Eraser composition

The eraser composition with vinyl chloride-vinyl acetate copolymer and cyclohexane-1,2-dicarboxylic acid ester ensures eraser debris remains attached, addressing scattering issues and facilitating easy disposal, thus maintaining cleanliness and erasability.

JP2024152653APending Publication Date: 2024-10-25PENTEL KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024060536
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-04
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Conventional eraser compositions face issues with eraser waste scattering and the need for manual collection due to the separation of eraser debris from the eraser surface during use, especially in environments like dining tables where cleanliness is crucial.

Method used

An eraser composition comprising vinyl chloride-vinyl acetate copolymer, cyclohexane-1,2-dicarboxylic acid ester, and a stabilizer, with specific polymerization and vinyl acetate content ranges, ensuring that eraser debris remains connected to the eraser surface, allowing easy removal without scattering.

Benefits of technology

The composition effectively keeps eraser debris attached to the eraser surface, facilitating easy disposal and maintaining cleanliness by preventing scattering, while maintaining erasability and hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152653000001
    Figure 2024152653000001
Patent Text Reader

Abstract

To provide an eraser in which eraser shavings stick to an eraser body and do not come off, the stuck eraser shavings can be easily removed by hand, and the eraser shavings do not remain on the surface of the eraser or on paper, but can be easily picked up and discarded, allowing a desk to be used clean.SOLUTION: The present invention includes at least a vinyl chloride-vinyl acetate copolymer, a cyclohexane-1,2-dicarboxylic acid ester, a filler, and a stabilizer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an eraser for erasing handwriting of a pencil, mechanical pencil, etc., and more specifically to an eraser composition which has appropriate hardness and erasability, and eraser dust does not come off the eraser body, and when discarding the eraser dust, the eraser dust stuck to the body can be easily removed by pinching it with fingers. [Background technology]

[0002] Conventionally, eraser compositions that use polyvinyl chloride, vinyl chloride copolymers, natural rubber, synthetic rubber, thermoplastic elastomers, etc. as a base resin are known. Eraser compositions that use polyvinyl chloride as a base resin are widely used due to their excellent erasability.

[0003] The writing of a pencil or mechanical pencil is the powder of the lead of the pencil or mechanical pencil worn by rubbing against the paper and adhering to the paper surface. This worn powder of the lead is removed from the paper surface by adhering to the eraser surface or the eraser dust surface, and the writing is erased. For this reason, in the conventional eraser composition, the worn powder of the lead on the paper surface is adhered to the eraser surface, and the eraser surface to which the worn powder is attached is discharged as eraser dust by surface wear due to friction, and a new eraser surface is exposed. It is necessary to repeat this cycle, and the eraser dust discharged needs to be collected from the paper surface or desk and discarded.

[0004] When eraser dust scatters into small pieces, it becomes difficult to collect and dispose of it, so in the examples of JP 2010-167717 A (Patent Document 1), a manufacturing method is described that improves the cohesiveness of eraser dust and makes it easier to collect by stirring or kneading an eraser composition containing vinyl chloride resin, a cyclohexane-1,2-dicarboxylic acid ester, and calcium carbonate as a filler at a temperature of 60°C or higher but lower than 150°C, and then molding the eraser composition.

[0005] The examples of JP 2014-54812 A (Patent Document 2) describe an eraser composition that contains vinyl chloride resin, adipic acid-based polyester, a liquid acrylic polymer with a glass transition point (Tg) of 0°C or less, calcium carbonate as a filler, and a mixture of calcium and zinc stearate as a stabilizer, and thus has excellent erasability, ease of eraser dust collection, and excellent plasticizer migration properties. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2010-167717 A [Patent Document 2] JP 2014-54812 A Summary of the Invention [Problem to be solved by the invention]

[0007] Patent Document 1 describes that the eraser dust can be made more cohesive by mixing and heating a cyclohexane-1,2-dicarboxylic acid ester as a plasticizer, and then molding it. Patent Document 2 describes that the eraser dust can be made more cohesive by using an adipic acid polyester as a plasticizer in combination with a liquid acrylic polymer with a glass transition point (Tg) of 0°C or less. Although both methods improve the cohesiveness of the eraser dust, the eraser dust still separates from the eraser surface as the handwriting is erased, and even if the eraser dust is less likely to scatter, it still remains necessary to collect the eraser dust on the paper or desk, recover it, and dispose of it.

[0008] Furthermore, studying in the living room has been gaining attention in recent years, and because studying takes place at the dining table, there is a demand for erasers that are easy to clean, especially before meals, and that do not leave eraser shavings scattered around for hygienic reasons.

