Heat treated cold rolled steel sheet and method of manufacturing thereof
Patent Information
- Application Number
- JP2024126669
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-29
Smart Images

Figure 2024153872000001 
Figure 2024153872000002 
Figure 2024153872000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength, highly formable cold-rolled steel sheet having a tensile strength of 950 MPa or more and a hole expansion ratio exceeding 56%, which is suitable for use as a steel sheet for vehicles. [Background technology]
[0002] Automotive parts must meet two conflicting requirements, namely ease of forming and strength, but in recent years, a third requirement, namely improved fuel efficiency, has also been imposed on automobiles in light of global environmental issues. Therefore, automotive parts must now be made of materials with high formability to meet the criteria of ease of fitting into complex automotive assemblies, and at the same time, must improve strength for the vehicle's impact resistance and durability while reducing the vehicle's weight and improving fuel efficiency.
[0003] Therefore, vigorous research and development is being conducted to reduce the amount of material used in automobiles by increasing the strength of materials. Conversely, as the strength of steel plate increases, its formability decreases, so there is a demand for the development of materials that combine high strength and high formability.
[0004] Previous research and development in the field of high strength and highly formable steel plates has resulted in several methods for producing high strength and highly formable steel plates, some of which are listed herein for a clear understanding of the present invention.
[0005] JP2012111978 is a patent application having a composition, which is 0.05-0.3% C, 0.01-3.0% Si, 0.5-3% Mn, 0.01-0.1% Al, the balance being Fe and unavoidable impurities, and has a composition consisting of ferrite and tempered martensite as the main components of high strength cold rolled steel plate, but such steel cannot reach a hole expansion ratio of more than 50%.
[0006] EP2971209 is a patent related to a high-strength hot-dip galvanized dual-phase steel strip with improved formability for use in the automotive industry, having an essential element composition where C is 0.13 - 0.19%, Mn is 1.70 - 2.50%, Si is 0 - 0.15%, Al is 0.40 - 1.00%, Cr is 0.05 - 0.25%, Nb is 0.01 - 0.05%, P is 0 - 0.10%, Ca is 0 - 0.004%, S is 0 - 0.05%, N is 0 - 0.007%, and the balance is Fe and inevitable impurities, with 0.40% < Al + Si < 1.05% and Mn + Cr > 1.90%, having a dual-phase microstructure containing 8 - 12% retained austenite, 20 - 50% bainite, and less than 10% martensite by volume percentage, with the balance being ferrite, but the granted patent cannot reach a tensile strength exceeding 900 MPa.
[0007] Known prior art related to the production of high-strength and high-formability steel sheets is brought about by one or the other lacuna, and thus, there is a need for cold-rolled steel sheets having high strength and high formability and a method for producing the same.
Prior Art Documents
Patent Documents
[0008]
Patent Document 1
Patent Document 2
Summary of the Invention
Problems to be Solved by the Invention
[0009] The object of the present invention is to solve these problems by making available a cold-rolled steel sheet having the following simultaneously.
[0010] - An ultimate tensile strength of 950 MPa or more, preferably exceeding 980 MPa, or even more preferably exceeding 1000 MPa, - An elongation at break of 8% or more - Hole expansion ratio of at least 56%, preferably at least 57%.
[0011] In a preferred embodiment, the steel plate according to the invention may have a yield strength value of 750 MPa or more.
[0012] Preferably, such steels should also have good weldability and coatability, and good suitability for forming, especially rolling.
[0013] Another object of the invention is also to make available a manufacturing method for these sheets that is robust to changes in manufacturing parameters, whilst being compatible with conventional industrial applications.
[0014] Other features and advantages of the present invention will become apparent from the following detailed description of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Carbon is present in steel in an amount of 0.09% to 0.15%. Carbon is an element necessary for generating low-temperature transformation phases such as martensite to increase the strength of steel sheets. If the content is less than 0.09%, a sufficient amount of martensite cannot be secured, which reduces strength and ductility. On the other hand, if the carbon content exceeds 0.15%, the welds and heat-affected zones are significantly hardened, which reduces the mechanical properties of the welds. The preferred limit of carbon is 0.1% to 0.14%, more preferably 0.1% to 0.13%.
