Seal member and vehicular suspension
A sealing member with porous carbon ceramic particles exceeding 40.0% by mass and a particle size of 150 μm or less effectively reduces friction, improving ride comfort and steering stability in vehicle suspensions.
Patent Information
- Application Number
- JP2023065451
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing sealing members made of rubber compositions containing porous carbon ceramic particles fail to achieve sufficient reduction in friction, necessitating further friction reduction for improved ride comfort and maneuverability.
A sealing member composed of a rubber composition with porous carbon ceramic particles exceeding 40.0% by mass, preferably with a particle size of 150 μm or less, and more preferably 10 μm, is used to reduce friction.
The sealing member achieves a significant reduction in friction, enhancing ride comfort and steering stability by smoothing the relative movement of vehicle suspension components.
Smart Images

Figure 2024151766000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a seal member made of a rubber composition and a vehicle suspension provided with the seal member. [Background technology]
[0002] Seal members made of rubber compositions are widely used in practice, and among them, a seal member made of a rubber composition containing a porous carbon ceramic is known (see, for example, Patent Document 1).
[0003] The sealing member disclosed in Patent Document 1 has a sliding surface with another member, and at least the sliding surface contains porous carbon ceramic particles having a Vickers hardness Hv of 400 or more in a proportion of 3 mass % or more and 40 mass % or less (Claim 1).
[0004] By setting the proportion of porous carbon ceramic to 40 mass % or less, it is possible to obtain the effect of preventing the seal member from decreasing in physical properties such as tensile strength and elongation, and preventing the seal member from becoming hard and brittle (Patent Document 1, paragraph 0034).
[0005] Also, a graph with the seal torque on the vertical axis is presented (Patent Document 1, Figure 2). According to this graph, the height of the center bar is about 25% lower than the height of the left bar, and the addition of 50 μm porous carbon ceramic particles achieves a friction reduction of about 25% compared to no additive.
[0006] However, there are a wide variety of requirements for sealing members, and for some requirements, the reduction in friction coefficient achieved by the technique of Patent Document 1 is insufficient, and further reduction in friction is required. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6519789 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a sealing member made of a rubber composition that can achieve even lower friction. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides a sealing member made of a rubber composition containing particles of a porous carbon ceramic material in a proportion of more than 40.0 mass %. Preferably, the particles have a diameter of 150 μm or less, and more preferably, the particles have a diameter of 10 μm or less. Effect of the Invention
[0010] According to the present invention, it is possible to achieve even lower friction of the seal member. [Brief description of the drawings]
[0011] [Figure 1] 1A to 1C are diagrams illustrating the structure of a vehicle suspension provided with an oil seal and a dust seal made of a sealing member according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will now be described with reference to the accompanying drawings. EXAMPLES
[0013] 1, the vehicle suspension 10 is, for example, a front suspension for a motorcycle. The vehicle suspension 10 is a shock absorber in which an inner tube 12 on the axle side is slidably inserted into an outer tube 11 on the vehicle body side, a spring 13 is provided inside the outer tube 11 and the inner tube 12, a damper 14 is housed, and oil and gas are sealed inside.
[0014] In this example, a dust seal 16 is attached to the lower end of the outer tube 11 , and an oil seal 17 is attached to the lower part of the outer tube 11 at a position above the dust seal 16 . The oil seal 17 slides against the inner tube 12 and seals in oil and gas.
[0015] The dust seal 16 slides against the inner tube 12 and prevents external dust, muddy water, and mud from entering the gap between the outer tube 11 and the inner tube 12 , thereby protecting the oil seal 17 .
[0016] The dust seal 16 and the oil seal 17 are collectively referred to as a seal member 18. However, the seal member 18 is not limited to the dust seal 16 and the oil seal 17, as the seal member 18 may include a sealing part such as an O-ring.
[0017] During running, the outer tube 11 moves axially relative to the inner tube 12. The relative movement includes all of the following: the outer tube 11 moves axially relative to the inner tube 12, the inner tube 12 moves axially relative to the outer tube 11, and both the outer tube 11 and the inner tube 12 move axially.
