Fire retardant paint, fire retardant coated matter and method for coating fire retardant
A fire-retardant paint with crushed materials and acrylic resin emulsions addresses the lack of fire protection and insulation in existing paints, ensuring strong adhesion and effective heat reflection for improved aesthetics.
Patent Information
- Application Number
- JP2023065944
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-13
AI Technical Summary
Existing paints made from crushed materials like waste tiles lack sufficient fire retardant and heat shielding properties, leading to poor adhesion and potential peeling, and there is a lack of clear improvement in fire protection and insulation.
A fire-retardant paint comprising a mixture of crushed materials (50-70% by weight) with a one-component water-based acrylic resin emulsion (30-50% by weight) applied over a two-component water-based acrylic resin emulsion undercoat, enhancing adhesion and providing fire retardant and heat-insulating properties.
The paint achieves excellent adhesion, fire retardancy, and heat shielding while improving aesthetic appearance by diffusing light and reflecting infrared heat, preventing peeling, and maintaining a durable coating.
Smart Images

Figure 2024152039000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a fireproof paint, a fireproof coating, and a fireproof coating method. [Background technology]
[0002] When replacing roof tiles or demolishing houses, large amounts of waste tiles are generated. Traditionally, these were disposed of as rubble in landfills at final disposal sites, but in recent years, the tiles have been crushed and used as aggregate for road paving, reducing waste and reusing resources.
[0003] There is a technology that mixes fine powder (grain size 3 mm or less) of waste tiles that have been discarded as industrial waste with elastic acrylic emulsion paints of different colors that have also been industrial waste up until now, and reuses them as exterior wall paint. JP 2008-106202 A (Patent Document 1) discloses an exterior wall paint that is a mixture of crushed fine powder of waste tiles with a grain size of 3 mm or less and elastic acrylic emulsion waste paint. This exterior wall paint is a mixture of 20 to 50% by weight of crushed fine powder of waste tiles and 50 to 80% by weight of elastic acrylic emulsion waste paint. This makes it possible to effectively reuse the fine powder of tiles that are generated in large quantities at roof re-thatching sites and house demolition sites, especially the fine powder of waste tiles that is generated when they are crushed to be used as paving materials, and also to reuse the elastic acrylic emulsion waste paint. In addition, because tiles are fired at around 1200 degrees, they remain sturdy even in powder form, and when mixed with acrylic emulsion paint, they do not become sticky, and no clayey substances are liberated. It is also said that painting is easy. Furthermore, because tiles are porous, this paint has a low thermal conductivity and a heat insulating effect, and because the corners of the fine powder of the waste tiles that is generated when they are crushed are covered with the elastic acrylic emulsion waste paint, it has a soft feel even if the painted surface is rough, and does not damage the skin or objects that are rubbed against it. The color unique to the tiles blends with the color of the elastic acrylic emulsion waste paint, giving the painted wall a beautiful appearance.
[0004] Also, JP 2010-156169 A (Patent Document 2) discloses a roof repair material that is a mixture of 53-58% by weight of crushed sand of roof tile material with a particle size of 0.5-2 mm, 20-25% by weight of one or more resin paints selected from acrylic resin paint, Sakubi resin paint, unsaturated polyester resin paint, and epoxy resin paint, 3-6% by weight of a thickener mainly made of polyvinyl alcohol, 4-7% by weight of calcium carbonate, 1-2% by weight of silicon, 3-6% by weight of cement, and 7-9% by weight of water. It is said that by adding a thickener mainly made of polyvinyl alcohol or a thickener mainly made of methyl cellulose, the viscosity of the roof repair material is improved and separation of the roof repair material can be prevented. It is also said that by adding calcium carbonate, the hardening property of the roof repair material is improved. Furthermore, since vinyl fine fibers are mixed in for the purpose of bonding, the stable adhesion of the applied coating layer is ensured, and a coating layer that is less likely to peel off or fall off is obtained. The application workability of the roof repair material is improved, making it easier to apply, and the surface of the completed coating layer is beautiful and strong. The color can of course be black or red, and other intermediate colors can also be freely obtained by mixing black or red repair materials in an appropriate mixing ratio. In addition, it is now possible to apply a thick layer of 2 to 3 mm, which was difficult to achieve with conventional roof repair materials, and as a result, the coating layer surface has excellent heat insulation properties, color retention, and durability.
