Conductive adhesive, manufacturing method of circuit connection structure, and circuit connection structure

JP2024152781AActive Publication Date: 2024-10-25RESONAC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024130664
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-25
Estimated Expiration
2040-05-13

AI Technical Summary

Benefits of technology

【0020】 本発明によれば、対向する電極の接続において低抵抗を示し、かつ、良好な接続信頼性を得ることができる導電性接着剤を提供することができる。本発明はまた、そのような導電性接着剤を用いて、低抵抗かつ接続信頼性に優れた回路接続構造体及びその製造方法を提供することができる。回路接続構造体は、例えば高温高湿の環境にさらされた場合であっても、接続信頼性を十分に確保することが可能であり、消費電力の低減に有用である。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152781000004
    Figure 2024152781000004
  • Figure 2024152781000005
    Figure 2024152781000005
  • Figure 2024152781000006
    Figure 2024152781000006
Patent Text Reader

Abstract

To provide a conductive adhesive which exhibits low resistance in connection of opposite electrodes and can obtain excellent connection reliability, a manufacturing method of a circuit connection structure using the conductive adhesive, and a circuit connection structure.SOLUTION: A conductive adhesive contains an adhesive composition, and conductive particles. A compressive hardness of the conductive particles in 20% compression is 10.0 GPa or more at 25°C, and 3.5 GPa or less at 150°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive adhesive, a method for producing a circuit connection structure, and a circuit connection structure. [Background technology]

[0002] In recent years, there has been a demand for displays with a wider viewing angle and lower power consumption, and the development of self-luminous displays such as organic electroluminescence (EL) displays is progressing. Organic EL displays employ a system in which electrical signals are input from FPCs (Flexible Printed Circuits) in the same way as liquid crystal panels, and in such a system, a large current of about several tens of mA to 200 mA flows through one connection terminal. For this reason, the electrodes on the organic EL display side are designed to obtain a sufficient current value by using a transparent electrode such as ITO on a glass substrate and a metal film with a thickness of several tens to several thousands of nm formed thereon (see, for example, Patent Document 1).

[0003] By the way, a circuit connecting material is usually used to connect the electrodes of the FPC and the electrodes of the display side. For example, a conductive adhesive having anisotropic conductivity containing an adhesive composition and conductive particles is known as a circuit connecting material. With such a circuit connecting material, the electrodes can be connected with low resistance by the conductive particles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 3641342 specification Summary of the Invention [Problem to be solved by the invention]

[0005] The demand for lower power consumption in displays is increasing, and circuit connecting materials with lower resistance than ever before are being required. In addition, as circuits become more dense, circuit connecting materials are also required to have excellent connection reliability, i.e., to prevent an increase in connection resistance after connection.

[0006] Therefore, an object of the present invention is to provide a conductive adhesive that exhibits low resistance when connecting opposing electrodes and can obtain good connection reliability. Another object of the present invention is to provide a method for producing a circuit connection structure using such a conductive adhesive, and a circuit connection structure. [Means for solving the problem]

[0007] In order to solve the above problems, one aspect of the present invention provides a conductive adhesive comprising an adhesive composition and conductive particles, wherein the compression hardness of the conductive particles at 20% compression is 10.0 GPa or more at 25°C and 3.5 GPa or less at 150°C.

[0008] The conductive adhesive exhibits low resistance in the connection of the opposing electrodes and can obtain good connection reliability. The reason why such an effect is obtained is not necessarily clear, but the inventors speculate as follows. The conductive particles contained in the conductive adhesive have a compression hardness that satisfies the above conditions at two predetermined temperatures, so that the conductive particles when mounted by thermocompression bonding can exhibit a hardness that allows sufficient contact with the electrodes and a softness that makes it difficult for resistance to increase due to the repulsion of the conductive particles immediately after mounting, and it is believed that this has achieved both a reduction in connection resistance and an improvement in connection reliability.

[0009] The conductive particles may have a compression recovery rate at 25°C of 50 to 75%.

[0010] The conductive particles may have an average particle size of 2 μm or more and 10 μm or less.

[0011] When a conductive adhesive is used to connect the circuit electrodes together, the connection may be a Flex on Glass connection, a Flex on Flex connection, or a Flex on Polymer connection.

[0012] Another aspect of the present invention relates to a method for producing a circuit connection structure, comprising the steps of interposing the above-described conductive adhesive according to the present invention between a first circuit member having a first circuit electrode and a second circuit member having a second circuit electrode, and thermocompression bonding the first circuit member and the second circuit member to electrically connect the first circuit electrode and the second circuit electrode.

[0013] According to the above-mentioned method for producing a circuit connection structure, by using the conductive adhesive according to the present invention, a circuit connection structure having low resistance and excellent connection reliability can be obtained.

[0014] In the above-mentioned method for producing a circuit connection structure, at least one of the first circuit electrode and the second circuit electrode may have a layer containing Ti on a surface thereof.

[0015] Titanium has excellent electrical conductivity, and its magnetic properties, strength, ductility and malleability make it suitable for use as a circuit-forming material. Furthermore, it is a metal that exhibits excellent corrosion resistance, chemical stability, physical stability, gas barrier properties and diffusion barrier properties at the interface between dissimilar metals due to the strong oxide coating that forms on its surface, making it easier to obtain a circuit connection structure that can withstand large currents.

[0016] In addition, the present inventors have found that when the electrodes are formed from an electrode material containing titanium, it tends to be more difficult to reduce the connection resistance and ensure the connection reliability with conventional circuit connection materials containing conductive particles. In contrast, the conductive adhesive of the present invention can reduce the connection resistance and ensure the connection reliability even when connecting electrodes having a layer containing Ti on the surface. Therefore, the method of the present invention can obtain a circuit connection structure corresponding to the above characteristics while reducing the connection resistance and ensuring the connection reliability.

[0017] Another aspect of the present invention relates to a circuit connection structure comprising a first circuit member having a first circuit electrode, a second circuit member having a second circuit electrode, and a connection portion interposed between the first circuit member and the second circuit member, wherein the connection portion is a cured product of the conductive adhesive according to the present invention described above.

[0018] The above circuit connection structure can have low resistance and excellent connection reliability because the connection portion is made of a cured product of the conductive adhesive according to the present invention.

