Toner
The capsule toner particles with a styrene acrylic core and high-melting-point shell, coated with hydrophobized silica, address the dye compatibility and stability issues in sublimation transfer dyeing, achieving efficient dye transfer and improved toner stability.
Patent Information
- Application Number
- JP2023065742
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing toners for sublimation transfer dyeing methods using polyester resin as a binder face challenges with sublimable dyes having difficulty in oozing out, leading to poor dyeing density, bleed-out, and reduced toner stability, especially when using styrene acrylic resin, which affects dye compatibility and charge properties.
The toner comprises capsule toner particles with a core made of styrene acrylic resin and a shell layer with a higher melting point, coated with hydrophobized silica particles, ensuring the sublimable dye is encapsulated, enhancing dye transfer efficiency and stability.
The solution effectively suppresses dye bleed-out, maintains high dye density, and improves heat-resistant storage stability, ensuring consistent image quality and color fastness to friction.
Smart Images

Figure 2024151922000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a toner suitable for dyeing by a sublimation transfer method in an electrophotographic system. [Background technology]
[0002] Dyeing methods using electrophotography for dyeing objects such as hydrophobic fibers, typically polyester fabric, can be broadly divided into two types: a direct method and a sublimation transfer method. The direct method is a dyeing method in which toner is directly attached to an object to be dyed, and then the dye contained in the toner is attached to the object to be dyed by heat treatment, and any attached substances other than the dye (resin, release agent, etc.) are dissolved and removed by alkaline cleaning. The sublimation transfer method is a dyeing method in which toner is attached to an intermediate recording medium such as paper, and then the toner-attached surface of the intermediate recording medium is superimposed on the object to be dyed, and then a heat press treatment (heating and pressure treatment) is performed to sublimate and transfer the dye contained in the toner to the object to be dyed.
[0003] Of these two dyeing methods, sublimation transfer is capable of transferring only the dye, one of the multiple components that make up the toner, from the intermediate recording medium to the fiber. In other words, no toner components other than the dye adhere to the dyed fabric, and this has the advantage of eliminating the need for processes such as washing and drying the dyed fabric. For this reason, it is considered suitable for dyeing applications where texture is important, such as clothing (sports apparel, etc.) and interiors (seats, sofas, etc.).
[0004] In addition, by eliminating the need for processes such as washing and drying, the dyeing process can be significantly reduced, and there are many other benefits, such as the absence of a washing and drying line that requires a large amount of space and energy to operate, and the absence of a treatment facility for washing water. Therefore, the sublimation transfer method is considered to be an excellent dyeing method in that it can be used in a small space.
[0005] As the dye in the toner used in the sublimation transfer method, among disperse dyes or oil-soluble dyes suitable for dyeing hydrophobic fibers, particularly, an easily sublimable dye excellent in sublimation transfer suitability to hydrophobic fibers by heat treatment is used.
[0006] In addition, as printing means in the sublimation transfer method, there are an inkjet method and an electrophotographic method, and generally the inkjet method is the mainstream. However, in the sublimation transfer in the inkjet method, there are problems such as an organic solvent, which is one of the components constituting the ink, being volatilized by the heat when transferring the dye and contaminating the working environment. On the other hand, the electrophotographic method has attracted attention in recent years because there are no volatile components in the toner and it does not contaminate the working environment.
[0007] As a toner for use in dyeing by the sublimation transfer method in the electrophotographic method, for example, in Patent Document 1, toner particles containing a binder resin mainly composed of a polyester resin and a dye having sublimability are surface-modified with silica as a fluidizing agent, and a toner in which silica as an external additive adheres to the surface of the surface-modified toner particles is disclosed. The volume-based median particle diameter (D50) of the toner is 4 μm to 10 μm, the glass transition temperature of the toner is 53°C to 70°C, and when the specific surface area of a true sphere at the volume-based median particle diameter of the toner is A0 and the BET specific surface area of the toner washed under specific conditions is A1, it is said that the heat-resistant storage property is improved by satisfying 1.2 < A1 / A0 < 2.6.
Prior Art Documents
Patent Documents
[0008]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0009] However, in toners for dyeing by sublimation transfer (sublimation transfer), when polyester resin is used as the binder resin, the dye having sublimability (hereinafter also referred to as sublimation dye) does not easily bleed out of the resin, making it difficult to use a sublimation transfer dyeing method capable of dyeing the object with high efficiency, and there is a problem that sufficient dyeing density cannot be obtained even if the disperse dye in the toner is increased. To solve this problem, when styrene acrylic resin is used as the binder resin, the compatibility between the sublimation dye and the binder resin decreases, making it possible to obtain an object with a high dyeing density, but while the toner is stored in an unused state, bleed-out occurs, which is a phenomenon in which the sublimation dye bleeds out from the inside of the toner particles to the surface (phenomenon illustrated in Figure 2), and the fluidity of the toner deteriorates or the charge amount of the toner decreases, making it difficult to use it as a toner for sublimation transfer.
[0010] The toner of the present disclosure has been discovered in consideration of the above-mentioned circumstances of toners in which the binder resin is a styrene acrylic resin, and has a primary object to provide a toner that can suppress bleeding out of sublimable dyes in dyeing by sublimation transfer method, and has excellent shell layer uniformity, sublimation transfer efficiency, and color fastness to friction. [Means for solving the problem]
[0011] The toner disclosed herein, which has been made to solve the above problems, is a toner having encapsulated toner particles containing a dye having sublimation properties, the encapsulated toner particles each having a core toner particle and a shell layer covering the surface of the core toner particle, the melting point of the resin forming the core toner particle being 105°C or higher and 135°C or lower, and the melting point of the resin forming the shell layer being 140°C or higher and 160°C or lower.
[0012] In the above toner, the ratio of the shell layer in the capsule toner particles is preferably 12 parts by mass or more and 23 parts by mass or less with respect to 100 parts by mass of the core toner particles.
[0013] In the above toner, the circularity of the capsule toner particles is preferably 0.950 or more.
[0014] In the above toner, it is preferable that silica particles having hydrophobic surfaces are present at the interface between the core toner particles and the shell layer.
[0015] In the above toner, the median particle size of the silica particles is preferably 20 nm or more and 50 nm or less.
[0016] In the above toner, it is preferable that the surfaces of the silica particles are hydrophobized with dimethylpolysiloxane.
[0017] In the toner, it is preferable that the coverage of the surface of the core toner particle with the silica particles is 45% or more and 75% or less.
[0018] The toner manufacturing method of the present disclosure, which has been made to solve the above problems, is characterized by including a core toner particle preparation step of preparing core toner particles, a resin microparticle preparation step of preparing resin microparticles that form a shell layer, a composite particle formation step of coating the surfaces of the core toner particles with the resin microparticles to form composite particles, and a capsule toner particle formation step of forming capsule toner particles by forming a film of the resin microparticles on the surfaces of the core toner particles.
[0019] In the above toner manufacturing method, the median particle diameter of the fine resin particles prepared in the fine resin particle preparation step is preferably 0.1 μm or more and 0.2 μm or less.
[0020] In the above-mentioned toner manufacturing method, it is preferable that in the composite particle formation step, the emulsion of resin microparticles and the core toner particles are mixed and dried under reduced pressure to form the composite particles, and in the capsule toner particle formation step, the composite particles are dispersed in an air flow circulating through a ring-shaped flow path to form the capsule toner particles.
[0021] In the above-mentioned toner manufacturing method, it is preferable that the composite particle formation process includes a process of mixing the core toner particles and the silica particles to obtain a mixture, and a process of mixing and drying the emulsion of resin microparticles and the mixture under reduced pressure to form the composite particles. Effect of the Invention
[0022] The toner of the present disclosure exhibits excellent effects such as suppressing bleeding out of dyes having sublimation properties, uniformity of the shell layer, excellent sublimation transfer efficiency, and excellent color fastness to friction. [Brief description of the drawings]
[0023] [Figure 1] FIG. 2 is a cross-sectional view illustrating a capsule toner. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic diagram of a non-encapsulated toner. [Diagram 3] FIG. 2 is a front view showing a schematic configuration of a capsule toner particle manufacturing apparatus used in the toner manufacturing method according to the embodiment of the present disclosure. [Figure 4] 4 is a schematic cross-sectional view of the manufacturing apparatus shown in FIG. 3 taken along the cross-sectional line A200-A200. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The toner of the present disclosure will be described in detail below.
