Repelling agent

Polymers with specific repeating units and alternating arrangements are used to create repellent agents that enhance liquid repellency on materials, addressing the lack of effective repellent polymers in existing technologies and maintaining repellency across temperature variations.

JP2024153749AActive Publication Date: 2024-10-29DAIKIN INDUSTRIES LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024119368
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-09
Filing Date
2024-07-25
Publication Date
2024-10-29
Estimated Expiration
2043-11-08

AI Technical Summary

Technical Problem

Existing repellent technologies do not effectively utilize polymers with acrylamide and acrylate units for repellent applications, and there is a lack of polymers specifically designed for imparting liquid repellency to materials.

Method used

Development of polymers comprising specific repeating units and alternating arrangements, such as -[CH2C(-Q1)C(=O)R1]-, -[CH2C(-Q2)C(=O)NHR2OH]-, -[CH2C(-Q3)C(=O)OH]-, and -[CH2C(-Q4)C(=O)OR41OC(=O)NHR42]-, which are used in repellent agents to enhance liquid repellency on materials like textiles and paper.

Benefits of technology

The developed polymers provide improved liquid repellency by forming phase-separated structures and maintaining repellency across varying temperatures, even without the use of fluorine compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153749000001
    Figure 2024153749000001
  • Figure 2024153749000002
    Figure 2024153749000002
  • Figure 2024153749000003
    Figure 2024153749000003
Patent Text Reader

Abstract

To provide a novel repelling agent or a novel polymer suitable for repellent applications.SOLUTION: The present invention provides a repelling agent including a polymer selected from polymers (I)-(III), which are defined as follows. (I) A polymer having a repeat unit (1) that is represented by the formula -[CH2C(-Q1)C(=O)R1]- (where each symbol in this formula is as defined in the description), and a repeat unit (2) that is represented by the formula -[CH2C(-Q2)C(=O)NHR2OH]- (where each symbol in this formula is as defined in the description). (II) A polymer that has an alternating arrangement (A) comprising the repeat unit (1) and the repeat unit (2). (III) A polymer that has an alternating arrangement (E) comprising a repeat unit (3) that is represented by the formula -[CH2C(-Q3)C(=O)OH]- (where each symbol in this formula is as defined in the description), and a repeat unit (4) that is represented by the formula -[CH2C(-Q4)C(=O)OR41OC(=O)NHR42]- (where each symbol in this formula is as defined in the description).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to repellents. [Background technology]

[0002] Non-Patent Document 1 discloses a method for synthesizing an alternating copolymer consisting of only acrylamide units from one type of monomer by using a divinyl monomer. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Kametani, Yuki, et al. Angewandte Chemie International Edition 59.13 (2020): 5193-5201. Summary of the Invention [Problem to be solved by the invention]

[0004] Non-Patent Document 1 does not describe or suggest the application of polymers to agent repellent applications. In addition, Non-Patent Document 1 only discloses an alternating copolymer consisting of only acrylamide units, and does not describe or suggest a polymer having acrylate units. The object of the present disclosure is to provide a novel repellent or a novel polymer that can be used for agent repellent applications. [Means for solving the problem]

[0005] The present disclosure includes the following aspects: [Section 1] A repellent comprising a polymer selected from the polymers (I) to (III) defined below. (I) the following formula: -[CH2C(-Q 1 )C(=O)R 1 ]- [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 1 is -NH(R 11 ) or -N(R 11 )2, where R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. A repeating unit represented by the formula (1), and The formula: -[CH2C(-Q 2 )C(=O)NHR 2 OH]- [In the formula, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 2 is an alkylene group having 1 to 10 carbon atoms. A polymer having a repeating unit (2) represented by the following formula: (II) A polymer having an alternating sequence (A) consisting of the repeating unit (1) and the repeating unit (2). (III) the following formula: -[CH2C(-Q 3 )C(=O)OH]- [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom. The repeating unit (3) represented by The formula: -[CH2C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The repeating unit (4) represented by A polymer having an alternating sequence (E) consisting of: [Section 2] Item 2. The repellent according to item 1, comprising a polymer (II). [Section 3] Item 3. The repellent according to item 1 or 2, comprising a polymer (III). [Section 4] The amount of the repeating unit (1) in the polymer is 15% by weight or more, and the amount of the repeating unit (2) in the polymer is 15% by weight or more; or Item 4. The repellent according to any one of items 1 to 3, wherein the amount of the alternating sequence (A) and / or the alternating sequence (E) is 30% by weight or more in the polymer. [Section 5] Item 5. The repellent according to any one of items 1 to 4, comprising a liquid medium which is water, an organic solvent, or a mixture of water and an organic solvent. [Section 6] Item 6. The repellent according to any one of items 1 to 5, which is for fibers or paper. [Section 7] Item 7. A substrate to which the polymer in the repellent according to any one of items 1 to 6 is adhered. [Section 8] Item 7. A method for producing a treated substrate, comprising applying the repellent according to any one of items 1 to 6 to a substrate. [Section 9] A polymer selected from polymer (II) and polymer (III) defined below. (II) the following formula: -[CH2C(-Q 1 )C(=O)R 1 ]- [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 1 is -NH(R 11 ) or -N(R 11 )2, where R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. The repeating unit (1) represented by The formula: -[CH2C(-Q 2 )C(=O)NHR 2 OH]- [In the formula, Q 2is a hydrogen atom, a monovalent organic group, or a halogen atom, R 2 is an alkylene group having 1 to 10 carbon atoms. The repeating unit (2) represented by The alternating sequence (A) consists of The repeating unit (1) is selected from two or more R 11 A polymer comprising: (III) the following formula: -[CH2C(-Q 3 )C(=O)OH]- [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom. The repeating unit (3) represented by The formula: -[CH2C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The repeating unit (4) represented by A polymer having an alternating sequence (E) consisting of: [Section 10] Item 10. The polymer according to item 9, which is polymer (II). [Section 11] Item 10. The polymer according to item 9, which is polymer (III). [Section 12] Item 12. The polymer according to any one of items 9 to 11, wherein the amount of the alternating sequence (A) and / or the alternating sequence (E) is 30% by weight or more in the polymer. [Section 13] A method for producing a polymer (II), comprising the steps of: The formula: CH2=C(-Q 1 )C(=O)-X A-OR 2 NHC(=O)C(-Q 2 )=CH2 [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, X A is a group removable by aminolysis, R 2 is an alkylene group having 1 to 10 carbon atoms, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom. to obtain a precursor (A) by cyclopolymerizing a divinyl monomer (A) represented by the formula: The precursor (A) and The formula: NH2(R 11 ) or NH(R 11 )2 [In the formula, R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. With an amine compound represented by the formula The polymer (II) The formula: -[CH2C(-Q 1 )C(=O)R 1 ]- [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 1 is -NH(R 11 ) or -N(R 11 )2, where R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. The repeating unit (1) represented by The formula: -[CH2C(-Q 2 )C(=O)NHR 2 OH]- [In the formula, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 2 is an alkylene group having 1 to 10 carbon atoms. The repeating unit (2) represented by The alternating sequence (A) consists of The repeating unit (1) is selected from two or more R 11 A method for producing a polymer (II), comprising the steps of: [Section 14] A method for producing a polymer (III), comprising the steps of: The formula: CH2=C(-Q 3 )C(=O)OX E -OR 41 -OC(=O)C(-Q 4 )=CH2 [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom, X E is a group removable by acidolysis, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms. a step of cyclopolymerizing a divinyl monomer (E) represented by the formula: The precursor (E1) is decomposed with an acid to obtain X E to obtain a precursor (E2); and The precursor (E2) The formula: R 42 -NCO [In the formula, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. With an isocyanate compound represented by the formula: The polymer (III) The formula: -[CH2C(-Q 3 )C(=O)OH]- [In the formula, Q 3is a hydrogen atom, a monovalent organic group, or a halogen atom. The repeating unit (3) represented by The formula: -[CH2C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The repeating unit (4) represented by A method for producing a polymer (III) having an alternating sequence (E) consisting of: Effect of the Invention

[0006] According to the present disclosure, novel repellents or novel polymers that can be used in repellent applications are provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] <Terminology> As used herein, the term "n-valent group" refers to a group having n bonds, i.e., a group that forms n bonds. The term "n-valent organic group" refers to an n-valent group containing carbon. Such an organic group is not particularly limited, but may be a hydrocarbon group or a derivative thereof. The derivative of a hydrocarbon group refers to a group having one or more N, O, S, Si, amide, sulfonyl, siloxane, carbonyl, carbonyloxy, etc. at the end of the hydrocarbon group or in the molecular chain.

[0008] As used herein, the term "hydrocarbon group" refers to a group containing carbon and hydrogen, which is a group obtained by removing a hydrogen atom from a hydrocarbon. Such a hydrocarbon group includes, but is not limited to, C 1-20Examples of the hydrocarbon group include an aliphatic hydrocarbon group and an aromatic hydrocarbon group. The "aliphatic hydrocarbon group" may be linear, branched, or cyclic, and may be saturated or unsaturated. The hydrocarbon group may contain one or more ring structures. The hydrocarbon group may be substituted with one or more substituents.

[0009] In this specification, regardless of whether "independently at each occurrence," "independently of each other," "independently of each other," or similar expressions are explicitly stated, unless otherwise stated, when a term (symbol) that may occur multiple times in a chemical structure is defined, the definition applies independently at each occurrence.

[0010] <Repellent> The repellent in the present disclosure provides liquid repellency to a substrate (e.g., a fiber substrate, a paper substrate, etc.) and can function as at least one selected from the group consisting of a water repellent, an oil repellent, an oil-resistant agent, and a water-resistant agent. In the polymer in the repellent, the coexistence of a hydrogen bond site such as an amide group and a hydrocarbon group can improve the liquid repellency. In the polymer in the present disclosure, the hydrogen bond sites such as amide groups are alternately arranged, which makes it easier to form a phase separation structure than a random arrangement, and the liquid repellency of the alternating copolymer can be improved. Furthermore, in the polymer in the present disclosure, the hydrogen bond sites such as amide groups are alternately arranged, which suppresses molecular motion and can suppress a decrease in liquid repellency due to temperature.

[0011] The repellent agent in the present disclosure may not contain any compound selected from the group consisting of a compound having a fluoroalkyl group having 8 or more carbon atoms, a compound having a perfluoroalkyl group having 8 or more carbon atoms, a compound having a fluoroalkyl group having 4 or more carbon atoms, a compound having a perfluoroalkyl group having 4 or more carbon atoms, a compound having a perfluoroalkyl group, a compound having a fluoroalkyl group, and a compound having a fluorine atom. The repellent agent in the present disclosure can impart liquid repellency to a substrate even if it does not contain these fluorine compounds.

[0012] [Polymer] The repellent in the present disclosure includes a polymer selected from the polymers (I) to (III) described below. The polymer may correspond to only one of the polymers (I) to (III), or may correspond to any two or all of the polymers (I) to (III). The polymer (II) may also correspond to the polymer (I) at the same time.

[0013] The polymer in the present disclosure may not have any group selected from the group consisting of a fluoroalkyl group having 8 or more carbon atoms, a perfluoroalkyl group having 8 or more carbon atoms, a fluoroalkyl group having 4 or more carbon atoms, a perfluoroalkyl group having 4 or more carbon atoms, a perfluoroalkyl group, a fluoroalkyl group, and a fluorine atom. Even if the polymer in the present disclosure does not contain these fluorine-containing groups, it can impart liquid repellency to a substrate.

[0014] [Polymer (I)] The polymer (I) has a repeating unit (1) and a repeating unit (2). The polymer (I) may be a random polymer having the repeating unit (1) and the repeating unit (2) arranged randomly. The explanation of the repeating unit (1) and the repeating unit (2) is incorporated in the description of the polymer (II).

[0015] [Polymer (II)] The polymer (II) has an alternating sequence (A) consisting of repeating units (1) and repeating units (2).

[0016] (Alternating Arrangement (A)) The alternating sequence (A) is composed of a repeating unit (1) and a repeating unit (2). In other words, the alternating sequence (A) is a sequence formed by alternately bonding the repeating unit (1) and the repeating unit (2), and is represented by the following formula: -[CH2C(-Q 1 )C(=O)R 1 ]-[CH2C(-Q 2 )C(=O)NHR 2 OH]- [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, R1 is -NH(R 11 ) or -N(R 11 )2, where R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 2 is an alkylene group having 1 to 10 carbon atoms. It is expressed as:

[0017] (Repeating unit (1)) The repeating unit (1) is The formula: -[CH2C(-Q 1 )C(=O)R 1 ]- [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 1 is -NH(R 11 ) or -N(R 11 )2, where R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. It is expressed as:

[0018] Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom. Examples of the monovalent organic group include a cyano group, an aliphatic hydrocarbon group having 1 to 6 carbon atoms (e.g., an alkyl group, an alkenyl group, etc.), and an aromatic group having 5 to 12 carbon atoms. Examples of the halogen atom include fluorine, chlorine, bromine, and iodine. Q 1 may be a hydrogen atom, a halogen atom, a methyl group, a cyano group, a substituted or unsubstituted benzyl group, or a substituted or unsubstituted phenyl group, for example a hydrogen atom, a methyl group, a chlorine atom, a bromine atom, an iodine atom, or a cyano group, preferably a hydrogen atom, a methyl group, or a chlorine atom, in particular a hydrogen atom or a methyl group.

[0019] R 1 is -NH(R11 ) or -N(R 11 )2. For example, R 1 is -NH(R 11 ) and -N(R 11 ) may be in combination with 2.

[0020] R 11 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The hydrocarbon group may be an aromatic hydrocarbon group or an aliphatic hydrocarbon group, preferably an aliphatic hydrocarbon group, and particularly preferably a saturated aliphatic hydrocarbon group (alkyl group). The hydrocarbon group may be cyclic, linear, or branched, preferably linear. The number of carbon atoms in the hydrocarbon group may be 4 or more, 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, 16 or more, or 18 or more, preferably 8 or more, and more preferably 12 or more. The number of carbon atoms in the hydrocarbon group may be 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, or 10 or less, preferably 30 or less, and more preferably 25 or less.

[0021] R 11 may contain other groups in addition to the hydrocarbon group having 4 to 40 carbon atoms. Examples of the other groups include ether oxygen and amino groups (e.g., secondary or tertiary amino groups). For example, R 11 may form a branched structure from the nitrogen atom.

