with lithium hydroxide precipitated thereon is damaged, causing various adverse effects on the membrane electrolysis.

[0006] Therefore, an object of the present invention is to provide a method for membrane electrolysis of an aqueous lithium salt solution, which includes a highly efficient membrane electrolysis step and is less likely to produce lithium hydroxide in or on the surface of the electrolytic membrane. [Means for solving the problem]

[0007] The present inventors have conducted extensive research in light of the above problems and have found that a method for membrane electrolysis of an aqueous lithium salt solution, which includes a cathode chamber introduction step of introducing at least one selected from the group consisting of a first aqueous lithium hydroxide solution having a lithium hydroxide concentration of 10 mass % or less and water into a cathode chamber of a membrane electrolysis device, exhibits high efficiency and is unlikely to generate lithium hydroxide in or on the surface of the electrolytic membrane. The present invention has been completed based on these findings.

[0008] The present invention relates to a membrane electrolysis method for an aqueous lithium salt solution, comprising: a cathode chamber introducing step of introducing at least one selected from the group consisting of a first aqueous lithium hydroxide solution having a lithium hydroxide concentration of 10 mass% or less and water into a cathode chamber of a membrane electrolysis device; and a membrane electrolysis step of carrying out membrane electrolysis until the lithium hydroxide concentration in the cathode chamber reaches a predetermined concentration. The cathode chamber charging step and the membrane electrolysis step are preferably repeated in sequence. A portion of the second lithium hydroxide aqueous solution obtained in the membrane electrolysis step is preferably diluted with water to form the first lithium hydroxide aqueous solution. The present invention preferably further includes an acid dissolution step of dissolving an active material powder obtained by pretreating waste lithium-ion batteries in a mineral acid to obtain an acid solution of the active material containing at least lithium, a neutralization step of neutralizing the acid solution by adding lithium hydroxide to the acid solution to obtain a neutralized solution, and a solvent extraction step of separating at least one metal, excluding lithium, among the metals contained in the active material powder from the neutralized solution by solvent extraction, and obtaining an aqueous lithium salt solution as a residual solution of the solvent extraction. A portion of the second lithium hydroxide aqueous solution obtained in the membrane electrolysis step is utilized in at least one selected from the group consisting of the neutralization step and the solvent extraction step, and the mineral acid obtained in the membrane electrolysis step is utilized in the acid dissolution step. The electricity used for the membrane electrolysis preferably includes electricity obtained from renewable energy. The electric power obtained by the renewable energy preferably includes at least one selected from the group consisting of electric power obtained by solar power generation and electric power obtained by wind power generation. Effect of the Invention

[0009] The present invention provides a method for membrane electrolysis of an aqueous lithium salt solution, which includes a highly efficient membrane electrolysis step and is less likely to produce lithium hydroxide in or on the surface of the electrolytic membrane. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is an explanatory diagram showing a method for recovering lithium from an aqueous lithium salt solution according to the present invention. [Diagram 2] FIG. 1 is an explanatory cross-sectional view showing one embodiment of the structure of an ion exchange membrane electrolytic cell used in the method of recovering lithium from an aqueous lithium salt solution of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will now be described in further detail. In addition, unless otherwise specified, "~" in a numerical range means from above to below, and both ends of the range are included. In addition, when a numerical range is indicated, the upper limit and the lower limit can be appropriately combined, and the numerical range obtained by combining them is also disclosed. In addition, in the description of the drawings, the same elements are denoted by the same reference numerals, and duplicated description will be omitted. Also, the dimensional ratios of the drawings are exaggerated for the convenience of explanation, and may differ from the actual ratios.

[0012] The membrane electrolysis method for a lithium salt aqueous solution of the present invention may start with an aqueous solution in which a lithium salt is dissolved. The aqueous solution is not limited to a specific aqueous solution. Examples of the aqueous solution include seawater, brackish water, and / or salt lake-derived brine, and aqueous solutions in which minerals are dissolved. Furthermore, in the method for membrane electrolysis of an aqueous lithium salt solution of the present invention, as shown in FIG. 1, active material powder 1 may be used as a starting material.