[0025] 1. Capsule toner particles As shown in FIG. 1, the encapsulated toner particles according to the present embodiment are composed of core toner particles containing a styrene acrylic resin as a binder resin and an internal additive, and a shell layer covering the surface of the core toner particles. The internal additives, such as a sublimable dye and a release agent, are dispersed in the binder resin. An external additive is attached to the surface of the encapsulated toner particles. If necessary, any optional component may be contained within a range that does not impair the effects of the present disclosure. The average primary particle size of the encapsulated toner particles can be appropriately selected depending on the purpose, and may be, for example, 4 μm or more and 8 μm or less.
[0026] In the capsule toner particles according to the present embodiment, the binder resin forming the core toner particles has a melting point of 105° C. or more and 135° C. or less, and preferably 110° C. or more and 130° C. or less. The resin forming the shell layer has a melting point of 140° C. or more and 160° C. or less, and preferably 145° C. or more and 155° C. or less. When the melting point of the binder resin forming the core toner particles is within the above range, and the melting point of the resin forming the shell layer is also within the above range, it is possible to suppress the sublimation dye from bleeding out from the inside of the core toner particles to the surface, and thus it is possible to improve the heat-resistant storage stability of the toner.
[0027] In the capsule toner particles according to the present embodiment, the resin forming the shell layer has a high melting point, which makes the shell layer hard. Therefore, the surface of the capsule toner particles is less likely to deteriorate, and the occurrence of toner bleeding out on the developing roller (developer carrier) in the developing device can be effectively suppressed. This makes it possible to maintain high image quality of the formed image throughout the life of the toner.
[0028] In addition, the capsule toner particles according to the present embodiment are formed by forming composite particles in which the surface of the core toner particles is covered with resin fine particles, and then forming the resin fine particles into a film. Since the resin fine particles are hard, the flowability of the composite particles and the capsule toner particles can be increased. Therefore, in the production of the capsule toner particles according to the present embodiment, the processing temperature during film formation by mechanical processing can be increased, so that a thin shell layer that is difficult to peel off can be formed. In addition, resin fine particles that are not attached to the surface of the core toner particles as a shell layer (also called residual shell) are less likely to be generated. Therefore, the heat is easily transferred during the fixing process in the image forming device, and the fixing property of the toner is improved.
[0029] Contrary to the capsule toner particles according to the present embodiment, if the melting point of the resin forming the shell layer is designed to be lower than the melting point of the resin forming the core toner particles, the capsule function of the shell layer may not be fully exhibited, and the effect of improving the heat-resistant storage stability may not be fully obtained. Note that, as described above, in toner particles not provided with a shell layer (non-encapsulated toner particles), when a styrene acrylic resin is used as a binder resin, there is a problem that bleed-out occurs during storage of the toner, in other words, there is a problem with the heat-resistant storage stability.
[0030] The encapsulated toner particles according to the present embodiment preferably have a circularity of 0.950 or more, more preferably 0.952 or more. The circularity of the encapsulated toner particles is an index for measuring the degree of completion of the core-shell structure, and when the circularity is within the above range, it is easy to exert the effects of suppressing bleed-out of the sublimation dye, enhancing the sublimation transfer efficiency, and enhancing the color fastness to friction.
[0031] <Core toner particles> -Binding resin- The core toner particles according to the present embodiment contain a styrene-acrylic resin as a binder resin. The styrene-acrylic resin is not particularly limited, but may be, for example, a resin obtained by polymerizing a styrene-based monomer and a monofunctional (meth)acrylic monomer. Note that the term "(meth)acrylic" is a concept that includes both "acrylic" and "methacrylic".
[0032] The styrene monomer is not particularly limited, but examples thereof include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, 4,α-dimethylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, 2,4,6-trimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-pentylstyrene, pn-hexylstyrene, pn-heptylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decanylstyrene, pn-dodecylstyrene, p-phenylstyrene, 3,4-dicyclosilstyrene, etc. Among these, styrene is preferable for the core toner particles according to the present embodiment.
[0033] In the core toner particles according to this embodiment, among the above styrene-based monomers, one type may be used alone, or two or more types may be used in combination.
[0034] The monofunctional (meth)acrylic monomer is not particularly limited, but examples thereof include: Acrylic monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, n-octadecyl acrylate, methyl α-chloroacrylate, and ethyl α-chloroacrylate; Methacrylic monomers such as methacrylic acid, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-cyclohexyl methacrylate, n-dodecyl methacrylate, n-tridecyl methacrylate, and n-octadecyl methacrylate; Among these, in the core toner particles according to the present embodiment, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, and tert-butyl methacrylate are preferred, and n-butyl acrylate and n-butyl methacrylate are particularly preferred.
[0035] In the core toner particles according to this embodiment, one of the above monofunctional (meth)acrylic monomers may be used alone, or two or more of them may be used in combination.
[0036] The volume average particle diameter of the core toner particles according to the present embodiment is preferably 4 μm or more and 8 μm or less. By having the volume average particle diameter within the above range, a high-definition image can be stably formed for a long period of time. In addition, by making the core toner particles small in diameter, that is, the volume average particle diameter is within the above range, a high image density can be obtained even if the amount of adhesion is small, and the effect of reducing the amount of toner consumption is also obtained. On the other hand, when the volume average particle diameter of the core toner particles is less than the above lower limit, the toner may become highly charged and less fluid because the particle diameter of the capsule toner particles is small. When the toner becomes highly charged and less fluid, the toner cannot be stably supplied to the photoreceptor, and there is a risk of background fogging (the phenomenon in which the toner adheres to the part that should be blank) and a decrease in image density. When the volume average particle diameter of the core toner particles exceeds the above upper limit, the formed image may have a large layer thickness and significant granularity due to the particle diameter of the core toner particles, and there is a risk of not being able to obtain a high-definition image. In addition, when the volume average particle diameter of the core toner particles becomes large, the specific surface area of the toner decreases, and the charge amount of the toner decreases. If the charge amount of the toner becomes small, the toner cannot be stably supplied to the photoconductor, and there is a risk of the toner scattering and causing contamination inside the machine.
[0037] The binder resin in the core toner particles according to this embodiment may be a styrene-acrylic resin having a glass transition temperature (Tg) of 50° C. or more and 110° C. or less. The glass transition temperature of the styrene-acrylic resin is preferably 52° C. or more and 68° C. or less, and more preferably 55° C. or more and 65° C. or less.
[0038] The content of the binder resin in the core toner particles according to the present embodiment can be appropriately selected depending on the purpose, but is usually 60% by mass or more and 99% by mass or less, and preferably 65% by mass or more and 98% by mass or less. If the content of the binder resin is less than the lower limit, the dispersion of the dye in the toner may be poor, which may lead to a deterioration in the electrical properties of the toner. If the content of the binder resin is more than the upper limit, the color density may be reduced.
[0039] -Sublimable dye- The core toner particles according to the present embodiment contain a sublimation dye. The sublimation dye is not particularly limited, but is preferably a dye suitable for sublimation transfer.
[0040] The term "dye suitable for sublimation transfer" refers to a dye whose staining (polyester) test result in the heat-sensitive treatment test (C method) in "Testing method for color fastness to dry heat treatment [JIS L 0879:2005] (revised on January 20, 2005, published by the Japan Standards Association)" is usually 3 to 4 or less, preferably 3 or less. Among such dyes, examples of known dyes include the following dyes.
[0041] Yellow dyes include CI Disperse Yellow 3, 7, 8, 23, 39, 51, 54, 60, 71, 86; CI Solvent Yellow 114, 163, and the like.
[0042] Orange dyes include CI Disperse Orange 1, 1:1, 5, 20, 25, 25:1, 33, 56, 76, and the like.
