Packaging bag for heat sterilization

A multilayer film structure with defined propylene-α-olefin block copolymers in the sealing layer addresses sealing strength issues during heat sterilization, ensuring effective steam release and maintaining integrity under high temperatures.

JP2024151898AInactive Publication Date: 2024-10-25TOYO SEIKAN KAISHA LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023065694
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Packaging bags for heat sterilization face issues with sealing strength degradation during retort sterilization, leading to potential seal retraction and internal pressure release failures, especially when equipped with steam release mechanisms.

Method used

A multilayer film structure with specific propylene-α-olefin block copolymers in the sealing layer, comprising innermost and outer layers with defined ratios and melt flow rates, ensuring a sealing strength of 13.7N at 80°C and less than 24.2N at 100°C, allowing smooth peeling for steam venting.

Benefits of technology

Maintains excellent sealing performance during heat sterilization and ensures smooth steam release, preventing seal retraction and internal pressure buildup, even under high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151898000002
    Figure 2024151898000002
  • Figure 2024151898000003
    Figure 2024151898000003
  • Figure 2024151898000001
    Figure 2024151898000001
Patent Text Reader

Abstract

To provide a packaging bag for heat sterilization which has seal strength capable of securing sealability of a packaging bag even in the case where it is exposed to heat sterilization under a high temperature such as retort sterilization and the like, and which has seal strength in which peeling of a seal layer progresses smoothly without causing inconvenience such as stringiness when an internal pressure increases, in the case where a vapor vent mechanism for microwave oven heating is formed.SOLUTION: In a packaging bag for heat sterilization which is formed by overlapping and sealing a multilayer film including a seal layer so that the seal layers are facing each other, the seal layer comprises a blend material which includes a propylene α-olefin block copolymer A in which MFR(230°C, 2.16 kg load)is within a range of 1.8-2.2 g / 10 min, and a propylene α-olefin block copolymer B in which MFR is within a range of 3.2-3.8 g / 10 min are included at the ratio of A:B=85:15-95:5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging bag for heat sterilization, and more specifically, to a packaging bag for heat sterilization in which the occurrence of sealing defects and the like during retort sterilization after filling with contents is effectively prevented. [Background technology]

[0002] Various types of packaged foods have been proposed in the past, which are made by filling and sealing food or other contents into a packaging bag. Since such packaged foods are subjected to heat sterilization such as retort sterilization when the contents are filled, it is necessary for the packaging bag to have a seal strength such that the airtightness of the packaging bag is not impaired even during retort sterilization. As a sealing layer (heat seal layer) used in packaging bags for heat sterilization, a propylene-based composition obtained by blending a propylene block copolymer or an ethylene-propylene random copolymer with a thermoplastic elastomer component is generally used because it has excellent heat resistance and is inexpensive (Patent Document 1, etc.).

[0003] However, even when the above-mentioned propylene-based polymers are used, when heat sterilization such as retort sterilization is performed, the seal portion recedes during retort, and the seal strength after heating is not fully satisfactory. As a technique for solving such problems, for example, Patent Document 2 listed below discloses a thermoplastic elastomer composition comprising: (A) two outer layers made of a propylene-α-olefin block copolymer consisting of (a) 95 to 70 mass % polypropylene block and (b) 5 to 30 mass % copolymer elastomer block of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3); and (B) (1) a thermoplastic elastomer composition having a main crystallization peak temperature (T CP1 ) and has a secondary crystallization peak temperature (T CP2 ) and has a main crystallization peak area (T CA1 ) versus the minor crystallization peak area (T CA2(1) the proportion (AR) of xylene solubles at a temperature of 25° C. (XI) is 10 to 30 mass %, and (2) the minor crystallization peak temperature (T CP2 The relationship between the amount of xylene solubles (XI) at 25°C is given by the formula: T CP2 A multilayer laminate consisting of at least three layers and an intermediate layer made of a propylene-based polymer composition satisfying ≦-1.05XI+104 has been proposed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-152596 [Patent Document 2] JP 2000-255012 A Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, among the above-mentioned packaging bags for heat sterilization, those having a steam vent mechanism for microwave heating are known. In this steam vent mechanism, when the internal pressure in the packaging bag rises, the seal layer around the steam vent hole peels off from its edge toward the steam vent hole, thereby releasing the internal pressure. However, as described above, if the seal strength between the seal layers of the laminate constituting the packaging bag is increased in order to prevent a decrease in seal strength due to retort sterilization or the like, peeling does not proceed smoothly even when the internal pressure rises, and the seal layers do not peel off completely, causing stretching, which may result in so-called "stringing." If such stringing occurs, it may block the steam vent hole, making it impossible to normally release the internal pressure.