[0018] The vehicle body is supported by the wheels that come into contact with the road surface via a vehicle suspension 10. During driving, the vehicle body can move up and down, as well as forward and backward and left and right. These movements are closely related to the ride comfort and maneuverability. It is known that the smaller the friction coefficient of the seal member 18, the better the ride comfort and maneuverability. Therefore, there is a demand for the seal member 18 to have even lower friction.
[0019] Although the technology of the above-mentioned Patent Document 1 can reduce friction by about 25%, the present inventors have made various attempts to achieve even lower friction. These attempts are listed below.
[0020] Measurement principle of friction coefficient: A stage that reciprocates over a specified stroke is prepared. Also prepared are a weight with a metal ball attached to its bottom and a load cell that measures the horizontal force applied to the weight. A sample is fixed to the stage, a weight is placed on the sample via a metal ball, and a few drops of lubricant are placed between the sample and the metal ball. In this state, the stage is moved back and forth, and the horizontal force is measured with a load cell. The dynamic friction coefficient (hereinafter referred to as the friction coefficient) is calculated based on the mass of the weight and the horizontal force.
[0021] Friction coefficient measurement conditions: The conditions for measuring the friction coefficient are as follows: Stage travel distance (travel stroke): 2.5mm to the left and 2.5mm to the right of the center, for a total of 5.0mm. ·Moving speed: 1mm / sec Load (mass of weight): 19.6N Number of round trips: 100
[0022] ○Hardness measurement method: In accordance with JIS K 6253-2 (International Rubber Hardness Test), a plunger is pressed against the sample with a constant force, and the depth of the indentation made in the sample is converted to obtain the International Rubber Hardness (IRHD).
[0023] ○ Sample preparation for Comparative Example 1: A sample was produced by blending 36.5% by mass of NBR (manufactured by JSR Corporation, product name N240S), 47.5% by mass of silica (manufactured by Tosoh Silica Corporation, product name Nipsil (registered trademark) ER-R), 1.8% by mass of carbon black (manufactured by Tokai Carbon Corporation, product name Seast SO), and 14.2% by mass of other additives. Since the manufacturer's name and product name are the same below, their description will be omitted.
[0024] Friction coefficient and hardness of Comparative Example 1: The friction coefficient and international rubber hardness were measured for the sample of Comparative Example 1. The results are shown in Table 1.
[0025] [Table 1]
[0026] Example: It is known that porous carbon ceramic materials such as RHSC (porous carbon material made by burning rice husks) have the sliding properties derived from carbon and the reinforcing properties due to the cell structure. Therefore, the inventors decided to prepare the samples of the embodiment by replacing a part of NBR and a part of silica with the porous carbon ceramic material.
[0027] Preparation of sample for Example 1: A sample was manufactured by adding and blending 20.1 mass% of NBR, 26.1 mass% of silica, 1.0 mass% of carbon black, and 7.8 mass% of other additives with 45.0 mass% of a porous carbon ceramic material (manufactured by Sanwa Yushi Co., Ltd., product name RHSC) having a particle size of 106 μm. Hereinafter, the manufacturer name and product name of the porous carbon ceramic material are the same, so these will be omitted.
[0028] The porous carbon ceramic may be RBC (RB ceramics) derived from rice bran, and is not limited to RHSC, but may be any product equivalent to RHSC.
[0029] Friction coefficient and hardness of Example 1: The friction coefficient and international rubber hardness were measured for the sample of Example 1. The results are shown in Table 2. For comparison, Comparative Example 1 is also shown.
[0030] [Table 2]
[0031] Focusing on the friction coefficient in Table 2, the reduction rate of Example 1 relative to Comparative Example 1 was calculated. The results are shown in Table 3.