[0022] R 11 Two or more types (e.g., two, three, or four types) of R may be combined. 11 By combining these, it may be possible to impart a number of properties to the polymer. An example of such a combination is a hydrocarbon group having 12 or more carbon atoms (e.g., a chain alkyl group). 11 and a combination of a cyclic hydrocarbon-containing group (e.g., a cycloalkyl-containing group, a phenyl-containing group, etc.). A hydrocarbon group having 12 or more carbon atoms can impart high liquid repellency, and a cyclic hydrocarbon-containing group can impart high heat resistance. 11 When used together, each R 11 is R 11may be present in an amount of 10 mol % or more, 20 mol % or more, or 30 mol % or more based on the total of

[0023] R 11 The carbon atom ratio of R may be 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 100%, and is preferably 60% or more. 11 The carbon atom ratio of R may be 100% or less, 95% or less, 90% or less, 85% or less, or 80% or less. 11 The carbon atom ratio of R 11 R relative to the total amount of heteroatoms (atoms other than carbon and hydrogen atoms) in 11 R is the molar ratio of the amount of carbon atoms in 11 When the carbon atom ratio is equal to or more than the above lower limit, liquid repellency can be satisfactorily exhibited.

[0024] R 11 The molecular weight of R may be 50 or more, 100 or more, 150 or more, 200 or more, 250 or more, or 300 or more. 11 may have a molecular weight of 750 or less, 600 or less, 500 or less, 400 or less, 300 or less, 200 or less, or 100 or less.

[0025] (Repeating unit (2)) The repeating unit (2) is The formula: -[CH2C(-Q 2 )C(=O)NHR 2 OH]- [In the formula, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 2 is an alkylene group having 1 to 10 carbon atoms. It is expressed as:

[0026] Q 2is a hydrogen atom, a monovalent organic group, or a halogen atom. Examples of the monovalent organic group include a cyano group, an aliphatic hydrocarbon group having 1 to 6 carbon atoms (e.g., an alkyl group, an alkenyl group, etc.), and an aromatic group having 5 to 12 carbon atoms. Examples of the halogen atom include fluorine, chlorine, bromine, and iodine. Q 2 may be a hydrogen atom, a halogen atom, a methyl group, a cyano group, a substituted or unsubstituted benzyl group, or a substituted or unsubstituted phenyl group, for example a hydrogen atom, a methyl group, a chlorine atom, a bromine atom, an iodine atom, or a cyano group, preferably a hydrogen atom, a methyl group, or a chlorine atom, in particular a hydrogen atom or a methyl group.

[0027] R 2 is an alkylene group having 1 to 10 carbon atoms. The alkylene group may be cyclic, linear, or branched, and is preferably linear. The number of carbon atoms in the alkylene group may be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, or 6 or more. The number of carbon atoms in the alkylene group may be 10 or less, 8 or less, 6 or less, 4 or less, or 2 or less, for example, 5 or less.

[0028] [Polymer (III)] The polymer (III) has an alternating sequence (E) consisting of the repeating unit (3) and the repeating unit (4).

[0029] (Alternating Arrangement (E)) The alternating sequence (E) is composed of a repeating unit (3) and a repeating unit (4). That is, the alternating sequence (E) is a sequence formed by alternately bonding the repeating unit (3) and the repeating unit (4), and is represented by the following formula: -[CH2C(-Q 3 )C(=O)OH]-[CH2C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41is an alkylene group having 1 to 10 carbon atoms, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. Each symbol is explained in detail below.

[0030] (Repeating unit (3)) The repeating unit (3) has the following formula: -[CH2C(-Q 3 )C(=O)OH]- [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom. It is expressed as:

[0031] Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom. Examples of the monovalent organic group include a cyano group, an aliphatic hydrocarbon group having 1 to 6 carbon atoms (e.g., an alkyl group, an alkenyl group, etc.), and an aromatic group having 5 to 12 carbon atoms. Examples of the halogen atom include fluorine, chlorine, bromine, and iodine. Q 3 may be a hydrogen atom, a halogen atom, a methyl group, a cyano group, a substituted or unsubstituted benzyl group, or a substituted or unsubstituted phenyl group, for example, a hydrogen atom, a methyl group, a chlorine atom, a bromine atom, an iodine atom, or a cyano group, preferably a hydrogen atom, a methyl group, or a chlorine atom, particularly preferably a hydrogen atom or a methyl group, and more preferably a methyl group.

[0032] (Repeating unit (4)) The repeating unit (4) has the following formula: -[CH2C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms, R 42is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. It is expressed as:

[0033] Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom. Examples of the monovalent organic group include a cyano group, an aliphatic hydrocarbon group having 1 to 6 carbon atoms (e.g., an alkyl group, an alkenyl group, etc.), and an aromatic group having 5 to 12 carbon atoms. Examples of the halogen atom include fluorine, chlorine, bromine, and iodine. Q 4 may be a hydrogen atom, a halogen atom, a methyl group, a cyano group, a substituted or unsubstituted benzyl group, or a substituted or unsubstituted phenyl group, for example, a hydrogen atom, a methyl group, a chlorine atom, a bromine atom, an iodine atom, or a cyano group, preferably a hydrogen atom, a methyl group, or a chlorine atom, particularly preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom.

[0034] R 41 is an alkylene group having 1 to 10 carbon atoms. The alkylene group may be cyclic, linear, or branched, and is preferably linear. The number of carbon atoms in the alkylene group may be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, or 6 or more. The number of carbon atoms in the alkylene group may be 10 or less, 8 or less, 6 or less, 4 or less, or 2 or less, for example, 5 or less.

[0035] R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The hydrocarbon group may be an aromatic hydrocarbon group or an aliphatic hydrocarbon group, preferably an aliphatic hydrocarbon group, and particularly preferably a saturated aliphatic hydrocarbon group (alkyl group). The hydrocarbon group may be cyclic, linear, or branched, preferably linear. The number of carbon atoms in the hydrocarbon group may be 4 or more, 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, 16 or more, or 18 or more, preferably 8 or more, and more preferably 12 or more. The number of carbon atoms in the hydrocarbon group may be 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, or 10 or less, preferably 30 or less, and more preferably 25 or less.

[0036] R42 may contain other groups in addition to the hydrocarbon group having 4 to 40 carbon atoms. Examples of the other groups include ether oxygen and amino groups (e.g., secondary or tertiary amino groups). For example, R 42 may form a branched structure from the nitrogen atom. 42 As the above, one type may be used, or two or more types may be used in combination.

[0037] R 42 Two or more types (e.g., two, three, or four types) of R may be combined. 42 By combining these, it may be possible to impart a number of properties to the polymer. An example of such a combination is a hydrocarbon group having 12 or more carbon atoms (e.g., a chain alkyl group). 42 and a combination of a cyclic hydrocarbon-containing group (e.g., a cycloalkyl-containing group, a phenyl-containing group, etc.). A hydrocarbon group having 12 or more carbon atoms can impart high liquid repellency, and a cyclic hydrocarbon-containing group can impart high heat resistance. 42 When used together, each R 42 is R 42 may be present in an amount of 10 mol % or more, 20 mol % or more, or 30 mol % or more based on the total of

[0038] R 42 The carbon atom ratio of R may be 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 100%, and is preferably 60% or more. 42 The carbon atom ratio of R may be 100% or less, 95% or less, 90% or less, 85% or less, or 80% or less. 42 The carbon atom ratio of R 42 R relative to the total amount of heteroatoms (atoms other than carbon and hydrogen atoms) in 42 R is the molar ratio of the amount of carbon atoms in 42 When the carbon atom ratio is equal to or more than the above lower limit, liquid repellency can be satisfactorily exhibited.

[0039] R 42The molecular weight of R may be 50 or more, 100 or more, 150 or more, 200 or more, 250 or more, or 300 or more. 42 may have a molecular weight of 750 or less, 600 or less, 500 or less, 400 or less, 300 or less, 200 or less, or 100 or less.

[0040] [Other repeating units] The polymers (polymers (I) to (III)) may have other repeating units in addition to the repeating units (1) to (4) described above. Examples of the other repeating units include repeating units derived from a hydrocarbon monomer, a crosslinkable monomer, a halogenated olefin monomer, and / or other monomers.

[0041] (Hydrocarbon monomers) The polymer has the formula: CH2=C(-Q)-C(=O)-XR n [In the formula, Q is a hydrogen atom, a monovalent organic group, or a halogen atom; X is at least one selected from the group consisting of a direct bond, -O-, -C(=O)-, -S(=O)2-, -NR'-, -C(OR')R'-, and -C(OR')(-)2 (wherein R' is independently a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms in each occurrence). 1 and, X is a hydrocarbon group having 1 to 40 carbon atoms. 2 and, is a 1+n valent group consisting of one or more selected from the group consisting of R is an aliphatic hydrocarbon group having 6 to 40 carbon atoms, n is 1 to 3. The copolymer may be a polymer having a repeating unit derived from a hydrocarbon monomer represented by the following formula:

[0042] Q is a hydrogen atom, a monovalent organic group, or a halogen atom. Examples of the monovalent organic group include a cyano group, an aliphatic hydrocarbon group having 1 to 6 carbon atoms (e.g., an alkyl group, an alkenyl group, etc.), and an aromatic group having 5 to 12 carbon atoms. Examples of the halogen atom include fluorine, chlorine, bromine, and iodine. Q may be a hydrogen atom, a halogen atom, a methyl group, a cyano group, a substituted or unsubstituted benzyl group, or a substituted or unsubstituted phenyl group, and is, for example, a hydrogen atom, a methyl group, a chlorine atom, a bromine atom, an iodine atom, or a cyano group, and is preferably a hydrogen atom, a methyl group, or a chlorine atom, and particularly preferably a hydrogen atom or a methyl group.

[0043] X is at least one selected from the group consisting of a direct bond, -O-, -C(=O)-, -S(=O)2-, -NR'-, -C(OR')R'-, and -C(OR')(-)2 (wherein R' is independently a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms in each occurrence). 1 and, X is a hydrocarbon group having 1 to 40 carbon atoms. 2 and, It is a 1+n valent group consisting of one or more selected from the group consisting of: where n may be 1 to 3, 2 to 3, 1 to 2, 1, 2, or 3.

[0044] X is represented by the following formula: -X 1 - or -X 1 -X 2 -X 1 - [In the formula, X 1 is independently in each occurrence -O-, -NR'-, -C(=O)-NR'-, -NR'-C(=O)-, or -NR'-C(=O)-NR'- (R' is a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms); X 2 is a hydrocarbon group having 1 to 40 carbon atoms.] It may be a group represented by the following formula:

[0045] R is a monovalent aliphatic hydrocarbon group having 6 to 40 carbon atoms. R may be cyclic, branched, or linear, preferably branched or linear, and more preferably linear. R is preferably a saturated aliphatic hydrocarbon group (alkyl group).

[0046] The number of carbon atoms in R may be 6 or more, 8 or more, 10 or more, 12 or more, 14 or more, 16 or more, or 18 or more, preferably 10 or more, and more preferably 12 or more. The number of carbon atoms in R may be 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, or 10 or less, preferably 30 or less, and more preferably 25 or less.

[0047] From the viewpoint of liquid repellency, the hydrocarbon monomer may include a hydrocarbon monomer containing an amide group, a urea group, or a urethane group in X. The hydrocarbon monomer may be a combination of a hydrocarbon monomer having an amide group, a urea group, or a urethane group and a hydrocarbon monomer not having an amide group, a urea group, or a urethane group.

[0048] The hydrocarbon monomer may be only a non-cyclic hydrocarbon group-containing monomer, but may also include a cyclic hydrocarbon group-containing monomer. The cyclic hydrocarbon group-containing monomer is a monomer having a cyclic hydrocarbon group, and may be a monomer having one ethylenically unsaturated double bond and a cyclic hydrocarbon group.

[0049] The cyclic hydrocarbon group-containing monomer preferably has a (meth)acrylic group as the ethylenically unsaturated double bond, and may, for example, have a (meth)acrylate group or a (meth)acrylamide group as the ethylenically unsaturated double bond.

[0050] The cyclic hydrocarbon group may be alicyclic or aromatic, preferably alicyclic. The cyclic hydrocarbon group may be saturated or unsaturated, preferably saturated. The cyclic hydrocarbon group may be a monocyclic group, a polycyclic group, or a bridged ring group, preferably a bridged ring group. The cyclic hydrocarbon group may have a chain group (e.g., a straight-chain or branched-chain hydrocarbon group).

[0051] The cyclic hydrocarbon group may have 4 or more, 6 or more, or 8 or more carbon atoms, and may have 30 or less, 26 or less, 22 or less, 18 or less, or 14 or less carbon atoms.

[0052] Specific examples of cyclic hydrocarbon groups include cyclohexyl, t-butylcyclohexyl, adamantyl, 2-methyl-2-adamantyl, 2-ethyl-2-adamantyl, bornyl, isobornyl, norbornyl, dicyclopentanyl, dicyclopentenyl, benzyl, phenyl, naphthyl, 2-t-butylphenyl, residues in which one or more hydrogen atoms have been removed from these groups (e.g., cyclohexylene, adamantylene, phenylene, naphthylene, etc.), and groups which are substitution products thereof.

[0053] Specific examples of the cyclic hydrocarbon group-containing monomer include cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, and compounds in which these acrylates are substituted with acrylamide, etc. These may be used alone or in combination of two or more.

[0054] Specific examples of hydrocarbon monomers are as follows: The compound of the following chemical formula is an acrylic compound in which the α-position is a hydrogen atom, but the α-position may be other Q, for example, a methacryl compound in which the α-position is a methyl group, an α-chloroacrylic compound in which the α-position is a chlorine atom, etc. CH2=CHC(=O)OC p H 2p NHC(=O)C q H 2q+1 CH2=CHC(=O)OC2H4NHC(=O)C17 H 35 CH2=CHC(=O)OC2H4NHC(=O)C 15 H 31 CH2=CHC(=O)OC2H4NHC(=O)C 17 H 35 and CH2=CHC(=O)OC2H4NHC(=O)C 15 H 31 and its mixture CH2=CHC(=O)OC q H 2q+1 CH2=CHC(=O)OC 18 H 37 CH2=CHC(=O)OC 16 H 33 CH2=CHC(=O)OC2H4OC(=O)NHC q H 2q+1 CH2=CHC(=O)OC2H4NHC(=O)OC q H 2q+1 CH2=CHC(=O)OC2H4NHC(=O)NHC q H 2q+1 CH2=CHC(=O)OC4H8OC(=O)NHC q H 2q+1 CH2=CHC(=O)OC2H4OC(=O)NHC 18 H 37 CH2=CHC(=O)OC2H4NHC(=O)OC 18 H 37 CH2=CHC(=O)NHC p H 2p OC(=O)NHC q H 2q+1 CH2=CHC(=O)OC p H 2p-1 (NH(C=O)C q H q+1 )(NH(C=O)C q H q+1 ) CH2=CHC(=O)OC p H 2p-1 (NH(C=O)C 17 H 35 )(NH(C=O)C 17 H 35 ) CH2=CHC(=O)OC p H 2p-1 (O(C=O)NHC q H q+1 )(CH2O(C=O)NHC q H q+1 ) CH2=CHC(=O)OCH2CH(O(C=O)NHC 18 H 37 )(CH2O(C=O)NHC 18 H 37 ) [In the above formula, p is 1 to 40 (for example, 1 to 6), and q is 6 to 40 (for example, 12 to 30).]

