Aluminum alloy sheet for can top
The aluminum alloy plate with controlled Si, Fe, Cu, Mn, and Mg compositions addresses the challenge of combining strength and toughness in can lids, enabling efficient use of recycled materials and reducing emissions.
Patent Information
- Application Number
- JP2023067145
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Conventional aluminum alloy plates for can lids, particularly those with compositions similar to 3104 aluminum alloy, face challenges in achieving both high strength and toughness, leading to issues with pressure resistance and formability, especially in positive-pressure cans, and require more new metal usage, contributing to higher CO2 emissions.
An aluminum alloy plate with specific compositions of Si, Fe, Cu, Mn, and Mg, along with optional Ti, Zn, and Cr, within defined ranges, ensuring a minimum yield strength and tensile strength across different directions, allowing for blending with 3104 alloy scraps, reducing new metal use and enhancing pressure resistance and toughness.
The alloy achieves high strength and toughness, enabling effective use of recycled materials, reducing CO2 emissions, and ensuring adequate pressure resistance without increasing thickness, thus improving formability and reducing material waste.
Smart Images

Figure 2024153327000005 
Figure 2024153327000006 
Figure 2024153327000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an aluminum alloy sheet for can ends. [Background technology]
[0002] In recent years, with growing environmental awareness, CO 2 There is a demand for aluminum alloy sheets with low CO emissions. 2 The indirect and major contributor to these emissions is the blending of new aluminum ingots in the casting process.
[0003] The production of primary aluminum ingots uses a large amount of electricity during the refining process and emits large amounts of CO 2 Therefore, reducing the amount of virgin aluminum used and increasing the horizontal recycling rate will reduce CO emissions in the manufacture of aluminum alloy sheets. 2 This will lead to reduced emissions.
[0004] Generally, CO emissions from aluminum scrap remelted and cast 2 It is said that emissions can be reduced to about one-thirtieth of those emitted when producing new aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used around the world is extremely large, and further improving the horizontal recycling rate for these cans is of great significance in reducing the environmental impact.
[0005] Among these, can ends made of 5182 aluminum alloy (AA5182 alloy) have lower upper limits for the composition standards of Si, Fe, Cu, Mn, etc. than can bodies made of 3104 aluminum alloy (AA3104 alloy), making it difficult to mix scrap derived from can materials that contain 3104 aluminum alloy.
[0006] For example, if can scrap (UBC: Used Beverage Can) generated in the city is mixed as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will easily exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.
[0007] Therefore, compared to aluminum alloy sheets for can bodies, aluminum alloy sheets for can ends use more virgin metal and have the composition adjusted to 5182 aluminum alloy, resulting in a low recycling rate. Therefore, by changing can ends to alloys whose composition is easily mixed with 3104 aluminum alloy, the usage rate of virgin metal for can ends can be significantly reduced.
[0008] Patent Documents 1 to 5 disclose aluminum alloy sheets for can ends that have compositions relatively close to those of 3104 aluminum alloy, which has excellent recyclability. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2001-73106 A [Patent Document 2] Japanese Patent Application Publication No. 9-070925 [Patent Document 3] Japanese Patent Application Publication No. 11-269594 [Patent Document 4] JP 2000-160273 A [Patent Document 5] JP 2016-160511 A Summary of the Invention [Problem to be solved by the invention]
[0010] The challenge in making the alloy for can lids closer to the 3104 aluminum alloy is that it reduces the pressure resistance of the can lids and the toughness of the material. The pressure resistance of a can lid is the internal pressure value when the can lid is inverted against the pressure inside the can, and is the resistance value when the internal pressure of the can increases unexpectedly due to a change in the external environment.
[0011] In particular, positive pressure cans for beer and carbonated beverages require high pressure resistance. Generally, the stronger the material and the thicker the plate, the higher the pressure resistance. For this reason, the lids of positive pressure cans are made of high-strength 5182 aluminum alloy, which contains a lot of Mg, an element that contributes to increased strength.
[0012] In contrast, if the conventional 3104 aluminum alloy is used for can lids, the pressure resistance is significantly reduced, and there is a high possibility that the lid will invert and leak contents if the internal pressure of the can suddenly increases. Also, if the plate thickness is increased to increase the pressure resistance, this will lead to an increase in the weight and cost of the lid.
[0013] Furthermore, the toughness of the material affects the formability and openability of the lid. If the material has low toughness, forming cracks may occur, especially in the rivet and countersink parts of the lid. Also, if the internal pressure of the can suddenly increases, cracks may occur in the score area, increasing the risk of the contents of the can leaking. In particular, these cracks occur along the rolling direction. Therefore, toughness against tensile stress and bending stress in the direction perpendicular to the rolling direction is required.
