Aqueous ink and laminate

A water-based ink with a specific (meth)acrylic resin and aziridine curing agent ratio addresses the shortcomings of conventional inks, providing enhanced adhesion, blocking resistance, and heat resistance for flexible packaging films.

JP2024151995AInactive Publication Date: 2024-10-25DIC GRAPHICS

Patent Information

Application Number
JP2023065869
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional water-based inks fail to meet the requirements of excellent adhesion, blocking resistance, heat resistance, and water friction resistance, particularly in applications involving flexible packaging films.

Method used

A water-based ink formulation containing a binder resin, specifically a (meth)acrylic resin with a glass transition temperature between -10°C and 60°C, and an aziridine curing agent in a ratio of 2.0 to 11.0 parts by mass per 100 parts of the binder resin's nonvolatile content, enhances film properties.

Benefits of technology

The formulation results in a film with improved adhesion, blocking resistance, heat resistance, and water friction resistance, suitable for applications requiring durability and resistance to external contact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151995000001
    Figure 2024151995000001
Patent Text Reader

Abstract

To provide an aqueous ink from which a film excellent in adhesion, blocking resistance, heat resistance, wet friction resistance, and alcohol resistance can be obtained.SOLUTION: The aqueous ink contains a binder resin, an aziridine-based curing agent, and an aqueous solvent. A (meth)acrylic resin (A) accounts for 50 mass% or more of the binder resin. The (meth)acrylic resin (A) has a glass transition temperature of -10°C or higher and 60°C or lower. The amount of a nonvolatile component of the aziridine-based curing agent is 2.0 pts.mass or more and 11.0 pts.mass or less based on 100 pts.mass of a nonvolatile component of the binder resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a water-based ink and a laminate. [Background technology]

[0002] Gravure inks and flexographic inks are widely used to impart beauty and functionality to printed flexible packaging films.

[0003] Specifically, for example, when packaging products, these gravure inks and flexographic inks are printed on the front side (the side that does not come into contact with the product being packaged) of the base plastic film for decoration and surface protection, and printed materials with a simple configuration (called surface printing method) are used in which the back side (the side that comes into contact with the product being packaged) is not printed.

[0004] Furthermore, in the case of labels wrapped around the body of PET bottles or shrink labels, a top coat varnish is generally printed on the outer surface to provide scratch protection for the film, and a decorative printing layer and a varnish layer to provide blocking protection for the PET bottle are provided on the inner surface. The ink and top coat varnish used in the surface printing described above are directly exposed to the outside and come into direct contact with other components, and therefore require film properties that are strong enough to withstand handling of the product, etc.

[0005] In recent years, based on the perspective of sustainability against the backdrop of worsening air pollution by VOCs, global warming, and other global-scale issues, and in addition to considerations of occupational safety and health, flammability, and explosiveness, and in response to the movement to shift away from petroleum resources, so-called water-based inks in which organic solvents in inks are replaced with water are expected to become more widespread. Under these circumstances, various studies are being conducted on water-based inks that can also be used as inks for surface printing and top coat varnishes (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2020 / 213413 Summary of the Invention [Problem to be solved by the invention]

[0007] Here, in addition to adhesion to the substrate, various physical properties (heat resistance, water abrasion resistance, alcohol resistance, and blocking resistance between films) are required for the ink film. However, conventional water-based inks have room for improvement in terms of satisfying all of these requirements.

[0008] Therefore, an object of the present invention is to provide a water-based ink that can provide a film that has excellent adhesion, blocking resistance, heat resistance, water-rubbing resistance, and alcohol resistance. Another object of the present invention is to provide a laminate having, as a coating, an ink layer that has excellent adhesion, blocking resistance, heat resistance, water-rub resistance, and alcohol resistance. [Means for solving the problem]

[0009] As a result of extensive research, the present inventors have found that using an aziridine-based curing agent in a predetermined ratio, calculated on a non-volatile basis, for a binder resin containing a predetermined (meth)acrylic resin is effective in solving the above problems. That is, the gist of the present invention is as follows.

[0010] [1] A binder resin, an aziridine-based curing agent, and an aqueous solvent are contained, the binder resin contains 50 mass % or more of a (meth)acrylic resin (A), the (meth)acrylic resin (A) has a glass transition temperature of −10° C. or higher and 60° C. or lower; 1. A water-based ink, characterized in that the amount of non-volatile content of the aziridine-based curing agent relative to 100 parts by mass of non-volatile content of the binder resin is 2.0 parts by mass or more and 11.0 parts by mass or less.

[0011] [2] The water-based ink according to [1], wherein the acid value of the (meth)acrylic resin (A) is 20 mgKOH / g or more and 80 mgKOH / g or less.

[0012] [3] The water-based ink according to [1] or [2], wherein the (meth)acrylic resin (A) is a styrene-acrylic resin.

[0013] [4] The water-based ink according to any one of [1] to [3], which is a top coat varnish that does not contain a pigment.

[0014] [5] The water-based ink according to any one of [1] to [4], which is used for flexographic printing or gravure printing.

[0015] [6] A laminate comprising a substrate and an ink layer provided on the substrate, wherein the ink layer is a printed layer of the water-based ink according to any one of [1] to [5].

[0016] [7] The laminate according to [6], further comprising an intermediate ink layer between the substrate and the ink layer.

[0017] [8] The laminate according to [6] or [7], which is used as a heat-shrinkable film. [Effects of the Invention]

[0018] According to the present invention, it is possible to provide a water-based ink that can give a film that is excellent in adhesion, blocking resistance, heat resistance, water-rubbing resistance, and alcohol resistance. Furthermore, according to the present invention, it is possible to provide a laminate having an ink layer as a coating that has excellent adhesion, blocking resistance, heat resistance, water friction resistance, and alcohol resistance. DETAILED DESCRIPTION OF THE INVENTION

[0019] The following describes in detail an embodiment of the present invention (hereinafter sometimes referred to as the "present embodiment"); however, the present invention is not limited to the following description and can be implemented in various modifications within the scope of its gist.

