Oxynitriding steel and oxynitrided component

By forming an iron oxide layer on the nitrogen compound layer with alloying elements, the oxynitriding process addresses the shallow diffusion and softening issues of nitriding, achieving enhanced seizure resistance and internal strength in sliding parts.

JP2024152306APending Publication Date: 2024-10-25DAIDO STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023066421
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing nitriding treatments for sliding parts like gears result in shallow nitrogen diffusion depth and softening of the base material, leading to issues such as case crush and internal plastic deformation due to low internal strength.

Method used

The formation of an iron oxide layer on the surface of a nitrogen compound layer, combined with appropriate alloying elements like Mo and V, ensures a hardened layer depth of 0.15 mm or more with a Vickers hardness of 500 HV, enhancing seizure resistance and internal strength.

Benefits of technology

The oxynitriding process results in oxynitrided parts with improved seizure resistance and internal strength, effectively preventing damage like case crush and maintaining hardness, suitable for sliding parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152306000004
    Figure 2024152306000004
  • Figure 2024152306000005
    Figure 2024152306000005
  • Figure 2024152306000006
    Figure 2024152306000006
Patent Text Reader

Abstract

To provide an oxynitriding steel that enables production of an oxynitrided component with superior seizure resistance and internal strength.SOLUTION: An oxynitriding steel comprises, in mass%, C: 0.15%-0.50%, Si: 0.01%-2.00%, Mn: 0.10%-2.00%, P: 0.030% or less, S: 0.030% or less, Cu: 2.00% or less, Ni: 3.00% or less, Cr: 0.40%-3.00%, Mo: 0.01%-2.00%, and V: 0.01%-2.00%, fulfilling a formula (1), with the balance being Fe and inevitable impurities. 1.00×[C]-0.20×[Cr]+0.40×[Mo]+0.60×[V]>0.05...the formula (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel for oxynitriding and an oxynitrided part, and more particularly to a steel for oxynitriding and an oxynitrided part suitable for use in sliding parts such as gears. [Background technology]

[0002] In the case of sliding parts such as gears used in the power transmission mechanisms of automobiles, steel is processed into a predetermined shape by forging, cutting, etc., and then subjected to a surface hardening treatment such as carburizing and quenching, carbonitriding and quenching, or nitriding to improve mechanical properties such as wear resistance. In recent years, there have been many cases of use in environments where seizure is more likely to occur than before, such as with higher rotation speeds and the associated increased slip speeds, and so there is a particular demand for high seizure resistance. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-227675 A [Patent Document 2] JP 2016-125132 A Summary of the Invention [Problem to be solved by the invention]

[0004] In order to improve seizure resistance, it is considered effective to form a nitrogen compound layer by nitriding on the sliding surfaces of parts to prevent direct contact between metals (for example, see Patent Documents 1 and 2 mentioned above). However, the nitriding process has a lower processing temperature (about 500 to 650°C) compared to carburizing and carbonitriding processes, and the nitrogen diffusion depth is shallow. In addition, the base material inside the diffusion layer softens at the nitriding process temperature. For this reason, for example, in the case of sliding parts that have been subjected to nitriding, there has been a problem in that case crashes (damage in which the surface hardened layer peels off over a wide area) and internal plastic deformation are likely to occur due to low internal strength.

[0005] In light of the above circumstances, an object of the present invention is to provide a steel for oxynitriding capable of producing oxynitrided parts having excellent seizure resistance and internal strength, and an oxynitrided part using the same. [Means for solving the problem]

[0006] As a result of extensive investigations aimed at solving the above problems, the present inventors have obtained the following findings. (a) By forming an iron oxide layer on the surface side of the nitrogen compound layer formed by nitriding, the seizure resistance of the nitrided parts can be further improved. (b) The secondary hardening with Mo and V is effective in suppressing the softening of the base material during the nitriding process. By properly balancing the amounts of each alloying element added to the steel, the desired effective hardened layer depth can be secured, thereby increasing the internal strength of the nitrided parts. The present invention was made based on these findings.

[0007] The gist of the present invention is as follows.