[0009] The present invention aims to provide an eraser composition that is generated by combining new and old eraser shavings while part of the eraser shavings generated during the erasing of handwriting always remains connected to the eraser surface. This eraser composition eventually combines into one piece, and the eraser shavings attached to the eraser body do not tear off halfway, so that the eraser shavings can be easily removed from the eraser surface in one go by pinching them with your hand, and the eraser shavings can be easily discarded without scattering on the paper or desk, allowing you to keep your desk clean. [Means for solving the problem]

[0010] The first gist of the present invention is an eraser composition containing at least a vinyl chloride-vinyl acetate copolymer, a cyclohexane-1,2-dicarboxylic acid ester, a filler, and a stabilizer, and the second gist of the present invention is an eraser composition characterized in that the vinyl chloride-vinyl acetate copolymer has an average degree of polymerization of 1000 or more and 2000 or less, and the vinyl acetate content is 3% by weight or more and 8% by weight or less. Effect of the Invention

[0011] The vinyl chloride-vinyl acetate copolymer is mixed with a plasticizer that softens the vinyl chloride-vinyl acetate copolymer to prepare a paste, and then heated to make the vinyl chloride-vinyl acetate copolymer absorb the plasticizer and lose fluidity, i.e., to obtain an eraser composition. Since the vinyl chloride-vinyl acetate copolymer has an ester group, the plasticizer penetrates the vinyl acetate portion more easily than polyvinyl chloride. Therefore, the vinyl acetate portion in the vinyl chloride-vinyl acetate copolymer gels and its strength increases, so that the vinyl chloride-vinyl acetate copolymer is less likely to be partially broken apart when the eraser composition is worn down, compared to polyvinyl chloride. As a result, a part of the eraser dust generated by the wear of the eraser composition during erasing has the ability to connect to the eraser surface and not separate, so that when erasing is continued and the eraser composition is worn down, the part of the eraser dust that was connected to the eraser body also separates from the eraser surface due to friction. However, the newly generated eraser dust remains connected to the eraser surface, and by twisting and merging with the previous eraser dust, the eraser dust always has a new part that connects to the eraser surface, so that the eraser dust is not discharged when it reaches an appropriate size, as in the case of conventional erasers. However, friction can expose new eraser surface, so the production of eraser dust itself is not inhibited and erasing can continue.