[0019] In the above circuit connection structure, at least one of the first circuit electrode and the second circuit electrode may have a layer containing Ti on the surface. Effect of the Invention

[0020] According to the present invention, it is possible to provide a conductive adhesive that exhibits low resistance in the connection of opposing electrodes and can obtain good connection reliability. The present invention also provides a circuit connection structure and a method for producing the same that use such a conductive adhesive and has low resistance and excellent connection reliability. The circuit connection structure can ensure sufficient connection reliability even when exposed to a high-temperature and high-humidity environment, for example, and is useful for reducing power consumption. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a schematic diagram showing a method for calculating the compression recovery rate of conductive particles. [Diagram 2] 1 is a graph showing an example of a compression curve of conductive particles. [Diagram 3] 1A to 1C are cross-sectional views illustrating process steps of a method for producing a circuit connection structure according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings where necessary. However, the present invention is not limited to the following embodiments.

[0023] In this specification, "(meth)acrylate" means acrylate or the corresponding methacrylate. Similarly, "(meth)acryloxy" means acryloxy or the corresponding methacryloxy. "A or B" may include either A or B, or may include both.

[0024] In addition, in this specification, a numerical range indicated using "~" indicates a range including the numerical values ​​described before and after "~" as the minimum and maximum values, respectively. Furthermore, in a numerical range described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage may be replaced with the upper limit or lower limit of a numerical range of another stage. Furthermore, in a numerical range described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in an example.

[0025] <Conductive adhesive> The conductive adhesive of the present embodiment contains conductive particles and an adhesive composition.

[0026] (Conductive particles) The conductive particles to be used may have a compression hardness at 20% compression of 10.0 GPa or more at 25° C. and 3.5 GPa or less at 150° C. The compression hardness of the conductive particles is an index of the hardness of the conductive particles.

[0027] The compression hardness (hereinafter sometimes referred to as "K value") of conductive particles can be measured using a microcompression tester (apparatus name: Fischer HM2000, manufactured by Fischer Instruments). Specifically, conductive particles are first scattered on a slide glass (product name: S1214, manufactured by Matsunami Glass Industry Co., Ltd.) on a stage set at a predetermined temperature (e.g., 25°C, 150°C). Then, one particle is selected from the particles and compressed from the center at a speed of 0.33 mN / s with an initial load of 0.1 mN using a prismatic diamond indenter with a square base of 50 μm on each side. The K value can be calculated from the stress-strain curve. Specifically, the compression equation of an elastic sphere is given by the load F (N), displacement S (mm), particle radius R (mm), elastic modulus E (Pa), and Poisson's ratio σ: F=(2 1 / 2 / 3)×(S 3 / 2 )×(E×R 1 / 2 ) / (1-σ 2 ) Using the following formula K = E / (1-σ 2 )=(3 / 2 1 / 2 )×F×(S -3 / 2 )×(R -1 / 2 ) Furthermore, if the deformation rate is X (%) and the diameter of the sphere is D (μm), the following formula can be used: K = 3000F / (D 2 X 3 / 2 ) x 10 6 The K value at any deformation rate can be calculated by the following formula. X = (S / D) x 100 The maximum test load in the compression test is set to, for example, 50 mN.

[0028] The K value at 20% compression is calculated with the deformation rate X set to 0.2.

[0029] The conductive particles have a compression hardness of 10.0 GPa or more, preferably 10.0 to 20.0 GPa, more preferably 10.0 to 15.0 GPa, even more preferably 10.0 to 13.0 GPa, and particularly preferably 10.5 to 12.0 GPa, when compressed by 20% at 25° C. When the K value of the conductive particles when compressed by 20% at 25° C. (hereinafter sometimes referred to as K value (25° C., 20%)) is within the above range, when opposing electrodes are connected to each other, the conductive particles tend to be appropriately flattened between the electrodes, making it easier to ensure the contact area between the electrodes and the conductive particles, and making it easier to further improve the connection reliability.

[0030] The conductive particles have a compression hardness of 3.5 GPa or less, preferably 1.0 to 3.5 GPa, more preferably 1.5 to 3.2 GPa, even more preferably 1.8 to 3.0 GPa, and particularly preferably 2.0 to 3.0 GPa, when compressed by 20% at 150° C. When the K value of the conductive particles when compressed by 20% at 150° C. (hereinafter sometimes referred to as K value (150° C., 20%)) is within the above range, the conductive particles immediately after mounting exhibit a suitable softness, and there is a tendency that an increase in resistance due to repulsion of the conductive particles is unlikely to occur, making it easy to further improve the connection reliability.

[0031] The compression recovery rate (compression deformation recovery rate) of the conductive particles at 25° C. may be more than 40%, 45% or more, 50% or more, 70% or more, 80% or less, 75% or less, or 60% or less. The compression recovery rate of the conductive particles at 25° C. may be in a range that is a combination of the above lower limit and the above upper limit, and may be, for example, more than 40% and 80% or less, 45 to 80%, 50 to 75%, 70 to 75%, or 55 to 60%.

[0032] The compression recovery rate can be measured, for example, using a microcompression tester (apparatus name: Fischer HM2000, manufactured by Fischer Instruments). Specifically, conductive particles are first spread on a slide glass (product name: S1214, manufactured by Matsunami Glass Industry Co., Ltd.) on a stage set at 25°C. Then, one particle is selected from the particles and compressed at a speed of 0.33 mN / sec from the center with a square diamond indenter having a square base with sides of 50 μm until a load of 5 mN is applied, with an initial load of 0.1 mN. The load is then reduced to the initial load value at a speed of 0.33 mN / sec. The relationship between the load value and the compression displacement during this process is measured, and the compression recovery rate can be measured.

[0033] This will be explained using the drawings. Fig. 1 is a schematic diagram showing a method for calculating the compression recovery rate of conductive particles. Meanwhile, Fig. 2 is a graph showing an example of a compression curve of a conductive particle. As shown in Figs. 1 and 2, the compression recovery rate is calculated by taking the displacement from the initial load (load 0.1 mN) to the load reversal (load 5 mN) as L2 and the displacement from the load reversal to the final load (load 0.1 mN) as L1 / L2 x 100 (%). This operation is carried out for 10 conductive particles and the average value is calculated to calculate the compression recovery rate in this embodiment.

