Whole resin heat use power generation element

The all-resin thermal power generation element addresses the limitations of conventional thermoelectric conversion elements by providing a flexible, cost-effective, and efficient power generation solution suitable for diverse applications without metal foils.

JP2024153998AActive Publication Date: 2024-10-30SANOH IND CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023067563
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Conventional thermoelectric conversion elements face challenges such as high cost, limited operating temperature range, low conversion efficiency, vulnerability to physical durability, and restricted installation due to the need for a temperature gradient, which limits their application to two-dimensional heat sources and requires cooling devices.

Method used

An all-resin thermal power generation element comprising a semiconductor layer, an electrolyte layer, and a conductive polymer layer, without metal layers, allowing for flexible, miniaturized, and self-supporting power generation capable of operating in diverse locations and applications.

Benefits of technology

The all-resin design reduces material costs, simplifies manufacturing, enhances flexibility, and improves interfacial resistance, enabling efficient power generation in various environments without the need for metal foils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153998000001_ABST
    Figure 2024153998000001_ABST
Patent Text Reader

Abstract

To provide a whole resin heat use power generation element capable of reducing a weight, having flexibility, being adopted to a place where a bent is required, reducing a size, realizing an autonomous, reducing an interface resistance, reducing a cost of an original material, simplifying a manufacturing step, being manufactured in a short time, and preventing an internal shot risk due to the break of a metal film.SOLUTION: In a whole resin heat use power generation element formed by a semiconductor film for generating a whole heat activation electron and a positive hole, an electrolyte film containing a solid electrolyte or an electrolyte solution in which a pair of electric charge transportation ions can be moved, and a conductive film containing an electron transportation material, a metal layer is not contained to each outside of the semiconductor film and the conductive film.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an all-resin thermal power generation element. [Background technology]

[0002] Thermoelectric power generation using the Seebeck effect has been known as a form of thermal power generation that utilizes geothermal energy or waste heat from factories (Patent Documents 1 and 2, and Non-Patent Document 1), and is expected to be put to practical use in order to efficiently utilize thermal energy. Thermoelectric power generation using the Seebeck effect is a power generation principle that utilizes the generation of voltage when a temperature gradient is created in a metal or semiconductor. Specifically, it is a thermoelectric power generation system that converts thermal energy into electrical energy by applying a temperature gradient to a thermoelectric conversion element that combines a p-type semiconductor and an n-type semiconductor.

[0003] However, conventional thermoelectric conversion elements using a temperature gradient have problems such as the high price of the semiconductors that make up the thermoelectric conversion element, the high operating temperature range, and low conversion efficiency. In addition, the physical durability of the joints is weak, making it impossible to install them in places where they are subject to vibration. Furthermore, since a temperature gradient is required for power generation, there are limitations on where they can be installed, and in some cases, a cooling device for the temperature gradient must be used. In particular, one dimension of the thermoelectric conversion module is used for the temperature gradient, so the heat source is used two-dimensionally, and all the surrounding heat cannot be used three-dimensionally, resulting in low heat utilization efficiency. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-147236 A [Patent Document 2] JP 2003-219669 A [Patent Document 3] International Publication No. 2017 / 038988 [Patent Document 4] International Publication No. 2020 / 031992 [Non-patent literature]

[0005] [Non-Patent Document 1] "Renewable and Sustainable Energy Reviews" (Netherlands) 2014, Vol. 33, p. 371 Summary of the Invention [Problem to be solved by the invention]

[0006] A heat-powered cell capable of converting thermal energy into electrical energy has been developed by combining a thermoelectric conversion material that generates thermally excited electrons and holes with an electrolyte (Patent Document 3). The present inventors have developed an even more stable heat-powered cell (Patent Document 4). However, there has been a demand for a heat-powered cell that can be used in a wider variety of locations and for a wider variety of applications. SUMMARY OF THE PRESENT EMBODIMENT It is therefore an object of the present invention to provide a thermal energy generating cell that can be used in a variety of locations and applications. [Means for solving the problem]