[0016] The manganese content of the steel of the present invention is between 1.8% and 2.5%. Manganese is an element that imparts strength by solid solution strengthening. Manganese in an amount of at least about 1.8% (by weight) has been found to impart strength and hardenability to the steel sheet. Higher percentages of manganese, such as 1.9% to 2.4%, are therefore preferred, with a more preferred limit of 2.0% to 2.3%. However, manganese in excess of 2.5% has adverse effects, such as a slower transformation of austenite to martensite during cooling after annealing, resulting in reduced strength. Moreover, manganese contents in excess of 2.5% also reduce the weldability of the steel.
[0017] Silicon is an essential element for the steel of the present invention, and silicon is present in an amount of 0.2% to 0.7%. Silicon is added to the steel of the present invention to impart strength by solid solution strengthening. Silicon participates in the formation of the microstructure by preventing the precipitation of carbides and promoting the formation of martensite. However, if the silicon content exceeds 0.7%, the surface properties and weldability of the steel are deteriorated, so that the silicon content is preferably 0.3% to 0.7%, more preferably 0.4% to 0.6%.
[0018] The aluminum content of the present invention is 0.01%-0.1%. Aluminum is added to deoxidize the steel of the present invention. Aluminum is an alpha generating element and also retards the formation of carbides. This can increase the formability and ductility of the steel. To obtain such an effect, an aluminum content of 0.01% or more is necessary. However, if the aluminum content exceeds 0.1%, the Ac3 point rises and exceeds the allowable range, making it very difficult to obtain an austenite single phase industrially, and therefore hot rolling in the complete austenite region is not possible. Therefore, the aluminum content must not exceed 0.1%. The preferred limit for the presence of aluminum is 0.01%-0.08%, more preferably 0.01%-0.05%.
[0019] The phosphorus content of the steel of the invention is limited to 0.09%. Phosphorus is an element that hardens in solid solution and also prevents the formation of carbides. Small amounts of phosphorus, at least 0.002%, can therefore be advantageous, but phosphorus also has negative effects, such as reduced spot weldability and hot ductility, due in particular to its tendency to segregate at grain boundaries or co-segregate with manganese. For these reasons, its content is preferably limited to a maximum of 0.02%.
[0020] Sulfur is not an essential element, but may be contained in the steel as an impurity. The lower the sulfur content, the better, but from the viewpoint of production costs, it is preferably 0.09% or less, and most preferably 0.01% or less. Furthermore, if a larger amount of sulfur is present in the steel, it will combine to form sulfides, especially with Mn and Ti, reducing their beneficial effects on the present invention.
[0021] Nitrogen is limited to 0.09% to avoid deterioration of the material over time; although nitrogen forms nitrides which impart strength to the steel of the present invention by precipitation strengthening with vanadium and niobium, whenever nitrogen is present in excess of 0.09%, it can form large amounts of aluminum nitrides which are detrimental to the present invention, therefore the preferred upper limit for nitrogen is 0.01%.
[0022] Niobium is an optional element that can be added to the steel up to 0.1%, preferably 0.001% to 0.1%. It is suitable for forming carbonitrides in order to give the steel according to the invention strength by precipitation hardening. Since niobium retards recrystallization during heating, the microstructure formed at the end of the holding temperature and, as a result, after full annealing is finer, which leads to hardening of the product. However, if the niobium content exceeds 0.1%, a large amount of carbonitrides tends to reduce the ductility of the steel, so that this amount of carbonitrides is not preferred for the invention.
[0023] Titanium is an optional element that can be added to the steel of the present invention up to 0.1%, preferably 0.001% to 0.1%. Niobium plays a role in hardening, since it participates in carbonitrides. But it also participates in the formation of TiN, which appears during the solidification of the casting. The amount of Ti is limited to 0.1% to avoid coarse TiN, which is detrimental to the expansion of the hole. If the titanium content is less than 0.001%, it does not have any effect on the steel of the present invention.
[0024] The chromium content of the steel of the present invention is between 0% and 1%. Chromium is an optional element that gives strength and hardness to the steel, but if used in excess of 1%, it will damage the surface finish of the steel.
[0025] Molybdenum is an optional element constituting 0% to 1% of the steel of the invention, it enhances the hardenability of the steel of the invention and influences the transformation of austenite to ferrite and bainite during cooling after annealing, however, the addition of molybdenum excessively increases the cost of adding alloying elements, so its content is limited to 1% for economic reasons.
