Adhesive composition, adhesive film and surface protective film
The adhesive composition addresses the challenge of balancing pot life and crosslinking rate by using specific monomers and catalysts, ensuring stable adhesive strength for surface protection films without organotin compounds, suitable for polarizing plates and precision electrical/electronic components.
Patent Information
- Application Number
- JP2024129787
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2034-07-03
AI Technical Summary
Existing adhesive compositions for optical applications face challenges in achieving a balance of long pot life and high crosslinking rate without using harmful organotin compounds, particularly in the context of surface protection films for polarizing plates and precision electrical/electronic components.
A pressure-sensitive adhesive composition comprising (meth)acrylic acid ester monomers with C4 to C18 alkyl groups, hydroxyl group-containing monomers, difunctional or higher-functional isocyanate compounds, metal chelate crosslinking catalysts, and ketoenol tautomers, with specific weight ratios and components to inhibit premature crosslinking and extend pot life.
The adhesive composition achieves a long pot life and high crosslinking rate, ensuring stable adhesive strength at varying peeling speeds without using organotin compounds, suitable for surface protection films on polarizing plates and precision electrical/electronic components.
Smart Images

Figure 2024152759000001 
Figure 2024152759000002 
Figure 2024152759000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition and a surface protective film. More specifically, the present invention relates to a pressure-sensitive adhesive composition and a surface protective film that have a long pot life and a fast crosslinking rate without using an organotin compound by using a crosslinking catalyst of a metal chelate compound other than an organotin compound, while the use of organotin compounds is restricted due to recent environmental concerns. [Background technology]
[0002] For optical adhesives, acrylic adhesives made of copolymers of alkyl (meth)acrylate as the main component and acrylic monomers having hydroxyl groups, carboxyl groups, etc. as functional groups are preferably used because of their excellent transparency. Furthermore, adhesives with various physical properties such as adhesive strength are required to be appropriately adjusted. In particular, adhesives for surface protection films are required to have an excellent balance of adhesive strength at low and high peeling speeds, which is suitable for laminating surface protection films using an automatic laminating device, so that they can be adapted to the manufacturing process of factory production. Furthermore, adhesives with excellent physical properties such as a long pot life in addition to a good balance of adhesive strength are required.
[0003] Various physical properties of such adhesives are adjusted by adjusting the adhesive strength, cohesive strength, etc., through a crosslinking reaction using an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, etc., which react with functional groups such as hydroxyl groups and carboxyl groups contained in the acrylic adhesive made of a copolymer.
[0004] Conventionally, an isocyanate-based crosslinking agent has been widely used as a crosslinking agent for an acrylic pressure-sensitive adhesive. In addition, in a crosslinking reaction using an isocyanate-based crosslinking agent, a metal chelate is often used as a catalyst for promoting the crosslinking reaction. In general, an organic tin compound such as dibutyltin dilaurate has been used as a catalyst for the crosslinking reaction because of its excellent reaction speed. However, the use of dibutyltin compounds is avoided because they are harmful and toxic. For this reason, there is a demand for a crosslinking catalyst that is inexpensive and has a superior reaction rate in the crosslinking reaction, as an alternative to the dibutyltin compounds used in combination with isocyanate-based crosslinking agents, but it has been difficult to find such a catalyst.
[0005] In this context, Patent Document 1 discloses that, among metal chelates, iron chelates are preferred as crosslinking catalysts to be used in combination with isocyanate-based crosslinking agents, and tris(acetylacetonate)iron is particularly preferred due to its excellent catalytic activity.
[0006] In the case of an acrylic adhesive composition containing a crosslinking catalyst, the crosslinking reaction proceeds gradually even while it is left at room temperature. Therefore, in the industrial production of adhesives, after the raw materials of the adhesive composition are mixed, a crosslinking catalyst and a reaction retarder are generally used in combination to stop the crosslinking reaction until the time when the crosslinking reaction is to be started. Regarding the combined use of this crosslinking catalyst and reaction retarder, Patent Document 2 discloses a method for producing polyurethane, which uses a reactive urethane mixture containing a catalyst system consisting of a mixture of at least one metal acetylacetonate and acetylacetone, in which the weight ratio of the metal acetylacetonate to the acetylacetone is 2:1. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2011-001440 A [Patent Document 2] JP 2008-285681 A Summary of the Invention [Problem to be solved by the invention]
[0008] In the adhesive composition described in Patent Document 1, the amount of metal compound (crosslinking catalyst) added to a copolymer containing (meth)acrylate as a constituent monomer unit and containing a hydroxyl group and a carboxyl group is shown, but there is no description of the amount of crosslinking retarder added. Patent Document 1 also lists methods for suppressing the viscosity increase rate after blending a crosslinking agent into the adhesive composition, such as using a reaction retarder, adding a viscosity increase suppressing solvent, and using a crosslinking agent with a blocked functional group such as blocked isocyanate, but does not provide any specific explanation.
[0009] Furthermore, Patent Document 2 discloses a method for producing polyurethane that utilizes a catalyst system containing a metal acetylacetonate and acetylacetone, which has excellent stability and good catalytic activity and does not cause premature curing even when a metal acetylacetonate catalyst such as iron or copper, which is very active at low temperatures, is used. However, in the method described in Patent Document 2, the weight ratio of metal acetylacetonate to acetylacetone is 2:1, but even when this blending ratio is applied to the manufacturing process of an acrylic adhesive, it is not possible to temporarily suspend the crosslinking reaction.
[0010] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a pressure-sensitive adhesive composition and a surface protection film that have a long pot life and a fast crosslinking rate even without using an organotin compound. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides a pressure-sensitive adhesive composition comprising, relative to 100 parts by weight of (A) at least one (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C4 to C18 and (B) a copolymerizable monomer containing a hydroxyl group as a copolymerizable monomer group, (C) 0.1 to 10 parts by weight of a difunctional or higher isocyanate compound, (D) 0.001 to 0.5 parts by weight of a crosslinking catalyst of a metal chelate compound, and (E) 0.1 to 300 parts by weight of a keto-enol tautomer compound, wherein the weight ratio of (E) / (D) is 70 to 1000.