[0020] (Water-based ink) The water-based ink of this embodiment contains a binder resin, an aziridine-based curing agent, and an aqueous solvent, wherein 50 mass % or more of the binder resin is a (meth)acrylic resin (A), the (meth)acrylic resin (A) has a glass transition temperature of −10° C. or more and 60° C. or less, and the amount of non-volatile content of the aziridine-based curing agent per 100 mass parts of non-volatile content of the binder resin is 2.0 mass parts or more and 11.0 mass parts or less.

[0021] Regarding curing agents, conventionally known curing agents that can be used in aqueous media include epoxy-based curing agents, carbodiimide-based curing agents, oxazoline-based curing agents, etc. However, it has surprisingly been discovered that in the aqueous ink of this embodiment, by using an aziridine-based curing agent in a predetermined ratio converted to nonvolatile content for a binder resin containing a predetermined (meth)acrylic resin, it is possible to obtain a film that is excellent in adhesion, blocking resistance, heat resistance, water-rubbing resistance, and alcohol resistance (hereinafter sometimes referred to as the "five properties").

[0022] In this specification, "(meth)acrylic" means acrylic and / or methacrylic, and "(meth)acrylate" means acrylate and / or methacrylate. In this specification, a (meth)acrylic resin having a glass transition temperature of −10° C. or higher and 60° C. or lower will be referred to as “(meth)acrylic resin (A)”.

[0023] The various components that can be contained in the water-based ink of this embodiment will be described below.

[0024] <Binder resin> The water-based ink of this embodiment contains a binder resin, and 50% by mass or more of the binder resin must be a (meth)acrylic resin (A). This (meth)acrylic resin (A) may be a single type or a combination of two or more types. If the proportion of the (meth)acrylic resin (A) in the binder resin is less than 50% by mass, it may not be possible to achieve all five properties, and in particular, it may not be possible to achieve improved blocking resistance and / or heat resistance.

[0025] The binder resin may contain a resin other than the (meth)acrylic resin (A). However, from the viewpoint of more effectively improving the five properties, the proportion of the (meth)acrylic resin (A) in the binder resin is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and also preferably 100% by mass (i.e., the binder resin consists solely of the (meth)acrylic resin (A)).

[0026] Here, the (meth)acrylic resin refers to a resin having a structural unit derived from a (meth)acrylic acid ester monomer, and examples thereof include acrylic resin, styrene-acrylic resin, polyester-acrylic resin, urethane-acrylic resin, vinyl chloride-vinyl acetate copolymer-acrylic resin, silicone-acrylic resin, acrylamide resin, and epoxy-acrylic resin. In other words, a (meth)acrylic resin refers to a resin obtained by (co)polymerizing a (meth)acrylic acid ester as an essential monomer together with other polymerizable unsaturated group-containing compounds as needed.

[0027] Examples of the (meth)acrylic acid ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-pentafluoropropyl (meth)acrylate, and perfluoro (meth)acrylate. Examples of the (meth)acrylate monomer include cyclohexyl (meth)acrylate, glycidyl (meth)acrylate, allyl glycidyl ether, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, (meth)acrylamide, N-monoalkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide, N-methylol (meth)acrylamide, N-isopropoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-isobutoxymethyl (meth)acrylamide, 2-aziridinylethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, acrolein, diacetone (meth)acrylamide, and acetoacetoxyethyl (meth)acrylate. The (meth)acrylic acid ester monomer may be used alone or in combination of two or more.

[0028] Examples of the polymerizable unsaturated group-containing compound include vinyl monomers such as vinyl acetate, vinyl propionate, vinyl versatate, methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, (meth)acrylonitrile, styrene, α-methylstyrene, divinylstyrene, isoprene, chloroprene, butadiene, ethylene, tetrafluoroethylene, vinylidene fluoride, and N-vinylpyrrolidone. The polymerizable unsaturated group-containing compound may be used alone or in combination of two or more.

[0029] The (meth)acrylic resin may also be reacted with a self-crosslinking component. That is, the (meth)acrylic resin may be a self-crosslinking type. Examples of the self-crosslinking component include an isocyanate compound, an epoxy compound, an amine compound, a melamine compound, a hydrazine compound, an aldehyde compound, and an oxazoline compound.

[0030] The (meth)acrylic resin can be produced, for example, by polymerizing various monomers in the presence of a polymerization initiator at a temperature range of 50°C to 180°C, more preferably 80°C to 150°C. Examples of the polymerization method include bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization. In addition, when the (meth)acrylic resin is a copolymer, it may be a random copolymer, block copolymer, graft copolymer, or the like, from the viewpoint of the polymerization mode.

[0031] The (meth)acrylic resin may be an emulsion that forms a core-shell type. The core-shell type emulsion refers to a state in which a first polymer is dispersed in an aqueous medium by a second polymer, and usually, the second polymer is present at the outermost part of the resin particles to form a shell portion, and a part or all of the first polymer forms a core portion.

[0032] <(Meth)acrylic resin (A)> The (meth)acrylic resin (A) used in this embodiment is a (meth)acrylic resin having a glass transition temperature (Tg) of -10°C or higher and 60°C or lower. If the glass transition temperature is lower than -10°C, it may not be possible to achieve all five properties, particularly, blocking resistance and / or heat resistance may be deteriorated. If the glass transition temperature is higher than 60°C, it may not be possible to achieve all five properties, particularly, adhesion may be deteriorated. From the viewpoint of more effectively improving the five properties, the glass transition temperature (Tg) of the (meth)acrylic resin (A) is more preferably 10°C or higher, even more preferably 30°C or higher, even more preferably 35°C or higher, and more preferably 55°C or lower.