[0014] However, aluminum alloy sheets for can ends that have a composition relatively close to that of the conventional 3104 aluminum alloy do not satisfy either or both of the above two issues, namely, material strength (i.e., pressure resistance of the end) and toughness (i.e., formability and openability).
[0015] An object of one aspect of the present disclosure is to provide an aluminum alloy sheet for can ends that can achieve both high strength and high toughness while incorporating scrap raw material derived from can stock. [Means for solving the problem]
[0016] In one embodiment of the present disclosure, the silicon (Si) content is 0.20 mass% or more and 0.47 mass% or less, the iron (Fe) content is 0.30 mass% or more and 0.59 mass% or less, the copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, the manganese (Mn) content is 0.70 mass% or more and 0.98 mass% or less, the magnesium (Mg) content is 1.1 mass% or more and 3.7 mass% or less, and the balance is aluminum (Al) and unavoidable impurities, and the 0.2% proof stress σ 0.2 , tensile strength σ B , and the average value of 0.2% yield strength and tensile strength σ fm Among the evaluation values S calculated by the following formula (1) using min The aluminum alloy sheet for can ends has a compressive strength of 330 MPa or more and 410 MPa or less. S = σ fm / (σ 0.2 / σ B ) ···(1)
[0017] According to this configuration, it is possible to achieve both high strength and high toughness in the aluminum alloy sheet while blending scrap raw material derived from can materials. In other words, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, reduce the usage rate of new ingots, and reduce CO 2 Furthermore, it is possible to obtain an aluminum alloy sheet for can ends having high formability and usable for positive pressure can ends which require high pressure resistance. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is an explanatory diagram of the L-ST cross section. [Diagram 2] FIG. 2 is a graph showing an example of the relationship between the cold rolling rate and the strength anisotropy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, embodiments to which the present disclosure is applied will be described with reference to the drawings. [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for can ends (hereinafter also simply referred to as "alloy sheet") of the present disclosure contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn) and magnesium (Mg).
[0020] The lower limit of the Si content is 0.20 mass%, preferably 0.30 mass%. If the Si content is less than 0.20 mass%, the amount of Si precipitated in the processing heat of the hot rolling and the cold rolling after the solution treatment decreases, and the strength of the alloy sheet may be insufficient.
[0021] In addition, the average Si content standard of 3104 aluminum alloy specified in JIS-H-4000: 2014 is 0.30 mass%. Therefore, by making the Si content 0.30 mass% or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0022] The upper limit of the Si content is 0.47 mass%, preferably 0.39 mass%, and more preferably 0.35 mass%. When the Si content exceeds 0.47 mass%, Mg 2 The amount of Si particles increases, and the toughness of the alloy plate decreases.
[0023] The lower limit of the Fe content is 0.30 mass%, and preferably 0.40 mass%. The average value of the Fe content standard of the 3104 aluminum alloy is 0.40 mass%. Therefore, by making the Fe content 0.40 mass% or more, a large amount of 3104 aluminum alloy scrap can be blended.
[0024] The upper limit of the Fe content is 0.59 mass%. If the Fe content exceeds 0.59 mass%, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, a crack propagation path is generated, and the toughness of the alloy plate decreases.
[0025] The lower limit of the Cu content is 0.11 mass%, preferably 0.15 mass%, and more preferably 0.20 mass%. If the Cu content is less than 0.11 mass%, the Cu that increases the strength by solid solution or precipitation is insufficient, and the strength of the alloy sheet is reduced. Note that, by precipitating Cu in the processing of hot rolling and cold rolling after solution treatment, the strength of the alloy sheet is significantly increased.
[0026] In addition, the average Cu content standard of 3104 aluminum alloy is 0.15 mass%, so by making the Cu content 0.15 mass% or more, it is possible to mix a large amount of 3104 aluminum alloy scrap.
[0027] The upper limit of the Cu content is 0.40 mass%, and preferably 0.25 mass%. If the Cu content exceeds 0.40 mass%, the toughness of the alloy plate decreases.
[0028] The lower limit of the Mn content is 0.70 mass%, and preferably 0.75 mass%. If the Mn content is less than 0.70 mass%, the Mn that increases the strength by solid solution or precipitation is insufficient, and the average strength of the alloy plate decreases.
[0029] In addition, the average value of the Mn content standard for 3104 aluminum alloy is 1.1 mass%, and the average value of the Mn content standard for 5182 aluminum alloy is 0.35 mass%. Therefore, by making the Mn content 0.75 mass% or more, it is possible to mix more 3104 aluminum alloy scrap than the conventional 5182 aluminum alloy.
[0030] The upper limit of the Mn content is 0.98 mass%, and preferably 0.90 mass%. If the Mn content exceeds 0.98 mass%, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, a crack propagation path is generated, and the toughness of the alloy plate decreases.