[0008] [1] A steel for oxynitriding containing, by mass%, C: 0.15% to 0.50%, Si: 0.01% to 2.00%, Mn: 0.10% to 2.00%, P: 0.030% or less, S: 0.030% or less, Cu: 2.00% or less, Ni: 3.00% or less, Cr: 0.40% to 3.00%, Mo: 0.01% to 2.00%, and V: 0.01% to 2.00%, and satisfying the following formula (1), with the remainder being Fe and unavoidable impurities. 1.00×[C]-0.20×[Cr]+0.40×[Mo]+0.60×[V]>0.05 …Formula (1) (In formula (1), [ ] indicates the mass% content of each element.)

[0009] [2] In [1], the steel for oxynitriding further contains, by mass%, one or more of the following: N: 0.05% or less, s-Al: 0.10% or less, Nb: 0.20% or less, Ti: 2.00% or less, and B: 0.01% or less.

[0010] [3] An oxynitrided part made of the steel according to any one of [1] and [2], having a surface layer including a nitrogen compound layer and an iron oxide layer having a thickness of 3 μm or more formed on the surface side of the nitrogen compound layer, and having an effective hardened layer depth of 0.15 mm or more with a Vickers hardness of 500 HV. [Brief description of the drawings]

[0011] [Figure 1] 1 is a diagram showing a schematic structure of a surface layer of an oxynitrided part according to an embodiment of the present invention; [Diagram 2] FIG. 1 shows the shape of the rollers used in the roller pitting test. (A) shows the test roller, and (B) shows the loaded roller. [Diagram 3] FIG. 2A is an explanatory diagram showing the quenching and tempering treatment in the embodiment, and FIG. 2B is an explanatory diagram showing the gas oxynitriding treatment in the embodiment. [Figure 4] FIG. 2 is a schematic explanatory view of a roller pitching test. [Diagram 5] FIG. 11 is an explanatory diagram of the vacuum carburizing, quenching and tempering treatment applied to Comparative Example 2. [Figure 6] FIG. 11 is an explanatory diagram of a gas soft nitriding treatment applied to Comparative Example 4. [Figure 7] FIG. 2 is a graph showing the relationship between the index for the effective case depth on the left side of formula (1) and the measured effective case depth. [Figure 8] FIG. 13 is a graph showing the relationship between the measured effective case depth and the depression depth. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Next, the steel for oxynitriding and the oxynitrided part according to the embodiment of the present invention will be specifically described.

[0013] 1. Oxynitriding steel The steel for oxynitriding according to the present embodiment contains C, Si, Mn, P, S, Cu, Ni, Cr, Mo, and V in predetermined ranges, with the balance being Fe and unavoidable impurities, and may further contain one or more of N, s-Al, Nb, Ti, and B in predetermined ranges.

[0014] The reasons for limiting the chemical components of the present steel for oxynitriding are described in detail below. In the following description, "%" means "mass %" unless otherwise specified.

[0015] C: 0.15% to 0.50% C is an element necessary for ensuring the internal strength of parts when they are manufactured using the present steel for oxynitriding. The present steel for oxynitriding contains 0.15% or more of C. However, if the C content exceeds 0.50%, the workability such as machinability deteriorates. The preferred range of C is 0.15% to 0.40%, and more preferably 0.15% to 0.35%.

[0016] Silicon: 0.01% to 2.00% Silicon is an element that has the effect of increasing softening resistance. It is also added as a deoxidizer during melting. For this reason, the present steel for oxynitriding contains 0.01% or more of silicon. However, since silicon reduces the hot workability and machinability of steel, the upper limit is set to 2.00%. The preferred range of silicon is 0.10% to 1.00%, more preferably 0.10% to 0.70%, and even more preferably 0.10% to 0.50%.

[0017] Mn: 0.10% to 2.00% Mn is an element effective in improving the hardenability of steel. It also has the effect of forming Mn-based sulfides and improving machinability. In order to obtain these effects, in this embodiment, Mn is contained in an amount of 0.10% or more. However, excessive addition increases the hardness of the steel and reduces the hot workability, so the upper limit is set to 2.00%. The preferred range of Mn is 0.20% to 1.30%, more preferably 0.20% to 0.80%, and even more preferably 0.20% to 0.60%.