[0032] [Table 3]
[0033] In Example 1, a reduction rate of 45% was obtained. The reduction rate in the conventional technology (Patent Document 1) is about 25%, while the reduction rate in Example 1 is 45%. By calculating 45%÷25%=1.8, Example 1 achieved a reduction rate 1.8 times that of the conventional technology (Patent Document 1).
[0034] That is, the sealing member of the present invention, which contains 45.0 mass % of RHSC having a particle size of 106 μm, achieved a preferable reduction in friction.
[0035] Next, the inventors attempted to change the particle size of RHSC in order to further reduce friction, and this example will be described below as Example 2.
[0036] Preparation of sample for Example 2: The particle size of the porous carbon ceramic material (RHSC) was changed to 10 μm. Other than that, the sample was manufactured in the same manner as in Example 1.
[0037] Friction coefficient and hardness of Example 2: The friction coefficient and international rubber hardness were measured for the sample of Example 2. The results are shown in Table 4. For comparison, Example 1 is also shown.
[0038] [Table 4]
[0039] Focusing on the friction coefficient in Table 4, the reduction rate of Example 2 relative to Comparative Example 1 was calculated. The results are shown in Table 5.
[0040] [Table 5]
[0041] In Example 2, a reduction rate of 58% was obtained. The reduction rate in the conventional technology (Patent Document 1) is about 25%, while the reduction rate in Example 2 is 58%. By calculating 58%÷25%=2.3, Example 2 achieved a reduction rate 2.3 times that of the conventional technology (Patent Document 1).
[0042] That is, the sealing member of the present invention, which contains 45 mass % RHSC having a particle size of 10 μm, achieved a more preferable reduction in friction.
[0043] Incidentally, as shown in Table 1, the hardness (IRHD) of Comparative Example 1 is 87, and as shown in Table 4, the hardness (IRHD) of Examples 1 and 2 is 97. Depending on the application of the sealing member, it may be preferable to reduce the hardness (IRHD) to less than that of Examples 1 and 2.
[0044] The inventors have found that since silica is harder than the porous carbon ceramic material (RHSC), the amount of silica should be reduced and the amount of porous carbon ceramic material (RHSC) should be increased. However, increasing the amount of porous carbon ceramic material (RHSC) increases the risk of aggregation. As a countermeasure, an appropriate amount of carbon black coupling agent with a dispersing effect is added. Based on the above findings, a sample of Example 3 was produced, which will be described in detail below.
[0045] Preparation of sample for Example 3: A sample was produced by mixing 24.8 mass% NBR, 8.4 mass% silica, 56.0 mass% porous carbon ceramic material (RHSC) having a particle size of 10 μm, 1.2 mass% carbon black, 9.4 mass% other additives, and 0.2 mass% carbon black coupling agent (manufactured by Sumitomo Chemical Co., Ltd., product name Sumilink (registered trademark) 200).
[0046] Friction coefficient and hardness of Example 3: The friction coefficient and international rubber hardness were measured for the sample of Example 3. The results are shown in Table 6. For comparison, Example 2 is also shown.
[0047] [Table 6]
[0048] In Example 3, the friction coefficient increased slightly, but the hardness decreased. Example 3 is compared with Comparative Example 1. The results are shown in Table 7.
[0049] [Table 7]
[0050] The hardness of Example 3 was the same as that of Comparative Example 1. Moreover, in Example 3, a reduction rate of 41% was obtained. The reduction rate in the conventional technology (Patent Document 1) is about 25%, while the reduction rate in Example 3 is 41%. By calculating 41%÷25%=1.6, Example 3 achieved a reduction rate 1.6 times that of the conventional technology (Patent Document 1).
[0051] In Example 3, although the porous carbon ceramic material (RHSC) was 56.0 mass%, by adding 0.2 mass% of carbon black coupling agent, the hardness was equivalent to that of Comparative Example 1, and the friction coefficient was reduced by 41% compared to Comparative Example 1.
