Two-component developer and image forming apparatus
The two-component developer with alicyclic (meth)acrylate monomer-coated magnetic carrier addresses the issue of toner particle adherence and carrier deterioration, ensuring high-quality prints by preventing fogging and ghosting.
Patent Information
- Application Number
- JP2023066249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Toner particles containing magnetic material tend to stay near the developer conveying member due to magnetism, leading to uneven toner density and increased risk of fogging and ghosting in printed matter, and the magnetic carrier deteriorates due to friction, affecting print quality.
A two-component developer with toner particles containing 30-60% magnetic material and a magnetic carrier with a resin coating layer made from alicyclic (meth)acrylate monomers, which enhances mechanical strength and reduces deterioration, ensuring consistent toner transport and improved print quality.
The developer maintains high durability and prevents fogging and ghosting, providing consistent high-quality prints even under varying environmental conditions.
Smart Images

Figure 2024152201000003 
Figure 2024152201000004 
Figure 2024152201000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a two-component developer and an image forming apparatus. [Background technology]
[0002] In recent years, the printing speed of electrophotographic copiers and printers has been increasing, and two-component developers containing a magnetic carrier and a toner have become mainstream as developers for these machines. In two-component developers, the toner and carrier are mechanically stirred to quickly impart a desired amount of charge to the toner. Therefore, two-component developers are considered to be very advantageous for high-speed development.
[0003] In the magnetic brush development method using a two-component developer, when the charged two-component developer is transported to the photoconductor (image carrier) by a developer transport member (developing roller), only the toner moves onto the charged photoconductor. Meanwhile, the toner and magnetic carrier remaining on the developer transport member are collected and reused.
[0004] Here, Patent Document 1 describes the use of toner particles in which a magnetic material is bound by a binder resin for a two-component developer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-72137 A Summary of the Invention [Problem to be solved by the invention]
[0006] Toner particles containing a magnetic material as described in the above Patent Document 1 tend to remain near the developer transport member due to their magnetism. Therefore, when developing, a sufficient amount of toner can be transported to the image carrier by the developer transport member. As a result, unevenness or insufficient density of toner is unlikely to occur in the resulting printed matter. Furthermore, since the toner (toner particles) is sufficiently charged, it is believed that the toner is unlikely to scatter on the image carrier side, and fogging is unlikely to occur on the printed matter.
[0007] However, the inventors of the present invention conducted extensive research and found that the toner particles containing the magnetic material are very hard, and the magnetic carrier is easily deteriorated due to friction between the toner (toner particles) and the magnetic carrier. When the magnetic carrier deteriorates, fog or ghosting occurs on the resulting printed matter. Therefore, there was a problem that it is difficult to obtain high-quality printed matter with the toner containing the toner particles.
[0008] The present invention has been made in consideration of the above problems, and has an object to provide a two-component developer that is less likely to cause fog or ghosts on printed matter and has high durability, and an image forming apparatus that uses the two-component developer. [Means for solving the problem]
[0009] One aspect of the present invention for achieving the above-mentioned object relates to a two-component developer including a toner and a magnetic carrier, the toner including toner particles containing a binder resin and a magnetic material, the amount of the magnetic material in the toner particles being 30% by mass or more and 60% by mass or less, the magnetic carrier including carrier particles having a magnetic core material and a resin coating layer coating the core material, and the resin coating layer including a polymer of an alicyclic (meth)acrylate monomer.
[0010] Another aspect of the present invention relates to an image forming apparatus including an image carrier and a developing unit for supplying toner to an electrostatic latent image formed on the surface of the image carrier, the developing unit including a developer storage unit that stores the above-described two-component developer, and a developer transport member that faces the image carrier and is supported so as to be freely rotatable, the developer transport member including a magnet roll therein and carrying the two-component developer on its surface, thereby transporting the developer from the developer storage unit side to the image carrier side. Effect of the Invention
[0011] According to the present invention, there are provided a two-component developer which is unlikely to cause fogging or ghosting on printed matter and has high durability, and an image forming apparatus which uses the two-component developer. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram showing an exemplary configuration of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a print pattern for evaluating ghosts. [Diagram 3] FIG. 3 is a diagram showing a print pattern for evaluating ghosts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the present invention will be described in detail based on embodiments, however, the present invention is not limited to these embodiments.
[0014] 1. Two-component developer This embodiment relates to a two-component developer containing a toner and a magnetic carrier. The toner of this embodiment contains toner particles containing 30% by mass or more and 60% by mass or less of a magnetic material, and the two-component developer is less likely to cause fog or ghosting on printed matter. In addition, the magnetic carrier is less likely to deteriorate over a long period of time. The reasons for this are as follows.
[0015] In the two-component developer of the present embodiment, the magnetic carrier has a core material having magnetism and a resin coating layer covering the surface thereof, and the resin coating layer contains a polymer of an alicyclic (meth)acrylate monomer. The magnetic carrier containing an alicyclic (meth)acrylate monomer has high mechanical strength and is not easily deteriorated by friction with toner particles containing a magnetic material, for example. Furthermore, the resin coating layer has low hygroscopicity, and the charge amount is not easily reduced even when the two-component developer is used under high temperature and high humidity. Therefore, high-quality images can be provided over a long period of time under various environments. Furthermore, the toner particles containing a magnetic material have high fluidity due to the filler effect of the magnetic material. Furthermore, as described above, the magnetic material tends to accumulate near the developer transport unit of the image forming apparatus. Therefore, even in a short development process such as a high-speed machine, it is possible to always move the toner to the image carrier side, and the resulting printed matter is less likely to have uneven toner concentration or a decrease in concentration, and further, ghosts are less likely to occur. In addition, since the resin coating layer containing the alicyclic (meth)acrylate monomer has a high mechanical strength, physical adhesion of toner particles is unlikely to occur, and the toner with a high magnetic component ratio is prevented from adhering to the carrier surface, which would otherwise cause the core surface to be exposed from the viewpoint of magnetization, and fogging is unlikely to occur. Each component of the two-component developer will be described below.
[0016] (1) Toner The toner should contain at least toner particles, but usually further contains an external additive.
[0017] (1-1) Toner particles The toner particles are particles that contain at least a binder resin and a magnetic material. The amount of the magnetic material in the toner particles may be 30% by mass or more and 60% by mass or less, preferably 31% by mass or more and 60% by mass or less, and more preferably 40% by mass or more and 60% by mass or less. When the amount of the magnetic material in the toner particles is 30% by mass or more, as described above, the flowability of the toner particles is likely to be increased due to the filler effect of the magnetic material. In addition, due to the magnetism, the toner particles are likely to remain in the vicinity of the developer transport member. On the other hand, when the amount of the magnetic material is 60% by mass or less, the toner particles are likely to move from the developer transport member to the image carrier side during development. Therefore, it is possible to form a high-quality printed matter even when printing with a high-speed printer or the like.
[0018] ·Magnetic material The magnetic material contained in the toner particles may be any known magnetic material as long as it is a component that exhibits magnetism. Examples of the magnetic material include metals such as iron, cobalt, and nickel, and their alloys; metal oxides such as Fe3O4, γ-Fe2O3, and cobalt-added iron oxide; various ferrites such as MnZn ferrite and NiZn ferrite; magnetite; and hematite. The toner particles may contain only one of these, or may contain two or more of them.