[0018] P:0.030% or less P is an impurity, so the lower the content, the better. P segregates at grain boundaries and reduces the hot workability of steel, so the P content should be 0.030% or less. It is difficult to reduce the P content to zero, so the practical lower limit is 0.004%.

[0019] S: 0.030% or less S is an impurity, so the lower the content, the better. S is likely to combine with Mn to form coarse MnS, which reduces the bending fatigue strength and hot workability of steel, so the content should be 0.030% or less. It is difficult to reduce the S content to zero, so the practical lower limit is 0.001%.

[0020] Cu:2.00% or less Cu is an element effective in improving the hardenability of steel. However, excessive addition of Cu leads to a decrease in hot forgeability and an increase in material costs, so the Cu content is set to 2.00% or less. The preferred range of Cu is 0.01% to 2.00%.

[0021] Ni: 3.00% or less Ni is an element effective in improving the hardenability of steel. However, excessive addition of Ni leads to a decrease in machinability and an increase in material costs, so the Ni content is set to 3.00% or less. The preferred range of Ni is 0.01% to 3.00%.

[0022] Cr: 0.40%~3.00% Cr forms fine nitrides (CrN) in the hardened layer during nitriding, improving the hardness of the surface layer of the part. To obtain this effect, Cr is contained in an amount of 0.40% or more. However, since excessive addition increases material costs, the upper limit is set to 3.00%. The preferred range of Cr is 0.60% to 2.00%, and more preferably 0.80% to 1.40%.

[0023] Mo: 0.01% to 2.00% Mo has the effect of suppressing the decrease in base material hardness (internal hardness) during nitriding by precipitating carbides through secondary hardening, and is an effective element for ensuring the effective hardened layer depth of nitrided parts. To obtain this effect, Mo is contained in an amount of 0.01% or more. However, since excessive addition increases material costs, the upper limit is set to 2.00%. The preferred range of Mo is 0.10% to 1.00%, and more preferably 0.10% to 0.60%.

[0024] V: 0.01% to 2.00% V, like Mo, is an element that has the effect of suppressing the decrease in base material hardness during nitriding by precipitating carbides through secondary hardening. To obtain this effect, V is contained in an amount of 0.01% or more. However, since excessive addition increases material costs, the upper limit is set to 2.00%. The preferred range of V is 0.10% to 0.60%, and more preferably 0.10% to 0.30%.

[0025] 1.00×[C]-0.20×[Cr]+0.40×[Mo]+0.60×[V]>0.05 …Formula (1) The left side of formula (1) is an index related to the effective hardened layer depth. C, Mo, and V contribute to secondary hardening by precipitating carbides at the nitriding temperature (500°C to 650°C), thereby increasing the effective hardened layer depth. On the other hand, Cr suppresses the diffusion of nitrogen during nitriding, thereby decreasing the effective hardened layer depth. By adjusting the components so that the value of the left side of formula (1) exceeds 0.05, it is possible to ensure that the effective hardened layer depth for a Vickers hardness of 500HV is 0.15mm or more in the nitrided parts.

[0026] N: 0.05% or less N forms nitrides with Al and contributes to suppressing the coarsening of crystal grains, so it can be added as necessary. However, excessive addition of N leads to coarsening of the nitrides, so the upper limit is set at 0.05%.

[0027] s-Al: 0.10% or less s-Al can be added as necessary because it combines with N to form nitrides and contributes to suppressing grain coarsening. However, excessive addition of s-Al leads to a decrease in strength due to the formation of Al2O3-based inclusions, so the upper limit is set at 0.10%.

[0028] Nb: 0.20% or less Nb precipitates carbides and contributes to suppressing grain coarsening, so it can be added as necessary. However, excessive addition leads to saturation of the effect and an increase in material costs, so the upper limit is set at 0.20%.

