Laminate for dry food packaging and dry food packaging bag using the same
A laminate with a biaxially stretched polypropylene base layer and ethylene α-olefin copolymer heat-sealing layer addresses the challenges of impact resistance, low-temperature heat-sealability, and bag-manufacturability, enhancing environmental sustainability and manufacturing efficiency.
Patent Information
- Application Number
- JP2023066306
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Existing packaging laminates and bags face challenges in achieving both impact resistance, low-temperature heat-sealability, and bag-manufacturability while considering environmental sustainability and reducing the number of layers.
A laminate structure comprising a biaxially stretched polypropylene base layer with an elastic modulus of 500 MPa or more and a heat-sealing layer made of polypropylene with ethylene α-olefin copolymer, optimized for low-temperature heat-sealability, combined with specific additives for improved properties.
The laminate achieves excellent heat resistance, impact resistance, and low-temperature heat-sealability, allowing for high-speed bag manufacturing with reduced material usage and improved environmental performance.
Smart Images

Figure 2024152239000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a dry food packaging laminate for food packaging and a dry food packaging bag using the same. [Background technology]
[0002] Common laminates and packaging bags for food packaging are made by laminating a heat-resistant base material such as biaxially oriented polyethylene terephthalate film (hereinafter sometimes referred to as PET) or biaxially oriented polyamide film (hereinafter sometimes referred to as ON) with a non-oriented polyethylene film (hereinafter sometimes referred to as PE) or polypropylene film (hereinafter sometimes referred to as CPP), and using the laminates PET / ON / PE or CPP, PET / PE or CPP, and OPP (biaxially oriented polypropylene film) / ON / PE or CPP. The required properties of these packaging bags are heat resistance, impact resistance, heat sealability, bag-making processability, etc.
[0003] In recent years, laws related to environmental friendliness of packaging have been enacted, making it essential for packaging bags to be designed with environmental considerations in mind. As a result, there is an increasing demand for packaging bags that have a reduced number of layers in multi-layer laminate films and that are made of mono-material, similar materials that are highly suitable for recycling.
[0004] Therefore, laminates of similar materials with an OPP / CPP structure, such as a biaxially oriented polypropylene film (hereinafter sometimes referred to as OPP), which has a high elastic modulus at high temperatures, and a CPP sealant layer, are also being considered, and there are increasing demands for the CPP sealant layer to have high impact resistance, low-temperature heat sealability, and slipperiness.
[0005] To solve the above problems, Patent Document 1 proposes an OPP in which a heat seal layer is laminated on one side of PP (polypropylene) with a high elastic modulus, and Patent Document 2 proposes a laminate in which a CPP is laminated on one side of an OPP with a low thermal shrinkage rate; however, these products do not sufficiently achieve both impact resistance and low-temperature heat sealability, and are also inferior in bag-making processability. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2020-7441 A [Patent Document 2] JP 2023-13959 A Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, the object of the present invention is to provide a laminate for packaging dry foods, which is excellent in heat resistance, impact resistance, and low-temperature heat sealability, and has excellent bag formability like conventional packaging bags, as a packaging bag for packaging food using the same material with consideration for the environment, and to provide a packaging bag for dry foods using the same. [Means for solving the problem]
[0008] The present inventors have come to solve the above problems by providing a laminate having the following configuration and a packaging bag using the same: That is, the laminate is a base layer and a heat seal layer, the base layer being a biaxially stretched film mainly composed of polypropylene having a longitudinal and transverse elastic modulus of 500 MPa or more at 100°C, the heat seal layer being mainly composed of polypropylene, containing an ethylene-α-olefin copolymer, having a melting point of 125°C or more and 145°C or less, and having a 719 cm -1 Peak of 973cm -1 The laminate for packaging dry foods has a seal strength of 15 N / 15 mm or more when the heat seal layers are overlapped and heat sealed at 135°C, and a packaging bag for dry foods using the same. Effect of the Invention
[0009] According to the present invention, it is possible to provide a laminate for packaging dry foods, which is a mono-material food packaging bag made of similar materials with consideration for the environment, maintains excellent heat resistance and impact resistance, has excellent low-temperature heat sealing properties and bag formability, and allows for reduction in the weight of the packaging bag, and a packaging bag for dry foods using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The dry food packaging laminate of the present invention and the dry food packaging bag using the same will be specifically described below. The laminate of the present invention is a laminate having a two-layer structure of a base layer and a heat seal layer. The base layer is a biaxially oriented film mainly composed of polypropylene having a modulus of elasticity in both the longitudinal and transverse directions at 100°C of 500 MPa or more. The heat seal layer is mainly composed of polypropylene, contains an ethylene-α-olefin copolymer, has a melting point of 125°C or more and 145°C or less, and has a 719 cm -1 Peak of 973cm -1 The value obtained by dividing the peak value by the peak value is in the range of 0.1 or more and 0.3 or less.
[0011] The elastic modulus of the biaxially stretched film, the main component of which is polypropylene, in the base layer is 500 MPa or more in both the longitudinal and transverse directions at 100°C, so that when a laminate having a heat seal layer laminated thereon is used to produce a packaging bag by sealing three sides of the laminate with a three-side seal packaging machine, a bag-making speed of 40 spm (shots per minute) or more can be achieved. If the elastic modulus is less than 500 MPa, the shape retention during bag making using the laminate decreases, and the content protection after food packaging may be poor. Here, the longitudinal and transverse directions of the biaxially stretched film refer to the direction parallel to the film-forming direction as the longitudinal direction (longitudinal direction or MD direction), and the direction perpendicular to the film-forming direction within the film plane as the transverse direction (transverse direction or TD direction).
[0012] The term "mainly composed of polypropylene" means that the polypropylene content is 50% by mass or more based on the total amount of the resin in the base layer.