[0012] It is also preferred that the pressure-sensitive adhesive composition be stored at 23° C. after formulation for 8 hours, and the viscosity of the pressure-sensitive adhesive composition be less than 1.25 times the viscosity immediately after formulation.
[0013] In addition, it is preferable that the (B) hydroxyl group-containing copolymerizable monomer is at least one selected from the group consisting of 8-hydroxyoctyl(meth)acrylate, 6-hydroxyhexyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, and N-hydroxyethyl(meth)acrylamide.
[0014] Among the (C) difunctional or higher isocyanate compounds, the difunctional isocyanate compound is preferably an acyclic aliphatic isocyanate compound produced by reacting a diisocyanate compound with a diol compound. The diisocyanate compound is preferably an aliphatic diisocyanate, and is preferably one selected from the group of compounds consisting of tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and lysine diisocyanate. The diol compound is preferably one selected from the group consisting of 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2-dimethyl-1,3-propanediol monohydroxypivalate, polyethylene glycol, and polypropylene glycol. Furthermore, among the (C) difunctional or higher isocyanate compounds, the trifunctional isocyanate compound is preferably at least one selected from the group consisting of an isocyanurate of a hexamethylene diisocyanate compound, an isocyanurate of an isophorone diisocyanate compound, an adduct of a hexamethylene diisocyanate compound, an adduct of an isophorone diisocyanate compound, a biuret of a hexamethylene diisocyanate compound, a biuret of an isophorone diisocyanate compound, an isocyanurate of a tolylene diisocyanate compound, an isocyanurate of a xylylene diisocyanate compound, an isocyanurate of a hydrogenated xylylene diisocyanate compound, an adduct of a tolylene diisocyanate compound, an adduct of a xylylene diisocyanate compound, and an adduct of a hydrogenated xylylene diisocyanate compound.
[0015] In addition, it is preferable that the pressure-sensitive adhesive composition does not contain an organotin compound as the crosslinking catalyst.
[0016] The copolymer is preferably an acrylic polymer containing at least one of a carboxyl group-containing monomer and a nitrogen-containing vinyl monomer not containing a hydroxyl group as other copolymerizable monomers.
[0017] The pressure-sensitive adhesive composition preferably has a gel fraction after crosslinking of 90 to 100%.
[0018] It is also preferred that the adhesive layer obtained by crosslinking the adhesive composition has an adhesive strength of 0.05 to 0.2 N / 25 mm at a low peel speed of 0.3 m / min, and an adhesive strength of 2.0 N / 25 mm or less at a high peel speed of 30 m / min.
[0019] The present invention also provides a pressure-sensitive adhesive film comprising a resin film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition on one or both sides of the resin film.
[0020] The present invention also provides a surface protection film comprising a resin film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition on one side of the resin film.
[0021] The surface protective film of the present invention can also be used as a surface protective film for a polarizing plate.
[0022] In addition, the surface protection film of the present invention can be used as a surface protection film for any precision electrical / electronic component selected from the group of precision electrical / electronic components consisting of flexible printed wiring boards, rigid printed wiring boards, and transparent conductive films. Effect of the Invention
[0023] According to the present invention, it is possible to provide a pressure-sensitive adhesive composition and a surface protective film which have a long pot life and a fast crosslinking rate even without using an organotin compound. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will be described below based on preferred embodiments. The pressure-sensitive adhesive composition of the present invention is characterized in that it contains, relative to 100 parts by weight of (A) at least one (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C4 to C18 and (B) a copolymerizable monomer containing a hydroxyl group as a copolymerizable monomer group, (C) 0.1 to 10 parts by weight of a difunctional or higher isocyanate compound, (D) 0.001 to 0.5 parts by weight of a crosslinking catalyst of a metal chelate compound, and (E) 0.1 to 300 parts by weight of a keto-enol tautomer compound, and the weight ratio of (E) / (D) is 70 to 1000.
[0025] The copolymer may be an acrylic polymer containing at least one of a carboxyl group-containing monomer and a nitrogen-containing vinyl monomer not containing a hydroxyl group as other copolymerizable monomers.
[0026] (A) Examples of (meth)acrylic acid ester monomers having an alkyl group with a carbon number of 4 to 18 include butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, and undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, myristyl (meth)acrylate, isomyristyl (meth)acrylate, cetyl (meth)acrylate, isocetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and the like. It is preferable that the copolymer contains 50 to 98 parts by weight of (A) a (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C4 to C18, based on 100 parts by weight of the copolymer.
[0027] (B) Examples of copolymerizable monomers containing a hydroxyl group include hydroxyalkyl (meth)acrylates such as 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate, as well as hydroxyl group-containing (meth)acrylamides such as N-hydroxy(meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide. It is preferable that the compound is at least one selected from the group consisting of 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide. It is preferable that the copolymer contains (B) the copolymerizable monomer having a hydroxyl group in a ratio of 0.1 to 10 parts by weight based on 100 parts by weight of the copolymer.
[0028] The copolymer may contain at least one of a carboxyl group-containing monomer, a nitrogen-containing vinyl monomer not containing a hydroxyl group, and a polyalkylene glycol mono(meth)acrylic acid ester monomer as other copolymerizable monomers.
[0029] The carboxyl group-containing monomer is preferably at least one selected from the group consisting of (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl maleic acid, carboxypolycaprolactone mono(meth)acrylate, and 2-(meth)acryloyloxyethyl tetrahydrophthalic acid. When the copolymer contains a carboxyl group-containing monomer as another copolymerizable monomer group, the carboxyl group-containing monomer is preferably contained in an amount of 0.1 to 1.0 part by weight per 100 parts by weight of the copolymer. The copolymer does not necessarily need to contain the carboxyl group-containing monomer.
