Toner for developing electrostatic charge image
The electrostatic image developing toner with a specific crystalline polyester resin and high BET carbon black surface area addresses adhesion and durability issues on plastic films, enhancing pencil hardness and resistance to peeling and curling.
Patent Information
- Application Number
- JP2024017487
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-02-07
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-02-07
AI Technical Summary
Existing electrostatic image developing toners struggle to form durable printed coatings on plastic films, particularly PET bottle labels and packaging films, due to issues with adhesion and heat sensitivity, leading to peeling and curling, and require improvements in pencil hardness tests.
The development of an electrostatic image developing toner containing a binder resin with a crystalline polyester resin having a specific ester group concentration and carbon black with a high BET specific surface area, which interacts through hydrogen bonding to enhance dispersion and recrystallization, resulting in a highly durable printed coating.
The toner achieves a printed coating film with improved pencil hardness and durability on plastic films, ensuring strong adhesion and resistance to peeling and curling.
Smart Images

Figure 2024152606000001 
Figure 2024152606000002 
Figure 2024152606000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing electrostatic images used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like. [Background technology]
[0002] With the diversification of print media, there is an increasing demand for electrophotographic printing on print media other than paper. Major media include plastic films such as polyethylene terephthalate film, polypropylene film, and polyethylene film, which are used for PET bottle labels and various packages. Since these plastic films have a smooth surface, the anchor effect between the surface and the coating film (printed coating film) formed by printing electrophotographic toner on the surface is difficult to work, and the printed coating film is easily peeled off from the plastic film. In addition, since plastic films are sensitive to heat, the print media curls and shrinks when electrophotographic toner is thermally fixed.
[0003] Patent Document 1 describes an electrostatic image developing toner that has excellent low-temperature fixing properties and heat-resistant storage stability of the toner and excellent storage stability of printed matter, and that contains an amorphous polyester resin and a crystalline polyester resin, in which the amorphous polyester resin is a polycondensate of an alcohol component (A-al) and a carboxylic acid component (A-ac) containing succinic acid or an anhydride thereof substituted with a linear aliphatic hydrocarbon group having 16 to 18 carbon atoms, and the crystalline polyester resin is a polycondensate of an alcohol component (C-al) and a carboxylic acid component (C-ac), in which the alcohol component (C-al) is a monoalcohol having 6 to 24 carbon atoms, and the carboxylic acid component (C-ac) is at least one selected from the group consisting of a monocarboxylic acid having 6 to 24 carbon atoms.
[0004] Patent Document 2 describes a method for forming an image on a polypropylene film or a polyethylene film with a toner containing crystalline polyester resin C in a binder resin, with the aim of providing an image forming method that provides an image with excellent image density and excellent abrasion resistance, in which the SP value of the crystalline polyester resin C is 9.0 or more and 10.1 or less, the content of the crystalline polyester resin C in the binder resin is 10% by mass or more and 60% by mass or less, the surface tension of the printed surface of the polypropylene film or polyethylene film is 35 mN / m or more and 49 mN / m or less, and the fixing temperature is not more than a temperature 5° C. higher than the melting point of the polypropylene film or polyethylene film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-60687 A [Patent Document 2] Patent Publication No. 2022-54448 Summary of the Invention [Problem to be solved by the invention]
[0006] Printed packaging materials such as PET bottle labels and packaging films are required to have high robustness in terms of protecting the quality of the contents and displaying information. In the case of printed coatings formed using printing inks for printed packaging materials, the coating hardness is evaluated by a pencil hardness test, and a pencil hardness of B or higher is required. As a result of the inventors' investigation, it was found that the above-mentioned printed packaging materials obtained by forming a printed coating on a printing medium such as a plastic film using the toner for developing electrostatic images described in Patent Document 1 and the image forming method described in Patent Document 2 have robustness to a tape peel test and a fingernail scratch test, but there is room for improvement in robustness to a pencil hardness test. The present invention relates to a toner for developing electrostatic images, which is capable of forming a highly durable printed coating film on a printing medium (substrate) such as a plastic film. [Means for solving the problem]
[0007] The present inventors have found that a printed coating film having high robustness can be formed by using a toner for developing electrostatic images, which comprises in combination a binder resin containing a crystalline polyester resin having an ester group concentration in a specific range and a colorant containing carbon black having a BET specific surface area in a specific range. The present invention relates to the following [1]. [1] A toner for developing electrostatic images, comprising a binder resin and a colorant, The binder resin contains a crystalline polyester resin C having an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less, The colorant has a BET specific surface area of 200m 2 / g or more of carbon black, Toner for developing electrostatic images. Effect of the Invention
[0008] According to the present invention, there is provided a toner for developing electrostatic images, which is capable of forming a highly fast printing coating film on a printing medium (substrate) such as a plastic film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Toner for developing electrostatic images] The toner for developing electrostatic images of the present invention (hereinafter, also simply referred to as "toner") contains a binder resin and a colorant. The binder resin contains a crystalline polyester resin C (hereinafter, simply referred to as "resin C") having an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less. The colorant contains a crystalline polyester resin C having a BET specific surface area of 200 m 2 / g or more of carbon black. Due to the above-mentioned characteristics, the toner of the present invention can provide a printed coating film having high fastness.
[0010] The reason why the toner of the present invention can provide a printed coating film with high fastness is not clear, but is thought to be as follows. As a result of the study by the present inventors, carbon black with a high BET specific surface area is useful in that it has a high coloring power because the primary particles are small, and therefore it is possible to obtain printed matter with a potentially high image density. However, carbon black with a high BET specific surface area also has an increased number of functional groups (e.g., carboxyl groups and hydroxyl groups) per mass unit present on the particle surface. Therefore, carbon black with a high BET specific surface area is difficult to disperse in a binder resin and is prone to agglomeration. When a toner is produced through kneading by a pulverization method or a fusing process by a chemical method, if a raw material mixture containing carbon black and a binder resin is heated and kept in a low viscosity state, carbon black with a high BET specific surface area will agglomerate due to the action of hydrogen bonds, etc. In the present invention, by using a binder resin containing a crystalline polyester resin in which the ester group concentration is controlled within a specific range, the functional groups on the carbon black surface and the ester moiety of the crystalline polyester resin interact with each other through hydrogen bonds or the like. Therefore, the carbon black with a high BET specific surface area (small primary particle size) is prevented from agglomerating in the raw material mixture containing the carbon black and the binder resin, and a toner in which the crystalline polyester resin and carbon black are uniformly dispersed in the toner particles can be obtained. It is believed that the dispersed carbon black induces cooling recrystallization of the crystalline polyester resin after fixing, and the crystalline polyester resin quickly recrystallizes, thereby improving the coating strength (pencil hardness) of the printed matter produced using the toner.
[0011] The definitions of various terms used in this specification are given below. In the specification, the carboxylic acid component of the polyester resin includes not only the compound itself, but also anhydrides that decompose during the reaction to produce a carboxylic acid, and alkyl esters of each carboxylic acid (alkyl groups having 1 to 3 carbon atoms). Whether a resin is crystalline or amorphous is determined by the crystallinity index. The crystallinity index is defined as the ratio of the softening point of the resin to the maximum endothermic peak temperature (softening point (°C) / maximum endothermic peak temperature (°C)) in the measurement method described in the examples below. A crystalline resin is one with a crystallinity index of 0.6 or more and 1.4 or less. An amorphous resin is one in which no endothermic peak is observed, or, if observed, has a crystallinity index of less than 0.6 or more than 1.4. The crystallinity index can be appropriately adjusted by the types and ratios of raw material monomers, as well as production conditions such as reaction temperature, reaction time, and cooling rate. With respect to hydrocarbon groups, the references "(iso or tertiary)" and "(iso)" in parentheses refer to both the cases with and without the prefixes present; the absence of the prefixes indicates normal. "(Meth)acrylic acid" means at least one selected from acrylic acid and methacrylic acid. By "styrenic compound" is meant unsubstituted or substituted styrene.
[0012] [Toner Particles] In the present invention, the toner particles contain a binder resin and a colorant.
[0013] <Binding resin> In the present invention, the binder resin contains a crystalline polyester resin C having an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less. Hereinafter, the crystalline polyester resin C having an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less may be simply referred to as "resin C".
[0014] (Crystalline polyester resin C) Resin C contains a polycondensate of an alcohol component and a carboxylic acid component, and has an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less. Crystalline polyester resin C is preferably a polycondensate of an alcohol component and a carboxylic acid component, and may be a composite resin containing a polyester resin segment and an addition polymerization resin segment.
[0015] From the viewpoint of fastness of the printed coating film, the resin C has an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less, preferably 6.7 mmol / g or more and preferably 8.8 mmol / g or less, more preferably 8.5 mmol / g or less, and further preferably 8.2 mmol / g or less. The ester group concentration of the resin C is calculated by the following formula.
[0016]
number
[0017] The alcohol component and the carboxylic acid component will be described below. The following alcohol components and carboxylic acid components can be used alone or in combination of two or more.
[0018] From the viewpoint of the robustness of the printed coating film and the adjustment of the ester group concentration, the alcohol component of the crystalline polyester-based resin C preferably contains a short-chain aliphatic diol and / or the carboxylic acid component preferably contains a short-chain aliphatic dicarboxylic acid, and it is more preferable that the alcohol component contains a short-chain aliphatic diol.
[0019] The aliphatic diol preferably has 2 or more carbon atoms, and preferably has 16 or less, more preferably 12 or less, even more preferably 8 or less, and even more preferably 6 or less. The aliphatic diol is preferably a straight-chain aliphatic diol, such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, and 1,16-hexadecanediol. Among these, a straight-chain short-chain aliphatic diol having 2 to 6 carbon atoms is preferred, and ethylene glycol, 1,4-butanediol, and 1,6-hexanediol are more preferred, with ethylene glycol being even more preferred.