[0013] When the waste lithium ion battery is a used lithium ion battery whose life as a battery product has expired, or a lithium ion battery discarded as a defective product in the manufacturing process, the active material powder 1 can be obtained by first discharging the battery in salt water to discharge all remaining charges, then forming an opening in the casing of the waste lithium ion battery, for example, heat treating (roasting) the battery at a temperature in the range of 100 to 800° C., or pulverizing the battery with a pulverizer such as a hammer mill or a jaw crusher without heat treating, and removing the casing, current collector, etc. constituting the waste lithium ion battery by sieving (classifying). Alternatively, the waste lithium ion battery after the discharge treatment may be pulverized with the pulverizer, and the casing, current collector, etc. may be removed by sieving, and the active material powder 1 may be obtained by heat treating the battery at a temperature in the range, or without heat treating the battery.

[0014] When the waste lithium ion batteries are residual positive electrode materials or the like used in commercialization in a manufacturing process, they may be pulverized in the pulverizer after being heat-treated at a temperature in the above range or without being heat-treated without performing the discharge treatment and the formation of openings, and the current collectors and the like may be removed by sieving to obtain the active material powder 1. Furthermore, the waste lithium ion batteries may be pulverized in the pulverizer, the current collectors and the like may be removed by sieving, and then the active material powder 1 may be obtained by being heat-treated at a temperature in the above range or without being heat-treated.

[0015] The membrane electrolysis method of the present invention preferably includes an acid dissolution step of dissolving the active material powder 1 obtained by pretreating the waste lithium ion battery in STEP 1 in a mineral acid to obtain an acid solution of the active material powder 1 containing at least lithium. The mineral acid includes at least one selected from the group consisting of hydrochloric acid, sulfuric acid, and nitric acid, and preferably includes hydrochloric acid, and more preferably is hydrochloric acid. In addition to lithium, the active material powder 1 includes valuable metals such as iron, aluminum, manganese, cobalt, and nickel.

[0016] The membrane electrolysis method of the present invention preferably includes a neutralization step in STEP 2 in which lithium hydroxide (LiOH) is added to the acid solution to neutralize the acid solution and obtain a neutralized solution. Furthermore, the membrane electrolysis method of the present invention preferably includes a solvent extraction step (STEP 3) in which at least one metal, excluding lithium, among the metals contained in the active material powder is separated from the neutralization solution by solvent extraction, and a lithium salt aqueous solution is obtained as a residual solution of the solvent extraction. In the solvent extraction, manganese, cobalt, and nickel, excluding lithium, among the valuable metals, are each solvent extracted, or iron and aluminum are separated and removed as the respective metal salt aqueous solutions 2, to obtain a first lithium salt aqueous solution. The lithium salt contained in the first lithium salt aqueous solution becomes lithium chloride when hydrochloric acid is used in the acid dissolution in STEP 1.

[0017] The membrane electrolysis method for a lithium salt aqueous solution of the present invention includes a cathode chamber introduction step (STEP 4-1) of introducing at least one selected from the group consisting of a first lithium hydroxide aqueous solution having a lithium hydroxide concentration of 10 mass% or less and water into a cathode chamber of a membrane electrolysis device, and a membrane electrolysis step (STEP 4-2) of carrying out membrane electrolysis until the lithium hydroxide concentration in the cathode chamber reaches a predetermined concentration. In FIG. 1, STEP 4-1 and STEP 4-2 are shown as STEP 4. The cathode chamber introduction step and the membrane electrolysis step can be carried out, for example, using an electrolytic cell 11 shown in FIG. 2. The water may include at least one selected from the group consisting of industrial water, pure water, and tap water.

[0018] The electrolytic cell 11 is equipped with an anode plate 12 on one of its inner surfaces and a cathode plate 13 on the inner surface opposite the anode plate 12, the anode plate 12 being connected to an anode 14 of a power supply, and the cathode plate 13 being connected to a cathode 15 of the power supply. The electrolytic cell 11 is also partitioned by an ion exchange membrane 16 into an anode chamber 17 equipped with the anode plate 12 and a cathode chamber 18 equipped with the cathode plate 13.