[0034] The conductive particles are not particularly limited, but examples thereof include core-shell particles having plastic particles and a metal layer covering the plastic particles. The metal layer does not need to cover the entire surface of the plastic particles, and may cover only a part of the surface of the plastic particles.

[0035] Examples of the plastic particles include those formed from at least one resin selected from the group consisting of acrylic resins such as polymethyl methacrylate and polymethyl acrylate, polyolefin resins such as polyethylene, polypropylene, polyisobutylene and polybutadiene, polystyrene resins, polyester resins, polyurethane resins, polyamide resins, epoxy resins, polyvinyl butyral resins, rosin resins, terpene resins, phenol resins, guanamine resins, melamine resins, oxazoline resins, carbodiimide resins, silicone resins, etc. The plastic particles may be composites of these resins with inorganic substances such as silica.

[0036] From the viewpoint of ease of control of compression recovery rate and compression hardness (K value), the plastic particles may be made of a resin obtained by polymerizing one type of polymerizable monomer having an ethylenically unsaturated group, or may be made of a resin obtained by copolymerizing two or more types of polymerizable monomer having an ethylenically unsaturated group. When obtaining a resin by copolymerizing two or more types of polymerizable monomer having an ethylenically unsaturated group, the compression recovery rate and compression hardness of the plastic particles can be easily controlled by using a non-crosslinkable monomer and a crosslinkable monomer in combination and appropriately adjusting the copolymerization ratio and type thereof. In addition, by using plastic particles containing two or more types of resin, the compression hardness may be adjusted so that the conductive particles satisfy the above-mentioned conditions of K value (25°C, 20%) and K value (150°C, 20%). As the non-crosslinkable monomer and the crosslinkable monomer, for example, the monomers described in JP-A-2004-165019 can be used.

[0037] The average particle size of the plastic particles is preferably 1 to 10 μm. From the viewpoint of high density mounting, the average particle size of the plastic particles is more preferably 1 to 5 μm. Furthermore, from the viewpoint of maintaining a more stable connection state when there is variation in the unevenness of the electrode surface, the average particle size of the plastic particles is even more preferably 2 to 5 μm.

[0038] In this embodiment, the average particle size of the particles can be determined as follows. That is, one particle is randomly selected and observed under a differential scanning electron microscope to measure its maximum and minimum diameters. The square root of the product of the maximum and minimum diameters is defined as the particle size of the particle. Using this method, the particle sizes of 50 randomly selected particles are measured and the average value is calculated to determine the average particle size.

[0039] The metal layer is preferably formed of at least one metal selected from the group consisting of Ni, Au, Pd, W, Cu, and NiB. The metal layer may have one or more layers selected from the group consisting of a Ni layer, a Ni layer / Au layer (an embodiment in which an Au layer is provided on a Ni layer; the same applies below), a Ni layer / Pd layer, a Ni layer / W layer, a Cu layer, and a NiB layer. The metal layer may be a thin film formed by a general method such as plating, vapor deposition, or sputtering. From the viewpoint of improving the insulation between adjacent electrodes, the conductive particles may have a layer of an insulating material such as silica or acrylic resin covering the metal layer on the outside of the metal layer.

[0040] From the viewpoint of balancing electrical conductivity and cost, the thickness of the metal layer is preferably 10 to 1000 nm, more preferably 20 to 200 nm, and even more preferably 50 to 150 nm. When a layer of an insulating material or an adhesion layer formed by adhering insulating fine particles is further provided on the metal layer, the thickness is preferably about 50 to 1000 nm. The thickness of these layers can be measured, for example, by a scanning electron microscope (SEM), a transmission electron microscope (TEM), an optical microscope, or the like.

[0041] The conductive particles preferably have an average particle size of 2 to 10 μm, more preferably 2 to 8 μm, even more preferably 2 to 6 μm, and most preferably 2 to 5 μm. If the conductive particles have an average particle size within the above range, for example when the conductive adhesive of the present embodiment is used as a circuit connecting material, the particle size of the conductive particles can be made smaller than the electrode height of the circuit member to be connected, making it easier to further reduce short circuits between adjacent electrodes.

[0042] The content of the conductive particles in the conductive adhesive is preferably 0.1 to 30 parts by volume, more preferably 0.25 to 25 parts by volume, and even more preferably 0.5 to 20 parts by volume, when the total volume of the conductive adhesive is taken as 100 parts by volume. If the content of the conductive particles is within the above range, for example, when the conductive adhesive of this embodiment is used as a circuit connecting material, it becomes easy to achieve a good balance between the conductivity between opposing electrodes and the insulation between adjacent electrodes.

[0043] (Adhesive Composition) The adhesive composition is not particularly limited, and may be, for example, thermosetting or photocurable. Examples of thermosetting adhesive compositions include a composition containing an epoxy resin and a latent curing agent for the epoxy resin (hereinafter referred to as the "first composition"), a composition containing a radical polymerizable substance and a curing agent that generates free radicals when heated (hereinafter referred to as the "second composition"), or a mixed composition of the first composition and the second composition.

[0044] Examples of the epoxy resin contained in the first composition include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, alicyclic epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, hydantoin type epoxy resin, isocyanurate type epoxy resin, aliphatic chain epoxy resin, etc. These epoxy resins may be halogenated or hydrogenated. Two or more of these epoxy resins may be used in combination.

[0045] The latent curing agent contained in the first composition may be any agent capable of curing an epoxy resin, and examples of such latent curing agents include anionic polymerization catalyst-type curing agents, cationic polymerization catalyst-type curing agents, polyaddition-type curing agents, etc. These may be used alone or in a mixture of two or more. Among these, anionic or cationic polymerization catalyst-type curing agents are preferred because they have excellent fast curing properties and do not require consideration of chemical equivalents.

[0046] Examples of anionic or cationic polymerizable catalyst-type curing agents include imidazole-based curing agents, hydrazide-based curing agents, boron trifluoride-amine complexes, sulfonium salts, aminimides, diaminomaleonitrile, melamine and its derivatives, polyamine salts, dicyandiamide, etc., and modified products thereof can also be used. Examples of polyaddition-type curing agents include polyamines, polymercaptans, polyphenols, acid anhydrides, etc.