[0043] Brown dyes include CI Disperse Brown 2 and the like.
[0044] Red dyes include CI Disperse Red 11, 50, 53, 55, 55:1, 59, 60, 65, 70, 75, 93, 146, 158, 190, 190:1, 207, 239, 240; CI Bat Red 41, and the like.
[0045] Violet dyes include CI Disperse Violet 8, 17, 23, 27, 28, 29, 36, 57, and the like.
[0046] Blue dyes include CI Disperse Blue 19, 26, 26:1, 35, 55, 56, 58, 64, 64:1, 72, 72:1, 81, 81:1, 91, 95, 108, 131, 141, 145, 359, 360; CI Solvent Blue 3, 63, 83, 105, 111, and the like.
[0047] In the toner according to the present embodiment, one of the above dyes may be used alone, or two or more may be used in combination. By combining two or more dyes, it is possible to obtain a hue that is completely different from the original dye. For example, a black dye can be obtained by appropriately blending a blue dye with a yellow dye and a red dye. In addition, by combining two or more dyes, it is possible to finely adjust the color tone of blue, yellow, orange, red, violet, black, etc. to a more preferred color tone, or to obtain an intermediate color.
[0048] The content of the sublimation dye in the core toner particles according to the present embodiment can be appropriately selected according to the purpose, but is usually 1% by mass or more and 40% by mass or less, preferably 2% by mass or more and 35% by mass or less, and more preferably 3% by mass or more and 12% by mass or less. If the content of the sublimation dye in the toner particles is less than the lower limit, the dyeing density may decrease. If the content of the sublimation dye in the toner particles exceeds the upper limit, the dye may not disperse well in the toner, which may cause the electrical properties of the toner to deteriorate.
[0049] -Release agent- The core toner particles according to the present embodiment preferably contain a wax as a release agent. As the release agent, any release agent commonly used in the art may be used, but it is more preferable to use a release agent having a penetration value of 3 to 11 at 45° C. This penetration value is measured according to the JIS K 2235 penetration value measurement test method, and can be measured, for example, using a penetration meter (manufactured by Rigo Co., Ltd.).
[0050] The release agent contained in the core toner particles according to this embodiment preferably has a peak temperature position of endothermic heat measured by differential scanning calorimetry (DSC) in the range of 70° C. to 150° C. This differential thermal analysis measurement is performed in accordance with ASTM D3418-82, and can be performed, for example, at room temperature and humidity using a differential thermal analysis measuring device DSC8230 (manufactured by Rigaku Corporation) with a measurement sample of 10 mg and a heating rate of 10° C. / min between 20° C. and 150° C.
[0051] Examples of natural waxes used as release agents include waxes derived from plants such as carnauba wax, rice wax, etc. Examples of synthetic waxes include polyethylene wax, polypropylene wax, synthetic ester wax, and polymers of α-olefins (hydrocarbons having double bonds at the molecular terminals) combined with maleic anhydride.
[0052] The content of the release agent in the core toner particles according to the present embodiment is preferably 0.1 parts by mass or more and 20 parts by mass or less, and more preferably 0.5 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the binder resin. If the content of the release agent is less than the lower limit, offset to the fixing roller may occur. If the content of the release agent is more than the upper limit, poor fixing to the intermediate recording medium may occur.
[0053] -Charge control agent- The core toner particles according to the present embodiment may contain a charge control agent. As the charge control agent, charge control agents commonly used in the art for positive charge control and negative charge control can be used.
[0054] Examples of charge control agents for positive charge control include nigrosine dyes, basic dyes, quaternary ammonium salts, quaternary phosphonium salts, aminopyrine, pyrimidine compounds, polynuclear polyamino compounds, aminosilanes, nigrosine dyes and derivatives thereof, triphenylmethane derivatives, guanidine salts, and amidine salts.
[0055] Examples of charge control agents for negative charge control include oil-soluble dyes such as oil black and spiron black, metal-containing azo compounds, azo complex dyes, metal naphthenates, metal complexes and metal salts of salicylic acid and its derivatives (metals include chromium, zinc, zirconium, etc.), boron compounds, fatty acid soaps, long-chain alkyl carboxylates, and resin acid soaps.
[0056] In the core toner particles according to this embodiment, among the above charge control agents, one type may be used alone, or two or more types may be used in combination.
[0057] The content of the charge control agent in the core toner particles according to the present embodiment is not particularly limited, but is preferably 0.5 parts by mass or more and 3.0 parts by mass or less, and more preferably 0.7 parts by mass or more and 2.5 parts by mass or less, relative to 100 parts by mass of the binder resin. By having the content of the charge control agent within the above range, it is possible to form an image having high image density and good image quality without impairing various physical properties of the toner. If the content of the charge control agent is less than the lower limit, the effect of charge control may not be obtained. If the content of the charge control agent exceeds the upper limit, the chargeability of the toner becomes too high, and the electrostatic attraction force with the developing roller increases, which may lead to a decrease in the fluidity of the toner and a decrease in image density.
[0058] -Silica particles attached to the surface of core toner particles- It is preferable that silica particles having a hydrophobic surface are attached to the surface of the core toner particles according to the present embodiment. In other words, in the capsule toner particles according to the present embodiment, it is preferable that silica particles having a hydrophobic surface are present at the interface between the core toner particles and the shell layer. This can increase the efficiency of dye seepage during sublimation transfer, and can efficiently dye fabric.
[0059] The median particle size of the silica particles whose surface is hydrophobized is preferably 20 nm or more and 50 nm or less, more preferably 30 nm or more and 40 nm or less. The median particle size of the silica particles is within the above range, and thus the efficiency of the dye bleeding can be further improved. If the median particle size of the silica particles is less than the lower limit, the effect of improving the efficiency of the dye bleeding may not be obtained due to the small particle size of the silica particles. If the median particle size of the silica particles is more than the upper limit, the amount of silica particles added to obtain a sufficient coverage rate on the core toner particle surface may increase, which may lead to an increase in cost.
[0060] The silica particles attached to the surface of the core toner particles are preferably those whose surfaces have been hydrophobized with dimethylpolysiloxane (PDMS). The presence of silica particles whose surfaces have been hydrophobized with dimethylpolysiloxane at the interface between the core toner particles and the shell layer can further increase the efficiency of dye seepage during sublimation transfer, allowing efficient dyeing of fabrics.
[0061] The coverage of the core toner particle surface by the silica particles attached to the core toner particle surface is preferably 45% to 75%, more preferably 48% to 72%, and even more preferably 55% to 65%. When the coverage is within the above range, the effect of improving the efficiency of dye bleeding during sublimation transfer can be fully exhibited. If the coverage is below the lower limit, the effect of improving the efficiency of dye bleeding may not be exhibited. If the coverage is above the upper limit, the effect of improving the efficiency of dye bleeding may be hindered, resulting in a decrease in the sublimation transfer efficiency, and the color fastness to friction may also decrease.
[0062] <Shell layer> The capsule toner particles according to the present embodiment have a shell layer covering the surface of the core toner particle, as exemplified in FIG. 1. The ratio of the shell layer in the capsule toner particle is preferably 12 parts by mass or more and 23 parts by mass or less, and more preferably 15 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the core toner particle. In the manufacturing process of the capsule toner particle, it is considered that the amount of resin fine particles (fine particles forming the shell layer) added to the core toner particle is related to the thickness of the shell layer of the capsule toner particle to be manufactured and the coverage rate of the core toner particle surface by the shell layer. It is desirable that the surface of the core toner particle is completely covered by the shell layer, but it is very difficult to achieve this state. The present inventor has found that if the coverage rate is 75% or more, the heat-resistant storage stability of the toner can be improved. By having the ratio of the shell layer in the capsule toner particle within the above range, such a coverage rate can be realized, and the toner according to the present embodiment can exhibit excellent heat-resistant storage stability.
[0063] The shell layer is preferably formed of an acrylic resin. The acrylic resin may be a resin obtained by polymerizing or copolymerizing a single monomer or a plurality of monomers including at least one of an acrylic monomer and a methacrylic monomer.