[0019] In the electrolytic cell 11, when electrolysis is performed by supplying, for example, lithium chloride as the first lithium salt aqueous solution to the anode chamber 17, chloride ions generate chlorine gas (Cl2) on the anode plate 12, while lithium ions move to the cathode chamber 18 through the ion exchange membrane 16.

[0020] In the cathode chamber 18, water (HO) is converted into hydroxide ions (OH - ) and hydrogen ions (H + ), and the hydrogen ions generate hydrogen gas (H2) on the cathode plate 13, while the hydroxide ions combine with lithium to generate the second lithium hydroxide aqueous solution 3. As the lithium hydroxide concentration in the second lithium hydroxide aqueous solution 3 increases, the hydroxide ions tend to move toward the anode chamber 17, and the membrane electrolysis efficiency decreases. Furthermore, lithium hydroxide tends to deposit in and on the ion exchange membrane 16. When lithium hydroxide deposits, the ion exchange membrane 16 is damaged, and various adverse effects occur in the membrane electrolysis process. Therefore, at least one selected from the group consisting of the first lithium hydroxide aqueous solution having a lithium hydroxide concentration of 10 mass% or less and water is introduced into the cathode chamber 18 at a flow rate sufficient to prevent a difference in lithium hydroxide concentration at the inlet and outlet of the cathode chamber 18. As a result, the lithium ions that have moved from the anode chamber 17 are diffused more quickly from the surface of the ion exchange membrane 16 on the cathode chamber 18 side, and lithium hydroxide does not deposit in and on the ion exchange membrane 16. The cathode chamber charging step and the membrane electrolysis step may be repeated in sequence or simultaneously. The cathode chamber charging step and the membrane electrolysis step are preferably repeated in sequence. In a typical ion exchange membrane electrolysis method for salt, the saline solution to be subjected to membrane electrolysis is continuously fed into an electrolysis chamber, and the sodium hydroxide concentration at the inlet of the electrolysis chamber is about 28 mass%, but the concentration at the outlet rises to 32 to 35 mass%.

[0021] When the lithium salt aqueous solution subjected to the membrane electrolysis process contains sulfate ions, sulfuric acid can be obtained in the anode chamber 17. When the lithium salt aqueous solution subjected to the membrane electrolysis process contains nitrate ions, nitric acid can be obtained in the anode chamber 17. That is, mineral acid 4 can be obtained in the membrane electrolysis process, and the mineral acid 4 can be used to dissolve the active material powder 1 in STEP 1.

[0022] The second lithium hydroxide aqueous solution 3 obtained in the membrane electrolysis step can be recovered as lithium hydroxide monohydrate (LiOH·H2O) by crystallization in STEP 8, or can be recovered as lithium carbonate (Li2CO3) by carbonation in STEP 9. The carbonation can be performed by reacting the second lithium hydroxide aqueous solution 3 with carbon dioxide gas (CO2).

[0023] In this embodiment, a part of the second lithium hydroxide aqueous solution 3 obtained in the membrane electrolysis step may be diluted with water to obtain the first lithium hydroxide aqueous solution. Furthermore, a part of the second lithium hydroxide aqueous solution 3 may be used as at least one selected from the group consisting of the lithium hydroxide added to the acid dissolution solution in STEP 2 and the alkali used for solvent extraction in STEP 3.

[0024] When the second lithium hydroxide aqueous solution 3 is used for solvent extraction in STEP 3, the second lithium hydroxide aqueous solution 3 is added to the extraction solvent. Since the extraction solvent used for solvent extraction in STEP 3 is a cation exchange extractant, if it is used continuously, the liquid tends to become acidic and the extraction rate decreases, but by adding the second lithium hydroxide aqueous solution 3, the decrease in the extraction rate can be suppressed.