[0047] When tertiary amines, imidazoles, etc. are blended as an anionically polymerizable catalytic curing agent, the epoxy resin is cured by heating at a medium temperature of about 160°C to 200°C for about several tens of seconds to several hours. Therefore, the pot life can be relatively long. As a cationic polymerizable catalytic curing agent, for example, a photosensitive onium salt (aromatic diazonium salt, aromatic sulfonium salt, etc.) that cures an epoxy resin by energy ray irradiation is preferable. In addition, aliphatic sulfonium salts, etc., are also available as agents that are activated by heating other than energy ray irradiation to cure an epoxy resin. This type of curing agent is preferable because it has the characteristic of fast curing.

[0048] These latent curing agents are preferably microencapsulated by coating with a polymeric substance such as polyurethane or polyester, a thin metal film such as nickel or copper, or an inorganic substance such as calcium silicate, since this extends the pot life.

[0049] The amount of the latent curing agent contained in the first composition is preferably 20 to 80 parts by mass, and more preferably 30 to 70 parts by mass, per 100 parts by mass of the epoxy resin and the film-forming material added as needed.

[0050] The radical polymerizable substance contained in the second composition is a substance having a functional group that polymerizes by radicals. Examples of such radical polymerizable substances include (meth)acrylate compounds, (meth)acryloxy compounds, maleimide compounds, citraconic imide resins, and nadimide resins. The radical polymerizable substance may be used in the form of a monomer or oligomer, and a monomer and an oligomer may be used in combination. In addition, a polymerization inhibitor such as hydroquinone or methyl ether hydroquinones may be used as necessary.

[0051] Specific examples of the (meth)acrylate compound include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, 2-hydroxy-1,3-di(meth)acryloxypropane, 2,2-bis[4-((meth)acryloxymethoxy)phenyl]propane, 2,2-bis[4-((meth)acryloxypolyethoxy)phenyl]propane, dicyclopentenyl (meth)acrylate, tricyclodecanyl (meth)acrylate, tris((meth)acryloyloxyethyl)isocyanurate, urethane (meth)acrylate, etc. These can be used alone or in combination of two or more.

[0052] From the viewpoint of improving heat resistance, the (meth)acrylate compound preferably has at least one substituent selected from the group consisting of a dicyclopentenyl group, a tricyclodecanyl group, and a triazine ring.

[0053] As the radical polymerizable substance other than the (meth)acrylate compound, for example, the compounds described in International Publication No. 2009 / 063827 can be suitably used. These can be used alone or in combination of two or more.

[0054] It is also preferable to use a radical polymerizable substance having a phosphate ester structure represented by the following general formula (I) in combination with the above radical polymerizable substance, which is suitable for bonding circuit electrodes together since the adhesive strength to inorganic surfaces such as metals is improved in this case.

[0055] [ka] [In the formula, n represents an integer of 1 to 3.]

[0056] The radical polymerizable substance having a phosphoric acid ester structure can be obtained by reacting phosphoric anhydride with 2-hydroxyethyl (meth)acrylate. Specific examples of the radical polymerizable substance having a phosphoric acid ester structure include mono(2-methacryloyloxyethyl) acid phosphate, di(2-methacryloyloxyethyl) acid phosphate, etc. These can be used alone or in combination of two or more.

[0057] The amount of the radical polymerizable substance having a phosphate ester structure represented by the above general formula (I) is preferably 0.01 to 50 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total of the radical polymerizable substance and the film-forming material added as necessary.

[0058] The radical polymerizable substance can be used in combination with allyl (meth)acrylate. In this case, the amount of allyl (meth)acrylate is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total of the radical polymerizable substance and the film-forming material added as necessary.

[0059] The curing agent contained in the second composition that generates free radicals upon heating is a curing agent that decomposes upon heating to generate free radicals. Examples of such curing agents include peroxides and azo-based compounds. Such curing agents are appropriately selected depending on the intended connection temperature, connection time, pot life, etc. From the viewpoint of high reactivity and improved pot life, organic peroxides having a 10-hour half-life temperature of 40°C or higher and a 1-minute half-life temperature of 180°C or lower are preferred, and organic peroxides having a 10-hour half-life temperature of 60°C or higher and a 1-minute half-life temperature of 170°C or lower are more preferred.

[0060] The amount of the curing agent may be 0.05 to 20 parts by mass, or 0.1 to 10 parts by mass, based on 100 parts by mass of the total of the radical polymerizable substance and the film-forming material that is added as required. When the conductive adhesive of the present embodiment is used as a circuit connecting material, the amount of the curing agent is preferably 1 to 10 parts by mass, and more preferably 2 to 8 parts by mass, based on 100 parts by mass of the total of the radical polymerizable substance and the film-forming material that is added as required. This makes it possible to obtain a sufficient reaction rate and reduce the connection time to 25 seconds or less.

[0061] Specific examples of the curing agent contained in the second composition that generates free radicals upon heating include diacyl peroxide, peroxydicarbonate, peroxyester peroxyketal, dialkyl peroxide, hydroperoxide, and silyl peroxide. In addition, when the conductive adhesive of this embodiment is used as a circuit connection material, from the viewpoint of suppressing corrosion of the circuit electrode, a curing agent containing chlorine ions and organic acids at a concentration of 5000 ppm or less is preferable, and a curing agent that generates less organic acid after thermal decomposition is more preferable. Specific examples of such a curing agent include peroxyester, dialkyl peroxide, hydroperoxide, and silyl peroxide, and a curing agent selected from peroxyesters that provide high reactivity is more preferable. The above curing agents can be used by mixing them appropriately.

[0062] Peroxyesters include cumyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, t-hexyl peroxyneodecanodate, t-butyl peroxypivalate, 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1-cyclohexyl-1-methylethyl peroxy-2-ethylhexanoate, t-hexyl peroxy-2-ethylhexanoate, and t-butyl peroxypivalate. Examples of the curing agent that generates free radicals by heating other than the above-mentioned peroxy esters include, for example, compounds described in International Publication No. 2009 / 063827. These may be used alone or in combination of two or more.

[0063] These curing agents can be used alone or in combination of two or more, and may be used in combination with a decomposition accelerator, decomposition inhibitor, etc. Furthermore, these curing agents may be microencapsulated by coating with a polyurethane or polyester polymeric substance, etc. Microencapsulated curing agents are preferred because they have an extended pot life.

[0064] Examples of the photocurable adhesive composition include compositions containing an epoxy resin or a radical polymerizable substance similar to those used in the above-mentioned thermosetting adhesive composition, and a photoinitiator.