[0012] Furthermore, the plasticizer cyclohexane-1,2-dicarboxylic acid ester is composed of an ester group that electrically adsorbs to the polarized bond of vinyl chloride-vinyl acetate copolymer, and a naphthene ring and an alkyl group that expand the molecular spacing of the polarized bond. The naphthene ring gives it a stronger ability to expand the molecular spacing of the polarized bond of vinyl chloride-vinyl acetate copolymer compared to other plasticizers such as phthalic acid esters, making it easier to break the vinyl chloride part of vinyl chloride-vinyl acetate copolymer. This makes it possible to make the strength of the connected part of the eraser body and eraser shavings connected by the vinyl acetate part smaller than the strength of the eraser shavings that have been united, making it easy to remove with a single finger pick. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Vinyl chloride-vinyl acetate copolymer is the resin base material of the eraser composition. Specifically, Solbin A (average polymerization degree 420, vinyl acetate content 3% by weight), Solbin AL (300, 2% by weight), Solbin C (420, 13% by weight), Solbin C5R (350, 21% by weight), Solbin CH (650, 14% by weight), Solbin CL (300, 14% by weight), Solbin CN (750, 11% by weight), Solbin CNL (200, 10% by weight), Solbin M5 (430, 14% by weight), TA3 (350, 4% by weight), TA5R (300, 1% by weight), TAO (360, 2% by weight), (all manufactured by Shin-Etsu Chemical Co., Ltd.), Ryuron Paste K650 (1,000, 4% by weight), Ryuron Paste 750 (1,250, 5% by weight), Ryuron Paste 751 (1,300, 5% by weight), Ryuron Paste 850 (1,600, 5% by weight), Ryuron Paste 9 52 (1,800, 7% by weight) (all manufactured by Tosoh Corporation), PCH-175 (1,650, 5% by weight), 843 (1,800, 8% by weight), 12 (1,550, 5% by weight), 72 (1,800, 8% by weight), PBM-6 (900, 3% by weight), Kanevinyl M1008 (780, 5% by weight), MA1008 (720, 7% by weight), %), MB1008 (same as above, 680% by weight), HM515 (same as above, 17% by weight), HM317 (same as above, 370% by weight), T555 (same as above, 15% by weight), T5HX (same as above, 480% by weight), T518A (same as above, 18% by weight), T428A (same as above, 370% by weight) (all manufactured by Kaneka Corporation). From the viewpoint of erasability, the average polymerization degree of the vinyl chloride-vinyl acetate copolymer is 1,000 or more, more preferably 1,300 or more, and even more preferably 1,500 or more. When the average polymerization degree is 1,000 or more, the hardness and elasticity of the resulting eraser composition are sufficient, and sufficient erasability is obtained. Furthermore, the average polymerization degree of the vinyl chloride-vinyl acetate copolymer is 3,000 or less, more preferably 2,500 or less, and even more preferably 2,000 or less. When the average polymerization degree is 3,000 or less, the resulting eraser composition is sufficiently worn and eraser dust is generated, and sufficient erasability is obtained. Furthermore, from the viewpoint of eraser dust adhesion, the vinyl acetate content in the vinyl chloride-vinyl acetate copolymer is 3% by weight or more, more preferably 4% by weight or more, and even more preferably 5% by weight or more. When the vinyl acetate content in the vinyl chloride-vinyl acetate copolymer is 3% by weight or more, the plasticizer is easily permeated into the vinyl chloride-vinyl acetate copolymer, and the resulting eraser composition has good eraser dust adhesion. On the other hand, from the viewpoint of erasability, the vinyl acetate content in the vinyl chloride-vinyl acetate copolymer is 8% by weight or less, more preferably 7% by weight or less, and even more preferably 6% by weight or less. When the vinyl acetate content in the vinyl chloride-vinyl acetate copolymer is 8% by weight or less, the vinyl chloride moieties in the vinyl chloride-vinyl acetate copolymer form more bonds due to polarization, so that the resulting eraser composition has sufficient hardness and elasticity, and does not deform significantly when the eraser composition is pressed against the surface of paper and rubbed, providing sufficient erasability. Specific examples of such preferred vinyl chloride-vinyl acetate copolymers include Ryuron Paste K650, Ryuron Paste K750, Ryuron Paste K751, Ryuron Paste K850, Ryuron Paste K952, Ryuron Paste KCH-175, Ryuron Paste K843, Ryuron Paste K12, Ryuron Paste K72, and the like. The amount of the vinyl chloride-vinyl acetate copolymer used is 6% by weight or more and 45% by weight or less, preferably 8% by weight or more and 40% by weight or less, more preferably 10% by weight or more and 35% by weight or less, based on the total amount of the eraser composition. The vinyl chloride-vinyl acetate copolymer may be used alone or in combination of two or more kinds. As the vinyl chloride-vinyl acetate copolymer, a paste resin is preferred because it is easy to mix with a plasticizer and to process.