[0031] The lower limit of the Mg content is 1.1 mass%, preferably 1.4 mass%. If the Mg content is less than 1.1 mass%, the Mg that increases the strength by solid solution is insufficient, and the average strength of the alloy sheet is reduced. Note that the strength of the alloy sheet is significantly increased by precipitating Mg during the processing of hot rolling and cold rolling after the solution treatment.
[0032] The upper limit of the Mg content is 3.7% by mass, and preferably 3.1% by mass. The average value of the Mg content standard of 3104 aluminum alloy is 1.05% by mass, and the average value of the Mg content standard of 5182 aluminum alloy is 4.5% by mass. Therefore, by setting the Mg content to 3.7% by mass or less, it is possible to mix a large amount of 3104 aluminum alloy scrap while reducing the amount of additional Mg-containing raw material.
[0033] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10 mass%. The ingot structure of the alloy plate is refined by including Ti. The alloy plate may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass%. Furthermore, the alloy plate may contain chromium (Cr). The upper limit of the Cr content is preferably 0.10 mass%.
[0034] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, Mg, Ti, Zn, and Cr in the above-mentioned ranges, with the balance being aluminum and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%.
[0035] <Material strength and pressure resistance> Rolled aluminum alloy plates are anisotropic materials, and their strength varies in the directions of 0°, 45°, and 90° to the rolling direction. When the pressure inside the can increases, deformation begins in the direction with the lowest strength.
[0036] Therefore, the alloy sheet of the present disclosure has a 0.2% yield strength σ 0.2 , tensile strength σ B , and the average value of 0.2% yield strength and tensile strength σ fm The evaluation value S (S 0° , S 45° , and S 90° ) the minimum evaluation value S min (=min(S 0° ,S 45° ,S 90° ) is 330 MPa or more and 410 MPa or less. S = σ fm / (σ 0.2 / σ B ) ···(1)
[0037] The pressure resistance of the lid made of aluminum alloy plate is the empirically minimum evaluation value S min and the plate thickness t, the value V of the following equation (2) is strongly positively correlated with V=t 2.27 ×S min (2)
[0038] Therefore, the minimum evaluation value S of the alloy plate min By setting the minimum evaluation value S to 330 MPa or more, a lid with sufficient pressure resistance can be formed without increasing the plate thickness. min The minimum evaluation value S is preferably 360 MPa or more. min By setting the pressure to 360 MPa or more, the pressure resistance of the lid can be further improved.
[0039] In addition, the minimum evaluation value S min If the stress exceeds 410 MPa, the material strength becomes excessively high, and the toughness of the material decreases. In other words, shear bands are more likely to occur due to the tensile stress and bending stress that occur in the material during forming, and forming cracks are more likely to occur. min By setting the pressure to 410 MPa or less, it is possible to achieve both the strength of the material (i.e., the pressure resistance of the lid) and the toughness (i.e., the formability and openability).
[0040] 0.2% proof stress σ in formula (1) 0.2 and tensile strength σ B is measured by the method specified in JIS-Z-2241: 2011. The plate thickness t is measured, for example, with a micro gauge.
[0041] <Toughness> It is known that the formability of the lid and the force required to open the score portion (i.e., opening force) are affected by the toughness of the aluminum alloy plate.
[0042] (Number of repeated bending) A repeated bending test is one of the evaluation indices for the toughness of an aluminum alloy plate. If the plate thickness is the same, the more repeated bending times the aluminum alloy plate is subjected to, the more excellent the toughness of the aluminum alloy plate is.
[0043] The repeated bending test is carried out as follows. For example, a test piece cut into a rectangular shape with a width of 12.5 mm and a length of 200 mm is placed so that the bending ridgeline is parallel to the rolling direction of the alloy plate. Both ends of the test piece are fixed with chucks, and a tension of 200 N is applied.
[0044] In this state, the test piece is repeatedly bent by rotating the other chuck 90° left and right, using a jig with a bending radius of 2.0 mm positioned 150 mm in the longitudinal direction of the test piece as a fulcrum from the end of the test piece fixed to one of the immovable chucks, and the number of bends until the test piece breaks is measured.
[0045] The number of bending times is counted as one bending operation to the left or right by 90° and returning to the original position. If the wire breaks during bending, the angle Θ (0°-90°) is read and the number of repeated bending times N is calculated using the following formula (3). In formula (3), N 0 is the total number of times that the test specimen is bent 90° to either side and then returned to its original 0° position before it breaks. N=N 0 +Θ / 90 ···(3)
[0046] Repeated bending evaluation is disadvantageous as the plate thickness increases, so it is necessary to correct for the standard plate thickness. Therefore, the normalized repeated bending times N was normalized by the following formula (4) using a plate thickness of 0.235 mm as the standard. s Here, t (mm) is the thickness of the test piece. N s = N × t / 0.235 (4)
[0047] Standardized repeated bending number N of the aluminum alloy plate of the present disclosure s Preferably, the number is 18 or more.