[0030] The polyalkylene glycol mono(meth)acrylic acid ester monomer may be a compound in which one of the multiple hydroxyl groups of a polyalkylene glycol is esterified as a (meth)acrylic acid ester. The (meth)acrylic acid ester group is a polymerizable group, so it can be copolymerized into the copolymer of the main agent. The other hydroxyl groups may remain as OH, or may be alkyl ethers such as methyl ether and ethyl ether, or saturated carboxylates such as acetate. The alkylene group of the polyalkylene glycol includes, but is not limited to, an ethylene group, a propylene group, a butylene group, etc. The polyalkylene glycol may be a copolymer of two or more polyalkylene glycols such as polyethylene glycol, polypropylene glycol, polybutylene glycol, etc. The copolymer of polyalkylene glycol includes polyethylene glycol-polypropylene glycol, polyethylene glycol-polybutylene glycol, polypropylene glycol-polybutylene glycol, etc., and the copolymer may be a block copolymer or a random copolymer. The polyalkylene glycol mono(meth)acrylic acid ester monomer preferably has an average repeat number of alkylene oxide constituting the polyalkylene glycol chain of 3 to 14. The "average repeat number of alkylene oxide" refers to the average number of repeats of alkylene oxide units in the "polyalkylene glycol chain" portion contained in the molecular structure of the polyalkylene glycol mono(meth)acrylic acid ester monomer.
[0031] The polyalkylene glycol mono(meth)acrylic acid ester monomer is preferably at least one selected from the group consisting of polyalkylene glycol mono(meth)acrylate, methoxypolyalkylene glycol (meth)acrylate, and ethoxypolyalkylene glycol (meth)acrylate. More specifically, polyethylene glycol-mono(meth)acrylate, polypropylene glycol-mono(meth)acrylate, polybutylene glycol-mono(meth)acrylate, polyethylene glycol-polypropylene glycol-mono(meth)acrylate, polyethylene glycol-polybutylene glycol-mono(meth)acrylate, polypropylene glycol-polybutylene glycol-mono(meth)acrylate, polyethylene glycol-polypropylene glycol-polybutylene glycol-mono(meth)acrylate; methoxypolyethylene glycol-(meth)acrylate, methoxypolypropylene glycol-(meth)acrylate, methoxypolybutylene glycol-(meth)acrylate, methoxy-polyethylene glycol-polypropylene glycol-(meth)acrylate, methoxy-polyethylene glycol methoxy-polybutylene glycol-polybutylene glycol-(meth)acrylate, methoxy-polyethylene glycol-polypropylene glycol-polybutylene glycol-(meth)acrylate; ethoxypolyethylene glycol-(meth)acrylate, ethoxypolypropylene glycol-(meth)acrylate, ethoxypolybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polypropylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polypropylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polypropylene glycol-polybutylene glycol-(meth)acrylate, and the like. It is preferable that the polyalkylene glycol mono(meth)acrylic acid ester monomer is contained in a ratio of 0 to 50 parts by weight based on 100 parts by weight of the copolymer. The copolymer does not necessarily need to contain the polyalkylene glycol mono(meth)acrylic acid ester monomer.
[0032] Examples of the nitrogen-containing vinyl monomer that does not contain a hydroxyl group include a vinyl monomer containing an amide bond, a vinyl monomer containing an amino group, and a vinyl monomer having a nitrogen-containing heterocyclic structure. More specifically, examples of the nitrogen-containing vinyl monomer include N-vinyl-substituted heterocyclic structures such as N-vinyl-2-pyrrolidone, N-vinylpyrrolidone, methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, and N-vinyllaurolactam. Cyclic nitrogen-containing vinyl compounds having a heterocyclic structure substituted with N-(meth)acryloyl, such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperazine, N-(meth)acryloylaziridine, N-(meth)acryloylazetidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylpiperidine, N-(meth)acryloylazepane, and N-(meth)acryloylazocane. Cyclic nitrogen-containing vinyl compounds; cyclic nitrogen-containing vinyl compounds having a heterocyclic structure having a nitrogen atom and an ethylenically unsaturated bond in the ring, such as N-cyclohexylmaleimide and N-phenylmaleimide; unsubstituted or monoalkyl-substituted (meth)acrylamides, such as (meth)acrylamide, N-methyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and Nt-butyl(meth)acrylamide; dialkyl-substituted (meth)acrylamides, such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropylacrylamide, N,N-diisopropyl(meth)acrylamide, N,N-dibutyl(meth)acrylamide, N-ethyl-N-methyl(meth)acrylamide, N-methyl-N-propyl(meth)acrylamide, and N-methyl-N-isopropyl(meth)acrylamide;Dialkylamino(meth)acrylates such as N,N-dimethylaminomethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, N,N-dimethylaminopropyl(meth)acrylate, N,N-dimethylaminoisopropyl(meth)acrylate, N,N-dimethylaminobutyl(meth)acrylate, N,N-diethylaminomethyl(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, N-ethyl-N-methylaminoethyl(meth)acrylate, N-methyl-N-propylaminoethyl(meth)acrylate, N-methyl-N-isopropylaminoethyl(meth)acrylate, N,N-dibutylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate; N,N-dimethylaminopropyl(meth)acrylamide, N,N-diethylaminopropyl(meth)acrylamide, N N,N-dialkyl-substituted aminopropyl(meth)acrylamide such as N-dipropylaminopropyl(meth)acrylamide, N,N-diisopropylaminopropyl(meth)acrylamide, N-ethyl-N-methylaminopropyl(meth)acrylamide, N-methyl-N-propylaminopropyl(meth)acrylamide, and N-methyl-N-isopropylaminopropyl(meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinylformamide, N-vinylacetamide, and N-vinyl-N-methylacetamide; (meth)acrylamides such as N-methoxymethyl(meth)acrylamide, N-ethoxyethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, diacetone acrylamide, and N,N-methylenebis(meth)acrylamide; and unsaturated carboxylic acid nitriles such as (meth)acrylonitrile.
[0033] The copolymer preferably contains 0 to 20 parts by weight of the nitrogen-containing vinyl monomer not containing a hydroxyl group relative to 100 parts by weight of the copolymer. The copolymer does not necessarily need to contain the nitrogen-containing vinyl monomer not containing a hydroxyl group.