[0033] The glass transition temperature (Tg) refers to the so-called calculated glass transition temperature, and refers to a value calculated by the following method. (Formula 1) 1 / Tg(K)=(W1 / T1)+(W2 / T2)+...(Wn / Tn) (Equation 2) Tg(°C)=Tg(K)-273 In Equation 1, W1, W2, ..., Wn represent the mass % of each monomer relative to the total mass of the monomers used in producing the polymer, and T1, T2, ..., Tn represent the glass transition temperature (K) of the homopolymer of each monomer. The values ​​of T1, T2, ..., Tn are those listed in Polymer Handbook (Fourth Edition, edited by J. Brandrup, EH Immergut, and EA Grulke). For the homopolymers of monomers whose glass transition temperatures are not listed in the Polymer Handbook, the glass transition temperatures were measured using a differential scanning calorimeter "DSCQ-100" (manufactured by TA Instrument) according to JIS K7121. Specifically, the polymer was vacuum-suctioned to completely remove the solvent, and the heat change was measured in the range of -100°C to +200°C at a temperature increase rate of 20°C / min. The glass transition temperature was determined as the point where a line equidistant in the vertical direction from the extended line of each baseline intersected with the curve of the stepwise change portion of the glass transition.

[0034] The acid value (also referred to as "AV") of the (meth)acrylic resin (A) is preferably 20 mgKOH / g or more and 80 mgKOH / g or less. If the acid value of the (meth)acrylic resin (A) is 20 mgKOH / g or more, the five properties, particularly alcohol resistance, can be more effectively improved. If the acid value is 80 mgKOH / g or less, the five properties, particularly at least one of blocking resistance, water friction resistance, and alcohol resistance, can be more effectively improved. From the same viewpoint, the acid value of the (meth)acrylic resin (A) is more preferably 30 mgKOH / g or more, more preferably 78 mgKOH / g or less, and even more preferably 60 mgKOH / g or less. The acid value indicates the number of milligrams of potassium hydroxide required to neutralize the acidic components contained in 1 g of resin.

[0035] In this embodiment, the (meth)acrylic resin (A) is preferably an acrylic resin (i.e., a resin obtained by polymerizing substantially only (meth)acrylic acid ester monomers) or a styrene-acrylic resin (i.e., a resin obtained by copolymerizing a styrene monomer and a (meth)acrylic acid ester monomer), and more preferably a styrene-acrylic resin. In this case, the five properties can be more effectively improved.

[0036] <Aziridine-based curing agent> The aqueous ink of this embodiment contains an aziridine-based curing agent. The aziridine-based curing agent is a compound having an aziridine group, and more specific examples include trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, trimethylolpropane-tri-β-(2-methylaziridine)propionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), and N,N'-toluene-2,4-bis(1-aziridinecarboxamide). The aziridine-based curing agent may be used alone or in combination of two or more.

[0037] Commercially available aziridine curing agents can be used, such as "PZ-33" manufactured by Nippon Shokubai Co., Ltd., "DZ-22E" manufactured by Nippon Shokubai Co., Ltd., "XL-706" manufactured by Stahl, and "SU-125F" manufactured by Meisei Chemical Industry Co., Ltd.

[0038] In the aqueous ink of this embodiment, the amount of the nonvolatile content of the aziridine curing agent relative to 100 parts by mass of the nonvolatile content of the binder resin must be 2.0 parts by mass or more and 11.0 parts by mass or less. If the amount is less than 2.0 parts by mass, it may be difficult to achieve all five properties, particularly improvement in at least one of heat resistance, water-rub resistance, and alcohol resistance. If the amount is more than 11.0 parts by mass, it may be difficult to achieve all five properties, particularly improvement in at least one of blocking resistance, water-rub resistance, and alcohol resistance. From the same viewpoint as above, the amount of the nonvolatile content of the aziridine curing agent relative to 100 parts by mass of the nonvolatile content of the binder resin is preferably 5.0 parts by mass or more, more preferably 7.0 parts by mass or more, and preferably 10.0 parts by mass or less, more preferably 9.0 parts by mass or less.

[0039] In addition, when used to prepare water-based inks, binder resins and aziridine-based curing agents are often dispersed in a solvent. Therefore, in order to calculate the mass ratio of the nonvolatile content mentioned above, it is important to know the NV value (Nonvolatile Content) of each binder resin and aziridine-based curing agent. The "non-volatile content" (NV) is also generally referred to as the "solid content."

[0040] <Water-based solvent> The aqueous solvent used in this embodiment may be water alone or an organic solvent miscible with water. Examples of the organic solvent include alcohols such as methyl alcohol, ethyl alcohol, isopropyl alcohol, and n-propyl alcohol; polyhydric alcohols such as propylene glycol and glycerin; and ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, and ethyl carbitol. The aqueous solvent may be used alone or in combination of two or more.

[0041] <Pigments> The aqueous ink of this embodiment can contain various pigments in addition to those described above. Examples of pigments include inorganic pigments and organic pigments from the viewpoint of material, and black pigments, indigo pigments, green pigments, red pigments, purple pigments, yellow pigments, orange pigments, and brown pigments from the viewpoint of coloring. When the aqueous ink contains these pigments, it can be used as an ink for so-called black-and-white printing or color printing. However, since the aqueous ink of this embodiment can exhibit strong film properties that can withstand external contact, it is preferable that the aqueous ink is a top coat varnish that does not contain a pigment (i.e., a colorless, transparent ink that is solid-printed on the outermost surface of a color print layer to protect the color print layer).

[0042] <Surfactant> The aqueous ink of this embodiment may further contain a surfactant in addition to the above. The surfactant is preferably an acetylene-based surfactant or an alcohol alkoxylate-based surfactant. These surfactants may be used alone or in combination of two or more.

[0043] Specific examples of acetylene surfactants include 2,5-dimethyl-3-hexyne-2,5-diol, 3,6-dimethyl-4-octyne-3,6-diol, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,5-dimethyl-1-hexyne-3-ol, 3-methyl-1-butyne-3-ol, 3-methyl-1-pentyne-3-ol, 3-hexyne-2,5-diol, 2-butyne-1,4-diol, etc. These acetylene surfactants may be used alone or in combination of two or more.