[0020] The amount of the aliphatic diol in the alcohol component is preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, still more preferably 85 mol % or more, and 100 mol % or less.
[0021] The amount of ethylene glycol in the alcohol component is preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, still more preferably 85 mol % or more, and is 100 mol % or less.
[0022] From the viewpoint of fastness of the printed coating film, the alcohol component may contain a monofunctional (monohydric) alcohol. Examples of the monohydric alcohol include aliphatic monoalcohols such as capric alcohol, lauryl alcohol, myristyl alcohol, palmityl alcohol, stearyl alcohol, and behenyl alcohol. When the alcohol component contains a monohydric alcohol, the amount of the monohydric alcohol in the alcohol component is preferably 1 mol% or more, more preferably 3 mol% or more, even more preferably 5 mol% or more, and preferably 25 mol% or less, more preferably 20 mol% or less, even more preferably 15 mol% or less.
[0023] The alcohol component may contain an alcohol component other than the aliphatic diol and the monohydric alcohol. Examples of other alcohol components include alkylene oxide adducts of aromatic diols, such as alkylene oxide adducts of bisphenol A; and trihydric or higher alcohols, such as glycerin, pentaerythritol, and trimethylolpropane.
[0024] From the viewpoint of fastness of the printed coating film, the number of carbon atoms of the aliphatic dicarboxylic acid is preferably 4 or more, more preferably 10 or more, even more preferably 12 or more, and is preferably 16 or less, more preferably 14 or less. The aliphatic dicarboxylic acid is preferably an α,ω-straight-chain aliphatic dicarboxylic acid. Specific examples of the aliphatic dicarboxylic acid include succinic acid, fumaric acid, adipic acid, sebacic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, and 1,14-tetradecanedioic acid. Among them, from the viewpoint of fastness of the printed coating film, one or more selected from fumaric acid, sebacic acid, 1,12-dodecanedioic acid, and 1,14-tetradecanedioic acid are preferred, and one or more selected from sebacic acid, 1,12-dodecanedioic acid, and 1,14-tetradecanedioic acid are more preferred. The amount of the aliphatic dicarboxylic acid component in the carboxylic acid component is preferably 70 mol% or more, more preferably 75 mol% or more, even more preferably 80 mol% or more, even more preferably 85 mol% or more, and 100 mol% or less. When the carboxylic acid component contains the following monocarboxylic acids, it is preferably 99 mol% or less, more preferably 97 mol% or less, even more preferably 95 mol% or less.
[0025] From the viewpoint of fastness of the printed coating film, the carboxylic acid component preferably contains a monocarboxylic acid. From the same viewpoint, the number of carbon atoms of the monocarboxylic acid is preferably 6 or more, more preferably 8 or more, even more preferably 12 or more, even more preferably 16 or more, and is preferably 24 or less, more preferably 22 or less, even more preferably 20 or less. Examples of monocarboxylic acids include caprylic acid, pelargonic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, lignoceric acid, etc. Among these, preferred are caprylic acid, lauric acid, stearic acid, and behenic acid, and from the viewpoint of obtaining a printing coating film having high low-temperature fixability and fastness, more preferred are stearic acid and behenic acid, and even more preferred is stearic acid. When the carboxylic acid component contains a monocarboxylic acid, the amount of the monocarboxylic acid in the carboxylic acid component is preferably 1 mol% or more, more preferably 3 mol% or more, even more preferably 5 mol% or more, and preferably 25 mol% or less, more preferably 20 mol% or less, even more preferably 15 mol% or less. The carboxylic acid component may contain other carboxylic acid components different from the aliphatic dicarboxylic acid and monocarboxylic acid. Examples of the other carboxylic acid components include aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid, and polyvalent carboxylic acids having three or more valences such as trimellitic acid.
[0026] From the viewpoint of fastness of the printed coating film, it is preferable that the resin C contains a polycondensate of an alcohol component containing 80 mol % or more of ethylene glycol and a carboxylic acid component. From the same viewpoint, it is preferable that the resin C contains a monoalcohol-derived structural unit and / or a monocarboxylic acid-derived structural unit, and it is more preferable that the resin C contains a monocarboxylic acid-derived structural unit.
[0027] The equivalent ratio of the carboxyl groups of the carboxylic acid component to the hydroxyl groups of the alcohol component [COOH groups / OH groups] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.
[0028] (Production method of crystalline polyester resin C) Resin C can be produced, for example, by polycondensing raw material monomers containing an alcohol component and a carboxylic acid component.
[0029] The polycondensation of the alcohol component and the carboxylic acid component can be carried out, for example, in an inert gas atmosphere, in the presence of an esterification catalyst, an esterification promoter, a polymerization inhibitor, etc., as necessary, at a temperature of about 120°C or higher and 250°C or lower. Examples of the esterification catalyst include tin compounds such as dibutyltin oxide and tin(II) di(2-ethylhexanoate), and titanium compounds such as titanium diisopropoxybis(triethanolaminate). Examples of the esterification promoter that can be used together with the esterification catalyst include gallic acid (3,4,5-trihydroxybenzoic acid). The amount of the esterification catalyst used is preferably 0.01 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass in total of the alcohol component and the carboxylic acid component which are raw material monomers for the resin C. The amount of the esterification promoter used is preferably 0.001 part by mass or more and 1 part by mass or less based on 100 parts by mass in total of the alcohol component and the carboxylic acid component. Furthermore, examples of the polymerization inhibitor include radical polymerization inhibitors such as 4-tert-butylcatechol. When a polymerization inhibitor is used, the amount of the polymerization inhibitor used is preferably 0.001 part by mass or more and 1 part by mass or less based on 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.
[0030] (Physical properties of crystalline polyester resin C) The softening point of Resin C is preferably 60°C or higher, more preferably 65°C or higher, and even more preferably 70°C or higher, and from the viewpoint of further improving low-temperature fixability, it is preferably 150°C or lower, more preferably 120°C or lower, and even more preferably 100°C or lower. The melting point of resin C is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 65°C or higher, and from the viewpoint of further improving low-temperature fixability, it is preferably 100°C or lower, more preferably 95°C or lower, and even more preferably 90°C or lower.
[0031] The acid value of resin C is preferably 2 mgKOH / g or more, more preferably 4 mgKOH / g or more, and preferably 20 mgKOH / g or less, more preferably 15 mgKOH / g or less, and even more preferably 10 mgKOH / g or less.
[0032] The ester group concentration, softening point, melting point and acid value of the resin C can be appropriately adjusted by the type and amount of the raw material monomer, and production conditions such as reaction temperature, reaction time, cooling rate, etc., and the softening point, melting point and acid value are determined by the method described in the Examples below. When two or more types of resin C are used in combination, it is preferable that the ester group concentration, softening point, melting point and acid value obtained as a mixture thereof are each within the above-mentioned ranges.
[0033] (Amorphous polyester resin A) In the present invention, the binder resin preferably contains an amorphous polyester resin A. Hereinafter, the amorphous polyester resin A may be simply referred to as "resin A". Resin A is used as a binder resin for the toner, and is, for example, an amorphous polyester resin containing a polycondensation product of an alcohol component and a carboxylic acid component. Examples of the resin A include polyester resin and modified polyester resin. Examples of the modified polyester resin include urethane modified polyester resin, epoxy modified polyester resin, and composite resin containing polyester resin segment and addition polymerization resin segment. Among these, the resin A is preferably polyester resin and composite resin, and more preferably composite resin.
[0034] Examples of the alcohol component of the resin A include alkylene oxide adducts of aromatic diols, aliphatic diols, alicyclic diols, and trihydric or higher polyhydric alcohols. Among these, alkylene oxide adducts of aromatic diols are preferred from the viewpoint of obtaining a toner having excellent low-temperature fixing properties. The alkylene oxide adduct of an aromatic diol is preferably an alkylene oxide adduct of bisphenol A, more preferably an alkylene oxide adduct of formula (I):
[0035] [ka] (In the formula, OR 1 and R 2 O is an oxyalkylene group, and R 1 and R 2 each independently represents an ethylene group or a propylene group, x and y represent the average number of moles of alkylene oxide added and are each positive numbers, and the sum of x and y is 1 or more, preferably 1.5 or more, and 16 or less, preferably 8 or less, and more preferably 4 or less.
[0036] Examples of the alkylene oxide adduct of bisphenol A represented by formula (I) include a propylene oxide adduct of bisphenol A and an ethylene oxide adduct of bisphenol A. Among these, it is preferable to contain a propylene oxide adduct of bisphenol A. In the alcohol component, the content of the alkylene oxide adduct of bisphenol A is preferably 80 mol % or more, more preferably 90 mol % or more, and is 100 mol % or less, and further preferably 100 mol %.
[0037] Examples of aliphatic diols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2,2-dimethyl-1,3-propanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, and 3-methyl-1,5-pentanediol. Examples of the alicyclic diol include hydrogenated bisphenol A [2,2-bis(4-hydroxycyclohexyl)propane] and adducts of hydrogenated bisphenol A with alkylene oxides having 2 to 4 carbon atoms (average number of moles added: 2 to 12). Examples of trihydric or higher polyhydric alcohols include glycerin, pentaerythritol, trimethylolpropane, and sorbitol. These alcohol components may be used alone or in combination of two or more.
[0038] Examples of the carboxylic acid component of the resin A include dicarboxylic acids and trivalent or higher polyvalent carboxylic acids. Examples of dicarboxylic acids include aromatic dicarboxylic acids, aliphatic dicarboxylic acids, and alicyclic dicarboxylic acids. Among these, at least one selected from aromatic dicarboxylic acids and aliphatic dicarboxylic acids is preferred. Examples of aromatic dicarboxylic acids include phthalic acid, isophthalic acid, and terephthalic acid. Among these, isophthalic acid and terephthalic acid are preferred, and terephthalic acid is more preferred. The amount of aromatic dicarboxylic acid in the carboxylic acid component is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 40 mol% or more, and preferably 85 mol% or less, more preferably 80 mol% or less, even more preferably 75 mol% or less.