[0006] Therefore, an object of the present invention is to provide a packaging bag for heat sterilization which has a seal strength sufficient to ensure the airtightness of the packaging bag even when subjected to high-temperature heat sterilization such as retort sterilization, and which, when a steam vent mechanism is formed, has a seal strength sufficient to allow smooth peeling of the seal layer without causing problems such as stringing when the internal pressure increases. [Means for solving the problem]

[0007] According to the present invention, in a packaging bag for heat sterilization, which is formed by overlapping and sealing multi-layer films each having a sealing layer so that the sealing layers face each other, the sealing layer is a single layer or a multi-layer, and the innermost surface of the single layer or multi-layer seal layer contains a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=95:5 to 60:40, and has an MFR (230°C, 2.16 kg load) in the range of 1.8 to 2.2 g / 10 min. The present invention provides a packaging bag for heat sterilization, which is characterized by comprising a blend of a propylene-α-olefin block copolymer A, a propylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=95:5 to 60:40, and a propylene-α-olefin block copolymer B having an MFR (230°C, 2.16 kg load) in the range of 3.2 to 3.8 g / 10 min, in a ratio of A:B=85:15 to 95:5.

[0008] In the packaging bag for heat sterilization of the present invention, (1) The multi-layer seal layer has at least a three-layer structure including the innermost layer, the outer layer, and an intermediate layer located between the innermost layer and the outer layer, the outer layer is made of a propylene-α-olefin block copolymer C containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=95:5 to 70:30, and the intermediate layer is made of a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3). the blend is made up of a propylene-α-olefin block copolymer C containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a mass ratio of 95:5 to 70:30, and a propylene-α-olefin block copolymer D containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a mass ratio of a:b=60:40 to 30:70, in a mass ratio of C:D=60:40 to 95:5; (2) The seal strength at 80°C is 13.7N or more. (3) The seal strength at 100°C is less than 24.2 N. (4) Equipped with a steam vent hole for microwave heating; is preferred. Effect of the Invention

[0009] According to the packaging bag for heat sterilization of the present invention, even when heat sterilization such as retort sterilization is performed after filling with the contents, it is possible to maintain excellent sealing performance without causing the seal part to recede or the contents to leak, etc. Furthermore, when a steam release mechanism for microwave heating is formed, the seal part peels off smoothly in response to an increase in internal pressure, allowing the steam release mechanism to function normally. That is, as is clear from the results of the Examples described later, the packaging bag for heat sterilization of the present invention can exhibit sufficient sealing performance if the seal strength at 80°C, the temperature assumed for heat sterilization such as retort sterilization, is 13.7 N or more. Also, if the seal strength at 100°C, the temperature assumed for microwave heating, is less than 24.2 N, the sealed portion around the steam vent hole is reliably peeled off by microwave heating, and the internal pressure of the packaging bag can be reliably released. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a cross-sectional view showing an example of a multilayer film used in the packaging bag for heat sterilization of the present invention. [Diagram 2] FIG. 1 is a plan view showing an example of a packaging bag for heat sterilization of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The packaging bag for heat sterilization of the present invention is composed of a multilayer film equipped with a sealing layer, and an important feature of the innermost layer of this sealing layer is that it is composed of a blend of two types of propylene-α-olefin block copolymers, propylene-α-olefin block copolymer A (hereinafter sometimes referred to as "component A") having an MFR of 1.8 to 2.2 g / 10 min and propylene-α-olefin block copolymer B (hereinafter sometimes referred to as "component B") having an MFR of 3.2 to 3.8 g / 10 min, in a ratio (mass ratio) of A:B = 85:15 to 95:5. By having such a sealing layer as the innermost layer, a packaging bag formed by overlapping the innermost layers facing each other and sealing the edges has a seal strength of 13.7 N or more at 80°C and less than 24.2 N at 100°C, enabling airtightness during heat sterilization such as retort sterilization and reliable steam release when a steam venting mechanism for microwave heating is formed.