[0005] In addition, JP 2023-5171 A (Patent Document 3) discloses a heat-shielding coating composition containing a heat-shielding agent and polyurea or a raw material thereof. The heat-shielding agent is at least one selected from the group consisting of hollow ceramic particles and white pigments, and the fire-resistant agent is a white fire-resistant material. It is said that this makes it possible to form a heat-shielding coating film with a long service life. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2008-106202 A [Patent Document 2] JP 2010-156169 A [Patent Document 3] JP 2023-5171 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0007] Generally, paints using crushed waste tiles and the like have the problem of insufficient fire resistance and heat insulation, and even now, extensive research is being conducted into the mixing ratio of the crushed materials, the selection of the type of binder, application form, etc. In particular, paints with insufficient fire resistance do not improve the fire resistance of building materials even if they are applied to the surface of the building materials, so many users give up on using them, and there is a problem that they are difficult to market.
[0008] In the technology described in Patent Document 1, a paint for exterior walls made of a mixture of crushed fine powder of waste tiles and waste elastic acrylic emulsion paint is applied to the exterior walls to improve the heat insulation of the exterior walls, but it is unclear whether the fire resistance is improved. In particular, the coating film of the exterior paint alone has insufficient adhesion to the exterior wall, and there is a high possibility that the coating film will peel off over time.
[0009] Furthermore, in the technology described in Patent Document 2, a thickener is added to the roof repair material to improve its viscosity and prevent it from separating from the roof. However, viscosity alone has a limit to the adhesive strength with the roof, and it is unclear whether fire resistance and insulation have been improved.
[0010] In addition, the technology described in Patent Document 3 combines a heat-shielding agent with polyurea to form a heat-shielding coating film with a long service life, but fire resistance and heat resistance are different properties, and it is unclear whether this technology improves fire resistance. In addition, a coating film made of a heat-shielding paint alone is likely to have insufficient adhesion to the object to which it is applied.
[0011] Therefore, the present invention has been made to solve the above-mentioned problems, and aims to provide a fireproof paint, a fireproof coating, and a fireproof coating method that have excellent adhesion to the object to be coated, and that have fireproofing and heat-shielding properties and can improve aesthetic appearance. [Means for solving the problem]
[0012] The fireproof paint according to the present invention contains a pulverized material and a one-component water-based acrylic resin emulsion. The pulverized material is obtained by pulverizing any one of roof tiles, bricks, ceramics, and tiles at a concentration within the range of 50% by weight to 70% by weight based on the total fireproof paint, and has an average particle size of 5.0 mm or less. The one-component water-based acrylic resin emulsion has a concentration within the range of 30% by weight to 50% by weight based on the total fireproof paint. The fireproof paint is applied to the surface of an undercoat film made of a two-component water-based acrylic resin emulsion formed on the surface of a building material.
[0013] The fireproof coating according to the present invention comprises an undercoat film made of a two-component water-based acrylic resin emulsion formed on the surface of a building material, and a fireproof paint applied to the surface of the undercoat film.
[0014] In addition, the fireproofing coating method of the present invention includes a first forming step of forming a primer coating film on a surface of a building material by applying a two-component water-based acrylic resin emulsion to the surface, and a second forming step of forming a fireproofing paint coating film on the surface by applying a fireproofing paint to the surface of the primer coating film. Effect of the Invention
[0015] The present invention provides excellent adhesion to the object of application, fire resistance and heat insulation properties, and can improve the aesthetic appearance. [Brief description of the drawings]
[0016] [Figure 1] 1 is a conceptual diagram of a fireproof paint, a fireproof coating, and a fireproof coating method according to the present invention. [Diagram 2] 1 is a conceptual photograph of a fireproof paint, a fireproof coating, and a fireproof coating method according to the present invention. [Diagram 3] 1 is a table showing the components and results of the primer paint and fireproof paint of Examples 1-4 and Comparative Examples 1-4. [Figure 4] 1 is a table showing the components and results of the primer paint and fireproof paint of Examples 5-10 and Comparative Examples 5-6. [Diagram 5] Photographs of fireproof paint coatings when the crushed material is tiles, bricks, ceramics, or tiles DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings to facilitate understanding of the present invention. Note that the following embodiment is an example of the present invention and is not intended to limit the technical scope of the present invention.