[0039] The aliphatic dicarboxylic acid preferably has 2 or more, more preferably 3 or more, and preferably has 30 or less, more preferably 20 or less. Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, adipic acid, sebacic acid, dodecanedioic acid, azelaic acid, and succinic acid substituted with an aliphatic hydrocarbon group having 1 to 20 carbon atoms. Examples of succinic acid substituted with an aliphatic hydrocarbon group having 1 to 20 carbon atoms include dodecylsuccinic acid, dodecenylsuccinic acid, and octenylsuccinic acid. Among these, fumaric acid, sebacic acid, adipic acid, and succinic acid substituted with an aliphatic hydrocarbon group having 1 to 20 carbon atoms are preferred. The amount of aliphatic dicarboxylic acid in the carboxylic acid component is preferably 5 mol% or more, more preferably 10 mol% or more, even more preferably 15 mol% or more, and preferably 50 mol% or less, more preferably 45 mol% or less, even more preferably 40 mol% or less. An example of the alicyclic dicarboxylic acid is cyclohexanedicarboxylic acid.
[0040] The trivalent or higher polyvalent carboxylic acid is preferably a trivalent carboxylic acid, and examples thereof include trimellitic acid and its anhydride. When a trivalent or higher polycarboxylic acid is contained, the amount of the trivalent or higher polycarboxylic acid in the carboxylic acid component is preferably 3 mol% or more, more preferably 6 mol% or more, even more preferably 9 mol% or more, and is preferably 25 mol% or less, more preferably 20 mol% or less, even more preferably 15 mol% or less. These carboxylic acid components may be used alone or in combination of two or more.
[0041] The equivalent ratio of the carboxyl groups of the carboxylic acid component to the hydroxyl groups of the alcohol component [COOH groups / OH groups] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.
[0042] When the resin A is a composite resin, an example of the addition polymerized resin segment is an addition polymer of raw material monomers containing a styrene-based compound. Examples of the styrene-based compound include unsubstituted or substituted styrene. Examples of the substituent substituted on styrene include an alkyl group having 1 to 5 carbon atoms, a halogen atom, an alkoxy group having 1 to 5 carbon atoms, a sulfonic acid group, or a salt thereof. Examples of styrene-based compounds include styrene, methylstyrene, α-methylstyrene, β-methylstyrene, tert-butylstyrene, chlorostyrene, chloromethylstyrene, methoxystyrene, styrenesulfonic acid, and salts thereof. Among these, styrene is preferred. The content of the styrene-based compound in the raw material monomers of the addition polymerization resin segment is preferably 50% by mass or more, more preferably 65% by mass or more, even more preferably 75% by mass or more, and is 100% by mass or less, preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less.
[0043] Examples of raw material monomers other than styrene-based compounds include (meth)acrylic acid esters such as alkyl (meth)acrylate, benzyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate; olefins such as ethylene, propylene, and butadiene; halovinyls such as vinyl chloride; vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether; vinylidene halides such as vinylidene chloride; and N-vinyl compounds such as N-vinylpyrrolidone. Among these, (meth)acrylic acid esters are preferred, and alkyl (meth)acrylates are more preferred. The number of carbon atoms in the alkyl group in the alkyl (meth)acrylate is preferably 1 or more, more preferably 4 or more, even more preferably 6 or more, and is preferably 24 or less, more preferably 22 or less, even more preferably 20 or less. Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, (iso)propyl (meth)acrylate, (iso- or tertiary)butyl (meth)acrylate, (iso)amyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, (iso)octyl (meth)acrylate, (iso)decyl (meth)acrylate, (iso)dodecyl (meth)acrylate, (iso)palmityl (meth)acrylate, (iso)stearyl (meth)acrylate, and (iso)behenyl (meth)acrylate. Of these, 2-ethylhexyl (meth)acrylate or stearyl (meth)acrylate is preferred, stearyl (meth)acrylate is more preferred, and stearyl methacrylate is even more preferred.
[0044] When the addition polymerization resin segment contains a structural unit derived from a (meth)acrylic acid ester, the content of the (meth)acrylic acid ester in the raw material monomers of the addition polymerization resin segment is preferably 5 mass% or more, more preferably 10 mass% or more, even more preferably 15 mass% or more, and preferably 50 mass% or less, more preferably 35 mass% or less, even more preferably 25 mass% or less.
[0045] The total amount of the styrene-based compound and the (meth)acrylic acid ester in the raw material monomers of the addition polymerization resin segment is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, and even more preferably 100 mass %.
[0046] The composite resin preferably has a constitutional unit derived from a bireactive monomer bonded via a covalent bond to a polyester resin segment and an addition polymerization resin segment. The term "structural unit derived from a bireactive monomer" refers to a unit formed by reaction of a functional group and an addition polymerizable group of a bireactive monomer. An example of the addition polymerizable group is a carbon-carbon unsaturated bond (ethylenically unsaturated bond). Examples of the bireactive monomer include addition polymerizable monomers having at least one functional group selected from a hydroxyl group, a carboxyl group, an epoxy group, a primary amino group, and a secondary amino group in the molecule. Among these, from the viewpoint of reactivity, addition polymerizable monomers having at least one functional group selected from a hydroxyl group and a carboxyl group are preferred, and addition polymerizable monomers having a carboxyl group are more preferred. Examples of the addition polymerizable monomer having a carboxy group include acrylic acid, methacrylic acid, fumaric acid, and maleic acid. Among these, from the viewpoint of reactivity in both the polycondensation reaction and the addition polymerization reaction, acrylic acid and methacrylic acid are preferred, and acrylic acid is more preferred. When the bireactive monomer is an addition polymerizable monomer having a carboxy group, the amount of the constitutional units derived from the bireactive monomer is preferably 1 mol part or more, more preferably 5 mol parts or more, even more preferably 8 mol parts or more, and preferably 30 mol parts or less, more preferably 25 mol parts or less, even more preferably 20 mol parts or less, relative to 100 mol parts of the alcohol component of the polyester resin segment of the composite resin.
[0047] The content of the polyester resin segment in the composite resin is preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 55% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, based on the total amount of the polyester resin segment and the addition polymerization resin segment. The constitutional unit derived from the bireactive monomer is defined as a polyester resin segment.
[0048] The content of the addition polymerization resin segment in the composite resin is preferably 5 mass% or more, more preferably 10 mass% or more, even more preferably 15 mass% or more, and preferably 60 mass% or less, more preferably 55 mass% or less, even more preferably 45 mass% or less, based on the total amount of the polyester resin segment and the addition polymerization resin segment.
[0049] The amount of the constitutional units derived from the bireactive monomer in the composite resin is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 0.8 mass% or more, and is preferably 10 mass% or less, more preferably 7 mass% or less, even more preferably 4 mass% or less, based on the total amount of the polyester resin segment and the addition polymerization resin segment.
[0050] The total amount of the polyester resin segment and the addition polymerization resin segment in the composite resin is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and is 100% by mass or less, even more preferably 100% by mass.
[0051] The above amount is calculated based on the ratio of the amounts of the polyester resin segment, the raw material monomer for the addition polymerization resin segment, the bireactive monomer, and the radical polymerization initiator, and the mass of the polyester resin segment, etc. is based on the mass excluding the mass of water generated by polycondensation. When a radical polymerization initiator is used, the mass of the radical polymerization initiator is calculated by including it in the addition polymerization resin segment.
[0052] (Production method of amorphous polyester resin A) <<Method of manufacturing amorphous polyester resin>> When the resin A is an amorphous polyester resin, the resin A can be produced, for example, in the same manner as the resin C described above, by polycondensing raw material monomers containing an alcohol component and a carboxylic acid component.
[0053] <<Composite resin manufacturing method>> When resin A is a composite resin containing a polyester resin segment and an addition polymerization resin segment, it may be produced, for example, by a method including a step A of polycondensing an alcohol component and a carboxylic acid component, and a step B of addition polymerizing raw material monomers of the addition polymerization resin segment and a bireactive monomer. Step B may be carried out after step A, step B may be carried out after step A, or step A and step B may be carried out simultaneously. In step A, a part of the carboxylic acid component is subjected to a polycondensation reaction, and then step B is carried out, and thereafter the remainder of the carboxylic acid component is added to the polymerization system to further proceed with the polycondensation reaction of step A and the polycondensation reaction with, for example, a carboxy group possessed by the bireactive monomer or the constituent unit derived from the bireactive monomer.
[0054] In the step A, if necessary, the esterification catalyst and the esterification promoter described in the above-mentioned method for producing the crystalline polyester resin C may be used in the same amounts to carry out polycondensation. When a monomer having an unsaturated bond such as fumaric acid is used in the polycondensation, the polymerization inhibitor described in the above-mentioned method for producing crystalline polyester resin C may be used in the same amount as above, if necessary. The temperature of the polycondensation reaction is preferably 120° C. or higher, more preferably 160° C. or higher, and even more preferably 180° C. or higher, and is preferably 250° C. or lower, more preferably 240° C. or lower. The polycondensation may be carried out in an inert gas atmosphere.
[0055] Examples of the radical polymerization initiator for the addition polymerization in step B include peroxides such as dibutyl peroxide, persulfates such as sodium persulfate, and azo compounds such as 2,2'-azobis(2,4-dimethylvaleronitrile). The amount of the radical polymerization initiator used is preferably 1 part by mass or more and 20 parts by mass or less based on 100 parts by mass of the raw material monomer of the addition polymerization resin segment. The temperature of the addition polymerization is preferably 110° C. or higher, more preferably 130° C. or higher, and preferably 230° C. or lower, more preferably 220° C. or lower, and further preferably 210° C. or lower.