[0055] (Halogenated olefin monomers) The polymer may have a repeating unit derived from a halogenated olefin monomer. The halogenated olefin monomer preferably does not have a fluorine atom. The halogenated olefin monomer is preferably an olefin having 2 to 20 carbon atoms substituted with 1 to 10 chlorine atoms, bromine atoms, or iodine atoms. The halogenated olefin monomer is preferably a chlorinated olefin having 2 to 20 carbon atoms, particularly an olefin having 2 to 5 carbon atoms and having 1 to 5 chlorine atoms. Preferred specific examples of the halogenated olefin monomer are vinyl halides, such as vinyl chloride, vinyl bromide, vinyl iodide, and vinylidene halides, such as vinylidene chloride, vinylidene bromide, and vinylidene iodide. Vinyl chloride is preferred because it enhances water repellency (particularly durability of water repellency). The presence of a repeating unit derived from a halogenated olefin monomer enhances the washing durability of the polymer.

[0056] (Cross-linking monomer) The polymer may have a repeat unit derived from a crosslinkable monomer. The crosslinkable monomer is a monomer capable of imparting crosslinkability to the polymer and may have at least two selected from the group consisting of a reactive group and an olefinic carbon-carbon double bond. The crosslinkable monomer may be a compound having at least two ethylenically unsaturated double bonds, or a compound having at least one ethylenically unsaturated double bond and at least one reactive group.

[0057] The crosslinkable monomer preferably has a (meth)acrylic group as the ethylenically unsaturated double bond, and may, for example, have a (meth)acrylate group or a (meth)acrylamide group as the ethylenically unsaturated double bond.

[0058] Examples of the reactive group include a hydroxyl group, an epoxy group, a chloromethyl group, a blocked isocyanate group, an amino group, a carboxyl group, a carbonyl group, and an isocyanate group.

[0059] Specific examples of crosslinkable monomers include diacetone (meth)acrylamide, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylamide, glycidyl (meth)acrylate, hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-acetoacetoxyethyl (meth)acrylate, butadiene, isoprene, chloroprene, vinyl monochloroacetate, vinyl methacrylate, glycidyl (meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, etc. These may be used alone or in combination of two or more. These may be used alone or in combination of two or more.

[0060] (Other monomers) The polymer may contain repeat units derived from monomers other than those mentioned above.

[0061] Specific examples of the other monomers include, for example, acrylonitrile, alkoxy polyalkylene glycol (meth)acrylate, dimethylaminoethyl (meth)acrylate, organosiloxane-containing (meth)acrylate, vinyl acetate, vinyl alkyl ether, etc. The other monomers are not limited to these examples. These may be used alone or in combination of two or more.

[0062] [Polymer composition, etc.] The amount of repeating unit (1) in the polymer may be 5% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 35% by weight or more, 45% by weight or more, 55% by weight or more, or 65% by weight or more, preferably 15% by weight or more. The amount of repeating unit (1) in the polymer may be 90% by weight or less, 80% by weight or less, 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, or 30% by weight or less.

[0063] The amount of repeating unit (2) in the polymer may be 5% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 35% by weight or more, 45% by weight or more, 55% by weight or more, or 65% by weight or more, preferably 15% by weight or more. The amount of repeating unit (2) in the polymer may be 90% by weight or less, 80% by weight or less, 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, or 30% by weight or less.

[0064] The molar ratio of repeating units (1) to repeating units (2) in the polymer (repeating unit (1) / repeating unit (2)) may be 0.5 or more, 0.75 or more, or 0.95 or more. The molar ratio of repeating units (1) to repeating units (2) in the polymer (repeating unit (1) / repeating unit (2)) may be 2 or less, 1.5 or less, 1.25 or less, or 1.05 or less.

[0065] The amount of the alternating sequence (A) in the polymer may be 10% by weight or more, 30% by weight or more, 50% by weight or more, 70% by weight or more, 90% by weight or more, and preferably 30% by weight or more. The amount of the alternating sequence (A) in the polymer may be 100% by weight or less, 80% by weight or less, 60% by weight or less, 40% by weight or less, or 20% by weight or less.

[0066] The amount of repeating unit (3) in the polymer may be 5% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 35% by weight or more, 45% by weight or more, 55% by weight or more, or 65% by weight or more. The amount of repeating unit (3) in the polymer may be 90% by weight or less, 80% by weight or less, 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, or 30% by weight or less.

[0067] The amount of repeating unit (4) in the polymer may be 5% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 35% by weight or more, 45% by weight or more, 55% by weight or more, or 65% by weight or more. The amount of repeating unit (4) in the polymer may be 90% by weight or less, 80% by weight or less, 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, or 30% by weight or less.

[0068] The molar ratio of repeating units (3) to repeating units (4) in the polymer (repeating unit (3) / repeating unit (4)) may be 0.5 or more, 0.75 or more, or 0.95 or more. The molar ratio of repeating units (1) to repeating units (2) in the polymer (repeating unit (3) / repeating unit (4)) may be 2 or less, 1.5 or less, 1.25 or less, or 1.05 or less.

[0069] The amount of the alternating sequence (E) in the polymer may be 10% by weight or more, 30% by weight or more, 50% by weight or more, 70% by weight or more, 90% by weight or more, and preferably 30% by weight or more. The amount of the alternating sequence (E) in the polymer may be 100% by weight or less, 80% by weight or less, 60% by weight or less, 40% by weight or less, or 20% by weight or less.

[0070] The amount of other repeating units contained in the polymer may be 10% by weight or more, 30% by weight or more, or 50% by weight or more in the polymer. The amount of other repeating units contained in the polymer may be 60% by weight or less, 40% by weight or less, or 20% by weight or less in the polymer.

[0071] The number average molecular weight (Mn) of the polymer may be 500 or more, 1000 or more, 2500 or more, 5000 or more, 10000 or more, 25000 or more, or 50000 or more, and is preferably 5000 or more. The number average molecular weight (Mn) of the polymer may be 1000000 or less, 500000 or less, 250000 or less, 100000 or less, 50000 or less, 25000 or less, or 10000 or less, and is preferably 100000 or less.

[0072] The Mw / Mn of the polymer may be 1 or more, 1.2 or more, 1.5 or more, or 1.7 or more. The Mw / Mn of the polymer may be 5 or less, 4.5 or less, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, or 1.5 or less.

[0073] The melting point of the polymer may be 30° C. or more, 40° C. or more, 60° C. or more, 80° C. or more, 100° C. or more, or 120° C. or more, and is preferably 50° C. or more, for example 100° C. or more. The melting point of the polymer may be 250° C. or less, 200° C. or less, 150° C. or less, 100° C. or less, or 50° C. or less. The polymer may have no melting point.

[0074] The glass transition temperature of the polymer may be 30° C. or more, 40° C. or more, 60° C. or more, 80° C. or more, 100° C. or more, or 120° C. or more, and is preferably 30° C. or more, for example 50° C. or more or 75° C. or more. The glass transition temperature of the polymer may be 250° C. or less, 200° C. or less, 150° C. or less, 100° C. or less, or 50° C. or less.

[0075] [Method for producing polymer (I)] The method for producing the polymer (I) is not limited, but it may be produced, for example, by copolymerization of a monomer that derives the repeating unit (1) and a monomer that derives the repeating unit (2).

[0076] An example of a monomer from which the repeating unit (1) is derived is the following formula: CH2=C(-Q 1 )C(=O)R 1 [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 1 is -NH(R 11 ) or -N(R 11 )2, where R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. It is a compound represented by Q 1 and R 1 The details are as explained above.

[0077] An example of a monomer from which the repeating unit (2) is derived is the following formula: CH2=C(-Q 2 )C(=O)NHR 2 OH [In the formula, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 2 is an alkylene group having 1 to 10 carbon atoms. It is a compound represented by Q 2 and R 2 The details are as explained above.

[0078] The copolymerization method is not limited, and any known polymerization method can be selected, and the polymerization reaction conditions can be arbitrarily selected. Examples of such polymerization methods include solution polymerization, suspension polymerization, emulsion polymerization, and condensation polymerization.

[0079] In solution polymerization, a method is adopted in which a monomer is dissolved in an organic solvent in the presence of a polymerization initiator, and after nitrogen substitution, the mixture is heated and stirred at a temperature in the range of 30 to 120°C for 1 to 10 hours. Examples of the polymerization initiator include azobisisobutyronitrile, benzoyl peroxide, di-t-butyl peroxide, lauryl peroxide, cumene hydroperoxide, t-butyl peroxypivalate, and diisopropyl peroxydicarbonate. The polymerization initiator is used in an amount of 0.01 to 20 parts by weight, for example, 0.01 to 10 parts by weight, based on 100 parts by weight of the monomer.

[0080] The organic solvent is inactive to the monomers and dissolves them, and may be, for example, an aprotic polar solvent (e.g., DMSO, DMF), an ester (e.g., an ester having 2 to 40 carbon atoms, specifically, ethyl acetate, butyl acetate), a ketone (e.g., a ketone having 2 to 40 carbon atoms, specifically, methyl ethyl ketone, diisobutyl ketone, methyl isobutyl ketone), or an alcohol (e.g., an alcohol having 1 to 40 carbon atoms, specifically, ethanol, butanol, isopropyl alcohol). Specific examples of the organic solvent include acetone, chloroform, HCHC225, isopropyl alcohol, cyclohexane, benzene, toluene, xylene, petroleum ether, tetrahydrofuran, 1,4-dioxane, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, ethyl acetate, butyl acetate, 1,1,2,2-tetrachloroethane, 1,1,1-trichloroethane, trichloroethylene, perchloroethylene, tetrachlorodifluoroethane, trichlorotrifluoroethane, and the like. The organic solvent is used in an amount of 10 to 3000 parts by weight, for example, 50 to 2000 parts by weight, based on 100 parts by weight of the total of the monomers.

[0081] In emulsion polymerization, a method is adopted in which a monomer is emulsified in water in the presence of a polymerization initiator and an emulsifier, and after nitrogen substitution, the monomer is polymerized by stirring at a temperature in the range of 50 to 80°C for 1 to 20 hours. As the polymerization initiator, water-soluble initiators such as benzoyl peroxide, lauroyl peroxide, t-butyl perbenzoate, 1-hydroxycyclohexyl hydroperoxide, 3-carboxypropionyl peroxide, acetyl peroxide, azobisisobutylamidine dihydrochloride, sodium peroxide, potassium persulfate, and ammonium persulfate, and oil-soluble initiators such as azobisisobutyronitrile, benzoyl peroxide, di-t-butyl peroxide, lauryl peroxide, cumene hydroperoxide, t-butyl peroxypivalate, and diisopropyl peroxydicarbonate are used. The polymerization initiator is used in the range of 0.01 to 10 parts by weight relative to 100 parts by weight of the monomer.

[0082] In order to obtain a polymer aqueous dispersion having excellent shelf stability, it is desirable to polymerize the monomer by dispersing it in water into fine particles using an emulsifier capable of applying strong crushing energy such as a high-pressure homogenizer or an ultrasonic homogenizer. As the emulsifier, various anionic, cationic or nonionic emulsifiers can be used, and are used in the range of 0.5 to 20 parts by weight per 100 parts by weight of the monomer. It is preferable to use an anionic and / or nonionic and / or cationic emulsifier. When the monomers are not completely compatible with each other, it is preferable to add a compatibilizer that can sufficiently make these monomers compatible, such as a water-soluble organic solvent or a low molecular weight monomer. The addition of a compatibilizer can improve emulsifiability and copolymerizability.

[0083] The water-soluble organic solvent may be the organic solvent described above. For example, acetone, methyl ethyl ketone, ethyl acetate, propylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol, tripropylene glycol, ethanol, etc. may be used in an amount of 1 to 50 parts by weight, for example, 10 to 40 parts by weight, based on 100 parts by weight of water. In addition, the low molecular weight monomer may be methyl methacrylate, glycidyl methacrylate, 2,2,2-trifluoroethyl methacrylate, etc., may be used in an amount of 1 to 50 parts by weight, for example, 10 to 40 parts by weight, based on 100 parts by weight of the total amount of the monomers.

[0084] In the polymerization, a chain transfer agent may be used. The molecular weight of the polymer can be changed depending on the amount of the chain transfer agent used. Examples of the chain transfer agent include mercaptan group-containing compounds such as lauryl mercaptan, thioglycol, and thioglycerol (particularly alkyl mercaptans (e.g., having 1 to 40 carbon atoms)), and inorganic salts such as sodium hypophosphite and sodium hydrogen sulfite. The amount of the chain transfer agent used may be in the range of 0.01 to 10 parts by weight, for example, 0.1 to 5 parts by weight, based on 100 parts by weight of the total amount of the monomers.

[0085] [Method for producing polymer (II)] The method for producing the polymer (II) comprises the steps of: The formula: CH2=C(-Q 1 )C(=O)-X A -OR 2 NHC(=O)C(-Q 2 )=CH2 [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, X A is a group removable by aminolysis, R 2 is an alkylene group having 1 to 10 carbon atoms, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom. to obtain a precursor (A) by cyclopolymerizing a divinyl monomer (A) represented by the formula: The precursor (A) and The formula: NH2(R 11 ) or NH(R 11 )2 [In the formula, R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. With an amine compound represented by the formula:

[0086] (Step of cyclopolymerizing divinyl monomer (A) to obtain precursor (A)) In this step, the divinyl monomer (A) is cyclically polymerized to obtain a precursor (A). By using the cyclic polymerization, it is possible to obtain a polymer (II) which is an alternating copolymer.

[0087] Divinyl monomer (A) is The formula: CH2=C(-Q 1 )C(=O)-X A -OR 2 NHC(=O)C(-Q 2 )=CH2 [In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, X A is a group removable by aminolysis, R 2 is an alkylene group having 1 to 10 carbon atoms, Q 2 is a hydrogen atom, a monovalent organic group, or a halogen atom. It is expressed as:

[0088] Q 1 , R 2 , and Q 2 The details are as explained above.

[0089] X Ais a group that can be removed by aminolysis. Here, aminolysis refers to a reaction in which an ester reacts with an amine to cleave the ester. X A -OR A may be a group represented by -(C=O)-, where R A R is an organic group, which may be a hydrocarbon group or a derivative thereof. A R may be an aromatic group (e.g., a phenylene group (e.g., a 1,2-phenylene group)), for example, an aromatic group having a substituent, and in particular an aromatic group having an electron-withdrawing group (e.g., -CF3, -CCl3, -NO2, -CN, etc.) that is activated for aminolysis reaction. A The molecular weight of R may be 150 or less, or 100 or less. A The number of carbon atoms in R may be 10 or less, 8 or less, or 6 or less. A Specific examples of the alkyl group include a 3-trifluoromethyl-1,2-phenylene group, a 5-trifluoromethyl-1,2-phenylene group, a 3,5-bis(trifluoromethyl)-1,2-phenylene group, a 3-trichloromethyl-1,2-phenylene group, a 5-trichloromethyl-1,2-phenylene group, a 3,5-bis(trichloromethyl)-1,2-phenylene group, and a 4-nitro-1,2-phenylene group.