[0064] As the acrylic monomer, for example, acrylic acid and acrylic acid derivatives such as methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, propyl acrylate, octyl acrylate, 2-chloroethyl acrylate, and phenyl acrylate can be used.
[0065] Examples of methacrylic monomers that can be used include methacrylic acid, methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, phenyl methacrylate, and dimethylamino methacrylate.
[0066] As monomers that can be used other than the acrylic and methacrylic monomers, styrene and styrene derivatives such as o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-ethylstyrene, and 2,4-dimethylstyrene can be used.
[0067] The shell layer of the capsule toner particle according to the present embodiment is formed by coating the surface of a core toner particle with resin fine particles to form a composite particle, and then forming the resin fine particles into a film on the surface of the core toner particle. The resin fine particles and a method for preparing them will be described later in the section "Toner manufacturing method".
[0068] 2.External additives The toner according to the present embodiment may have an external additive attached to the surface of the capsule toner particles. The functions of the external additive include improving the powder flowability, triboelectric charging property, heat-resistant storage stability, and cleaning property of the toner, and controlling the wear property of the photoreceptor surface.
[0069] As the external additive, for example, inorganic fine particles having a median particle size of 5 nm to 200 nm, such as silica, titanium oxide, alumina, etc., can be used. Inorganic fine particles whose surfaces have been given hydrophobicity by surface treatment with a silane coupling agent, a titanium coupling agent, or silicone oil are more suitable because they reduce the decrease in electrical resistance and charge amount under high humidity conditions.
[0070] The content of the external additive is preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 0.2 parts by mass or more and 3 parts by mass or less, relative to 100 parts by mass of the capsule toner particles. If the content of the external additive is less than the lower limit, it becomes difficult to impart the effect of improving the fluidity. If the content of the external additive is more than the upper limit, the fixing property may decrease.
[0071] As a method for adding an external additive to the capsule toner particles, there is a method in which the capsule toner particles and the external additive are mixed with an air flow mixer such as a Henschel mixer.
[0072] The toner according to the present embodiment may be used as a one-component developer as it is, or may be mixed with a carrier and used as a two-component developer.
[0073] 3. Toner manufacturing method The toner manufacturing method according to this embodiment includes a core toner particle preparation process P1 for preparing core toner particles, a resin microparticle preparation process P2 for preparing resin microparticles that form a shell layer, a composite particle formation process P3 for forming composite particles by coating the surfaces of core toner particles with resin microparticles, a capsule toner particle formation process P4 for forming capsule toner particles by applying a mechanical impact force to the composite particles to form a film of the resin microparticles on the surfaces of the core toner particles, and an external addition process P5 for adhering an external additive to the surfaces of the capsule toner particles.
[0074] (1) Core toner particle production process P1 In the core toner particle preparation process P1, core toner particles are prepared. Methods for preparing core toner particles include, for example, dry methods such as a kneading and pulverizing method, and wet methods such as a suspension polymerization method, an emulsion aggregation method, a dispersion polymerization method, a dissolution suspension method, and a melt emulsification method. The method for preparing core toner particles by the kneading and pulverizing method will be described below.
[0075] In the production of core toner particles by the pulverization method, raw materials for core toner particles, including a binder resin and an internal additive such as a sublimable dye, are dry-mixed in a mixer, and then melt-kneaded in a kneader to obtain a molten kneaded product. The molten kneaded product is cooled and solidified, and the solidified product is pulverized in a pulverizer to obtain a finely pulverized product. Then, particle size adjustment such as classification is performed as necessary to obtain core toner particles.
[0076] Mixing is preferably a dry type, and a known device commonly used in the technical field can be used as the mixer. For example, Henschel type mixers such as Henschel Mixer (product name, manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (product name, manufactured by Kawata Corporation), Mechano Mill (product name, manufactured by Okada Seiko Co., Ltd.), Ang Mill (product name, manufactured by Hosokawa Micron Corporation), Hybridization System (product name, manufactured by Nara Machinery Works, Ltd.), Cosmo System (product name, manufactured by Kawasaki Heavy Industries, Ltd.), etc. can be mentioned.
[0077] As the kneader, a known device commonly used in the technical field can be used, and examples thereof include general kneaders such as a twin-screw extruder, a triple roll, and a lab blast mill. Specific examples thereof include single-screw or twin-screw extruders such as TEM-100B (trade name, manufactured by Toshiba Machine Co., Ltd.), PCM-65 / 87, and PCM-30 (all of which are trade names, manufactured by Ikegai Corporation), and open-roll type kneaders such as Kneadex (trade name, manufactured by Nippon Coke and Engineering Co., Ltd.). Among these, open-roll type kneaders are preferred in that they have a strong shear during kneading and can highly disperse the toner raw materials.
[0078] As the pulverizer, a known device commonly used in the technical field can be used, for example, Counter Jet Mill AFG (trade name, manufactured by Hosokawa Micron Corporation), which pulverizes using a supersonic jet stream, etc. As the classifier, for example, rotary classifier TSP Separator (trade name, manufactured by Hosokawa Micron Corporation) etc. can be used.
[0079] (2) Resin fine particle preparation process P2 Examples of methods for preparing resin microparticles include a method of emulsifying and dispersing a resin, which is a raw material for the resin microparticles, using a homogenizer or the like, and a method of polymerizing a monomer using a method such as emulsion polymerization or soap-free emulsion polymerization. The resin microparticles are prepared as an emulsion with a solid content of 30% by mass (water content of 70% by mass). The resin used as the raw material for the resin microparticles forms the above-mentioned shell layer.
[0080] The median particle diameter of the resin fine particles (primary particles) must be sufficiently smaller than the median particle diameter of the core toner particles, and is preferably 0.05 μm or more and 1 μm or less, and more preferably 0.1 μm or more and 0.2 μm or less. The median particle diameter of the resin fine particles is considered to be related to the thickness of the shell layer, and if the median particle diameter of the resin fine particles is less than the above lower limit, the protective effect by the formation of the shell layer may not be obtained sufficiently. In addition, in order to obtain this effect, it is necessary to add more resin fine particles, which may increase costs. If the median particle diameter of the resin fine particles exceeds the above upper limit, the adhesion of the shell layer may be weakened due to the melting point of the resin forming the shell layer being within the above range, and the shell layer may not be formed in a complete form, or the dye may bleed out onto the intermediate recording medium.
[0081] In addition, by having the median particle size of the resin microparticles within the above range, a shell layer of suitable thickness can be formed on the surface of the core toner particle, so that the toner produced by the production method according to this embodiment is easily caught by a cleaning blade and has excellent cleaning characteristics.
[0082] The softening temperature of the resin used as the resin microparticle raw material is preferably higher than the glass transition temperature of the binder resin contained in the core toner particles, and more preferably 60° C. or higher. This prevents the toner particles produced by the production method according to this embodiment from fusing together during storage, and suppresses the occurrence of bleed-out. Therefore, the toner produced by the production method according to this embodiment has excellent heat resistance and storage stability.
[0083] (3) Composite particle formation process P3 The composite particle forming step P3 is a step of forming composite particles by coating the surface of core toner particles with resin fine particles. For example, a method of forming composite particles can be used in which core toner particles and a resin fine particle emulsion are put into a Henschel mixer (model: FM20C, manufactured by Nippon Coke & Engineering Co., Ltd.), and the inside of the mixer tank is decompressed while stirring at a peripheral speed of the tip of the stirring blade of 10 m / s to 30 m / s. Composite particles that have been dried to a moisture content of less than 1% by mass can be obtained by mixing and drying under reduced pressure. The mixing ratio of the core toner particles and the resin fine particles is preferably such that the surface of the core toner particles is completely and thinly coated with the resin fine particles, and the blending ratio is 5 to 15 parts by mass of the resin fine particles per 100 parts by mass of the core toner particles. If the blending ratio of the resin fine particles is less than 5 parts by mass, it is difficult to sufficiently coat the core toner particles, and the storage stability becomes insufficient. If it exceeds 15 parts by mass, the coating amount will be excessive, making it difficult to make the shell layer thin, and low-temperature fixability will deteriorate.