[0014] The resin substrate of the present invention can use a vinyl chloride resin in addition to the vinyl chloride-vinyl acetate copolymer within a range that does not impair the effects of the present invention, such as vinyl chloride resin, chlorinated vinyl chloride resin, vinyl chloride-ethylene copolymer, vinyl chloride-ethylene-vinyl acetate copolymer, vinyl chloride-methyl acrylate copolymer, vinyl chloride-methyl methacrylate copolymer, and vinyl chloride-octyl acrylate copolymer. The content of the vinyl chloride resin used in addition to the vinyl chloride-vinyl acetate copolymer is preferably vinyl chloride-vinyl acetate copolymer:vinyl chloride resin=1:0.70 or less, more preferably 1:0.25 or less, in terms of eraser adhesion, and more preferably an extremely small amount or no vinyl chloride resin is added. The vinyl chloride resins used in addition to the vinyl chloride-vinyl acetate copolymer are specifically polyvinyl chloride, such as TK-500, 600, 700, 800, 1000, 1300, 1400, 1700E, 2000E, 2500LS, 2500HS, 2500PE, GR-800T, 1300, 1300S, 2500S, Vinyblan 271, and 2500E. 78, 690, 902, 900, 603, 985, 700, 701, 715H (all manufactured by Shin-Etsu Chemical Co., Ltd.), TH-500, 640, 700, 800, 1000, 1300, 1400, 1700, 2000, 2500, 2800, 3000, 3800, TU-300, 400 (all manufactured by Taiyo PVC Co., Ltd.), ZEST700L, 700Z, 700G, 800Y, 800Z, 1000H, 1000Z, 1000S, 1300Z, 1300SI, 1400Z, 1700ZI, 2000Z, 2500Z, PQB83, PQLT, PQ92, P22, PQ130, PQ137, P21, PQHT, PQHH, PN900 (all made by Shin-Daiichi PVC), S-400 , S1006, S1007, S1008, S1001, S1001N, S1003, S1003N, S1004, KS-1700, 2500, 3000, PSH-180, 161 , 261, 247, 985, 945, 947, PSM-154, 162, PSM-176, PSL-180, 675, 685, PSH-10, 31, 24, 90,PSM-30, PSM-31, PSM-271R, PSL-31, PSM-275, PSM-290R, PBM-B5F, PS-300K, XPS-300L (all manufactured by Kaneka Corporation), T70A, K72Z, K75Z, 200, T80A, K80, K94Z, T10Z, 732, 310, K615, 616, 630, K640, K670, 800, 860, 810, 772, 815A, 762, 761, 960 (all manufactured by Tosoh Corporation), vinyl chloride-ethylene copolymers TE-650, TE-800, TE-1050, TE-1300, TE-1700, TE-2200, TE-2400, TE-2600, TE-2800, TE-2900, TE-3000, TE-3100, TE-3200, TE-3300, TE-3400, TE-3500, TE-3600, TE-3700, TE-3800, TE-3900, TE-4000, TE-4100, TE-4200, TE-4300, TE-4400, TE-4500, TE-4600, TE-4700, TE-4800, TE-49 ... 2800 (all manufactured by Taiyo PVC Co., Ltd.), vinyl chloride-ethylene-vinyl acetate copolymers such as TG-110, TG-120, TG-130, and TG-40 (all manufactured by Sekisui Chemical Co., Ltd.), chlorinated polyvinyl chloride resins such as H305, H536, H547, H516, H527, H727, H716S, and H829 (all manufactured by Kaneka Corporation), HA-05K, HA-15E, HA-15F, HA-15H, HA-17F, HA-27F, HA-25H, HA-24KL, HA-28K, HA-27L, HA-35F, HA-31K, HA-53K, and HA-58K (all manufactured by Sekisui Chemical Co., Ltd.), and the like.

[0015] Cyclohexane-1,2-dicarboxylic acid ester is essential as a plasticizer. The amount of this cyclohexane-1,2-dicarboxylic acid ester is preferably in a weight ratio of vinyl chloride-vinyl acetate copolymer:cyclohexane-1,2-dicarboxylic acid ester=1:1.30 or more and 1.60 or less in order to obtain an eraser composition with good erasability. By making the amount of cyclohexane-1,2-dicarboxylic acid ester in a weight ratio of vinyl chloride-vinyl acetate copolymer:cyclohexane-1,2-dicarboxylic acid ester=1:1.30 or more, the vinyl chloride-vinyl acetate copolymer that has absorbed the cyclohexane-1,2-dicarboxylic acid ester has adhesiveness and elasticity, so that the surface of the obtained eraser can be easily adhered to handwriting such as graphite, resulting in sufficient erasability, and also in eraser dust adhesion. By setting the amount of cyclohexane-1,2-dicarboxylic acid ester to a weight ratio of vinyl chloride-vinyl acetate copolymer:cyclohexane-1,2-dicarboxylic acid ester = 1:1.60 or less, the cyclohexane-1,2-dicarboxylic acid ester can be sufficiently absorbed into the vinyl chloride-vinyl acetate copolymer, and the bleeding phenomenon in which the cyclohexane-1,2-dicarboxylic acid ester seeps out onto the surface of the resulting eraser does not occur, erasing can be performed without soiling the paper surface during erasing, and good eraser waste disposal can be obtained. The amount used is 10% by weight or more and 70% by weight or less, preferably 20% by weight or more and 70% by weight or less, and more preferably 20% by weight or more and 60% by weight or less, based on the total amount of the eraser composition. Specific examples of cyclohexane-1,2-dicarboxylic acid esters include cyclohexane-1,2-dicarboxylic acid diisopentyl ester, cyclohexane-1,2-dicarboxylic acid diisoheptyl ester, cyclohexane-1,2-dicarboxylic acid diisononyl ester, cyclohexane-1,2-dicarboxylic acid dinonyl ester, cyclohexane-1,2-dicarboxylic acid diisodecyl ester, cyclohexane-1,2-dicarboxylic acid di(C7-11) alkyl ester, cyclohexane-1,2-dicarboxylic acid di(C9-11) alkyl ester, cyclohexane-1,2-dicarboxylic acid di(C7-9) alkyl ester, and cyclohexane-1,2-dicarboxylic acid di(C8-13) alkyl ester. The above cyclohexane-1,2-dicarboxylic acid esters may be used alone or in combination of two or more.

