MANUFACTURING METHOD FOR Na-CONTAINING OXIDES

A manufacturing method for Na-containing oxides with a P2 type structure reduces the O3 phase by controlling the temperature increase rate and thickness ratio during firing, producing a material suitable for sodium ion batteries.

JP2024153417AActive Publication Date: 2024-10-29TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023067299
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

In Na-containing oxides with a P2 type structure, the O3 phase tends to be generated alongside the desired P2 phase, necessitating a method to reduce the O3 phase content.

Method used

A manufacturing method involving the production of a precursor containing Mn, Ni, and Co, coating it with a Na source to form a composite, and firing the composite at a controlled temperature increase rate and thickness ratio to produce a Na-containing oxide with a predominantly P2 type structure.

Benefits of technology

The method effectively reduces the O3 phase, resulting in a Na-containing oxide with a predominantly P2 type structure, suitable for use as a positive electrode active material in sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153417000001_ABST
    Figure 2024153417000001_ABST
Patent Text Reader

Abstract

To reduce O3 phases in Na-containing oxides having P2 type structure.SOLUTION: A manufacturing method for Na-containing oxides of the present disclosure includes: obtaining a precursor including at least one element selected from Mn, Ni, and Co; coating a surface of the precursor with a Na source to obtain a composite; and firing the composite to obtain Na-containing oxides having P2 type structure, and is characterized by that on firing the composite, a rate of temperature rise A(°C / min) from 300°C to 500°C and a volume B(mm3) of the composite, A / B, is 4.5 or under.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a method for producing a Na-containing oxide. [Background technology]

[0002] Patent Document 1 describes a compound having a P2 type structure and Na x Fe y Mn 1-y A Na-containing oxide having a chemical composition represented by O2 (x is less than 1, and y is 1 / 3 or more and less than 2 / 3) is disclosed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-201588 A Summary of the Invention [Problem to be solved by the invention]

[0004] In Na-containing oxides with a P2-type structure, the O3 phase is likely to form along with the P2 phase. A new technology capable of reducing the O3 phase in Na-containing oxides with a P2-type structure is needed. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A method for producing a Na-containing oxide having a P2 type structure, comprising the steps of: Obtaining a precursor comprising at least one element of Mn, Ni and Co; Coating the surface of the precursor with a Na source to obtain a composite; and The composite is fired to obtain a Na-containing oxide having a P2 type structure. Including, When firing the composite, the ratio A / B of the heating rate A (°C / min) from 300°C to 500°C to the thickness B (mm) of the composite is 4.5 or less. Manufacturing method. <Aspect 2> The manufacturing method according to Aspect 1, wherein the heating rate A is 13.5°C / min or less. Manufacturing method. <Aspect 3> The manufacturing method according to Aspect 1 or 2, wherein the precursor is spherical particles, the composite is obtained by coating 40 area% or more of the surface of the precursor with the Na source, and the Na-containing oxide having the P2-type structure is spherical particles. Manufacturing method. <Aspect 4> The manufacturing method according to any one of Aspects 1 to 3, wherein a precipitate as the precursor is obtained by coprecipitation using a transition metal ion and an ion source capable of forming a precipitate in an aqueous solution, and a transition metal compound containing at least one element among Mn, Ni, and Co. Manufacturing method. <Aspect 5> The manufacturing method according to any one of Aspects 1 to 4, wherein the Na-containing oxide having the P2-type structure is Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). Manufacturing method.

Advantages of the Invention

[0006] According to the method of the present disclosure, when manufacturing a Na-containing oxide having a P2-type structure, the O3 phase can be reduced. [Brief description of the drawings]

[0007] [Figure 1] 1 shows an example of a flow of a method for producing a Na-containing oxide having a P2 type structure. [Diagram 2] 1 shows SEM photographs of the appearance of each of the Na-containing oxides in Examples 1, 2, and 4 and the Comparative Example. [Diagram 3] 1 shows X-ray diffraction patterns of each of the Na-containing oxides of Examples 1 to 5 and a Comparative Example. [Figure 4] The relationship between A / B and the peak intensity ratio IP2 / IO3 is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Method for producing sodium-containing oxide having P2 structure 1, a method for producing a Na-containing oxide having a P2 type structure according to one embodiment includes obtaining a precursor containing at least one element selected from Mn, Ni, and Co (S1), coating the surface of the precursor with a Na source to obtain a composite (S2), and calcining the composite to obtain a Na-containing oxide having a P2 type structure (S3). Here, during calcination of the composite, the ratio A / B of the heating rate A (°C / min) from 300°C to 500°C to the thickness B (mm) of the composite is 4.5 or less.