[0084] In the composite particle forming step P3, it is preferable to mix the core toner particles with the silica particles having the hydrophobized surface to obtain a mixture before coating the core toner particle surfaces with the resin fine particles, and then mix and dry the mixture with the resin fine particle emulsion under reduced pressure. This makes it possible to produce capsule toner particles in which the silica particles exist at the interface between the core toner particles and the shell layer.
[0085] (4) Capsule toner particle formation process P4 The capsule toner particle forming step P4 is a step of forming capsule toner particles by applying a mechanical impact force to the composite particles to turn the resin fine particles into a film on the surface of the core toner particles. FIG. 3 is a front view showing a schematic configuration of a capsule toner particle manufacturing apparatus 201 used in the toner manufacturing method according to the present embodiment. FIG. 4 is a schematic cross-sectional view of the manufacturing apparatus 201 shown in FIG. 3 taken along the cutting line A200-A200. In the capsule toner particle forming step P4, for example, the capsule toner particle manufacturing apparatus 201 shown in FIG. 3 is used to form a shell layer on the surface of the core toner particles by impact force due to the synergistic effect of circulation and stirring in the capsule toner particle manufacturing apparatus 201 for the composite particles produced in the composite particle forming step P3. The capsule toner particle manufacturing apparatus 201 is a rotary stirring apparatus, and includes a powder flow path 202, a rotary stirring means 203 (rotary stirring section), a temperature adjustment jacket (not shown), a powder input section 206, and a powder recovery section 207. The rotary stirring means 203 and the powder flow path 202 constitute a circulation means.
[0086] The powder flow path 202 is composed of an agitation section 208 and a powder flow section 209. The agitation section 208 is a cylindrical container-like member having an internal space. Openings 210 and 211 are formed in the agitation section 208, which is a rotary agitation chamber. The opening 210 is formed at the approximate center of a surface 208a on one axial side of the agitation section 208, so as to penetrate the side wall including the surface 208a of the agitation section 208 in the thickness direction. The opening 211 is formed at a side surface 208b perpendicular to the surface 208a on the axial side of the agitation section 208, so as to penetrate the side wall including the side surface 208b of the agitation section 208 in the thickness direction. The powder flow section 209, which is a circulation pipe, is connected at one end to the opening 210 and at the other end to the opening 211. As a result, the internal space of the agitation section 208 and the internal space of the powder flow section 209 are connected to each other, and the powder flow path 202 is formed. The composite particles and gas flow through this powder flow passage 202. The powder flow passage 202 is provided so that the powder flow direction, which is the direction in which the composite particles flow, is constant.
[0087] The rotary stirring means 203 includes a rotating shaft member 212, a disk-shaped rotating plate 213, and a plurality of stirring blades 214. The rotating shaft member 212 is a cylindrical rod-shaped member having an axis that coincides with the axis of the stirring portion 208, and is inserted into a through hole 205 formed in a surface 208c on the other side of the axial direction of the stirring portion 208 so as to penetrate a side wall including the surface 208c in the thickness direction, and rotates about its axis by a motor (not shown). The rotating plate 213 is a disk-shaped member supported by the rotating shaft member 212 so that its axis coincides with the axis of the rotating shaft member 212, and rotates with the rotation of the rotating shaft member 212. The plurality of stirring blades 214 are supported by the peripheral portion of the rotating plate 213, and rotate with the rotation of the rotating plate 213.
[0088] In the capsule toner particle forming process P4, the peripheral speed of the outermost periphery of the rotary stirring means 203 is preferably set to 30 m / sec or more, more preferably 50 m / sec or more. The outermost periphery of the rotary stirring means 203 is the portion 203a of the rotary stirring means 203 that is the longest distance from the axis of the rotary shaft member 212 of the rotary stirring means 203 in a direction perpendicular to the direction in which the rotary shaft member 212 of the rotary stirring means 203 extends. By setting the peripheral speed of the outermost periphery of the rotary stirring means 203 during rotation to 30 m / sec or more, the composite particles can be dispersed in an air flow circulating through the annular flow path (powder flow path 202) with a flow speed of 30 m / sec or more. This allows the composite particles to flow in isolation. If the peripheral speed of the outermost periphery is less than 30 m / sec, it is difficult to flow the composite particles in isolation, and therefore it is difficult to uniformly coat the core toner particles with a resin film.
[0089] A temperature adjusting jacket (not shown) serving as a temperature adjusting means is provided on at least a part of the outside of the powder flow path 202, and a cooling medium or a heating medium is passed through the space inside the jacket to adjust the inside of the powder flow path 202 and the rotary stirring means 203 to a predetermined temperature. This makes it possible to control the temperature inside the powder flow path and the outside of the rotary stirring means to a temperature below which the core toner particles and the resin fine particles do not soften and deform.
[0090] In the toner of this embodiment, in the composite particle formation process P3, an emulsion of resin microparticles and core toner particles are mixed and dried under reduced pressure to form composite particles, and in the capsule toner particle formation process P4, the composite particles are dispersed in an airflow circulating through a ring-shaped flow path to form capsule toner particles. This makes it possible to reduce the generation of agglomerates of the resin microparticles and to efficiently use the resin microparticles to form the shell layer.
[0091] (5) External addition process P5 In the external addition step P5, the capsule toner particles and the external additive are mixed in a mixer to adhere the external additive to the capsule toner particle surface. As the mixer, a known mixer can be used, such as a Henschel Mixer (product name, manufactured by Nippon Coke and Engineering Co., Ltd.) or a Super Mixer (product name, manufactured by Kawata Co., Ltd.).
[0092] 4. Two-component developer When performing two-component development, the toner according to the present embodiment and the carrier are mixed to prepare a two-component developer. As a mixer for mixing the toner and the carrier, for example, a powder mixer such as a V-type mixer (product name: V-5, manufactured by Tokuju Machinery Co., Ltd.) can be used.
[0093] The blending ratio of the toner and the carrier is preferably within the range of 10:90 to 5:95 by mass ratio. As the carrier, a carrier that is normally used in the technical field can be used. In addition, a coated carrier can also be used. EXAMPLES
[0094] The toner and the method for producing the toner according to the present disclosure will be specifically described below based on examples and comparative examples. First, various measurement methods and evaluation methods will be described.
[0095] <Measurement and evaluation methods>
[0096] -Measurement of the melting points of the resins that form the core toner particles and the shell layer- Using a flow characteristic evaluation device (product name: Flow Tester CFT-100C, manufactured by Shimadzu Corporation), 1 g of sample was heated at a temperature increase rate of 6°C per minute and subjected to a load of 20 kgf / cm 2 (9.8×10 5 The sample was made to flow out of the die (nozzle diameter 1 mm, length 1 mm) at a pressure of 1 Pa. The temperature at which the sample started to flow out was taken as the flow initiation temperature (Tfb), and the temperature (softening point) at which half of the sample had flowed out was taken as the melting point (Tm).
[0097] -Measurement of average particle size of core toner particles and capsule toner particles- 20 mg of sample and 1 mL of sodium alkyl ether sulfate were added to 50 mL of electrolyte (product name: ISOTON-II, manufactured by Beckman Coulter, Inc.), and dispersed for 3 minutes at a frequency of 20 kHz using an ultrasonic disperser (product name: tabletop dual-frequency ultrasonic cleaner VS-D100, manufactured by AS ONE Corporation) to prepare a measurement sample. This measurement sample was measured using a particle size distribution measuring device (product name: Multisizer3, manufactured by Beckman Coulter, Inc.) under the conditions of an aperture diameter of 100 μm and a measurement particle count of 50,000, and the volume average particle size was obtained from the volume particle size distribution of the sample particles.