[0056] (Physical properties of amorphous polyester resin A) The softening point of resin A is preferably 70° C. or higher, more preferably 90° C. or higher, and even more preferably 100° C. or higher, and is preferably 140° C. or lower, more preferably 130° C. or lower, and even more preferably 125° C. or lower. The glass transition temperature of resin A is preferably 30°C or higher, more preferably 35°C or higher, and even more preferably 40°C or higher, and is preferably 80°C or lower, more preferably 75°C or lower, and even more preferably 70°C or lower.
[0057] The acid value of Resin A is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, even more preferably 15 mgKOH / g or more, and preferably 40 mgKOH / g or less, more preferably 35 mgKOH / g or less, even more preferably 30 mgKOH / g or less.
[0058] The softening point, glass transition temperature and acid value of Resin A can be appropriately adjusted by the type and amount of raw material monomer used, as well as production conditions such as reaction temperature, reaction time and cooling rate, and these values can be determined by the methods described in the examples. When two or more resins A are used in combination, the softening point, glass transition temperature and acid value of the resulting mixture are preferably within the above-mentioned ranges.
[0059] From the viewpoint of image density of the printed matter, the content of the binder resin in the toner particles is preferably 60% by mass or more, more preferably 65% by mass or more, even more preferably 70% by mass or more, and preferably 98% by mass or less. The content of resin C in the binder resin is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and preferably 45% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less. From the viewpoint of image density of the printed matter, the total content of resin C and resin A in the binder resin is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and is preferably 100% by mass or less, more preferably 100% by mass. In the toner particles, the mass ratio of the content of resin C to the content of resin A (resin C / resin A) is, from the viewpoint of the robustness of the printed coating film, preferably 10 / 90 or more, more preferably 15 / 85 or more, even more preferably 20 / 80 or more, and is preferably 45 / 55 or less, more preferably 40 / 60 or less, even more preferably 35 / 65 or less.
[0060] <Coloring agent> In the present invention, the colorant has a BET specific surface area of 200 m 2 / g or more of carbon black (hereinafter, sometimes simply referred to as "carbon black" or "pigment").
[0061] Examples of carbon black include furnace black, thermal lamp black, acetylene black, and channel black. Among these, furnace black is preferred from the viewpoint of coloring power. From the viewpoint of further improving the image density of the toner, the pH value of the carbon black is preferably 5.0 or more, more preferably 6.0 or more, and even more preferably 7.0 or more, and is preferably 10 or less, more preferably 9.0 or less, and even more preferably 8.5 or less. Specifically, the pH value of carbon black can be measured by the following procedure. (1) 6 g of carbon black, 79 mL of distilled water with a pH of 7, and 1 g of ethanol are placed in a container and mixed. (2) Boil for 15 minutes and then cool to room temperature in 30 minutes. (3) The supernatant is removed by decantation to obtain a slurry having a solid content of 30 to 35% by mass. (4) Insert a pH electrode into the slurry and measure the pH. The pH value of this slurry is the pH value of the carbon black. An example of a pH meter is the "Seven2Go S2" (manufactured by METTLER TOLEDO). From the viewpoint of the chargeability of the toner, the dibutyl phthalate (DBP) oil absorption of the carbon black is preferably 30 ml / 100 g or more, more preferably 60 ml / 100 g or more, even more preferably 100 ml / 100 g or more, and is preferably 160 ml / 100 g or less, more preferably 140 ml / 100 g or less, even more preferably 125 ml / 100 g or less. The DBP oil absorption of carbon black is measured in accordance with "Determination of oil absorption" of ISO4656 (JIS K6217-4:2008). The BET specific surface area of the carbon black is preferably 205 m from the viewpoint of obtaining a toner for developing electrostatic images that can obtain a printed matter with a higher image density and has excellent environmental stability. 2 / g or more, preferably 210m 2 / g or more, and preferably 290m 2 / g or less, more preferably 275m 2 / g or less, more preferably 260m 2 / g or less, more preferably 250m 2 / g or less. The BET specific surface area of carbon black can be measured in accordance with JIS K 6217-2:2017 by the method described in the examples. Some carbon blacks are approved by the FDA (Food and Drug Administration) as food contact substances, and it is preferable to use them when applying the toner of the present invention to printed matter that may come into contact with food, such as packaging paper. That is, in accordance with the FDA approval standards, it is preferable that the amount of polycyclic aromatic hydrocarbons (PAH) contained in the carbon black is 10 ppb or less by mass.
[0062] An example of a commercially available carbon black is “Printex F80” (manufactured by Orion Engineered Carbon Co., Ltd., pH 8.1, DBP oil absorption 105 ml / 100 g, BET specific surface area 225 m 2 / g), "Black Pearls 4750" (manufactured by Ciyabot Corporation, pH 7.9, DBP oil absorption 117 ml / 100 g, BET specific surface area 240 m 2 / g), "Monarch 4750" (manufactured by CABOT Corporation, pH 7.9, DBP oil absorption 122 ml / 100 g, BET specific surface area 258 m 2 / g) and "Monarch 880" (manufactured by CABOT Corporation, pH 7.4, DBP oil absorption 105 ml / 100 g, BET specific surface area 258 m 2 / g) is an example. One or more types of carbon black may be used.
[0063] From the viewpoint of image density of printed matter, the carbon black content in the toner particles is preferably 2% by mass or more, more preferably 3% by mass or more, even more preferably 4% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less. Furthermore, the content of carbon black in the toner particles is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, relative to 100 parts by mass of the binder resin, from the viewpoint of obtaining a printed matter with high image density, and from the viewpoint of environmental stability, it is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less.
[0064] The toner particles may contain, as a colorant, in addition to the carbon black having the above-mentioned specific BET specific surface area, other colorants within a range that does not impair the effects of the present invention. However, the content of the other colorants is preferably 20% by mass or less of the total colorants, more preferably 10% by mass or less, even more preferably 5% by mass or less, even more preferably 3% by mass or less, and even more preferably no other colorants are contained.
[0065] <Release agent> The toner particles preferably contain a release agent. Examples of the release agent include polypropylene wax, polyethylene wax, ethylene propylene copolymer wax, hydrocarbon waxes such as microcrystalline wax, paraffin wax, Fischer-Tropsch wax, and oxides thereof, ester waxes such as carnauba wax, montan wax, and deacidified waxes thereof, and fatty acid ester wax, fatty acid amides, fatty acids, higher alcohols, and fatty acid metal salts. These may be used alone or in combination.
[0066] The melting point of the release agent is preferably 60° C. or higher, more preferably 70° C. or higher, and preferably 160° C. or lower, more preferably 140° C. or lower, even more preferably 120° C. or lower, and even more preferably 100° C. or lower. The content of the release agent in the toner particles is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and preferably 15% by mass or less, more preferably 10% by mass or less, even more preferably 6% by mass or less.
[0067] In addition, the toner particles may contain additives such as a charge control agent, a magnetic powder, a flowability improver, a conductivity adjuster, a reinforcing filler such as a fibrous substance, an antioxidant, an antiaging agent, and a cleaning property improver.
[0068] <Physical properties of toner particles> Volume median particle size of toner particles D 50 From the viewpoint of obtaining a printed coating film with good image quality and further improving the cleaning properties of the toner, the thickness is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.
[0069] The circularity of the toner particles is preferably 0.955 or more, more preferably 0.960 or more, from the viewpoint of obtaining a printed coating film (image) of good quality, and is preferably 0.990 or less, more preferably 0.985 or less, and even more preferably 0.980 or less, from the viewpoint of cleaning ability.
[0070] The CV value of the toner particles is preferably 10% or more, more preferably 12% or more, and even more preferably 14% or more, from the viewpoint of improving the productivity of the toner, and is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less, from the viewpoint of obtaining good image quality. Volume median particle size of toner particles D 50 The circularity can be measured by the method described in the Examples.
[0071] [Toner manufacturing method] A method for producing a toner according to one embodiment of the present invention may be any known method such as a melt kneading method, an emulsion phase inversion method, a suspension polymerization method, or an emulsion aggregation method. The emulsion aggregation method and the melt kneading method are preferred, and the emulsion aggregation method is more preferred.
[0072] <Emulsification aggregation method> The emulsion aggregation method includes a step of aggregating and fusing resin particles containing resin C and a colorant containing carbon black in an aqueous medium.
[0073] (Process for agglomerating resin particles) In the step of aggregating the resin particles, resin particles containing resin C and carbon black are aggregated in an aqueous medium to obtain aggregated particles 1. It is preferable to mix a resin particle dispersion liquid containing resin particles with a colorant particle dispersion liquid containing a colorant (carbon black) to aggregate these particles to obtain aggregated particles 1. When the binder resin contains a resin other than resin C, such as resin A, in addition to resin C, the resin may be contained in the same or different particles as resin C and aggregated, and it is preferable to contain resin C and resin A in the same particles and aggregate them. Here, it is preferable to further aggregate a release agent in addition to the resin particles and the colorant. In addition, in the process of aggregating the resin particles, the aggregated particles 1 may contain additives such as a charge control agent, a magnetic powder, a flowability improver, a conductivity adjuster, a reinforcing filler such as a fibrous substance, an antioxidant, an anti-aging agent, and a cleaning property improver. In the present invention, the aqueous medium is a medium containing water as a main component, and the water content in the aqueous medium is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more and 100% by mass or less. The water is preferably deionized water or distilled water. Examples of components other than water that can constitute an aqueous medium together with water include water-soluble organic solvents such as alkyl alcohols having 1 to 5 carbon atoms; dialkyl ketones having 3 to 5 carbon atoms, such as acetone and methyl ethyl ketone; and cyclic ethers, such as tetrahydrofuran.