[0012] (Sealing layer) The components A and B in the present invention are composed of a propylene-α-olefin block copolymer containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3), in a ratio of a:b=95:5 to 60:40.

[0013] In the above-mentioned A component and B component, the (a) polypropylene block may be a homopolypropylene or a random copolymer of propylene and 5% by mass or less of an α-olefin having 2 to 12 carbon atoms (excluding 3). The copolymerization ratio of the α-olefin is 5% by mass or less, and preferably 4.5% by mass or less. If the copolymerization ratio exceeds 5% by mass, the rigidity and heat resistance are impaired, or the amount of low-crystalline components increases, causing blocking of the film, which is not preferable.

[0014] In the above-mentioned components A and B, the (b) elastomer block is made of a copolymer elastomer of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3). In the A and B components, the (a) component and the (b) component are contained in a ratio (mass ratio) in the range of a:b=95:5 to 70:30. If the ratio of the (b) component is less than 5% by mass, the heat seal strength after retort sterilization is significantly reduced, and impact resistance and cold resistance are poor, which is not preferable. On the other hand, if the (b) component is more than 30% by mass, the heat resistance is poor, and there is a problem of films blocking each other due to heat sterilization such as retort treatment.

[0015] Examples of the α-olefin in the above components (a) and (b) include 1-butene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 4,4-dimethyl-1-pentene, vinylcyclopentane, vinylcyclohexane, etc. These α-olefins may be used alone or in combination of two or more.

[0016] The MFR (melt flow rate) of component A and component B was measured in accordance with JIS K7210 at a temperature of 230°C and a load of 2.16 kg. It is important that the MFR of component A is in the range of 1.8 to 2.2 g / 10 min, and that the MFR of component B is in the range of 3.2 to 3.8 g / 10 min. By combining two types of propylene-α-olefin block copolymers with different MFRs in this way, it is possible to prevent a decrease in impact strength and seal strength after retort sterilization without impairing film formability.

[0017] As described above, the A component and the B component are blended in a ratio of A:B = 85:15 to 95:5, particularly 90:10 to 95:5, and if the A component is more than the above range, the high temperature resistance decreases and the seal strength decreases. On the other hand, if the B component is more than the above range, the seal strength becomes too high, and when a steam release mechanism is formed, peeling does not proceed smoothly even if the internal pressure increases due to microwave heating, and the seal layers do not peel completely from each other, causing stretching and stringiness.

[0018] The sealing layer in the multilayer film constituting the packaging bag for heat sterilization of the present invention may be a single layer consisting of a blend of the above-mentioned components A and B. However, it is preferable that the sealing layer have a three-layer structure in which the blend is the innermost layer, an outer layer, and an intermediate layer located between the innermost layer and the outer layer. The outer layer is preferably made of a propylene-α-olefin block copolymer C (hereinafter sometimes referred to as "component C") containing the above-mentioned polypropylene block (a) and the above-mentioned copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3), in a ratio of a:b=95:5 to 70:30. By containing components (a) and (b) in the above ratio, the product has excellent rigidity and heat resistance, and is effectively prevented from decreasing in heat seal strength due to retort sterilization or the like.