[0098] -Measurement of the median particle size of resin fine particles and silica particles- The median particle size of the resin microparticles and silica particles was measured twice using a dynamic light scattering particle size distribution measuring device (product name: Nanotrac Wave series, manufactured by Nikkiso Co., Ltd.), and the average value was used. The measurement conditions were a measurement time of 30 seconds, a sample particle refractive index of 1.49, a dispersion medium of water, and a dispersion medium refractive index of 1.33. The volumetric particle size distribution of the measurement sample was measured, and the particle size at which the cumulative volume from the small particle size side in the cumulative volume distribution became 50% was calculated as the median particle size [μm] of the measured particles.
[0099] - Calculation of the coverage rate of the core toner particle surface by silica particles - The coverage rate [%] of the core toner particle surface by silica particles was calculated from the median particle size and the surface area of the core toner particles, assuming that the particle size of all silica particles is the median particle size measured above as 100% when the entire surface of the core toner particles is covered with the closest-packed silica particles. Specifically, the coverage rate by silica particles was determined by dividing the total projected area of the silica particles obtained as follows by the total surface area of the core toner particles.
[0100] First, the projected area per particle is calculated from the particle size of the silica particles using the formula for the area of a circle. Next, the volume of the silica particles is calculated using the formula for the volume of a sphere, and the mass of the silica particles is calculated by multiplying this by the specific gravity. Furthermore, the number of silica particles attached to each core toner particle is calculated. This is calculated using the mass parts of silica particles added to the core toner particle and the mass per silica particle. The total projected area per core toner particle is calculated from this number of silica particles. The total surface area of the core toner particles is calculated based on the surface area per core toner particle calculated using the formula for the surface area of a sphere.
[0101] -Measurement of circularity of capsule toner particles- The circularity of the capsule toner particles was measured using an automatic particle shape and size analyzer (product name: FPIA-3000, manufactured by Sysmex Corporation). The specific measurement procedure is as follows.
[0102] In this measurement, the sample to be measured is fed into a sheath flow cell as a particle suspension. The flow of the particle suspension is transformed into a narrow flat stream as it passes through the sheath flow cell. This ensures that the maximum area of the particles is oriented towards the camera and that all particles are in focus. In this measurement, the CCD camera captures 60 images per second, which are analyzed in real time. The captured images are processed to extract the outline of each particle, and the projected area S and perimeter L of the particle image are measured. From this, the circle equivalent diameter and circularity are calculated.
[0103] The equivalent circle diameter is the diameter of a circle that has the same area as the projected area of a particle image, and circularity is defined as the perimeter of the circle calculated from the equivalent circle diameter divided by the perimeter of the projected particle image. If the area of the circle calculated from the equivalent circle diameter is S and the perimeter of the projected particle image is L, then circularity can be calculated using the following formula. Circularity = 2 × (π × S) 1 / 2 / L
[0104] The sample is dispersed using Particle Sheath "PSE-900A" (Malvern Instruments) as the sheath liquid, a 5% by mass aqueous dispersion of commercially available household detergent as the dispersant, and the autosampler device of the same device as the disperser, and introduced into the above-mentioned automatic particle shape and size analyzer, and 10,000 capsule toner particles are measured in total count in HPF measurement mode. The binarization threshold for particle analysis is set to 85%, and the average circularity of the capsule toner particles is calculated for the entire particle size range.
[0105] -Evaluation item 1: Evaluation of shell layer uniformity- The hardened product in which the capsule toner particles were embedded in a room temperature curing epoxy resin was cut into ultra-thin slices (about 200 nm) at multiple locations using a microtome equipped with diamond teeth, and stained with ruthenium. The slices were magnified 50,000 times using a transmission electron microscope (product name: H-8100, manufactured by Hitachi, Ltd.) to photograph the cross section of the capsule toner particle. Since the shell layer was stained to clearly show the film state and could be distinguished from the core toner particles, the film thickness of the shell layer covering the core toner particles was measured using image analysis software. The evaluation criteria for the uniformity of the shell layer are as follows:
[0106] Excellent: The shell layer has a thickness of less than 25 nm. The core toner particles are uniformly coated with a thin film. ◯ (Good): The thickness of the shell layer is 25 nm or more and less than 30 nm. The core toner particles are uniformly coated. △ (Fair): The shell layer thickness is 30 nm or more. The shell layer thickness is non-uniform. × (unacceptable): The thickness of the shell layer is non-uniform, and the core toner particles are exposed.
[0107] -Evaluation item 2: Evaluation of bleed-out- 5.0 g of toner was weighed as a measurement sample into a 50 mL glass tube (product name: SV-50A, manufactured by Nichiden Rika Glass Co., Ltd.), sealed with a cap, and stored under the following conditions 1 and 2, and then allowed to stand until it returned to room temperature. Condition 1: Store at room temperature (25°C) for 24 hours. Condition 2: Store in an incubator at 60℃±1℃ for 24 hours.
[0108] Next, the presence or absence of bleed-out was observed from the powder of each measurement sample using an electron microscope (S-4800 field emission scanning electron microscope, manufactured by Hitachi High-Technologies Corporation) and evaluated according to the following evaluation criteria.
[0109] ◎ (Excellent): Almost no bleed-out solids were observed. ◯ (Good): Bleeding out of solids was observed, but most of the solids were small, with particle sizes less than 1 μm. △ (Fair): Bleeding out solids are observed, and many medium-sized solids with particle sizes of 1 μm or more and less than 3 μm are observed. × (Not acceptable): A large amount of bled out solid matter was observed, and many large solid matter with a particle size of 3 μm or more was observed.
[0110] -Evaluation item 3: Evaluation of sublimation transfer efficiency- The toners of the examples and comparative examples and a coated carrier (genuine carrier for MX-5111FN manufactured by Sharp Corporation) were mixed for 20 minutes in a V-type mixer (product name: V-5, manufactured by Tokuju Machine Works Co., Ltd.) so that the toner concentration was 7% by mass, to prepare a two-component developer.
[0111] The two-component developer was filled into a commercially available copying machine (product name: MX-5111FN, manufactured by Sharp Corporation), and an A4 test document having a rectangular solid image of 20 mm length and 50 mm width was printed on an intermediate recording medium (product name: PPC paper SF-4AM3, manufactured by Sharp Corporation). At this time, the amount of toner attached to the solid image area was 0.5 mg / cm 2The temperature of the fixing roller was set to 135°C.
[0112] For the intermediate recording medium obtained by the above two-component development, the magenta dye density was measured using a spectrophotometer (product name: Spectroeye, manufactured by GretagMacbeth) for a portion of the intermediate recording medium corresponding to 100% of the print output before and after sublimation transfer by heat press processing. The sublimation transfer efficiency was calculated from the dye concentration attached to the intermediate recording medium before and after transfer using the following formula. Sublimation transfer efficiency = (dye concentration after transfer - dye concentration before transfer) / (dye concentration before transfer) x 100%
[0113] Based on the calculated sublimation transfer efficiency, evaluation was performed according to the following criteria. ◎ (Excellent): Sublimation transfer efficiency is 60% or more. ◯ (Good): Sublimation transfer efficiency is 45% or more and less than 60%. △(Fair): Sublimation transfer efficiency is 40% or more and less than 45%. × (Fail): Sublimation transfer efficiency is less than 40%.
[0114] -Evaluation item 4: Evaluation of color fastness to friction- The toners of the examples and comparative examples were loaded into a commercially available copying machine (product name: MX-5111FN, manufactured by Sharp Corporation) and images were formed on an intermediate recording medium. The intermediate recording medium and fabric were superimposed and then heat-pressed to dye the fabric by sublimation transfer. Specifically, the following three types of fabric were heat-pressed at 180°C for 35 seconds to dye the fabric by sublimation transfer, and three types of test fabric were prepared. Fabric 1: PET tromat (a thick polyester fabric with eyelets and bag stitching) Fabric 2: T / C blend (polyester and cotton blend) Fabric 3: Cotton Brode (a plain weave fabric with high density and luster)
[0115] For each test cloth obtained as described above, a color fastness test against rubbing was carried out using a type II (Gakushin type) testing machine according to the method specified in JIS L0849. Dry rubbing was tested according to the dry test specified in JIS L0849, and wet rubbing was tested according to the wet test specified in JIS L0849, and the results were evaluated according to the following criteria using the stain gray scale.