[0029] Ti:2.00% or less Like Cr, Ti forms fine nitrides in the hardened layer and has the effect of improving the hardness of the surface layer of the part, so it can be added as necessary. However, excessive addition can form large nitride-based inclusions in the steel that can become the starting point of fatigue fracture, so the upper limit is set at 2.00%.

[0030] B: 0.01% or less B has the effect of increasing the hardenability of steel and can be added as necessary. However, excessive addition of B leads to a decrease in the effect of increasing hardenability due to the formation of BN, so the upper limit is set at 0.01%.

[0031] 2. Oxynitriding parts Next, the oxynitrided part of this embodiment will be described. Fig. 1 is a diagram showing a schematic structure of a surface layer 2 of an oxynitrided part 1 of this embodiment. The oxynitrided part 1 is made of steel for oxynitriding having the above-mentioned component composition, and a hardened layer is formed in the surface layer 2 by oxynitriding treatment. More specifically, as shown in Fig. 1, an iron oxide layer 4 is formed in the outermost layer of the surface layer 2, a nitrogen compound layer 6 is formed below that, and a nitrogen diffusion layer 8 is formed further below that.

[0032] The nitrogen compound layer 6 is made of a γ' (FeN) compound and an ε (Fe 2-3The nitrogen compound layer 6 contains N compounds, and has an extremely high hardness compared to the base material, and has the effect of suppressing seizure on the sliding surface. The thickness of the nitrogen compound layer 6 is preferably 5 μm to 25 μm.

[0033] Here, the nitrogen compound layer 6 contains a porous layer that is brittle and prone to peeling and cracking. In order to prevent a decrease in seizure resistance due to peeling and wear of the porous layer, in this embodiment, an iron oxide layer 4 containing Fe3O4 and Fe2O3 as main components is provided on the surface side of the nitrogen compound layer 6. According to evaluations by the present inventors, it has been confirmed that by providing the iron oxide layer 4 with a thickness of 3 μm or more, seizure resistance is improved compared to nitrided parts that do not have an iron oxide layer. The thickness of the iron oxide layer is more preferably 3 μm to 10 μm.

[0034] The nitrogen diffusion layer 8 is a layer strengthened by the intrusion of nitrogen elements into the base material directly below the nitrogen compound layer 6. It is hardened by the solid solution strengthening of the intruded nitrogen and the dispersion of nitride particles.

[0035] Effective hardened layer depth for Vickers hardness 500HV: 0.15mm or more When measuring the hardness distribution from the surface of a part toward the inside, the depth from the surface of the part where the Vickers hardness is 500 HV is called the effective hardened layer depth. The shallower the effective hardened layer depth, the higher the possibility of damage occurring from the inside. According to the inventors' research, by ensuring an effective hardened layer depth of 0.15 mm or more, damage originating from the inside (e.g., case crush) can be suppressed more effectively than in the nitriding treatment layer including the nitrogen compound layer and the nitrogen diffusion layer.

[0036] Next, a method for manufacturing the present oxynitrided part will be described. The present oxynitrided part can be manufactured by processing (rough processing) steel having the above-mentioned composition (oxynitriding steel) into a predetermined shape, followed by quenching and tempering, finishing (precise processing) of the sliding surface, etc., and further oxynitriding.

[0037] In the quenching process, the intermediate member processed into a predetermined shape is held at a quenching temperature of 850 to 950°C. The holding time at the quenching temperature is not particularly limited, but is, for example, 30 to 60 minutes. After holding at heat for a predetermined time, it is rapidly cooled to a martensitic transformation start temperature Ms or lower. The quenching medium is, for example, water or oil. The intermediate member after quenching is subjected to a well-known tempering process. The tempering temperature is, for example, 550 to 650°C. The holding time at the tempering temperature is, for example, 60 to 120 minutes.

[0038] In the oxynitriding step, a nitriding step is followed by an oxidation step. In the nitriding process, nitrogen is penetrated into the surface layer 2 of the precisely machined intermediate part by heating it to a temperature below the A1 transformation point in an atmosphere containing NH3, and as a result, a nitrogen compound layer 6 containing mainly iron nitrides and a nitrogen diffusion layer 8 directly below it are formed in the surface layer 2 of the intermediate part.