[0009] 1.1 S1 In S1, a precursor containing at least one element of Mn, Ni, and Co is obtained. The precursor may contain at least Mn, one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor may be a salt containing at least one element of Mn, Ni, and Co. For example, the precursor may be at least one of carbonate, sulfate, nitrate, and acetate. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple types of compounds. The precursor may have various shapes. For example, the precursor may be particulate, or may be spherical particles as described later. The particle size of the particles made of the precursor is not particularly limited.

[0010] In S1, a precipitate as the precursor may be obtained by a coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. This makes it easier to obtain spherical particles as the precursor. The "ion source capable of forming a precipitate in an aqueous solution with transition metal ions" may be at least one selected from, for example, sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above salt or hydroxide containing at least one element selected from Mn, Ni, and Co. Specifically, in S1, the ion source and the transition metal compound may be prepared as solutions, and the solutions may be dropped and mixed to obtain a precipitate as the precursor. In this case, for example, water is used as the solvent. In this case, various sodium compounds may be used as the base, and an aqueous ammonia solution or the like may be added to adjust the basicity. In the case of the coprecipitation method, for example, an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate are prepared, and the aqueous solutions are dropped and mixed to obtain a precipitate as the precursor. Alternatively, the precursor can be obtained by a sol-gel method, and in particular, by a coprecipitation method, spherical particles can be easily obtained as the precursor.

[0011] As described above, the precursor may be a spherical particle. In the present application, the term "spherical particle" refers to a particle having a circularity of 0.80 or more. The circularity of the particle may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particle is 4πS / L 2 Here, S is the orthogonal projected area of ​​the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of a particle can be determined by observing the appearance of the particle with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. When a particle is composed of more than 100 particles, the circularity is measured, for example, as an average value as follows.

[0012] (1) First, the particle size distribution of the particles is measured. Specifically, the particle size at 10% cumulative value (D10) and the particle size at 90% cumulative value (D90) in the volume-based particle size distribution are determined by a laser diffraction / scattering method. (2) Regarding the appearance of the particles whose particle size distribution has been measured, images are observed using a SEM, TEM, or optical microscope, and from the particles contained in the images, 100 particles having a circle equivalent diameter (the diameter of a circle having the same area as the orthogonal projected area of ​​the particle) equal to or greater than D10 and equal to or less than D90 as determined in (1) are randomly selected. (3) The circularity of each of the 100 extracted particles is determined by image processing, and the average value is regarded as the "circularity of the particle."

[0013] In S1, the precursor may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. These elements M have, for example, a function of stabilizing the P2 type structure. The method of obtaining a precursor containing element M is not particularly limited. When the precursor is obtained by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dropped and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped when Na-doping baking is performed in S2 and S3 described later.

[0014] 1.2 S2 In S2, the surface of the precursor obtained in S1 is coated with a Na source to obtain a composite. The Na source may be a salt containing Na, such as a carbonate or a nitrate, or may be a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor may be determined taking into account the amount of Na lost during the subsequent calcination.

[0015] In S2, the coverage of the Na source on the surface of the precursor is not particularly limited. For example, in S2, the above-mentioned composite may be obtained by covering 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the above-mentioned precursor with the Na source. Here, when the precursor obtained by S1 is a spherical particle, and the composite obtained by S2 is obtained by covering 40 area% or more of the surface of the precursor with the Na source, the Na-containing oxide having the P2 type structure is likely to become a spherical particle in S3 described later. If the coverage of the Na source is small, when the composite is fired, P2 type crystals are likely to grow on the surface of the composite, and the Na-containing oxide is likely to become a plate-like. If the coverage of the Na source is large, when the composite is fired, the crystallites of the P2 type crystals are likely to become small, and the Na-containing oxide is likely to become a spherical particle corresponding to the shape of the precursor.