[0074] <<Method of manufacturing resin particle dispersion>> The resin particles are preferably produced as an aqueous dispersion using an aqueous medium.
[0075] The dispersion can be carried out by a known method, but it is preferable to disperse the resin by a phase inversion emulsification method. For example, the phase inversion emulsification method includes a method of adding an aqueous medium to an organic solvent solution of a resin or a molten resin to carry out phase inversion emulsification. A method of adding an aqueous medium to an organic solvent solution of a resin to carry out phase inversion emulsification is preferable. The organic solvent used for phase inversion emulsification is not particularly limited as long as it dissolves the resin and is water-soluble. For resin C and resin A, for example, methyl ethyl ketone is included. A neutralizing agent may be added to the organic solvent solution. Examples of the neutralizing agent include basic substances. Examples of the basic substance include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; and nitrogen-containing basic substances such as ammonia, trimethylamine, and diethanolamine. Among these, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide are preferred. The degree of neutralization of the resin constituting the resin particles is preferably 40 mol% or more, more preferably 50 mol% or more, even more preferably 55 mol% or more, and preferably 100 mol% or less, more preferably 95 mol% or less, even more preferably 90 mol% or less. The degree of neutralization of the resin constituting the resin particles can be calculated by the following formula. Degree of neutralization (mol%) = [{weight of neutralizing agent added (g) / equivalent weight of neutralizing agent} / [{weighted average acid value of resin constituting resin particle (mgKOH / g) × weight of resin constituting resin particle (g)} / (56 × 1000)]] × 100
[0076] While stirring the organic solvent solution of the resin or the molten resin, the aqueous medium is gradually added to cause phase inversion. From the viewpoint of improving the dispersion stability of the resin particles, the temperature of the organic solvent solution when the aqueous medium is added is preferably not less than the glass transition temperature of the resin constituting the resin particles, more preferably not less than 70°C, and is preferably not more than 100°C, more preferably not more than 95°C, and even more preferably not more than 90°C.
[0077] After the phase inversion emulsification, the organic solvent may be removed from the obtained dispersion by distillation or the like, if necessary. The resin particles may also be isolated by filtration or the like. It is preferable to use an aqueous dispersion of resin particles obtained by removing the organic solvent from the dispersion obtained after the phase inversion emulsification. In this case, the remaining amount of the organic solvent in the dispersion is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably substantially 0% by mass.
[0078] Volume median particle size of resin particles D 50 is preferably 0.08 μm or more, more preferably 0.12 μm or more, and is preferably 1 μm or less, more preferably 0.5 μm or less, and further preferably 0.3 μm or less. The CV value of the resin particles is preferably 10% or more, more preferably 15% or more, and is preferably 35% or less, more preferably 30% or less. Volume median particle size of resin particles D 50 The CV value is measured by the method described in the Examples.
[0079] From the viewpoint of improving the productivity of the toner and the dispersion stability of the aqueous dispersion of the resin particles, the solids concentration of the aqueous dispersion of the resin particles is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less. The solid content is the total amount of non-volatile components.
[0080] <<Method of manufacturing colorant particle dispersion>> The colorant particle dispersion is preferably obtained by dispersing a colorant containing carbon black and an aqueous medium using a dispersing machine such as a homomixer, a homogenizer, or an ultrasonic dispersing machine. The dispersion is preferably performed in the presence of a dispersant from the viewpoint of improving the dispersion stability of the pigment. Examples of the dispersant include a surfactant. The dispersion may also be performed in the presence of an addition polymer E. The addition polymer E preferably has a constitutional unit derived from an addition polymerizable monomer a having an aromatic group, and further preferably contains at least one selected from the group consisting of an addition polymerizable monomer b having an ionic group, an addition polymerizable monomer c having a polyalkylene oxide group, and a macromonomer d. For the colorant particle dispersion using the addition polymer E, the addition polymer E described in JP-A-2021-026129 is referred to.
[0081] Examples of surfactants that improve the dispersion stability of the pigment include nonionic surfactants, anionic surfactants, and cationic surfactants, and from the viewpoint of improving the dispersion stability of the pigment, nonionic surfactants are preferred. Examples of nonionic surfactants include polyoxyalkylene alkyl ethers, polyoxyalkylene alkenyl ethers, and polyoxyalkylene aryl ethers. Among these, polyoxyethylene aryl ethers are preferred, and polyoxyethylene distyrenated phenyl ether is more preferred.
[0082] In the colorant particle dispersion, the mass ratio of the colorant (carbon black) to the dispersant (colorant / dispersant) is preferably 50 / 50 or more, more preferably 60 / 40 or more, and even more preferably 65 / 35 or more, from the viewpoints of the electrostatic chargeability of the toner and the image density of the printed matter, and is preferably 95 / 5 or less, and more preferably 90 / 10 or less.
[0083] The content of the colorant in the colorant particle dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and even more preferably 25% by mass or less. The solids concentration of the colorant particle dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less.
[0084] Volume median particle size D of colorant particles 50 From the viewpoint of improving dispersibility in toner particles, the average particle diameter is preferably 0.02 μm or more, more preferably 0.04 μm or more, even more preferably 0.06 μm or more, and is preferably 0.20 μm or less, more preferably 0.15 μm or less, even more preferably 0.10 μm or less. From the viewpoint of improving dispersibility in the toner particles, the CV value of the colorant particles is preferably 10% or more, more preferably 20% or more, and is preferably 40% or less, more preferably 35% or less, and even more preferably 30% or less. Volume median particle size D of colorant particles 50 and CV values are measured by the methods in the Examples.
[0085] <<Method of manufacturing release agent particle dispersion>> The release agent particle dispersion liquid can be obtained, for example, by dispersing a dispersion liquid of the release agent and resin particles, and optionally an aqueous medium, at a temperature equal to or higher than the melting point of the release agent, using a dispersing machine such as a homogenizer, a high-pressure dispersing machine, or an ultrasonic dispersing machine. The heating temperature during dispersion is preferably equal to or higher than the melting point of the release agent and equal to or higher than 80°C, more preferably equal to or higher than 85°C, even more preferably equal to or higher than 90°C, and is preferably equal to or lower than 100°C, more preferably equal to or lower than 98°C, even more preferably equal to or lower than 96°C.
[0086] The release agent particle dispersion can be obtained by using a surfactant, but is preferably obtained by mixing the release agent and resin particles. By preparing the release agent particles using the release agent and resin particles, the release agent particles are stabilized by the resin constituting the resin particles, and it becomes possible to disperse the release agent in an aqueous medium without using a surfactant. It is considered that the release agent particle dispersion has a structure in which a large number of resin particles are attached to the surface of the release agent particles. The resin constituting the resin particles in which the release agent is dispersed is preferably a polyester resin, and it is more preferable to use a composite resin having a polyester resin segment and an addition polymerization resin segment. For the release agent particle dispersion and the composite resin, reference is made to JP2021-182045A. In addition, the above-mentioned amorphous polyester resin A may be used. The dispersion of resin particles in which the release agent is dispersed is obtained by the above-mentioned method for producing the resin particle dispersion.
[0087] Volume median particle size D of release agent particles 50 From the viewpoint of obtaining uniform aggregated particles by aggregation, the average particle size is preferably 0.05 μm or more, more preferably 0.2 μm or more, even more preferably 0.3 μm or more, and is preferably 1 μm or less, more preferably 0.8 μm or less, even more preferably 0.6 μm or less. The CV value of the release agent particles in the release agent particle dispersion is preferably 10% or more, more preferably 20% or more, and is preferably 40% or less, more preferably 35% or less. Volume median particle diameter D of release agent particles in release agent particle dispersion 50 The CV value is measured by the method described in the Examples.
[0088] -Surfactants- In the step of aggregating the resin particles, when the dispersions of the respective particles are mixed to prepare a mixed dispersion, the process may be carried out in the presence of a surfactant from the viewpoint of improving the dispersion stability of the resin particles, the release agent particles, the colorant particles, etc. Examples of the surfactant include anionic surfactants such as alkylbenzene sulfonates and alkyl ether sulfates; and nonionic surfactants such as polyoxyethylene alkyl ethers and polyoxyethylene alkenyl ethers. When a surfactant is used, the total amount used is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the binder resin in the aggregated particles 1, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less.
[0089] -Flocculant- In the step of aggregating the resin particles, it is preferable to add an aggregating agent from the viewpoint of efficient aggregation. Examples of the flocculant include cationic surfactants such as quaternary salts, organic flocculants such as polyethyleneimine, and inorganic flocculants. Examples of the inorganic flocculant include inorganic metal salts such as sodium sulfate, sodium nitrate, sodium chloride, calcium chloride, and calcium nitrate; inorganic ammonium salts such as ammonium sulfate, ammonium chloride, and ammonium nitrate; and divalent or higher metal complexes. From the viewpoint of improving the coagulation properties and obtaining uniformly coagulated particles 1, inorganic coagulants having a valence of 1 to 5 are preferred, inorganic metal salts having a valence of 1 to 2 and inorganic ammonium salts are more preferred, inorganic ammonium salts are even more preferred, and ammonium sulfate is even more preferred.
[0090] For example, 25 parts by mass or more and 50 parts by mass or less of the aggregating agent is added to a mixed dispersion liquid containing resin particles, release agent particles, and colorant particles at 0° C. or more and 40° C. or less, relative to 100 parts by mass of the binder resin in aggregated particles 1, and the resin particles, release agent particles, and colorant particles are aggregated in an aqueous medium to obtain aggregated particles 1. Furthermore, from the viewpoint of promoting aggregation, it is preferable to increase the temperature of the dispersion liquid after adding the aggregating agent.