[0048] (second phase particles) Toughness is affected by strength and the distribution of second phase particles. In other words, the higher the strength and the higher the density of the second phase particles, the lower the toughness. In particular, when the Mg and Si contents are high, the Mg 2 Si particles are easily formed. As a result, Mg 2 The Si particles act as the initiation points and propagation paths of cracks, which leads to a decrease in toughness.
[0049] In the aluminum alloy sheet of the present disclosure, the area of the L-ST cross section in the width direction central portion shown by the diagonal line in FIG. 2 More than Mg 2 The ratio of the total area of the Si particles in the L-ST cross section is preferably 0.2% or less. In Fig. 1, L indicates the longitudinal direction, ST indicates the plate thickness direction, and LT indicates the width direction.
[0050] Mg 2 The area ratio of Si particles can be measured, for example, by the following method. First, the measurement sample is cut and the surface to be measured (i.e., the L-ST cross section) is mechanically polished to a mirror finish. Next, the polished surface (i.e., the L-ST cross section) is observed using a SEM (scanning electron microscope) to obtain 10 fields of view in the central region of the plate thickness. The accelerating voltage of the SEM is 15 kV, the magnification is 1000 times, and the range of one field of view is 0.012 mm 2 The image is then taken and a COMPO (backscattered electron composition) image is obtained.
[0051] The captured COMPO image was analyzed using the image analysis software "ImageJ". Specifically, the most frequent brightness value of the image in 256 gradations was taken as the background brightness, and particles with brightness lower than the brightness of the most frequent value minus 30 were determined as Mg. 2 It is determined to be a Si particle.
[0052] Determined Mg 2 Of the Si particles, 0.3 μm 2 The total area of particles with an area of 0.3 μm or more was calculated and divided by the area of 10 fields of view (i.e., the total area photographed). 2 More than Mg 2 The percentage of the total area of the Si particles in the L-ST cross section is calculated.
[0053] <Calculation of phase diagrams using computer software> In the alloy plate disclosed in the present disclosure, in order to increase the toughness of the material, Mg, which acts as a crack initiation point and propagation path and affects the decrease in toughness, is used. 2 It is preferable that the Si particles are redissolved in a homogenization heat treatment step of the ingot.
[0054] While avoiding local melting of the aluminum matrix, Mg 2 In order to redissolve Si, the solidus temperature must be higher than Mg 2 It is preferable that the temperature is higher than the solidus temperature of Si, and that the temperature is higher than the solidus temperature of Mg. 2 It is preferable that the temperature difference minus the solid solution temperature of Si is 30° C. or more.
[0055] In addition, Al 6 In materials where the crystallization temperature of (Mn,Fe) is higher than the solidification temperature of aluminum, Al 6 The formation of coarse crystals of (Mn,Fe) leads to molding defects such as pinholes. Therefore, the primary crystal (i.e. Al) is formed at a temperature higher than the solidification start temperature of aluminum. 6 It is preferable that the crystallization temperature of (Mn,Fe) is low.
[0056] The Mg 2 The solid solution temperature of Si is the equilibrium phase diagram of Mg 2It is the highest temperature at which Si can exist, and the lowest temperature at which a liquid phase can exist. The solidification temperature of aluminum is the highest temperature at which solid Al can exist in the equilibrium diagram, and the crystallization temperature of the primary crystal is the lowest temperature at which Al 6 This is the highest temperature at which (Mn,Fe) can exist.
[0057] Mg 2 The solution temperature of Si, the solidus temperature, the solidification start temperature of aluminum, and the crystallization temperature of the primary crystals can be obtained from the equilibrium phase diagram of the aluminum alloy calculated using thermodynamic calculation software.
[0058] Mg 2 The solution temperature of silicon, the solidus temperature, the solidification start temperature of aluminum, and the crystallization temperature of the primary crystal are uniquely determined by the composition of the aluminum alloy. One method for determining these boundary temperatures from the alloy composition is to calculate the thermodynamic quantities required for each calculation using the CALPHAD method.
[0059] Such thermodynamic calculations for multi-component alloys can be performed using commercially available system software (e.g., "JMatPro" developed by Sente Software) that combines the thermodynamic database, interface, and phase diagram creation functions required for the calculations.
[0060] In the aluminum alloy plate of the present disclosure, Mg 2 Since the solution temperature of Si is low and the crystallization temperature of the primary crystals is lower than the solidification start temperature of Al, no coarse crystals are generated during casting, and the performance degradation caused by coarse crystals can be avoided.
[0061] In addition, below the solidus temperature and Mg 2 By homogenizing heat treatment at a temperature above the solid solution temperature of Si, Mg 2 Mg redissolves Si, which acts as a crack initiation point and propagation path, and affects the decrease in toughness. 2 The amount of Si particles can be reduced.