[0026] Vanadium is an optional element that can be added to the steel of the present invention up to 0.1%, preferably 0.001% to 0.01%. Niobium plays a role in hardening, since it participates in carbonitrides. But it also participates in the formation of VN, which appears during the solidification of the casting. The amount of V is limited to 0.1% to avoid coarse VN, which is detrimental to the expansion of the hole. If the vanadium content is less than 0.001%, it does not have any effect on the steel of the present invention.
[0027] Calcium is an optional element that may be added to the steel of the present invention at up to 0.005%, preferably 0.001% to 0.005%. Calcium is added to the steel of the present invention as an optional element, especially during inclusion treatment. Calcium contributes to the refinement of the steel by preventing harmful sulfur content during spheroidization.
[0028] Other elements such as cerium, boron, magnesium or zirconium can be added individually or in combination in the following proportions: Ce≦0.1%, B≦0.01%, Mg≦0.05% and Zr≦0.05%. Up to the maximum content levels indicated, these elements make it possible to refine the grains during solidification. The invention does not contemplate the addition of copper and nickel, although these elements may be present individually or cumulatively as residuals up to 0.1%.
[0029] The remainder of the steel composition consists of iron and unavoidable impurities resulting from processing.
[0030] The microstructure of the steel sheet according to the present invention comprises, by area fraction, 65% to 85% tempered martensite, 0% and 5% retained austenite, and a cumulative amount of bainite and ferrite of 15% to 35%. The tempered martensite constitutes the matrix phase of the steel according to the present invention. Tempered martensite constitutes 65%-85% of the microstructure by area fraction. Tempered martensite is formed from martensite formed during the second cooling step after annealing, in particular below the Ms temperature, more particularly between Ms-50°C and 20°C. Such martensite is then tempered during a hold at a tempering temperature Temper of 150°C to 400°C. The martensite of the present invention imparts ductility and strength to such steel. Preferably, the martensite content is 65%-80%, more preferably 68%-78%.
[0031] Bainite and ferrite are cumulatively present in the steel in an amount of 15% to 35%. In a preferred embodiment, the cumulative amount of ferrite and bainite is in the range of 20% to 35%, more preferably 22% to 32%.
[0032] The ferrite content improves the properties of the steel of the present invention, especially in terms of elongation and hole expansion ratio, since ferrite is a soft and inherently ductile component. This ferrite is mainly formed during the first step of cooling after annealing. In a preferred embodiment, ferrite may be present in an amount of at least 15%.
[0033] Bainite can impart strength to steel, but if present in large amounts can adversely affect the hole expansion ratio and elongation of the steel. Bainite forms during reheating before tempering. In a preferred embodiment, the bainite content is kept between 0% and 10%, more preferably less than 8%, and even more preferably less than 5%.
[0034] Retained austenite is an optional phase that may be present in the steel at 0%-5%, but is preferably absent.
[0035] In a preferred embodiment, the steel sheet according to the invention can be obtained by any suitable method, however it is preferable to use a method according to a preferred embodiment of the invention comprising the following successive steps:
[0036] Such a method comprises resulting in a semi-finished product of steel having a chemical composition according to the invention, which can be cast in ingots or continuously cast in the form of thin slabs or thin strip, i.e. having a thickness ranging for example from about 220 mm for slabs to a few tens of millimeters for thin strip.
[0037] For the sake of simplicity of the present invention, the slabs are considered as semi-finished products. The slabs having the above-mentioned chemical composition are produced by continuous casting, and the slabs preferably undergo direct soft reduction during casting to ensure the elimination of central segregation and the reduction of porosity. The slabs obtained by the continuous casting process can be used directly at high temperature after continuous casting, or they can be first cooled to room temperature and then reheated for hot rolling.
[0038] The temperature of the slabs subjected to hot rolling must be at least 1000°C, preferably above 1100°C, but below 1250°C. If the temperature of the slab is less than 1000°C, the rolling mill will be overloaded and the temperature of the steel may drop to the ferrite transformation temperature during the finish rolling, so that the steel is rolled with the transformation of ferrite included in the structure. Furthermore, the temperature must not exceed 1250°C, since this may lead to the formation of coarse ferrite particles, which reduces the ability of these particles to recrystallize during hot rolling. The larger the initial ferrite grain size, the less likely the recrystallization will occur. This means that reheating temperatures above 1250°C must be avoided, as they are industrially expensive and unfavorable in terms of ferrite recrystallization.