[0013] The polypropylene is selected from homopolymers, ethylene-propylene random copolymers, ethylene-propylene block copolymers, and ethylene-propylene-butene random copolymers. When used as the base layer of the present invention, homopolymer polypropylene is preferred in terms of its elastic modulus at 100°C.
[0014] The polypropylene preferably has a xylene soluble portion at 20°C (hereinafter sometimes referred to as CXS) of 4% by mass or less, a mesopentad fraction of a xylene insoluble portion at 20°C (hereinafter sometimes referred to as CXIS) of 95% or more, and a melt flow rate (hereinafter sometimes referred to as MFR) of 1 g / 10 min or more and 10 g / 10 min or less (230°C, 21.18 N load).
[0015] The xylene soluble portion (CXS) of the polypropylene at 20°C is preferably 4% by mass or less, more preferably 3% by mass or less, and particularly preferably 2% by mass or less. The lower the CXS, the better, but the lower limit is about 0.1% by mass. To obtain polypropylene having such a CXS, a method of increasing catalytic activity when obtaining the resin, or a method of washing the obtained resin with a solvent or propylene monomer itself can be used. By making the CXS 4% by mass or less, the elastic modulus at 100°C is 500 MPa or more, and the thermal shrinkage rate at 130°C in the vertical and horizontal directions when the three-side sealed packaging bag is produced is 5% or less.
[0016] The polypropylene preferably has a mesopentad fraction of 95% or more, more preferably 96% or more, and even more preferably 97% or more, of the xylene insoluble portion (CXIS) at 20°C. The mesopentad fraction is an index of the stereoregularity of the crystalline phase of polypropylene measured by nuclear magnetic resonance (NMR), and the higher the value, the higher the crystallinity and melting point, which is preferable for use at high temperatures. There is no particular upper limit for the mesopentad fraction, but if it exceeds 99%, biaxial stretching becomes difficult. In order to obtain a resin with such high stereoregularity, a method of washing the resin powder obtained with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or cocatalyst, and a method of appropriately selecting a composition are preferably used.
[0017] The polypropylene preferably has an MFR of 1 g / 10 min or more and 10 g / 10 min or less (230° C., 21.18 N load), more preferably 2 g / 10 min or more and 7 g / 10 min or less, from the viewpoint of film formability. In order to adjust the MFR to the above value, a method of controlling the average molecular weight or molecular weight distribution is adopted.
[0018] The polypropylene is mainly composed of a homopolymer of propylene, but may contain copolymerization components of other unsaturated hydrocarbons within the scope of the present invention, or may be blended with polymers other than propylene alone. Examples of monomer components constituting such copolymerization components or blends include ethylene, propylene (in the case of copolymerized blends), 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, vinylcyclohexene, styrene, allylbenzene, cyclopentene, norbornene, and 5-methyl-2-norbornene. From the viewpoint of improving the elastic modulus, it is preferable that the copolymerization amount or blend amount is less than 1 mol% in terms of copolymerization amount and less than 10 mass% in terms of blend amount.
[0019] The melting point of the base material layer is preferably 160° C. or higher, more preferably 163° C. or higher. The melting point of polypropylene can be measured using a differential scanning calorimeter (DSC). The high melting point makes it suitable for bag making, and allows the production of packaging bags with little deviation in size or pitch of the bag product.
[0020] The above-mentioned base layer may contain various additives, such as a crystal nucleating agent, an antioxidant, a heat stabilizer, a slipping agent, an antistatic agent, an antiblocking agent, a filler, a viscosity modifier, and a coloring inhibitor, within the scope of the invention.
[0021] Among these, the selection of the type and amount of antioxidant is important from the viewpoint of long-term stability. That is, the antioxidant is a phenolic type having steric hindrance, and at least one of them is preferably a high molecular weight type having a molecular weight of 500 or more. Specific examples include various types, and it is preferable to use 2,6-di-t-butyl-p-cresol (BHT) together with 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., "Irganox" (registered trademark) 1330 manufactured by BASF) or tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (e.g., "Irganox" (registered trademark) 1010 manufactured by BASF) in combination. The total content of these antioxidants is preferably in the range of 0.03 to 1.0 mass% based on the total amount of polypropylene. If the amount of antioxidant is too small, the film may be colored due to thermal degradation during the extrusion process, and long-term heat resistance may be poor. If the amount of antioxidant is too large, the transparency may be reduced due to the bleed-out of the antioxidant. The content is more preferably 0.1 to 0.9% by mass, and particularly preferably 0.2 to 0.8% by mass.
[0022] A crystal nucleating agent can be added to the polypropylene as long as it does not interfere with the object of the present invention. Examples of crystal nucleating agents include α crystal nucleating agents (dibenzylidene sorbitols, sodium benzoate, etc.), β crystal nucleating agents (potassium 1,2-hydroxystearate, magnesium benzoate, amide-based compounds such as N,N'-dicyclohexyl-2,6-naphthalenedicarboxamide, quinacridone-based compounds, etc.). The amount added is preferably 0.01% by mass or more and 0.5% by mass or less. If the amount added is less than 0.01% by mass, no effect of addition is observed, and if it exceeds 0.5% by mass, it may cause a decrease in stretchability or a decrease in transparency and strength due to void formation, etc.
[0023] The base layer preferably contains 100 to 1000 ppm of a fatty acid amide lubricant. If the amount of the fatty acid amide lubricant added is less than 100 ppm, the lubrication may be poor, whereas if it exceeds 1000 ppm, the amount of heat scattering during melt extrusion may increase, causing contamination of the film-forming process and deteriorating film-forming properties.
[0024] Preferred examples of the fatty acid amide lubricants include oleamide, erucamide, stearamide, palmitamide, and behenamide, with erucamide being particularly preferred from the standpoint of dispersibility in the resin composition and ability to provide lubrication.
[0025] It is preferable to add inorganic or organic particles to the base layer in an amount of 300 to 3000 ppm based on the total amount of the resin composition in order to prevent blocking. If the amount added is less than 300 ppm, the effect of the addition is ineffective, whereas if the amount added is more than 3000 ppm, the film-forming process may be contaminated during melt extrusion, resulting in deterioration of film-forming properties.