[0016] The plasticizer of the present invention can be used in combination with a plasticizer other than cyclohexane-1,2-dicarboxylic acid ester that is used in conventional erasers, in addition to the cyclohexane-1,2-dicarboxylic acid ester, within a range that does not impair the effects of the present invention, and from the viewpoint of eraser dust disposal, the content of the plasticizer other than cyclohexane-1,2-dicarboxylic acid ester is preferably cyclohexane-1,2-dicarboxylic acid ester:other plasticizer=1:0.50 or less, more preferably 1:0.25 or less, in terms of the weight ratio. Among these, from the viewpoint of the eraser dust disposal of the obtained eraser composition, it is preferable to add an extremely small amount of the plasticizer to be used in combination with the cyclohexane-1,2-dicarboxylic acid ester, or to add no plasticizer at all. Specifically, phthalate esters include dimethyl phthalate, diethyl phthalate, dibutyl phthalate, di-2-ethylhexyl phthalate, diisononyl phthalate, diisodecyl phthalate, ditridecyl phthalate, butyl benzyl phthalate, dioctyl phthalate, dinonyl phthalate, and diundecyl phthalate, and benzoate ester plasticizers include diethylene glycol dibenzoate, triethylene glycol dibenzoate, polyethylene glycol dibenzoate, propylene glycol dibenzoate, dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, 1,3-butanediol dibenzoate, 1,4-butanediol dibenzoate, 1,6-hexanediol dibenzoate, 3-methyl-1,5-pentanediol dibenzoate, 1,8-octanediol dibenzoate, and 1,9-octanediol dibenzoate. Examples of the plasticizers include butanediol dibenzoate esters, adipic acid plasticizers include di-2-ethylhexyl adipate, diisononyl adipate, and diisodecyl adipate, citric acid plasticizers include triethyl acetyl citrate and tributyl acetyl citrate, trimellitic acid plasticizers include trialkyl trimellitate and tris-2-ethylhexyl trimellitate, ricinoleic acid plasticizers include methyl acetyl ricinoleate and butyl acetyl ricinoleate, and epoxy plasticizers include epoxidized fatty acid octyl esters, epoxidized fatty acid monoesters, epoxidized linseed oil, epoxidized hexahydrophthalate di-2-ethylhexyl, 4,5-epoxy-1,2-cyclohexanedicarboxylate bis(2-ethylhexyl), and alkylsulfonic acid phenyl ester plasticizers.