[0007] The present inventors conducted extensive research into heat-powered power generating cells that can be used in a variety of locations and for a variety of purposes, and as a result, they surprisingly discovered that an all-resin heat-power generating element that does not have metal foil can be used in a variety of applications. The present invention is based on these findings. Thus, the present invention provides [1] An all-resin thermal power generating element including a semiconductor layer that generates thermally excited electrons and holes, an electrolyte layer that includes a solid electrolyte or electrolyte solution in which charge-transporting ion pairs can move, and a conductive polymer layer that includes an electron transport material, the all-resin thermal power generating element not including a metal layer on the outside of each of the semiconductor layer and the conductive polymer layer; [2] A laminated all-resin heat-utilizing power generation element in which two or more all-resin heat-utilizing power generation elements according to [1] are laminated; [3] The laminated all-resin heat-utilizing power generating element according to [2], which has a metal layer on the outer side of one semiconductor layer of the laminated all-resin heat-utilizing power generating element and on the outer side of the other conductive polymer layer. [4] The thermal energy generating element according to any one of [1] to [3], 15 / m 3 A method of generating electricity by placing the device in an environment with a temperature equal to or higher than the temperature at which the device is heated. [5] A thermoelectric power generation device including the heat utilization power generation element according to any one of [1] to [3]. [6] A thermobattery including the thermoelectric power generation element according to any one of [1] to [3]. [7] A thermoelectric power generation module including the thermoelectric power generation element according to any one of [1] to [3]. [8] A thermoelectric power generation method including a step of installing the thermoelectric power generation module according to [7] at a heat generation location, and a step of heating the thermoelectric power generation module with heat to generate electric power; and [9] The thermoelectric power generation method according to [8], wherein the heat is geothermal heat or exhaust heat. Regarding. Effect of the Invention

[0008] The all-resin heat-utilizing power generation element of the present invention does not have a metal foil, so it can be made lighter in weight. The all-resin heat-utilizing power generation element of the present invention does not have a metal foil, so it is highly flexible and can be applied to places where bending is required, and can also be made smaller. The all-resin heat-utilizing power generation element of the present invention can be made to stand on its own, even though it does not have a metal foil. The all-resin heat-utilizing power generation element of the present invention can reduce interface resistance because it does not have a metal foil. The all-resin heat-utilizing power generation element of the present invention does not have a metal foil, so it is possible to reduce the cost of raw materials, the manufacturing process is simplified, and it can be manufactured in a short time. The all-resin heat-utilizing power generation element of the present invention can prevent the risk of internal shots caused by cracking of the metal film. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a diagram showing a conventional thermal power generation element. [Diagram 2] FIG. 2 is a diagram showing an all-resin heat-utilizing power generating element of the present invention. [Diagram 3] 1 shows a conventional laminated heat-utilizing power generating element (A) having a metal layer between the heat-utilizing power generating elements, and a laminated all-resin heat-utilizing power generating element of the present invention (B or C) having no metal layer between the all-resin heat-utilizing power generating elements. (B) has a metal layer on the outside of one semiconductor layer and on the outside of the other conductive polymer layer of the laminated all-resin heat-utilizing power generating element. [Figure 4] FIG. 1A shows the adhesion between a semiconductor layer and a metal foil produced by a conventional method, and FIG. 1B shows the adhesion between a semiconductor layer and a metal foil produced by the method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [1] All-resin thermoelectric generation element The all-resin thermoelectric generator of the present invention includes a semiconductor layer that generates thermally excited electrons and holes, an electrolyte layer that includes a solid electrolyte or an electrolyte solution in which charge-transporting ion pairs can move, and a conductive polymer layer that includes an electron transport material. The all-resin thermoelectric generator of the present invention does not include a metal layer on the outside of each of the semiconductor layer and the conductive polymer layer. As used herein, "all resin" means that the internal active cell structure does not include a metal layer, and the semiconductor layer, electrolyte layer, and conductive polymer layer include resin. No metal is used in the laminate structure, but metal current collectors may be used for the positive and negative electrodes. Also, metal wires, carbon sheets, graphene, or conductive fibers can be used as current collectors instead of metal layers.

[0011] Semiconductor layer The semiconductor layer constituting the thermoelectric generating element of the present invention contains a semiconductor. In this specification, the term "semiconductor" refers to a material capable of generating thermally excited electrons and holes by heat. Specific examples include metal semiconductors, tellurium compound semiconductors, silicon germanium (Si-Ge) compound semiconductors, silicide compound semiconductors, skutterudite compound semiconductors, clathrate compound semiconductors, Heusler compound semiconductors, half-Heusler compound semiconductors, metal oxide semiconductors, organic semiconductors, and other semiconductors. The semiconductor used in the present invention functions as a thermoelectric conversion material.