[0062] <Strength anisotropy> It is known that materials with low cold rolling reductions (hereafter referred to as cold rolling reductions) have high toughness. For example, a material in which a rolled sheet is annealed in a continuous annealing furnace (CAL) during cold rolling to reduce the final cold rolling reduction (i.e., the cold rolling reduction after annealing) has high toughness.
[0063] In addition, the higher the cold rolling ratio, the higher the 0.2% yield strength σ 0.2_90° 0.2% yield strength σ in the 0° direction 0.2_0° Therefore, the difference in 0.2% yield strength between the 0° direction and the 90° direction with respect to the rolling direction, that is, the strength anisotropy, can be associated with the cold rolling rate of the material.
[0064] The alloy sheet of the present disclosure has a 0.2% yield strength σ in the 0° direction relative to the rolling direction, which is calculated by the formula (5). 0.2_0° From the above, the 0.2% yield strength σ 0.2_90° It is preferable that the value D obtained by subtracting this is in the range of -13 MPa to 13 MPa. D=σ 0.2_0° -σ 0.2_90° (5)
[0065] 0.2% proof stress σ in the 0° direction to the rolling direction 0.2_0° From the above, the 0.2% yield strength σ 0.2_90° The material structure meaning of the strength anisotropy minus can be explained as follows.
[0066] After hot rolling or annealing, the material is in a recrystallized state, with a high concentration of isotropic cube orientation. From here, the plastic deformation caused by cold rolling transforms the cube orientation into a rolling texture with anisotropy in the rolling direction. Furthermore, the larger the cold rolling rate, the more the crystal grains are elongated in the rolling direction, so the diameter of the crystal grains aligned at 0° to the rolling direction becomes larger, while the change in the diameter of the crystal grains aligned at 90° to the rolling direction becomes smaller than in the 0° direction.
[0067] The structural changes caused by these rolling processes and the 0.2% yield strength σ 0.2The relationship between these two can be expressed by the Hall-Petch equation as shown in Equation (6): In Equation (6), κ is the resistance to grain boundary sliding, and d is the grain size. σ 0.2 ∝κ×d -1 / 2 (6)
[0068] The resistance κ is different when tension is applied in the 0° or 90° direction to the rolling direction. This is because the resistance to grain boundary slippage changes depending on the tension direction as the cold reduction rate increases and the degree of integration of the rolling texture, which has anisotropy in the rolling direction, increases.
[0069] In addition, while the grains elongate and their diameter increases with increasing cold rolling in the 0° direction, the change in grain size with increasing cold rolling is relatively small in the 90° direction. The cumulative effect of these effects results in strength anisotropy with increasing cold rolling.
[0070] <Method of manufacturing aluminum alloy plate> The aluminum alloy plate of the present disclosure can be produced, for example, as follows: First, an aluminum alloy having the composition of the aluminum alloy plate of the present disclosure is subjected to semi-continuous casting (i.e., DC casting) according to a conventional method to produce an ingot.
[0071] Next, the four faces of the ingot, excluding the front and rear ends, are chamfered. After that, the ingot is placed in a soaking furnace and subjected to homogenization treatment. The temperature in the homogenization treatment is preferably, for example, 470°C or higher and 620°C or lower. The time for the homogenization treatment is preferably, for example, 1 hour or higher and 20 hours or lower.
[0072] When the homogenization temperature is 400°C or higher, it is easy to eliminate segregation in the ingot structure. Furthermore, when the homogenization temperature is 450°C or higher, Mg 2 The homogenization treatment temperature is preferably 470°C or higher, and more preferably Mg 2 When the temperature is above the solid solution temperature of Si, Mg 2The redissolution of Si particles is promoted, and the strength and toughness of the alloy plate can be further improved. On the other hand, when the temperature in the homogenization treatment is 620° C. or lower, more preferably the solidus temperature or lower, local melting of the aluminum alloy is unlikely to occur.
[0073] If the homogenization treatment time is 1 hour or more, the temperature of the entire slab becomes uniform, segregation of the ingot structure is easily eliminated, and Mg 2 The longer the homogenization time, the easier it is to redissolve the Si particles. 2 The silicon particles can be redissolved. However, if the homogenization treatment time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.
[0074] After the homogenization treatment, the ingot is subjected to hot rolling. The hot rolling process includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of mm by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several mm by, for example, tandem rolling, and the plate material is wound into a coil to form a hot rolled coil.
[0075] If the total reduction rate of the finish rolling is high, the recrystallized structure will be formed after coiling, and the concentration of the isotropic cube orientation can be increased. If the coiling temperature of the finish rolling is high, the recrystallized structure will be formed after coiling, and the concentration of the cube orientation can be increased.