[0019] Furthermore, the magnetic body may be one in which the surface of the above-mentioned metals, alloys, etc. is treated with a surface treatment agent such as a silane coupling agent or a titanate coupling agent, may be coated with an inorganic material such as a silicon-based compound or an aluminum-based compound, or may be coated with a polymer.
[0020] The particle shape of the magnetic material is not particularly restricted, but the number-average particle size is preferably 0.05 μm or more and 0.35 μm or less. When the number-average particle shape of the magnetic material is within this range, the fluidity of the toner particles (toner) is likely to be increased. The number-average particle shape is a value measured by a Coulter counter, and is a value measured using ISOTON-II (manufactured by Beckman Coulter, Inc.) as an electrolyte. The number of particles measured is 50,000 per sample.
[0021] ·Binding resin The binder resin is not particularly limited as long as it is a resin capable of binding the magnetic material. Examples of the binder resin include styrenes such as styrene, parachlorostyrene, and α-methylstyrene; esters having a vinyl group such as methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, and 2-ethylhexyl methacrylate; vinyl nitriles such as acrylonitrile and methacrylonitrile; vinyl ethers such as vinyl methyl ether and vinyl isobutyl ether; vinyl ketones such as vinyl methyl ketone, vinyl ethyl ketone, and vinyl isopropenyl ketone; olefins such as ethylene, propylene, and butadiene; and resins obtained by polymerizing one or more types of monomers (vinyl monomers) having an unsaturated double bond.
[0022] Other examples of the binder resin include non-vinyl condensation resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, and polyether resins. The binder resin may also be a mixture of these resins and polymers of the vinyl monomers described above, or a graft polymer obtained by polymerizing a vinyl monomer in the presence of these resins. The toner particles may contain only one type of binder resin, or may contain two or more types.
[0023] The glass transition temperature Tg of the binder resin is appropriately selected according to the desired performance such as ease of production of toner particles, storage stability, shape stability, low-temperature fixability, image storage stability, etc., and is preferably 40° C. or higher and 80° C. or lower, more preferably 45° C. or higher and 70° C. or lower.
[0024] The amount of binder resin in the toner particles is not particularly limited as long as it can bind the magnetic material, but is preferably 15% by mass or more and 55% by mass or less, and more preferably 20% by mass or more and 50% by mass or less, based on the mass of the toner particles.
[0025] Coloring agents The toner particles may further contain a colorant. For example, the toner particles may contain a black colorant, or may contain a colorant of any color. The toner particles may contain only one type of colorant, or may contain two or more types of colorants.
[0026] Examples of black colorants include black iron hydroxide, black titanium oxide, carbon black, etc. Among these, black titanium oxide (titanium black) is preferable. When the toner particles contain black titanium oxide, the dispersibility of the above-mentioned magnetic material tends to be good.
[0027] On the other hand, examples of colorants other than black include DuPont Oil Red, Orient Oil Red, Rose Bengal, CI Pigment Red 5, 112, 123, 139, 144, 149, 166, 177, 178, 222, 48:1, 48:2, 48:3, 53:1, 57:1, and 81:1, CI Pigment Orange 31 and 43, quinoline yellow, chrome yellow, CI Pigment Yellow 12, 14, 17, 93, 94, 97, 138, 174, 180, and 188, ultramarine blue, aniline blue, chalcoil blue, methylene blue chloride, copper phthalocyanine, CI Pigment Blue 15, 60, 15:1, 15:2, and 15:3, CI Pigment Green 7, and malachite green oxalate. The toner particles may contain only one of these, or may contain two or more of them.
[0028] The amount of the colorant is not particularly limited, but when the colorant contains titanium black, the amount is preferably more than 0% by mass and not more than 30% by mass, more preferably 0% by mass or more and not more than 20% by mass, based on the mass of the toner particles. Also, when the toner particles contain other colorants, the total amount of these is preferably 30% by mass or less, more preferably 0% by mass or more and not more than 20% by mass, based on the mass of the toner particles. When the amount of the colorant is within this range, it is unlikely to affect the charging performance of the toner.
[0029] Release agent The toner particles may further contain a release agent. When the toner particles contain a release agent, offset is less likely to occur. A known compound can be used as the release agent. Examples of the release agent include low molecular weight polyolefins such as polyethylene, polypropylene, and polybutene; silicones that exhibit a softening point when heated; fatty acid amides such as oleic acid amide, erucic acid amide, ricinoleic acid amide, and stearic acid amide; vegetable waxes such as carnauba wax, rice wax, candelilla wax, wood wax, and jojoba oil; animal waxes such as beeswax; mineral and petroleum waxes such as montan wax, ozokerite, ceresin, paraffin wax, microcrystalline wax, and Fischer-Tropsch wax; and modified products thereof.
[0030] The amount of the release agent is not particularly limited, but is preferably 0.1% by mass or more and 20% by mass or less, more preferably 2% by mass or more and 15% by mass or less, based on the mass of the toner particles. When the amount of the release agent is within this range, offset is easily suppressed. In addition, when the amount of the release agent is within this range, it is difficult to affect the charging performance and storage stability of the toner.
[0031] Internal additives The toner particles may further contain an internal additive within a range that does not impair the object and effect of the present embodiment. Examples of the internal additive include fluorine-based surfactants, salicylic acid complexes, iron-based dyes such as iron complexes, chromium-based dyes such as chromium complexes, polymeric acids such as maleic acid polymers, quaternary ammonium salts, azine dyes such as nigrosine, etc.
[0032] (1-2) External additives The external additive serves to control the fluidity, chargeability, etc. of the toner particles. The toner may contain only one type of external additive, or may contain two or more types.
[0033] Examples of the external additive include silica particles, titania particles, alumina particles, zirconia particles, zinc oxide particles, chromium oxide particles, cerium oxide particles, antimony oxide particles, tungsten oxide particles, tin oxide particles, tellurium oxide particles, manganese oxide particles, and boron oxide particles.
[0034] The external additive is preferably subjected to a hydrophobic treatment on its surface. A known surface treatment agent is used for the hydrophobic treatment. The surface treatment agent may be used alone or in combination of two or more. Examples of the surface treatment agent include silane coupling agents, silicone oils, titanate coupling agents, aluminate coupling agents, fatty acids, fatty acid metal salts, esters thereof, and rosin acids.
[0035] Examples of the silane coupling agent include dimethyldimethoxysilane, hexamethyldisilazane (HMDS), methyltrimethoxysilane, isobutyltrimethoxysilane, and decyltrimethoxysilane, etc. Examples of the silicone oil include cyclic compounds and linear or branched organosiloxanes, etc., more specifically, organosiloxane oligomers, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, tetramethylcyclotetrasiloxane, and tetravinyltetramethylcyclotetrasiloxane, etc.
[0036] Examples of the silicone oil include silicone oils with high reactivity, at least terminally modified, in which modified groups are introduced into the side chain, one terminal, both terminals, one terminal of the side chain, or both terminals of the side chain. The type of the modified group may be one or more. Examples of the modified group include alkoxy, carboxyl, carbinol, higher fatty acid modified, phenol, epoxy, (meth)acryloyl, and amino.
[0037] The content of the external additive is preferably from 0.1% by mass to 10.0% by mass, and more preferably from 1.0% by mass to 3.0% by mass, based on the total amount of the toner.