[0039] The temperature of the slab is preferably high enough so that the hot rolling can be completed entirely in the austenitic range, with the final hot rolling temperature remaining above Ac3, preferably above Ac3+50°C. The final rolling must be performed above Ac3, since below this temperature the steel sheet shows a significant decrease in rollability. In order to have a structure favourable for recrystallization and rolling, the final rolling temperature is preferably above Ac3+50°C.
[0040] The sheet thus obtained is then cooled to a coiling temperature below 600° C. at a cooling rate of at least 30° C. / s. Preferably, the cooling rate is less than or equal to 65° C. / s and greater than 35° C. / s. A coiling temperature of at least 350° C. is preferred to avoid the transformation of austenite into ferrite and pearlite and to favor the formation of homogeneous bainite and martensite microstructures.
[0041] The coiled hot rolled steel sheet may be cooled to room temperature before being subjected to the optional hot strip anneal, or may be sent directly to the optional hot strip anneal.
[0042] The hot rolled steel sheet may be subjected to optional pickling, if necessary, to remove scale formed during hot rolling, and then the hot rolled sheet is subjected to optional hot band annealing at a temperature between 400°C and 750°C, preferably for a period of 1 to 96 hours.
[0043] Thereafter, the hot-rolled steel sheet may be pickled to remove scale, if necessary.
[0044] The hot rolled steel sheet is then cold rolled with a thickness reduction of 35 to 90%. The cold rolled steel sheet is then annealed to impart the targeted microstructure and mechanical properties to the steel of the present invention.
[0045] To anneal the cold rolled steel sheet, the cold rolled steel sheet is heated in a two-step heating process, in step 1, the cold rolled steel sheet is heated to a temperature HT1 of 600°C-650°C with a heating rate HR1 of at least 10°C / s. Then, in step 2, the cold rolled steel sheet is heated from HT1 to an annealing temperature between Ac3 and Ac3+200°C with a heating rate HR2 of at least 1°C / s, preferably at least 2.0°C / s, HR1 is always higher than HR2.
[0046] The preferred HR1 is at least 15° C. / sec, and the preferred temperature HT1 ranges from 600° C. to 630° C. The preferred range of the annealing temperature is Ac3+10° C. to Ac3+150° C., more preferably Ac3+20° C. to Ac3+100° C.
[0047] The cold rolled steel sheet is then held at the annealing temperature for at least 5 seconds to 1000 seconds, the temperature and time being selected to ensure 100% recrystallization, i.e. to obtain a 100% austenite percentage at the end of the annealing.
[0048] The sheet is then cooled in a three-stage cooling process. In step 1, the cold-rolled sheet is cooled from the annealing temperature to a temperature CT1 of 675°C to 725°C at a cooling rate CR1 of 10°C / s or less. Then, in step 2, the cold-rolled sheet is cooled from CT1 to a temperature CT2 of 450°C to 550°C at a cooling rate CR2 of at least 30°C / s. Then, in step 3, the cold-rolled sheet is cooled from CT2 to a temperature CT3 of Ms-50°C to 20°C at a cooling rate CR3 of at least 200°C / s.
[0049] In a preferred embodiment, the cooling rate CR1 is less than or equal to 5°C / sec, and CT1 is preferably between 685°C and 720°C, more preferably between 685°C and 700°C. The preferred range for CR2 is at least 40°C / sec, and the preferred range for CT2 is between 450°C and 525°C, more preferably between 460°C and 510°C. The preferred range for CR3 is at least 300°C / sec, more preferably at least 400°C / sec. The preferred limits for CT3 are Ms-80°C to 20°C, more preferably Ms-100°C to 20°C.
[0050] The cold rolled steel sheet is then brought to a tempering temperature of 300°C-380°C with a heating rate of at least 10°C / s, or better still at least 20°C / s, and held at the tempering temperature for at least 100 seconds, but not more than 1000 seconds, so as to obtain a tempered martensite which gives the steel of the invention good mechanical properties. The preferred tempering temperature range is 320°C-360°C, more preferably 330°C-350°C.
[0051] The cold rolled steel sheet is then cooled to room temperature, preferably at a cooling rate of 200° C. / sec or less.
[0052] At that stage, an optional skin passing operation may be performed with a reduction of less than 1%, and an optional tension leveling operation may be performed.