[0016] In S2, the method for coating the surface of the precursor with the Na source is not particularly limited. As described above, when 40% or more of the area of ​​the surface of the precursor is coated with the Na source, various methods can be used. For example, a tumbling fluidized coating method or a spray drying method can be used. That is, a coating solution in which a Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor, and dried at the same time or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), 40% or more of the area of ​​the surface of the precursor can be coated with the Na source.

[0017] In S2, the precursor may be coated with an M source together with a Na source. For example, in S2, the precursor obtained in S1, a Na source, and an M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W may be mixed to obtain a composite. The M source may be, for example, a salt containing the element M, such as a carbonate or sulfate, or a compound other than a salt, such as an oxide or hydroxide. The amount of the M source relative to the precursor may be determined depending on the chemical composition of the Na-containing oxide after firing.

[0018] 1.3 S3 In S3, the composite obtained in S2 is fired to obtain a Na-containing oxide having a P2 type structure. In S3, when firing the composite, the ratio A / B of the heating rate A (°C / min) from 300°C to 500°C to the thickness B (mm) of the composite is 4.5 or less. According to the findings of the present inventors, when firing the composite, by controlling the heating rate A from 300°C to 500°C to a low rate equal to or lower than a predetermined rate according to the thickness B of the composite, the O3 phase is easily reduced regardless of the scale, and a Na-containing oxide mainly composed of the P2 phase is easily obtained.

[0019] In S3, the heating rate A may be any rate that satisfies the above ratio A / B. According to the knowledge of the present inventor, when the heating rate A is 13.5°C / min or less, the O3 phase is more likely to be reduced. The lower limit of the heating rate A is not particularly limited. The heating rate A may be, for example, 0.05°C / min or more, or 0.10°C / min or more. The heating rate A may be 12.0°C / min or less, 11.0°C / min or less, 10.0°C / min or less, 9.0°C / min or less, 8.0°C / min or less, or 7.0°C / min or less. The heating rate A refers to a target heating rate set in the heating device. In the case of a heating furnace, it is a heating rate based on the display temperature of the heating furnace.

[0020] In S3, the thickness B of the composite is the thickness of the composite in a container when the container containing the composite is placed inside a heating device such as a heating furnace, and refers to the thickness of the composite when the composite is lightened so as to have a uniform height inside the container. For example, the height of the composite in the container when the container is placed on the bottom surface inside the heating furnace is "thickness B". The thickness B of the composite may be, for example, 1 mm or more and 100 mm or less, or 1 mm or more and 50 mm or less.

[0021] In S3, the ratio A / B is 4.5 or less. The ratio A / B may be 4.0 or less, 3.5 or less, 3.0 or less, 2.5 or less, 2.0 or less, 1.5 or less, 1.0 or less, or 0.5 or less. The lower limit of the ratio A / B is not particularly limited, and may be more than 0, 0.01 or more, 0.02 or more, or 0.03 or more.

[0022] In S3, the heating rate up to 300°C is not particularly limited. The heating rate from 500°C to the firing temperature is also not particularly limited. In this embodiment, regardless of the heating rate up to 300°C or the heating rate from 500°C to the firing temperature, the O3 phase can be reduced by controlling the heating rate from 300°C to 500°C as described above.

[0023] In S3, the above composite may be optionally molded, optionally pre-fired, and then the main firing may be performed. The pre-firing of the composite may be performed at a temperature equal to or lower than the main firing temperature. For example, the pre-firing may be performed at a temperature higher than 500°C and lower than 700°C. The pre-firing time is not particularly limited. The pre-firing atmosphere is also not particularly limited. The pre-firing atmosphere may be the same as or different from the main firing atmosphere.

[0024] In S3, the composite may be sintered at a temperature of, for example, 700° C. to 1100° C., preferably 800° C. to 1000° C. If the sintering temperature is too low, Na doping is not performed, and if the sintering temperature is too high, O3 phase, etc., is likely to be generated instead of P2 phase. The temperature rise conditions from the preliminary sintering temperature to the sintering temperature are not particularly limited.