[0038] Toner manufacturing method The method for producing the toner particles containing the above-mentioned magnetic material and binder is not particularly limited, and they can be produced by a kneading and grinding method, a wet production method, etc., depending on the desired physical properties. When it is desired to produce toner particles with little surface unevenness, a wet production method is more preferable.
[0039] The type of wet manufacturing method is not limited, and may be a suspension polymerization method. Alternatively, a method may be used in which a binder resin or a magnetic material is added to an oil medium to prepare an oil dispersion mixture, and the oil dispersion mixture is dispersed in an aqueous medium to form oil droplets and harden. Alternatively, an emulsion polymerization method may be used in which a binder resin dispersion liquid in which a binder resin is dispersed by an ionic surfactant and a dispersion liquid in which a magnetic material is dispersed by an ionic surfactant of the opposite polarity are prepared in advance, and these are subjected to hetero-aggregation to form aggregated particles, and the aggregated particles are hardened by heating to a temperature equal to or higher than the glass transition point Tg of the binder resin. According to this method, it is also possible to sharpen the particle shape distribution of toner particles and prepare toner particles with a small diameter.
[0040] On the other hand, after the toner particles are prepared, the toner particles may be mixed with an external additive, if necessary, to obtain a toner containing the external additive.
[0041] The volume average particle diameter D50v of the toner particles is preferably 5.0 μm or more and 8.0 μm or less, more preferably 5.5 μm or more and 7.0 μm or less. When the volume average particle shape D50v of the toner particles is in the above range, the two-component developer can be easily used in various image forming devices. The volume average particle shape is a value measured by the Coulter counter method.
[0042] (2) Magnetic carrier The magnetic carrier only needs to contain carrier particles having a magnetic core material and a resin coating layer that coats the core material, and may contain other components as necessary.
[0043] Core material The core material may be any particulate component having magnetism. Examples of particulate components having magnetism include porous magnetic particles. The peak pore size in the pore size distribution of the porous magnetic particles from 0.1 μm to 3.0 μm is preferably from 0.40 μm to 1.00 μm. When the peak pore size is within this range, the physical properties of the magnetic carrier are unlikely to change even if the environment in which the two-component developer is used changes, and the durability of the magnetic carrier is likely to be increased. In addition, the pore volume, which is the integral value of the differential pore volume, in the pore size distribution of the porous magnetic particles from 0.1 μm to 3.0 μm is 58 mm 3 / g or more 100mm 3 From the viewpoint of the stability of the magnetic carrier, the pore distribution diameter is preferably 1 / g or less. The pore distribution diameter is a value measured by mercury pressure spectrometry, for example, using a fully automatic multifunctional mercury porosimeter PoreMaster series / PoreMaster-GT series manufactured by Yuasa Ionics Corporation, an automatic porosimeter AutoPore IV 9500 series manufactured by Shimadzu Corporation, or the like.
[0044] Examples of materials for the porous magnetic particles include magnetite and ferrite, with ferrite being more preferred in terms of ease of controlling the porous structure of the porous magnetic core particles and adjusting the resistance.
[0045] Ferrite is a sintered body represented by the following general formula: (M 1 2O) x (M 2 O) y (Fe2O3) z In the general formula, M 1 represents a monovalent metal, M 2 represents a divalent metal. 1 and M. 2Examples of the elements include Li, Fe, Mn, Mg, Sr, Cu, Zn, Ca, Ni, Co, Ba, Y, V, Bi, In, Ta, Zr, B, Mo, Na, Sn, Ti, Cr, Al, Si, and rare earth elements, and among these, Li, Fe, Mn, Mg, Sr, Cu, Zn, and Ca are preferred. Furthermore, when x+y+z=1.0, x and y are each 0≦(x,y)≦0.8, and z is 0.2 <z<1.0である
[0046] Among the above ferrites, Mn-based ferrites, Mn-Mg-based ferrites, Mn-Mg-Sr-based ferrites, and Li-Mn-based ferrites, which contain Mn atoms, are more preferable from the viewpoint of stability and the like.
[0047] Furthermore, the physical strength of the porous magnetic particles may be reduced depending on the internal pore volume, so in order to increase the physical strength, it is preferable that at least a portion of the voids in the porous magnetic particles is filled with a resin.
[0048] The resin filled in the porous magnetic particles may be a thermoplastic resin or a thermosetting resin. Examples of the thermoplastic resin include novolac resin, saturated alkyl polyester resin, polyarylate, polyamide resin, acrylic resin, etc. Examples of the thermosetting resin include phenolic resin, epoxy resin, unsaturated polyester resin, silicone resin, etc.
[0049] The amount of resin is preferably 2% by mass or more and 15% by mass or less based on the total mass of the core material. If there is little variation in the amount of resin for each core material, the resin may be filled only in the voids near the surfaces of the porous magnetic particles, or all of the voids may be filled with resin.
[0050] The volume average particle size of the core material is preferably 10 to 100 μm, and more preferably 20 to 80 μm. The volume average particle size of the core material can be measured typically by a laser diffraction particle size distribution measuring device (Heros, manufactured by Sympatique) equipped with a wet disperser.
[0051] Furthermore, the saturation magnetization of the core material is 30 to 75 A·m 2 / kg is preferable, and the residual magnetization is 5.0 A m 2 / kg or less is preferable. When a core material having such magnetic properties is used, the magnetic carrier particles are less likely to partially aggregate. In addition, the two-component developer is more likely to adhere uniformly to the surface of the developer transport member, making it possible to form a uniform, high-definition toner image without uneven density.
[0052] The core material containing the porous magnetic particles can be prepared by a known method. For example, a desired ferrite raw material is pre-sintered and pulverized. Then, the ferrite raw material is granulated together with a pore regulator (e.g., a foaming agent or resin particles) and sintered to prepare the porous magnetic particles.
[0053] Furthermore, the filling of the voids in the porous magnetic particles with the resin can be carried out by introducing a resin solution into the voids in the porous magnetic particles by a dipping method, a spraying method, a brush coating method, a fluidized bed method, etc., and then volatilizing the solvent, etc. However, the method is not limited to these methods.
[0054] Resin coating layer The resin coating layer may be a layer that coats the core material and contains a polymer of an alicyclic (meth)acrylate monomer. If the resin coating layer contains a structure derived from an alicyclic (meth)acrylate monomer, the mechanical strength of the magnetic carrier is likely to be increased as described above. In this specification, the term "(meth)acrylate" includes acrylate, methacrylate, and mixtures thereof, and the term "(meth)acrylic" includes methacrylic, acrylic, and mixtures thereof.
[0055] The resin coating layer may be composed of a homopolymer of an alicyclic (meth)acrylate monomer, but is preferably a copolymer of an alicyclic (meth)acrylate monomer and another monomer.
[0056] In this specification, the alicyclic (meth)acrylate monomer refers to a (meth)acrylate monomer containing an alicyclic hydrocarbon in the molecule, and the number of carbon atoms of the alicyclic hydrocarbon is preferably 5 or more and 8 or less. Specific examples of the alicyclic (meth)acrylate monomer include cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate, and among these, cyclohexyl methacrylate is preferred from the viewpoints of mechanical strength and environmental stability of the charge amount.