[0039] In the nitriding step, a mixed gas of (NH3+CO2+N2) can be used as the nitriding gas. The treatment temperature and treatment time can be adjusted as appropriate. If the treatment temperature is too low, the diffusion rate of nitrogen decreases, resulting in a long treatment time. On the other hand, if the treatment temperature is too high, softening of the base material progresses, resulting in a decrease in internal hardness. An example of the treatment temperature is 500 to 650°C. The treatment time can be determined in conjunction with the treatment temperature so that a desired nitrogen compound layer thickness can be obtained. An example of the treatment time is 2 to 5 hours.

[0040] In the subsequent oxidation step, the intermediate member having the nitrogen compound layer 6 formed on its surface is heat-treated in an atmosphere containing an oxidizing gas such as water vapor, whereby a portion of the nitrogen compound layer 6 is converted to form an iron oxide layer 4 mainly composed of Fe3O4 and Fe2O3. The treatment temperature in the oxidation step can be, for example, 500 to 600° C. The treatment time can be determined in conjunction with the treatment temperature so as to obtain a desired iron oxide layer thickness. The treatment temperature can be, for example, 1 to 3 hours.

[0041] The oxynitrided parts manufactured in this manner have excellent seizure resistance and internal strength, and are suitable for use in sliding parts having sliding surfaces, such as gears and bearings.

[0042] <Example> The present invention will be described in more detail below with reference to examples. Here, for 27 examples and 4 comparative examples shown in Table 1 below, the iron oxide layer thickness, effective hardened layer depth, seizure resistance, and internal strength were evaluated using test pieces (test rollers and loaded rollers) manufactured through the steps of melting / casting → rolling → rough machining → quenching and tempering → precision machining → gas oxynitriding.

[0043] (Production of test specimens) In a vacuum induction melting furnace, 150 kg of steel ingots having the specified chemical composition shown in Table 1 below were melted and cast into ingots. Next, the ingots were rolled into bars, which were then cut to produce test rollers 10 shown in Fig. 2(A) and load rollers 20 shown in Fig. 2(B) by rough machining. Note that the dimension B of test roller 10 shown in Fig. 2(A) is 18 mm, and 12 in the figure is a through hole that engages with a separate shaft body. The dimension G of load roller 20 shown in Fig. 2(B) is 18 mm, the dimension R is 700 mm, and 22 in the figure is a through hole that engages with a separate shaft body.

[0044] [Table 1]

[0045] Next, the test roller 10 and the load roller 20 were subjected to quenching and tempering treatment using the heat pattern shown in Fig. 3(A). After that, a lapping process was performed so that the surface roughness Ra of the rolling surface 10a of the roller 10 was 0.1 ± 0.05 µm, and the surface roughness Rz of the rolling surface 20a of the roller 20 was 1.6 ± 0.5 µm.

[0046] (Gas oxynitriding treatment) The test roller 10 and the load roller 20 produced as described above were subjected to a gas oxynitriding treatment. In the gas oxynitriding treatment, as shown by the heat pattern in Fig. 3(B), first, nitriding was performed in a mixed gas atmosphere of (NH3+CO2+N2) to form a nitrogen compound layer on the surface layer (see Table 2 below for specific treatment temperatures and treatment times), and then oxidation treatment was performed in a water vapor atmosphere at 520°C for 2 hours to form an iron oxide layer on the nitrogen compound layer.

[0047] However, for Comparative Example 2, vacuum carburization was performed instead of gas oxynitriding. At that time, acetylene gas was used as the carburizing gas, and the treatment was performed according to the heat pattern shown in Figure 5. Also, for Comparative Example 4 (see Table 3 below), gas soft nitriding was performed instead of gas oxynitriding. At that time, a mixed gas of (NH3+CO2+N2) was used as the nitriding gas, and the treatment was performed according to the heat pattern shown in Figure 6.