[0091] Examples of a method for stopping the aggregation include a method of cooling the dispersion, a method of adding an aggregation terminator, a method of diluting the dispersion, etc. From the viewpoint of reliably preventing unnecessary aggregation, a method of stopping the aggregation by adding an aggregation terminator is preferred.
[0092] -Aggregation stopper- The aggregation terminator is preferably a surfactant, more preferably an anionic surfactant. Examples of the anionic surfactant include alkylbenzenesulfonate, alkyl sulfate, alkyl ether sulfate, polyoxyalkylene alkyl ether sulfate, arylsulfonate, and arylsulfonic acid formalin condensate, and are preferably an alkali metal salt of arylsulfonic acid formalin condensate, and more preferably a sodium salt of β-naphthalenesulfonic acid formalin condensate. These may be used alone or in combination. The aggregation terminator may be added in the form of an aqueous solution. The amount of the aggregation terminator added is preferably 1 part by mass or more, and more preferably 3 parts by mass or more, relative to 100 parts by mass of the binder resin in the aggregated particles 1 from the viewpoint of reliably preventing unnecessary aggregation, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 9 parts by mass or less, from the viewpoint of reducing residue in the toner.
[0093] Volume median particle size D of aggregate 1 50 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less. Volume median particle diameter D of aggregated particles 1 in the dispersion 50 is measured by the method described in the Examples.
[0094] In the present invention, after the step of aggregating the resin particles and before the step of fusing, a step of adhering shell resin particles containing an amorphous resin to the obtained aggregated particles 1 and aggregating them to obtain aggregated particles 2 may be included. By including the step of aggregating the shell resin particles, toner particles having a core-shell structure can be obtained. The shell resin particles are preferably made of a non-crystalline resin, more preferably a non-crystalline polyester resin, and the above-mentioned resin A may be used. The shell resin particle dispersion liquid can be obtained by the above-mentioned method for producing a resin particle dispersion liquid. Furthermore, when the toner manufacturing method includes a step of aggregating shell resin particles, it is preferable to stop the aggregation in the step when the aggregated particles 2 have grown to an appropriate particle size for toner particles, and a method of stopping the aggregation by adding the above-mentioned aggregation terminator is preferable. The mass ratio of the shell resin particles to the mass of the aggregated particles 1 [shell resin particles / aggregated particles 1] is, from the viewpoint of low-temperature fixing property of the toner, preferably 1 / 99 or more, more preferably 3 / 97 or more, even more preferably 5 / 95 or more, and is preferably 25 / 75 or less, more preferably 20 / 80 or less, even more preferably 15 / 85 or less.
[0095] (Fusing process) In the fusion step, for example, the aggregated particles are fused in an aqueous medium. By fusion, the individual particles contained in the aggregated particles are fused together to obtain fused particles. In the fusion step, from the viewpoint of improving the fusion properties of the aggregated particles and from the viewpoint of improving the low-temperature fixing properties of the toner, the aggregated particles are maintained at a temperature equal to or higher than the glass transition temperature of the resin having the highest glass transition temperature among the amorphous polyester resins contained in the aggregated particles. From the viewpoint of improving the productivity of the toner, the holding (heating) temperature when fusing the aggregated particles is preferably equal to or higher than the glass transition temperature of the resin having the highest glass transition temperature among the amorphous polyester resins, more preferably equal to or higher by 2° C., and even more preferably equal to or higher by 5° C., and is preferably equal to or lower than a temperature 30° C. higher, more preferably equal to or lower by 25° C., and even more preferably equal to or lower by 20° C. higher than the glass transition temperature of the resin having the highest glass transition temperature among the amorphous polyester resins. In this case, it is preferable to maintain the temperature at the above temperature until the desired circularity is achieved.
[0096] The volume median particle size D of the fused particles obtained by fusion 50 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.
[0097] The circularity of the fused particles obtained by fusion is preferably 0.955 or more, more preferably 0.960 or more, and is preferably 0.990 or less, more preferably 0.985 or less, and further preferably 0.980 or less. The fusion is preferably terminated after the desired circularity is reached. The circularity is measured by the method described in the Examples.
[0098] (Post-processing) After the fusion step, a post-treatment step may be performed, and the fused particles are isolated to obtain toner particles. Since the fused particles obtained in the fusion step are present in an aqueous medium, it is preferable to first perform solid-liquid separation. For the solid-liquid separation, a suction filtration method or the like is preferably used. It is preferable to wash the solid-liquid separation product. In this case, it is preferable to remove the surfactant added, and therefore it is preferable to wash the product with an aqueous medium at a temperature below the cloud point of the surfactant. It is preferable to wash the product several times. Next, drying is preferably performed. Examples of the drying method include vacuum constant temperature drying, vibration type fluidized bed drying, spray drying, freeze drying, and flash jet drying.
[0099] <Melt kneading method> In the present invention, the melt-kneading method involves, for example, uniformly mixing a binder resin, a colorant, and, if necessary, additives such as a release agent in a mixer such as a Henschel mixer, and then melt-kneading the mixture in an internal kneader, a single-screw or twin-screw extruder, an open roll type kneader, etc. The mixture is then cooled, pulverized, and classified to produce toner particles.
[0100] The toner contains toner particles. The obtained toner particles can be used as the toner of the present invention as they are. It is also preferable to use the toner particles, which are treated by adding an external additive to the surface thereof, as the toner of the present invention.
[0101] <External additives> Examples of the external additive include inorganic fine particles such as hydrophobic silica, titanium oxide, alumina, cerium oxide, and carbon black, and polymer fine particles such as polycarbonate, polymethyl methacrylate, and silicone resin. Among these, hydrophobic silica is preferred. One type of external additive may be used alone, or two or more types may be used. Two or more types of hydrophobic silica having different particle sizes may also be used. When the toner particles are surface-treated using an external additive, the amount of the external additive added is, relative to 100 parts by mass of the toner particles, preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, and preferably 5 parts by mass or less, more preferably 4.5 parts by mass or less, even more preferably 4 parts by mass or less.
[0102] Toners are used for developing electrostatic images in electrophotographic printing. The toners can be used, for example, as one-component developers or mixed with a carrier to form two-component developers. EXAMPLES
[0103] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Each property value was measured and evaluated by the following methods. In the notation such as "alkylene oxide (X)", the number X in parentheses means the average number of moles of alkylene oxide added.
[0104] [Measurement method] [Acid value of resin] The acid value of the resin was measured according to the neutralization titration method described in JIS K 0070:1992, except that the measurement solvent was chloroform.
[0105] [Softening point, crystallinity index, melting point and glass transition temperature of resin] (1) Softening point Using a flow tester "CFT-500D" (Shimadzu Corporation), 1 g of sample was heated at a temperature increase rate of 6°C / min, while applying a load of 1.96 MPa with the plunger, and extruding the sample from a nozzle with a diameter of 1 mm and a length of 1 mm. The plunger descent amount of the flow tester was plotted against the temperature, and the temperature at which half of the sample flowed out was taken as the softening point. (2) Crystallinity index Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of sample was weighed into an aluminum pan and cooled to 0°C at a rate of 10°C / min. The temperature was then held for 1 minute, and the temperature was then raised to 180°C at a rate of 10°C / min to measure the calorific value. The temperature of the peak with the largest peak area among the observed endothermic peaks was taken as the endothermic maximum peak temperature (1), and the crystallinity index was calculated by (softening point (°C)) / (endothermic maximum peak temperature (1) (°C)). (3) Melting point and glass transition temperature Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of the sample was weighed into an aluminum pan, heated to 200°C, and cooled to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min, and the amount of heat was measured. The temperature of the peak with the largest peak area among the endothermic peaks observed was taken as the maximum endothermic peak temperature (2). In the case of a crystalline resin, the peak temperature was taken as the melting point. In the case of an amorphous resin, when a peak was observed, the temperature of the peak was taken, and when a step was observed without a peak, the temperature of the intersection of the tangent showing the maximum slope of the curve of the step and the extension of the baseline on the low temperature side of the step was taken as the glass transition temperature.
[0106] [Melting point of release agent] Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of the sample was weighed into an aluminum pan, heated to 200°C, and cooled to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min, the calorific value was measured, and the maximum endothermic peak temperature was taken as the melting point.
[0107] [Volume median particle size D of resin particles, release agent particles, and colorant particles 50 and CV value] (1) Measuring device: Laser diffraction type particle size measuring device "LA-920" (manufactured by Horiba Ltd.) (2) Measurement conditions: Put the sample dispersion into the measurement cell, add distilled water, and measure the volume median particle size D at a concentration where the absorbance is in the appropriate range. 50 and volume average particle size D V The CV value (particle size distribution) was calculated according to the following formula. CV value (%) = (Standard deviation of particle size distribution / Volume average particle size D V ) x 100
[0108] [Solid Content Concentration of Resin Particle Dispersion, Colorant Particle Dispersion, and Release Agent Particle Dispersion] Using an infrared moisture meter "FD-230" (Kett Electric Laboratory Co., Ltd.), the moisture content (mass%) of 5 g of the measurement sample was measured at a drying temperature of 150°C and measurement mode 96 (monitoring time 2.5 min / fluctuation range 0.05%). The solid content concentration was calculated according to the following formula. Solid content concentration (mass%) = 100-moisture (mass%)
[0109] [Volume median particle diameter of agglomerated particles D 50 〕 Volume median particle size of agglomerated particles D 50 was measured as follows: Measuring instrument: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50μm Analysis software: "Multisizer (registered trademark) III version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured and the volume median particle size D is calculated from the particle size distribution. 50 asked for.