[0026] Preferred examples of the inorganic particles include silica, zeolite, calcium carbonate, etc. Examples of the organic particles include acrylic resin particles, styrene resin particles, polyolefin resin particles, polyester resin particles, polyurethane resin particles, polycarbonate resin particles, polyamide resin particles, silicone resin particles, fluorine resin particles, and copolymer resin particles of two or more monomers used in the synthesis of the above resins, which may be used alone or in combination.
[0027] The average particle size of the particles is preferably 1 μm or more, more preferably 3 μm or more. If the average particle size is less than 1 μm, the desired arithmetic average surface roughness may not be obtained. On the other hand, the upper limit of the average particle size is preferably 20 μm or less, more preferably 15 μm or less. If the average particle size exceeds 20 μm, the particles may adhere to the lip of the die in a jelly-like manner during film formation, resulting in a decrease in productivity, or the particles may fall off, resulting in a decrease in processability.
[0028] The amount of the particles added is preferably 0.1 to 3% by mass. If the amount is less than 0.1% by mass, the effect of the addition may not be observed, whereas if the amount exceeds 3% by mass, the particles may adhere to the lip of the die in the form of gunk during film formation, resulting in poor productivity, and the total haze may increase, resulting in poor transparency.
[0029] The biaxially oriented polypropylene film of the base layer can be obtained using the above-mentioned raw materials by any of the inflation simultaneous biaxial stretching method, the stenter simultaneous biaxial stretching method, and the stenter sequential biaxial stretching method. Among these, it is preferable to adopt the stenter sequential biaxial stretching method in terms of film formation stability, thickness uniformity, and control of high rigidity and dimensional stability of the film.
[0030] It is preferable that the stretching ratio in the biaxial stretching is 3.5 to 6 times in the longitudinal direction (MD) and 3.5 to 10 times in the transverse direction (TD), since this stably forms the film and gives a film with an elastic modulus of 500 MPa or more in the longitudinal direction (MD) and transverse direction (TD) at 100°C.
[0031] It is preferable that the above-mentioned base material layer is subjected to a surface treatment such as corona discharge treatment, corona discharge treatment in a nitrogen or carbon dioxide gas atmosphere, plasma treatment, or ozone treatment, which is usually carried out industrially, at least on the laminate side with the CPP of the heat seal layer, to have a wettability index of 36 mN / m or more.
[0032] The biaxially oriented polypropylene film for the base layer is not limited to that produced by the above method, and a commercially available film may be used as long as it has an elastic modulus of 500 MPa or more in the longitudinal direction (MD direction) and transverse direction (TD direction) at 100°C.
[0033] The heat seal layer of the laminate is composed mainly of polypropylene, contains an ethylene-α-olefin copolymer, has a melting point of 125°C or higher and 145°C or lower, and has a thermal expansion coefficient of 719 cm by infrared absorptiometry. -1 Peak of 973cm -1 When the heat seal layers are overlapped and heat sealed at 135° C., the seal strength is 15 N / 15 mm or more.
[0034] The term "polypropylene as the main component" in the heat seal layer means that the polypropylene content is 50% by mass or more relative to the total amount of the heat seal layer resin. If the polypropylene content is less than 50% by mass, it is difficult to obtain a seal strength of 15 N / 15 mm when the heat seal layers are overlapped and heat sealed at 135°C.
[0035] The polypropylene may be selected from homopolymers, ethylene-propylene random copolymers, ethylene-propylene block copolymers, and ethylene-propylene-butene random copolymers, with ethylene-propylene random copolymers (hereinafter sometimes referred to as EPC) being preferred in terms of heat seal strength.
[0036] The ethylene-propylene random copolymer (EPC) is preferably one obtained by copolymerizing polypropylene with one or more members selected from 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, and 1-octene.
[0037] From the viewpoint of heat seal strength, the copolymerization amount is preferably 1 mol% or more and 10 mol% or less. If the copolymerization amount is less than 1 mol%, the heat seal strength will be low, and if it exceeds 10 mol%, the blocking force will be high, and the film will be prone to wrinkles when wound up and may break when unwound.
[0038] The melting point of the heat seal layer is preferably 125°C or more and 145°C or less. The melting point can be measured using a differential scanning calorimeter (DSC). If the melting point is less than 125°C, the blocking force is high, which may cause the bag to be difficult to open when filling the bag with contents, and may slow down the bag making speed. If the melting point exceeds 145°C, the heat seal strength at 135°C will drop to 15N / 15mm or less.
[0039] By including an ethylene-α-olefin copolymer in the heat seal layer, the low-temperature heat sealability and impact resistance are improved, which is preferable.
[0040] The content of the ethylene-α-olefin copolymer is preferably 5% by mass or more and 20% by mass or less. If the content is less than 5% by mass, the effect of improving low-temperature heat sealability and impact resistance is not observed, whereas if the content exceeds 20% by mass, the blocking force becomes high, which may result in poor opening properties of the bag when filling the contents into the bag made using the laminate, and a decrease in the bag making speed.
[0041] The ethylene-α-olefin copolymer is a copolymer of 50 to 95% by mass of ethylene as a main component and an α-olefin as a copolymerization monomer, and specifically, it is preferable to use one produced by using a metallocene catalyst.
[0042] As the α-olefin, propylene, 1-butene, 1-hexene, 1-octene, etc., having 3 to 10 carbon atoms can be used. Specific examples of ethylene-α-olefin include ethylene-propylene copolymer elastomers, ethylene-butene copolymer elastomers, ethylene-octene copolymer elastomers, linear low-density polyethylenes in which ethylene is copolymerized with α-olefins such as butene, octene, hexene, etc., and in particular, ethylene-propylene copolymer elastomers and ethylene-butene copolymer elastomers are preferred from the standpoint of impact resistance.