[0048] (Measurement of iron oxide layer thickness) The portion of the test roller 10 including the rolling surface 10a was cut, and the cross section perpendicular to the rolling surface 10a was polished and etched, and observed under an optical microscope to measure the thickness of the iron oxide layer. For five fields of view of structure photographs taken under an optical microscope at 1000x, three iron oxide layers were extracted at 20 μm intervals and their thicknesses were measured, and the average of the measurements for a total of 15 locations was taken as the iron oxide layer thickness. The iron oxide layer thicknesses thus obtained are shown in Table 2 below.

[0049] (Measurement of effective hardened layer depth) The Vickers hardness (HV) was measured according to the Vickers hardness test method specified in "JIS Z2244," and a micro Vickers hardness tester was used. The indenter used was a diamond pyramid indenter with a facing angle of 136° specified in "JIS B7725," and an indentation was made on the mirror-polished designated surface of each test piece with a test load that was not destructive. The Vickers hardness was calculated from the diagonal length d [mm] of the indentation and the test load F [N] using the following formula. HV=0.189×(F / d^2)

[0050] The effective case depth was measured by measuring the hardness at 100 μm intervals in the depth direction from a position 100 μm deep from the surface (rolling surface surface) on a cut surface perpendicular to the rolling surface 10a of the test roller 10 under a load of 300 g. From the approximation curve showing the relationship between the depth from the surface and Vickers hardness, the depth from the surface corresponding to 500 HV was determined as the effective case depth (ECD), and the results are shown in Table 2.

[0051] (Seizure resistance evaluation) The test roller 10 and the loaded roller 20 prepared above were attached to a roller pitting tester, and a roller pitting test was carried out to evaluate the seizure resistance. Fig. 4 is a schematic diagram of the roller pitting test. As shown in the figure, the outer periphery 20a of the loaded roller 20 was pressed against the outer periphery 10a of the test roller 10 with a predetermined surface pressure P, and the two were rotated while supplying lubricant to the contact area to check for the occurrence of seizure. In the figure, 16 is a torque measuring instrument, and 18 is a thermocouple for measuring the rolling surface temperature. The specific test conditions are as follows: Contact pressure P calculated from Hertz's law: 1.5 GPa Test roller speed: 4000 rpm Sliding speed V: 0 to 14.3 m / s (increasing step) Lubricant temperature: 90℃

[0052] While increasing the sliding velocity V, test roller 10 was rotated 5×10 4 The roller was rotated in a cycle and the presence or absence of seizure was examined. In detail, the friction coefficient was calculated from the measured torque of the test roller 10 according to the following formula, and a friction coefficient exceeding 0.08 was judged to be the occurrence of seizure. Friction coefficient = (measured torque) / ((test load) x (roller radius)) The results are shown in Table 2 below. In addition to the evaluation of ○ and ×, the table also shows the P×V value when seizure occurred (if seizure did not occur, it was set to >21.5).

[0053] (Internal strength evaluation) As in the evaluation of seizure resistance, the test roller 10 and the loaded roller 20 were attached to a roller pitting tester, and a roller pitting test was performed to evaluate the internal strength. The test conditions were as follows. Contact pressure P calculated from Hertz's law: 2.0 GPa Test roller speed: 1500 rpm Sliding velocity V: 0.1 m / s Lubricant temperature: 90℃

[0054] Under the above test conditions, test roller 10 is 1×10 5 After the cycle of rotation, the deformation amount (depression depth) in the depth direction of the rolling surface 10a was investigated. The shape profile of the rolling surface 10a (unpeeled portion) was measured before and after the test, and the depth from the initial surface was defined as the depression depth. The shape profile in the axial direction of the rolling surface 10a was measured using a surface roughness measuring device (Tokyo Seimitsu Co., Ltd., SURFACOM 1500SD-13). In this case, the measurement length was 14 mm, and the cutoff wavelength was 0.8 mm. The internal strength was judged as "good" if the depression depth was less than 10 μm, and "bad" if the depression depth was 10 μm or more, and the results are shown in Table 2. In the table, the depression depth value is also shown together with the grade of good or bad.