[0018] The present inventors have focused on the heat resistance of waste materials such as roof tiles for many years, and have conducted intensive research into fireproof paints, fireproof coatings, and fireproof coating methods using waste materials. They have surprisingly discovered that by adopting the composition described below, the coating has excellent adhesion to the object to be coated, fireproofing properties, heat insulation properties, and aesthetic appearance, and have completed the present invention based on the examples described below.
[0019] That is, the fireproof paint 1 according to the present invention contains a pulverized material 10 and a one-component water-based acrylic resin emulsion 11, as shown in Fig. 1. The pulverized material 10 is obtained by pulverizing any one of roof tiles, bricks, ceramics, and tiles at a concentration within a range of 50% by weight to 70% by weight relative to the total fireproof paint 1, and has an average particle size of 5 mm or less. Also, the one-component water-based acrylic resin emulsion 11 has a concentration within a range of 30% by weight to 50% by weight relative to the total fireproof paint 1.
[0020] The fireproof paint 1 is applied to the surface of an undercoat film 22 made of a two-liquid water-based acrylic resin emulsion 2, which is a mixture of a water-based acrylic resin emulsion 20 and an adhesion promoter 21, formed on the surface of a building material B. This provides excellent adhesion to the object to be coated, as well as fireproofing and heat-shielding properties, and makes it possible to improve the aesthetic appearance.
[0021] That is, in the present invention, first, a two-component water-based acrylic resin emulsion 2 with excellent adhesive strength is adopted as an undercoat paint, and this is applied to the surface of a building material B to form an undercoat coating film 22. Here, the two-component water-based acrylic resin emulsion 2 has higher adhesive strength and adhesion to the coating target and has excellent weather resistance after curing compared to a one-component water-based acrylic resin emulsion, so it is extremely effective as an undercoat for fireproofing paint, not only for interior and exterior use.
[0022] Next, in the present invention, a fireproof paint 1 containing pulverized material 10 and one-component water-based acrylic resin emulsion 11 is applied to the surface of the undercoat coating film 22. Here, since both the undercoat coating film 22 and the fireproof paint 1 contain a common acrylic resin, it is possible to increase the adhesive strength and adhesion between the two and increase the adhesive strength of the fireproof paint coating film 12 to the coating target (building material B), and prevent the fireproof paint coating film 12 and the pulverized material 10 from peeling off over time.
[0023] Furthermore, in the present invention, the pulverized material 10 contained in the fireproof paint 1 is obtained by pulverizing any one of roof tiles, bricks, ceramics, and tiles, and has a concentration within a range of 50% to 70% by weight with respect to the total fireproof paint 1. Here, roof tiles, bricks, ceramics, and tiles are all composed of inorganic materials, and therefore can enhance the fireproofing properties of all of them.
[0024] In the present invention, the pulverized material 10 contained in the fireproof paint 1 has an average particle size of 5.0 mm or less. By applying this fireproof paint 1, an uneven surface caused by the pulverized material 10 is formed on the fireproof paint coating film 12. Light irradiated to this uneven surface is diffused by the pulverized material 10 having an average particle size of 5.0 mm or less, suppressing light absorption. In particular, the pulverized material 10 having an average particle size of 5.0 mm or less promotes diffuse reflection of infrared light caused by heat. As a result, the present invention can improve heat insulation properties.
[0025] In the present invention, both the undercoat film 22 and the fireproof paint 1 contain a common acrylic resin, and since acrylic resin is basically transparent, the color of the fireproof paint film 12 is entirely influenced by the pulverized material 10. Here, the pulverized material 10 is any of roof tiles, bricks, ceramics, and tiles, each of which has its own unique color, and each color is beautifully reflected in the fireproof paint film 12. As a result, it is possible to increase the aesthetic value of the object to be coated (building material B) and improve its aesthetic appearance.