[0090] The method of cyclic polymerization is not limited, and a known polymerization method can be selected, and the polymerization reaction conditions can be selected arbitrarily. Examples of such polymerization methods include solution polymerization, suspension polymerization, emulsion polymerization, and condensation polymerization. The details of the polymerization method are as described above.

[0091] The precursor (A) is TIFF2024153749000001.tif3457[In the formula, Q 1 is a hydrogen atom, a monovalent organic group, or a halogen atom, X A is a group removable by aminolysis, R 2 is an alkylene group having 1 to 10 carbon atoms, Q 2is a hydrogen atom, a monovalent organic group, or a halogen atom. It is a polymer having a repeating unit represented by the following formula:

[0092] (Step of reacting precursor (A) with an amine compound) In this step, the precursor (A) is reacted with an amine compound, whereby the ester in the precursor (A) reacts with the amine and is cleaved to give the polymer (II).

[0093] Amine compounds are The formula: NH2(R 11 ) or NH(R 11 )2 [In the formula, R 11 is independently in each occurrence a monovalent organic group having a hydrocarbon group having from 4 to 40 carbon atoms. It is expressed as:

[0094] R 11 The details are as explained above.

[0095] The reaction conditions for the precursor (A) and the amine compound can be appropriately set, and for example, the reaction may be carried out at 20° C. to 80° C. for 3 hours to 48 hours.

[0096] The amine compound is a polymer (II) having two or more R 11 Two or more amine compounds may be used, such as

[0097] [Method for producing polymer (III)] The method for producing the polymer (III) comprises the steps of: The formula: CH2=C(-Q 3 )C(=O)OX E -OR 41 -OC(=O)C(-Q 4 )=CH2 [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom, X Eis a group removable by acidolysis, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms. a step of cyclopolymerizing a divinyl monomer (E) represented by the formula: The precursor (E1) is decomposed with an acid to obtain X E to obtain a precursor (E2); and The precursor (E2) The formula: R 42 -NCO [In the formula, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. With an isocyanate compound represented by the formula (I),

[0098] (Step of cyclopolymerizing divinyl monomer (E) to obtain precursor (E1)) In this step, the divinyl monomer (E) is cyclically polymerized to obtain the precursor (A). By using the cyclic polymerization, it is possible to obtain the polymer (III), which is an alternating copolymer.

[0099] Divinyl monomer (E) is The formula: CH2=C(-Q 3 )C(=O)OX E -OR 41 -OC(=O)C(-Q 4 )=CH2 [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom, X E is a group removable by acidolysis, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms. It is expressed as:

[0100] Q 3 , Q 4 , and R 41 The details are as explained above.

[0101] X E is a group removable by acidolysis. E -CHR E -or-C(R E )2-, which may form an acetal structure. E R is an organic group, which may be a hydrocarbon group or a derivative thereof. A R may be an aliphatic group, for example an aliphatic hydrocarbon group, in particular an alkyl group. E The molecular weight of R may be 150 or less, or 100 or less. E The number of carbon atoms in R may be 8 or less, 6 or less, 4 or less, 3 or less, or 2 or less. E Specific examples include a methyl group, an ethyl group, and a propyl group.

[0102] The method of cyclic polymerization is not limited, and a known polymerization method can be selected, and the polymerization reaction conditions can be selected arbitrarily. Examples of such polymerization methods include solution polymerization, suspension polymerization, emulsion polymerization, and condensation polymerization. The details of the polymerization method are as described above.

[0103] The precursor (E1) is The formula: TIFF2024153749000002.tif2841[in the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom, X E is a group removable by acidolysis, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms. It is a polymer having a repeating unit represented by the following formula:

[0104] (Precursor (E1) to X E to obtain a precursor (E2) In this step, the precursor (E1) is decomposed with an acid to obtain X E is removed to obtain the precursor (E2).

[0105] The conditions for the acid decomposition are not limited and can be set appropriately. For example, the reaction may be carried out at 20° C. to 80° C. for 3 hours to 48 hours.

[0106] The precursor (E2) is The formula: TIFF2024153749000003.tif3141[in the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms. It is a polymer having a repeating unit represented by the following formula:

[0107] (Step of reacting precursor (E2) with an isocyanate compound) In this step, the precursor (E2) is reacted with an isocyanate compound, whereby a hydroxy group in the precursor (E2) reacts with an isocyanate group in the isocyanate compound to produce a polymer (III).

[0108] Isocyanate compounds The formula: R 42 -NCO [In the formula, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. It is expressed as:

[0109] R 42 For details, the explanation of the polymer mentioned above can be referred to.

[0110] The reaction conditions for the precursor (E2) and the isocyanate compound can be appropriately set, and for example, the reaction may be carried out at 20° C. to 80° C. for 3 hours to 48 hours.

[0111] The isocyanate compound is a compound having two or more types of polymer (III) R 42 Two or more amine compounds may be used, such as

[0112] [Amount of polymer] The amount of the polymer in the repellent may be 0.01% by weight or more, 0.5% by weight or more, 1% by weight or more, 3% by weight or more, 5% by weight or more, 10% by weight or more, 20% by weight or more, or 30% by weight or more. The amount of the polymer in the repellent may be 60% by weight or less, 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, 10% by weight or less, 5% by weight or less, or 3% by weight or less.

[0113] [Liquid medium] The repellent agent of the present disclosure may comprise a liquid medium. The liquid medium may be water, an organic solvent, or a mixture of water and an organic solvent. The repellent agent may be a dispersion or a solution.

[0114] Examples of the organic solvent include esters (e.g., esters having 2 to 40 carbon atoms, specifically, ethyl acetate, butyl acetate), ketones (e.g., ketones having 2 to 40 carbon atoms, specifically, methyl ethyl ketone, diisobutyl ketone), alcohols (e.g., alcohols having 1 to 40 carbon atoms, specifically, isopropyl alcohol), aromatic solvents (e.g., toluene and xylene), and petroleum solvents (e.g., alkanes having 5 to 10 carbon atoms, specifically, naphtha, kerosene). The organic solvent is preferably a water-soluble organic solvent. The water-soluble organic solvent may contain a compound having at least one hydroxyl group (e.g., polyhydric alcohols such as alcohols, glycol-based solvents, ethers of polyhydric alcohols (e.g., monoethers), etc.). These may be used alone or in combination of two or more.

[0115] [Amount of liquid medium] The amount of the liquid medium may be 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 100 parts by weight or more, 200 parts by weight or more, 300 parts by weight or more, 500 parts by weight or more, or 1000 parts by weight or more, relative to 1 part by weight of the polymer. The amount of the liquid medium may be 3000 parts by weight or less, 2000 parts by weight or less, 1000 parts by weight or less, 500 parts by weight or less, 200 parts by weight or less, 175 parts by weight or less, 150 parts by weight or less, 125 parts by weight or less, 100 parts by weight or less, 80 parts by weight or less, 60 parts by weight or less, 40 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, relative to 1 part by weight of the polymer.

[0116] The amount of water may be 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 100 parts by weight or more, 200 parts by weight or more, 300 parts by weight or more, 500 parts by weight or more, or 1000 parts by weight or more, relative to 1 part by weight of the polymer. The amount of water may be 3000 parts by weight or less, 2000 parts by weight or less, 1000 parts by weight or less, 500 parts by weight or less, 200 parts by weight or less, 175 parts by weight or less, 150 parts by weight or less, 125 parts by weight or less, 100 parts by weight or less, 80 parts by weight or less, 60 parts by weight or less, 40 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, relative to 1 part by weight of the polymer.

[0117] The amount of the organic solvent may be 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, 30 parts by weight or more, 40 parts by weight or more, 50 parts by weight or more, 100 parts by weight or more, 200 parts by weight or more, 300 parts by weight or more, 500 parts by weight or more, or 1000 parts by weight or more, relative to 1 part by weight of the polymer. The amount of the organic solvent may be 3000 parts by weight or less, 2000 parts by weight or less, 1000 parts by weight or less, 500 parts by weight or less, 200 parts by weight or less, 175 parts by weight or less, 150 parts by weight or less, 125 parts by weight or less, 100 parts by weight or less, 80 parts by weight or less, 60 parts by weight or less, 40 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, relative to 1 part by weight of the polymer.

[0118] [Surfactant] The repellent may include a surfactant, which may include one or more surfactants selected from a nonionic surfactant, a cationic surfactant, an anionic surfactant, and an amphoteric surfactant.

[0119] [Nonionic surfactants] Examples of nonionic surfactants include ethers, esters, ester ethers, alkanolamides, polyhydric alcohols and amine oxides.

[0120] An example of an ether is a compound having an oxyalkylene group (preferably a polyoxyethylene group).

[0121] An example of the ester is an ester of an alcohol and a fatty acid. An example of the alcohol is a monohydric to hexahydric (particularly dihydric to pentahydric) alcohol (e.g., an aliphatic alcohol) having 1 to 50 carbon atoms (particularly 10 to 30 carbon atoms). An example of the fatty acid is a saturated or unsaturated fatty acid having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms.

[0122] An example of the ester ether is a compound in which an alkylene oxide (particularly ethylene oxide) is added to an ester of an alcohol and a fatty acid. An example of the alcohol is a monohydric to hexahydric (particularly dihydric to pentahydric) alcohol (e.g., aliphatic alcohol) having 1 to 50 carbon atoms (particularly 3 to 30 carbon atoms). An example of the fatty acid is a saturated or unsaturated fatty acid having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms.

[0123] An example of an alkanolamide is formed from a fatty acid and an alkanolamine. The alkanolamide may be a monoalkanolamide or a dialkanolamine. An example of a fatty acid is a saturated or unsaturated fatty acid having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms. The alkanolamine may be an alkanol having 2 to 50 carbon atoms, particularly 5 to 30 carbon atoms, having 1 to 3 amino groups and 1 to 5 hydroxyl groups.

[0124] The polyhydric alcohol may be a dihydric to pentahydric alcohol having 10 to 30 carbon atoms. The amine oxide may be an oxide (eg, having 5 to 50 carbon atoms) of an amine (secondary amine or preferably tertiary amine).

[0125] The nonionic surfactant is preferably a nonionic surfactant having an oxyalkylene group (preferably a polyoxyethylene group). The number of carbon atoms in the alkylene group in the oxyalkylene group is preferably 2 to 10. The number of oxyalkylene groups in the molecule of the nonionic surfactant is generally preferably 2 to 100. The nonionic surfactant is selected from the group consisting of ethers, esters, ester ethers, alkanolamides, polyhydric alcohols and amine oxides, and is preferably a nonionic surfactant having an oxyalkylene group.

[0126] The nonionic surfactant may be an alkylene oxide adduct of a linear and / or branched aliphatic (saturated and / or unsaturated) group, a polyalkylene glycol ester of a linear and / or branched fatty acid (saturated and / or unsaturated), a polyoxyethylene (POE) / polyoxypropylene (POP) copolymer (random copolymer or block copolymer), an alkylene oxide adduct of acetylene glycol, etc. Among these, those in which the structure of the alkylene oxide adduct portion and the polyalkylene glycol portion is polyoxyethylene (POE) or polyoxypropylene (POP) or a POE / POP copolymer (which may be a random copolymer or a block copolymer) are preferred. Moreover, the nonionic surfactant preferably has a structure that does not contain an aromatic group in view of environmental issues (biodegradability, environmental hormones, etc.).

[0127] The nonionic surfactant has the formula: R 1 O-(CH2CH2O) p -(R 2 O) q -R 3 [In the formula, R 1 is an alkyl group having 1 to 22 carbon atoms or an alkenyl group or acyl group having 2 to 22 carbon atoms, R 2 each is independently the same or different and is an alkylene group having 3 or more carbon atoms (e.g., 3 to 10), R 3 is a hydrogen atom, an alkyl group having 1 to 22 carbon atoms, or an alkenyl group having 2 to 22 carbon atoms, p is a number equal to or greater than 2, q is a number equal to or greater than 0. The compound may be represented by the formula:

[0128] R 1 R preferably has 8 to 20 carbon atoms, particularly preferably 10 to 18 carbon atoms. 1 Preferred specific examples include a lauryl group, a tridecyl group, and an oleyl group. R 2 Examples are a propylene group and a butylene group. In the nonionic surfactant, p may be a number of 3 or more (for example, 5 to 200). q may be a number of 2 or more (for example, 5 to 200). That is, -(R 2 O) q may form a polyoxyalkylene chain. The nonionic surfactant may be a polyoxyethylene alkylene alkyl ether containing a hydrophilic polyoxyethylene chain and a hydrophobic oxyalkylene chain (particularly, a polyoxyalkylene chain) in the center. Examples of the hydrophobic oxyalkylene chain include an oxypropylene chain, an oxybutylene chain, and a styrene chain, and among these, an oxypropylene chain is preferred.

[0129] Specific examples of nonionic surfactants include ethylene oxide and hexylphenol, isooctatylphenol, hexadecanol, oleic acid, alkanes (C 12 -C 16 ) Thiol, Sorbitan Mono Fatty Acid (C7-C 19 ) or alkyl(C 12 -C 18 ) amines and the like.

[0130] The proportion of the polyoxyethylene block may be 5 to 80% by weight, for example 30 to 75% by weight, particularly 40 to 70% by weight, based on the molecular weight of the nonionic surfactant (copolymer). The average molecular weight of the nonionic surfactant is generally 300 to 5,000, for example, 500 to 3,000. The nonionic surfactant may be a mixture of a compound having an HLB (hydrophilic-hydrophobic balance) of less than 15 (particularly 5 or less) and a compound having an HLB of 15 or more. An example of a compound having an HLB of less than 15 is a sorbitan fatty acid ester. An example of a compound having an HLB of 15 or more is a polyoxyethylene alkyl ether. The weight ratio of the compound having an HLB of less than 15 to the compound having an HLB of 15 or more may be 90:10 to 20:80, for example 85:15 to 55:45. The nonionic surfactant may be used alone or in combination of two or more kinds.

[0131] [Cationic surfactants] The cationic surfactant is preferably a compound having no amide group.

[0132] The cationic surfactant may be an amine salt, a quaternary ammonium salt, or an oxyethylene adduct ammonium salt.Specific examples of the cationic surfactant include, but are not limited to, amine salt surfactants such as alkylamine salts, amino alcohol fatty acid derivatives, polyamine fatty acid derivatives, imidazoline, etc., alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, alkyl dimethyl benzyl ammonium salts, pyridinium salts, alkyl isoquinolinium salts, and quaternary ammonium salt surfactants such as benzethonium chloride.