[0053] The heat treated cold rolled sheet may then optionally be coated by electrochemical or vacuum coating or any other suitable process.
[0054] In order to reduce the hardness gradient between the phases and ensure degassing of the coated product, an optional post-batch anneal can be optionally performed after annealing for uncoated products or after coating for coated products, preferably at 170 to 210° C. for 12 to 30 hours. EXAMPLES
[0055] The following tests and examples presented herein are non-limiting in nature and must be considered for illustrative purposes only, showing the advantageous features of the invention, explaining the importance of the parameters selected by the inventors after extensive experimentation, and further establishing the properties that may be achieved by the steel according to the invention.
[0056] Samples of steel sheets according to the invention and some comparative grades were prepared with the compositions summarized in Table 1 and the processing parameters summarized in Table 2. The corresponding microstructures of these steel sheets are summarized in Table 3 and the properties are summarized in Table 4.
[0057] Table 1 shows the composition of the steels in weight percent.
[0058] [Table 1]
[0059] Table 2 summarizes the annealing process parameters performed on the steels in Table 1.
[0060] Table 2 also shows the Ac3 and martensitic transformation Ms temperatures of the sample steels. The calculation of Ac3 and Ms is performed using the following formulas:
[0061]
number
[0062]
number
[0063] The samples were further heated to temperatures between 1000° C. and 1250° C. and then hot rolled with a finishing temperature of 890° C. and then coiled at a temperature below 600° C. The hot rolled coils were then processed as claimed and cold rolled with a thickness reduction of 35 to 90%.
[0064] [Table 2]
[0065] [Table 3]
[0066] Table 3 summarizes the results of tests carried out according to standards with different microscopes, such as scanning electron microscopes, to determine the microstructural composition of both the steel of the invention and the reference tests.
[0067] [Table 4]
[0068] Table 4 summarizes the mechanical properties of both the inventive and reference steels. Tensile strength, yield strength and total elongation tests are performed according to the ISO 6892 standard, while to estimate the hole expandability a test called hole expandability is applied according to the ISO 16630:2009 standard. In this test, a 10 mm (=Di) hole is drilled in the specimen and deformed. After deformation, the hole diameter Df is measured and the hole expansion ratio (HER) is calculated using the following formula:
[0069] HER%=100 * (Df-Di) / Di
[0070] [Table 5]
[0071] The examples show that the steel sheets according to the invention are unique in that they exhibit all the target properties thanks to their specific composition and microstructure.
Claims
1. Heat treated cold rolled steel sheet containing, in weight percent, the following elements: 0.09%≦Carbon≦0.15% 1.8%≦Manganese≦2.5% 0.2%≦Silicon≦0.7% 0.01%≦Aluminum≦0.1% 0%≦phosphorus≦0.09% 0%≦sulfur≦0.09% 0%≦Nitrogen≦0.09% having a composition comprising One or more of the following optional elements: 0%≦Niobium≦0.1% 0%≦Titanium≦0.1% 0%≦Chromium≦1% 0%≦Molybdenum≦1% 0%≦Vanadium≦0.1% 0%≦Calcium≦0.005% 0%≦Boron≦0.01% 0%≦Cerium≦0.1% 0%≦Magnesium≦0.05% 0%≦Zirconium≦0.05% with the remainder of the composition consisting of iron and unavoidable impurities resulting from processing, and the microstructure of said steel sheet comprising, by area fraction, 65-85% tempered martensite, 0%-5% retained austenite, and a cumulative presence of between 15-35% ferrite and bainite.
2. 2. The heat treated cold rolled steel sheet of claim 1, wherein the composition comprises 0.3% to 0.7% silicon.
3. 3. Heat treated cold rolled steel sheet according to claim 1 or 2, the composition of which comprises 0.01% to 0.08% aluminium.
4. 4. Heat treated cold rolled steel sheet according to claim 1, the composition of which comprises 1.9% to 2.4% manganese.
5. 5. Heat treated cold rolled steel sheet according to any one of claims 1 to 4, the composition of which contains 0.1% to 0.13% carbon.
6. 6. The heat-treated cold rolled steel sheet according to claim 1, wherein the cumulative amount of silicon and aluminum is 0.3% to 0.8%.
7. 7. The heat treated cold rolled steel sheet according to any one of claims 1 to 6, wherein the cumulative amount of ferrite and bainite is between 22% and 35%, the proportion of ferrite being at least 15% of the total area fraction of the steel.