[0065] The amount of the adhesive composition is preferably 70 to 99.9 parts by volume, more preferably 75 to 99.75 parts by volume, and even more preferably 80 to 99.5 parts by volume, when the total volume of the conductive adhesive is taken as 100 parts by volume. When the amount of the adhesive composition is within the above range, when the conductive adhesive of the present embodiment is used as a circuit connecting material, it becomes easier to ensure the strength and elastic modulus required to maintain the gap between electrodes during and after circuit connection and to provide excellent connection reliability.

[0066] The adhesive composition according to the present embodiment may be used by adding a film-forming material as necessary. The film-forming material is a material that, when the liquid is solidified to form the constituent composition into a film shape, makes the film easy to handle under normal conditions (room temperature and normal pressure) and imparts mechanical properties such as not easily tearing, cracking, or sticking to the film. Examples of the film-forming material include phenoxy resin, polyvinyl formal resin, polystyrene resin, polyvinyl butyral resin, polyester resin, polyamide resin, xylene resin, polyurethane resin, etc. Among these, phenoxy resin is preferred because of its excellent adhesion, compatibility, heat resistance, and mechanical strength.

[0067] The phenoxy resin is a resin obtained by reacting a bifunctional phenol with epihalohydrin until it is polymerized, or by polyaddition of a bifunctional epoxy resin with a bifunctional phenol. The phenoxy resin can be obtained, for example, by reacting 1 mole of a bifunctional phenol with 0.985 to 1.015 moles of epihalohydrin in a non-reactive solvent at a temperature of 40 to 120°C in the presence of a catalyst such as an alkali metal hydroxide. In addition, from the viewpoint of the mechanical properties and thermal properties of the resin, it is preferable to use a phenoxy resin obtained by polyaddition reaction in an organic solvent such as an amide, ether, ketone, lactone, or alcohol solvent having a boiling point of 120°C or more, heated to 50 to 200°C under the condition that the reaction solid content is 50 mass% or less, in a blending equivalent ratio of the bifunctional epoxy resin and the bifunctional phenol, i.e., epoxy group / phenol hydroxyl group=1 / 0.9 to 1 / 1.1, in the presence of a catalyst such as an alkali metal compound, an organic phosphorus compound, or a cyclic amine compound. The phenoxy resins may be used alone or in combination of two or more kinds.

[0068] Examples of the bifunctional epoxy resin include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD ​​type epoxy resin, bisphenol S type epoxy resin, biphenyl diglycidyl ether, methyl-substituted biphenyl diglycidyl ether, etc. The bifunctional phenol has two phenolic hydroxyl groups. Examples of the bifunctional phenol include hydroquinones, bisphenol A, bisphenol F, bisphenol AD, bisphenol S, bisphenol fluorene, methyl-substituted bisphenol fluorene, dihydroxybiphenyl, methyl-substituted dihydroxybiphenyl, and other bisphenols. The phenoxy resin may be modified (e.g., epoxy-modified) with a radically polymerizable functional group or other reactive compound.

[0069] The amount of the film-forming material blended is preferably 10 to 90 parts by mass, and more preferably 20 to 60 parts by mass, when the total mass of the conductive adhesive is 100 parts by mass.

[0070] The adhesive composition according to the present embodiment may further contain a polymer or copolymer containing at least one of acrylic acid, acrylic acid ester, methacrylic acid ester, and acrylonitrile as a monomer component. Here, the adhesive composition preferably contains a copolymer-based acrylic rubber containing glycidyl acrylate and / or glycidyl methacrylate containing a glycidyl ether group in combination, because such a copolymer has excellent stress relaxation properties. The weight-average molecular weight of such an acrylic rubber is preferably 200,000 or more in order to increase the cohesive strength of the adhesive composition.

[0071] The adhesive composition according to this embodiment may further contain rubber fine particles, fillers, softeners, accelerators, antioxidants, colorants, flame retardants, thixotropic agents, coupling agents, phenolic resins, melamine resins, isocyanates, and the like.

[0072] The rubber fine particles preferably have an average particle size of not more than twice the average particle size of the conductive particles to be blended, and a storage modulus at room temperature (25°C) of not more than half the storage modulus at room temperature of the conductive adhesive. In particular, when the material of the rubber fine particles is silicone, acrylic emulsion, SBR, NBR, or polybutadiene rubber, it is preferable to use them alone or in a mixture of two or more kinds. These three-dimensionally crosslinked rubber fine particles have excellent solvent resistance and are easily dispersed in the adhesive composition.

[0073] The filler can improve the connection reliability of the electrical properties between circuit electrodes when the conductive adhesive of this embodiment is used as a circuit connecting material. As the filler, for example, one whose average particle size is 1 / 2 or less of the average particle size of the conductive particles can be suitably used. In addition, when non-conductive particles are used in combination, any filler having an average particle size equal to or less than that of the non-conductive particles can be used.

[0074] The amount of the filler is preferably 5 to 60 parts by mass relative to 100 parts by mass of the conductive adhesive. When the amount is 60 parts by mass or less, the effect of improving connection reliability tends to be more sufficiently obtained, while when the amount is 5 parts by mass or more, the effect of adding the filler tends to be sufficiently obtained.

[0075] As the coupling agent, a compound containing an amino group, a vinyl group, an acryloyl group, an epoxy group or an isocyanate group is preferred since it improves the adhesiveness.

[0076] The conductive adhesive of the present embodiment can be suitably used as a circuit connecting material. The circuit connecting material melts and flows during connection to obtain a connection between opposing circuit electrodes, and then hardens to maintain the connection, and the fluidity of the circuit connecting material is an important factor. Examples of indicators showing this include the following. That is, when a circuit connecting material having a thickness of 35 μm and a size of 5 mm×5 mm is sandwiched between two glass plates having a thickness of 0.7 mm and a size of 15 mm×15 mm, and heated and pressed under conditions of 170° C., 2 MPa, and 10 seconds, the value of fluidity (B) / (A) expressed using the area (A) of the main surface of the circuit connecting material before heating and pressing and the area (B) of the main surface after heating and pressing is preferably 1.3 to 3.0, and more preferably 1.5 to 2.5. If it is 1.3 or more, the fluidity is suitable and there is a tendency that good connection is easily obtained, and if it is 3.0 or less, there is a tendency that bubbles are less likely to occur and reliability is more excellent.