[0057] The amount of the constituent units derived from the alicyclic (meth)acrylate monomer relative to the total constituent units of the resin constituting the resin coating layer is preferably 20 to 80 mass%, more preferably 40 to 80 mass%, and even more preferably 60 to 80 mass%. When the amount of the constituent units derived from the alicyclic (meth)acrylate monomer is within this range, the mechanical strength of the magnetic carrier is more likely to be increased, and the stability of the charge amount of the magnetic carrier is further improved. The content of the constituent units is substantially the same as the polymerization ratio when the resin is produced.
[0058] Examples of monomers that can be copolymerized with the alicyclic (meth)acrylate monomer include (meth)acrylic monomers such as linear or branched (meth)acrylic acid esters and (meth)acrylic acid aminoalkyl esters, and vinyl monomers such as styrene, vinyl acetate, and vinyl chloride. Among these, (meth)acrylic monomers are preferred from the viewpoint of increasing the stability of the resin coating layer, and methyl methacrylate is particularly preferred.
[0059] The amount of the resin coating layer in the magnetic carrier is preferably 0.5 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the core material. When the amount of the resin coating layer is within the above range, the wear resistance of the magnetic carrier becomes even better.
[0060] The method of forming the resin coating layer around the core material is not particularly limited, and known methods can be applied. Examples of such methods include a fluidized bed spray coating method in which a coating liquid in which the coating resin is dissolved in a solvent is spray-coated on the surface of the core material and dried; a dip coating method in which the core material is immersed in a solution in which the coating resin is dissolved in a solvent and dried; a polymerization method in which the core material is immersed in a solution containing the monomer (alicyclic (meth)acrylic monomer or other monomer), the solvent is then removed, and the monomer is polymerized by heating; and a dry coating method in which the coating resin is fixed to the surface of the core material while applying a mechanical impact; and the like.
[0061] The volume average particle diameter D50v of the carrier particles in which the core material is coated with a resin coating layer is preferably 10 μm or more and 100 μm or less, more preferably 20 μm or more and 80 μm or less. When the volume average particle shape D50v of the carrier particles is in the above range, the two-component developer can be easily used in various image forming devices. The volume average particle shape is a value measured by the Coulter counter method.
[0062] (3) Method for preparing two-component developer The two-component developer of the present embodiment can be produced by mixing the above-mentioned toner and magnetic carrier using a mixing device. Examples of the mixing device include a Henschel mixer, a Nauta mixer, and a V-type mixer. The amount of the toner and the amount of the magnetic carrier are appropriately selected according to the desired performance.
[0063] 2. Image forming equipment The two-component developer can be used in known image forming apparatuses, and can be used, for example, in an electrophotographic image forming apparatus 1 shown in FIG.
[0064] Fig. 1 is a schematic diagram showing an exemplary configuration of an image forming apparatus having a photoconductor 100. As shown in Fig. 1, the image forming apparatus 1 includes an image reading unit 10, an operation display unit 20, an image processing unit 30, an image forming unit 40, a paper conveying unit 50, a fixing unit 60, and a control unit 70.
[0065] The control unit 70 is a device for centrally controlling the operation of each block of the image forming apparatus 1 in cooperation with the deployed program, and includes, for example, a CPU (Central Processing Unit), a ROM (Read Only Memory), and a RAM (Random Access Memory).
[0066] The image reading unit 10 is configured with an automatic document feeder 111 called an ADF (Auto Document Feeder), an original image scanning device 112 (scanner), etc. The operation display unit 20 is configured with, for example, a liquid crystal display (LCD: Liquid Crystal Display) with a touch panel, and functions as a display unit and an operation unit. The image processing unit 30 is equipped with a circuit that performs digital image processing on input image data according to initial settings or user settings, etc.
[0067] The image forming section 40 normally includes image forming units 41 (41Y, 41M, 41C, and 41K) using toners of the respective colors of Y (yellow), M (magenta), C (cyan), and K (black) (the above-mentioned two-component developer). The image forming section 40 further includes an intermediate transfer unit 42 and a secondary transfer unit 43. These correspond to transfer means.
[0068] The image forming unit 41 includes an exposure section 411, a development section 412, a photoconductor (image carrier) 413, a charging section 414, and a drum cleaning device 415. The photoconductor 413 is used, for example, as a negatively charged organic photoconductor. The charging section 414 is, for example, a corona charger. The charging section 414 may be a contact charging means that charges the photoconductor 413 by contacting a contact charging member such as a charging roller, a charging brush, or a charging blade with the photoconductor 413. The exposure section 411 includes, for example, a semiconductor laser as a light source, and a light deflection device (polygon motor) that irradiates the photoconductor 413 with laser light according to the image to be formed.
[0069] The developing unit 412 includes a developer container that contains the above-mentioned two-component developer, a developer transport member (developing roller) that is rotatably arranged at the opening of the developer container so as to face the photoconductor 413 and includes a magnet roll therein, a partition that divides the inside of the developer container so that the two-component developer can communicate with each other, a transport roller for transporting the two-component developer on the opening side of the developer container toward the developer transport member, and a stirring roller for stirring the two-component developer in the developer container. The developing unit 412 also includes a bias application unit for applying an AC bias voltage to the developer transport member (developing roller). If a bias application unit for applying an AC bias is provided, the supply of toner from the developer transport member side to the photoconductor (image carrier) 413 side becomes smoother.
[0070] The intermediate transfer unit 42 has an intermediate transfer belt 421, a primary transfer roller 422 that presses the intermediate transfer belt 421 against the photoconductor 413, a plurality of support rollers 423 including a backup roller 423A, and a belt cleaning device 426. The intermediate transfer belt 421 is stretched in a loop shape around the plurality of support rollers 423. By rotating at least one drive roller among the plurality of support rollers 423, the intermediate transfer belt 421 runs at a constant speed in the direction of arrow A.
[0071] The secondary transfer unit 43 has an endless secondary transfer belt 432 and a plurality of support rollers 431 including a secondary transfer roller 431A. The secondary transfer belt 432 is stretched by the secondary transfer roller 431A and the support rollers 431 in a loop shape.
[0072] The fixing section 60 is disposed as a unit within the fixing device F. The fixing section 60 has a fixing roller 62, a heat generating belt 63 for heating the fixing roller 62, and a pressure roller 64 disposed so as to be biased relative to the fixing roller 62.
[0073] The paper transport section 50 includes a paper feed section 51, a paper discharge section 52, and a transport section 53. The three paper feed tray units 51a to 51c that make up the paper feed section 51 store paper S, identified based on basis weight, size, and the like, by preset type. The paper S corresponds to a recording medium, and is, for example, standard paper, special paper, etc. The transport section 53 includes a pair of intermediate transport rollers 53a.
[0074] In the image forming apparatus 1, the automatic document feeder 11 conveys the document D placed on the document tray by a conveying mechanism and sends it to the document image scanning device 12. The automatic document feeder 11 can continuously read images (including both sides) of a large number of documents D placed on the document tray at once. The document image scanning device 12 optically scans the document conveyed from the automatic document feeder 111 onto the contact glass or the document placed on the contact glass, and forms an image of the reflected light from the document on the light receiving surface of a CCD (Charge Coupled Device) sensor 112a to read the document image. The image reading unit 10 generates input image data based on the reading result by the document image scanning device 112. This input image data is subjected to predetermined image processing in the image processing unit 30 as necessary.