[0017] The filler may be any filler that has been used in erasers in the past, such as calcium carbonate, silica, diatomaceous earth, kaolin, clay, zinc oxide, magnesium oxide, magnesium carbonate, magnesium hydroxide, etc. In order to obtain an eraser composition with good erasability, the amount of the filler is set to a weight ratio of vinyl chloride-vinyl acetate copolymer:filler=1:0.6 or more, so that the eraser composition obtained is not too soft, and does not deform too much when pressed against a paper surface and rubbed, so that sufficient erasability is obtained, and sufficient wear resistance is obtained, so that eraser dust disposal is possible. By setting the weight ratio of vinyl chloride-vinyl acetate copolymer:filler=1:1.0 or less, the eraser composition obtained is not too hard, and the elasticity of the eraser composition obtained is sufficient, so that sufficient erasability is obtained. In addition, sufficient eraser dust adhesion is obtained. The amount used is 5% by weight or more and 50% by weight or less, preferably 10% by weight or more and 40% by weight or less, and more preferably 20% by weight or more and 30% by weight or less, based on the total amount of the eraser composition. Specifically, calcium carbonate includes Softon 3200, Softon 2600, Softon 2200, Softon 1800, Softon 1500, Softon 1200, Softon 1000, BF100, BF200, BF300, BF400 (all manufactured by Bihoku Funka Kogyo Co., Ltd.), Super S, Super SS, Super SSS, Super 4S, Super #1500, Super #1700, Super #2000, Super #2300, Special Rice S, Nanox #25, Nanox #30, Caltex 5-7, MC Coat S-10-23, MC Coat P-10-23, Snow Light S-#1500, Nano Coat S-25-3 0, M White, M-300J (all manufactured by Maruo Calcium Co., Ltd.), MSK-P, PO, Calfine 200, 200M, 500, 20S, M-350, N-40, Carlex 100, 300, N-2, MC-K, CUBE-18HS, 50KAS, 80KAS, Whiscal, (all manufactured by Maruo Calcium Co., Ltd.), Hakuenka PZ, CC, CC-R, U, A, AA, O, DD, T-DD, Calmos, Brilliant-15, 1500, Tsunex-E, PC,Viscolite-700, Viscolite X-850, Vigot-10, Viscolite 15, Viscolite-SV, Viscoexcle-30, Silver W, Homocal D, Viscoexcle DM, Gelton 50, Whiten P-10, 30, 50, 70, Whiten H (all manufactured by Shiraishi Kogyo Co., Ltd.), Sunlight SL-100, SL-300, SL-700, SL-1000, SL-1500, SL-2200, White Series WS-K, WS-KK, WS-3K, WS-810, W S-2200 (all manufactured by Takehara Chemical Industry Co., Ltd.), HTO-12, 10, 8, 6, KP-700, 300, 200 (all manufactured by Hitachi Crushed Stone Co., Ltd.), as silica, Toxil U, Toxil UR, Toxil GU-N, Toxil NR, Toxil PR, Toxil USA, Toxil GU, Toxil NP, Toxil NPS, Toxil 315, Toxil 233, Toxil 255, Toxil 255DL, Toxil 233G, Toxil 255G, Toxil 195G, Toxil 200G, Toxil USG-T, Toxil 315EG, Toxil 255EG, Toxil 923, Toxil 928, Toxil 532, Toxil 732, as fine silica, Oriental Silica Corporation's NipSeal X-12, X-35, X-37, X-37B, X-30, X-40, X-45, X-60, B, E-50, T-32, US-F, OSCC132, C136, C152, C158, 927, UC116, UC800, DT267, DA95, BM224, BM225, T610 (all manufactured by Oriental Silica Corporation), NipSeal AQ, VN3, LP, L-300, ER, RS-150, Examples of the fillers include NS, NA, KQ, EL, K-500, G-300, N-300A, SP-200, and TB-5012 (all manufactured by Tosoh Silica Corporation), Carplex #80, #67, #101, #1120, #XR, Carplex #FPS-1, #2, #101, #101M, #500, Carplex CS-5, #7, #8, Carplex BS-308N, #510BX, #303, and #306 (all manufactured by EVONIK). The above fillers may be used alone or in combination of two or more.

[0018] In the present invention, it is preferable to use calcium carbonate and silica in combination from the viewpoint of erasability, and the amount of silica is calcium carbonate:silica=1:0.03 or more and 0.14 or less in weight ratio, preferably calcium carbonate:silica=1:0.05 or more and 0.11 or less, more preferably calcium carbonate:silica=1:0.06 or more and 0.09 or less. When the amount of silica is calcium carbonate:silica=1:0.03 or more in weight ratio, the obtained eraser composition has sufficient hardness and does not deform too much when pressed against a paper surface and rubbed, so that sufficient erasability is obtained. When the amount of silica is calcium carbonate:silica=1:0.14 or less in weight ratio, the obtained eraser composition does not become too hard and is sufficiently worn when pressed against a paper surface and rubbed, so that sufficient erasability is obtained, and the amount of filler added is not significantly increased, so that eraser dust adhesion is obtained.

[0019] Stabilizers that can be used are those used for polyvinyl chloride, plastic products, etc. Examples of heat stabilizers for polyvinyl chloride include metal soaps of barium, zinc, calcium, etc., and stearic acid, lauric acid, ricinoleic acid, naphthenic acid, 2-ethylhexanoic acid, etc., as metal soap-based stabilizers, and as composite stabilizers that combine metal soap-based stabilizers and stabilizing assistants, there are barium-zinc composite stabilizers and calcium-zinc composite stabilizers, and as organotin-based stabilizers, there are non-toxic dioctyltin compounds, and epoxy-based plasticizers also have a heat stabilizing effect. Epoxidized soybean oil, which is liquid at a molding temperature of 120°C to 140°C, is well dispersed and is preferred as a heat stabilizer.

[0020] The coloring material can be used to give the eraser composition a desired color. Coloring agents that have been conventionally used in polyvinyl chloride, thermoplastic elastomers, rubber, plastics, etc. can be used, and conventionally known inorganic pigments such as titanium oxide and carbon black, organic pigments such as azo, phthalocyanine, threne, dioxazine, isoindoline, and lake pigments, dyes, and special pigments such as colored resin particles and fluorescent pigments can be used.