[0019] The (a) polypropylene block in component C constituting the outer layer may be, like the (a) component in components A and B described above, a homopolypropylene or a random copolymer of propylene and 5% by mass or less of an α-olefin having 2 to 12 carbon atoms (excluding 3). The copolymerization ratio of the α-olefin in component (a) is preferably 5% by mass or less, and particularly preferably 4.5% by mass or less. If the copolymerization ratio exceeds 5% by mass, the rigidity and heat resistance are impaired, or the amount of low-crystalline components increases, causing blocking of the film, which is not preferable. Similarly, the (b) elastomer block in the above-mentioned component C is composed of a copolymer elastomer of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3), similar to the (b) components in the above-mentioned components A and B. The copolymerization ratio of the α-olefin in the (b) component is preferably 5 to 40 mass%, and more preferably in the range of 10 to 35 mass%.

[0020] The ratio of the (a) component to the (b) component in the above-mentioned C component is preferably in the range of a:b=95:5 to 70:30. If the ratio of the (b) component is less than the above range, the heat seal strength after retort sterilization is significantly reduced, and impact resistance and cold resistance are poor, which is not preferable. On the other hand, if the amount of the (b) component is more than the above range, the heat resistance is poor, and there is a problem of films blocking each other due to heat sterilization such as retort treatment. The MFR of the C component is not particularly limited, and is generally in the range of 0.5 to 5 g / 10 min, preferably 0.8 to 4 g / 10 min, and particularly preferably 1.0 to 3 g / 10 min. If the MFR is less than 0.5 g / 10 min, eye discharge is likely to occur during molding, which is undesirable as it is poor in productivity. On the other hand, if the MFR exceeds 5 g / 10 min, the impact strength and compatibility with the intermediate layer described below tend to be poor, and the degree of reduction in heat seal strength after retort sterilization tends to be large, which is undesirable.

[0021] The intermediate layer is suitably made of a blend of the above-mentioned component C, i.e., a propylene-α-olefin block copolymer C containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a mass ratio of 95:5 to 70:30, and a propylene-α-olefin block copolymer D (hereinafter sometimes referred to as “component D”) containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=60:40 to 30:70, with the blend containing the above-mentioned component C:D=60:40 to 95:5. The proportion of component D in the intermediate layer is 5 to 40% by mass, preferably 8 to 35% by mass, and particularly preferably 10 to 30% by mass. If the proportion of component D is less than 5% by mass, the effect of improving the heat seal strength after heat sterilization is poor, and if it exceeds 40% by mass, the heat resistance, rigidity, and chemical resistance are deteriorated, which is not preferable.

[0022] The component C constituting the intermediate layer is the same as the component C constituting the outer layer. The (a) polypropylene block in component D constituting the intermediate layer may be a copolymer of propylene and an α-olefin having 12 or less carbon atoms, with the copolymerization ratio of the α-olefin being 8.0% by mass or more, preferably 9.0% by mass or more, and particularly preferably 10% by mass or more. If the copolymerization ratio is less than 8% by mass, the rigidity and heat resistance are impaired and the heat seal strength due to heat sterilization is significantly reduced, which is undesirable. The (b) propylene block copolymer elastomer in component D includes a copolymer elastomer of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3), and the copolymerization ratio of the α-olefin is 30 to 80 mass%, preferably 35 to 75 mass%, and particularly preferably 38 to 72 mass%. If the copolymerization ratio is less than 30 mass%, the impact resistance and cold resistance are poor. On the other hand, if it exceeds 80 mass%, the heat resistance is impaired, which is not preferable.

[0023] The ratio of component (a) to component (b) in component D is preferably in the range of a:b=60:40 to 30:70. If the ratio of component (b) is less than the above range, there is a risk of a decrease in impact resistance, cold resistance, and heat seal strength after heat sterilization, while if the amount of component (b) is more than the above range, there is a risk of poor rigidity and retort resistance such as film blocking. There are no particular limitations on the MFR of the blend of components C and D constituting the intermediate layer, and similarly to the outer layer, it is preferably in the range of 0.5 to 5 g / 10 min, preferably 0.8 to 4 g / 10 min, and particularly preferably 1.0 to 3 g / 10 min.