[0075] The control unit 70 controls a drive current supplied to a drive motor (not shown) that rotates the photoconductor 413. This causes the photoconductor 413 to rotate at a constant peripheral speed. The charging unit 414 uniformly charges the surface of the photoconductor 413, which has photoconductivity, to a negative polarity. The exposure unit 411 irradiates the photoconductor 413 with laser light corresponding to an image of each color component, and an electrostatic latent image of each color component is formed on the surface of the photoconductor 413 due to a potential difference with the surroundings. The developing unit 412 visualizes the electrostatic latent image by attaching toner of each color component to the surface of the photoconductor 413, thereby forming a toner image.
[0076] Meanwhile, intermediate transfer belt 421 runs at a constant speed in the direction of arrow A by the rotation of support roller 423, which serves as a drive roller. Intermediate transfer belt 421 is pressed against photoconductor 413 by primary transfer roller 422 to form a primary transfer nip, and the toner images of each color on photoconductor 413 are primarily transferred onto intermediate transfer belt 421 so that the toner images of each color are sequentially superimposed on each other. Residual toner remaining on the surface of photoconductor 413 is removed from the surface after primary transfer by the elastic blade of drum cleaning device 415, which comes into contact with the surface of photoconductor 413.
[0077] On the other hand, a secondary transfer nip is formed by pressing secondary transfer roller 431A against backup roller 423A via intermediate transfer belt 421. Paper S fed from paper discharge unit 51 is transported to the secondary nip transfer unit. The inclination and widthwise position (bias) of paper S are corrected during the process of being transported by transport unit 53.
[0078] When the paper S passes through the secondary transfer nip portion, the toner image carried on the intermediate transfer belt 421 is secondarily transferred to the paper S. The paper S onto which the toner image has been transferred is transported toward the fixing unit 60. Residual toner remaining on the surface of the intermediate transfer belt 421 after the secondary transfer is removed from the surface by the elastic blade of the belt cleaning device 426, which contacts the surface of the intermediate transfer belt 421.
[0079] The fixing unit 60 heats and presses the conveyed paper S in a fixing nip, thereby fixing the toner image onto the paper S. The drive control of the pressure roller 64, heat generating belt 63, etc. is performed by a control unit .
[0080] The heating device heats the heat-generating belt 63, and as a result, the heat-generating belt 63 becomes uniform at a predetermined fixing temperature (e.g., 170°C) across the width. The fixing temperature is a temperature that can supply the thermal energy required to melt the toner on the paper S, and differs depending on the type of paper S on which an image is formed, etc.
[0081] The sheet S on which the desired image has been formed is discharged outside the image forming apparatus 1 by a sheet discharge section 52 having a sheet discharge roller 52a.
[0082] It goes without saying that the present invention is not limited to the above-described embodiment, and various modifications are possible within the scope of the concept of the present invention. EXAMPLES
[0083] Specific examples of the present invention will be described below together with comparative examples, but the present invention is not limited to these.
[0084] 1. Toner manufacturing method (1-1) Preparation of binder resin dispersion a The following components were mixed and dissolved to prepare a raw material solution. Styrene (Wako Pure Chemical Industries, Ltd.): 330 parts by weight n-Butyl acrylate (Wako Pure Chemical Industries, Ltd.): 70 parts by weight β-Carboxyethyl acrylate (manufactured by Rhodia Nikka): 9 parts by weight 1',10-Decanediol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.): 1.5 parts by mass Dodecanethiol (Wako Pure Chemical Industries, Ltd.): 2.7 parts by mass
[0085] A solution was prepared by dissolving 4 parts by mass of anionic surfactant (Dowfax, manufactured by Rhodia) in 550 parts by mass of ion-exchanged water, and the solution was mixed with the above raw material solution, and dispersed and emulsified in a flask. A solution of 6 parts by mass of ammonium persulfate dissolved in 50 parts by mass of ion-exchanged water was added over 10 minutes while slowly stirring and mixing. Next, after thoroughly replacing the system with nitrogen, the flask was heated in an oil bath while stirring until the system reached 70°C, and emulsion polymerization was continued for 5 hours to obtain an anionic resin microparticle dispersion a.
[0086] The resulting resin microparticles had a median particle size of 220 nm, a solid content of 45 mass %, a glass transition point of 53.0° C., a mass average molecular weight Mw of 31,000, and a Z-average molecular weight of 78,000.
[0087] (1-2) Preparation of resin particle dispersion b The following components were mixed and dissolved to prepare a raw material solution. Styrene (Wako Pure Chemical Industries, Ltd.): 330 parts by weight n-Butyl acrylate (Wako Pure Chemical Industries, Ltd.): 70 parts by weight β-Carboxyethyl acrylate (manufactured by Rhodia Nikka): 9 parts by weight 1',10-Decanediol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.): 1.2 parts by mass
[0088] A solution was prepared by dissolving 8 parts by mass of anionic surfactant (Dowfax, manufactured by Rhodia) in 550 parts by mass of ion-exchanged water, and the solution was mixed with the above raw material solution, and dispersed and emulsified in a flask. While slowly stirring and mixing, 50 parts by mass of ion-exchanged water in which 3 parts by mass of ammonium persulfate was dissolved was added over 10 minutes. Next, after thoroughly replacing the system with nitrogen, the flask was heated in an oil bath while stirring until the system reached 65°C, and emulsion polymerization was continued for 5 hours to obtain an anionic resin microparticle dispersion b.
[0089] The resulting resin microparticles had a median particle size of 200 nm, a solid content of 45 mass %, a glass transition point of 53.5° C., a mass average molecular weight Mw of 780,000, and a Z-average molecular weight of 2,200,000.
[0090] (1-3) Preparation of magnetic material dispersion The following ingredients were mixed and pre-dispersed for 10 minutes using a homogenizer (Ultra Turrax, manufactured by IKA). Magnetite (Toda Kogyo Co., Ltd., particle size 150 nm, saturation magnetization at 796 kA / m 84 Am 2 / g):25 parts by mass Ionic surfactant (Neogen RK, Daiichi Kogyo Seiyaku): 5 parts by weight Ion-exchanged water: 70 parts by weight Thereafter, a counter-impingement wet grinding machine (Altimizer, manufactured by Sugino Machine Co., Ltd.) was used to carry out dispersion processing at a pressure of 245 MPa for 15 minutes to obtain a magnetic material dispersion (solid content 30 mass%). The median particle size of the magnetic material in the obtained magnetic material dispersion was 270 nm.
[0091] (1-4) Preparation of colorant dispersion The following components were mixed and dispersed for 15 minutes at a pressure of 245 MPa using a homogenizer (Ultra Turrax, IK projectile wet mill (Ultimizer, manufactured by Sugino Machine Co., Ltd.) to obtain a colorant dispersion (solid content 30% by mass). Carbon black (R330 manufactured by Cabot Corporation): 25 parts by weight Ionic surfactant (Neogen RK, Daiichi Kogyo Seiyaku): 5 parts by weight Ion-exchanged water: 70 parts by weight The median particle size of the colorant in the resulting colorant dispersion was 150 nm.