[0044] Commercially available acetylene surfactants include commercially available alkylene oxide unmodified acetylene glycol surfactants and commercially available alkylene oxide modified acetylene glycol surfactants. Commercially available alkylene oxide unmodified acetylene glycol surfactants include Surfynol 61, 82, and 104 (all manufactured by Air Products Co., Ltd.). Commercially available alkylene oxide-modified acetylene glycol surfactants include Surfynol 420, 440, 465, 485, TG, 2502, Dynol 604, and 607 (all manufactured by Air Products Co., Ltd.); Surfynol SE, MD-20, Olfine E1004, E1010, PD-004, EXP4300, PD-501, PD-502, and SPC (all manufactured by Nissin Chemical Industry Co., Ltd.); and Acetylenol EH, E40, E60, E81, E100, and E200 (all manufactured by Kawaken Fine Chemicals Co., Ltd.). Among these, alkylene oxide-modified acetylene glycol surfactants are preferred as the acetylene surfactants.

[0045] Specific examples of the alcohol alkoxylate surfactant include alcohol ethoxylate and alcohol polyethoxylate. Commercially available alcohol alkoxylate surfactants include "BYK-DYNWET800" (manufactured by BYK). These alcohol alkoxylate surfactants may be used singly or in combination of two or more.

[0046] In addition to the surfactants mentioned above, acrylic polymer surfactants (e.g., "Polyflow WS-314" manufactured by Kyoeisha Chemical Co., Ltd.) and modified silicone surfactants (e.g., "Polyflow KL-401" manufactured by Kyoeisha Chemical Co., Ltd.) may also be used as needed.

[0047] When the aqueous ink of this embodiment contains a surfactant, the total proportion of the surfactant in the total amount of the aqueous ink is preferably 0.1% by mass or more and 3.0% by mass or less. If the proportion is 0.1% by mass or more, the wettability of the substrate can be improved, and the effect of maintaining adhesion to the substrate can be obtained. Furthermore, if the proportion is 3.0% by mass or less, the abrasion resistance, water abrasion resistance, and scratch resistance can be maintained well. From the same viewpoint, the proportion is more preferably 1.0% by mass or less.

[0048] <Wax> The water-based ink of this embodiment may further contain a wax in addition to the above. The wax is preferably a hydrocarbon wax. Specific examples of the wax include liquid paraffin, natural paraffin, synthetic paraffin, microcrystalline wax, polyethylene wax, fluorocarbon wax, ethylene-propylene copolymer wax, tetrafluoroethylene resin wax, and Fischer-Tropsch wax. These waxes may be used alone or in combination of two or more. Among these, polyethylene wax is preferred as the wax.

[0049] When the aqueous ink of this embodiment contains wax, the total proportion of wax in the total amount of the aqueous ink is preferably 0.5% by mass or more and 5.0% by mass or less. If the proportion is 0.5% by mass or more, the effect of maintaining water abrasion resistance can be obtained. Furthermore, if the proportion is 5.0% by mass or less, adhesion to the substrate, water abrasion resistance, and blocking resistance can be maintained well.

[0050] <Other ingredients> In addition to the above, the water-based ink of this embodiment may contain appropriate amounts of other components, such as a general-purpose resin other than the above-mentioned binder resin, an extender pigment, a lubricant (oleic acid amide, stearic acid amide, erucic acid amide, etc.), a pigment dispersant, a leveling agent, an antifoaming agent (a silicone-based antifoaming agent, a non-silicone-based antifoaming agent, etc.), a plasticizer, an infrared absorbing agent, an ultraviolet absorbing agent, a fragrance, a flame retardant, etc., as needed.

[0051] (Water-based ink manufacturing) The method for producing the aqueous ink of this embodiment is not particularly limited, but for example, the aqueous ink can be obtained by dispersing a mixture to which an aqueous solvent and an antifoaming agent etc. have been added, and then adding a binder resin, an aqueous solvent, an aziridine-based curing agent, and, if necessary, additives such as a surfactant, and stirring and mixing. For the above dispersion and stirring and mixing, a dispersing machine such as a bead mill, Eiger mill, sand mill, gamma mill, or attritor, which is commonly used in the production of inks for flexographic printing or gravure printing, can be used.

[0052] Furthermore, the water-based ink of this embodiment is preferably used for flexographic printing or gravure printing, as described below.

[0053] When the aqueous ink of this embodiment is used for flexographic printing or gravure printing, i.e., when the aqueous ink of this embodiment is used as a flexographic ink or gravure ink, the viscosity should be 7 to 25 seconds, more preferably 10 to 20 seconds, at 25°C using a Zahn Cup #4 (manufactured by Rigo Co., Ltd.). Furthermore, the surface tension of the ink at 25°C is preferably 25 to 50 mN / m. The lower the surface tension of the ink, the better the ink's wetting ability to a substrate such as a film. However, if the surface tension is below 25 mN / m, the ink tends to spread and connect adjacent dots in halftone dot areas. This can easily cause a stain on the printed surface known as dot bridging. On the other hand, if the surface tension exceeds 50 mN / m, the ink's wetting ability to a substrate such as a film decreases, which can easily cause cissing. From the same viewpoint, the surface tension of the ink at 25° C. is more preferably 33 mN / m or more, and more preferably 43 mN / m or less.

[0054] (Laminate) The laminate of this embodiment is characterized in that it includes a substrate and an ink layer provided on the substrate, and the ink layer is a printed layer of the above-mentioned water-based ink. That is, the laminate of this embodiment is obtained by printing the above-mentioned water-based ink on the substrate.