[0110] [Circularity of Fused Particles and Toner Particles] The circularity of the fused particles was measured under the following conditions. Measurement equipment: Flow-type particle image analyzer "FPIA-3000" (Sysmex Corporation) Preparation of dispersion: A dispersion of fused particles or toner particles was prepared by diluting with deionized water so that the solid content concentration was 0.001 to 0.05% by mass. Measurement mode: HPF measurement mode
[0111] [Volume median particle size of toner particles D 50 〕 Volume median particle size of toner particles D 50 was measured as follows: The measuring instrument, aperture diameter, analysis software, and electrolyte were set to the volume median particle diameter D50 The same one used in the measurement was used. Dispersion liquid: Polyoxyethylene lauryl ether "EMULGEN (registered trademark) 109P" (manufactured by Kao Corporation, HLB (hydrophile-lipophile balance): 13.6) was dissolved in the electrolyte to obtain a dispersion liquid with a concentration of 5% by mass. Dispersion conditions: 10 mg of a measurement sample of toner particles was added to 5 mL of the dispersion liquid, and the mixture was dispersed for 1 minute using an ultrasonic disperser. Thereafter, 25 mL of the electrolyte was added, and the mixture was further dispersed for 1 minute using an ultrasonic disperser to prepare a sample dispersion liquid. Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured and the volume median particle size D is calculated from the particle size distribution. 50 asked for.
[0112] [BET specific surface area] The BET specific surface area of carbon black was measured in accordance with JIS K6217-2:2017 "Determination of specific surface area". The measurement device used was a multi-sample high-performance specific surface area / pore distribution measurement device "3FLEX" (manufactured by Shimadzu Corporation), and 1.0 g of the sample was measured using the volumetric method for detection and the multipoint method for measurement.
[0113] [Resin manufacturing] [Production of Crystalline Polyester Resin C] Production examples C1~C4, C51, C52 (manufacture of resins C-1~C-4, C-51, C-52) The alcohol and carboxylic acid components shown in Table 1 were placed in a 10 L four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 200°C over 8 hours in a nitrogen atmosphere in a mantle heater. Then, an esterification catalyst was added, and the reaction was carried out at 8 kPa until the softening point shown in Table 1 was reached, obtaining crystalline polyester resins C-1 to C-4, C-51, and C-52. The physical properties are shown in Table 1.
[0114] Manufacturing Example C5 (Manufacturing of Resin C-5) The alcohol component, carboxylic acid component, and polymerization inhibitor shown in Table 1 were placed in a 10 L four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 200°C over 8 hours in a nitrogen atmosphere in a mantle heater. Then, the esterification catalyst shown in Table 1 was added, and the reaction was carried out at 8 kPa until the softening point shown in Table 1 was reached, obtaining crystalline polyester resin C-5. The physical properties are shown in Table 1.
[0115] [Table 1]
[0116] [Production of amorphous polyester resin] Production Example A1 (Production of Resin A-1) The inside of a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was replaced with nitrogen, and 4367g of propylene oxide (2.2) adduct of bisphenol A, 1098g of terephthalic acid, 32g of tin (II) di(2-ethylhexanoate), and 3.2g of gallic acid (3,4,5-trihydroxybenzoic acid) were added. The reaction system was heated to 235°C under a nitrogen atmosphere while stirring, and then maintained at 235°C for 5 hours. The pressure in the flask was then reduced and maintained at 8kPa for 1 hour. After that, the pressure was returned to atmospheric pressure, and the mixture was cooled to 160°C. While maintaining the temperature at 160°C, a mixture of 1070g of styrene, 267g of stearyl methacrylate, 144g of acrylic acid, and 160g of dibutyl peroxide was added dropwise to the reaction system over 3 hours. After that, the reaction system was kept at 160°C for 30 minutes, then heated to 200°C, and the pressure in the flask was further reduced and kept at 8kPa for 1 hour. After that, the pressure was returned to atmospheric pressure, and the mixture was cooled to 190°C, and 174g of fumaric acid, 378g of sebacic acid, 240g of trimellitic anhydride, and 3.2g of 4-tert-butylcatechol were added, and the temperature was raised to 210°C at 10°C / hr, and then the reaction was continued at 4kPa until the desired softening point, to obtain Resin A-1. The physical properties are shown in Table 2.
[0117] Manufacturing Example D1 (Manufacturing of Resin D-1) The inside of a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was replaced with nitrogen, and 3450g of a propylene oxide (2.2) adduct of bisphenol A, 655g of terephthalic acid, 24g of tin (II) di(2-ethylhexanoate), and 2.4g of gallic acid (3,4,5-trihydroxybenzoic acid) were added, and the reaction system was heated to 235°C while stirring under a nitrogen atmosphere, and then maintained at 235°C for 5 hours, after which the pressure in the flask was reduced and maintained at 8kPa for 1 hour. After that, the pressure was returned to atmospheric pressure, and then cooled to 160°C, and a mixture of 2133g of styrene, 533g of stearyl methacrylate, 114g of acrylic acid, and 320g of dibutyl peroxide was added dropwise over 3 hours while maintaining the temperature at 160°C. The reaction system was then held at 160°C for 30 minutes, then heated to 200°C, and the pressure in the flask was further reduced and held at 8kPa for 1 hour. After that, the pressure was returned to atmospheric pressure, and the mixture was cooled to 190°C, 582g of succinic acid was added, and the mixture was heated to 210°C at 10°C / hr, and then reacted at 4kPa until the desired softening point was reached, yielding Resin D-1. The physical properties are shown in Table 2.
[0118] [Table 2]
[0119] [Production of Resin Particle Dispersion] Production Example X1 (Production of Resin Particle Dispersion X-1) 75 g of resin C-1, 225 g of resin A-1, 300 g of methyl ethyl ketone, and 59 g of deionized water were placed in a 3 L vessel equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen inlet tube, and the resins were dissolved over 2 hours at 73° C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution so that the degree of neutralization was 60 mol% relative to the acid value of the resin, and the mixture was stirred for 30 minutes. Next, while maintaining the temperature at 73°C, 600 g of deionized water was added over 60 minutes while stirring at 280 r / min (circumferential speed 88 m / min) to cause phase inversion emulsification. While continuing to maintain the temperature at 73°C, methyl ethyl ketone was distilled off under reduced pressure to obtain an aqueous dispersion. Thereafter, while continuing to stir at 280 r / min (circumferential speed 63 m / min), the aqueous dispersion was cooled to 30°C, and deionized water was added so that the solid concentration was 20 mass%, thereby obtaining resin particle dispersion X-1. The volume median particle diameter D of the obtained resin particles was 50 and CV values are shown in Table 3.
[0120] Production examples X2~X5, X51, X52 (manufacture of resin particle dispersions X-2~X-5, X-51, X-52) Resin particle dispersions X-2 to X-5, X-51, and X-52 were obtained in the same manner as in Production Example X1, except that the type of resin used was changed as shown in Table 3. The volume median particle diameter D 50 and CV values are shown in Table 3.
[0121] [Table 3]
[0122] Production Example Y1 (Production of Resin Particle Dispersion Y-1) 200 g of Resin D-1 and 200 g of methyl ethyl ketone were placed in a 3 L vessel equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen inlet tube, and the resin was dissolved for 2 hours at 73° C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution so that the degree of neutralization was 60 mol% relative to the acid value of Resin D-1, and the mixture was stirred for 30 minutes. Next, while maintaining the temperature at 73°C, 700g of deionized water was added over 50 minutes while stirring at 280 r / min to cause phase inversion emulsification. While maintaining the temperature at 73°C, the methyl ethyl ketone was distilled off under reduced pressure to obtain an aqueous dispersion. Thereafter, while stirring at 280 r / min, the aqueous dispersion was cooled to 30°C, and deionized water was added so that the solid content concentration was 20 mass%, to obtain resin particle dispersion Y-1. The volume median particle diameter of the resin particles was 0.09 μm, and the CV value was 23%.
[0123] [Preparation of Release Agent Particle Dispersion] Production Example W1 (Production of Release Agent Particle Dispersion W-1) Into a 1 L beaker were added 120 g of deionized water, 86 g of resin particle dispersion Y-1, and 40 g of paraffin wax "HNP-9" (manufactured by Nippon Seiro Co., Ltd., melting point 75°C), and the mixture was melted by maintaining the temperature at 90 to 95°C and stirred to obtain a molten mixture. The obtained molten mixture was dispersed for 20 minutes using an ultrasonic homogenizer "US-600T" (manufactured by Nippon Seiki Seisakusho Co., Ltd.) while maintaining the temperature at 90 to 95°C, and then cooled to room temperature (20°C). Deionized water was added to the obtained dispersion to adjust the solid content to 20 mass%, thereby obtaining a release agent particle dispersion W-1. The volume median particle diameter D of the release agent particles was 50 The diameter was 0.47 μm and the CV value was 27%.
[0124] [Preparation of Colorant Particle Dispersion] Production Example E1 (Production of Colorant Particle Dispersion E-1) Carbon black "Printex F80" (BET specific surface area 225 m) in a 2L container 2160g of 1,2-dichlorophenyl ether (1.2g / g) (manufactured by Orion Engineered Carbon), 40g of nonionic surfactant (polyoxyethylene distyrenated phenyl ether) "Emulgen A-60", and 750g of deionized water were added, and the mixture was stirred at 6400 rpm / min at 20°C for 1 hour using a mixer "Labo-lution" (manufactured by Primix Corporation) equipped with a dispersing blade. The mixture was then passed through a 200-mesh filter and treated 15 times at a pressure of 150 MPa using a homogenizer "Microfluidizer M-110EH" (manufactured by Microfluidics). The mixture was then passed through a 200-mesh filter, and deionized water was added so that the solid content concentration was 20% by mass, to obtain colorant particle dispersion E-1. The volume median particle diameter D of the colorant particles was 1.2g / g. 50 and CV values are shown in Table 4.