[0034] (C) The difunctional or higher isocyanate compound may be at least one or more selected from polyisocyanate compounds having at least two isocyanate (NCO) groups in one molecule. Polyisocyanate compounds are classified into aliphatic isocyanates, aromatic isocyanates, acyclic isocyanates, alicyclic isocyanates, etc., and any of them may be used. Specific examples of polyisocyanate compounds include aliphatic isocyanate compounds such as hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and trimethylhexamethylene diisocyanate (TMDI), and aromatic isocyanate compounds such as diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI), hydrogenated xylylene diisocyanate (H6XDI), dimethyldiphenylene diisocyanate (TOID), and tolylene diisocyanate (TDI). Examples of trifunctional or higher isocyanate compounds include biuret modified or isocyanurate modified difunctional isocyanate compounds (compounds having two NCO groups in one molecule), and adducts (polyol modified compounds) with trivalent or higher polyols (compounds having at least three OH groups in one molecule) such as trimethylolpropane (TMP) or glycerin. As the difunctional or higher isocyanate compound (C), it is possible to use only the trifunctional isocyanate compound (C-1) or only the difunctional isocyanate compound (C-2). It is also possible to use the trifunctional isocyanate compound (C-1) and the difunctional isocyanate compound (C-2) in combination.
[0035] Furthermore, the (C-1) trifunctional isocyanate compound used in the present invention is selected from the (C-1-1) first aliphatic isocyanate compound group consisting of an isocyanurate of a hexamethylene diisocyanate compound, an isocyanurate of an isophorone diisocyanate compound, an adduct of a hexamethylene diisocyanate compound, an adduct of an isophorone diisocyanate compound, a biuret of a hexamethylene diisocyanate compound, and a biuret of an isophorone diisocyanate compound. In addition, it is preferable to include at least one or more selected from (C-1-2) a second aromatic isocyanate compound group consisting of an isocyanurate of a tolylene diisocyanate compound, an isocyanurate of a xylylene diisocyanate compound, an isocyanurate of a hydrogenated xylylene diisocyanate compound, an adduct of a tolylene diisocyanate compound, an adduct of a xylylene diisocyanate compound, and an adduct of a hydrogenated xylylene diisocyanate compound. It is preferable to use (C-1-1) the first aliphatic isocyanate compound group and (C-1-2) the second aromatic isocyanate compound group in combination. In the present invention, the balance of adhesive strength between the low-speed peeling region and the high-speed peeling region can be further improved by using, as the (C-1) trifunctional isocyanate compound, at least one selected from the (C-1-1) first group of aliphatic isocyanate compounds and at least one selected from the (C-1-2) second group of aromatic isocyanate compounds in combination. In addition, the (C-1) trifunctional isocyanate compound contains at least one selected from the (C-1-1) first aliphatic isocyanate compound group and at least one selected from the (C-1-2) second aromatic isocyanate compound group, and is preferably contained in a total amount of 0.5 to 5.0 parts by weight per 100 parts by weight of the copolymer. In addition, the mixing ratio of at least one selected from the (C-1-1) first aliphatic isocyanate compound group and at least one selected from the (C-1-2) second aromatic isocyanate compound group is preferably within the range of 10%:90% to 90%:10% by weight (C-1-1):(C-1-2).
[0036] Furthermore, the (C-2) bifunctional isocyanate compound used in the present invention is preferably an acyclic aliphatic isocyanate compound, which is a compound produced by reacting a diisocyanate compound with a diol compound. For example, when a diisocyanate compound is represented by the general formula "O=C=NXN=C=O" (where X is a divalent group) and a diol compound is represented by the general formula "HO-Y-OH" (where Y is a divalent group), an example of a compound produced by reacting a diisocyanate compound with a diol compound is a compound represented by the following general formula Z.
[0037] [General formula Z] O=C=NX-(NH-CO-OYO-CO-NH-X) n -N=C=O
[0038] Here, n is an integer of 0 or more. When n is 0, the general formula Z represents "O=C=NXN=C=O". The bifunctional acyclic aliphatic isocyanate compound may contain a compound in which n is 0 in the general formula Z (a diisocyanate compound unreacted with a diol compound), but it is preferable to contain a compound in which n is an integer of 1 or more as an essential component. The bifunctional acyclic aliphatic isocyanate compound may be a mixture of multiple compounds in which n in the general formula Z is different.
[0039] The diisocyanate compound represented by the general formula "O=C=NXN=C=O" is an aliphatic diisocyanate. X is preferably an acyclic aliphatic divalent group. The aliphatic diisocyanate is preferably one or more selected from the group consisting of tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and lysine diisocyanate.
[0040] The diol compound represented by the general formula "HO-Y-OH" is an aliphatic diol. Y is preferably an acyclic aliphatic divalent group. The diol compound is preferably one or more selected from the group consisting of 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2-dimethyl-1,3-propanediol monohydroxypivalate, polyethylene glycol, and polypropylene glycol.
[0041] The weight ratio (C-1 / C-2) of the (C-1) trifunctional isocyanate compound to the (C-2) difunctional isocyanate compound is preferably 1 to 90. The (C) di- or higher functional isocyanate compound is preferably 0.1 to 10 parts by weight per 100 parts by weight of the copolymer.
[0042] (D) The crosslinking catalyst of the metal chelate compound may be any substance that functions as a catalyst for the reaction (crosslinking reaction) between the copolymer and the crosslinking agent when a polyisocyanate compound is used as the crosslinking agent, and examples of such crosslinking catalyst include amine compounds such as tertiary amines, metal chelate compounds, organotin compounds, organolead compounds, organozinc compounds, and other organometallic compounds. In the present invention, a metal chelate compound is used as the crosslinking catalyst.
[0043] A metal chelate compound is a compound in which one or more polydentate ligands L are bonded to a central metal atom M. The metal chelate compound may or may not have one or more monodentate ligands X bonded to the metal atom M. For example, the general formula of a metal chelate compound having one metal atom M is M(L) m (X) n When m is 2 or more, m L's may be the same ligand or different ligands. When n is 2 or more, n X's may be the same ligand or different ligands.
[0044] Examples of the metal atom M include Fe, Ni, Mn, Cr, V, Ti, Ru, Zn, Al, Zr, and Sn. Examples of the polydentate ligand L include β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, octyl acetoacetate, oleyl acetoacetate, lauryl acetoacetate, and stearyl acetoacetate, and β-diketones such as acetylacetone (also known as 2,4-pentanedione), 2,4-hexanedione, and benzoylacetone. These are keto-enol tautomer compounds, and in the polydentate ligand L, the enol may be deprotonated to form an enolate (e.g., acetylacetonate). Examples of the monodentate ligand X include halogen atoms such as chlorine and bromine atoms, acyloxy groups such as pentanoyl, hexanoyl, 2-ethylhexanoyl, octanoyl, nonanoyl, decanoyl, dodecanoyl, and octadecanoyl groups, and alkoxy groups such as methoxy, ethoxy, n-propoxy, isopropoxy, and butoxy groups.