[0021] The eraser composition of this embodiment can be manufactured by a conventionally known method. For example, the raw material composition obtained by blending the above-mentioned components in a predetermined amount is mixed and stirred, defoamed to prepare a paste, and then heated and molded into a predetermined shape and cooled to obtain the eraser composition. The paste can be defoamed after mixing and stirring, or can be simultaneously defoamed by mixing and stirring under reduced pressure. The paste can be prepared from 5°C or higher, and is preferably prepared at 25°C to 40°C. For the heat molding, a conventionally known method can be selected depending on the desired shape. For example, the defoamed paste can be poured into a mold and the mold is heated to mold, or the paste can be placed in an extrusion molding machine or an injection molding machine and heated and molded to prepare the eraser composition. The eraser composition can be molded at a temperature of 120°C to 140°C, and preferably 125°C to 135°C. EXAMPLES

[0022] Examples and comparative examples are shown below, but are not intended to limit the present invention in any way.

[0023] Example 1 Ryuron Paste 850 (vinyl chloride-vinyl acetate copolymer, average degree of polymerization 1600, vinyl acetate content 5% by weight, manufactured by Tosoh Corporation) 28.8 parts by weight Hexamol DINCH (cyclohexane-1,2-diisononyl ester, manufactured by BASF) 41.0 parts by weight HTO-10 (calcium carbonate) 27.3 parts by weight Epoxidized soybean oil (stabilizer) 2.9 parts by weight The above ingredients were mixed in a mixer and degassed under reduced pressure to produce a paste. The paste was poured into a mold capable of forming a shape of 44 mm in length, 17 mm in width, and 12 mm in height, and heated at 130°C for 30 minutes to obtain an eraser.

[0024] Example 2 PCH-175 (vinyl chloride-vinyl acetate copolymer, average degree of polymerization 1650, vinyl acetate content 5% by weight, manufactured by Kaneka Corporation) 28.8 parts by weight Hexamol DINCH (cyclohexane-1,2-diisononyl ester, manufactured by BASF) 41.0 parts by weight HTO-10 (calcium carbonate) 27.3 parts by weight Epoxidized soybean oil (stabilizer) 2.9 parts by weight The above components were used in the same manner as in Example 1 to obtain an eraser.

[0025] Example 3 Ryuron Paste 850 (vinyl chloride-vinyl acetate copolymer, average degree of polymerization 1600, vinyl acetate content 5% by weight, manufactured by Tosoh Corporation) 28.8 parts by weight Hexamol DINCH (cyclohexane-1,2-diisononyl ester, manufactured by BASF) 41.0 parts by weight HTO-10 (calcium carbonate) 26.0 parts by weight Toxil U (silica) 1.3 parts by weight Epoxidized soybean oil (stabilizer) 2.9 parts by weight The above components were used in the same manner as in Example 1 to obtain an eraser.

[0026] Example 4 Ryuron Paste 850 (vinyl chloride-vinyl acetate copolymer, average degree of polymerization 1600, vinyl acetate content 5% by weight, manufactured by Tosoh Corporation) 28.5 parts by weight Hexamol DINCH (cyclohexane-1,2-diisononyl ester, manufactured by BASF) 41.0 parts by weight HTO-10 (calcium carbonate) 26.0 parts by weight Toxil U (silica) 1.6 parts by weight Epoxidized soybean oil (stabilizer) 2.9 parts by weight The above components were used in the same manner as in Example 1 to obtain an eraser.

[0027] Example 5 PBM-6 (vinyl chloride-vinyl acetate copolymer, average degree of polymerization 900, vinyl acetate content 3% by weight, Kaneka Corporation) 31.5 parts by weight Hexamol DINCH (cyclohexane-1,2-diisononyl ester, manufactured by BASF) 41.0 parts by weight Softon 1000 (calcium carbonate, manufactured by Bihoku Funka Kogyo Co., Ltd.) 22.5 parts by weight Nipsil LP (silica) 2.0 parts by weight Epoxidized soybean oil (stabilizer) 3.0 parts by weight The above components were used in the same manner as in Example 1 to obtain an eraser.

[0028] Example 6 Solvin CN (vinyl chloride-vinyl acetate copolymer, average degree of polymerization 750, vinyl acetate content 11% by weight, manufactured by Shin-Etsu Chemical Co., Ltd.) 28.0 parts by weight Hexamol DINCH (cyclohexane-1,2-diisononyl ester, manufactured by BASF) 37.0 parts by weight Softon 1000 (calcium carbonate, manufactured by Bihoku Funka Kogyo Co., Ltd.) 32.0 parts by weight Epoxidized soybean oil (stabilizer) 3.0 parts by weight The above components were used in the same manner as in Example 1 to obtain an eraser.