[0043] The MFR of the ethylene / α-olefin copolymer is preferably in the range of 0.5 to 10 g / 10 min at 190° C. under a load of 21.18 N, from the viewpoints of miscibility with polypropylene resins and blocking resistance.
[0044] The content of ethylene and rubber components in the heat seal layer was measured by a Fourier transform infrared spectrophotometer (measured by infrared absorptiometry) and found to be 719 cm -1 The peak intensity at 973cm -1 It is preferable that the value obtained by dividing the peak intensity by the peak intensity is 0.1 or more and 0.3 or less. -1 The peak intensity at 973cm -1 If the value obtained by dividing the peak strength by the heat sealability is less than 0.1, the impact resistance and low-temperature heat sealability are poor, and when the laminate is used as a packaging bag and the contents are filled therein, the contents may leak from the packaging bag when the bag is dropped. If the value exceeds 0.3, the heat seal layers may block each other, resulting in poor opening properties when the contents are filled in a bag making machine, and the contents may leak or the bag making speed may decrease.
[0045] The heat seal layer may contain, within the scope of the object of the present invention, an antioxidant, a heat stabilizer, a neutralizing agent, an antistatic agent, a hydrochloric acid absorbent, an antiblocking agent, a lubricant, etc. These additives may be used alone or in combination of two or more.
[0046] Specific examples of antioxidants include hindered phenols such as 2,6-di-t-butylphenol (BHT), n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate ("Irganox" 1076, "Sumilizer" BP-76), tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane ("Irganox" 1010, "Sumilizer" BP-101), and tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate ("Irganox" 3114, Mark AO-20).
[0047] Phosphite (phosphorus) antioxidants include tris(2,4-di-t-butylphenyl)phosphite ("Irgafos" 168, Mark 2112), tetrakis(2,4-di-t-butylphenyl)-4-4'-biphenylene-diphosphonite ("Sandstab" P-EPQ), bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite ("Ultranox" 626, Mark PEP-24G), distearyl pentaerythritol diphosphite (Mark PEP-8), and the like.
[0048] Among these, 6-[3-(3-t-butyl-4-hydroxy-5-methyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]-dioxaphosphepine ("Sumilizer" GP) and 2[1-2-hydroxy-3,5-di-t-pentylphenyl]ethyl]-4,6-di-t-pentylphenyl acrylate ("Sumilizer" GS) which combine both hindered phenol and phosphite functions are preferred, and the combined use of these two is particularly preferred because it is effective in suppressing resin decomposition during film formation and contributes to achieving both impact resistance and blocking resistance.
[0049] The amount of antioxidant to be added may be appropriately set within the range of 100 to 10,000 ppm, depending on the type of antioxidant used.
[0050] As the neutralizing agent, hydrotalcite compounds, calcium hydroxide, etc. are preferable for reducing smoke generation during film formation.
[0051] The heat seal layer preferably contains 100 to 1000 ppm of fatty acid amide lubricant based on the total amount of the resin composition. If the amount of fatty acid amide lubricant added is less than 100 ppm, the lubricity may deteriorate, and if it exceeds 1000 ppm, the amount of heat scattering during melt extrusion increases, causing contamination of the film-forming process, deteriorating film-forming properties, and reducing heat seal strength.
[0052] Preferred examples of the fatty acid amide lubricants include oleamide, erucamide, stearamide, palmitamide, and behenamide, with erucamide being particularly preferred from the standpoint of dispersibility in the resin composition and ability to provide lubrication.
[0053] It is preferable to add inorganic or organic particles to the heat seal layer in an amount of 300 to 3000 ppm based on the total amount of the resin composition in order to prevent blocking. If the amount is less than 300 ppm, the effect of the addition is not obtained, whereas if the amount is more than 3000 ppm, the film-forming process may be contaminated during melt extrusion, resulting in deterioration of film-forming properties and a decrease in heat seal strength.
[0054] Preferred examples of the inorganic particles include silica, zeolite, calcium carbonate, etc. Examples of the organic particles include acrylic resin particles, styrene resin particles, polyolefin resin particles, polyester resin particles, polyurethane resin particles, polycarbonate resin particles, polyamide resin particles, silicone resin particles, fluorine resin particles, and copolymer resin particles of two or more monomers used in the synthesis of the above resins, which may be used alone or in combination.
[0055] The average particle size of the particles is preferably 1 μm or more, more preferably 3 μm or more. If the average particle size is less than 1 μm, the desired arithmetic average surface roughness may not be obtained. On the other hand, the upper limit of the average particle size is preferably 20 μm or less, more preferably 15 μm or less. If the average particle size exceeds 20 μm, the particles may adhere to the lip of the die in a jelly-like manner during film formation, resulting in a decrease in productivity, or the particles may fall off, resulting in a decrease in processability.
[0056] The amount of the particles added is preferably 0.1 to 3% by mass. If the amount is less than 0.1% by mass, the effect of the addition may not be observed, whereas if the amount exceeds 3% by mass, the particles may adhere to the lip of the die in the form of gunk during film formation, resulting in poor productivity, and the total haze may increase, resulting in poor transparency.
[0057] The heat seal layer is preferably a non-oriented film in terms of heat seal strength. Methods for obtaining a non-oriented film include a method of melting the resin composition, extruding it from a T-shaped die onto a cooling drum and cooling and solidifying it, and a method of melt-extruding it onto the biaxially oriented polypropylene and laminating it, but in the present invention, a non-oriented film extruded from a T-shaped die onto a cooling drum and cooling and solidifying it is preferred because it has high heat seal strength.
[0058] It is preferable that the thickness of the base layer of the laminate of the present invention is 20 μm or more and 30 μm or less, and the thickness of the heat seal layer is 50 μm or more and 70 μm or less, since this provides impact resistance and low-temperature heat sealability and maintains bag formability.