[0045] Specific examples of metal chelate compounds include iron tris(2,4-pentanedionato)(III), iron trisacetylacetonate, titanium trisacetylacetonate, ruthenium trisacetylacetonate, zinc bisacetylacetonate, aluminum trisacetylacetonate, zirconium tetrakisacetylacetonate, iron tris(2,4-hexanedionato)(III), zinc bis(2,4-hexanedionato), titanium tris(2,4-hexanedionato), aluminum tris(2,4-hexanedionato), and zirconium tetrakis(2,4-hexanedionato).
[0046] Examples of organotin compounds include dialkyltin oxide, fatty acid salts of dialkyltin, and fatty acid salts of stannous tin. Traditionally, dibutyltin compounds have been widely used, but in recent years, the toxicity of organotin compounds has been pointed out, and tributyltin (TBT) contained in dibutyltin compounds in particular is also a concern as an endocrine disrupting substance. From the viewpoint of safety, long-chain alkyltin compounds such as dioctyltin compounds are preferred. Specific examples of organotin compounds include dioctyltin oxide and dioctyltin dilaurate. Although Sn compounds can be used provisionally, in the future, in view of the trend toward the use of safer substances, it is preferable to use metal chelate compounds such as Al, Ti, and Fe, which are safer than Sn. The metal chelate compound in the pressure-sensitive adhesive composition according to the present invention preferably contains at least one selected from the group consisting of aluminum chelate compounds, titanium chelate compounds, and iron chelate compounds. The crosslinking catalyst (D) of a metal chelate compound is preferably contained in an amount of 0.001 to 0.5 parts by weight per 100 parts by weight of the copolymer.
[0047] Examples of the (E) keto-enol tautomer compound include β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, octyl acetoacetate, oleyl acetoacetate, lauryl acetoacetate, and stearyl acetoacetate, and β-diketones such as acetylacetone, 2,4-hexanedione, and benzoylacetone. In a pressure-sensitive adhesive composition using a polyisocyanate compound as a crosslinking agent, these compounds block the isocyanate groups of the crosslinking agent, thereby suppressing excessive viscosity increase and gelation of the pressure-sensitive adhesive composition after blending the crosslinking agent, and thereby extending the pot life of the pressure-sensitive adhesive composition. The (E) keto-enol tautomer compound is preferably contained in an amount of 0.1 to 300 parts by weight based on 100 parts by weight of the copolymer.
[0048] Since the (E) keto-enol tautomer compound has an effect of suppressing crosslinking, in contrast to the (D) metal chelate compound crosslinking catalyst, it is preferable to appropriately set the ratio of the (E) keto-enol tautomer compound to the (D) metal chelate compound crosslinking catalyst. In order to extend the pot life of the pressure-sensitive adhesive composition and improve storage stability, it is preferable that the weight ratio (E) / (D) of the (E) keto-enol tautomer compound to the (D) metal chelate compound crosslinking catalyst is high. The value of (E) / (D) is preferably in the range of 70 to 1000, more preferably 70 to 800, and most preferably 80 to 600.
[0049] More specifically, the pressure-sensitive adhesive composition having a long pot life according to the present invention is preferably such that the viscosity of the pressure-sensitive adhesive composition after 8 hours of storage at 23° C. is less than 1.25 times the viscosity immediately after the composition is blended, thereby making it possible to obtain a pressure-sensitive adhesive composition in which the increase in viscosity after blending is suppressed.
[0050] The pressure-sensitive adhesive composition of the present invention may contain, as additives, an antistatic agent, a polyether siloxane compound, and other conventional additives such as an antioxidant.
[0051] The antistatic agent may be an antistatic agent contained in the pressure-sensitive adhesive composition or an antistatic agent copolymerized in the copolymer. The antistatic agent is preferably contained in an amount of 0.05 to 5.0 parts by weight per 100 parts by weight of the copolymer. The antistatic agent is preferably an ionic compound having a melting point of 25 to 50° C. and / or an ionic compound containing an acryloyl group. These antistatic agents are presumed to have high affinity with the acrylic copolymer because they have a low melting point and a long-chain alkyl group.
[0052] The ionic compound having a melting point of 25 to 50°C is an ionic compound having a cation and an anion, in which the cation is a nitrogen-containing onium cation such as a pyridinium cation, an imidazolium cation, a pyrimidinium cation, a pyrazolium cation, a pyrrolidinium cation, or an ammonium cation, a phosphonium cation, or a sulfonium cation, and the anion is a hexafluorophosphate (PF6 - ), thiocyanate (SCN - ), alkylbenzene sulfonate (RC6H4SO3 - ), perchlorate (ClO4 - ), tetrafluoroborate (BF4 - Examples of the anion include inorganic or organic anions such as bis(fluorosulfonyl)imide salts (FSI), bis(trifluoromethanesulfonyl)imide salts (TFSI), and trifluoromethanesulfonate salts (TF). The anion is preferably solid at room temperature (e.g., 25°C), and a melting point of 25 to 50°C can be obtained by selecting the chain length of the alkyl group, the position and number of the substituents, and the like. The cation is preferably a quaternary nitrogen-containing onium cation, and examples thereof include quaternary pyridinium cations such as 1-alkylpyridinium (carbon atoms at positions 2 to 6 may be substituted or unsubstituted), quaternary imidazolium cations such as 1,3-dialkylimidazolium (carbon atoms at positions 2, 4, and 5 may be substituted or unsubstituted), and quaternary ammonium cations such as tetraalkylammonium. The ionic compound having a melting point of 25 to 50° C. is preferably contained in an amount of 0.05 to 5 parts by weight per 100 parts by weight of the copolymer.