[0077] When the conductive adhesive of this embodiment is used as a circuit connecting material, the elastic modulus of the cured conductive adhesive is preferably 100 to 3000 MPa, and more preferably 200 to 2000 MPa at 40° C. The elastic modulus of the cured conductive adhesive can be measured using, for example, a dynamic viscoelasticity measuring device (DVE, DMA, etc.).

[0078] When the conductive adhesive of the present embodiment is used as a circuit connecting material, the circuit connecting material is used to connect circuit electrodes to each other, and is preferably used for FOG (Flex on Glass) connection, FOF (Flex on Flex) connection, FOP (Flex on Polymer) connection, etc. Here, the FOG connection is a method of connecting a flexible substrate and an organic EL panel or an LCD panel, for example, represented by TCP, COF, and FPC, and refers to the connection between a circuit electrode formed on a flexible substrate and a circuit electrode formed on a glass substrate constituting an organic EL panel or an LCD panel. In addition, the FOF connection refers to the connection between a circuit electrode formed on a flexible substrate and a circuit electrode formed on a flexible substrate, and the FOP connection refers to the connection between a circuit electrode formed on a flexible substrate and a circuit electrode formed on a polymer substrate constituting an organic EL panel or an LCD panel.

[0079] The conductive adhesive of the present embodiment can also be formed into a film. Specifically, the above-mentioned predetermined components are dissolved in an organic solvent or the like to prepare a conductive adhesive-containing liquid containing an adhesive composition and conductive particles, which is then applied onto a film made of polyethylene terephthalate (PET) or the like using a coating device, and then a predetermined drying process is performed to obtain a film-like conductive adhesive. Such a conductive adhesive preferably has a thickness of 3 to 100 μm, more preferably 5 to 50 μm. When a film-like conductive adhesive having such a thickness is used as a circuit connection material, it is easy to ensure suitable circuit connectivity and handling properties.

[0080] The conductive adhesive of the present embodiment can be used as a circuit connecting material such as an anisotropic conductive adhesive.

[0081] <Circuit connection structure> The circuit connection structure of the present embodiment has a first circuit member having a first circuit electrode, a second circuit member having a second circuit electrode, and a connection portion interposed between the first circuit member and the second circuit member, the connection portion being made of the cured product of the conductive adhesive of the present embodiment described above.

[0082] In this embodiment, the circuit electrodes may be made of Ti, Al, Mo, Co, Cu, Cr, Sn, Zn, Ga, In, Ni, Au, Ag, V, Sb, Bi, Re, Ta, Nb, W, etc., but it is preferable that at least one of the first circuit electrode and the second circuit electrode has a layer containing Ti on the surface. Examples of such electrodes include an electrode having an Al layer and a layer containing Ti in this order from the substrate side, an electrode having a Ti layer, an Al layer, and a layer containing Ti in this order, an electrode having a Mo layer, an Al layer, and a layer containing Ti in this order, an electrode having an AlNd layer and a layer containing Ti in this order, etc.

[0083] Here, the layer containing Ti may be a layer containing at least Ti as a constituent element, a layer containing Ti as a main component as a constituent element, or a layer containing Ti alone (a layer made of Ti). Here, the "main component" refers to a component that is contained in an amount of 40 atm% or more of all the constituent elements. However, from the viewpoint of being able to fully exhibit the characteristics of the circuit connecting material described above, the layer containing Ti is preferably a layer containing at least 50 atm% Ti, and more preferably a layer containing 100 atm% Ti (a layer made of Ti).

[0084] The thickness of the circuit electrode is preferably 100 to 5000 nm, more preferably 100 to 2500 nm, from the viewpoint of balancing the connection resistance and the price. The lower limit can also be set to 500 nm. On the other hand, the thickness of the Ti-containing layer is preferably about 5 to 2000 nm, from the viewpoint of easily ensuring sufficient corrosion resistance, chemical stability, physical stability, gas barrier properties, and diffusion barrier properties.

[0085] The circuit connection structure of this embodiment can be produced by arranging a first circuit member having a first circuit electrode and a second circuit member having a second circuit electrode so that the first circuit electrode and the second circuit electrode face each other, interposing the conductive adhesive of this embodiment between the opposed first and second circuit electrodes, and thermocompression bonding the first and second circuit members to electrically connect the first and second circuit electrodes. Thus, the circuit connection material made of the conductive adhesive of this embodiment is useful as a material for bonding electrical circuits to each other.

[0086] More specifically, examples of the circuit members include chip components such as semiconductor chips, resistor chips, and capacitor chips, and substrates such as printed circuit boards. These circuit members are usually provided with a large number of the above-mentioned circuit electrodes (or may be a single electrode in some cases). At least some of the circuit electrodes are arranged to face each other, a circuit connection material made of the conductive adhesive of the present embodiment is interposed between the opposed circuit electrodes, and at least one set of the circuit members is heated and pressurized to electrically connect the opposed circuit electrodes. At this time, the opposed circuit electrodes are electrically connected to each other via the conductive particles contained in the conductive adhesive, while insulation between adjacent circuit electrodes is maintained. In this way, the circuit connection material made of the conductive adhesive of the present embodiment exhibits anisotropic conductivity.

[0087] Next, one embodiment of a method for producing a circuit connection structure will be described with reference to Fig. 3. Fig. 3 is a process cross-sectional view that typically illustrates a process for producing a circuit connection structure according to one embodiment of the present invention. Fig. 3(a) is a process cross-sectional view before circuit members are connected to each other, Fig. 3(b) is a process cross-sectional view when circuit members are connected to each other, and Fig. 3(c) is a process cross-sectional view after circuit members are connected to each other.

[0088] 3(a), a circuit member having a circuit electrode 2 and a circuit board 4 provided on an organic EL panel 3, and a circuit member having a circuit electrode 6 provided on a circuit board 5 are prepared. Then, a film-like circuit connecting material 1 is placed on the circuit electrode 2. The film-like circuit connecting material 1 is made of the conductive adhesive of this embodiment formed into a film shape.