[0076] Following hot rolling, the plate material is cold rolled. In cold rolling, the hot rolled coil is rolled until the product plate thickness is reached. Cold rolling may be either single rolling or tandem rolling. In single cold rolling, rolling is preferably performed in multiple passes, such as two or more passes.
[0077] In addition, by subjecting the coil to solution treatment during cold rolling and resolving Mg and other elements, it is possible to obtain an alloy sheet with high strength and reduced anisotropy by lowering the final cold rolling rate. For example, by using a continuous annealing furnace (CAL) to perform heat treatment (i.e. annealing) at a target actual temperature of 440°C or higher, and then forcibly cooling by air cooling, it is possible to effectively increase the strength of the alloy sheet.
[0078] In addition, by setting the finishing temperature of cold rolling in the intermediate passes other than the final pass to 120°C or higher, Si, Cu and Mg are finely precipitated and age hardened, so that the strength of the alloy sheet can be increased. Furthermore, by setting the finishing temperature to 130°C or higher, the strength of the alloy sheet can be further increased.
[0079] If no solution treatment is performed during cold rolling, the cold rolling rate is preferably 80% or more. When the cold rolling rate is 80% or more, the strength of the alloy sheet can be increased. In addition, the lower the cold rolling rate, the more isotropic cube orientation remains, so the cold rolling rate is preferably 92% or less.
[0080] When performing solution treatment during cold rolling, the cold rolling rate after solution treatment (i.e. annealing) is preferably 50% or more. By resolving Mg and other elements through solution treatment, the strength of the alloy sheet can be increased even with a low cold rolling rate. In addition, the lower the cold rolling rate, the more isotropic cube orientation remains, so the cold rolling rate is preferably 80% or less.
[0081] The cold rolling rate R (%) is the thickness t after hot rolling or solution treatment. 0 (mm), product thickness after cold rolling t 1 Using the distance (mm), it can be calculated using the following formula (7). R = (t 0 -t 1 ) / t 0 ×100 ···(7)
[0082] The product thickness can be appropriately selected so as to obtain a desired pressure resistance. As shown in the above formula (2), the pressure resistance improves as the thickness increases. The product thickness can be selected according to the value V of formula (2), and is preferably under the condition that the value V is 13.0 or more, preferably 14.0 or more. As described above, according to the aluminum alloy sheet of the present disclosure, it is possible to suppress an increase in the thickness in order to maintain a high pressure resistance.
[0083] After the coils have been cold-rolled to the product thickness, they are pre-coated in a painting line, etc. The surface of the cold-rolled coils is degreased, cleaned, and chemically treated, and then painted, after which the paint is baked.
[0084] In chemical conversion treatment, chromate-based, zirconium-based, or other chemicals are used. Epoxy-based, polyester-based, or other paints are used. These can be selected according to the application. In paint baking treatment, the coil is heated to a peak metal temperature (PMT) of 220°C to 270°C for approximately 30 seconds or less. The lower the PMT, the more the material recovery is suppressed, and the higher the strength of the alloy plate can be maintained.
[0085] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained. (1a) It is possible to achieve both high strength and high toughness of aluminum alloy plate while blending scrap raw materials derived from can materials. In other words, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, reduce the usage rate of new ingots, and reduce CO 2 Furthermore, it is possible to obtain an aluminum alloy sheet for can ends having high formability and usable for positive pressure can ends which require high pressure resistance.
[0086] 2. Other embodiments Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take various forms.
[0087] (2a) In addition to the aluminum alloy sheet of the above embodiment, the present disclosure also includes various embodiments of a member constituted by this aluminum alloy sheet, a manufacturing method of this aluminum alloy sheet, and the like.
[0088] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. In addition, a part of the configuration of the above embodiments may be omitted. In addition, at least a part of the configuration of the above embodiments may be added to or substituted for the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified from the wording of the claims are embodiments of the present disclosure.
[0089] 3. Working Examples The following describes the tests conducted to confirm the effects of the present disclosure and the evaluation results thereof.
[0090] <Production of aluminum alloy sheets> As examples and comparative examples, aluminum alloy sheets S1 to S17 shown in Tables 1 and 2 were produced. Specific production procedures are described below.
[0091] First, an ingot containing the components (% by mass) of Alloy Nos. 1-9 shown in Table 3, with the balance being aluminum and unavoidable impurities, was produced by semi-continuous casting. The ingot contained 0.10% by mass or less of Ti, 0.25% by mass or less of Zn, 0.10% by mass or less of Cr, and 0.15% by mass or less of unavoidable impurities.
[0092] Next, the four sides of the ingot, excluding the front and rear ends, were chamfered. The ingot was then placed in a furnace and subjected to homogenization treatment. The homogenization temperature is shown in Table 1. After the homogenization treatment, the ingot was removed from the furnace and immediately hot rolling was started to produce a rolled sheet.