[0026] Due to such comprehensive effects, the present invention is able to provide excellent adhesion to the object to be coated, fire resistance, heat insulation properties, and improved aesthetic appearance.
[0027] Here, the types of tiles, bricks, ceramics, and tiles used for the pulverized material 10 are not particularly limited, but may be, for example, tiles collected as waste materials, bricks collected as waste materials, ceramics collected as waste materials, tiles collected as waste materials, or new materials. These may also contain inorganic matter such as shells, soil, and sand. The tiles, bricks, ceramics, and tiles used for the pulverized material 10 may be one type or a combination of multiple types.
[0028] The average particle size of the pulverized material 10 is not particularly limited as long as it is 5.0 mm or less, but is preferably within the range of 1.0 mm to 5.0 mm, and more preferably within the range of 2.0 mm to 5.0 mm. For example, a method for obtaining the pulverized material 10 having an average particle size of 5.0 mm or less may be a method of passing the pulverized material through a sieve with a mesh size of 5.0 mm.
[0029] The type of the one-liquid water-based acrylic resin emulsion 11 is not particularly limited, but may be, for example, a water-based acrylic resin emulsion containing a crosslinking agent. Here, examples of the one-liquid water-based acrylic resin emulsion include an emulsion of a "polymer of (meth)acrylic monomer" or an emulsion of a "copolymer of (meth)acrylic monomer and other monomer". The one-liquid water-based acrylic resin emulsion is obtained by emulsion polymerization under stirring in water, for example, of a (meth)acrylic monomer containing at least one of an acrylic acid ester and a methacrylic acid ester, and other monomers as necessary, in the presence of an emulsifier or a dispersion stabilizer. The glass transition temperature of the acrylic resin is preferably within a range of 30 degrees to 60 degrees, since this improves the weather resistance and fire resistance of the coating film 12 of the fireproof coating material 1. The acrylic monomer may contain silicon or fluorine.
[0030] Also, the thickness of the fireproof paint coating film 12 is not particularly limited, but is preferably within the range of 0.5mm to 5.0mm, and more preferably within the range of 1.0mm to 5.0mm. Here, if the average particle size of the pulverized material 10 is 5mm or less and the thickness of the fireproof paint coating film 12 is within the range of 0.5mm to 5.0mm, the pulverized material 10 will inevitably be exposed on the surface, forming an uneven surface due to the pulverized material 10. This can reliably improve fireproofing, heat insulation, and aesthetics. Also, if the thickness of the fireproof paint coating film 12 is within the range of 0.5mm to 5.0mm, the minimum amount of fireproof paint 1 to be applied is sufficient, and the application operation can be simplified.
[0031] The mixing ratio of the pulverized material 10 to the one-liquid water-based acrylic resin emulsion 11 is preferably 1:0.3-1.0 by weight. This allows the uneven surface caused by the pulverized material 10 to be appropriately formed, and prevents problems such as clogging caused by the pulverized material 10 when applying the fireproof paint 1 by spray coating or the like.
[0032] In addition, the method of applying the fireproof paint 1 is not particularly limited, but examples thereof include a spray coating method (spray method), a brush coating method, a roller coating method, etc. In addition, the number of times the fireproof paint 1 is applied is not particularly limited, but examples thereof include one coat, two coats, three coats, four coats, etc.
[0033] The amount of the fireproof paint 1 to be applied is not particularly limited. For example, the amount is 0.5 kg / m 2 ~3.0kg / m 2 It is preferable that the range is 1.0 kg / m 2 ~2.5kg / m 2 It is more preferable that the ratio is within the range of 1.
[0034] The type of the aqueous acrylic resin emulsion 20 contained in the two-component aqueous acrylic resin emulsion 2 is not particularly limited, but examples thereof include an emulsion of a "polymer of (meth)acrylic monomer" or an emulsion of a "copolymer of (meth)acrylic monomer and other monomer". The aqueous acrylic resin emulsion 20 is obtained by emulsion polymerization under stirring in water in the presence of an emulsifier or dispersion stabilizer, for example, of a (meth)acrylic monomer containing at least one of an acrylic acid ester and a methacrylic acid ester, and other monomers as necessary, in the same manner as described above. The glass transition temperature of the acrylic resin is preferably within the range of 30°C to 60°C, since this improves the weather resistance and fire resistance of the undercoat coating film 22.