[0012] Examples of metal semiconductors include Si semiconductors and Ge semiconductors. Tellurium compound semiconductors include Bi-Te compounds (e.g., Bi2Te3, Sb2Te3, CsBi4Te6, Bi2Se3, Bi 0.4 Sb 1.6 Te3, Bi2(Se,Te)3, (Bi,Sb)2(Te,Se)3, (Bi,Sb)2Te3, or Bi2Te 2.95 Se 0.05 ), Pb-Te compounds (e.g., PbTe or Pb 1-x Sn x Te), SnTe, Ge-Te, AgSbTe2, Ag-Sb-Ge-Te compounds (e.g., GeTe-AgSbTe2 (TAGS)), Ga2Te3, (Ga 1-x In x )2Te3, Tl2Te-Ag2Te, Tl2Te-Cu2Te, Tl2Te-Sb2Te3, Tl2Te-Bi2Te3, Ti2Te-GeTe, Ag8Tl2Te5, Ag9TlTe5, Tl9BiTe6, Tl9SbTe6, Tl9CuTe5, Tl4SnTe3, Tl4PbTe3, or Tl 0.02 Pb 0.98 Te can be mentioned.

[0013] Silicon germanium (Si-Ge) compound semiconductors include Si x Ge 1-x , or SiGe-GaP.

[0014] Silicide compound semiconductors include β-FeSi2 compounds (e.g., β-FeSi2, Fe 1-x Mn x Si2, Fe 0.95 Mn 0.05 S (2-y) Al y , FeSi (2-y) Al y , Fe 1-y Co y Si2), Mg2Si, MnSi 1.75-x , Ba8Si 46 , Ba8Ga 16 S 30 , or CrSi2.

[0015] Skutterudite compound semiconductors include compounds represented by the formula TX3 (wherein T is a transition metal selected from the group consisting of Co, Fe, Ru, Os, Rh, and Ir, and X is a pnictogen selected from the group consisting of P, As, and Sb), and derivatives of the compounds represented by the formula RM4X 12 (wherein R is a rare earth selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu; M is selected from the group consisting of Fe, Ru, Os, and Co; and X is selected from the group consisting of P, As, and Sb), y Fe 4-x Co x Sb 12 , (CeFe3CoSb 12 ) 1-x (MoO2) x or (CeFe3CoSb 12 ) 1-x (WO2) x The following can be mentioned.

[0016] Clathrate compound semiconductors include those with the formula M8X 46 (M is selected from the group consisting of Ca, Sr, Ba, and Eu, and X is selected from the group consisting of Si, Ge, and Sn), a compound represented by the formula (II)8(III) 16 (IV) 30(wherein II is a group II element, III is a group III element, and IV is a group IV element) can be mentioned. 16 (IV) 30 As an example of the compound, Ba8Ga x Ge 46-x , B.A. 8-x (Sr,Eu) x Au6Ge 40 , or Ba 8-x EU x Cu6Si 40 ) can be mentioned.

[0017] Heusler compound semiconductors include Fe2VAl, (Fe 1-x Re x )2VAl, or Fe2(V 1-x-y Ti x Ta y )Al can be mentioned.

[0018] Examples of the half-Heusler compound semiconductor include a compound represented by the formula MSiSn (wherein M is selected from the group consisting of Ti, Zr, and Hf), a compound represented by the formula MNiSn (wherein M is Ti or Zr), a compound represented by the formula MCoSb (wherein M is selected from the group consisting of Ti, Zr, and Hf), or a compound represented by the formula LnPdX (wherein Ln is selected from the group consisting of La, Gd, and Er, and X is Bi or Sb).