[0053] The acryloyl group-containing ionic compound is an ionic compound having a cation and an anion, and the cation is (meth)acryloyloxyalkyltrialkylammonium [R + -C n H 2n -OCOCQ=CH2, where Q=H or CH3, R=alkyl], and the anion is hexafluorophosphate (PF6 - ), thiocyanate (SCN - ), organic sulfonates (RSO3 - ), perchlorate (ClO4 - ), tetrafluoroborate (BF4 - ), F-containing imide salt (R F 2N - ) and other inorganic or organic anions. F 2N - )R F Examples of the F-containing imide salt include perfluoroalkanesulfonyl groups such as trifluoromethanesulfonyl and pentafluoroethanesulfonyl groups, and fluorosulfonyl groups. Examples of the F-containing imide salt include bis(fluorosulfonyl)imide salts [(FSO2)2N - 〕, bis(trifluoromethanesulfonyl)imide salt [(CF3SO2)2N - 〕, bis(pentafluoroethanesulfonyl)imide salt [(C2F5SO2)2N - and the like. The acryloyl group-containing ionic compound is preferably copolymerized in the copolymer in an amount of 0.1 to 5.0% by weight.
[0054] Specific examples of the antistatic agent are not particularly limited, but specific examples of ionic compounds having a melting point of 25 to 50°C include 1-octylpyridinium hexafluorophosphate, 1-nonylpyridinium hexafluorophosphate, 2-methyl-1-dodecylpyridinium hexafluorophosphate, 1-octylpyridinium dodecylbenzenesulfonate, 1-dodecylpyridinium thiocyanate, 1-dodecylpyridinium dodecylbenzenesulfonate, 4-methyl-1-octylpyridinium hexafluorophosphate, and quaternary ammonium salts of trifluoromethanesulfonic acid. Specific examples of ionic compounds containing an acryloyl group include dimethylaminomethyl (meth)acrylate hexafluorophosphate methyl salt [(CH3)3N + CH2OCOCQ=CH2 PF6 - , where Q=H or CH3], dimethylaminoethyl (meth)acrylate bis(trifluoromethanesulfonyl)imide methyl salt [(CH3)3N + (CH2)2OCOCQ=CH2·(CF3SO2)2N - , where Q=H or CH3], dimethylaminomethyl methacrylate bis(fluorosulfonyl)imide methyl salt [(CH3)3N + CH2OCOCQ=CH2·(FSO2)2N - , where Q=H or CH3).
[0055] The polyether-modified siloxane compound is a siloxane compound having a polyether group, and has a general siloxane unit [—SiR 1 2-O-], as well as siloxane units with polyether groups [-SiR 1 (R 2 O(R 3 O) n R 4 )-O-], where R 1 is one or more alkyl or aryl groups, R 2 and R 3 is one or more alkylene groups, R 4indicates one or more alkyl or acyl groups (terminal groups). The polyether group is a polyoxyethylene group [(C2H4O) n 〕 and polyoxypropylene group〔(C3H6O) n ] and the like polyoxyalkylene groups. The polyether-modified siloxane compound is preferably a polyether-modified siloxane compound having an HLB value of 7 to 15. The content of the polyether-modified siloxane compound is preferably 0.01 to 1.0 part by weight, more preferably 0.1 to 0.5 part by weight, per 100 parts by weight of the copolymer. HLB is the hydrophilic-lipophilic balance (hydrophilic-lipophilic ratio) defined in, for example, JIS K3211 (terminology for surfactants). The polyether-modified siloxane compound can be obtained, for example, by grafting an organic compound having an unsaturated bond and a polyoxyalkylene group onto a polyorganosiloxane main chain having a silicon hydride group by a hydrosilylation reaction.Specific examples include dimethylsiloxane-methyl(polyoxyethylene)siloxane copolymer, dimethylsiloxane-methyl(polyoxyethylene)siloxane-methyl(polyoxypropylene)siloxane copolymer, dimethylsiloxane-methyl(polyoxypropylene)siloxane polymer, etc. By blending the polyether-modified siloxane compound in the pressure-sensitive adhesive composition, the adhesive strength and reworkability of the pressure-sensitive adhesive can be improved. When the pressure-sensitive adhesive composition does not contain the polyether-modified siloxane compound, the cost becomes lower.
[0056] Examples of the antioxidant include hindered phenol-based antioxidants, polyphenol compounds, and tocopherol-based compounds. Among them, tocopherol-based compounds are preferred. Tocopherol-based compounds are generally vitamin E and are also naturally derived chemical substances. For this reason, they have little adverse effect on the human body, are highly safe to handle, and are environmentally friendly. In addition, they are oil-soluble and liquid at room temperature, so they are highly compatible with the adhesive composition and have excellent precipitation resistance. By incorporating a tocopherol-based compound as the antioxidant, the storage stability of the adhesive is improved, and the pot life of the adhesive composition containing the curing agent is improved. The tocopherol-based compound used in the present invention is preferably a compound in which the ferrule hydroxyl group of tocopherol is not changed to an ester or the like and has a ferrule hydroxyl group, since it is used by blending it with the adhesive composition (it is not metabolized like in the human body). Examples include tocopherol and tocotrienol. It is known that tocopherol and tocotrienol are classified into natural compounds (d-form), non-natural compounds (l-form), and racemic mixtures of these compounds (dl-form), which are equal amounts of these compounds. Natural compounds (d-form) and racemic compounds (dl-form) are preferred because they are used as food additives, etc. Specific examples of tocopherol compounds include at least one selected from the group consisting of d-α-tocopherol, dl-α-tocopherol, d-β-tocopherol, dl-β-tocopherol, d-γ-tocopherol, dl-γ-tocopherol, d-δ-tocopherol, dl-δ-tocopherol, d-α-tocotrienol, dl-α-tocotrienol, d-β-tocotrienol, dl-β-tocotrienol, d-γ-tocotrienol, dl-γ-tocotrienol, d-δ-tocotrienol, and dl-δ-tocotrienol. Two or more tocopherol compounds may be used in combination. As a food additive, "mixed tocopherols" is a mixture whose main components are d-α-tocopherol, d-β-tocopherol, d-γ-tocopherol, and d-δ-tocopherol, while "tocotrienol" is a mixture whose main components are d-α-tocotrienol, d-β-tocotrienol, d-γ-tocotrienol, and d-δ-tocotrienol. When the pressure-sensitive adhesive composition of the present invention contains a tocopherol-based compound, it preferably contains 0.01 to 5 parts by weight of the tocopherol-based compound per 100 parts by weight of the copolymer.