[0024] In the case of a single layer, the above-mentioned seal layer is preferably in the range of 20 to 180 μm from the viewpoint of heat seal strength and transparency, and in the case of the above-mentioned three-layer seal layer, the total thickness is in the above range, and the thickness ratio of the innermost layer / middle layer / outer layer is preferably in the range of 0.5 to 2.0 / 6.0 to 9.0 / 0.5 to 2.0, preferably 0.6 to 1.7 / 6.6 to 8.8 / 0.6 to 1.7, and particularly preferably in the range of 0.8 to 1.5 / 7.0 to 8.4 / 0.8 to 1.5. If the thickness ratio of the inner and outer layers is less than 0.5, there is a risk of eye discharge and heat resistance being inferior compared to the case in the above range, while if it exceeds 2.0, there is a risk of a large decrease in whitening resistance, impact strength, and heat seal strength after retort sterilization treatment compared to the case in the above range.

[0025] Each layer constituting the above-mentioned sealing layer may contain an appropriate amount of known resin additives such as antioxidants, weather resistance stabilizers, antistatic agents, lubricants, antiblocking agents, antifogging agents, dyes, pigments, oils, waxes, and fillers, as well as other thermoplastic resins, within a range that does not impair the object of the present invention. Furthermore, each component constituting the sealing layer can be prepared by a conventionally known method. When making a sealing layer having a three-layer structure, a sealing layer film having a three-layer structure can be formed in advance by coextrusion, or a laminate can be formed by extrusion lamination directly onto a substrate, etc., as described below.

[0026] (Multilayer film) The packaging bag for heat sterilization of the present invention can have the same structure as the conventionally known packaging bags for heat sterilization, except that the laminated film having the above-mentioned seal layer is used. That is, the laminated film is composed of at least the above-mentioned seal layer and base layer, and other layers can be further formed depending on the type of contents, functions to be added, etc.

[0027] From the viewpoint of heat resistance, the base layer can be preferably made of any of the materials conventionally used as base layers for packaging bags for heat sterilization, such as polyester resin, polycarbonate resin, polyether ether ketone resin, nylon, etc. In particular, the base layer is preferably made of any of the following materials, although it is not limited thereto: polybutylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, a blend of polyethylene terephthalate and polybutylene terephthalate, a co-extruded film of polyethylene terephthalate and polybutylene terephthalate, and a copolymer of ethylene terephthalate and ethylene naphthalate. From the viewpoint of recyclability, it is preferable that most of the films constituting the multi-layer film are made of propylene-based materials, and therefore it is preferable to use a polypropylene film. The film constituting the base layer is preferably uniaxially or biaxially stretched, and a biaxially stretched film having excellent mechanical strength, crack resistance, and heat resistance can be preferably used.

[0028] The substrate layer may be made of the above-mentioned film alone, or may be made into a multi-layer substrate layer (outermost layer and intermediate layer) by laminating a number of different types of films by the lamination method described below. The thickness of the base layer depends on the layer structure, but is preferably in the range of 9 μm to 30 μm, particularly 12 μm to 15 μm. If the thickness of the base layer is thinner than the above range, the mechanical strength and crack resistance are inferior to those in the above range, while if the thickness is thicker than the above range, the tear resistance and economic efficiency are inferior to those in the above range.