[0035] The type of adhesion promoter 21 contained in the two-component water-based acrylic resin emulsion 2 is not particularly limited, but may be, for example, a coupling agent that reacts with the acrylic monomer contained in the water-based acrylic resin emulsion 20 to polymerize the acrylic resin. The coupling agent may be, for example, a silane coupling agent, which can improve the weather resistance and adhesion of the undercoat coating film 22.
[0036] Although there is no particular limitation on the thickness of the undercoat coating film 22, it is preferably within the range of 0.5 mm to 5.0 mm, and more preferably within the range of 1.0 mm to 5.0 mm, for example. This maintains adhesion to the fireproof paint coating film 12, and requires only the minimum necessary amount of undercoat paint 2 to be applied, simplifying the application operation.
[0037] The method of applying the undercoat film 22 is not particularly limited, but examples thereof include a spray coating method (spray method), a brush coating method, a roller coating method, etc. The number of times the fireproof paint 1 is applied is not particularly limited, but examples thereof include one coat, two coats, three coats, four coats, etc.
[0038] The amount of the undercoat coating 22 to be applied is not particularly limited. For example, the amount is 0.5 kg / m 2 ~3.0kg / m 2 It is preferable that the range is 1.0 kg / m 2 ~2.5kg / m 2 It is more preferable that the ratio is within the range of 1.
[0039] Furthermore, the fireproof paint 1 and the two-component water-based acrylic resin emulsion 2 may contain other additives within the scope of not impairing the object of the present invention. Examples of other additives include coloring agents, curing agents, weather resistance agents, organic solvents, pigment dispersants, drying agents, antioxidants, reaction catalysts, defoamers, viscosity adjusters, dehydrating agents, leveling agents, anti-settling agents, anti-sagging agents, adhesion imparting agents, anti-algae agents, anti-mildew agents, preservatives, ultraviolet absorbers, light stabilizers, etc.
[0040] In addition, there is no particular limitation on the type of building material B, but examples include wall materials, flooring materials, roofing materials, architectural wood products, synthetic wood, artificial wood, reclaimed wood, ceiling materials, laminated plywood, decorative plywood, base materials (for interior and exterior use), repair and base adjustment materials, staircase materials, handrail materials, wrought iron, eaves, interior and exterior decorative materials, interior and exterior finishing materials, designer architectural products, Japanese-style architecture and Japanese-style interiors, etc.
[0041] The fireproof coating according to the present invention is constructed by using the above-mentioned undercoat coating film and fireproof paint. Specifically, the fireproof coating comprises an undercoat coating film 22 made of a two-component water-based acrylic resin emulsion 2 formed on the surface of a building material B, and a fireproof paint 1 applied to the surface of the undercoat coating film 22.
[0042] The fireproof coating method according to the present invention is formed by using the above-mentioned undercoat coating film and fireproof paint. Specifically, the fireproof coating method includes a first forming step of forming an undercoat coating film 22 on the surface of a building material B by applying a two-component water-based acrylic resin emulsion 2 to the surface of the building material B, and a second forming step of forming a fireproof paint coating film 12 on the surface of the undercoat coating film 22 by applying a fireproof paint 1 to the surface of the fireproof paint 1.