[0019] Metal oxide semiconductors include In2O3-SnO2, (CaBi)MnO3, Ca(Mn, In)O3, and Na x V2O5, V2O5, ZnMnGaO4 and its derivatives, LaRhO3, LaNiO3, SrTiO3, SrTiO3:Nb, Bi2Sr2Co2O y , Na x CoO2, NaCo2O4, CaPd3O4, formula Ca a M 1 b Co c M 2 d Ag e Of (In the formula, M 1 is one or more elements selected from the group consisting of Na, K, Li, Ti, V, Cr, Mn, Fe, Ni, Cu, Zn, Pb, Sr, Ba, Al, Bi, Y and rare earth elements, and M 2 is one or two elements selected from the group consisting of Ti, V, Cr, Mn, Fe, Ni, Cu, Mo, W, Nb, Ta and Bi, and 2.2≦a≦3.6, 0≦b≦0.8, 2≦c≦4.5, 0≦d≦2, 0≦e≦0.8, 8≦f≦10), ZnO, Na(Co,Cu)2O4, ZnAlO, Zn 1-x Al x O or La 1.98 Sr 0.02 CuO4 can be mentioned.

[0020] The organic semiconductor may include an organic perovskite, a polyaniline, a polyacetylene, a polythiophene, a polyalkylthiophene, or a polypyrrole.

[0021] Other semiconductors include alloys containing Co and Sb (e.g., CoSb3, CeFe3CoSb 12 , CeFe4CoSb 12 , or YbCo4Sb 12 ), alloys containing Zn and Sb (e.g., ZnSb, Zn3Sb2, or Zn4Sb3), alloys containing Bi and Sb (e.g., Bi 88 Sb 12 ), CeInCu2, (Cu,Ag)2Se, Gd2Se3, CeRhAs, or CeFe4Sb 12 , Li 7.9 B 105 , BaB6, SrB6, CaB6, AlPdRe compounds (e.g., Al 71 Pd 20 (Re 1-x Fe x )9), AlCuFe quasicrystal, Al 82.6-x Re 17.4 S x 1 / 1-cubic approximation crystal, YbAl3, YbMn x Al3, β-CuAgSe, B4C / Ba3C, (Ce 1-x Lax )Ni2, or (Ce 1-x La x )In3 can be mentioned.

[0022] The semiconductor layer may contain components other than the semiconductor, so long as the semiconductor can generate a sufficient number of thermally excited electrons and holes for power generation when exposed to an appropriate temperature. Examples of the components include, but are not limited to, binders (polyvinyl alcohol, methyl cellulose, acrylic resin, agar, etc.) that bind the thermoelectric conversion material, and sintering aids (magnesium oxide, yttrium oxide, calcium oxide, etc.) that help mold the thermoelectric conversion material. In addition, a solvent used in the manufacturing process may remain. The first layer used in the present invention essentially functions as a thermoelectric conversion layer. The semiconductor layer of the present invention contains a resin, which may include, but is not limited to, the binder described above.

[0023] 《Electrolyte layer》 The electrolyte layer includes a solid electrolyte or an electrolyte solution in which a charge-transporting ion pair can move. As used herein, a "charge-transporting ion pair" refers to two stable ions of different valences, one of which can be oxidized or reduced to the other ion and can transport electrons and holes. The ions may be of the same element but with different valences. The ion source contained in the solid electrolyte of the present invention is not particularly limited as long as it is a metal ion, and examples thereof include copper ions, iron ions, vanadium ions, manganese ions, nickel ions, tin ions, zinc ions, aluminum ions, calcium ions, potassium ions, magnesium ions, palladium, titanium ions, alkali metal ions, and rare earth metal ions. For example, copper ions or iron ions include monovalent copper ions, divalent copper ions, divalent iron ions, and trivalent iron ions. However, it is preferable that the copper ions or iron ions are two stable ions with different valences. This is because one ion is oxidized or reduced to become the other ion, which can transport electrons and holes. Therefore, in the case of copper ions, monovalent copper ions and divalent copper ions are preferred, and in the case of iron ions, divalent iron ions and trivalent iron ions are preferred. As the monovalent copper ions, for example, CuCl, CuBr, copper(I) acetate, copper(I) iodide, or copper(I) sulfate can be used. As the divalent copper ions, CuCl2, CuTSFI2, copper(II) acetate, copper(II) sulfate, or copper(II) acetylacetonate can be used. As the divalent iron ions, Fe(C5H5)2 (ferrocene), K4[Fe(CN)6], iron(II) acetylacetonate, iron(II) chloride, iron(II) sulfate, or iron(II) acetate can be used. As the trivalent iron ions, FeCl3, K3[Fe(CN)6], iron(III) acetylacetonate, or iron(III) sulfate can be used.