[0055] [Table 2]

[0056] The evaluation results in Table 2 reveal the following: Comparative Example 1 is a material equivalent to SCR420H, which is used as a general-purpose carburizing steel, which was subjected to oxynitriding treatment. The V content of the steel of Comparative Example 1 is below the lower limit of the range specified for the steel of this embodiment, and does not satisfy the requirement of formula (1). As a result, the effective case depth (ECD) is shallow at 0.10 mm, and the evaluation result for internal strength is "x".

[0057] Comparative Example 2 uses a material equivalent to SCR420H like Comparative Example 1, but is subjected to vacuum carburizing instead of oxynitriding. The effective case depth (ECD) is as deep as 0.7 mm, and the internal strength is evaluated as "○", but no nitrogen compound layer is formed on the surface, and the seizure resistance is evaluated as "×".

[0058] Comparative Example 3 is an example in which the composition of the steel does not satisfy the requirement of formula (1) of this embodiment, and therefore the effective case depth was shallow at 0.12 mm, and the evaluation result for internal strength was "x".

[0059] [Table 3]

[0060] Table 3 shows a comparison of evaluation results between an example in which oxynitriding was performed (Example 1) and an example in which soft nitriding was performed (Comparative Example 4). Comparative Example 4 is a steel having the same composition as Example 1, but in which soft nitriding was performed instead of oxynitriding. In Comparative Example 4, although a nitrogen compound layer was present on the surface layer portion, there was no iron oxide layer on the surface side of the nitrogen compound layer, and therefore the evaluation result for seizure resistance was "X".

[0061] Thus, in Comparative Examples 1 to 4, the evaluation results for seizure resistance or internal strength were "x".

[0062] In contrast, Examples 1 to 27, which were made of steel with the content of each element satisfying the range specified in this embodiment, had a nitrogen compound layer in the surface layer and an iron oxide layer with a thickness of 3 μm or more formed on the surface side of the nitrogen compound layer, and had an effective hardened layer depth of 0.15 mm or more with a Vickers hardness of 500 HV, were evaluated as "○" for both seizure resistance and internal strength. Therefore, it is presumed that sliding parts such as gears that meet the same requirements as those of these examples will have excellent seizure resistance and will be able to effectively suppress damage such as case crashes that result from low internal strength.

[0063] 7 is a diagram showing the relationship between the index for the effective case depth on the left side of formula (1) and the measured effective case depth. It can be seen that if the value on the left side of formula (1) exceeds 0.05, an effective case depth (500HV) of 0.15mm or more can be ensured. Next, Fig. 8 shows the relationship between the measured effective case depth and the depression depth. If the effective case depth is ensured to be 0.15 mm or more, the depression depth can be made less than 10 μm. In other words, it can be seen that even in the case of a nitrided test piece, if a steel whose composition is adjusted to satisfy formula (1) is used, the internal strength can be equivalent to that of Comparative Example 2, which was subjected to vacuum carburization.

Claims

1. By mass% C: 0.15% to 0.50%, Si: 0.01% to 2.00%, Mn: 0.10% to 2.00%, P: 0.030% or less, S: 0.030% or less, Cu: 2.00% or less, Ni: 3.00% or less, Cr: 0.40% to 3.00%, Mo: 0.01% to 2.00%, V: 0.01% to 2.00%, and a steel for oxynitriding that satisfies the following formula (1), with the balance being Fe and unavoidable impurities: 1.00×[C]−0.20×[Cr]+0.40×[Mo]+0.60×[V]>0.05…Formula (1) (In formula (1), [ ] indicates the mass % content of each element.)

2. In claim 1, in mass % N: 0.05% or less, s-Al: 0.10% or less, Nb: 0.20% or less, Ti: 2.00% or less, B: 0.01% or less, The steel for oxynitriding further contains one or more of the above.

3. 3. An oxynitrided part made of the steel according to claim 1 or 2, comprising a surface layer including a nitrogen compound layer and an iron oxide layer having a thickness of 3 μm or more formed on the surface side of the nitrogen compound layer, and having an effective hardened layer depth of 0.15 mm or more having a Vickers hardness of 500 HV.

Citation Information

Patent Citations

  • Gear excellent in seizure resistance

    JP2013227675A

  • Nitrided member and friction drive transmission using the same

    JP2016125132A