[0057] Furthermore, as other components, known additives such as copolymerizable (meth)acrylic monomers containing alkylene oxides, (meth)acrylamide monomers, dialkyl-substituted acrylamide monomers, surfactants, curing catalysts, plasticizers, fillers, curing retarders, processing aids, antioxidants, antioxidants, etc. may be appropriately blended. These may be used alone or in combination of two or more.
[0058] The copolymer of the main component used in the pressure-sensitive adhesive composition of the present invention can be synthesized by copolymerizing (A) at least one (meth)acrylic acid ester monomer having an alkyl group with a carbon number of C4 to C18 and (B) a copolymerizable monomer containing a hydroxyl group as a copolymerizable monomer group. The polymerization method of the copolymer is not particularly limited, and any appropriate polymerization method such as solution polymerization or emulsion polymerization can be used. The copolymer may further contain at least one of a carboxyl group-containing monomer and a nitrogen-containing vinyl monomer not containing a hydroxyl group as other copolymerizable monomers. The pressure-sensitive adhesive composition of the present invention can be prepared by blending the above-mentioned copolymer with (C) a difunctional or higher isocyanate compound, (D) a crosslinking catalyst of a metal chelate compound, (E) a keto-enol tautomer compound, and further any additives as appropriate.
[0059] The copolymer is preferably an acrylic polymer, and preferably contains 50 to 100% by weight of an acrylic monomer such as a (meth)acrylic acid ester monomer, (meth)acrylic acid, or a (meth)acrylamide. The acid value of the copolymer is preferably 8.0 or less, more preferably 0.01 to 8.0, which can improve staining properties and enhance the ability to prevent adhesive residue from occurring. Here, the "acid value" is an index representing the acid content, and is expressed as the number of milligrams of potassium hydroxide required to neutralize 1 g of a polymer containing a carboxyl group.
[0060] The adhesive layer obtained by crosslinking the adhesive composition preferably has an adhesive strength of 0.05 to 0.2 N / 25 mm at a low peeling speed of 0.3 m / min, and an adhesive strength of 2.0 N / 25 mm or less at a high peeling speed of 30 m / min. This provides performance with little change in adhesive strength depending on the peeling speed, and enables rapid peeling even at high-speed peeling. In addition, even when the surface protection film is peeled off once for re-adhesion, excessive force is not required, and it is easy to peel off from the adherend.
[0061] The gel fraction of the pressure-sensitive adhesive layer (crosslinked pressure-sensitive adhesive) obtained by crosslinking the pressure-sensitive adhesive composition of the present invention is preferably 90 to 100%. With such a high gel fraction, the adhesive strength is not excessively high at a low peel speed, the elution of unpolymerized monomers or oligomers from the copolymer is reduced, reworkability and durability at high temperatures and high humidity are improved, and contamination of the adherend can be suppressed.
[0062] The pressure-sensitive adhesive film of the present invention is formed by forming a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition of the present invention on one or both sides of a resin film. The surface protection film of the present invention is formed by forming a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition of the present invention on one side of a resin film. The pressure-sensitive adhesive composition of the present invention has a long pot life and a fast crosslinking rate even without using an organotin compound because the above-mentioned components (A) to (E) are blended in a well-balanced manner. Therefore, the surface protection film of the present invention can be suitably used as a surface protection film for polarizing plates, or as a surface protection film for any precision electric / electronic component selected from the group of precision electric / electronic components consisting of flexible printed wiring boards, rigid printed wiring boards, and transparent conductive films.
[0063] In the pressure-sensitive adhesive film and surface protection film according to the present invention, a polyester film or the like can be used as the base material for the resin film or the release film (separator) that protects the pressure-sensitive adhesive layer. In addition, the resin film may be subjected to an antifouling treatment using a silicone-based or fluorine-based release agent or coating agent, silica microparticles, or the like, or an antistatic treatment by coating or kneading an antistatic agent, on the side opposite the side on which the pressure-sensitive adhesive layer is formed. In addition, the release film is subjected to a release treatment with a silicone-based or fluorine-based release agent on the surface thereof that is to be joined to the adhesive surface of the adhesive layer. EXAMPLES
[0064] The present invention will now be described in detail with reference to examples.
[0065] <Production of Acrylic Copolymer> [Example 1] Nitrogen gas was introduced into a reactor equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, and the air in the reactor was replaced with nitrogen gas. Then, 100 parts by weight of 2-ethylhexyl acrylate and 3.5 parts by weight of 8-hydroxyoctyl acrylate were added to the reactor. Then, 0.1 parts by weight of azobisisobutyronitrile as a polymerization initiator was dropped over 2 hours, and the mixture was reacted at 65°C for 6 hours to obtain an acrylic copolymer solution 1 used in Example 1 having a weight average molecular weight of 500,000. A portion of the acrylic copolymer was collected and used as a sample for measuring the acid value described below. [Examples 2 to 6 and Comparative Examples 1 to 3] The acrylic copolymer solutions used in Examples 2 to 6 and Comparative Examples 1 to 3 were obtained in the same manner as in the acrylic copolymer solution 1 used in Example 1 above, except that the monomer compositions were as shown in Table 1 (A), (B), and (I), respectively.
[0066] <Production of Pressure-Sensitive Adhesive Composition and Surface Protective Film> [Example 1] To the acrylic copolymer solution 1 of Example 1 produced as described above, 6.0 parts by weight of acetylacetone was added and stirred, and then 1.5 parts by weight of Coronate HX (isocyanurate of hexamethylene diisocyanate compound) and 0.05 parts by weight of tris(2,4-pentanedionato)iron(III) were added and mixed by stirring to obtain an adhesive composition of Example 1. This adhesive composition was applied onto a release film made of a silicone resin-coated polyethylene terephthalate (PET) film, and then dried at 90°C to remove the solvent, thereby obtaining an adhesive sheet with an adhesive layer thickness of 25 μm. Thereafter, an adhesive sheet was transferred to the side opposite the antistatic and antifouling treated side of a polyethylene terephthalate (PET) film having one side treated with antistatic and antifouling treatment, thereby obtaining a surface protection film of Example 1 having a laminate structure of "antistatic and antifouling treated PET film / adhesive layer / release film (silicone resin coated PET film)". [Examples 2 to 6 and Comparative Examples 1 to 3] The surface protection films of Examples 2 to 6 and Comparative Examples 1 to 3 were obtained in the same manner as the surface protection film of Example 1 above, except that the compositions of the additives were as shown in Table 1 (C) to (E), respectively.