[0059] The dry lamination adhesive for laminating the base layer and heat seal layer of the laminate is not particularly limited, but examples include two-liquid reaction type aromatic adhesives composed of a first liquid consisting of one or more polyols selected from the group consisting of polyurethane polyols, polyester polyols, and polyether polyols, and a second liquid (curing agent) consisting of an isocyanate, or adhesives formed from a two-liquid reaction type aliphatic adhesive, a polyurethane adhesive, an acrylic adhesive, an epoxy adhesive, a polyolefin adhesive, an elastomer adhesive, a fluorine-based adhesive, etc.
[0060] The thickness of the adhesive layer is preferably 0.5 to 5 μm, more preferably 0.5 to 3.0 μm. If the thickness of the adhesive layer is 0.5 μm or more, it is easy to control the film thickness, and if it is 5 μm or less, it is easy to shorten the drying time and reduce the production cost while imparting sufficient adhesive strength.
[0061] The heat seal strength is preferably 15 N / 15 mm or more when the heat seal layers of the laminate are overlapped and heat sealed at 135° C. If the heat seal strength is less than 15 N / 15 mm, the laminate may be used in a packaging bag and the contents may be packed therein, and the contents may leak from the packaging bag during transportation, loading, or when the bag is dropped.
[0062] The heat shrinkage rate of the laminate in both the longitudinal direction and the transverse direction at 130°C is preferably 5% or less. If the heat shrinkage rate in the longitudinal direction (MD) and the transverse direction (TD) at 130°C exceeds 5%, twists and wrinkles occur in the packaging bag, which deteriorates the appearance and reduces the commercial value, which is not preferable. Here, the heat shrinkage rate is calculated by cutting out five samples of 10 mm wide and 200 mm long (measurement direction) from the laminate, marking the positions 25 mm from both ends as benchmarks, measuring the distance between the benchmarks with a universal projector to determine the test length (10), then sandwiching the test pieces between paper and heating them in an oven kept at 130°C for 60 minutes under zero load, removing them, cooling them at room temperature, and then measuring the dimensions (1 l ) was measured using a universal projector and calculated using the formula below. The average value of five pieces was taken as the thermal shrinkage rate. Heat shrinkage rate = {(10-11) / 10} x 100(%)
[0063] In this application, the direction parallel to the film production direction is referred to as the longitudinal direction (machine direction or MD direction), and the direction perpendicular to the film production direction within the film plane is referred to as the width direction (transverse direction or TD direction).
[0064] In the three-sided sealed packaging bag using the laminate of the base material layer and the heat seal layer, it is preferable that the bag making speed is 40 spm or more when packaging 1 kg of contents at a bottom seal temperature (bottom side) of the packaging bag of the bag making machine of 140 to 150° C., a vertical seal temperature of 130 to 140° C., and a top seal temperature (sealed part after filling with contents) of 130 to 140° C. If the bag making speed is less than 40 spm, the product yield is poor and the production cost is high, which is not preferable.
[0065] In the bags made by the above bag making machine, it is preferable that the bag breakage rate when 1 kg of contents is put in and dropped from a height of 1 m is 5% or less. If the bag breakage rate exceeds 5%, the contents may leak from the packaging bag during transportation or loading of the product or when the bag is dropped, making it less practical.
[0066] The above-mentioned packaging bag can also be used after being processed into a flat bag (flat pouch), a standing pouch, or the like, with the heat seal layer serving as the inner surface of the bag.
[0067] The packaging bag is appropriately selected according to the required characteristics of the packaging bag, such as water vapor barrier performance to meet the shelf life of the packaged food, size and impact resistance to accommodate the weight of the contents, heat seal strength, visibility of the contents, etc. EXAMPLES
[0068] The present invention will be described in detail below with reference to examples, but the scope of the present invention is not limited thereto. In addition, the measurement values of each evaluation item in the detailed description of the present invention and the examples were measured by the following methods.
[0069] (1) Content of 20°C xylene soluble (CXS) and insoluble (CXIS) parts of polypropylene 5 g of polypropylene resin was completely dissolved in 500 ml of boiling xylene (Kanto Chemical Co., Ltd. Grade 1), cooled to 20°C, and left for 4 hours or more. Then, the precipitate and solution were filtered to separate into a xylene-soluble portion and a xylene-insoluble portion. The mass of the xylene-insoluble portion (CXIS) was determined by drying the precipitate at 70°C under reduced pressure, measuring the mass at 23°C, and determining the content (mass%). The xylene-soluble portion (CXS) was determined by drying the filtrate at 70°C under reduced pressure, measuring the mass, and determining the content (mass%).
[0070] (2) Mesopentand fraction The mesopentad fraction (isotactic mesopentad fraction) of the xylene insoluble portion was calculated according to the method described in "Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973)". 13 C-NMR measurements were performed using a BRUKER AVANCE500 at 110°C by dissolving 200 mg of a sample in a mixed solution of o-dichlorobenzene and deuterated benzene at a volume ratio of 8:2 at 135°C.
[0071] (3) Melt flow rate (MFR) In accordance with JIS K-7210-1999, the polypropylene resin was measured at 230°C, and the polyethylene, ethylene-α-olefin copolymer, and ethylene-α-olefin copolymer elastomer were measured at 190°C, with a load of 21.18 N for each.
[0072] (4) Elastic modulus at 100°C Based on JIS K 7127:1999, a biaxially oriented polypropylene film was measured five times in the longitudinal direction (MD) and transverse direction (TD) of the film in an atmosphere of 100°C using an Orientec Tensilon universal material testing machine (PTG-1210, parallel clamping type air jaw), and the average value was calculated.
[0073] (5) Blocking resistance Prepare a film sample with a width of 30 mm and a length of 100 mm. The sealing layers are overlapped in an area of 30 mm x 40 mm, and the sample is weighed at 1 kg / 12 cm. 2 After heating for 24 hours in an oven at 80°C under a load of 100 N / 12 cm, the specimen was left in an atmosphere of 23°C and 65% humidity for 30 minutes or more, after which the shear peel strength was measured at a pulling speed of 300 mm / min using a Tensilon manufactured by Orientec Co., Ltd. 2 If it is less than 20N / 12cm, the blocking resistance is good (〇). 2 If the blocking resistance was more than 100%, it was rated as poor blocking resistance "X".