[0055] Examples of substrates include thermoplastic resin films, paper, synthetic paper, steel plates, aluminum foil, wood, woven fabrics, knitted fabrics, nonwoven fabrics, gypsum boards, and wooden boards. Among these, paper, synthetic paper, thermoplastic resin films, and the like are preferred as substrates. The substrate may also be a combination of multiple types of the above-mentioned materials, such as a laminated substrate in which paper and a thermoplastic resin film are laminated, or a laminated substrate in which a thermoplastic resin film and aluminum foil are laminated. In the case of a combination of multiple types, the lamination method is not particularly limited, and they may be bonded using a general-purpose one-component adhesive, two-component adhesive, or the like, or a laminated substrate in which multiple thermoplastic resin films are bonded by extrusion molding.

[0056] The thermoplastic resin film is not particularly limited, and examples thereof include films made of thermoplastic resins such as polyamide resins such as nylon 6, nylon 66, and nylon 46; polyester resins such as polyethylene phthalate (PET), polyethylene naphthalate, polytrimethylene terephthalate, polytrimethylene naphthalate, polybutylene terephthalate, and polybutylene naphthalate; biodegradable resins typified by polyhydroxycarboxylic acids such as polylactic acid, and aliphatic polyester resins such as poly(ethylene succinate) and poly(butylene succinate); polyolefin resins such as polypropylene (PP) and polyethylene; polyimide resins; polyarylate resins; and mixtures thereof, as well as laminate films made of multiple layers of these. Among these, films made of polyester, polyamide, polyethylene, and polypropylene are preferred as thermoplastic resin films.

[0057] These thermoplastic resin films may be unstretched or stretched films, and their manufacturing method is not particularly limited. The thickness of the thermoplastic resin film used as a substrate is not particularly limited, but is generally within the range of 1 to 500 μm. It is preferable that the surface of the thermoplastic resin film to be printed is subjected to a corona discharge treatment. This can further improve adhesion. Furthermore, silica, alumina, or the like may be vapor-deposited on the surface of the thermoplastic resin film to be printed, and a gas barrier coating layer such as an oxygen gas barrier layer may be laminated thereon.

[0058] Examples of paper substrates include kraft paper, liner paper, art paper, coated paper, and carton paper. The structure of the synthetic paper is not particularly limited and may be a single-layer structure or a multilayer structure. Examples of multilayer structures include a two-layer structure consisting of a base layer and a surface layer, a three-layer structure consisting of a base layer and a surface layer on both sides, and a multilayer structure consisting of another resin film layer between the base layer and the surface layer. Each layer in the multilayer structure may or may not contain an inorganic or organic filler. Microporous synthetic paper with numerous fine voids can also be used.

[0059] In this embodiment, a printed matter is obtained by printing an aqueous ink onto a substrate and providing a printed layer. In this regard, the ink is typically applied to the substrate using a printing method such as gravure printing or flexographic printing, and then dried and fixed in an oven to obtain a printed layer. The drying temperature is typically about 40 to 60°C.

[0060] The thickness of the printed layer of the above-mentioned aqueous ink is not particularly limited, and can be determined appropriately taking into account various factors such as the drying properties of the ink when forming the printed layer and running costs.

[0061] The above-mentioned water-based ink printing layer is preferably formed using a printing method such as flexographic printing or gravure printing. Both flexographic printing and gravure printing are types of rotary printing, and can form a printing layer that maintains the five properties well. Flexographic printing and gravure printing are also preferred in terms of high-speed printing suitability, print reproducibility, etc.

[0062] Flexographic printing is a type of relief printing that mainly uses a rubber plate as the printing plate (relief plate) and a fine mesh engraved roll called an anilox roll to supply ink to the plate. The anilox roll receives ink from a chamber-type doctor and applies it to the printing plate, and has the advantage of being able to transfer ink evenly to the printing plate through the anilox roll.

[0063] Specifically, ink is applied to the surface of an anilox roll, which has partition walls and numerous openings surrounded by the partition walls, and a doctor is pressed against the surface of the anilox roll to scrape off the ink present on the top surfaces of the partition walls of the anilox roll and fill the recessed openings with ink. Next, a flexographic plate is pressed against the anilox roll to transfer the ink present in the recessed parts of the anilox roll to the raised parts (pattern parts) of the printing plate, and the plate is then brought into contact with a substrate to transfer the ink present in the pattern parts of the plate to the substrate, thereby obtaining a printed product.

[0064] Rotary printing methods may also be combined. For example, when rotary printing is performed using a thermoplastic resin film as the substrate, rotary printing is performed using water-based ink on the surface of a rolled thermoplastic resin film. After printing, processes such as lamination, slitting (cutting off unnecessary width portions), and bag making (cutting and heat sealing to make bags) can be performed. Rotary printing of water-based ink on a rolled thermoplastic resin film enables high-speed printing and is highly productive.

[0065] As described above, rotary printing includes gravure printing and flexographic printing, and either method can be used. However, it is preferable to use flexographic printing for printing with the water-based ink of this embodiment. Therefore, flexographic printing will be described in detail below. In this specification, rotary printing means gravure printing and flexographic printing, and does not include other printing methods such as ink jet printing and silk screen printing.

[0066] In flexographic printing, water-based ink is supplied from a container to an anilox roller, which has an uneven surface, either directly or via an ink supply pump or the like. The water-based ink supplied to the anilox roller is transferred to the plate surface upon contact with the raised portions of the plate surface, and then finally transferred to the thermoplastic resin film upon contact between the plate surface and the thermoplastic resin film, forming a pattern and / or characters.

[0067] When using aqueous ink, the ink drying property is slightly inferior to that of solvent-based flexographic printing ink, so it is preferable that the ink film thickness is as thin as possible. From this perspective, it is preferable that the amount of ink supplied to the Aronix roller is as small as possible. On the other hand, as a thinner film thickness tends to result in a thinner print density, it is preferable to appropriately control the pigment concentration of the aqueous ink used. Specifically, an appropriate print density can be obtained by increasing the pigment concentration of the aqueous ink by 1 to 5% by weight compared to the concentration of the solvent-based flexographic printing ink.