[0067] [Table 1]
[0068] In Table 1, the numerical values in parts by weight, calculated with the total of group (A) being 100 parts by weight, are enclosed in parentheses. The ratio values of (E) / (D) are shown in Table 2. The compound names of the abbreviations of each component used in Table 1 are shown in Table 3. Note that Coronate (registered trademark) HX, Coronate (registered trademark) HL, and Coronate (registered trademark) L are product names of Nippon Polyurethane Industry Co., Ltd., Takenate (registered trademark) D-140N is a product name of Mitsui Chemicals, Inc., and Duranate (registered trademark) D101 is a product name of Asahi Kasei Chemicals Corporation.
[0069] [Table 2]
[0070] [Table 3]
[0071] <Test methods and evaluation> The surface protection films in Examples 1 to 6 and Comparative Examples 1 to 3 were aged for 7 days under an atmosphere of 23°C and 50% RH, and then the release film (a silicone resin-coated PET film) was peeled off to expose the adhesive layer. The surface protection film with the exposed adhesive layer was then attached to the surface of a polarizing plate attached to a liquid crystal cell via the adhesive layer, and left for 1 day, after which it was autoclaved at 50°C, 5 atm, for 20 minutes, and then left at room temperature for another 12 hours to prepare a sample for measuring adhesive strength.
[0072] <Adhesive strength> The measurement sample obtained above (a 25 mm wide surface protection film bonded to the surface of a polarizing plate) was peeled in a 180° direction using a tensile tester at a low peel speed (0.3 m / min) and a high peel speed (30 m / min), and the measured peel strength was taken as the adhesive strength.
[0073] <Pot life> The viscosity η0 (initial viscosity) of the adhesive composition was measured immediately after the additives (C) to (E) were added, and the viscosity η1 (viscosity after 8 hours) of the adhesive composition was measured after the adhesive composition was left in a sealed state at 23°C for 8 hours. As an index of pot life, the value of η1 when η0 was set to 1.0, i.e., the ratio of η1 / η0, was calculated. The evaluation target criteria were as follows: if the viscosity after 8 hours was less than 1.25 times the initial viscosity, it was evaluated as "○", if it was 1.25 times or more but less than 1.50 times, it was evaluated as "△", and if it was 1.50 times or more or gelled after being left for 8 hours, it was evaluated as "×".
[0074] Table 4 shows the evaluation results.
[0075] [Table 4]
[0076] The surface protection films of Examples 1 to 6 had an adhesive strength of 0.05 to 0.2 N / 25 mm at a low peel speed of 0.3 m / min and an adhesive strength of 2.0 N / 25 mm or less at a high peel speed of 30 m / min, and had a sufficiently long pot life. That is, at both low and high peel speeds, the adhesive strength is well balanced, the pot life is long, and the properties as a surface protection film are excellent. Moreover, the surface protection films of Examples 1 to 6 are highly safe since the pressure-sensitive adhesive composition does not contain an organotin compound.
[0077] The surface protection film of Comparative Example 1 had excessively high adhesive strength at a low peel speed of 0.3 m / min and a high peel speed of 30 m / min, possibly because it did not contain the difunctional or higher isocyanate compound (C) which serves as a crosslinking agent. The surface protection film of Comparative Example 2 had a short pot life due to a small ratio of the keto-enol tautomer compound (E) to the crosslinking catalyst of the metal chelate compound (D). The surface protection film of Comparative Example 3 had a small ratio of the keto-enol tautomer compound (E) to the crosslinking catalyst (D) of the metal chelate compound, so the pot life was too short and crosslinking progressed before coating, making it impossible to coat. Thus, the surface protection films of Comparative Examples 1 to 3 were unable to simultaneously satisfy all of the required performance characteristics, namely, an excellent balance of adhesive strength at both low and high peel speeds, and a long pot life.
Claims
1. A pressure-sensitive adhesive composition comprising an acrylic polymer and a crosslinking agent, the acrylic polymer is a copolymer obtained by copolymerizing (A) at least one (meth)acrylic acid ester monomer having an alkyl group with a carbon number of 4 to 18 carbon atoms and (B) at least one copolymerizable monomer containing a hydroxyl group as a copolymerizable monomer group, the pressure-sensitive adhesive composition contains, relative to 100 parts by weight of the copolymer, (C) 0.1 to 10 parts by weight of a difunctional or higher isocyanate compound as the crosslinking agent, (D) 0.001 to 0.5 parts by weight of a crosslinking catalyst of a metal chelate compound, and (E) 0.1 to 300 parts by weight of a keto-enol tautomer compound, and a weight ratio of (E) / (D) is 80 to 600; A pressure-sensitive adhesive composition, characterized in that the pressure-sensitive adhesive composition is blended and then stored at 23°C, and the viscosity of the pressure-sensitive adhesive composition after 8 hours is less than 1.25 times the viscosity immediately after blending.
2. 2. The pressure-sensitive adhesive composition according to claim 1, wherein the copolymer is an acrylic polymer containing at least one of a carboxyl group-containing monomer and a nitrogen-containing vinyl monomer not containing a hydroxyl group as other copolymerizable monomers.
3. 3. A pressure-sensitive adhesive film comprising a resin film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition according to claim 1 or 2 on one or both sides of the resin film.
4. 3. A surface protective film comprising a resin film and a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition according to claim 1 or 2 on one side of the resin film.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition and surface protective film for optical member
JP2008013634A
Adhesive composition
JP2011001440A
Pressure-sensitive adhesive composition, pressure-sensitive adhesive layer, and pressure-sensitive adhesive sheet
JP2013147631A
Pressure-sensitive adhesive composition, pressure-sensitive adhesive sheet, and optical member
JP2013216756A
Adhesive composition for adhesive sheet for semiconductor wafer processing and adhesive sheet using the adhesive composition