[0074] (6) Film thickness and thickness composition The film thickness was measured at 10 random locations on the film using a dial gauge in accordance with JIS K7130 (1992) A-2 method, and the average value was taken as the film thickness.
[0075] (7) 719cm Fourier transform infrared spectrophotometer of film -1 and 973cm -1 Peak intensity ratio. The transmission measurement (10 times accumulation) of polypropylene-based film using a Fourier transform infrared spectrophotometer (Shimadzu Corporation IR Tracer-100) showed a wavelength of 719 cm -1 and 973cm -1 The peak intensity of 719 cm was measured. -1 The peak intensity at 973cm -1 This value is an indication of the content of ethylene and rubber components in the film.
[0076] (8) Heat shrinkage rate The type of base material layer and the lamination configuration of the heat seal layer were changed, and the base material layer and the heat seal layer were bonded together by a conventional dry lamination method using an aliphatic ester adhesive (Takelac A385 / Takenate A50, manufactured by Mitsui Chemicals, Inc., adhesive layer thickness 2.5 μm), and the laminate was then aged at 40°C for 3 days to create a laminate.
[0077] Five samples of 10 mm width and 200 mm length (measurement direction) were cut out from the above laminate, and marked with benchmark lines 25 mm from both ends. The distance between the benchmark lines was measured with a universal projector to obtain the test length (10). Next, the test pieces were sandwiched between paper and heated for 60 minutes in an oven kept at 130°C under zero load, and then removed. After cooling at room temperature, the dimension (11) was measured with a universal projector and calculated using the following formula. The average value of the five pieces was determined as the thermal shrinkage rate. Heat shrinkage rate = {(10-1 l ) / 10}× 100(%) In this application, the direction parallel to the film production direction is referred to as the longitudinal direction (machine direction or MD direction), and the direction perpendicular to the film production direction within the film plane is referred to as the width direction (transverse direction or TD direction).
[0078] (9) Bag breakage rate The type of base material layer and the lamination configuration of the heat seal layer were changed, and the base material layer and the heat seal layer were bonded together by a conventional dry lamination method using an aliphatic ester adhesive (Takelac A385 / Takenate A50, manufactured by Mitsui Chemicals, Inc., adhesive layer thickness 2.5 μm), and the laminate was then aged at 40°C for 3 days to create a laminate.
[0079] Using this laminate, 60 packaging bags containing 1 kg of salt were made in a bag making machine at a bottom seal temperature (bottom side) of 140 to 150°C, a vertical seal temperature of 130 to 140°C, and a top seal temperature (sealed part after filling) of 130 to 140°C. The 60 bags were then dropped from a height of 1m to check for leakage of the contents and determine the bag breakage rate. A bag breakage rate of 5% or less was evaluated as "Good", and a rate of more than 5% was evaluated as "Poor".
[0080] (10) Bag making speed In the bag-making conditions for calculating the bag breakage rate in (9) above, the number of packaging bags filled with 1 kg of salt that could be produced in one minute was evaluated as the bag-making speed spm (shots per minute).
[0081] (11) Heat seal strength The heat seal layers of the laminate prepared in (9) were overlapped and heat sealed at 135°C to measure the heat seal strength at a peel speed of 300mm / min using a Tensilon made by Orientec Co., Ltd. If the heat seal strength at 23°C was 15N / 15mm or more by this measurement method, it was evaluated as "Good", and if it was less than 15N / 15mm, it was evaluated as "Poor".
[0082] The compositions and formulations of the various raw materials used in the present invention are described below. The properties of the polypropylene film and the packaging bag produced from the raw material formulations are summarized in Table 1.
[0083] (1) Polypropylene (a1) MFR: 2.2g / 10min CXS amount: 0.5% by mass Mesopentand fraction: 96% Antioxidants: Contains 2000 ppm of "Irganox" (registered trademark) 1010 and 2000 ppm of "Irgafos" (registered trademark) 168 Melting point (Tm): 164℃
[0084] (2) Polypropylene (a2) MFR: 2.5g / 10min CXS amount: 4.5% by mass Mesopentane fraction: 92% Melting point (Tm): 162℃ Antioxidants: Contains 2000 ppm of "Irganox" (registered trademark) 1010 and 2000 ppm of "Irgafos" (registered trademark) 168
[0085] (3) Ethylene-propylene block copolymer (a3) MFR: 2.0g / 10min CXS amount: 12.0% by mass Mesopentane fraction: 92% Melting point (Tm): 162℃ Antioxidants: Contains 2000 ppm of "Irganox" (registered trademark) 1010 and 2000 ppm of "Irgafos" (registered trademark) 168
[0086] (4) Ethylene-propylene random copolymer (a4) Ethylene content: 4% by mass MFR: 3.0g / 10min. Melting point (Tm): 142℃ Antioxidants: Contains 2000 ppm of "Irganox" (registered trademark) 1010 and 300 ppm of "Irgafos" (registered trademark) 168 Inorganic particles: 1.5% by mass
[0087] (5) Ethylene-propylene random copolymer (a5) Ethylene content: 6% by mass MFR: 3.0g / 10min. Melting point (Tm): 132℃ Antioxidants: Contains 2000 ppm of "Irganox" (registered trademark) 1010 and 300 ppm of "Irgafos" (registered trademark) 168 Inorganic particles: 1.5% by mass
[0088] (6) Polyethylene (b1) Linear low density polyethylene copolymerized with butene MFR: 2.2g / 10min Density: 0.921g / cm 3 Melting point: 123℃
[0089] (7) Polyethylene (b2) High Density Polyethylene MFR: 1.1g / 10min Density: 0.950g / cm 3 Melting point: 132℃
[0090] (8) Ethylene-propylene copolymer elastomer (c1) "Tafmer" (registered trademark) manufactured by Mitsui Chemicals, Inc. MFR: 5.0g / 10min Ethylene content: 74% by mass
[0091] (9) Ethylene-butene copolymer elastomer (C2) "Tafmer" (registered trademark) manufactured by Mitsui Chemicals, Inc. MFR: 6.5g / 10min Ethylene content: 85% by mass
[0092] (10) Lubricant masterbatch (d1) (4) Polypropylene-ethylene random copolymer (a4): 95% by mass Erucamide: 5% by mass MFR: 10g / 10min
[0093] [Example 1] As the base layer, polypropylene (a1) was fed into a single-screw melt extruder, melt extruded at a melt temperature of 260°C, and discharged into a casting drum with a surface temperature controlled at 30°C to obtain an unstretched sheet. The sheet was then preheated to 145°C and stretched 4.5 times in the longitudinal direction of the film between rolls with a peripheral speed difference. The film was then introduced into a tenter-type stretching machine with its ends held by clips, preheated at 170°C, stretched 8.0 times at 165°C, and heat-treated at 165°C while giving 10% relaxation in the width direction, and then cooled at 100°C, and one side was subjected to corona discharge treatment to obtain a biaxially stretched polypropylene film with a thickness of 20 μm.