[0133] Preferred examples of the cationic surfactant are: R 21 -N + (-R 22 )(-R 23 )(-R 24 )X - [In the formula, R 21 , R22 , R 23 and R 24 is a hydrocarbon group having 1 to 40 carbon atoms, X is an anionic group. It is a compound of the formula: R 21 , R 22 , R 23 and -R 24 Specific examples of X include alkyl groups (e.g., methyl, butyl, stearyl, and palmityl groups). Specific examples of X include halogens (e.g., chlorine) and acids (e.g., hydrochloric acid and acetic acid). The cationic surfactant is particularly preferably a monoalkyltrimethylammonium salt (alkyl having 4 to 40 carbon atoms).

[0134] The cationic surfactant is preferably an ammonium salt. The cationic surfactant has the formula: R 1 p -N + R 2 q X - [In the formula, R 1 is C12 or higher (e.g. C 12 ~C 50 ) linear and / or branched aliphatic (saturated and / or unsaturated) groups, R 2 is H or a C1-4 alkyl group, a benzyl group, a polyoxyethylene group (the number of oxyethylene groups is, for example, 1 (particularly 2, particularly 3) to 50); (CH3, C2H5 are particularly preferred), X is a halogen atom (for example), a C1-C4 fatty acid base, p is 1 or 2, q is 2 or 3, and p+q=4. R 1 may have 12 to 50 carbon atoms, for example, 12 to 30 carbon atoms.

[0135] Specific examples of cationic surfactants include dodecyltrimethylammonium acetate, trimethyltetradecylammonium chloride, hexadecyltrimethylammonium bromide, trimethyloctadecylammonium chloride, (dodecylmethylbenzyl)trimethylammonium chloride, benzyldodecyldimethylammonium chloride, methyldodecyldi(hydropolyoxyethylene)ammonium chloride, benzyldodecyldi(hydropolyoxyethylene)ammonium chloride, and N-[2-(diethylamino)ethyl]oleamide hydrochloride.

[0136] [Anionic surfactants] Examples of anionic surfactants include alkyl ether sulfates, alkyl sulfates, alkenyl ether sulfates, alkenyl sulfates, olefin sulfonates, alkanesulfonates, saturated or unsaturated fatty acid salts, alkyl or alkenyl ether carboxylates, α-sulfonic fatty acid salts, N-acylamino acid type surfactants, phosphoric acid mono- or diester type surfactants, and sulfosuccinic acid esters.

[0137] [Amphoteric surfactants] Examples of amphoteric surfactants include alanines, imidazolinium betaines, amido betaines, and betaine acetate. Specific examples include lauryl betaine, stearyl betaine, lauryl carboxymethyl hydroxyethyl imidazolinium betaine, lauryl dimethylamino acetate betaine, and fatty acid amidopropyl dimethylamino acetate betaine.

[0138] The surfactant may be a nonionic surfactant, a cationic surfactant, or an amphoteric surfactant, each of which may be one type or a combination of two or more types.

[0139] [Amount of surfactant] The amount of the surfactant may be 0.01 parts by weight or more, 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the polymer. The amount of the surfactant may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, or 1 part by weight or less, relative to 100 parts by weight of the polymer. It may be.

[0140] 〔silicone〕 The repellent in the present disclosure may contain silicone (polyorganosiloxane). By containing silicone, it is possible to obtain good texture and durability in addition to good liquid repellency.

[0141] As the silicone, known silicones can be used, and examples of silicones include polydimethylsiloxane and modified silicones (amino-modified, epoxy-modified silicone, carboxy-modified silicone, methylhydrogen silicone, etc.). The silicone may be a silicone wax having wax-like properties. These may be used alone or in combination of two or more.

[0142] The weight average molecular weight of the silicone may be 1000 or more, 10000 or more, or 50000 or more. The weight average molecular weight of the silicone may be 500000 or less, 2500000 or less, 100000 or less, or 50000 or less.

[0143] [Amount of silicone] The amount of silicone may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, based on 100 parts by weight of the polymer. The amount of silicone may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less, based on 100 parts by weight of the polymer.

[0144] 〔wax〕 The repellent in the present disclosure may contain a wax. By containing a wax, it is possible to impart good liquid repellency to the substrate.

[0145] Examples of waxes include paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyolefin wax (polyethylene wax, polypropylene wax, etc.), oxidized polyolefin wax, silicone wax, animal and vegetable wax, mineral wax, etc. Paraffin wax is preferred. Specific examples of compounds constituting the wax include normal alkanes (e.g., tricosane, tetracosane, pentacosane, hexacosane, heptacosane, octacosane, nonacosane, triacontane, hentriacontane, dotriacontane, tritriacontane, tetratriacontane, pentatriacontane, hexatriacontane), and normal alkenes (e.g., 1-eicosene, 1-docosene, 1-tricosene, 1-tetracosene, 1-pentacosene, 1-hexacosene, 1-heptacosene, 1-octacosene, nonacosane, triacontane, hentriacontane, dotriacontane, tritriacontane, tetratriacontane, pentatriacontane, hexatriacontane). The carbon number of the compound constituting the wax is preferably 20 to 60, for example, 25 to 45. The molecular weight of the wax may be from 200 to 2000, for example, from 250 to 1500, or from 300 to 1000. These may be used alone or in combination of two or more.

[0146] The melting point of the wax may be 50° C. or higher, 55° C. or higher, 60° C. or higher, 65° C. or higher, or 70° C. or higher, preferably 55° C. or higher, more preferably 60° C. or higher. The melting point of the wax is measured in accordance with JIS K 2235-1991.

[0147] [Amount of wax] The amount of wax may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, based on 100 parts by weight of the polymer. The amount of wax may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less, based on 100 parts by weight of the polymer.

[0148] [Organic acid] The repellent may contain an organic acid. As the organic acid, a known one may be used. As the organic acid, carboxylic acid, sulfonic acid, sulfinic acid, etc. are preferably mentioned, and carboxylic acid is particularly preferable. As the carboxylic acid, formic acid, acetic acid, propionic acid, butyric acid, oxalic acid, succinic acid, glutaric acid, adipic acid, malic acid, citric acid, etc. are mentioned, and formic acid or acetic acid is particularly preferable. In the present disclosure, the organic acid may be used alone or in combination of two or more kinds. For example, formic acid and acetic acid may be used in combination.

[0149] [Amount of organic acid] The amount of the organic acid may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the polymer. The amount of the organic acid may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less, relative to 100 parts by weight of the polymer. The amount of the organic acid may be adjusted so that the pH of the repellent is 3 to 10, for example, 5 to 9, particularly 6 to 8. The repellent may be acidic (pH 7 or less, for example 6 or less).

[0150] [Hardening agent] The repellent agent may include a curing agent (an active hydrogen reactive compound or an active hydrogen containing compound).

[0151] The curing agent (crosslinking agent) in the repellent can cure the polymer well. The curing agent may be an active hydrogen reactive compound or an active hydrogen-containing compound that reacts with the active hydrogen or active hydrogen reactive group of the polymer. Examples of the active hydrogen reactive compound are isocyanate compounds, epoxy compounds, chloromethyl group-containing compounds, carboxyl group-containing compounds, and hydrazide compounds. Examples of the active hydrogen-containing compound are hydroxyl group-containing compounds, amino group-containing compounds, carboxyl group-containing compounds, ketone group-containing compounds, hydrazide compounds, and melamine compounds.

[0152] The curing agent may include an isocyanate compound. The isocyanate compound may be a polyisocyanate compound. The polyisocyanate compound is a compound having two or more isocyanate groups in one molecule. The polyisocyanate compound acts as a crosslinking agent. Examples of the polyisocyanate compound include aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, aromatic polyisocyanates, and derivatives of these polyisocyanates. The isocyanate compound may be a blocked isocyanate compound (e.g., a blocked polyisocyanate compound). The blocked isocyanate compound is a compound in which the isocyanate group of the isocyanate compound is masked with a blocking agent to suppress the reaction.

[0153] Examples of aliphatic polyisocyanates are trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, 2,6-di ... Aliphatic diisocyanates such as cyanatomethyl caproate, and aliphatic triisocyanates such as lysine ester triisocyanate, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane, etc. These may be used alone or in combination of two or more.

[0154] Examples of alicyclic polyisocyanates include alicyclic diisocyanates and alicyclic triisocyanates. Specific examples of alicyclic polyisocyanates include 1,3-cyclopentene diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate), and 1,3,5-triisocyanatocyclohexane. These may be used alone or in combination of two or more.

[0155] Examples of the araliphatic polyisocyanate are araliphatic diisocyanate and araliphatic triisocyanate.Specific examples of the araliphatic polyisocyanate are 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene (tetramethylxylylene diisocyanate) or a mixture thereof, and 1,3,5-triisocyanatomethylbenzene.These may be used alone or in combination of two or more.

[0156] Examples of aromatic polyisocyanates are aromatic diisocyanates, aromatic triisocyanates, and aromatic tetraisocyanates. Specific examples of aromatic polyisocyanates are m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4'- or 4,4'-diphenylmethane diisocyanate or a mixture thereof, 2,4- or 2,6-tolylene diisocyanate or a mixture thereof, triphenylmethane-4,4',4''-triisocyanate, and 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate. These may be used alone or in combination of two or more.

[0157] Examples of the polyisocyanate derivatives include various derivatives of the above-mentioned polyisocyanate compounds, such as dimers, trimers, biurets, allophanates, carbodiimides, uretdione, uretoimine, isocyanurates, iminooxadiazinedione, etc. These may be used alone or in combination of two or more.

[0158] These polyisocyanates can be used alone or in combination of two or more. As the polyisocyanate compound, it is preferable to use a blocked polyisocyanate compound (blocked isocyanate), which is a compound in which the isocyanate group of the polyisocyanate compound is blocked with a blocking agent. It is preferable to use a blocked polyisocyanate compound because it is relatively stable even in a solution and can be used in the same solution as the repellent.

[0159] The blocking agent blocks free isocyanate groups. When the blocked polyisocyanate compound is heated to, for example, 100°C or higher, for example, 130°C or higher, the isocyanate group is regenerated and can easily react with the hydroxyl group. Examples of the blocking agent include phenol-based compounds, lactam-based compounds, aliphatic alcohol-based compounds, and oxime-based compounds. The polyisocyanate compounds can be used alone or in combination of two or more kinds.

[0160] The epoxy compound is a compound having an epoxy group. Examples of the epoxy compound include epoxy compounds having a polyoxyalkylene group, such as polyglycerol polyglycidyl ether and polypropylene glycol diglycidyl ether; and sorbitol polyglycidyl ether. The chloromethyl group-containing compound is a compound having a chloromethyl group. An example of the chloromethyl group-containing compound is chloromethyl polystyrene. The carboxyl group-containing compound is a compound having a carboxyl group. Examples of the carboxyl group-containing compound include (poly)acrylic acid and (poly)methacrylic acid.

[0161] Specific examples of the ketone group-containing compound include (poly)diacetone acrylamide and diacetone alcohol. Specific examples of the hydrazide compound include hydrazine, carbohydrazide, adipic acid hydrazide, and the like. Specific examples of the melamine compound include melamine resins and methyl etherified melamine resins.

[0162] [Amount of hardener] The amount of the curing agent may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, based on 100 parts by weight of the polymer. The amount of the curing agent may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less, based on 100 parts by weight of the polymer.

[0163] [Other ingredients] The repellent may contain other components in addition to the above components. Examples of the other components include polysaccharides, paper strength agents, flocculants, retention aids, coagulants, binder resins, slip prevention agents, sizing agents, paper strength agents, fillers, antistatic agents, preservatives, ultraviolet absorbers, antibacterial agents, deodorants, fragrances, etc. These may be used alone or in combination of two or more. In addition to the above-mentioned components, other components include other water and / or oil repellents, dispersants, texture adjusters, softeners, flame retardants, paint fixing agents, anti-wrinkle agents, drying speed adjusters, crosslinking agents, film-forming agents, compatibilizers, antifreeze agents, viscosity adjusters, UV absorbers, antioxidants, pH adjusters, insect repellents, defoamers, shrink prevention agents, laundry wrinkle prevention agents, shape retention agents, drape retention agents, ironing improvers, whitening agents, whitening agents, fabric softening clay, dye transfer inhibitors such as polyvinylpyrrolidone, polymer dispersants, dirt removers, scum dispersants, fluorescent whitening agents such as 4,4-bis(2-sulfostyryl)biphenyl disodium (Ciba Specialty Chemicals' Chinopearl CBS-X), dye fixatives, and discoloration inhibitors such as 1,4-bis(3-aminopropyl)piperazine. The following can be blended: stain removers, enzymes such as cellulase, amylase, protease, lipase, keratinase, etc. as fiber surface modifiers, foam inhibitors, silk protein powders, their surface modified products or emulsified dispersions (e.g., K-50, K-30, K-10, A-705, S-702, L-710, FP series (Idemitsu Petrochemicals), hydrolyzed silk liquid (Jomo), Silkgen G Soluble S (Ichimaru Falcos)), stain prevention agents (e.g., nonionic polymer compounds consisting of alkylene terephthalate and / or alkylene isophthalate units and polyoxyalkylene units (e.g., FR627 manufactured by GOO Chemical Industry Co., Ltd., SRC-1 manufactured by Clariant Japan, etc.), etc. These may be used alone or in combination of two or more.

[0164] [Polysaccharide] Examples of polysaccharides include starch, xanthan gum, karaya gum, welan gum, guar gum, pectin, tamarind gum, carrageenan, chitosan, gum arabic, locust bean gum, cellulose, alginic acid, agar, dextran, pullulan, etc. The polysaccharide may be a modified polysaccharide having a substitution, in particular a modified polysaccharide having a hydroxyl group or a cationic group introduced therein.

[0165] [Paper strength agents, flocculants, retention aids or coagulants] Examples of paper strength agents, flocculants, retention aids or coagulants include styrene polymers (styrene / maleic acid polymers, styrene / acrylic acid polymers), urea-formaldehyde polymers, polyethyleneimine, melamine-formaldehyde polymers, polyamidoamine-epichlorohydrin polymers, polyacrylamide polymers, polyamine polymers, polydiallyldimethylammonium chloride, alkylamine-epichlorohydrin condensates, condensates of alkylene dichlorides and polyalkylenepolyamines, dicyandiamide-formaldehyde condensates, dimethyldiallylammonium chloride polymers, and olefin / maleic anhydride polymers.