[0029] Layers other than the seal layer and the base layer may include, but are not limited to, a barrier layer, an easy-tear layer, an adhesive layer, a printed layer, and the like. As the barrier layer, a vapor deposition layer formed by vapor depositing an inorganic material such as silicon oxide, a ceramic such as alumina, carbon, or the like by chemical vapor deposition (CVD), vacuum deposition, sputtering, ion plating, or the like on a resin film used for the base layer, or a coating layer formed of a barrier resin coating agent made of a polycarboxylic acid polymer, vinylidene chloride, an ethylene-vinyl alcohol copolymer, a compound having a metalloxane bond, or the like, can be preferably used, and a vapor deposition layer of silica or alumina is particularly preferably used. The resin film used for the barrier layer is preferably biaxially stretched. The barrier layer may be the outermost layer or may be located between the substrate layer and the seal layer. The thickness of the resin film on which the deposition layer or coating layer is formed is preferably in the range of 12 μm to 15 μm. If the thickness of the resin film is thinner than the above range, the mechanical strength and crack resistance are inferior to those in the above range, while if the thickness is thicker than the above range, the tearability and economic efficiency are inferior to those in the above range.

[0030] The easy-tear layer is disposed adjacent to a seal layer having poor tearability, so that the seal layer conforms to the easy-tear layer, thereby improving the tearability of the packaging bag. Examples of the film constituting the easy-tear layer include, but are not limited to, a film made of a blend of polybutylene terephthalate containing polytetramethylene glycol units and polyethylene terephthalate, or a film made of a blend of polyethylene terephthalate and polyester elastomer, with the polyester elastomer dispersed in the polyethylene terephthalate, which is biaxially stretched. Also, a polyester film processed with a laser or the like to impart tearability can be used. The thickness of the easy-tear layer is preferably in the range of 12 to 15 μm. If the thickness of the resin film is thinner than the above range, the mechanical strength and crack resistance will be inferior to those in the above range, while if the thickness is thicker than the above range, the tearability and economic efficiency will be inferior to those in the above range.

[0031] The multi-layer film used in the present invention may have a conventionally known layer structure, so long as the innermost layer is the above-mentioned sealing layer. FIG. 1 shows an example of a multilayer film used in the packaging bag of the present invention. The multilayer film, generally designated by 1, is composed of, from the outside, an outermost layer (base material layer) 2, an intermediate layer (barrier layer) 3, and an inner layer (sealing layer) 4, with adhesive layers 5 provided between each layer. In the embodiment shown in FIG. 1, the sealing layer 4 is composed of an innermost layer 4a, an intermediate layer 4b, and an outer layer 4c. The intermediate layer (barrier layer) 3 is a barrier layer 3 composed of a resin layer 3b having a vapor deposition layer or coating layer 3a. A multilayer structure in which the vapor deposition layer or coating layer 3a is located on the substrate layer 2 side of the outermost layer can be preferably used. In addition to the specific example shown in FIG. 1, the multilayer film used in the present invention can also be a multilayer film having a two-layer structure of, from the outside, an outermost layer (substrate layer) / sealing layer, a multilayer film having a layer structure of an outermost layer (substrate layer / barrier layer) / intermediate layer (substrate layer) / sealing layer, a multilayer film having a layer structure of an outermost layer (substrate layer) / barrier layer / easy-tear layer / sealing layer, a multilayer film having a layer structure of an outermost layer (substrate layer) / intermediate layer (substrate layer) / barrier layer / easy-tear layer / sealing layer, etc.

[0032] The multi-layer film used in the present invention can be laminated by a conventionally known lamination method such as a dry lamination method, a sandwich lamination method, or an extrusion lamination method. For example, but not limited to, each film such as the outermost layer, the base layer, the seal layer, and the barrier layer may be prepared separately and then laminated by a dry lamination method. Alternatively, a multilayer film can be produced by extrusion laminating a resin constituting the outermost layer (substrate layer) onto the vapor deposition or coating layer side of a film constituting a barrier layer having a vapor deposition layer or coating layer to produce a laminate consisting of two layers, a barrier layer and a substrate layer, and extrusion laminating the above-mentioned blend constituting the seal layer onto the surface of the vapor deposition layer or coating layer via an adhesive resin. Examples of adhesives that can be used in the multilayer film used in the present invention include conventionally known polyether polyurethane or polyester polyurethane urethane adhesives, epoxy adhesives, and acid-modified thermoplastic resin adhesives such as maleic anhydride-modified polypropylene. From the viewpoint of retort resistance, however, it is preferable to use a urethane adhesive.