[0093] Furthermore, for S1-S7, S14, S15, and S17, the rolled sheets after hot rolling were cold rolled until they reached the CAL thickness shown in Table 1. The rolled sheets with the CAL thickness were then annealed in a continuous annealing furnace (CAL). The CAL temperature during annealing is shown in Table 1. After annealing, the rolled sheets were air-cooled to room temperature. After cooling, the rolled sheets were cold-rolled again. The target cold reduction ratio in cold rolling after annealing is shown in Table 1.
[0094] For S8-S13 and S16, the hot-rolled sheets were cold-rolled without annealing. The target cold rolling reduction ratios are shown in Table 1.
[0095] The thickness of the product after cold rolling in S1-S17 (i.e., t in Eq. (7)) 1 ) was in the range of approximately 0.235±0.03 mm.
[0096] For S1-S17, after cold rolling, paint was applied to the sheet surface and a paint baking treatment was performed for about 30 seconds. The practical temperature (PMT) during paint baking is as shown in Table 1. The aluminum alloy sheets S1-S17 were obtained by baking the paint. The sheet thickness (i.e., product sheet thickness) of the aluminum alloy sheets S1-S17 measured by a microgauge is also shown in Table 1.
[0097] [Table 1]
[0098] [Table 2]
[0099] [Table 3]
[0100] <Evaluation of aluminum alloy sheets> (Tensile properties) Three No. 5 test pieces as specified in JIS-Z-2241:2011 were prepared from each of the S1-S17 aluminum alloy sheets by milling. The longitudinal directions of the three test pieces were aligned at angles of 0°, 45°, and 90° to the rolling direction, respectively.
[0101] Tensile tests were conducted on these test pieces in accordance with JIS-Z-2241:2011 to measure the 0.2% yield strength and tensile strength. 0.2 and tensile strength σ B The measurement results and the average value of 0.2% yield strength and tensile strength σ fm These are shown in Tables 1 and 2.
[0102] In addition, three evaluation values S were calculated from the measurement results of the tensile tests in the 0° direction, 45° direction, and 90° direction with respect to the rolling direction and formula (1). The minimum evaluation value S was the minimum evaluation value S. min is shown in Table 2.
[0103] (Toughness) In the aluminum alloy plates of S1-S17, the area is 0.3 μm by the measurement method described in the embodiment. 2 More than Mg 2 The ratio of the total area of the Si particles in the L-ST cross section (area ratio) was calculated. The measurement results are shown in Table 2.
[0104] For the aluminum alloy sheets S1-S17, the number of repeated bending and the normalized number of repeated bending were calculated from the measurement method described in the embodiment and the formulas (3) and (4). The results are shown in Table 2.
[0105] (Strength anisotropy) For the aluminum alloy sheets S1-S17, the strength anisotropy (i.e., value D) was calculated from the formula (5) explained in the embodiment. The results are shown in Table 2.
[0106] (Phase diagram calculation) Calculated based on the composition (mass%) of alloy numbers 1-9, Mg 2The solidus temperature of Si, the solidification start temperature of aluminum, and the initial phase (i.e. Al 6 The crystallization temperatures of (Mn,Fe) are shown in Table 3.
[0107] Each boundary temperature was calculated based on the equilibrium phase diagram based on the five main components (Si, Fe, Cu, Mn, Mg) using "JMatPro." The effects of Ti, Zn, Cr, and unavoidable impurities were not taken into account.
[0108] (scrap mixture ratio) Regarding the composition of the S1-S17 aluminum alloy plates, it was judged whether the possible blending ratio of 3104 aluminum alloy scrap was 50 mass% or more. The results are shown in Table 2.
[0109] In Table 2, aluminum alloy plates marked with "≧50" can contain 50 mass% or more of 3104 aluminum alloy. The possible content of 3104 aluminum alloy scrap is determined based on Table 4.
[0110] Table 4 shows the relationship between the blend ratio of 3104 aluminum alloy and 5182 aluminum alloy and the average value of the component specifications. The first line of Table 4 shows the average value of the component specifications of 3104 aluminum alloy, and the second line shows the average value of the component specifications of 5182 aluminum alloy.
[0111] For example, when the blend ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.
[0112] Therefore, when the ratio of each component of the aluminum alloy plate is equal to or greater than the above values of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of the 3104 aluminum alloy plate is 50% by mass or more. As the blending ratio of the 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase and the content of Mg decreases. The aluminum alloy plates of S1-S10 can be blended with 50% by mass or more of the 3104 aluminum alloy scrap.
[0113] [Table 4]
[0114] (evaluation) The S1-S15 aluminum alloy plates have higher strength (i.e., S) than the S16 aluminum alloy plates. min In particular, the aluminum alloy sheets S1-S7 and S14-S15 were able to achieve the same strength as the conventional 5182 aluminum alloy for can ends shown in S17, despite having a lower Mg content.