[0089] 3(b), the circuit board 5 provided with the circuit electrode 6 is placed on the film-like circuit connecting material 1 while being aligned so that the circuit electrodes 2 and 6 face each other, and the film-like circuit connecting material 1 is interposed between the circuit electrodes 2 and 6. The circuit electrodes 2 and 6 have a structure in which a plurality of electrodes are arranged in the depth direction (not shown), and the circuit electrode 2 has a layer containing Ti on its surface (not shown).

[0090] The circuit connecting material 1 in this figure is in a film form and is therefore easy to handle. Therefore, this film-like circuit connecting material 1 can be easily interposed between the circuit electrode 2 and the circuit electrode 6, facilitating the connection work between the organic EL panel 3 and the circuit board 5.

[0091] Next, the film-like circuit connecting material 1 is pressed in the direction of arrow A in Fig. 3(b) between the organic EL panel 3 and the circuit board 5 while being heated, to carry out a curing treatment. This results in a circuit connection structure 20 in which the circuit members are connected to each other via a cured product 11 of the circuit connecting material, as shown in Fig. 3(c). As a method of curing treatment, one or both of heating and light irradiation can be adopted depending on the adhesive composition used.

[0092] In the manufacturing method of the circuit connection structure of this embodiment, a circuit connection material consisting of the conductive adhesive of this embodiment, which has a heat or light curing property, is formed on one electrode circuit, the surface of which is a metal selected from gold, silver, tin, and the platinum group, and then the other circuit electrode, the surface of which is titanium, is aligned and connected by heating and pressurization. EXAMPLES

[0093] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0094] (Preparation of conductive particles) Six types of conductive particles were prepared as shown in Table 1 below. These particles are core-shell particles with a plastic particle as the core and a metal layer, the main component of which is Ni, that covers the plastic particle as the shell. The average particle size of conductive particles No. 1 to 6 is 3 μm.

[0095] [Table 1]

[0096] <Measurement of 20% compression hardness of conductive particles> The compression hardness of the conductive particles was determined by the following procedure. A microcompression tester (Fischer HM2000, Fisher Instruments) was prepared, and conductive particles were scattered on a slide glass (product name: S1214, Matsunami Glass Industrial Co., Ltd.) on a stage set at a specified temperature (25°C, 150°C). One particle was selected from the slide glass and compressed from the center at a speed of 0.33 mN / sec with an initial load of 0.1 mN using a diamond indenter with a square base of 50 μm on a side, to obtain a stress-strain curve. The 20% compression hardness K value (20%) of the conductive particle was calculated from the following formula. K value (20%) = (3 / √2) × F 20 ×S 20 -3 / 2 ×R -1 / 2 ×10 -3 R: Radius of conductive particle (μm), S 20 : Mutation amount at 20% deformation, F 20 : Load when deformation rate is 20% (N)

[0097] <Measurement of compression recovery rate of conductive particles> The compression recovery rate of the conductive particles was determined by the following procedure. A microcompression tester (Fischer HM2000, Fisher Instruments) was prepared, and conductive particles were scattered on a slide glass (product name: S1214, Matsunami Glass Industrial Co., Ltd.) on a stage set at 25°C. One particle was selected from the sample and compressed with a diamond indenter with a square base of 50 μm on each side at a speed of 0.33 mN / sec from the center until a load of 5 mN was applied with an initial load of 0.1 mN. The load was then reduced to the initial load at a speed of 0.33 mN / sec. The relationship between the load and the compression displacement was measured. The displacement from the initial load (load 0.1 mN) to the load reversal (load 5 mN) was defined as L2, and the displacement from the load reversal to the final load (load 0.1 mN) was defined as L1, and the value of L1 / L2 × 100 (%) was calculated. This operation was carried out for 10 conductive particles, and the average value was taken as the compression recovery rate.

[0098] <Preparation of adhesive composition-containing liquid> (Preparation example A) A phenoxy resin was synthesized from a bisphenol A type epoxy resin and a phenolic compound (4,4'-(9-fluorenylidene)-diphenyl) having a fluorene ring structure in the molecule, and this resin was dissolved in a mixed solution of toluene and ethyl acetate (toluene / ethyl acetate = 50 / 50 (mass ratio)) to make a solution with a solid content of 40 mass%.

[0099] On the other hand, acrylic rubber (a copolymer of 40 parts by weight of butyl acrylate, 30 parts by weight of ethyl acrylate, 30 parts by weight of acrylonitrile, and 3 parts by weight of glycidyl methacrylate, with a weight average molecular weight of 800,000) was prepared as a rubber component, and this acrylic rubber was dissolved in a mixed solution of toluene and ethyl acetate (toluene / ethyl acetate = 50 / 50 (mass ratio)) to obtain a solution with a solid content of 15 mass %. In addition, a liquid curing agent-containing epoxy resin (epoxy equivalent: 202) containing a microencapsulated latent curing agent (a microencapsulated amine-based curing agent), a bisphenol F type epoxy resin, and a naphthalene type epoxy resin in a mass ratio of 34:49:17 was prepared.

[0100] The materials prepared above were mixed in a ratio of 20 g / 30 g / 50 g (by solid mass) of phenoxy resin / acrylic rubber / curing agent-containing epoxy resin to prepare adhesive composition-containing liquid A.

[0101] (Preparation example B) 50 g of phenoxy resin (product name: PKHC, manufactured by Union Carbide Corporation, weight average molecular weight 5000) was dissolved in a mixed solvent of toluene / ethyl acetate = 50 / 50 (mass ratio) to prepare a phenoxy resin solution with a solid content of 40 mass %.

[0102] On the other hand, 400 parts by mass of polycaprolactone diol having a weight average molecular weight of 800, 131 parts by mass of 2-hydroxypropyl acrylate, 0.5 parts by mass of dibutyltin dilaurate as a catalyst, and 1.0 part by mass of hydroquinone monomethyl ether as a polymerization inhibitor were mixed by heating to 50° C. while stirring. Next, 222 parts by mass of isophorone diisocyanate was dropped into this mixed liquid, and the temperature was raised to 80° C. while stirring to carry out a urethane reaction. After confirming that the reaction rate of the isocyanate group was 99% or more, the reaction temperature was lowered to obtain a urethane acrylate.

[0103] Next, the phenoxy resin solution was weighed out so that it contained 50 g of solids, and mixed with 30 g of the urethane acrylate, 15 g of an isocyanurate type acrylate (product name: M-215, manufactured by Toagosei Co., Ltd.), 1 g of a phosphate ester type acrylate (product name: P-1M, manufactured by Kyoeisha Chemical Co., Ltd.), and 4 g of benzoyl peroxide (product name: Niper BMT-K40, manufactured by NOF Corporation) as a free radical generator to prepare adhesive composition-containing liquid B.