[0052] From another perspective, in Example 3, by reducing the amount of silica, the compounding ratio of the porous carbon ceramic material (RHSC) was increased to 56.0 mass%, which is greater than 40.0 mass%, while still achieving the same hardness as Comparative Example 1.
[0053] To summarize the above, the following can be said: First, compared to Comparative Example 1 in which no porous carbon ceramic material (RHSC) was added, Examples 1 and 2 in which 45.0 mass% RHSC was added and Example 3 in which 56.0 mass% RHSC was added achieved a 41 to 58% reduction in friction.
[0054] For this reason, from the viewpoint of reducing friction in a sealing member made of a rubber composition, it is recommended that the particles of the porous carbon ceramic material be blended in an amount of more than 40.0 mass%, preferably 45.0 mass% or more, and furthermore, it is recommended that the amount be in the range of 45.0 mass% to 56.0 mass%.
[0055] Next, when porous carbon ceramic material (RHSC) is added, both particle sizes of 106 μm and 10 μm contributed to reducing friction, so a particle size of 150 μm or less is expected to reduce friction equally, with a particle size of 106 μm or less being preferable.
[0056] According to Table 4, a particle size of 10 μm can reduce friction more than a particle size of 106 μm. From this trend, it is expected that the smaller the particle size, the lower the friction. A particle size of 10 μm is more preferable than a particle size of 106 μm, and a particle size smaller than 10 μm is even more preferable than a particle size of 10 μm. From the above, a particle size of 10 μm or less is more preferable.
[0057] The use of a dust seal with a low friction coefficient facilitates relative axial movement of the outer tube 11 relative to the inner tube 12, improving the ride comfort and handling stability of the vehicle. As described above, since the friction coefficients of Examples 1 to 3 are lower than that of Comparative Example 1, it is believed that a vehicle equipped with the dust seal 16 using Examples 1 to 3 will have improved ride comfort and handling stability.
[0058] Furthermore, the use of an oil seal with a low friction coefficient facilitates relative axial movement of the outer tube 11 with respect to the inner tube 12, improving the ride comfort and handling stability of the vehicle. As described above, since the friction coefficients of Examples 1 to 3 are lower than that of Comparative Example 1, it is believed that a vehicle equipped with the oil seal 17 using Examples 1 to 3 will have improved ride comfort and handling stability.
[0059] As described above, it is believed that the ride comfort and driving stability of a vehicle are improved by providing either the dust seal 16 using Examples 1 to 3 or the oil seal 17 using Examples 1 to 3. Therefore, it is believed that a vehicle provided with both the dust seal 16 using Examples 1 to 3 and the oil seal 17 using Examples 1 to 3 will have improved ride comfort and driving stability.
[0060] In the embodiment, the vehicle suspension is a front suspension of a motorcycle, but it may be a rear suspension of a motorcycle. Also, the vehicle may be a three-wheeled vehicle or a four-wheeled vehicle in addition to a motorcycle. Therefore, the vehicle suspension is not limited to a front suspension of a motorcycle. [Industrial Applicability]
[0061] The seal member of the present invention is suitable for use in vehicle suspensions. [Explanation of symbols]
[0062] 10...vehicle suspension, 16...dust seal, 17...oil seal, 18...sealing member.
Claims
1. A sealing member made of a rubber composition containing particles of a porous carbon ceramic material in an amount exceeding 40.0 mass %.
2. The seal member according to claim 1 , wherein the particles have a diameter of 150 μm or less.
3. The seal member according to claim 2 , wherein the particles have a diameter of 10 μm or less.
4. The seal member according to any one of claims 1 to 3, wherein the rubber composition contains a coupling agent.
5. A vehicle suspension comprising an oil seal made of the seal member according to any one of claims 1 to 3.
6. A vehicle suspension comprising an oil seal comprising the seal member according to claim 4.
7. A vehicle suspension comprising a dust seal made of the seal member according to any one of claims 1 to 3.
8. A vehicle suspension comprising a dust seal comprising the seal member according to claim 4.
Citation Information
Patent Citations
Sealing material
JP6519789B2