[0043] As a result, similarly to the above, it is possible to provide excellent adhesion to the object to be coated, fire resistance and heat insulation properties, and improve the aesthetic appearance. EXAMPLES
[0044] Examples and comparative examples of the present invention will be described below in detail, but the application of the present invention is not limited to these examples. (Fireproof paints, fireproof coatings, and fireproof coating methods)
[0045] As shown in FIG. 2, a two-liquid water-based acrylic resin emulsion 2, which is a mixture of a water-based acrylic resin emulsion 20 and an adhesion promoter 21, was prepared as an undercoat paint, and the undercoat paint 2 was applied to the surface of a long building material B to form an undercoat paint film 22 with a thickness of about 1.0 mm. Next, a fireproof paint 1, which is a mixture of a pulverized material 10 and a one-liquid water-based acrylic resin emulsion 11, was prepared, and the fireproof paint 1 was applied to the surface of the undercoat paint film 22. The fireproof paint 1 was applied a predetermined number of times by spray painting to produce a fireproof coated product after application. These fireproof coated products were designated as Examples 1-4. The type of the pulverized material 10 was changed to any one of tiles, bricks, ceramics, and tiles.
[0046] On the other hand, when the average particle size of the pulverized material 10 exceeds 5 mm or is less than 0.5 mm, the fireproof coating material 1 is directly applied to the surface of the building material B without using a primer, or the type of primer is a two-component water-based urethane resin emulsion. These fireproof coating materials are called Comparative Examples 1-4. Figure 3 is a table showing the components and results of the primer and fireproof coating materials of Examples 1-4 and Comparative Examples 1-4.
[0047] In addition, fireproof coatings were produced by combining any two of the types of crushed material 10, such as roof tiles, bricks, ceramics, and tiles, and by increasing the thickness of the fireproof coating film 12 to 10.0 mm or decreasing it to 0.1 mm. These fireproof coatings were designated as Examples 5-10.
[0048] On the other hand, fireproof coatings were produced with the concentration of the pulverized material 10 set to 80% by weight or 40% by weight. These fireproof coatings were designated as Comparative Examples 5-6. Figure 4 is a table showing the components and results of the undercoat paint and fireproof paint of Examples 5-10 and Comparative Examples 5-6. (Evaluation method)
[0049] Next, the performance of the fireproof coating material after production was evaluated. The performance evaluation items were adhesion, fireproofing, heat insulation, and aesthetics. (Adhesiveness)
[0050] Adhesion was evaluated by leaving the manufactured fireproof coated product outside for a specified period (one month), and then stroking the uneven surface of the fireproof coated product a specified number of times to check whether the fireproof paint film peeled off. (standard)
[0051] ◯: When the fireproof paint film did not peel off, the adhesion was judged to be good. Δ: When crushed pieces of the fireproof paint film peeled off, the adhesion was judged to be partially poor. ×: When the fireproof paint film peeled off, the adhesion was judged to be partially poor. (Fireproof)
[0052] Fire resistance was evaluated by cutting the manufactured fireproof coating material, including the building material, undercoat film, and fireproof paint film, into 100mm x 100mm square test pieces, which were then subjected to a cone calorimeter test to measure the total heat generation of the test pieces. (standard)
[0053] ○: Total heat generation for 20 minutes is 8MJ / m 2 The fire resistance was judged to be good in the following cases: △: Total heat generation for 10 minutes is 8MJ / m 2 In the following cases, the fire resistance was judged to be partially poor. ×: Total heat generation for 5 minutes is 8MJ / m 2 The fire resistance was judged to be poor in the following cases: (Heat insulation)
[0054] To evaluate the heat insulation properties, test pieces were cut out from the manufactured fireproof coating, with the building material, undercoat film, and fireproof paint film all combined, and the spectral reflectance was measured in the wavelength range of 300nm-2500nm using an ultraviolet-visible-near-infrared spectrophotometer. The solar reflectance (all wavelength range) was calculated in accordance with JIS K5602. (standard)
[0055] ◯: When the solar reflectance in the entire wavelength range was 20% or more, the heat shielding property was judged to be good. △: When the solar reflectance in the entire wavelength range was less than 20% and was 10% or more, the heat shielding property was judged to be partially poor. ×: When the solar reflectance in the entire wavelength range was less than 10%, the heat shielding property was judged to be poor. (Aesthetics)
[0056] To evaluate the aesthetics, test pieces were cut out from the manufactured fireproof coating, with the building material, undercoat film, and fireproof paint film integrated together, and the spectral reflectance was measured in the wavelength range of 300nm-2500nm using an ultraviolet-visible-near infrared spectrophotometer. The lightness (L*) at a 10-degree field of view was calculated in accordance with JIS K5600-4-4 3-2. (standard)
[0057] A: When the lightness (L*) was 30 or more, the aesthetic appearance was judged to be good. △: When the lightness (L*) was less than 30% and 20% or more, the aesthetics were judged to be partially poor. ×: When the lightness (L*) was less than 20%, the aesthetic appearance was judged to be poor. (Evaluation Results)
[0058] 3, in Comparative Examples 1 and 3-4, all performance evaluation items were rated "x", and in Comparative Example 2, two performance evaluation items were rated "x", indicating that these were defective products. On the other hand, in Examples 1-4, all performance evaluation items were rated "o", indicating that these were acceptable products.