[0166] [Sizing agent] Examples of sizing agents include cellulose-reactive sizing agents, e.g., rosin-based sizing agents such as rosin-based soaps, rosin-based emulsions / dispersions, cellulose-reactive sizing agents, e.g., emulsions / dispersions of anhydrides such as alkyl and alkenyl succinic anhydrides (ASA), alkenyl and alkyl ketene dimers (AKD) and polymers, and anionic, cationic and amphoteric polymers of ethylenically unsaturated monomers, e.g., copolymers of styrene and acrylates.

[0167] [Antistatic agent] Examples of the antistatic agent include cationic antistatic agents having cationic functional groups such as quaternary ammonium salts, pyridinium salts, and primary, secondary, and tertiary amino groups; anionic antistatic agents having anionic functional groups such as sulfonates, sulfates, phosphonates, and phosphates; amphoteric antistatic agents such as alkylbetaines and their derivatives, imidazolines and their derivatives, alanines and their derivatives, nonionic antistatic agents such as aminoalcohols and their derivatives, glycerin and its derivatives, and polyethylene glycols and its derivatives. The antistatic agent may be an ion-conductive polymer obtained by polymerizing or copolymerizing monomers having these cationic, anionic, or amphoteric ion-conductive groups. These may be used alone or in combination of two or more.

[0168] [Preservatives] The preservatives are mainly used to enhance the preservative and bactericidal power and maintain the preservative properties during long-term storage. Examples of the preservatives include isothiazolone organic sulfur compounds, benzisothiazolone organic sulfur compounds, benzoic acids, 2-bromo-2-nitro-1,3-propanediol, etc.

[0169] [Ultraviolet absorber] An ultraviolet absorber is a drug that has an ultraviolet protection effect, and is a component that absorbs ultraviolet light and converts it into infrared light, visible light, etc. Examples of ultraviolet absorbers include aminobenzoic acid derivatives, salicylic acid derivatives, cinnamic acid derivatives, benzophenone derivatives, azole compounds, 4-t-butyl-4'-methoxybenzoylmethane, etc.

[0170] [Antibacterial agents] Antibacterial agents are components that have the effect of suppressing the growth of bacteria on fibers and further suppressing the generation of unpleasant odors resulting from the decomposition products of microorganisms. Examples of antibacterial agents include cationic bactericides such as quaternary ammonium salts, bis-(2-pyridylthio-1-oxide) zinc, polyhexamethylene biguanidine hydrochloride, 8-oxyquinoline, polylysine, etc.

[0171] [Deodorant] Examples of deodorants include cluster dextrin, methyl-β-cyclodextrin, 2-hydroxypropyl-β-cyclodextrin, monoacetyl-β-cyclodextrin, acylamidopropyldimethylamine oxide, and aminocarboxylic acid metal complexes (zinc complex of trisodium methylglycine diacetate described in WO2012 / 090580).

[0172] [Amount of other ingredients] The amount or total amount of each of the other components may be 0.1 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 50 parts by weight or more, 75 parts by weight or more, or 100 parts by weight or more, relative to 100 parts by weight of the polymer. The amount or total amount of each of the other components may be 500 parts by weight or less, 300 parts by weight or less, 200 parts by weight or less, 100 parts by weight or less, 50 parts by weight or less, 40 parts by weight or less, 30 parts by weight or less, 20 parts by weight or less, 10 parts by weight or less, or 5 parts by weight or less, relative to 100 parts by weight of the polymer.

[0173] <Method of manufacturing treated substrate> The method of making a repellent treated product of the present disclosure includes treating a substrate with the repellent agent described above.

[0174] "Treatment" means that the repellent is applied to the substrate by dipping, spraying, painting, etc. By the treatment, the polymer, which is the active ingredient of the repellent, penetrates into the substrate and / or adheres to the surface of the substrate.

[0175] [Base material] The substrate to be treated with the repellent of the present disclosure is not limited, but is preferably a textile product or a paper product.

[0176] Examples of the substrate for textile products include natural fibers of animal and vegetable origin such as cotton, hemp, wool, silk, etc., synthetic fibers such as polyamide, polyester, polyvinyl alcohol, polyacrylonitrile, polyvinyl chloride, polypropylene, etc., semi-synthetic fibers such as rayon, acetate, etc., inorganic fibers such as glass fiber, carbon fiber, asbestos fiber, etc., or mixtures of these fibers. Textile products include woven fabrics, knitted fabrics, nonwoven fabrics, clothing-type cloths, and carpets, but the treatment may be performed on fibers, yarns, and intermediate textile products (e.g., slivers, rovings, etc.) before being made into cloth.

[0177] Examples of the substrate for paper products include paper made of bleached or unbleached chemical pulp such as kraft pulp or sulfite pulp, bleached or unbleached high-yield pulp such as groundwood pulp, mechanical pulp or thermomechanical pulp, waste paper pulp such as recycled newsprint, recycled magazine paper, recycled corrugated cardboard or deinked recycled paper, paper containers, paper molded articles, etc. Specific examples of paper products include food packaging paper, gypsum board base paper, coated base paper, medium quality paper, general liners and cores, neutral pure white roll paper, neutral liners, rust-proof liners and metal interleaving paper, kraft paper, neutral printing and writing paper, neutral coated base paper, neutral PPC paper, neutral heat-sensitive paper, neutral pressure-sensitive base paper, neutral inkjet paper and neutral information paper, molded paper (molded containers), etc.

[0178] Substrates that can be treated with the repellent of the present disclosure are not limited to textiles or paper products, but also include stone, filters (e.g., electrostatic filters), dust masks, fuel cell components (e.g., gas diffusion electrodes and gas diffusion supports), glass, wood, leather, fur, asbestos, bricks, cement, metals and oxides, ceramic products, plastics, painted surfaces, and plaster.

[0179] [Processing method] The repellent of the present disclosure can be applied to a substrate as a treatment agent (particularly a surface treatment agent) by a conventionally known method. The treatment method may be a method in which the repellent of the present disclosure is dispersed and diluted in an organic solvent or water as necessary, and attached to the surface of the substrate by a known method such as dip coating, spray coating, foam coating, etc., and then dried. After drying, a textile product to which the solid components of the repellent are attached is obtained. If necessary, it may be applied together with a suitable crosslinking agent and cured. The repellent of the present disclosure may be used in combination with various additives such as water and / or oil repellents, slip prevention agents, antistatic agents, texture adjusters, softeners, antibacterial agents, flame retardants, paint fixing agents, anti-wrinkle agents, drying speed adjusters, crosslinking agents, film-forming assistants, compatibilizers, antifreeze agents, viscosity adjusters, ultraviolet absorbers, antioxidants, pH adjusters, insect repellents, and defoamers. Examples of various additives may be the same as those described in the "other components" of the water repellent composition above. The concentration of the repellent in the treatment agent to be brought into contact with the substrate may be appropriately changed depending on the application, but may be 0.01 to 10% by weight, for example 0.05 to 5% by weight.

[0180] The repellent can be applied to the substrate by any of the methods known for treating substrates with liquids. The substrate may be immersed in the repellent, or the solution may be applied or sprayed onto the substrate. The treated substrate is preferably dried and cured by heating to develop liquid repellency. The heating temperature may be, for example, 100°C to 200°C, 100°C to 170°C, or 100°C to 120°C. In the present disclosure, good performance can be obtained even with low-temperature heating (for example, 100°C to 140°C). In the present disclosure, the heating time may be 5 seconds to 60 minutes, for example, 30 seconds to 3 minutes. When the textile product is paper, the paper may be coated with the repellent, or the solution may be applied or sprayed onto the paper, or the paper may be mixed with the pulp slurry before papermaking and treated. The treatment may be an external addition treatment or an internal addition treatment. Alternatively, the repellent may be applied to the textile product by a cleaning method, for example, by washing application or dry cleaning method.

[0181] [Paper processing] Examples of the paper substrate include paper, paper containers, and paper molded articles (eg, pulp molds).

[0182] The paper can be produced by a conventional papermaking method, either an internal treatment method in which the repellent is added to the pulp slurry before papermaking, or an external treatment method in which the repellent is applied to the paper after papermaking.

[0183] The internal addition treatment method may mean a treatment method of adding a repellent to a pulp slurry before papermaking. The internal addition treatment method may include, but is not limited to, one or more of the steps of adding a repellent to a pulp slurry and stirring and mixing it, suction-dehydrating the pulp composition prepared in the step through a mesh body of a predetermined shape to deposit the pulp composition to form a pulp mold intermediate, and molding and drying the pulp mold intermediate with a heated mold to obtain paper, a paper container, or a paper molded article. The treated paper may be heat-treated, depending on the properties of the paper, after simple drying at room temperature or at a high temperature. The temperature of the heat treatment may be 150°C or higher, 180°C or higher, or 210°C or higher, and may be 300°C or lower, 250°C or lower, or 200°C or lower, and may be particularly 80°C to 180°C. By performing heat treatment in such a temperature range, excellent oil resistance and water resistance can be exhibited.

[0184] The size press for external additive treatment can be divided into the following types according to the coating method: One application method is a so-called pond-type two-roll size press, in which a coating liquid (size liquid) is supplied to a nip formed by passing paper between two rubber rolls, a coating liquid pool called a pond is created, and the paper is passed through this coating liquid pool to apply the size liquid to both sides of the paper. Other application methods are a gate roll type in which the size liquid is applied by a surface transfer type, and a rod metering size press. In a pond-type two-roll size press, the size liquid is likely to penetrate into the inside of the paper, and in a surface transfer type, the size liquid component is likely to remain on the surface of the paper. In the surface transfer type, the coating layer is more likely to remain on the surface of the paper than in a pond-type two-roll size press, and the coating layer formed on the surface is larger than in a pond-type two-roll size press. In the present disclosure, performance can be imparted to the paper even when the former pond-type two-roll size press is used. The paper thus treated can exhibit excellent oil resistance, water resistance, etc. by optionally accompanying a heat treatment that can take a temperature range of up to 300°C, for example up to 200°C, particularly 80°C to 180°C, depending on the properties of the paper, after simple drying at room temperature or high temperature.

[0185] The present disclosure can be used in gypsum board base paper, coated base paper, medium quality paper, general liners and cores, neutral pure white roll paper, neutral liners, rust-proof liners and metal interleaving paper, kraft paper, etc. It can also be used in neutral printing and writing paper, neutral coated base paper, neutral PPC paper, neutral thermal paper, neutral pressure-sensitive base paper, neutral inkjet paper, and neutral information paper.

[0186] Pulp raw materials include bleached or unbleached chemical pulp such as kraft pulp or sulfite pulp, groundwood pulp, mechanical pulp, or thermomechanical pulp. Any of bleached or unbleached high-yield pulp, recycled newspaper, magazine, corrugated cardboard, deinked recycled paper, etc. may be used. Mixtures of the above pulp raw materials with synthetic fibers such as asbestos, polyamide, polyimide, polyester, polyolefin, polyvinyl alcohol, etc. may also be used.

[0187] The water resistance of paper can be improved by adding a sizing agent. Examples of the sizing agent include cationic sizing agents, anionic sizing agents, and rosin-based sizing agents (e.g., acidic rosin-based sizing agents, neutral rosin-based sizing agents). The amount of the sizing agent may be 0.01 to 5% by weight based on the pulp.

[0188] If necessary, the paper may contain additives used in the manufacture of paper, such as paper strength enhancers such as starch, modified starch, carboxymethyl cellulose, and polyamide polyamine-epichlorohydrin resin, flocculants, fixing agents, retention improvers, dyes, fluorescent dyes, slime control agents, and defoamers, to the extent that they are commonly used. For example, starch or modified starch may be used. If necessary, a repellent may be applied to the paper using starch, polyvinyl alcohol, dyes, coating colors, anti-slip agents, etc., by a size press, gate roll coater, building blade coater, calendar, etc.

[0189] In the case of external addition, the amount of the liquid repellent compound contained in the coating layer is 0.01 to 2.0 g / m 2 , especially 0.1 to 1.0 g / m 2 The coating layer may be formed of a repellent and starch and / or modified starch. The solid content of the paper repellent in the coating layer is preferably 2 g / m. 2 It is preferable that: In the case of internal addition, it is preferable to mix the repellent with the pulp so that the amount of the repellent is 0.01 to 50 parts by weight or 0.01 to 30 parts by weight, for example 0.01 to 10 parts by weight, and particularly 0.2 to 5.0 parts by weight, per 100 parts by weight of the pulp forming the paper.

[0190] In the case of external addition, oil resistance can also be imparted to paper by using a so-called pond-type two-roll size press process in which the treatment solution is pooled between rolls and the base paper is passed through the treatment solution between the rolls at any roll speed and nip pressure.

[0191] In the external addition treatment, the paper substrate may contain additives such as sizing agents, paper strength agents, flocculants, retention agents or coagulants. The additives may be nonionic, cationic, anionic or amphoteric. The ionic charge density of the additives may be -10000 to 10000 μeq / g, preferably -4000 to 8000 μeq / g, more preferably -1000 to 7000 μeq / g. Additives such as sizing agents, paper strength agents, flocculants, retention agents or coagulants (solids or active ingredients) can generally be used in an amount of 0.1 to 10% by weight (e.g., 0.2 to 5.0% by weight) based on the pulp. In the case of a paper substrate containing a cationic additive (e.g., sizing agents, paper strength agents, flocculants, retention agents or coagulants), the repellent is preferably anionic.

[0192] In the internal addition treatment, it is preferable to make a pulp slurry having a pulp concentration of 0.5 to 5.0% by weight (for example, 2.5 to 4.0% by weight). Additives (for example, sizing agents, paper strength agents, flocculants, retention agents, coagulants, etc.) and liquid repellent compounds can be added to the pulp slurry. Examples of additives (e.g., sizing agents, paper strength agents, flocculants, retention agents, or coagulants) include alkylketene dimers, alkenyl succinic anhydrides, styrene polymers (styrene / maleic acid polymers, styrene / acrylic acid polymers), urea-formaldehyde polymers, polyethyleneimine, melamine-formaldehyde polymers, polyamidoamine-epichlorohydrin polymers, polyacrylamide polymers, polyamine polymers, polydiallyldimethylammonium chloride, alkylamine-epichlorohydrin condensates, condensates of alkylene dichlorides and polyalkylenepolyamines, dicyandiamide-formaldehyde condensates, dimethyldiallylammonium chloride polymers, and olefin / maleic anhydride polymers.

[0193] [Pretreatment of textile products] The textile product may be pretreated before being treated with the repellent of the present disclosure. Pretreatment of the textile product may impart excellent fastness to the textile product after treatment with the repellent.

[0194] Examples of pretreatments of textile products include cationization treatment by reaction with a reactive quaternary ammonium salt, anionization treatment such as sulfonation, carboxylation, and phosphation, and acetylation treatment, benzoylation treatment, carboxymethylation treatment, grafting treatment, tannic acid treatment, and polymer coating treatment after anionization treatment.