[0025] The firing time is not particularly limited, and may be, for example, 30 minutes or more and 48 hours or less. However, the shape of the Na-containing oxide can be controlled by the firing time. As described above, in the method of the present disclosure, when the coverage rate of the Na source in the composite is 40 area % or more, when the composite is fired, a P2 type crystal with small crystallites is easily formed on the surface. In this embodiment, the shape of the Na-containing oxide corresponds to the shape of the precursor by growing the P2 type crystal along the surface of the particle so that one P2 type crystallite and another P2 type crystallite are connected to each other. For example, when the precursor is a spherical particle, the Na-containing oxide can also be a spherical particle. If the firing time is too short, Na doping is not performed, and it is difficult to obtain the desired P2 type structure. On the other hand, if the firing time is too long, the P2 type structure grows and the particles become plate-like instead of spherical. As far as the present inventors have confirmed, if the firing time is 30 minutes or more and 3 hours or less, spherical particles of the Na-containing oxide are easily obtained. The Na-containing oxide obtained after the main firing may have a structure in which a plurality of crystallites are present on the surface and the crystallites are connected to each other.

[0026] The firing atmosphere in S3 is not particularly limited, and may be, for example, an oxygen-containing atmosphere such as air atmosphere, or an inert gas atmosphere.

[0027] 2. Na-containing oxides with P2 structure By the above-mentioned method, it is possible to produce a Na-containing oxide having a P2 type structure and a reduced O3 phase. Hereinafter, a Na-containing oxide according to one embodiment will be described.

[0028] 2.1 Chemical composition The Na-containing oxide according to one embodiment contains, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O. In particular, when the constituent elements contain at least Na, Mn, one or both of Ni and Co, and O, and especially when the constituent elements contain at least Na, Mn, Ni, Co, and O, higher performance is likely to be obtained. In one embodiment, the Na-containing oxide having a P2 type structure contains Na a Mnx-p Ni y-q Co z-r M p+q+r O₂ (where 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). It may have a chemical composition represented thereby. When the Na-containing oxide has such a chemical composition, the P2-type structure is likely to be maintained. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, or 0.70 or less. Also, x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, and may be 0.10 or more or 0.20 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, and may be 0.10 or more, 0.20 or more, or 0.30 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has a small contribution to charge and discharge. In this regard, in the above chemical composition, since p + q + r is less than 0.17, a high charge and discharge capacity is likely to be ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, since the element M is included, the P2-type structure is likely to be stabilized. In the above chemical composition, p + q + r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.

[0029] 2.2 Crystal structure The Na-containing oxide according to one embodiment has at least a P2 type structure (belonging to space group P63mc) as a crystal structure. The Na-containing oxide has the P2 type structure and may have a crystal structure other than the P2 type structure. Examples of crystal structures other than the P2 type structure include various crystal structures formed when Na is desorbed from the P2 type structure. Here, the Na-containing oxide according to this embodiment has a P2 type structure, but has little O3 type structure. The Na-containing oxide according to this embodiment may have a P2 type structure as a main phase. For example, the X-ray diffraction pattern of the Na-containing oxide according to this embodiment has a refractive index of 0.5≦I P2 / I O3 ≦20.0, where I P2 is the X-ray diffraction peak intensity due to the (102) plane of the P2 type structure. O3 is the X-ray diffraction peak intensity due to the (015) plane of the O3 type structure. I P2 / I O3 may be 1.0 or more, 2.0 or more, 3.0 or more, or 4.0 or more, and may be 18.0 or less, 16.0 or less, 14.0 or less, 12.0 or less, 10.0 or less, 9.0 or less, 8.0 or less, or 7.0 or less.

[0030] X-ray diffraction peak intensity I originating from the (102) plane of the P2 structure P2 is specified as follows: (1) In the X-ray diffraction pattern using CuKα as a radiation source, the average value I of the diffraction peak intensity at 35.0° ± 0.2° is used as the background. 35 Request. (2) In the X-ray diffraction pattern, the maximum diffraction peak intensity I between 39.23° and 40.05° 39 Request. (3)I 39 From I 35 The value obtained by subtracting P2 Let (I P2 =I 39 -I 35 ).