[0068] A rolled thermoplastic resin film is a thermoplastic resin film in a rolled form that is aligned to a specified width. It is a film for rotary printing, unlike pre-cut sheets. The width of the film is selected appropriately based on the plate width of the rotary printing press used and the width of the image (design) portion of the gravure plate. When using multiple colors of rotary printing ink to overlay colors, the order of printing is not particularly limited.

[0069] When performing surface printing, it is common to print white ink first, and then print colored inks, if necessary. When multiple colored inks are used, the order of printing can be, for example, yellow, magenta, cyan, and black, but this is not particularly limited. In the case of surface printing, an overcoat agent can be applied to the printing surface of the web-printed product as needed to improve abrasion resistance, water resistance, etc.

[0070] When the color of the substrate is white, that is, when the substrate is a paper substrate or a thermoplastic resin film with a white pigment kneaded therein, printing with only colored ink is possible as needed.

[0071] Furthermore, when reverse printing is performed, it is common to first print color inks on a rolled thermoplastic resin film, followed by white ink. When multiple color inks are used, they can be printed in the order of, for example, black, cyan, magenta, and yellow, but this is not particularly limited. Large-format printing machines can also use special colors in addition to the basic colors. That is, large-format printing machines have multiple printing units corresponding to 5 to 10 colors, each equipped with one ink color, allowing for 5 to 10 colors to be printed simultaneously. The printed material obtained by reverse printing can be used as is, or an anchor coating agent and adhesive can be applied to the printed surface of the obtained rotary printed material, and after drying, the resulting product can be laminated with a film or the like to form a laminate.

[0072] The ink layer (printed layer) in the laminate of this embodiment has strong film properties that can withstand external contact, and is particularly excellent in blocking resistance and water-rub resistance, so it is preferably located as the outermost layer. Therefore, the laminate of this embodiment may further include an intermediate ink layer between the substrate and the ink layer. Such an intermediate ink layer may be a printed layer of any ink, and may consist of only one layer or two or more layers. Furthermore, the intermediate ink layer may be a colored ink layer that appropriately contains coloring materials such as pigments based on the desired design. The method for producing the intermediate ink layer is not particularly limited, and it may be produced, for example, in the same manner as the water-based ink printed layer of this embodiment described above.

[0073] The laminate of this embodiment has excellent adhesion regardless of the type of substrate, including plastic films. In addition to the physical properties described in the examples, it also has excellent coating strength, particularly abrasion resistance and scratch resistance, making it suitable for applications in which the printed layer is the outermost layer. Therefore, for front-printed or reverse-printed printed materials, printed materials having a printed layer of the water-based ink of this embodiment on the surface that will be the outermost layer during distribution are preferred, as they maximize the effects of the present invention. The laminate of this embodiment can be used in a variety of applications, including plastic labels (such as shrink labels and wrap-around labels) for beverage and food bottles, integrated packaging, and exterior packaging. In particular, the laminate of this embodiment is suitable for use as a heat-shrinkable film in the various applications described above. [Example]

[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0075] [Preparation of Resin E] A reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser was charged with 60.0 parts by mass of n-propyl acetate. The mixture was heated to 90°C while stirring under a nitrogen atmosphere. Meanwhile, 36.0 parts by mass of methyl methacrylate, 10.0 parts by mass of ethyl methacrylate, 20.0 parts by mass of n-butyl methacrylate, 10.0 parts by mass of isobutyl methacrylate, 10.0 parts by mass of 2-ethylhexyl acrylate, 14.0 parts by mass of acrylic acid, and 1.0 part by mass of azobisisobutyronitrile were dissolved in 40.0 parts by mass of n-propyl acetate and added dropwise using a dropping funnel over 4 hours. After the addition was complete, the reaction was continued for an additional 6 hours. After the reaction was complete, the mixture was cooled, and the resulting acrylic resin solution was neutralized by adding 8.0 parts by mass of 30% aqueous ammonia. Ion-exchanged water was then added and solvent substitution was performed while heating, yielding an aqueous acrylic resin solution with a solids content of 55%. The resin had an acid value of 105 mgKOH / g and a Tg of 65°C. Next, 158.7 parts by weight of the above acrylic resin aqueous solution was charged into a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser, and 195.5 parts by weight of ion-exchanged water was added. The temperature was raised to 75°C while stirring under a nitrogen atmosphere. Next, using the dropping funnel, 30.0 parts by weight of methyl methacrylate, 25.0 parts by weight of butyl acrylate, 8.0 parts by weight of ethyl methacrylate, 25.0 parts by weight of isobutyl methacrylate, and 3.5 parts by weight of 30% ammonium persulfate were added dropwise over 4 hours. After the dropwise addition was completed, the reaction was continued for an additional 6 hours, yielding a core-shell acrylic emulsion (Resin E) with a solids content of 41%. Resin E had an acid value of 55 mgKOH / g and a Tg of 40°C.

[0076] [Preparation of Resin H] A reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser was charged with 65.0 parts of n-propyl acetate. The mixture was heated to 90°C while stirring under a nitrogen atmosphere. Meanwhile, 38.0 parts by mass of styrene, 29.0 parts by mass of ethyl methacrylate, 24.0 parts by mass of 2-ethylhexyl acrylate, 9.0 parts by mass of acrylic acid, and 1.6 parts by mass of azobisisobutyronitrile were dissolved in 35.0 parts by mass of n-propyl acetate and added dropwise using a dropping funnel over 4 hours. After the addition was completed, the reaction was continued for an additional 6 hours. After the reaction was completed, the mixture was cooled, and the resulting acrylic resin solution was neutralized by adding 20.0 parts by mass of 30% ammonia water. Ion-exchanged water was then added and the solvent was replaced while heating, yielding an aqueous styrene-acrylic resin solution with a solids content of 30%. The resin had an acid value of 70 mgKOH / g and a Tg of 52°C. Next, 104.6 parts by weight of the above styrene-acrylic resin aqueous solution was charged into a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser, and 119.6 parts by weight of ion-exchanged water was added. The temperature was raised to 75°C while stirring under a nitrogen atmosphere. Next, using the dropping funnel, 16.0 parts by weight of methyl methacrylate, 16.0 parts by weight of butyl acrylate, 39.0 parts by weight of ethyl methacrylate, 29.0 parts by weight of isobutyl methacrylate, and 3.5 parts by weight of 30% ammonium persulfate were added dropwise over 4 hours. After the dropwise addition was completed, the reaction was continued for an additional 6 hours, yielding a core-shell styrene-acrylic emulsion (Resin H) with a solids content of 41%. Resin H had an acid value of 33 mgKOH / g and a Tg of 53°C.