[0195] The method for pretreating a textile product is not limited, and the textile product can be pretreated by a conventionally known method. The pretreatment liquid may be dispersed and diluted in an organic solvent or water as necessary, and applied to the surface of the textile product by a known method such as dip coating, spray coating, foam coating, etc., and then dried. The pH and temperature of the pretreatment liquid may be adjusted depending on the desired degree of treatment. As an example of a method for pretreating a textile product, a method for pretreating a textile product with a hydrocarbon-based water repellent will be described in detail.

[0196] The pretreatment method for textile products is to add -SO3M to the fibers. 1 (In the formula, M 1 represents a monovalent cation), -COOM 2 (In the formula, M 2 represents a monovalent cation), and -OP(O)(OX 1 )(OX 2 )(wherein, X 1 and X 2 each independently represents a hydrogen atom or an alkyl group having 1 to 22 carbon atoms) (hereinafter, also referred to as a "specific functional group").

[0197] M 1 Examples of M include H, K, Na, and ammonium ion which may have a substituent. 2 Examples of X include H, K, Na, and ammonium ion which may have a substituent. 1 Or X 2 When is an alkyl group, it is preferably an alkyl group having 1 to 22 carbon atoms, and more preferably an alkyl group having 4 to 12 carbon atoms.

[0198] The fibers containing the specific functional groups (hereinafter, sometimes referred to as "functional group-containing fibers") can be prepared, for example, by the following method. (i) A compound having the specific functional group is attached to a fiber material. The attachment of the compound may be in a state where a part of the compound is chemically bonded to a part of the fiber to the extent that a sufficient amount of the specific functional group remains. (ii) A fiber is prepared in which the specific functional group is directly introduced into the material constituting the fiber.

[0199] In the case of (i), for example, a functional group-containing fiber can be obtained by a functional group introduction step in which a fiber material is treated with a pretreatment liquid containing one or more compounds having the specific functional group.

[0200] The material of the fiber material is not particularly limited, and examples thereof include natural fibers such as cotton, hemp, silk, wool, etc., semi-synthetic fibers such as rayon, acetate, etc., synthetic fibers such as polyamide (nylon, etc.), polyester, polyurethane, polypropylene, etc., and composite fibers, blended fibers, etc. The form of the fiber material may be any of fibers (tow, sliver, etc.), yarn, knitted fabric (including interwoven fabric), woven fabric (including interwoven fabric), nonwoven fabric, etc.

[0201] In this embodiment, from the viewpoint of improving the water repellency of the obtained textile product, it is preferable to use textile materials containing polyamide and polyester as raw materials, and in particular, it is preferable to use nylons such as nylon 6 and nylon 6,6, polyesters such as polyethylene terephthalate (PET), polytrimethyl terephthalate, and polylactic acid, and mixed fibers containing these.

[0202] Above -SO3M 1 As the compound having the formula (I), a phenol-based polymer can be used. As such a phenol-based polymer, for example, one containing at least one compound represented by the following general formula can be mentioned.

[0203] TIFF2024153749000004.tif4678[where, X 2 Ha-SO3M 3 (In the formula, M 3 represents a monovalent cation) or a group represented by the following general formula, and n is an integer of 20 to 3000.

[0204] TIFF2024153749000005.tif2661[In formula, M 4 represents a monovalent cation.

[0205] The above M 3 Examples of the cation include H, K, Na, and ammonium ion which may have a substituent.

[0206] The above M 4 Examples of the cation include H, K, Na, and ammonium ion which may have a substituent.

[0207] The compound represented by the above general formula may be, for example, a formalin condensate of phenolsulfonic acid or a formalin condensate of sulfonated bisphenol S.

[0208] Above - COOM 2 Examples of compounds having the formula include polycarboxylic acid polymers.

[0209] As the polycarboxylic acid polymer, for example, a polymer synthesized by a conventionally known radical polymerization method using acrylic acid, methacrylic acid, maleic acid, or the like as a monomer, or a commercially available product can be used.

[0210] Examples of the method for producing a polycarboxylic acid polymer include a method in which a radical polymerization initiator is added to an aqueous solution of the above-mentioned monomer and / or its salt, and the mixture is heated and reacted at 30 to 150° C. for 2 to 5 hours. At this time, an alcohol such as methanol, ethanol, isopropyl alcohol, or an aqueous solvent such as acetone may be added to the aqueous solution of the above-mentioned monomer and / or its salt. Examples of the radical polymerization initiator include persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate, redox-based polymerization initiators such as combinations of persulfates and sodium bisulfite, hydrogen peroxide, and water-soluble azo-based polymerization initiators. These radical polymerization initiators may be used alone or in combination of two or more. Furthermore, during radical polymerization, a chain transfer agent (e.g., octyl thioglycolate) may be added for the purpose of adjusting the degree of polymerization.

[0211] In addition to the above monomers, copolymerizable monomers can be used in the radical polymerization. Examples of the copolymerizable monomers include vinyl monomers such as ethylene, vinyl chloride, and vinyl acetate, acrylamide, acrylates, and methacrylates. The acrylates and methacrylates are preferably those having a hydrocarbon group having 1 to 3 carbon atoms which may have a substituent such as a hydroxyl group. Examples of such acrylates or methacrylates include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, propyl acrylate, and propyl methacrylate. These copolymerizable monomers may be used alone or in combination of two or more.

[0212] The carboxyl group in the polycarboxylic acid polymer may be free or may be neutralized with an alkali metal, an amine compound, etc. Examples of the alkali metal include sodium, potassium, and lithium, and examples of the amine compound include ammonia, monoethanolamine, diethanolamine, and triethanolamine.

[0213] The weight average molecular weight of the polycarboxylic acid polymer is preferably from 1,000 to 20,000, and more preferably from 3,000 to 15,000, from the viewpoint of improving the water repellency of the resulting textile product.

[0214] As the polycarboxylic acid polymer, commercially available products such as "Neocrystal 770" (product name, manufactured by Nicca Chemical Co., Ltd.) and "Ceropol PC-300" (product name, manufactured by Sanyo Chemical Industries, Ltd.) can be used.

[0215] Above -OP(O)(OX 1 )(OX 2 ) is exemplified by a phosphate ester compound represented by the following general formula: TIFF2024153749000006.tif3243[where, X 1 Or X 2 is the same as above, and X 3 represents an alkyl group having 1 to 22 carbon atoms.

[0216] As the phosphate ester compound, phosphate monoesters, diesters and triesters, in which the alkyl ester moiety is an alkyl group having 1 to 22 carbon atoms, and mixtures thereof can be used.

[0217] From the viewpoint of improving the water repellency of the resulting textile product, it is preferable to use lauryl phosphate and decyl phosphate.

[0218] As the phosphate ester compound, for example, a commercially available product such as "Phosphanol ML-200" (product name, manufactured by Toho Chemical Industry Co., Ltd.) can be used.

[0219] The pretreatment liquid containing one or more compounds having the specific functional group may be, for example, an aqueous solution of the above-mentioned compounds. The pretreatment liquid may also contain an acid, an alkali, a surfactant, a chelating agent, etc.

[0220] Examples of the method for treating the textile material with the pretreatment liquid include padding, immersion, spraying, and coating. Examples of padding include a method using a padding device described on pages 396-397 of Textile Dyeing and Processing Dictionary (published by Nikkan Kogyo Shimbun, 1963) and pages 256-260 of Color Dyeing Chemistry III (published by Jikkyo Publishing Co., Ltd., 1975). Examples of coating include a method using a coating machine described on pages 473-477 of Dyeing and Finishing Equipment Directory (published by Sen-sha, 1981). Examples of immersion include a method using a batch-type dyeing machine described on pages 196-247 of Dyeing and Finishing Equipment Directory (published by Sen-sha, 1981), and a liquid flow dyeing machine, air flow dyeing machine, drum dyeing machine, winch dyeing machine, washer dyeing machine, cheese dyeing machine, etc. can be used. Examples of the spray treatment include an air spray in which the treatment liquid is sprayed in the form of a mist using compressed air, and a method using an air spray of a liquid pressure atomization type. The treatment conditions, such as the concentration of the treatment liquid and the heat treatment after application, can be appropriately adjusted in consideration of various conditions such as the purpose and performance. In addition, when the pretreatment liquid contains water, it is preferable to dry the pretreatment liquid after it is applied to the fiber material in order to remove the water. There is no particular limit to the drying method, and either a dry heat method or a wet heat method may be used. There is also no particular limit to the drying temperature, and for example, drying may be performed at room temperature to 200°C for 10 seconds to several days. If necessary, heat treatment may be performed at a temperature of 100 to 180°C for about 10 seconds to 5 minutes after drying.

[0221] When the textile material is to be dyed, the treatment with the pretreatment liquid may be carried out before dyeing or in the same bath as the dyeing. However, when reduction soaping is carried out, there is a risk that the compound having the specific functional group (e.g., a phenolic polymer compound, etc.) adsorbed during the process may fall off, so it is preferable to carry out the treatment after reduction soaping after dyeing.

[0222] The treatment temperature in the immersion treatment can be 60 to 130° C. The treatment time can be 5 to 60 minutes.

[0223] In the functional group introduction step using a pretreatment liquid, the amount of the compound having the specific functional group attached is preferably 1.0 to 7.0 parts by weight per 100 parts by weight of the textile material. Within this range, durable water repellency and texture can be simultaneously achieved at high levels.

[0224] The pretreatment liquid is preferably adjusted to a pH of 3 to 5. The pH can be adjusted using a pH adjuster such as acetic acid or malic acid.

[0225] In the pretreatment solution, a salt may be used in combination in order to effectively adsorb the compound having the specific functional group to the fiber material by the salting-out effect. Examples of salts that can be used include sodium chloride. Examples of suitable salts include sodium carbonate, ammonium sulfate, and sodium sulfate.

[0226] In the functional group introduction step using the pretreatment liquid, it is preferable to remove the compound having the specific functional group that has been treated in excess. An example of a removal method is washing with water. By removing the compound sufficiently, it is possible to prevent the development of water repellency in the subsequent water repellent treatment from being hindered, and in addition, the feel of the resulting textile product is improved. In addition, it is preferable to thoroughly dry the resulting functional group-containing fiber before contacting it with a hydrocarbon-based water repellent.

[0227] (ii) An example of a fiber in which the specific functional group is directly introduced into the material constituting the fiber is cationic dyeable polyester (CD-PET).

[0228] From the viewpoint of improving the water repellency of the resulting textile product, the functional group-containing fiber preferably has a surface zeta potential of −100 to −0.1 mV, more preferably −50 to −1 mV. The zeta potential of the fiber surface can be measured, for example, by a zeta potential / particle size measuring system ELSZ-1000ZS (manufactured by Otsuka Electronics Co., Ltd.).

[0229] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES

[0230] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples.

[0231] <Test Method> The test procedure is as follows.

[0232] [Number average molecular weight (Mn), weight average molecular weight (Mw), molecular weight distribution (Mw / Mn)] The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) were determined by gel permeation chromatography (GPC). GPC used tetrahydrofuran or DMF as a developing solution and Shodex LF-404 and KF-805L as columns, and the molecular weight was calculated in terms of PMMA.

[0233] [Copolymer composition by NMR (nuclear magnetic resonance) method] For 1H-NMR (nuclear magnetic resonance) measurements, deuterated chloroform was used as the solvent.

[0234] [Measurement of thermal properties by differential scanning calorimetry (DSC)] The melting point of the polymer was calculated by differential scanning calorimetry (DSC). In the DSC measurement, the polymer was cooled to -20°C under a nitrogen atmosphere, heated to 180°C at 10°C / min, cooled again to -20°C, and the melting point observed during the subsequent heating process to 180°C at 10°C / min was measured. For polymers showing multiple melting peaks, the peak with the largest heat of fusion resulting from the melting of the long-chain alkyl was taken as the melting point. The glass transition point (glass transition temperature) was determined as the temperature indicated by the midpoint between the intersection of the extension lines of the baselines before and after the secondary transition of the DSC curve and the tangent line at the inflection point of the DSC curve.

[0235] [Static contact angle measurement] A chloroform solution of the polymer (solid concentration 1.0%) was spin-coated onto a silicon wafer substrate and heated at 120°C for 15 minutes to produce a coating film. 2 μL of water or hexadecane (n-HD) was dropped onto the coating film, and the static contact angle 1 second after the drop landed was measured using a fully automatic contact angle meter (DropMaster701 manufactured by Kyowa Interface Science Co., Ltd.).

[0236] [Adhesion] A chloroform solution of the polymer (solid content concentration 5.0%) was bar-coated onto a polyester film (Lumirror, manufactured by Toray Industries, Inc.) having a thickness of 250 μm, and heated at 80° C. for 20 minutes to prepare a coating film. A checkerboard pattern of 1mm intervals was cut into the coating with a cutter knife, cellophane tape was applied and then peeled off. Peeling was evaluated as follows: 0-15% peeled area was rated as good, 15-50% peeled area was rated as fair, and 50% or more peeled area was rated as bad.

[0237] [Water repellency test] A treatment solution with a solid content of 1.5% was prepared using chloroform as a solvent. Polyester fabric (PET) was immersed in this test solution and passed through a mangle. The water repellency of the heat-treated test fabric was evaluated. The test was carried out according to the spray method of JIS-L-1092 (AATCC-22), and the water repellency of the treated fabric was evaluated with a grade of yes or no. ○: No wetting ×: Overall wetness is observed

[0238] [Making paper plates] The wood pulp slurry was used to make paper plates (untreated) weighing 10 g in an automatic molding machine.

[0239] [Water and oil resistance test] A treatment solution with a solids concentration of 10% was prepared using chloroform as a solvent. Paper plates were immersed in this test solution, and then 100 mL of water or corn oil was poured onto the heat-treated test plates. The water and oil resistance was evaluated with a Yes or No depending on whether or not the water or oil soaked in. 〇: No stains on the back ×: There is a stain on the entire back side

[0240] <Production Example> The synthesis and cyclopolymerization of divinyl monomers were carried out as follows.

[0241] [Production Example 1: Synthesis of Divinyl Monomer 1] TIFF2024153749000007.tif32113 4-(Trifluoromethyl)salicylic acid (250g), N-(2-Hydroxyrthyl)acrylamide (167g), 4-dimethylaminopyridine (37g), and dichloromethane (2.1L) were added to a reactor and stirred at room temperature for 1.5 hours. After cooling to 0°C, 1-(3-Dimethylaminopropyl)-3-ethylcarbodiimide Hydrochloride (278g) was added and stirred for 3 hours and overnight at room temperature. After the reaction was completed, the mixture was quenched with a citric acid methanol solution, separated, and purified by column chromatography to obtain 2-Acrylamidoethyl 4-(trifluoromethyl)salicylate (272g) in a yield of 74%. TIFF2024153749000008.tif30106 2-Acrylamidoethyl 4-(trifluoromethyl)salicylate (101 g) and tetrahydrofuran (1.4 L) were added to a reactor, and acrylic acid chloride (28 mL) and triethylamine (51 mL) were added under stirring at 0°C and stirred for 4 hours. After the reaction was completed, the mixture was quenched with methanol, filtered, and purified by column chromatography to obtain divinyl monomer 1 (93 g) in a yield of 78%.