[0025] When the second lithium hydroxide aqueous solution 3 is used for solvent extraction in STEP 3, the second lithium hydroxide aqueous solution 3 can be used for at least one of the solvent extractions of manganese, cobalt, and nickel, which are performed separately.

[0026] The electricity used in the membrane electrolysis step may include, for example, at least one renewable energy selected from the group consisting of electricity obtained by solar power generation and electricity obtained by wind power generation. EXAMPLES

[0027] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0028] [Example 1] 2, membrane electrolysis was carried out until the lithium hydroxide concentration of the lithium hydroxide aqueous solution in the cathode chamber 18 changed from 2% by mass to 8% by mass. The current efficiency was 67%.

[0029] [Example 2] Membrane electrolysis was carried out in the same manner as in Example 1, except that the lithium hydroxide concentration of the lithium hydroxide aqueous solution in the cathode chamber 18 was kept constant at 5 mass %. The current efficiency was 64%.

[0030] [Example 3] Membrane electrolysis was carried out in the same manner as in Example 1, except that the lithium hydroxide concentration of the lithium hydroxide aqueous solution in the cathode chamber 18 was kept constant at 8 mass %. The current efficiency was 53%. [Explanation of symbols]

[0031] 1...active material powder, 2...metal salt aqueous solution, 3...lithium hydroxide aqueous solution, 4...mineral acid, 11...membrane electrolytic cell, 16...ion exchange membrane, 17...anode chamber, 18...cathode chamber.

Claims

1. A method for membrane electrolysis of an aqueous lithium salt solution, comprising the steps of: A cathode chamber introduction step of introducing at least one selected from the group consisting of a first lithium hydroxide aqueous solution having a lithium hydroxide concentration of 10 mass% or less and water into a cathode chamber of a membrane electrolysis device; A method for membrane electrolysis of an aqueous lithium salt solution, comprising: a membrane electrolysis step of performing membrane electrolysis until the concentration of lithium hydroxide in the cathode chamber exceeds the concentration of lithium hydroxide in a first aqueous lithium hydroxide solution.

2. The method for membrane electrolysis of a lithium salt aqueous solution according to claim 1, A method for membrane electrolysis of an aqueous lithium salt solution, comprising sequentially repeating the cathode chamber charging step and the membrane electrolysis step.

3. The method for membrane electrolysis of a lithium salt aqueous solution according to claim 1, a step of diluting a part of the second aqueous lithium hydroxide solution obtained in the membrane electrolysis step with water to obtain the first aqueous lithium hydroxide solution.

4. The method for membrane electrolysis of a lithium salt aqueous solution according to claim 1, an acid dissolution step of dissolving the active material powder obtained by pretreating the waste lithium ion batteries in a mineral acid to obtain an acid solution of the active material containing at least lithium; A neutralization step of adding lithium hydroxide to the acid solution to neutralize the acid solution and obtain a neutralized solution; and The method for membrane electrolysis of an aqueous lithium salt solution further comprises a solvent extraction step of separating at least one metal, excluding lithium, from the neutralized solution by solvent extraction, among the metals contained in the active material powder, and obtaining an aqueous lithium salt solution as a residual liquid of the solvent extraction.

5. The method for membrane electrolysis of a lithium salt aqueous solution according to claim 4, a part of the second lithium hydroxide aqueous solution obtained in the membrane electrolysis step is utilized in at least one step selected from the group consisting of the neutralization step and the solvent extraction step, and a mineral acid obtained in the membrane electrolysis step is utilized in the acid dissolution step.

6. A method for membrane electrolysis of a lithium salt aqueous solution according to any one of claims 1 to 5, comprising: A method for membrane electrolysis of an aqueous lithium salt solution, characterized in that the electricity used for the membrane electrolysis includes electricity obtained from renewable energy.

7. 7. The method for membrane electrolysis of a lithium salt aqueous solution according to claim 6, 13. The method for membrane electrolysis of a lithium salt aqueous solution, wherein the electricity obtained from the renewable energy source includes at least one selected from the group consisting of electricity obtained by solar power generation and electricity obtained by wind power generation.