[0077] [Preparation of Resin A, Resin B, Resin C, Resin D, Resin F, Resin G, Resin M, Resin N, and Resin O] Resin A, Resin B, Resin C, Resin D, Resin F, Resin G, Resin M, and Resin N were prepared by appropriately changing the conditions for preparing the above-mentioned acrylic emulsion (Resin E) so that the Tg and acid value values ​​would be as shown in Table 1. Resin O was prepared by appropriately changing the conditions for preparing the above-mentioned styrene acrylic emulsion (Resin H) so that the Tg and acid value values ​​shown in Table 1 were obtained.

[0078] [Preparation of Resin I, Resin J, and Resin K] Resin I and Resin J were prepared by adding 1% by mass of adipic acid dihydrazide (ADH) as a self-crosslinking component to the above-mentioned acrylic emulsion (Resin E), and by appropriately changing the conditions so that the Tg and acid value values ​​shown in Table 1 were obtained. Resin K was prepared by adding 1% by mass of adipic acid dihydrazide (ADH) as a self-crosslinking component to the above-mentioned styrene acrylic emulsion (Resin H), and by appropriately changing the conditions so that the Tg and acid value values ​​shown in Table 1 were obtained.

[0079] [Preparation of Resin L, Resin P, and Resin Q] As the resin L, "Hi-Loss X AW-36H" (water-based acrylic) manufactured by Seiko PMC Corporation was prepared. As the resin P, "Hiros X-2010L" (water-soluble styrene-acrylic) manufactured by Seiko PMC Corporation was prepared. As the resin Q, "Takelac WS-4022" (urethane emulsion) manufactured by Mitsui Chemicals, Inc. was prepared.

[0080] [Preparation of Water-Based Ink and Laminate] In each example, a water-based ink was prepared according to the formulation shown in Table 1 in a conventional manner. On the other hand, a corona-treated polystyrene heat-shrinkable film (Bonset BS55S, 50 μm thick, manufactured by Takiron C.I. Co., Ltd.) was prepared as the substrate, and a Flexoproof100 test printing machine (200 lines / inch anilox, manufactured by Testing Machines, Inc.) was prepared as the printing device. Then, using the anilox roll and resin plate of this test printing machine, a 240 mm x 80 mm solid image was printed with each example of aqueous ink at a printing speed of 100 m / min. The resulting print was then aged at 25°C for 24 hours to obtain a printed ink laminate.

[0081] The resulting laminate was evaluated as follows, and the results are shown in Table 1.

[0082] <Adhesion to substrate> Cellophane tape was applied to the surface of the laminate on which the ink layer was formed. The cellophane tape was then quickly peeled off, and the degree of peeling of the ink layer (film) from the substrate was visually observed and evaluated according to the following criteria. A rating of 4.5 was given when, among multiple evaluations, ratings of 4 and 5 were mixed at the same level. A practical level is 4 or higher. 5: No peeling of the ink layer 4: The area of ​​the ink layer peeling is more than 0% but less than 10% of the printed area 3: The area of ​​the ink layer peeling is 10% or more but less than 30% of the printed area 2: The area of ​​the ink layer peeling is 30% or more but less than 75% of the printed area 1: The ink layer peels off over 75% of the printed area

[0083] <Blocking resistance> Two laminates were prepared, and the printed surfaces of the ink layers were placed together at a pressure of 5 kg / cm. 2 The ink layer was left to stand for one day at 40°C and 80% humidity under a load of 10 ... 5: No ink layer transfer, no peeling resistance 4: No ink layer transfer, but peel resistance 3: The ink layer transfer amount is less than 10% of the printing area, and there is peeling resistance 2: The ink layer transfer amount is 10% or more but less than 50% of the printing area, and there is peeling resistance. 1: The ink layer transfers to 50% or more of the printing area and has peel resistance

[0084] <Heat resistance> Two laminates were prepared, and with the printed surfaces of the ink layers facing each other, a load of 0.1 MPa was applied for 1 second using a heat seal tester (top and bottom 90°C). The laminates were then peeled off by hand, and the presence or absence of peel resistance and the degree of fusion of the ink layers (films) were visually observed and evaluated according to the following criteria. A practical level is 4 or higher. 5: No ink layer fusion, no peeling resistance 4: No ink layer fusion, but relatively weak peel resistance 3: No ink layer fusion, but relatively strong peel resistance 2: Relatively small amount of ink layer fused, peel resistance 1: Relatively large amount of ink layer adhered, peeling resistance

[0085] <Water friction resistance> A water-soaked Kanakin was placed on the surface of the laminate where the ink layer was formed, and rubbed 100 times with a load of 200 g using a Gakushin-type rub fastness tester. The degree of peeling of the ink layer (film) was then visually observed and evaluated according to the following criteria. A practical level is 4 or higher. 5: No peeling of the ink layer 4: The area of ​​the ink layer peeling is more than 0% but less than 10% of the printed area 3: The area of ​​the ink layer that has peeled off is 10% or more but less than 50% of the printed area 2: The area of ​​the ink layer that has peeled off is 50% or more but less than 70% of the printed area 1: The ink layer peels off over 70% of the printed area

[0086] <Alcohol resistance> A 50 μm drop of the alcohol solution for evaluation was applied to the ink layer-formed surface of the laminate and allowed to dry at room temperature for 24 hours. The ink layer (film) was then washed with room temperature water, and the degree of ink layer (film) detachment and whitening was visually observed and evaluated according to the following criteria. A rating of 4.5 was given when, among multiple evaluations, ratings of 4 and 5 were mixed at the same level. A practical level is 4 or higher. 5: No ink layer separation, no whitening (no change in appearance) 4: No ink layer separation, relatively small amount of whitening 3: No ink layer separation, relatively large amount of whitening 2: A relatively small amount of ink layer has come off 1: A relatively large amount of ink layer has come off

[0087] [Table 1]

[0088] Table 1 also shows the glass transition temperature (Tg, unit: ° C.), oxidation (AV, unit: mgKOH / g), and non-volatile content (NV value, unit: mass%) for each binder resin.