[0033] (packaging bag) The heating packaging bag of the present invention is formed by overlapping the above-mentioned multilayer film so that the sealing layers face each other and sealing the periphery. When the heating packaging bag of the present invention is made microwave compatible, it is preferable that it is provided with a steam release mechanism that automatically opens during microwave heating to release steam. Any conventionally known steam release mechanism can be used, but the packaging bag of the present invention, as described above, is provided with a seal layer having a seal strength of 13.7 N or more at 80°C and less than 24.2 N at 100°C, and therefore the steam release seal portion can be sealed with the same seal strength as the peripheral seal portion, resulting in excellent productivity and economy.

[0034] FIG. 2 is a plan view of an example of the packaging bag for microwave heating of the present invention. The packaging bag, generally designated 10, is formed by overlapping two multilayer films 1a, 1b with the sealing layer on the inside and heat-sealing the four sides; as a result, the four sides of the packaging bag 10 are sealed by a bottom seal portion 11, side seal portions 12a, 12b, and a top seal portion 13, forming a storage section 14. In this embodiment, a steam release mechanism 15 is formed on the upper right side of the package 1. The steam release mechanism 15 is composed of a steam release seal portion 20 which allows the overlapping multilayer films 1a, 1b to be rearwardly peeled away when the internal pressure rises, a non-adhesive portion 21 which is located inside this steam release seal portion 20 and where the overlapping multilayer films 1a, 1b are not adhered to each other, and a steam release hole 22 formed in the multilayer film 1a on the surface side of this non-adhesive portion 21.

[0035] In the heating packaging bag of the present invention, the shape of the package is not limited to the four-sided sealed form described above, and it can be formed into various shapes such as a three-sided sealed packaging bag made by folding a single multilayer film and sealing three sides, a gusseted packaging bag, a standing-type packaging bag, and a pillow-type packaging bag. In the heating packaging bag of the present invention, the steam release mechanism formed to accommodate microwave heating is not limited to the embodiment shown in FIG. 2, so long as it can be automatically opened during microwave heating. In addition, the steam vent mechanism is preferably located near the peripheral seal of the packaging bag from the standpoint of allowing steam inside the packaging bag caused by microwave heating to escape while preventing the contents from leaking. EXAMPLES

[0036] (Resin used) Component A: Contains a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=80:20, Propylene-α-olefin block copolymer with MFR (230℃, 2.16 kg load) of 2.0 g / 10 min. Component B: A polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=70:30, Propylene-α-olefin block copolymer with MFR (230℃, 2.16 kg load) of 3.5 g / 10 min. Component C: A propylene-α-olefin block copolymer containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3), in a ratio of a:b=80:20. Component D: A propylene-α-olefin block copolymer containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3), in a ratio of a:b=35:65.

[0037] (Examples 1 to 3 and Comparative Examples 1 and 2) An innermost layer made of a blend of the above-mentioned A and B components in the mixing ratio shown in Table 1, an outer layer made of the above-mentioned C component, and an intermediate layer made of a blend of the above-mentioned C and D components in a mass ratio of 80:20 were co-extruded so that the thicknesses of the innermost layer / intermediate layer / outer layer were 20 μm / 20 μm / 20 μm to create a three-layer seal layer film. A 12 μm biaxially oriented polyethylene terephthalate film was used as the base layer, and laminated with the above-mentioned sealing layer film to create a multilayer film. From the resulting multilayer film, a packaging bag with a steam release mechanism as shown in Figure 2 was created. The heat sealing conditions were 175°C and a pressure of 0.2 kg / cm. 2 The test was performed under the condition of 1 second.