[0242] [Production Example 2: Synthesis of Divinyl Monomer 2] TIFF2024153749000009.tif1572 Ethylene glycol monovinyl ether (196 g), triethylamine (101 g), and dichloromethane (1.9 L) were added to a reactor, and acrylic acid chloride (168 g) was added dropwise under stirring at 0°C, and the mixture was further stirred at room temperature. After the reaction was completed, the mixture was quenched with water, separated, and purified by column chromatography to obtain 2-(vinyloxy)ethyl acrylate (124 g) in a yield of 47%. TIFF2024153749000010.tif2085Methacrylic acid (271 g), 2-(vinyloxy)ethyl acrylate (124 g), and dichloromethane (1.1 L) were added to a reactor and heated and stirred at 60° C. for 86 hours. After the reaction was completed, a 5% aqueous solution of sodium bicarbonate was added, and the mixture was separated and purified by column chromatography to obtain divinyl monomer 2 (189 g) in a yield of 95%.

[0243] [Production Example 3: Cyclopolymerization of Divinyl Monomer 1] TIFF2024153749000011.tif3070Divinyl monomer 1 (715.7 mg), AIBN (7.2 mg), and DME (19.7 mL) were added to a reactor under an argon atmosphere, and the mixture was heated and stirred at 60°C for 6 hours, and then cooled to -78°C to stop the reaction. The consumption rates of the two vinyl groups (acrylate; A, acrylamide; Am) were both 88% by 1H-NMR (CDCl3). The number average molecular weight (Mn) was 10,300 and the molecular weight distribution (Mw / Mn) was 2.49 by SEC.

[0244] [Production Example 4: Cyclopolymerization of Divinyl Monomer 2] TIFF2024153749000012.tif2573Divinyl monomer 2 (6.85 g), AIBN (0.02 eq.), and toluene (300 mL) were added to a reactor under an argon atmosphere, and the mixture was heated and stirred at 60°C for 4 hours, and then cooled to -78°C to stop the reaction. The consumption rates of the two vinyl groups (methacrylate; M, acrylate; A) were both 82% by 1H-NMR (CDCl3). The number average molecular weight (Mn) was 25,300 and the molecular weight distribution (Mw / Mn) was 3.04 by SEC.

[0245] [Production Example 5: Scale-up of cyclopolymerization of divinyl monomer 1] TIFF2024153749000013.tif3070Divinyl monomer 1 (2.5 g), AIBN (23 mg), and DME (70 mL) were added to a reactor under an argon atmosphere, and the mixture was heated and stirred at 60°C for 6 hours, and then cooled to -78°C to stop the reaction. SEC showed that the number average molecular weight (Mn) was 7400 and the molecular weight distribution (Mw / Mn) was 2.31.

[0246] <Examples and Comparative Examples> A polymer was synthesized as follows: The obtained polymer was used to carry out the above-mentioned tests.

[0247] Example 1: Alternating Copolymer 1 (Conversion with C12 Amine) TIFF2024153749000014.tif3596The polymerization solution (5 mL; monomer unit 0.5 mmol) and dodecylamine (10 eq.) of Production Example 3 were added to a reactor, stirred overnight at room temperature, and then purified by methanol dialysis. SEC showed that the number average molecular weight (Mn) was 10,400 and the molecular weight distribution (Mw / Mn) was 1.85.

[0248] Example 2 The reaction was carried out in the same manner as in Example 1, except that the amine was changed to octadecylamine and the reaction temperature was changed to 80°C.

[0249] Example 3 The reaction was carried out in the same manner as in Example 1, except that the amine was changed to n-octylamine.

[0250] Example 4 The reaction was carried out in the same manner as in Example 1, except that the amine was changed to 2-ethylhexylamine.

[0251] Example 5 The reaction was carried out in the same manner as in Example 1, except that the amine was changed to cyclooctylamine.

[0252] Example 6 The reaction was carried out in the same manner as in Example 1, except that the amine was changed to 3-(dibutylamino)propylamine.

[0253] Example 7 The polymerization solution (5 mL; monomer unit 0.5 mmol) of Production Example 3 and 4-tBu-benzylamine (10 eq.) were added to the reactor and stirred at room temperature overnight to convert one side of the side chain. Furthermore, in order to complete the conversion to a hydroxyethyl group, n-butylamine (5 eq.) was added and stirred at room temperature overnight, and then purified by methanol dialysis. From SEC, the number average molecular weight (Mn) was 10,300 and the molecular weight distribution (Mw / Mn) was 2.09.

[0254] [Example 8: Random Copolymer 1] TIFF2024153749000015.tif3095N-dodecylacrylamide (166 mg), N-hydroxyethylacrylamide (80 mg), AIBN (2.3 mg), and DMF (7 mL) were added to a reactor under an argon atmosphere, and the mixture was heated and stirred at 60°C for 48 hours, and then cooled to -78°C to stop the reaction. SEC showed that the number average molecular weight (Mn) was 5500 and the molecular weight distribution (Mw / Mn) was 1.71. 1H-NMR (CDCl3) confirmed that the product was a random copolymer with a composition ratio of 1:1.

[0255] Example 9 The reaction was carried out in the same manner as in Example 8, except that N-dodecylacrylamide was changed to N-octylacrylamide.

[0256] Example 10 The reaction was carried out in the same manner as in Example 8, except that N-dodecylacrylamide was changed to N-(2-ethylhexyl)acrylamide.

[0257] Example 11 The reaction was carried out in the same manner as in Example 8, except that N-dodecylacrylamide was changed to N-cyclooctylacrylamide.

[0258] Example 12: Alternating Copolymer 2 (Cleavage with TFA, Conversion with C18 Isocyanate) TIFF2024153749000016.tif35153 Cyclized polymer 2 (0.18 g), THF (20 mL), trifluoroacetic acid (1 mL), and water (0.5 mL) were added to a reactor and stirred for 24 hours at 30° C. After completion of the reaction, the solvent was distilled off and the intermediate polymer was purified by reprecipitation with diethyl ether to obtain the intermediate polymer. The intermediate polymer (0.18 g), octadecyl isocyanate (1.05 eq.), DMSO (5 mL), and THF (5 mL) were added and stirred overnight at room temperature, and then purified by methanol dialysis. SEC showed that the number average molecular weight (Mn) was 15,100 and the molecular weight distribution (Mw / Mn) was 3.11.

[0259] Example 13 The reaction was carried out in the same manner as in Example 12, except that octadecyl isocyanate was changed to dodecyl isocyanate and the solvent was changed to THF alone.

[0260] [Example 14: Synthesis of alternating copolymers with two types of amines (conversion with C12 amine and cyclooctylamine)] TIFF2024153749000017.tif41153 0.89 g (7 mmol, 5 eq.) of cyclooctylamine / 1.30 g (7 mmol, 5 eq.) of dodecylamine were added to the polymerization solution of Production Example 3 (14 mL; monomer unit 1.4 mmol) in a reactor, and the mixture was stirred at room temperature for 24 hours. The reaction solution was then placed in a Spectra / Por 7 dialysis membrane and dialyzed in methanol (2.0 L). The methanol was replaced about every 5 hours, and dialyzed four times. The resulting white suspension was concentrated under reduced pressure to obtain 0.25 g of an amorphous solid alternating polymer. NMR analysis showed that the molar ratio of cyclooctylamine to dodecylamine was 1:3.25. SEC revealed that the number average molecular weight (Mn) was 8613 and the molecular weight distribution (Mw / Mn) was 1.38.

[0261] Example 15: Scale-up of the synthesis of alternating copolymers with two amines (C12 amine and cyclooctylamine) The procedure of Example 14 was scaled up. In a reactor, 4.45 g (35 mmol, 5 eq.) of cyclooctylamine / 6.48 g (35 mmol, 5 eq.) of dodecylamine were added to the polymerization solution (70 mL; monomer unit 7 mmol) of Production Example 3, and the mixture was stirred at room temperature for 24 hours. The post-treatment was carried out in the same manner as in Example 14, and 1.7 g of an amorphous solid alternating polymer was obtained. From NMR analysis, the ratio of amines introduced was cyclooctylamine / dodecylamine = 1:21.03. From SEC, the number average molecular weight (Mn) was 10514, and the molecular weight distribution (Mw / Mn) was 1.48. As a result of scaling up, the introduction rate of cyclooctylamine was significantly reduced.

[0262] [Comparative Example 1: Random Copolymer 2] TIFF2024153749000018.tif30143 tBuMA (0.41 mL), C18URA (1.03 g), AIBN (8.6 mg), and 1,4-dioxane (5.2 mL) were added to a reactor under an argon atmosphere, and the mixture was heated and stirred at 60°C for 22 hours, after which it was cooled to -78°C to stop the reaction. The consumption rates of the two vinyl groups (methacrylate; M, acrylate; A) were M: 99%, A: 95% by 1H-NMR (CDCl3). The number average molecular weight (Mn) was 27,400 and the molecular weight distribution (Mw / Mn) was 3.95 by SEC. The product was purified by methanol reprecipitation, and it was confirmed to be a random copolymer with a composition ratio of 1:1 by 1H-NMR (CDCl3). To a reactor, HCl (100 eq.) and 1,4-dioxane (200 mL) were added to the copolymer (tBuMA unit concentration 2 mmol), and the mixture was heated and stirred at 90°C for 12 hours. After the reaction was completed, the solvent was distilled off, and it was confirmed by 1H-NMR (CDCl3) that the copolymer had a deprotected tBu group, giving random copolymer 2.

[0263] Comparative Example 2 The reaction was carried out in the same manner as in Comparative Example 1, except that C18URA was changed to C12URA.

[0264] [Comparative Example 3] Homopolymer 1 TIFF2024153749000019.tif2057 N-dodecylacrylamide (4.79 g), AIBN (32.8 mg), and THF (5.2 mL) were added to a reactor under an argon atmosphere, and the mixture was heated and stirred at 60° C. for 3 hours, and then cooled to −78° C. to stop the reaction. SEC showed that the number average molecular weight (Mn) was 27,200 and the molecular weight distribution (Mw / Mn) was 1.97.

[0265] Comparative Example 4 The reaction was carried out in the same manner as in Comparative Example 3, except that N-dodecylacrylamide was changed to N-cyclooctylacrylamide.

[0266] 〔result〕 The results are summarized in the table below.

[0267] [Table 1] (Static contact angle test (water)) JPEG2024153749000020.jpg86154

[0268] [Table 2] (Static Contact Angle Test (n-HD)) JPEG2024153749000021.jpg43151

[0269] [Table 3] (Adhesion test) JPEG2024153749000022.jpg26154

[0270] [Table 4] (Water repellency test (textile)) JPEG2024153749000023.jpg48153

[0271] [Table 5] (Static contact angle test (water and n-HD)) JPEG2024153749000024.jpg32150

[0272] [Table 6] (Water and oil resistance test (paper)) TIFF2024153749000025.tif24154

[0273] [Abbreviation] The abbreviations have the following meanings: HEAAm: N-(2-hydroxyethyl)acrylamide DAAm: N-dodecylacrylamide ODAAm: N-octadecylacrylamide OAAm: N-octylacrylamide EHAAm: N-(2-ethylhexyl)acrylamide CyOAAm: N-cyclooctylacrylamide DBAPAAm: N-(3-(dibutylamino)propyl)acrylamide tBuBnAAm: N-(4-(t-butyl)benzyl)acrylamide MAA: Methacrylic acid C18URA: 2-((octadecylcarbamoyl)oxy)ethyl acrylate C12URA: 2-((dodecylcarbamoyl)oxy)ethyl acrylate C12 amine: N-dodecylamine CyONH2: N-cyclooctylamine

Claims

1. A polymer which is polymer (III) as defined below. (III) a compound represented by the following formula: -[CH 2 C(-Q 3 )C(=O)OH]- [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom. The repeating unit (3) represented by The following formula: -[CH 2 C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The repeating unit (4) represented by A polymer having an alternating sequence (E) consisting of:

2. 2. The polymer of claim 1, wherein the amount of said alternating sequence (E) is 30% by weight or more in said polymer.

3. A repellent comprising a polymer, which is polymer (III) as defined below. (III) a compound represented by the following formula: -[CH 2 C(-Q 3 )C(=O)OH]- [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom. The repeating unit (3) represented by The following formula: -[CH 2 C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The repeating unit (4) represented by A polymer having an alternating sequence (E) consisting of:

4. The repellent according to claim 3, wherein the amount of the alternating sequence (E) is 30% by weight or more in the polymer.

5. 4. The repellent of claim 3, comprising a liquid medium which is water, an organic solvent, or a mixture of water and an organic solvent.

6. The repellent according to claim 3, which is for textiles or paper.

7. A substrate having the polymer in the repellent agent according to any one of claims 3 to 6 adhered thereto.

8. A method for producing a treated substrate comprising applying a repellent agent according to any one of claims 3 to 6 to a substrate.

9. A method for producing polymer (III), comprising the steps of: The following formula: CH 2 =C(-Q 3 )C(=O)O-X E -O-R 41 -OC(=O)C(-Q 4 )=CH 2 [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom, X E is a group removable by acidolysis, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms. a step of cyclopolymerizing a divinyl monomer (E) represented by the formula: The precursor (E1) is decomposed with an acid to obtain X E to obtain a precursor (E2); and The precursor (E2), The following formula: R 42 -NCO [In the formula, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. With an isocyanate compound represented by the formula: The polymer (III) The following formula: -[CH 2 C(-Q 3 )C(=O)OH]- [In the formula, Q 3 is a hydrogen atom, a monovalent organic group, or a halogen atom. The repeating unit (3) represented by The following formula: -[CH 2 C(-Q 4 )C(=O)OR 41 OC(=O)NHR 42 ]- [In the formula, Q 4 is a hydrogen atom, a monovalent organic group, or a halogen atom, R 41 is an alkylene group having 1 to 10 carbon atoms, R 42 is a monovalent organic group having a hydrocarbon group having 4 to 40 carbon atoms. The repeating unit (4) represented by A method for producing a polymer (III) having an alternating sequence (E) consisting of:

Citation Information

Patent Citations

  • Monomers capable of forming four hydrogen bridges and supramolecular polymers formed by copolymerization of these monomers with ordinary monomers

    JP2006508201A

  • Manufacturing method for polyfunctional (METH)acrylic ester

    JP2013010726A

  • Vinyl ether derivative polymer, method for producing the same, and application thereof