[0031] X-ray diffraction peak intensity I originating from the (015) plane of the O3 structure O3 is specified as follows: (1) In the X-ray diffraction pattern using CuKα as a radiation source, the average value I of the diffraction peak intensity at 35.0° ± 0.2° is used as the background. 35 Request. (2) In the X-ray diffraction pattern, the maximum diffraction peak intensity I between 45.35° and 45.65° 45 Request. (3)I 45 From I 35 The value obtained by subtracting O3 Let (I O3 =I 45 -I 35 ).

[0032] The Na-containing oxide according to an embodiment may be a single crystal consisting of one crystallite, or may be a polycrystal having a plurality of crystallites. For example, the surface of the Na-containing oxide according to an embodiment may be composed of a plurality of crystallites. In other words, the Na-containing oxide may have a structure in which a plurality of crystallites are connected to each other on the surface. When the surface of the Na-containing oxide is composed of a plurality of crystallites, a crystal grain boundary is present on the surface. Here, the crystal grain boundary may be an inlet and an outlet of intercalation. That is, when the Na-containing oxide is a polycrystal having a plurality of crystallites, the effect of increasing the number of inlets and outlets of intercalation to reduce the reaction resistance, the effect of shortening the distance of movement of sodium ions to reduce the diffusion resistance, the effect of reducing the absolute amount of expansion and contraction during charging and discharging, and the effect of making it difficult for cracks to occur can be expected. The size of the crystallite may be large or small, but it is considered that the smaller the size of the crystallite, the more the crystal grain boundaries will be, and the more likely the above-mentioned advantageous effects will be exhibited. For example, when the diameter of the crystallite constituting the Na-containing oxide is less than 1 μm, higher performance is likely to be obtained. The "crystallite" and "diameter of the crystallite" can be determined by observing the surface of the Na-containing oxide with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when the surface of the Na-containing oxide is observed and a closed region surrounded by a grain boundary is observed, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is determined and regarded as the "diameter of the crystallite". If the Na-containing oxide is composed of a single crystal, the particle itself can be said to be a single crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can be determined by EBSD or XRD. For example, the diameter of the crystallite can be determined based on the Scherrer formula from the half-width of the diffraction line of the XRD pattern. If the diameter of the crystallite of the Na-containing oxide specified by any method is less than 1 μm, the performance of the Na-containing oxide is likely to be higher.

[0033] 2.3 Shape The P2 type structure is a hexagonal crystal system, has a large diffusion coefficient of Na ions, and is likely to grow crystals in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2 type structure, the crystals are likely to grow in a plate-like shape in a specific direction. Therefore, the Na-containing transition metal oxide having the P2 type structure usually becomes a plate-like particle with a large aspect ratio in which the crystal growth direction is biased in a specific direction. In contrast, the Na-containing oxide according to one embodiment may be a spherical particle as described above. When the Na-containing oxide is a spherical particle, as described above, the reaction resistance is reduced by reducing the crystallite size, and the diffusion resistance inside the particle is likely to be reduced. Furthermore, when applied to a secondary battery or the like, it is considered that the degree of bending is reduced by spheroidization, and the sodium ion conduction resistance is reduced. As a result, for example, the rate characteristic is improved and the reversible capacity is likely to be increased.

[0034] The Na-containing oxide according to one embodiment may be a solid particle, a hollow particle, or a particle having a void. The size of the Na-containing oxide particles is not particularly limited, but it is considered that a smaller size is more advantageous. For example, the average particle diameter (D50) of the Na-containing oxide particles may be 0.1 μm or more and 10 μm or less, 1.0 μm or more and 8.0 μm or less, or 2.0 μm or more and 6.0 μm or less. The average particle diameter (D50) is the particle diameter (D50, median diameter) at an integrated value of 50% in the volume-based particle size distribution by a laser diffraction / scattering method.

[0035] 2.4 Supplementary Information In summary, the Na-containing oxide according to one embodiment may have, for example, the following configurations (1) to (4). (1) The Na-containing oxide contains at least one element selected from the group consisting of Mn, Ni, and Co, Na, and O as constituent elements. (2) The Na-containing oxide has a P2 type structure. (3) The X-ray diffraction pattern of the Na-containing oxide is 0.5≦I P2 / I O3 <= 20.0. (4) The Na-containing oxide is a spherical particle.