[0038] (Seal strength) The resulting packaging bag was placed in a thermostatic chamber, heated to 80°C and 100°C, and held for 2 minutes, after which the seal strength of the side seal and bottom seal were measured at 80°C and 100°C using a tensile tester at a tensile speed of 300 mm / min. The evaluation criteria were as follows: [Seal strength 80℃] The seal strength at 80°C in Comparative Example 1 was less than 13.7N, and sufficient sealability for retort sterilization and the like could not be exhibited, whereas Examples 1 to 3 and Comparative Example 2, which had a seal strength of more than 13.7N at 80°C, exhibited sufficient sealability. The seal strength tends to increase as the ratio of component B increases, and it was 24.4N in Comparative Example 2. From the above results, in Table 1, cases where the seal strength at 80°C was 13.7N or more are indicated by "◯", and cases where it was less than 13.7N are indicated by "X". [Seal strength 100℃] In Comparative Example 2, the seal strength at 100°C was 24.2 N or more, and stringiness occurred, whereas in Comparative Example 1 and Examples 1 to 3, where the seal strength at 100°C was less than 24.2 N, no stringiness occurred. The seal strength tends to increase as the ratio of component B increases, and it was 10.9 N in Comparative Example 1. From the above results, in Table 1, cases where the seal strength at 100°C was less than 24.2 N are indicated as "◯", and cases where it was 24.2 N or more are indicated as "X".

[0039] (Stringiness Evaluation) The resulting packaging bag was filled with water and retort sterilized at 121°C for 30 minutes. The retort sterilized packaging bag was heated in a 600W microwave for about 2 minutes and the steam release holes were observed after heating. The results are shown in Table 1, with "○" indicating that no stringiness occurred in the seal layer and "×" indicating that stringiness occurred.

[0040] [Table 1] [Explanation of symbols]

[0041] 1 multilayer film, 2 outermost layer (base material layer), 3 middle layer (barrier layer), 4 inner layer (sealing layer), 5 adhesive layer, 10 packaging bag, 11 bottom seal portion, 12 side seal portion, 13 top seal portion, 14 storage portion, 20 steam release seal portion, 21 non-adhesive portion, 22 steam release hole.

Claims

1. A packaging bag for heat sterilization, which is formed by overlapping and sealing a multi-layer film having a sealing layer so that the sealing layers face each other, The sealing layer is a single layer or a multi-layer, The packaging bag for heat sterilization, characterized in that the innermost surface of the single-layer seal layer or the multi-layer seal layer is made of a blend containing a propylene-α-olefin block copolymer A, which contains a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=95:5 to 60:40 and has an MFR (230°C, 2.16 kg load) in the range of 1.8 to 2.2 g / 10 min, and a propylene-α-olefin block copolymer B, which contains a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=95:5 to 60:40 and has an MFR (230°C, 2.16 kg load) in the range of 3.2 to 3.8 g / 10 min, in a ratio of A:B=85:15 to 95:

5.

2. The multi-layer sealing layer has at least a three-layer structure including an innermost layer, an outer layer, and an intermediate layer located between the innermost layer and the outer layer; the outer layer is made of a propylene-α-olefin block copolymer C containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3), in a ratio of a:b=95:5 to 70:30; 2. The packaging bag for heat sterilization according to claim 1, wherein the intermediate layer is made of a blend containing a propylene-α-olefin block copolymer C containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a mass ratio of 95:5 to 70:30, and a propylene-α-olefin block copolymer D containing a polypropylene block (a) and a copolymer elastomer block (b) of propylene and an α-olefin having 2 to 12 carbon atoms (excluding 3) in a ratio of a:b=60:40 to 30:70, in a ratio of C:D=60:40 to 95:

5.

3. 3. The packaging bag for heat sterilization according to claim 1 or 2, which has a seal strength of 13.7 N or more at 80°C.

4. 3. The packaging bag for heat sterilization according to claim 1 or 2, which has a seal strength of less than 24.2 N at 100°C.

5. 5. The packaging bag for heat sterilization according to claim 4, further comprising a steam vent hole for use in heating in a microwave oven.

Citation Information

Patent Citations

  • Sealant film for retort

    JP1998152596A

  • Multilayered laminate

    JP2000255012A