[0116] ◎ (Very good): Dye fastness is 4.5 grade or higher. ○ (Good): Dye fastness is grade 4. △(usable): Dye fastness is grade 3. × (unusable): Dye fastness is grade 2 or lower.
[0117] -comprehensive evaluation- The evaluation results of the above evaluation items 1 to 4 were scored as follows: "◎" = +2, "○" = +1, "△" = ±0, and "×" = -1. Based on the total score, a comprehensive evaluation was made according to the following criteria.
[0118] ◎ (Excellent): Total score is 6 to 8 (usable). ○ (Good): Total score is 4 to 5 (usable). △(Acceptable): Total score is 0 to 3 (usable). × (Not allowed): There is at least one assessment item with an "×" rating (not available).
[0119] <Toner manufacturing> [Example 1] -Core toner particle production process P1- The following toner raw materials were used to prepare the core toner particles. Binder resin: styrene acrylic resin (product name: CPR-190, manufactured by Mitsui Chemicals, Inc.) 85.0% by mass Sublimation dye: Disperse Yellow 54 (product name: Plast Yellow 8040, Arimoto Chemical Industry Co., Ltd.) 6.0% by mass Charge control agent: Salicylic acid compound (product name: Bontron E-84, Orient Chemical Industries Co., Ltd.) 1.0% by mass Release agent: refined carnauba wax (product name: TOWAX-131, manufactured by Toa Kasei Co., Ltd.) 8.0% by mass
[0120] The above toner raw materials were premixed for 5 minutes using an air flow mixer (Henschel mixer, model: FM20C, manufactured by Nippon Coke & Engineering Co., Ltd.) [mixing process]. Next, using a twin-screw extruder (model: PCM30, manufactured by Ikegai Co., Ltd.), the materials were melt-kneaded under the conditions of a cylinder setting temperature of 110°C, a barrel rotation speed of 200 rpm, and a raw material supply rate of 15 kg / h to obtain a molten kneaded product [kneading process].
[0121] The resulting molten kneaded product was cooled in a drum flaker and then coarsely pulverized using a cutting mill (model: VM-16, manufactured by Orient Crusher Co., Ltd.) to obtain a coarsely pulverized product [coarse pulverization step].
[0122] Next, the obtained coarsely pulverized product was finely pulverized using a jet pulverizer (model: IDS-2, manufactured by Nippon Pneumatic Mfg. Co., Ltd.) to obtain a finely pulverized product [finely pulverizing step].
[0123] The resulting finely pulverized product was classified using an elbow jet classifier (model: EJ-LABO, manufactured by Nittetsu Mining Co., Ltd.) to obtain core toner particles having an average primary particle size of 6.0 μm [classification step].
[0124] -Resin fine particle preparation process P2- In a reaction vessel equipped with a stirring heater, a thermometer, a nitrogen inlet tube and a cooling tube, 168 parts by mass of deionized water was charged and heated to 80° C. To this, a monomer mixture (pre-emulsion) consisting of 252 parts by mass of deionized water, 65 parts by mass of styrene, 27 parts by mass of n-butyl acrylate and 8 parts by mass of acrylic acid, and 56 parts by mass of an aqueous initiator solution consisting of 1 part by mass of ammonium peroxodisulfate, 0.2 parts by mass of n-dodecyl mercaptan and 62 parts by mass of deionized water were simultaneously dropped over 110 minutes, and after stirring for another 60 minutes, the reaction was terminated to obtain an emulsion (solid content 30% by mass) of almost monodispersed resin fine particles having a glass transition point of 80° C., a softening point of 145° C., a weight average molecular weight (Mw) of 310000 and a particle size of 0.150 μm.
[0125] -Composite particle formation process P3- 100 parts by mass of core toner particles and 15 parts by mass of resin fine particles were put into an air flow mixer (Henschel mixer, model: FM20C, manufactured by Nippon Coke & Engineering Co., Ltd.) (50 parts by mass were put in for 100 parts by mass of core particles in an emulsion state), and stirring and mixing was started with the peripheral speed of the tip of the stirring blade set to 15 m / s, while at the same time the pressure inside the mixer tank was reduced to a vacuum of 0.01 MPa. By stirring and mixing for 10 minutes under reduced pressure, composite particles with resin fine particles uniformly attached to the surface of the core toner particles were obtained. The moisture content of the composite particles was 0.1% by mass.
[0126] - Capsule toner particle formation process P4 - The composite particles were placed in a hybridization system (product name: NHS-3 type, manufactured by Nara Machinery Works, Ltd.) similar to the device shown in Figure 3, and the peripheral speed at the outermost periphery of the rotating stirring means was set to 50 m / s, and the particles were stirred and mixed for 10 minutes, thereby forming a film of resin fine particles on the surface of the core toner particles, and capsule toner particles were obtained.
[0127] -External addition process P5- 100 parts by mass of the encapsulated toner particles obtained in the encapsulated toner particle formation process and 2 parts by mass of hydrophobic silica particles having a primary particle median particle size of 12 nm as an external additive were charged into an air flow mixer (Henschel mixer, model: FM20C, manufactured by Nippon Coke and Engineering Co., Ltd.), and stirred and mixed for 3 minutes with a circumferential speed of the rotating shaft member set to 30 m / s, thereby obtaining the toner of Example 1.
[0128] [Examples 2 to 18, Comparative Examples 1 to 6] A toner was obtained in the same manner as in Example 1, except that the molecular weight distribution of the resin to be blended in the core toner particles and the shell layer was controlled to adjust the melting point as shown in Table 1, and the median particle size and addition amount of the resin fine particles forming the shell layer were set to the values shown in Table 1.
[0129] [Examples 19 to 50] A toner was obtained in the same manner as in Example 1, except that the composite particle formation process was changed as follows to produce capsule toner particles in which silica particles were present at the interface between the core toner particle and the shell layer, and the median particle size and addition amount of the resin microparticles forming the shell layer, and the addition amount of the silica particles were set to the values shown in Table 2.
[0130] -Composite particle formation process P3- In an air flow mixer (Henschel mixer, model: FM20C, manufactured by Nippon Coke & Engineering Co., Ltd.), 100 parts by mass of core toner particles and hydrophobized silica particles shown in Table 2 were put in, and the peripheral speed of the tip of the stirring blade was set to 15 m / s to stir and mix and thoroughly disperse. Next, 20 parts by mass of resin fine particles were put in (67 parts by mass in emulsion state, per 100 parts by mass of core toner particles), and the peripheral speed of the tip of the stirring blade was set to 15 m / s to start stirring and mixing, while simultaneously reducing the pressure inside the mixer tank to a vacuum degree of 0.01 MPa. By stirring and mixing for 10 minutes under reduced pressure, composite particles in which resin fine particles were uniformly attached to the surface of the core toner particles were obtained. The moisture content of the composite particles was 0.1% by mass.
[0131] [Table 1]
[0132] [Table 2]
[0133] [Table 3]
[0134] [Table 4]
[0135] Tables 1 and 2 show the physical properties, types and amounts of toner raw materials in the examples and comparative examples, and Tables 3 and 4 show the evaluation results of the examples and comparative examples. In Tables 1 and 2, the "amount of resin particles added" and the "amount of silica particles added" are the amounts added per 100 parts by mass of core toner particles. In the "type of silica particles" in Table 2, "R972", "RY300S", "NX130", "NAX50", "NY50", "RX50", "RY50", and "RY40S" are product names manufactured by Nippon Aerosil Co., Ltd.
[0136] As is clear from the evaluation results in Tables 3 and 4, the toners of Examples 1 to 50, which are toners having encapsulated toner particles containing a sublimation dye, the encapsulated toner particles having a core toner particle and a shell layer covering the surface of the core toner particle, the melting point of the resin forming the core toner particle being 105°C or more and 135°C or less, and the melting point of the resin forming the shell layer being 140°C or more and 160°C or less, had excellent uniformity of the shell layer, were able to suppress bleed-out of the sublimation dye in dyeing by sublimation transfer method, and were excellent in uniformity of the shell layer, sublimation transfer efficiency, and color fastness to friction.