[0115] Generally, the higher the strength of a material, the lower the number of repeated bending times, i.e., the toughness. However, by homogenizing the material at high temperatures, Mg 2 S14, which contains re-dissolved Si, is Mg 2 Compared to S15, which has insufficient redissolution of Si, S14 has been repeatedly bent many times, despite having the same alloy composition and equivalent strength. In other words, S14 has both high toughness and high strength.
[0116] In S1-S7, the cold rolling rate is reduced by the intermediate annealing process. Therefore, S1-S7 has smaller strength anisotropy than S8-S13, which has a cold rolling rate of over 80%. In other words, it can be seen that the strength anisotropy corresponds to the cold rolling rate. S1-S7, which has a lower cold rolling rate by the intermediate annealing process, has both high strength and high toughness (i.e., more repeated bending times) compared to S8-S13, which has a cold rolling rate of over 80%.
[0117] As shown in Figure 2, when comparing S1, S7, and S8, which have the same alloy composition but different cold rolling rates, there is a negative correlation between strength anisotropy and cold rolling rate. In highly tough materials in which the cold rolling rate is kept between 50% and 80% by intermediate annealing, the absolute value of strength anisotropy is thought to be maximum in the negative direction at a cold rolling rate of 80%. Here, based on the trend in Figure 2, it is estimated that the strength anisotropy at a cold rolling rate of 80% will be -13 MPa, so -13 MPa can be said to be the lower limit of strength anisotropy.
[0118] Similarly, the absolute value of strength anisotropy is considered to be maximum at a cold rolling rate of 50% in the positive direction, and from the trend in Figure 2, the strength anisotropy at a cold rolling rate of 50% is estimated to be 7 MPa. On the other hand, when looking at the strength anisotropy of S3, S5, etc., it is found that some degree of variation in strength anisotropy is unavoidable. Therefore, it is considered appropriate that the strength anisotropy at a cold rolling rate of 50% is about 13 MPa.
Claims
1. The silicon (Si) content is 0.20% by mass or more and 0.47% by mass or less, The iron (Fe) content is 0.30 mass% or more and 0.59 mass% or less, The copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.70% by mass or more and 0.98% by mass or less, The magnesium (Mg) content is 1.1% by mass or more and 3.7% by mass or less, The balance is aluminum (Al) and unavoidable impurities, 0.2% yield strength σ in the 0°, 45°, and 90° directions relative to the rolling direction 0.2 , tensile strength σ B , and the average value of 0.2% yield strength and tensile strength σ fm Among the evaluation values S calculated by the following formula (1) using min The aluminum alloy sheet for can ends has a compressive strength of 330 MPa or more and 410 MPa or less. S = σ fm / (σ 0.2 / σ B ) ... (1)
2. The aluminum alloy sheet for can ends according to claim 1, The silicon (Si) content is 0.20% by mass or more and 0.39% by mass or less, The manganese (Mn) content is 0.75 mass% or more and 0.98 mass% or less, The magnesium (Mg) content is 1.4% by mass or more and 3.1% by mass or less, Solidus temperature to Mg 2 The temperature difference minus the solid solution temperature of Si is 30° C. or more, The crystallization temperature of the primary crystal is lower than the solidification start temperature of aluminum, In the L-ST cross section at the center in the width direction, the area is 0.3 μm 2 More than Mg 2 The ratio of the total area of the Si particles in the L-ST cross section is 0.2% or less, The minimum evaluation value S min The aluminum alloy sheet for can ends has a compressive strength of 360 MPa or more and 410 MPa or less.
3. The aluminum alloy sheet for can lids according to claim 1 or 2, 0.2% proof stress σ in the direction of 0° to the rolling direction 0.2_0° From the above, the 0.2% yield strength σ 0.2_90° The aluminum alloy sheet for can ends, wherein the value obtained by subtracting
4. The aluminum alloy sheet for can lids according to claim 1 or 2, A test piece cut into a rectangular shape having a width of 12.5 mm and a length of 200 mm was repeatedly bent in a direction in which the bending ridge line was parallel to the rolling direction, by bending the test piece by 90° and then returning it to the 0° position. The number of repeated bending operations N until the test piece broke was normalized by the plate thickness t of the test piece and the following formula (2) to obtain the normalized number of repeated bending operations N s The aluminum alloy sheet for can ends has a rolling resistance of 18 times or more. N s = N × t / 0.235 ... (2)
Citation Information
Patent Citations
3104 Aluminum alloy can lid material and production method thereof
CN105568085A
Can lid material excellent in bendability and its production
JP1996060284A
Resin-coated aluminum alloy sheet for end part
JP2002180173A
Casting recycled aluminum scrap
JP2020514556A
5xxx aluminium sheets for can making
WO2022233577A1