8. 8. The heat treated cold rolled steel sheet according to claim 1, wherein the carbon content of the retained austenite is between 0.7% and 0.9%.
9. 9. The heat treated cold rolled steel sheet according to any one of claims 1 to 8, wherein the tempered martensite is between 65% and 80%.
10. 10. The heat treated cold rolled steel sheet according to any one of claims 1 to 9, wherein bainite is 0% to 10%.
11. 11. The heat treated cold rolled steel sheet according to any one of claims 1 to 10, wherein the steel sheet has an ultimate tensile strength of at least 950 MPa and a total elongation of at least 8%.
12. 12. The cold rolled coated steel sheet according to claim 11, wherein the steel sheet has an ultimate tensile strength of 1000 MPa or more and a hole expansion ratio of at least 55%.
13. A method for producing a heat treated cold rolled steel sheet, comprising the following successive steps: Providing a steel composition according to any one of claims 1 to 6, reheating the semi-finished product to a temperature of between 1000°C and 1250°C; rolling said semi-finished product in a temperature range of Ac3 to Ac3+100°C, such that the hot rolling finishing temperature exceeds Ac3 to obtain hot rolled steel; cooling the hot rolled steel at a cooling rate of at least 30°C / s to a coiling temperature of less than 600°C and coiling the hot rolled steel; Cooling the hot rolled steel to room temperature; Optionally, subjecting the hot rolled steel sheet to a descaling process; Optionally, performing annealing on the hot rolled steel sheet between 400°C and 750°C; Optionally, subjecting the hot rolled steel sheet to a descaling process; cold rolling the hot-rolled steel sheet at a rolling reduction of 35 to 90% to obtain a cold-rolled steel sheet; Annealing the cold-rolled steel sheet by two-stage heating, a first step begins with heating the steel sheet to a temperature HT1 between 600 ° C. and 650 ° C. with a heating rate HR1 of at least 10 ° C. / s; a second step of annealing, starting with further heating the steel sheet from HT1 to an annealing temperature range between Ac3 and Ac3+200°C, with a heating rate HR2 equal to or greater than 1°C / s, HR2 being lower than HR1; then annealing at an annealing temperature for a period of 5 to 1000 seconds; Then, the cold rolled steel sheet is cooled in three stages, The first step begins with cooling the steel sheet from the annealing temperature to a temperature CT1 between 675 ° C. and 725 ° C. at a cooling rate CR1 of not more than 10 ° C. / s; The second step starts with further cooling of the steel plate from CT1 to CT2 of 450°C-550°C at a cooling rate CR2 of at least 30°C / s; a third step starting with further cooling of the steel sheet from CT2 to CT3 of Ms-50°C to 20°C at a cooling rate CR2 of at least 200°C / s; Then, the cold-rolled steel sheet is heated to a tempering temperature of 300° C. to 380° C. at a heating rate of at least 10° C. / s and tempered for 100 to 1000 seconds. and then cooling to room temperature range to obtain a heat treated cold rolled steel sheet. A method comprising:
14. The method according to claim 13, wherein the coiling temperature is from 350°C to 600°C.
15. 15. The method according to claim 13 or 14, wherein the temperature HT1 is between 600° C. and 630° C. and the heating rate HR1 is at least 15° C. / s.
16. The method according to any one of claims 13 to 15, wherein the annealing soak temperature is from Ac3+10°C to Ac3+150°C.
17. The method according to any one of claims 13 to 16, wherein the tempering temperature range is from 320°C to 360°C.
18. 18. Use of a steel sheet according to any one of claims 1 to 12 or produced according to the method of claims 13 to 17 for the manufacture of structural or safety parts of a vehicle.
19. A vehicle comprising a component obtained according to claim 18.
Citation Information
Patent Citations
Super-strength cold-roll steel sheet with excellent bending machining property and manufacturing method thereof
CN103290317A
High strength hot dip galvanised complex phase steel strip
EP2971209A1
High-strength hot-dip galvanized steel sheet with excellent processability and method for producing the same
JP2009209450A
High-strength hot-dip galvanized steel sheet excellent in bendability and weldability, and manufacturing method of the same
JP2012012703A
Method for producing high-strength cold-rolled steel sheet with excellent steel sheet shape
JP2013227657A