[0089] Furthermore, the "amount (parts by mass) of non-volatile content of curing agent per 100 parts by mass of non-volatile content of binder resin" in Table 1 is calculated as follows, taking Example 1 as an example. {(3.0×100 / 100) ÷ (84.0×50 / 100)}×100 ≒ 7.1

[0090] Details of each component other than the binder resin in Table 1 are as follows:

[0091] Antifoaming agent: organically modified polysiloxane emulsifier (manufactured by Evonik, "TEGO (registered trademark) Formax 1488") Surfactant: Alcohol alkoxylate (BYK, "BYK-DYNWET800") Wax: Polyethylene wax (BYK, "AQUACER531") Titanium oxide: White pigment, manufactured by Teika Corporation, "TITANIX JR-701" Aziridine curing agent A: "PZ-33" manufactured by Nippon Shokubai Co., Ltd., NV value: 100% by mass Aziridine curing agent B: Stahl's "XL-706", NV value: 100% by mass Epoxy curing agent C: Epoxy compound, manufactured by Nagase ChemteX Corporation, "EX-614B" Carbodiimide curing agent D: "Carbodilite E-05" manufactured by Nisshinbo Chemical Inc.

[0092] As can be seen from Table 1, the examples according to the present invention have good evaluation results in all of the substrate adhesion, blocking resistance, heat resistance, water friction resistance, and alcohol resistance, and are excellent in various durability properties in addition to adhesion to the substrate.

[0093] In contrast, in the comparative examples, at least one of the substrate adhesion, blocking resistance, heat resistance, water friction resistance, and alcohol resistance was evaluated as poor.

[0094] The reasons for this are as follows: In Comparative Example 1, this is thought to be because the glass transition temperature of the (meth)acrylic resin used was too low. In Comparative Examples 2 and 3, this is thought to be because the glass transition temperature of the (meth)acrylic resin used was too high. In Comparative Example 4, this is thought to be because the glass transition temperature of the (meth)acrylic resin used was too high, and the amount of non-volatile matter in the aziridine curing agent relative to the non-volatile matter in the binder resin was too large. In Comparative Example 5, this is thought to be because the amount of non-volatile matter in the aziridine-based curing agent was too large relative to the non-volatile matter in the binder resin. In Comparative Example 6, this is thought to be because the amount of nonvolatile matter in the aziridine-based curing agent relative to the nonvolatile matter in the binder resin was too small (the curing agent itself was not used). This is thought to be because in Comparative Examples 7 and 8, a curing agent other than an aziridine-based curing agent was used. This is presumably because in Comparative Example 9, a resin other than a (meth)acrylic resin was used as the binder resin. In Comparative Example 10, it is believed that the amount of non-volatile matter in the aziridine-based curing agent relative to the non-volatile matter in the binder resin was too large due to the incorporation of a certain amount of titanium oxide (white pigment).

[0095] According to the present invention, it is possible to provide a water-based ink that can give a film that is excellent in adhesion, blocking resistance, heat resistance, water-rubbing resistance, and alcohol resistance. Furthermore, according to the present invention, it is possible to provide a laminate having an ink layer as a coating that has excellent adhesion, blocking resistance, heat resistance, water friction resistance, and alcohol resistance.

Claims

1. The composition contains a binder resin, an aziridine-based curing agent, and an aqueous solvent, The binder resin contains 50% by mass or more of a (meth)acrylic resin (A), The (meth)acrylic resin (A) has a glass transition temperature of −10° C. or more and 60° C. or less, 1. A water-based ink, characterized in that an amount of a non-volatile content of the aziridine-based curing agent per 100 parts by mass of a non-volatile content of the binder resin is 2.0 parts by mass or more and 11.0 parts by mass or less.

2. The water-based ink according to claim 1, wherein the (meth)acrylic resin (A) has an acid value of 20 mgKOH / g or more and 80 mgKOH / g or less.

3. The water-based ink according to claim 1 or 2, wherein the (meth)acrylic resin (A) is a styrene-acrylic resin.

4. 3. The water-based ink according to claim 1, which is a top coat varnish that does not contain a pigment.

5. 3. The water-based ink according to claim 1, which is used in flexographic printing or gravure printing.

6. A laminate comprising a substrate and an ink layer provided on the substrate, the ink layer being a printed layer of the water-based ink according to claim 1 or 2.

7. The laminate of claim 6 further comprising an intermediate ink layer between the substrate and the ink layer.

8. The laminate according to claim 6, which is used as a heat shrinkable film.

Citation Information

Patent Citations

  • Undercoating agent for plastic with inorganic thin film, plastic with inorganic thin film, decorative film for in-mold molding and decorative film for insert molding

    JP2011195835A

  • Printable flame-retardant polymer film

    JP2012509980A

  • Aqueous resin composition for coating

    JP2017179274A

  • Water-based liquid ink and laminate

    WO2020213413A1

Cited By

  • Water-based matte ink composition, laminate, and packaging material

    JP2026136486A

  • Water-based varnish compositions, laminates, and packaging materials

    JP2026136490A

  • Water-based ink compositions, laminates, and packaging materials

    JP2026136505A

  • Water-based matte ink composition, laminate, and packaging material

    JP7925100B2

  • Water-based varnish compositions, laminates, and packaging materials

    JP7925101B2