[0029] Comparative Example 1 ZEST P21 (polyvinyl chloride, average degree of polymerization 1550, manufactured by Shin-Daiichi Vinyl Co., Ltd.) 28.8 parts by weight Hexamol DINCH (cyclohexane-1,2-diisononyl ester, manufactured by BASF) 41.0 parts by weight HTO-10 (calcium carbonate, manufactured by Shiraishi Kogyo Co., Ltd.) 27.3 parts by weight Epoxidized soybean oil (stabilizer) 2.9 parts by weight The heating temperature in Example 1 was changed from 130° C. to 140° C. The rest of the procedure was the same as in Example 1 to obtain an eraser.

[0030] Comparative Example 2 Ryuron Paste 850 (vinyl chloride-vinyl acetate copolymer, average degree of polymerization 1600, vinyl acetate content 5% by weight, manufactured by Tosoh Corporation) 28.8 parts by weight Di-2-ethylhexyl phthalate 41.0 parts by weight HTO-10 (calcium carbonate, manufactured by Shiraishi Kogyo Co., Ltd.) 27.3 parts by weight Epoxidized soybean oil (stabilizer) 2.9 parts by weight The heating temperature was changed from 130° C. in Example 1 to 120° C. The rest of the procedure was the same as in Example 1 to obtain an eraser.

[0031] The erasers obtained in the above Examples 1 to 6 and Comparative Examples 1 and 2 were subjected to confirmation tests regarding erasability, eraser dust adhesion, and eraser dust disposal properties.

[0032] Erasure rate: The erasure rate was measured according to the test method for JIS S6050 (2002) "Plastic Eraser" 6.4 Erasability (Erasure Rate). If the erasure rate is 80% or more, it can be used without any problems in practice, if it is 85% or more, it is considered to have good erasability, and if it is 90% or more, it is very good erasability.

[0033] Eraser Dust Adhesion According to the erasability test of JIS S6050 (Plastic Eraser), the test piece was run back and forth 50 times. In other words, the test piece was made by cutting the sample into a 5 mm thick plate and finishing the contact part with the test paper into a circular arc with a radius of 6 mm. The test piece was then placed in contact with the paper perpendicularly, a weight was placed on the test piece so that the sum of the weight and the holder's mass was 0.5 kg, and the test piece was run back and forth 50 times at a speed of 150 ± 10 cm / min to erase it. After 50 runs, the test piece was lifted by hand and removed from the test paper, and it was confirmed whether eraser dust was attached to the test piece. The eraser dust adhesion was evaluated according to the following criteria. ○: Eraser dust is stuck to the test piece. ×: Eraser dust is discharged without adhering to the test piece.

[0034] Eraser dust disposal After the eraser dust adhesion test, the edge of the eraser dust stuck to the test piece was pinched with fingers and the eraser dust was removed from the test piece. At this time, it was visually confirmed whether the eraser dust was completely removed from the test piece. The eraser dust disposal was evaluated according to the following criteria. ◯: Eraser dust could be completely removed from the test piece. Δ: The eraser dust was slightly difficult to peel off from the test piece, but no eraser dust remained. ×: The eraser chip broke off midway and the eraser chip remained on the test piece.

[0035] [Table 1]

[0036] In Examples 1 to 6, when characters are erased, the eraser dust sticks to the eraser body and does not come off, and the stuck eraser dust can be easily removed by hand. Among them, Examples 1 to 4 are excellent in terms of the erasability of characters, the adhesion of eraser dust, and the ease of disposal of eraser dust. Comparative Example 1 is formulated to improve the cohesiveness of eraser dust, but because vinyl chloride-vinyl acetate copolymer is not used, some of the eraser dust generated in a bundle does not connect to the eraser body, and the eraser dust is discharged without adhering to the eraser body. Comparative Example 2 uses di-2-ethylhexyl phthalate instead of cyclohexane-1,2-dicarboxylic acid ester, so the eraser dust sticks to the eraser body, but cannot be removed by picking it up in a bundle, and the eraser dust breaks off midway, making it difficult to dispose of.

Claims

1. The eraser composition comprises at least a vinyl chloride-vinyl acetate copolymer, a cyclohexane-1,2-dicarboxylic acid ester, a filler, and a stabilizer.

2. 2. The eraser composition according to claim 1, wherein the vinyl chloride-vinyl acetate copolymer has an average degree of polymerization of 1,000 to 2,000 and a vinyl acetate content of 3% by weight to 8% by weight.

Citation Information

Patent Citations

  • Manufacturing method of eraser

    JP2010167717A

  • Eraser

    JP2014054812A