[0092] (1-5) Preparation of release agent dispersion The following ingredients were mixed and heated to 130°C, and then homogenized at 560 kg / cm using a Gaulin homogenizer (Gaulin Co., Ltd.). 2 The dispersion treatment was carried out for 30 minutes under a pressure of 1000 g / ml, and then cooled to 50° C. to obtain a release agent dispersion. Polyethylene wax (PW850, manufactured by Toyo Petrolite Co., Ltd.): 200 parts by weight Ionic surfactant (Neogen RK, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.): 10 parts by weight Ion-exchanged water: 630 parts by weight The median particle size of the release agent in the obtained release agent dispersion was 200 nm, and the solid content concentration was 25% by mass.
[0093] (2-1) Adjustment of Toner A The following components were thoroughly mixed and dispersed in a round stainless steel flask using an Ultra Turrax (T50, manufactured by IKA). ·Resin particle dispersion liquid a: 120 parts by mass ·Resin particle dispersion b: 20 parts by mass ·Magnetic material dispersion: 160 parts by mass Colorant dispersion: 16 parts by weight Release agent dispersion: 44 parts by weight
[0094] 0.4 parts by mass of polyaluminum chloride was added to the dispersion obtained above, and the dispersion operation was continued with the Ultra Turrax. After that, the flask was heated to 50°C while stirring in a heating oil bath. After maintaining at 50°C for 60 minutes, 40 parts by mass of resin microparticle dispersion a was slowly added. Then, the pH of the system was adjusted to 5.4 with a 0.5N sodium hydroxide aqueous solution. Then, the stainless steel flask was sealed, and the mixture was heated to 94°C while continuing stirring using a magnetic seal, and maintained for 5 hours.
[0095] After cooling and filtration, the mixture was thoroughly washed with ion-exchanged water, and then subjected to solid-liquid separation by Nutsche suction filtration. The separated solid was redispersed in 3 liters of ion-exchanged water at 40°C, and stirred and washed for 15 minutes at 300 rpm. This process was repeated five more times, and solid-liquid separation was performed using No. 5A filter paper by Nutsche suction filtration. Vacuum drying was then continued for 12 hours to obtain toner particles A (magnetic material ratio 31.5% by mass).
[0096] To 100 parts by mass of the toner particles A, 1.5 parts by mass of dimethyl silicone oil-treated silica (TS720: manufactured by Cabot Corporation, primary particle diameter 12 nm) was added, and mixed and externally added using a sample mill to obtain toner A. The volume average particle diameter D50v of the obtained toner A measured by the Coulter counter method was 6.5 μm.
[0097] (2-2) Adjustment of Toner B Toner B was obtained in the same manner as Toner A, except that the dispersion liquid was changed to the following composition. The magnetic material ratio in toner particles B was 29.0% by mass. The volume average particle diameter D50v of the obtained Toner B measured by the Coulter counter method was 6.5 μm. ·Resin particle dispersion (1): 120 parts by mass ·Resin fine particle dispersion (2): 20 parts by mass ·Magnetic material dispersion: 140 parts by mass Colorant dispersion: 16 parts by weight Release agent dispersion: 44 parts by weight
[0098] (2-3) Adjustment of Toner C Toner C was obtained in the same manner as Toner A, except that the dispersion liquid was changed to the following composition. The magnetic material ratio in toner particles C was 59.3% by mass. The volume average particle diameter D50v of the obtained Toner C measured by the Coulter counter method was 6.7 μm. ·Resin particle dispersion (1): 120 parts by mass ·Resin fine particle dispersion (2): 20 parts by mass ·Magnetic material dispersion: 650 parts by mass Colorant dispersion: 16 parts by weight Release agent dispersion: 44 parts by weight
[0099] (2-4) Adjustment of Toner D Toner D was obtained in the same manner as Toner A, except that the dispersion liquid was changed to the following composition. The magnetic material ratio in toner particles D was 60.1% by mass. The volume average particle diameter D50v of the obtained Toner D measured by the Coulter counter method was 6.7 μm. ·Resin particle dispersion (1): 120 parts by mass ·Resin fine particle dispersion (2): 20 parts by mass ·Magnetic material dispersion: 680 parts by mass Colorant dispersion: 16 parts by weight Release agent dispersion: 44 parts by weight
[0100] (2-5) Adjustment of Toner E Toner E was obtained in the same manner as Toner A, except that the dispersion liquid was changed to the following composition. The magnetic material ratio in toner particles E was 40.6% by mass. The volume average particle diameter D50v of the obtained Toner E measured by the Coulter counter method was 6.6 μm. ·Resin particle dispersion (1): 120 parts by mass ·Resin fine particle dispersion (2): 20 parts by mass ·Magnetic material dispersion: 250 parts by mass Colorant dispersion: 16 parts by weight Release agent dispersion: 44 parts by weight
[0101] (2-6) Adjustment of Toner F Toner F was obtained in the same manner as Toner A, except that the dispersion liquid was changed to the following composition. The magnetic material ratio in toner particles F was 39.8% by mass. The volume average particle diameter D50v of the obtained Toner F measured by the Coulter counter method was 6.6 μm. ·Resin particle dispersion (1): 120 parts by mass ·Resin fine particle dispersion (2): 20 parts by mass ·Magnetic material dispersion: 240 parts by mass Colorant dispersion: 16 parts by weight Release agent dispersion: 44 parts by weight
[0102] 2. Manufacturing method of magnetic carrier (1) Preparation of the core material ·Mixing process The following ferrite raw materials were weighed, and 80 parts by mass of the ferrite raw materials were mixed with 20 parts by mass of water. Then, the mixture was wet mixed in a ball mill for 3 hours using zirconia having a diameter (φ) of 10 mm to prepare a slurry. The solid content of the slurry was 80% by mass. ·Fe2O3:68.3% by mass ·MnCO3:28.5% by mass ·Mg(OH)2:2.0% by mass ·SrCO3: 1.2% by mass
[0103] Pre-firing process The obtained slurry was dried using a spray dryer (manufactured by Okawara Kakoki Co., Ltd.) and then fired in a batch-type electric furnace in a nitrogen atmosphere (oxygen concentration: 1.0% by volume) at a temperature of 1050° C. for 3.0 hours to produce calcined ferrite.
[0104] Crushing process The calcined ferrite was crushed to about 0.5 mm using a crusher, and water was added to prepare a slurry. The solid content of the slurry was set to 70 mass %. The slurry was further crushed for 3 hours using a wet ball mill with 1 / 8 inch stainless steel beads to obtain a slurry. The slurry was crushed for 4 hours using a wet bead mill with 1 mm diameter zirconia to obtain a calcined ferrite slurry with a volume-based 50% particle size (D50) of 1.3 μm.
[0105] ·Granulation process To 100 parts by mass of the calcined ferrite slurry, 1.0 part by mass of ammonium polycarboxylate as a dispersant and 1.5 parts by mass of a binder (polyvinyl alcohol) were added. The mixture was then granulated into spherical particles using a spray dryer (manufactured by Okawara Kakoki Co., Ltd.) and dried. The resulting granulated material was subjected to particle size adjustment, and then heated at 700°C for 2 hours using a rotary electric furnace to remove organic substances such as the dispersant and binder.
[0106] · Firing process In a nitrogen atmosphere (oxygen concentration 1.0% by volume), the temperature was raised from room temperature to the firing temperature (1100°C) over 2 hours, and the temperature was held at 1100°C for 4 hours for firing. The temperature was then lowered to 60°C over 8 hours, and the material was returned from the nitrogen atmosphere to the air and removed at a temperature of 40°C or less.