[0137] In contrast, Comparative Examples 1 to 6, which did not satisfy these requirements, were inferior to the Examples in at least one of the evaluation items of shell layer uniformity, bleed-out, sublimation transfer efficiency, and color fastness to rubbing.
[0138] Comparative Examples 1 and 2 are examples in which a resin with a low melting point of 90° C. was used to form the core toner particles, and as a result, a phenomenon occurred in which the resin fine particles forming the shell layer were locally embedded in the core toner particles during the capsule toner particle formation process (encapsulation process). When the melting point of the resin forming the shell layer was increased from 110° C. to 140° C. (Comparative Example 2), this phenomenon became more pronounced, and a decrease in circularity was confirmed.
[0139] In Comparative Example 3, in which there was no difference in melting point between the resin forming the core toner particles and the resin forming the shell layer, the viscosity of both resins decreased almost simultaneously, so the uniformity of the shell layer could not be maintained.
[0140] Comparative Examples 4 to 6 are examples in which a resin with a high melting point of 140°C was used to form the core toner particles. As a result, it was confirmed that the shape of the shell layer after the capsule toner particle formation process (after the encapsulation process) was improved, but when dyeing was performed by the sublimation transfer method, a decrease in the sublimation transfer efficiency was confirmed. This is because the increase in the melting point of the resin that forms the core toner particles reduced the efficiency of the dye seeping out. If the temperature of the fixing roller is increased to solve this problem, there is a problem that offset occurs and there is also a problem that an increase in power consumption is expected.
[0141] Examples 7 to 18 are examples in which the median particle diameter and the amount of resin fine particles added were changed. When the median particle diameter of the resin fine particles was examined using Examples 9, 11, 14, and 17 in which the amount of resin fine particles added was 20 parts by mass relative to 100 parts by mass of the core toner particles, it was found that Examples 9, 11, and 14 in which the median particle diameter was 0.1 μm or more and 0.2 μm or less were superior in the evaluation of the uniformity of the shell layer to Example 17 in which the median particle diameter exceeded the above upper limit.
[0142] When the amount of resin microparticles added per 100 parts by mass of core toner particles (in other words, the proportion of the shell layer) is examined using Examples 10 to 12 in which the median particle size of the resin microparticles is 0.15 μm, it is found that Example 11, in which the amount of resin microparticles added is 12 parts by mass or more and 23 parts by mass or less, has a superior evaluation of color fastness to friction than Examples 10 and 12 in which the amount added is outside the above range.
[0143] Examples 19 to 50 are examples in which silica particles having hydrophobized surfaces are attached to the surfaces of core toner particles. In other words, in these capsule toner particles, silica particles are present at the interface between the core toner particle and the shell layer.
[0144] When the surface treatment agents for silica particles were examined using Examples 19 to 24, it was found that Examples 21 and 22, which were hydrophobically treated with PMDS (dimethylpolysiloxane), were superior in terms of sublimation transfer efficiency to Examples 18, 19, 23, and 24, which were hydrophobically treated with DDS (dimethyldichlorosilane) or HMDS (hexamethyldisilazane).
[0145] When the median particle size of the silica particles adhered to the surface of the core toner particle is examined using Examples 18, 24, 28, and 30, it is found that Examples 24 and 28, in which the median particle size of the silica particles is 20 nm or more and 50 nm or less, have a sublimation transfer efficiency of over 70%, and are superior to Examples 18 and 30, in which the median particle size of the silica particles is outside the above range.
[0146] Examples 35 to 50 are examples in which the amount of silica particles added to adhere to the core toner particle surface is changed. When the coverage of the core toner particle surface by silica particles is examined using, for example, Examples 35, 37, 39, and 41, it is found that Examples 37 and 39, in which the coverage is 45% or more and 75% or less, are superior in various evaluations to Example 35, in which the coverage is below the lower limit. It is also found that Examples 37 and 39 are superior in evaluations of sublimation transfer efficiency and color fastness to friction to Example 41, in which the coverage exceeds the upper limit.
[0147] The embodiments disclosed herein are illustrative in all respects and are not intended to be limiting. Therefore, the technical scope of the present disclosure is not interpreted solely by the above-described embodiments, but is defined based on the claims. Also, all modifications within the scope and meaning equivalent to the claims are included. [Explanation of symbols]
[0148] 1. Binder resin (styrene acrylic resin) 2. Shell Layer 3 Sublimable dye T Capsule Toner T′ Unencapsulated toner 201 Capsule toner particle manufacturing equipment 202 Powder flow path 203 Rotary stirring means (rotary stirring unit) 203a Rotary stirring means part 205 Through hole 206 Powder input section 207 Powder Recovery Section 208 Mixing section 208a One side surface of the stirring part in the axial direction 208b Side 208c: the surface on the other side of the stirring portion in the axial direction 209 Powder flow section 210 Opening 211 Opening 212 Rotating shaft members 213 Turntable 214 Mixing blade
Claims
1. A toner having capsule toner particles containing a dye having sublimation properties, The capsule toner particle includes a core toner particle and a shell layer that covers a surface of the core toner particle, The melting point of the resin forming the core toner particle is 105° C. or more and 135° C. or less, The toner according to the present invention is characterized in that the melting point of the resin forming the shell layer is 140° C. or more and 160° C. or less.
2. 2. The toner according to claim 1, The toner according to claim 1, wherein the ratio of the shell layer in the capsule toner particles is 12 parts by mass or more and 23 parts by mass or less with respect to 100 parts by mass of the core toner particles.
3. The toner according to claim 1 or 2, The toner, wherein the circularity of the capsule toner particles is 0.950 or more.
4. The toner according to claim 1 or 2, The toner, characterized in that silica particles having hydrophobic surfaces are present at the interface between the core toner particles and the shell layer.
5. The toner according to claim 4, The toner is characterized in that the median particle diameter of the silica particles is 20 nm or more and 50 nm or less.
6. The toner according to claim 4, The toner is characterized in that the surfaces of the silica particles are hydrophobized with dimethylpolysiloxane.
7. The toner according to claim 4, The toner according to claim 1, wherein the coverage of the surface of the core toner particle with the silica particles is 45% or more and 75% or less.
8. A method for producing the toner according to claim 1 or 2, comprising the steps of: A core toner particle preparation step of preparing core toner particles; a resin fine particle preparation step of preparing resin fine particles that form a shell layer; a composite particle forming step of forming composite particles by coating the surfaces of the core toner particles with the resin fine particles; and forming a capsule toner particle by forming a film of the resin fine particles on the surface of the core toner particle.
9. A method for producing the toner according to claim 8, comprising the steps of: The method for producing a toner, wherein the fine resin particles prepared in the fine resin particle preparation step have a median particle size of 0.1 μm or more and 0.2 μm or less.
10. A method for producing the toner according to claim 8, comprising the steps of: In the composite particle forming step, the emulsion of the resin fine particles and the core toner particles are mixed and dried under reduced pressure to form the composite particles; The toner manufacturing method according to the present invention, wherein in the encapsulated toner particle forming step, the encapsulated toner particles are formed by dispersing the composite particles in an air current circulating through an annular flow path.
11. A method for producing the toner according to claim 4, comprising the steps of: A core toner particle preparation step of preparing core toner particles; a resin fine particle preparation step of preparing resin fine particles that form a shell layer; a composite particle forming step of forming composite particles by coating the surfaces of the core toner particles with the resin fine particles; a capsule toner particle forming step of forming a capsule toner particle by forming the resin fine particles into a film on the surface of the core toner particle, the composite particle forming step includes a step of mixing silica particles having hydrophobized surfaces with the core toner particles to obtain a mixture, and a step of mixing and drying the emulsion of resin fine particles with the mixture under reduced pressure to form the composite particles, The toner manufacturing method according to the present invention, wherein in the encapsulated toner particle forming step, the encapsulated toner particles are formed by dispersing the composite particles in an air current circulating through an annular flow path.
Citation Information
Patent Citations
Toner for sublimation transfer, method for producing the same, and sublimation transfer dyeing method