[0094] As the heat seal layer, 89.5% by mass of polypropylene-ethylene random copolymer (a4), 10% by mass of ethylene-propylene copolymer elastomer (c1), and 0.5% by mass of lubricant master batch (d1) were mixed and fed into a twin-screw extruder whose temperature was controlled at 260°C to melt-knead, and then extruded from a T-die at 250°C at 60 m / min., brought into contact with a cooling roll at 45°C to cool and solidify, and then one side was corona discharge treated to obtain a 60 μm-thick unstretched polypropylene film.
[0095] The biaxially oriented polypropylene film and unoriented polypropylene film of the above-mentioned base layer were bonded together by the above-mentioned conventional dry lamination method using an aliphatic ester-based adhesive (Takelac A385 / Takenate A50, manufactured by Mitsui Chemicals, Inc., adhesive layer thickness 2.5 μm), and then aged at 40°C for 3 days to produce a laminate.
[0096] Using the above laminate, packaging bags containing 1 kg of salt were made in a bag making machine at a bottom seal temperature (bottom part) of 145°C, a vertical seal temperature of 135°C, and a top seal temperature (sealed part after filling with contents) of 135°C.
[0097] The properties of the obtained biaxially oriented polypropylene film, the properties of the unoriented polypropylene film, the bag-making properties, and the properties of the packaging bags are shown in Table 1.
[0098] The biaxially oriented polypropylene film has a modulus of elasticity of 500 MPa or more in the longitudinal and transverse directions at 100°C, and a 719 cm -1 Peak of 973cm -1 The value obtained by dividing the peak value by the heat seal strength was 0.25, and when the heat seal layers were overlapped and heat sealed at 135°C, the heat seal strength was 25 N / 15 mm, the heat shrinkage rate at 130°C was 5% or less, a bag making speed of 45 spm was obtained, and the bag breakage rate of the bag filled with 1 kg of salt as the content was 0%, thereby satisfying all of the required properties of the present invention.
[0099] [Example 2] A 60 μm-thick unstretched polypropylene film was obtained in the same manner as in Example 1, except that 89.5 mass% of polypropylene-ethylene random copolymer (a5), 10 mass% of ethylene-propylene copolymer elastomer (c1), and 0.5 mass% of lubricant master batch (d1) were mixed as the heat seal layer.
[0100] Using the unstretched polypropylene film, a two-layer laminate was obtained in the same manner as in Example 1. The laminate and packaging bag obtained were evaluated in the same manner as in Example 1, and the results are shown in Table 1. -1 Peak of 973cm -1 The value obtained by dividing the peak value by the heat seal strength was 0.3, and when the heat seal layers were overlapped and heat sealed at 135°C, the heat seal strength was 23 N / 15 mm, the heat shrinkage rate at 130°C was 5% or less, a bag making speed of 45 spm was obtained, and the bag breakage rate of the bag filled with 1 kg of salt as the content was 0%, satisfying all of the required properties of the present invention.
[0101] [Examples 3 and 4] In Example 3, polypropylene (a1) was used as the heat seal layer, and a 50 μm thick unstretched polypropylene film was prepared in the same manner as in Example 1. In Example 4, polypropylene (a1) was used as the heat seal layer, and a 70 μm thick unstretched polypropylene film was prepared in the same manner as in Example 1, except that the heat seal layer was laminated with a base layer to obtain a two-layer laminate.
[0102] The obtained laminate and packaging bag were evaluated in the same manner as in Example 1, and the results are shown in Table 1. When the heat seal layers were overlapped and heat sealed at 135°C, the heat seal strength was 15 N / 15 mm or more, the heat shrinkage rate at 130°C was 5% or less, a bag making speed of 45 spm was obtained, and the bag breakage rate of the bag filled with 1 kg of salt as the content was 5% or less, satisfying all the required properties of the present invention.
[0103] [Example 5] A two-layer laminate was obtained in the same manner as in Example 1, except that a commercially available biaxially oriented polypropylene film (Pylen Film-OT (registered trademark)) P2171 manufactured by Toyobo Co., Ltd., having a thickness of 20 μm, was used as the biaxially oriented polypropylene film for the base layer.