[0036] 3.Applications The Na-containing oxide having the P2 type structure produced by the above method can be used, for example, as a positive electrode active material of a sodium ion battery. A sodium ion battery according to one embodiment includes a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, and is characterized in that the positive electrode active material layer contains the Na-containing oxide having the P2 type structure of the present disclosure as a positive electrode active material. The sodium ion battery can have the same configuration as a conventional battery, except that it contains the specific positive electrode active material. EXAMPLES

[0037] As described above, one embodiment of the method for producing a Na-containing oxide having a P2 type structure has been described, but the method for producing the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the present disclosure. The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0038] 1. Preparation of Na-containing oxides with P2 structure 1.1 Preparation of precursor (1) MnSO4·5H2O, NiSO4·6H2O, and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to obtain a concentration of 1.6 mol / L to obtain a first solution. In a separate container, Na2CO3 was dissolved in distilled water to obtain a concentration of 1.6 mol / L to obtain a second solution. (2) 850 mL of pure water was placed in a reaction vessel (with a baffle plate), and 500 mL of the first solution and 500 mL of the second solution were each added dropwise at a rate of about 4 mL / min. (3) After the dropwise addition was completed, the mixture was stirred at room temperature for 1 hour at a stirring speed of 160 rpm to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 150°C, crushed in a mortar, and then fine particles were removed by air classification to obtain precursor particles. The precursor particles were a composite salt containing Mn, Ni, and Co, and were spherical particles with a circularity of 0.80 or more.

[0039] 1.2 Preparation of the complex (1) Na2CO3 as a Na source and the above precursor particles are mixed to obtain a composition after calcination as described below. 0.7 Mn 0.5 Ni 0.2 Co 0.3 It was weighed to be O2. (2) The weighed Na source and precursor particles were mixed by spray drying. Specifically, the weighed Na source and precursor particles were added to a solvent, and the dispersion solution in which the Na source was dissolved and the precursor particles were dispersed was spray dried. The spray drying temperature was 200°C, and the spray pressure was 0.3 MPa. A composite in which 75 area % of the surface of the precursor particles was covered with the Na source was obtained by spray drying.

[0040] 1.3 Firing of the composite 1 g of the composite was placed in an alumina crucible and sintered in an air atmosphere under the following conditions (1) to (5). (1) An alumina crucible containing the above composite is placed in a heating furnace. Here, the thickness B of the composite is 3 mm. (2) The temperature inside the heating furnace is increased from room temperature to 900° C. at a predetermined temperature increase rate A. The relationship between the temperature increase rate A and the thickness B is as shown in Table 1 below. (3) The temperature in the heating furnace is kept at 900°C for one hour to perform the main firing. (4) After the main firing, the temperature in the heating furnace is lowered from 900°C to 250°C over a period of 4 hours. (5) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in the air.

[0041] The fired product after cooling in the air was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles having a P2 type structure. 0.7 Mn 0.5Ni 0.2 Co 0.3 It had a chemical composition indicated as O2.

[0042] 2.Evaluation of Na-containing oxide particles 2.1 Appearance observation by SEM FIG. 2 shows SEM photographs of the appearance of the Na-containing oxides according to Examples 1, 2, 4, and Comparative Example. As is clear from FIG. 2, the Na-containing oxides according to Examples 1, 2, 4, and Comparative Example are spherical particles having a circularity of 0.80 or more. It is also found that the surfaces of the spherical particles are composed of a plurality of crystallites, and the crystallite diameter is less than 1 μm. The Na-containing oxides according to Examples 3 and 5 also had a similar morphology.

[0043] 2.2 Identification of crystal structure by X-ray diffraction measurement For each of the Na-containing oxides in Examples 1 to 5 and Comparative Example, an X-ray diffraction measurement was performed using CuKα as a radiation source to obtain an X-ray diffraction pattern. From the X-ray diffraction pattern, the diffraction peak intensity I P2 and the diffraction peak intensity I originating from the (015) plane of the O3 type structure O3 Comparison with I P2 / I O3 The X-ray diffraction patterns of the Na-containing oxides of Examples 1 to 5 and the Comparative Example are shown in Fig. 3. As shown in Fig. 3, the Na-containing oxide according to the Comparative Example has a diffraction peak intensity I P2 and the diffraction peak intensity I due to the O3 type structure O3 Comparison with I P2 / I O3 In contrast, the Na-containing oxides according to Examples 1 to 5 had a small I P2 / I O3In Examples 1 to 5, the amount of the O3 phase was significantly reduced compared to the comparative example. It is believed that the reduction in the O3 phase was due to the slow heating rate during main sintering in Examples 1 to 5. According to a more detailed confirmation by the present inventors, the amount of the O3 phase can be controlled by the heating rate from 300°C to 500°C when sintering the composite. Specifically, as shown in Table 1 and FIG. 4 below, when the ratio A / B of the heating rate A (°C / min) from 300°C to 500°C to the thickness B (mm) of the composite is 4.5 or less, I P2 / I O3 becomes significantly large, that is, the O3 phase is easily reduced significantly.