[0107] ·Sorting process After the agglomerated particles were crushed, they were sieved through a sieve with 150 μm openings to remove coarse particles, air classification to remove fine powder, and magnetic separation to remove low magnetic force particles to obtain porous magnetic particles.
[0108] 100 parts by mass of the porous magnetic particles were weighed out and placed in a stirring vessel of a mixer (Dalton's universal stirrer NDMV type) and heated to 60°C. 5 parts by mass of a filling resin consisting of 95.0% by mass of methyl silicone oligomer and 5.0% by mass of γ-aminopropyltrimethoxysilane was dripped into the stirring vessel at normal pressure. After dripping was completed, stirring was continued while adjusting the time, the temperature was raised to 70°C, and the resin composition was filled into the porous magnetic particles.
[0109] After cooling, the obtained resin-filled magnetic particles were transferred to a mixer (UD-AT type drum mixer manufactured by Sugiyama Heavy Industries Co., Ltd.) with a spiral blade in a rotatable mixing container, and the temperature was raised to 140°C while stirring at a heating rate of 2°C / min under a nitrogen atmosphere. Heating and stirring were then continued at 140°C for 50 minutes. After that, the particles were cooled to room temperature, and the ferrite particles with the resin filled and hardened in the voids were taken out and non-magnetic matter was removed using a magnetic separator. Furthermore, coarse particles were removed using a vibrating sieve to obtain a core material filled with resin. The peak pore diameter of the obtained core material was 0.60 μm, and the pore volume was 75 mm 3 / g.
[0110] (2-1) Preparation of coating resin solution 1 0.38 parts by mass of cyclohexyl methacrylate and 1.62 parts by mass of methyl methacrylate were added to a four-neck flask equipped with a reflux condenser, a thermometer, a nitrogen suction tube, and a grinding stirrer. 3.0 parts by mass of toluene, 3.0 parts by mass of methyl ethyl ketone, and 0.072 parts by mass of azobisisovaleronitrile were further added, and the mixture was kept at 80°C for 10 hours under a nitrogen stream to obtain a coating resin solution 1 (solid content 35% by mass).
[0111] (2-2) Preparation of coating resin solutions 2 to 9 Coating resin solutions 2 to 9 were obtained in the same manner as for coating resin solution 1, except that the ratio of cyclohexyl methacrylate and methyl methacrylate was changed as shown in Table 1.
[0112] [Table 1]
[0113] (3) Preparation of magnetic carrier (3-1) Preparation of magnetic carrier (carrier particle) 1 The coating resin solution was diluted with toluene so that the concentration of the coating resin in the above-mentioned coating resin solution 1 was 5% by mass. Then, the coating resin solution 1 was weighed so that the amount of the coating resin was 2 parts by mass per 100 parts by mass of the core material. Then, the core material was placed in a planetary motion mixer (Nauta Mixer VN type manufactured by Hosokawa Micron Corporation) maintained at a temperature of 60°C, and half of the above-mentioned coating resin solution 1 was added. Then, the resin was applied around the core material while removing the solvent for 30 minutes. Next, the remaining coating resin solution was added, and the resin was applied around the core material for 40 minutes.
[0114] Thereafter, the magnetic carrier on which the resin coating layer was formed was transferred into a mixing vessel of a drum mixer UD-AT type mixer manufactured by Sugiyama Heavy Industries Co., Ltd., which has a rotatable mixing vessel (with a spiral blade inside), and heat-treated for 2 hours at a temperature of 120°C in a nitrogen atmosphere while stirring by rotating the mixing vessel 10 times per minute. The obtained particles were separated into low magnetic particles by magnetic separation, and passed through a sieve with an opening of 150 μm. Then, the particles were classified by a wind classifier to obtain magnetic carrier 1. The arithmetic average roughness Ra of the particle surface of magnetic carrier 1 was 0.30 μm.
[0115] (3-2) Preparation of Magnetic Carriers 2 to 9 Magnetic carriers 2 to 9 were obtained, except that the coating resin solution 1 was changed to coating resin solutions 2 to 9.
[0116] 3. Preparation of two-component developer As shown in Table 2 below, the toner and the magnetic carrier were combined, and each material was shaken in a shaker (YS-8D type, manufactured by Yayoi Co., Ltd.) so that the toner concentration was 8% by mass. The vibration conditions of the shaker were 200 rpm and 2 minutes.
[0117] 4. Evaluation (1) Durability test method The image forming apparatus used was a modified imagePRESS C850 color copier manufactured by Canon Inc. A two-component developer was placed in the developing section (developer container) of the image forming apparatus, and a printed matter was produced.
[0118] Durability test in N / L environment: A specified number of prints were made using a FFH output chart with an image ratio of 1% at a temperature of 23°C / humidity of 5RH%. Durability test in H / H environment: A certain number of sheets were printed using a FFH output chart with an image ratio of 1% at a temperature of 30°C and humidity of 80RH%. Note that FFH is a hexadecimal value representing 256 gradations, with 00h being the first gradation (white background) of the 256 gradations, and FFH being the 256th gradation (solid background) of the 256 gradations.
[0119] (conditions) Paper: Laser beam printer paper CS-814 (81.4 g / m 2 ) (Canon Marketing Japan) Image formation speed: Modified to be able to print A4 size, full color, 90 sheets / min. Development conditions: The development contrast was made adjustable to any value, and the automatic correction by the main unit was not activated. The peak-to-peak voltage (Vpp) of the alternating electric field was modified to a frequency of 2.0 kHz, so that Vpp could be changed in 0.1 kV increments from 0.7 kV to 1.8 kV. Each color was modified so that a monochrome image could be output.
[0120] (2) Fog evaluation A solid image (solid white image) with an image ratio of 100% and 00h was printed on A3 size paper (CS-814) in a H / H environment and judged according to the following criteria. The average reflectance Dr (%) of six points on the unprinted paper and the average reflectance Ds (%) of six points on the printed paper were measured using a reflectometer (Tokyo Denshoku Co., Ltd., REFLECTOMETER MODEL TC-6DS) to determine the fogging rate (%). Fog rate (%) = Dr (%) - Ds (%) Furthermore, the durability test (printing 20,000 sheets) was conducted in the H / H environment. After that, the fog rate was calculated under the same development conditions as before the durability test. The results are shown in Table 2. A to I are in the acceptable range.
[0121] <Evaluation criteria> A: Fog rate is less than 0.2% B: Fog rate is 0.2% or more and less than 0.4% C: Fog rate is 0.4% or more and less than 0.6% D: Fog rate is 0.6% or more and less than 0.8% E: Fog rate is 0.8% or more and less than 1.0% F: Fog rate is 1.0% or more and less than 1.2% G: Fog rate is 1.2% or more and less than 1.4% H: Fog rate is 1.4% or more and less than 1.6% I: Fog rate is 1.6% or more and less than 2.0% J: Fog rate is 2.0% or more
[0122] (3) Ghost evaluation The mechanism for discharging the excess magnetic carrier from the developing section was removed from the image forming apparatus. The amount of toner on the paper in the FFH image (solid black image) was 0.45 mg / cm2. 2 It was adjusted so that Then, 10,000 sheets were printed under N / L environment. The 10,000 sheets were printed continuously under the same development and transfer conditions (without calibration) as the first sheet. The evaluation paper was plain copy paper GF-C081 (A4 size, basis weight 81.4 g / m 2 , manufactured by Canon Marketing Japan) was used.