[0104] The laminate and the packaging bag obtained were evaluated in the same manner as in Example 1, and the results are shown in Table 1. The biaxially oriented polypropylene film had a modulus of elasticity in the longitudinal and transverse directions of 500 MPa or more at 100° C., and the non-oriented polypropylene film in the heat seal layer had an elastic modulus of 719 cm by infrared absorptiometry. -1 Peak of 973cm -1 The value obtained by dividing the peak value by the heat seal strength was 0.25, and when the heat seal layers were overlapped and heat sealed at 135°C, the heat seal strength was 15 N / 15 mm or more, the heat shrinkage rate at 130°C was 5% or less, a bag making speed of 45 spm was obtained, and the bag breakage rate of the bag filled with 1 kg of salt as the content was 5% or less, thereby satisfying all of the required properties of the present invention.
[0105] [Comparative Example 1] Except for using polypropylene (a2) as the base layer, a biaxially oriented polypropylene film having a thickness of 20 μm was obtained in the same manner as in Example 1. The biaxially oriented polypropylene film was laminated in the same manner as in Example 1 with the non-oriented polypropylene film of the heat seal layer of Example 1 to obtain a two-layer laminate.
[0106] The obtained laminate and packaging bag were evaluated in the same manner as in Example 1, and the results are shown in Table 1. Since the elastic modulus in the longitudinal direction (MD) of the biaxially oriented polypropylene film of the base layer at 100°C was less than 500 MPa, and the heat shrinkage rate in the width direction of the laminate at 130°C was 5% or more, the dimensional change and deformation during bag making were large, and as a result, the heat seal strength was less than 15 N / 15 mm, the bag making speed was less than 40 spm, and the productivity was poor.
[0107] [Comparative Example 2] A 60 μm thick unstretched polypropylene film was obtained in the same manner as in Example 1, except that 85% by mass of a propylene-ethylene block copolymer (a3), 5% by mass of a high-density polyethylene (b2), and 10% by mass of an ethylene-propylene copolymer elastomer (c1) were mixed as the heat seal layer. Using the unstretched polypropylene film, a two-layer laminate was obtained in the same manner as in Example 1.
[0108] The laminate and the packaging bag obtained were evaluated in the same manner as in Example 1, and the results are shown in Table 1. The melting point of the unstretched polypropylene film of the heat seal layer was 162° C., and the infrared absorption spectrum was 719 cm -1 Peak of 973cm -1 The value obtained by dividing the peak value by the heat seal strength was 0.5, and when the heat seal layers were overlapped and heat sealed at 135°C, the heat seal strength was low at 10 N / 15 mm, and the bag breakage rate of the bags filled with 1 kg of salt was 10%, which is outside the object of the present invention.
[0109] [Comparative Example 3] A two-layer laminate was obtained in the same manner as in Example 1, except that the thickness of the unstretched polypropylene film in the heat seal layer in Example 1 was 40 μm. The laminate and packaging bag obtained were evaluated in the same manner as in Example 1, and the results are shown in Table 1. Because the heat seal layer was thin, the heat seal strength was low at 12 N / 15 mm when the heat seal layers were overlapped and heat sealed at 135° C., and the bag breakage rate of the bag filled with 1 kg of salt as the content was 8%, which was outside the object of the present invention.
[0110] [Comparative Example 4] A 60 μm thick non-oriented polypropylene film was obtained in the same manner as in Example 1, except that 40% by mass of ethylene-propylene random copolymer (a4) and 60% by mass of low-density polyethylene (b1) were mixed as the heat seal layer. Using the non-oriented polypropylene film, a two-layer laminate was obtained in the same manner as in Example 1.
[0111] The laminate and the packaging bag obtained were evaluated in the same manner as in Example 1, and the results are shown in Table 1. The melting point of the heat seal layer was 123° C., and the non-oriented polypropylene film of the heat seal layer had an infrared absorption spectrophotometric value of 719 cm -1 Peak of 973cm -1 The value obtained by dividing the value by the peak value was 0.6, which indicated high blocking between the heat-sealed layers and poor bag formability. In addition, the bag breakage rate of the bags filled with 1 kg of salt was 6%, which was outside the scope of the invention.
[0112] [Table 1] [Industrial Applicability]
[0113] The present invention can provide a laminate for packaging dry foods that has excellent heat resistance, impact resistance, and low-temperature heat sealability and has excellent bag formability similar to conventional packaging bags, using the same base material as a packaging bag for packaging food using the same environmentally friendly material, and a packaging bag for dry foods using the same.
Claims
1. The laminate is a laminate of a base layer and a heat seal layer, the base layer being a biaxially stretched film mainly composed of polypropylene having a modulus of elasticity in the longitudinal direction and the transverse direction of 500 MPa or more at 100° C., the heat seal layer being mainly composed of polypropylene, containing an ethylene-α-olefin copolymer, having a melting point of 125° C. or more and 145° C. or less, and having a wavelength of 719 cm by infrared absorptiometry. -1 The peak is 973 cm -1 The laminate for packaging dry foods has a seal strength of 15 N / 15 mm or more when the heat seal layers are overlapped and heat sealed at 135° C., and the value of the peak strength of the unstretched film is in the range of 0.1 to 0.
3.
2. 2. The dry food packaging laminate according to claim 1, wherein the thickness of the base layer is from 20 μm to 30 μm, and the thickness of the heat seal layer is from 50 μm to 70 μm.
3. 2. The dry food packaging laminate according to claim 1, which has a heat shrinkage rate of 5% or less at 130°C in the longitudinal and transverse directions.
4. A three-side sealed packaging bag using the laminate according to any one of claims 1 to 3, the packaging bag for dry goods having a bag-making speed of 40 spm or more when packaging 1 kg of contents within a temperature range of a bottom seal temperature of 140 to 150°C, a vertical seal temperature of 130 to 140°C, and a top seal temperature of 130 to 140°C.
5. 5. The packaging bag for dry foods according to claim 4, wherein the rate of breakage of said three-side sealed packaging bag when 1 kg of contents is placed in said three-side sealed packaging bag and dropped from a height of 1 m is 5% or less.
Citation Information
Patent Citations
Packaging film for food product, and package for food product
JP2020007441A
Biaxially oriented laminated polypropylene film
JP2023013959A