[0044] [Table 1]

[0045] 3. Supplementary Information In the above examples, the precursor is obtained by coprecipitation, but the precursor can be obtained by other methods. In the above examples, the surface of the precursor is coated with a Na source by spray drying to obtain a composite, but the composite can be obtained by other methods. In the above examples, the Na-containing oxide having a P2 type structure is exemplified as having a predetermined chemical composition, but the chemical composition of the Na-containing oxide is not limited to this. Various chemical compositions having a P2 type structure can be adopted. In addition, the Na-containing oxide may be doped with an element M other than Mn, Ni, and Co. The element M is as described in the embodiment. In the above examples, the spherical precursor is used to finally obtain spherical Na-containing oxide particles, but the precursor and the Na-containing oxide are not limited to spherical particles. However, when the particles are spherical, for example, a high effect can be expected as a positive electrode active material for a battery.

[0046] 4. Summary As described above, the method for producing a Na-containing oxide having a P2 type structure, which includes the following steps S1 to S3, can reduce the O3 phase in the Na-containing oxide. That is, a Na-containing oxide having a P2 type structure and reduced O3 phase can be produced. S1: A precursor containing at least one element of Mn, Ni, and Co is obtained. S2: The surface of the precursor is coated with a Na source to obtain a composite. S3: The composite is fired to obtain a Na-containing oxide having a P2 type structure, wherein the ratio A / B of the heating rate A (°C / min) from 300°C to 500°C and the thickness B (mm) of the composite during firing is 4.5 or less.

[0047] According to the above-mentioned production method, for example, a Na-containing oxide satisfying the following properties (1) to (4) can be obtained. (1) The alloy contains, as its constituent elements, at least one of Mn, Ni, and Co, as well as Na and O. (2) It has a P2 type structure. (3) 0.5≦I P2 / I O3 The X-ray diffraction pattern satisfies ≦20.0. (4) The particles are spherical.

Claims

1. A method for producing a Na-containing oxide having a P2 type structure, comprising the steps of: Obtaining a precursor comprising at least one element of Mn, Ni and Co; Coating the surface of the precursor with a Na source to obtain a composite; and The composite is fired to obtain a Na-containing oxide having a P2 type structure. Including, When the composite is fired, a ratio A / B of a temperature rise rate A (°C / min) from 300°C to 500°C to a thickness B (mm) of the composite is 4.5 or less. Manufacturing method.

2. The method according to claim 1, The temperature rise rate A is 13.5 ° C. / min or less; Manufacturing method.

3. The method according to claim 1, The precursor is a spherical particle, The composite is obtained by covering 40% by area or more of the surface of the precursor with the Na source; and The Na-containing oxide having a P2 type structure is a spherical particle. Manufacturing method.

4. The method according to claim 1, obtaining a precipitate as the precursor by a coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution together with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co; Manufacturing method.

5. The method according to any one of claims 1 to 4, The Na-containing oxide having a P2 type structure is a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Manufacturing method.

Citation Information

Patent Citations

  • P2 type layered transition metal oxide and preparation method and application thereof

    CN115504525A

  • Manufacturing method of oriented sintered body of sodium containing metal oxide

    JP2004349434A

  • Hardly graphitizable carbonaceous material for nonaqueous electrolyte secondary battery, negative electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

    JP2019008910A

  • Manufacturing method of positive electrode of sodium all-solid-state battery

    JP2021068672A

  • Sodium metal oxide material for secondary batteries and manufacturing method

    JP2022504285A