[0104] <Preparation of circuit connection materials> Example 1 A circuit connecting material-containing liquid was prepared by dispersing 10 parts by mass of No. 1 conductive particles in 100 parts by mass of the adhesive composition-containing liquid A obtained above. This circuit connecting material-containing liquid was applied to a 50 μm-thick polyethylene terephthalate (PET) film with one surface-treated side using a coating device, and dried with hot air at 70° C. for 3 minutes to obtain a film-like circuit connecting material with a thickness of 20 μm on the PET film. When the total mass of the obtained circuit connecting material was taken as 100 parts by volume, the contents of the adhesive composition and conductive particles were 94 parts by volume and 6 parts by volume, respectively.

[0105] (Examples 2 to 3 and Comparative Examples 1 to 3) A film-shaped circuit connecting material was produced in the same manner as in Example 1, except that the type of conductive particles was changed as shown in Table 2.

[0106] Example 4 A circuit connecting material-containing liquid was prepared by dispersing 10 parts by mass of No. 1 conductive particles in 100 parts by mass of the adhesive composition-containing liquid B obtained above. This circuit connecting material-containing liquid was applied to a 50 μm-thick PET film with one surface-treated side using a coating device, and dried with hot air at 70° C. for 3 minutes to obtain a film-like circuit connecting material with a thickness of 20 μm on the PET film. When the total volume of the obtained circuit connecting material was taken as 100 parts by volume, the contents of the adhesive composition and conductive particles were 94 parts by volume and 6 parts by volume, respectively.

[0107] (Examples 5 to 6 and Comparative Examples 4 to 6) A film-shaped circuit connecting material was produced in the same manner as in Example 4, except that the type of conductive particles was changed as shown in Table 2.

[0108] <Evaluation of connection reliability> The film-like circuit connection material with the PET film obtained in the examples and comparative examples was cut to a predetermined size (width 1.5 mm, length 3 cm), and the adhesive surface was transferred to a glass substrate (thickness 0.7 mm) coated with titanium (film thickness 50 nm) and aluminum (film thickness 250 nm) in that order from the outermost surface by heating and pressing at 70 ° C. and 1 MPa for 2 seconds, and the PET film was peeled off. Next, a flexible circuit board (FPC) having 800 tin-plated copper circuits with a pitch of 25 μm and a thickness of 8 μm was placed on the transferred circuit connection material, and the FPC was temporarily fixed on the glass substrate by pressing at 24 ° C. and 0.5 MPa for 1 second. Next, this was placed in a main pressure bonding device, and a 200 μm thick silicone rubber sheet was used as a cushioning material, and the FPC side was connected over a width of 1.5 mm by heating and pressing at 170 ° C. and 4.5 MPa for 6 seconds with a heat tool to obtain a circuit connection structure. The resistance between adjacent circuits of the FPC including the connection of this circuit connection structure was measured using a multimeter (device name: TR6845, manufactured by Advantest Corporation). The resistance between adjacent circuits was measured at 32 points and the average value was calculated, which was used as the initial connection resistance. In addition, the members after measurement were treated under conditions of 85°C and 85% RH for 250 hours, and the connection resistance after high temperature and humidity treatment was measured in the same manner. At this time, the resistance increase rate from the initial connection resistance was also calculated. The results are shown in Table 2.

[0109] [Table 2]

[0110] As shown in Table 2, the circuit connecting materials obtained in the Examples exhibited lower resistance than the circuit connecting materials obtained in the Comparative Examples, and also showed a small increase in connection resistance even after high-temperature, high-humidity treatment, demonstrating excellent connection reliability. [Explanation of symbols]

[0111] Reference Signs List 1: circuit connecting material; 2, 6: circuit electrodes; 3: organic EL panel; 4, 5: circuit board; 11: cured product of circuit connecting material; 20: circuit connecting structure.

Claims

1. The adhesive composition includes conductive particles, the conductive particles are core-shell particles including plastic particles made of a resin obtained by copolymerizing a non-crosslinkable monomer having an ethylenically unsaturated group with a crosslinkable monomer having an ethylenically unsaturated group, and a metal layer coating the plastic particles; The conductive adhesive, wherein the conductive particles have a compression hardness of 10.0 GPa or more at 25°C and 3.5 GPa or less at 150°C when compressed by 20%.

2. The conductive adhesive according to claim 1, wherein the conductive particles have a compression recovery rate of 50 to 75% at 25°C.

3. The conductive adhesive according to claim 1 or 2, wherein the conductive particles have an average particle size of 2 μm or more and 10 μm or less.

4. Used to connect circuit electrodes together, The conductive adhesive according to any one of claims 1 to 3, wherein the connection is a Flex on Glass connection, a Flex on Flex connection, or a Flex on Polymer connection.

5. A method for manufacturing a circuit connection structure, comprising the steps of: interposing the conductive adhesive according to any one of claims 1 to 4 between a first circuit member having a first circuit electrode and a second circuit member having a second circuit electrode; and thermocompression bonding the first circuit member and the second circuit member to electrically connect the first circuit electrode and the second circuit electrode.

6. The method for producing a circuit connection structure according to claim 5 , wherein at least one of the first circuit electrode and the second circuit electrode has a layer containing Ti on a surface thereof.

7. a first circuit member having a first circuit electrode, a second circuit member having a second circuit electrode, and a connection portion interposed between the first circuit member and the second circuit member; A circuit connection structure, wherein the connection portion is a cured product of the conductive adhesive according to any one of claims 1 to 4.

8. 8. The circuit connection structure according to claim 7, wherein at least one of the first circuit electrode and the second circuit electrode has a layer containing Ti on a surface thereof.

Citation Information

Patent Citations

  • Circuit connecting material and connection structure of circuit terminal using the same

    JP2003323813A

  • Conductive fine particle and anisotropic conductive material

    JP2006196411A

  • Conductive fine particulate and anisotropic conductive material

    JP2012064559A

  • Electroconductive particulates and anisotropic electroconductive material using the same

    JP2014207193A

  • Circuit connection material and circuit connection structure

    JP2016001562A