[0059] 4, in Comparative Examples 5-6, all performance evaluation items were rated "X", indicating that these were defective products. On the other hand, in Examples 5-8, all performance evaluation items were rated "O", and in Examples 9-10, all performance evaluation items were rated "O" or "△", indicating that these were acceptable products.
[0060] Also, Figure 5 shows a photograph of the fireproof paint coating when the crushed material is either roof tile, brick, ceramic, or tile. It can be seen that in all cases, the coating has excellent aesthetic appearance. [Industrial Applicability]
[0061] As described above, the fireproof paint, fireproof coating, and fireproof application method of the present invention are useful for the surfaces of all building materials, have excellent adhesion to the object to be coated, and are effective as a fireproof paint, fireproof coating, and fireproof application method that have fireproofing and heat-shielding properties and can improve aesthetic appearance. [Explanation of symbols]
[0062] 1 Fire retardant paint 10 Crushed material 11 One-component water-based acrylic resin emulsion 12 Fire protection paint film 2. Two-component water-based acrylic resin emulsion 20 Water-based acrylic resin emulsion 21 Adhesion promoter 22 Base coating B. Building Materials
Claims
1. A pulverized material obtained by pulverizing any one of roof tiles, bricks, ceramics, and tiles at a concentration in the range of 50% by weight to 70% by weight based on the total fireproof paint, and having an average particle size of 5.0 mm or less; A one-component water-based acrylic resin emulsion having a concentration in the range of 30% by weight to 50% by weight based on the total fireproof paint; Contains The coating is applied to the surface of a base coat film formed on the surface of a building material and made of a two-part water-based acrylic resin emulsion obtained by mixing a water-based acrylic resin emulsion and an adhesion promoter. Fire retardant paint.
2. The film thickness of the fireproof paint is within the range of 0.5 mm to 5.0 mm. The fireproof coating material according to claim 1.
3. a primer coating film formed on the surface of the building material and made of a two-part water-based acrylic resin emulsion obtained by mixing a water-based acrylic resin emulsion and an adhesion promoter; A fireproof paint applied to the surface of the undercoat coating; Equipped with The fireproof paint is A pulverized material obtained by pulverizing any one of roof tiles, bricks, ceramics, and tiles at a concentration in the range of 50% by weight to 70% by weight based on the total fireproof paint, and having an average particle size of 5.0 mm or less; A one-component water-based acrylic resin emulsion having a concentration in the range of 30% by weight to 50% by weight based on the total fireproof paint; Contains Fireproof coatings.
4. a first forming step of applying a two-part water-based acrylic resin emulsion obtained by mixing a water-based acrylic resin emulsion and an adhesion promoter to a surface of a building material to form an undercoat coating film on the surface; A second forming step of applying a fireproof paint to the surface of the undercoat coating film to form a fireproof paint coating film on the surface; Equipped with The fireproof paint is A pulverized material obtained by pulverizing any one of roof tiles, bricks, ceramics, and tiles at a concentration in the range of 50% by weight to 70% by weight based on the total fireproof paint, and having an average particle size of 5.0 mm or less; A one-component water-based acrylic resin emulsion having a concentration in the range of 30% by weight to 50% by weight based on the total fireproof paint; Contains Fireproofing application method.
Citation Information
Patent Citations
Coating material for outer wall
JP2008106202A
Roof repair material
JP2010156169A
Thermal barrier coating composition
JP2023005171A