[0123] After 10,000 sheets of paper were printed (image output), the solid black (toner amount 0.45 mg / cm) shown in Figure 2 was printed. 2 ) and the rest of the test chart was solid white (left white) and 999 sheets were printed in succession. After that, as the 1000th sheet, within the same job, a full-face halftone image (1200 dpi, 1 line formed by 2 dots and 2 spaces) as shown in Figure 3 was printed.
[0124] Region (a) in FIG. 3 corresponds to the solid black vertical band shown in FIG. 2, and region (b) corresponds to the solid white region shown in FIG. 2. The image density of region (a) and region (b) shown in FIG. 3 were measured, and the ghost was evaluated based on the difference in density. Regions (a) and (b) are within the range of the first rotation of the developer transport member (transport roller). In other words, the width of regions (a) and (b) shown in FIG. 3 is equal to the circumference of the developer transport member (transport roller), which is 6.3 mm. The image density was measured using an X-Rite color reflection densitometer (X-rite500Series, manufactured by X-rite).
[0125] The measurements were carried out at a temperature of 23° C. and a relative humidity of 5%. The concentration difference was ranked according to the following evaluation criteria. A to C are in the acceptable range. A: The density difference between area (a) and area (b) is less than 0.02. B: The density difference between area (a) and area (b) is 0.02 or more and less than 0.04. C: The density difference between area (a) and area (b) is 0.04 or more and less than 0.06. D: The density difference between area (a) and area (b) is 0.06 or more and less than 0.10.
[0126] (3) Evaluation of in-plane density unevenness Under N / L environment, a FFH image of 200 mm x 280 mm size was printed on A4 size paper (CS-814) (toner load on paper: 0.35 mg / cm 2 ), and the resulting image was divided into 140 sections of 20 mm x 20 mm each, and the density of the center of each image was measured using an X-Rite color reflection densitometer (X-Rite 404A). Of the resulting image densities, the maximum was taken as Dmax and the minimum was taken as Dmin, and the difference between these, Dmax - Dmin, was calculated and the in-plane density unevenness was evaluated according to the following criteria. Furthermore, a durability test (printing 20,000 sheets) was conducted in an N / L environment. After that, the in-plane density unevenness was evaluated in the same manner as before the durability test. The respective results are shown in Table 2. A to I are in the acceptable range. <Evaluation criteria> A: 0.00≦Dmax-Dmin≦0.02 B: 0.02 <Dmax-Dmin≦0.05 C: 0.05 <Dmax-Dmin≦0.08 D: 0.08 <Dmax-Dmin≦0.10 E:0.10 <Dmax-Dmin≦0.13 F:0.13 <Dmax-Dmin≦0.15 G: 0.15 <Dmax-Dmin≦0.18 H:0.18 <Dmax-Dmin≦0.20 I:0.20 <Dmax-Dmin≦0.25 J:0.25 <Dmax-Dmin
[0127] [Table 2]
[0128] As shown in the above table, a two-component developer that combines a toner containing toner particles containing 30% by mass or more and 60% by mass or less of a magnetic material with a magnetic carrier containing carrier particles having a resin coating layer containing a polymer of an alicyclic (meth)acrylate monomer around a core material was less likely to cause fogging, ghosting, and in-plane density unevenness (Examples 1 to 10).
[0129] In contrast, in a two-component developer in which the magnetic material content in the toner particles is less than 30% by mass, ghosting was likely to occur (Comparative Example 2). One of the reasons for this is thought to be the low fluidity of the toner particles. On the other hand, when the magnetic material content in the toner particles exceeds 60% by mass, not only ghosting but also fogging was likely to occur (Comparative Example 1). In this case, since the amount of magnetic material in the toner particles is large, it is considered that the toner particles are difficult to move from the conveying roller of the developing section of the printing machine to the image carrier side. Furthermore, when the resin coating layer of the magnetic carrier does not contain a polymer of an alicyclic (meth)acrylate monomer, not only ghosting and fogging were likely to occur, but also in-plane density unevenness was likely to occur (Comparative Example 1). It is considered that the magnetic carrier was easily deteriorated. [Industrial Applicability]
[0130] According to the present invention, there are provided a two-component developer which is unlikely to cause fogging or ghosting on printed matter and has high durability, and an image forming apparatus which uses the two-component developer. [Explanation of symbols]
[0131] 1. Image forming device 10 Image reading unit 20 Operation display section 30 Image processing section 40 Image forming section 41, 41Y, 41M, 41C, 41K Image forming unit 42 Intermediate transfer unit 43 Secondary transfer unit 50 Paper transport section 51 Paper feed section 51a, 51b, 51c Paper feed tray unit 52 Paper output section 52a Paper ejection roller 53 Conveyor 53a Intermediate conveying roller pair 60 Fixing unit 62 Fixing roller 63 Heating Belt 64 Pressure roller 70 Control section 111 Automatic document feeder 112 Scanner 112a CCD sensor 411 Exposure section 412 Development section 413 Photoconductor (image carrier) 414 Charging section 415 Drum cleaning device 421 Intermediate transfer belt 422 Primary transfer roller 423, 431 Support roller 423A Backup roller 426 Belt cleaning device 431 Support Roller 431A Secondary transfer roller 432 Secondary transfer belt D Manuscript S paper
Claims
1. A two-component developer including a toner and a magnetic carrier, The toner includes toner particles containing a binder resin and a magnetic material, the amount of the magnetic material in the toner particles is 30% by mass or more and 60% by mass or less, The magnetic carrier includes carrier particles having a magnetic core material and a resin coating layer that coats the core material, The resin coating layer contains a polymer of an alicyclic (meth)acrylate monomer, Two-component developer.
2. the proportion of the structural units derived from the alicyclic (meth)acrylate monomer relative to the total structural units of the polymer is 20 to 80 mass%; The two-component developer according to claim 1 .
3. the proportion of the structural units derived from the alicyclic (meth)acrylate monomer relative to the total structural units of the polymer is 40 to 80 mass%; The two-component developer according to claim 1 .
4. the proportion of the structural units derived from the alicyclic (meth)acrylate monomer relative to the total structural units of the polymer is 60 to 80 mass%; The two-component developer according to claim 1 .
5. The alicyclic (meth)acrylate monomer comprises cyclohexyl methacrylate; The two-component developer according to claim 1 .
6. An image carrier; a developing section for supplying toner to the electrostatic latent image formed on the surface of the image carrier; Including, The developing unit comprises: A developer container that contains the two-component developer according to any one of claims 1 to 5; a developer transport member supported rotatably and facing the image carrier; the developer transport member includes a magnet roll therein and carries the two-component developer on a surface thereof, thereby transporting the developer from the developer container side to the image carrier side; Image forming device.
7. the developing unit has a bias application unit for applying an AC bias voltage to the developer transport member; The image forming apparatus according to claim 6.
Citation Information
Patent Citations
Toner, and developing device, image forming apparatus and image forming method using toner
JP2006072137A
Cited By
vehicle
DE102025132207A1