[0125] Production Examples E2, E3, and E51 (Production of Colorant Particle Dispersions E-2, E-3, and E-51) A colorant particle dispersion was obtained in the same manner as in Production Example E1, except that the colorant used was changed. The volume median particle diameter D of the colorant particles in the obtained colorant particle dispersions E-2, E-3, and E-51 was 50 and CV values are shown in Table 4.
[0126] [Table 4]
[0127] [Toner manufacturing] Example 1 (Production of Toner 1) 500 g of resin particle dispersion X-1, 35 g of release agent particle dispersion W-1, 44 g of colorant particle dispersion E-1, and 1.1 g of 15% by mass sodium dodecylbenzenesulfonate aqueous solution "Neopelex G-15" (Kao Corporation, anionic surfactant) were placed in a 3 L four-neck flask equipped with a dehydration tube, a stirrer, and a thermocouple, and mixed at a temperature of 25° C. Next, while stirring the resulting mixture, a solution obtained by dissolving 40 g of ammonium sulfate in 570 g of deionized water and adding a 4.8% by mass potassium hydroxide aqueous solution to adjust the pH to 8.4 was added dropwise over 10 minutes at 25° C., and the temperature was then raised to 61° C. over 2 hours, and the volume median particle diameter D of the aggregated particles was measured. 50 The temperature was maintained at 61° C. until the particle size reached 6.3 μm, thereby obtaining a dispersion of aggregated particles 1. To the obtained dispersion of aggregated particles 1, an aqueous solution obtained by mixing 20 g of sodium polyoxyethylene lauryl ether sulfate "EMAL E-27C" (manufactured by Kao Corporation, anionic surfactant, effective concentration 27% by mass), 280 g of deionized water, and 40 g of 0.1 mol / L aqueous sulfuric acid solution was added. Thereafter, the temperature was raised to 75°C over 1 hour, and the mixture was kept at 75°C for 30 minutes, after which 15 g of 0.1 mol / L aqueous sulfuric acid solution was added, and the mixture was further kept at 75°C for 15 minutes. Thereafter, 15 g of 0.1 mol / L aqueous sulfuric acid solution was added again, and the mixture was kept at 75°C until the circularity reached 0.970, thereby obtaining a dispersion of fused particles in which aggregated particles 1 were fused. The obtained dispersion of fused particles was cooled to 30°C, and the solid content was separated by suction filtration of the dispersion, washed with deionized water at 25°C, and suction filtration was performed for 2 hours at 25°C. Thereafter, the solid content was vacuum dried at 33°C for 24 hours using a vacuum constant temperature dryer "DRV622DA" (manufactured by ADVANTEC Co., Ltd.) to obtain toner particles. 100 parts by mass of toner particles, 2.5 parts by mass of hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd., number average particle size; 0.04 μm), and 1.0 part by mass of hydrophobic silica "Cabosil (registered trademark) TS720" (manufactured by Cabot Corporation, number average particle size; 0.012 μm) were put into a Henschel mixer and stirred, and the mixture was passed through a 150 mesh sieve to obtain toner 1. The volume median particle size D of the obtained toner particles was 50The particle diameter was 6.0 μm and the circularity was 0.970. The obtained toner 1 was evaluated as follows. The evaluation results of toner 1 are shown in Table 5.
[0128] [Toner Evaluation] [Evaluation of pencil hardness of printed coating (fastness of printed coating)] A polypropylene film label, OPP50C (manufactured by Lintec Corporation), cut to A4 size was printed using a commercially available printer, Microline (registered trademark) 5400 (manufactured by Oki Electric Industry Co., Ltd.), with the toner adhesion amount on the film label being 0.43 to 0.45 mg / cm 2 A solid image of the above was printed without fixing, leaving a 5 mm margin from the top of an A4 size film label, and a length of 50 mm. Next, the same printer was prepared with a temperature-variable fixing unit, the fixing unit temperature was set to 100°C, and Toner 1 was fixed at a speed of 3 seconds per sheet in the A4 portrait direction to form a printing coating, and a label print was obtained (equivalent to 20 sheets / minute in A4 portrait). The pencil hardness of the printed coating film of the obtained label print was measured in accordance with JIS K5600-5-4 using a pencil scratch coating hardness tester ("D-NP (model number)", manufactured by Toyo Seiki Seisakusho Co., Ltd.) and pencils for pencil scratch value testing (6B, 5B, 4B, 3B, 2B, B, HB, F, H) (manufactured by Mitsubishi Pencil Co., Ltd.). The printed coating film was scratched five times with pencils of each hardness in the order of 6B, 5B, 4B, 3B, 2B, B, HB, F, and H, and the hardest pencil that did not produce scratches three or more times was taken as the pencil hardness of the printed coating film of the label print. "H" is the most excellent in pencil hardness (fastness of the printed coating film) of the printed coating film.
[0129] Examples 2 to 7 and Comparative Examples 1 to 3 (Production of Toners 2 to 7 and 81 to 83) Toners 2 to 7 and 81 to 83 were produced in the same manner as in Example 1, except that the types of resin particle dispersion and colorant particle dispersion used were changed as shown in Table 5. The evaluation results of toners 2 to 7 and 81 to 83 are shown in Table 5.
[0130] [Table 5]
[0131] Example 8 (Preparation of Toner 8) 75 parts by mass of resin A-1, 25 parts by mass of resin C-1, 7 parts by mass of carbon black (Printex F80, manufactured by Cabot Corporation), and 5 parts by mass of paraffin wax "HNP-9" (manufactured by Nippon Seiro Co., Ltd., melting point 75°C) as a release agent were mixed in a Henschel mixer. The obtained mixture was melt-kneaded at a screw rotation speed of 200 r / min and a barrel set temperature of 100°C using a co-rotating twin-screw extruder with a kneading section total length of 1560 mm, a screw diameter of 42 mm, and a barrel inner diameter of 43 mm, to obtain a melt-kneaded product. The feed rate of the mixture was 20 kg / hour, and the average residence time was about 18 seconds. The obtained melt-kneaded product was cooled and coarsely crushed, then crushed in a jet mill, and classified using an airflow classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd.) to obtain a volume median particle size D 50 As a result, powder (toner particles) with a particle size of 6.0 μm was obtained. 100 parts by mass of toner particles, 2.5 parts by mass of hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd., number average particle size: 0.04 μm), and 1.0 part by mass of hydrophobic silica "Cabosil (registered trademark) TS720" (manufactured by Cabot Corporation, number average particle size: 0.012 μm) were placed in a Henschel mixer, stirred, and passed through a 150 mesh sieve to obtain Toner 8. The evaluation results of Toner 8 are shown in Table 6.
[0132] [Table 6]
[0133] The toner of the present invention (the toners of Examples 1 to 8) is a binder containing a crystalline polyester resin C having an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less, and a BET specific surface area of 200 m 2 The toner contains a colorant containing carbon black of at least 100 / g, and the printed coating film obtained from the toner has a pencil hardness of "B" or higher, and the printed coating film has excellent fastness. In contrast, the toner of Comparative Example 1 used a binder containing resin C having an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less, but had a BET specific surface area of 200 m 2 / g (116m 2 The toner of Comparative Example 2 had a BET specific surface area of 200 m2, and the toner of Comparative Example 2 had a BET specific surface area of 200 m2. 2 The toner of Comparative Example 3 used carbon black having a BET specific surface area of 200 m or more, but the resin C having an ester group concentration of more than 9.0 mmol / g (12.0 mmol / g) was used, so that the pencil hardness of the printed coating film obtained from the toner was "4B", and sufficient fastness of the printed coating film was not obtained. 2 / g or more of carbon black was used, but because resin C with an ester group concentration of less than 6.5 mmol (6.3 mmol / g) was used, the pencil hardness of the printed coating film obtained from the toner was "5B," and sufficient robustness of the printed coating film was not obtained.
Claims
1. A toner for developing electrostatic images, comprising a binder resin and a colorant, the binder resin contains a crystalline polyester resin C having an ester group concentration of 6.5 mmol / g or more and 9.0 mmol / g or less, The colorant has a BET specific surface area of 200 m 2 / g or more of carbon black, Toner for developing electrostatic images.
2. The colorant has a BET specific surface area of 210 m 2 / g or more 250m 2 2. The toner for developing electrostatic images according to claim 1, which contains carbon black in an amount of 0.1 to 1.0 g / g or less.
3. 3. The toner for developing electrostatic images according to claim 1, wherein the binder resin further comprises an amorphous polyester resin A.
4. 3. The toner for developing electrostatic images according to claim 1, wherein the crystalline polyester resin C comprises a polycondensate of an alcohol component containing 80 mol % or more of ethylene glycol and a carboxylic acid component.
5. 3. The toner for developing electrostatic images according to claim 1, wherein the crystalline polyester resin C contains a constituent unit derived from a monoalcohol and / or a constituent unit derived from a monocarboxylic acid.
6. 3. A method for producing the toner for developing electrostatic images according to claim 1 or 2, comprising the steps of aggregating and fusing the resin particles and the colorant particles, The resin particles contain a crystalline polyester resin C having an ester group concentration of 6.5 smol / g or more and 9.0 mmol / g or less, The colorant particles have a BET specific surface area of 200 m 2 / g or more of carbon black, A method for producing a toner for developing electrostatic images.
Citation Information
Patent Citations
Negative charge type black toner
JP2005352247A
Toner for developing electrostatic charged image and manufacturing method therefor, developer for developing electrostatic charged image, toner cartridge, process cartridge, and image forming apparatus
JP2009075342A
Manufacturing method of toner for electrostatic charge image development
JP2015036720A
Toner
JP2022174943A
Method for manufacturing toner for electrostatic charge image development
JP2020060687A