[0024] The concentration of the ion source is not particularly limited as long as the effects of the present invention can be obtained, but it is preferable to add the ion source so that the concentration is, for example, 0.01 to 98 mol % relative to the polymer, etc. By being in the above range, the ion source can efficiently transport electrons and holes.

[0025] (electrolyte) The electrolyte includes a solid electrolyte or an electrolyte solution, and is not limited as long as it can transport two ions of a charge-transporting ion pair. That is, the electrolyte used in the electrolyte layer is not particularly limited as long as the oxidation-reduction potential is in an appropriate position relative to the valence electron charge potential of the thermoelectric conversion material used in the thermoelectric power generation element and the charge-transporting ion pair can move back and forth within the electrolyte. Note that the electrolyte is preferably physically and chemically stable at a temperature at which the thermoelectric conversion material generates a sufficient number of thermally excited electrons and holes for power generation.

[0026] The electrolyte may be a solid electrolyte or an electrolyte solution (liquid electrolyte) depending on the form. Here, the electrolyte may be an electrolyte solution (liquid electrolyte) or a solid electrolyte depending on the temperature. That is, the compounds contained in the electrolyte solution (liquid electrolyte) and the compounds contained in the solid electrolyte overlap. The electrolyte also includes a molten salt, an ionic liquid, or a deep eutectic solvent. The molten salt means a salt consisting of a cation and an anion, which is in a molten state. Among molten salts, a molten salt having a relatively low melting point (for example, 100°C or less, or 150°C or less) is called an ionic liquid. In this specification, a molten salt in a solid state is called a solid electrolyte, and a molten salt in a solution state is called an electrolyte solution (liquid electrolyte). Specific examples of electrolyte solutions (liquid electrolytes), solid electrolytes, and molten salts are given below, but they may overlap.

[0027] The electrolyte solution used is in a solution (liquid) state at a temperature at which the semiconductor in the semiconductor layer generates a sufficient number of thermally excited electrons and holes for power generation.Specific examples of the electrolyte solution include, but are not limited to, methoxide ions, hydrogen ions, ammonium ions, pyridinium ions, lithium ions, sodium ions, potassium ions, calcium ions, magnesium ions, aluminum ions, iron ions, copper ions, zinc ions, cobalt ions, fluoride ions, cyanide ions, thiocyanate ions, chloride ions, acetate ions, sulfate ions, carbonate ions, phosphate ions, hydrogen carbonate ions, and bromine ions.

[0028] The solid electrolyte is in a solid state in which charge-transporting ion pairs can move inside at a temperature at which the semiconductor in the semiconductor layer generates a sufficient number of thermally excited electrons and holes for power generation. The high-temperature solid electrolyte can be used in a thermoelectric generator that generates thermally excited electrons and holes at high temperatures. Specifically, the solid electrolyte is not limited to, but may include, for example, a sodium ion conductor, a copper ion conductor, a lithium ion conductor, a silver ion conductor, a hydrogen ion conductor, a strontium ion conductor, an aluminum ion conductor, a fluorine ion conductor, a chloride ion conductor, or an oxide ion conductor. Specific examples of the solid electrolyte include RbAg4I5, Li3N, Na2O·11Al2O3, Sr-β alumina, Al(WO4)3, PbF2, PbCl2, (ZrO2) 0.9 (Y2O3) 0.1 , (Bi2O3) 0.75 (Y2O3) 0.25 , CuZr2(PO4)3, CuTi2(PO4)3, Cu x Nb 1-x Ti 1+x (PO4)3, H 0.5 Cu 0.5 Zr2(PO4)3, Cu 1+x Cr x Ti 2-x (PO4)3, Cu 0.5 TiZr(PO4)3, CuCr2Zr(PO4)3, Cu2ScZr(PO4)3, CuSn2(PO4)3, CuHf2(PO4)3, Li7La3Zr2O 12 , Li7La3Zr 2-x Nb x O 12 , Li7La3Zr 2-x TaxO 12 , Li5La3Ta2O 12 , Li 0.33 La 0.55 TiO3, Li 1.5 Al 0.5 Ge 1.5 P3O 12 , Li 1.3 Al 0.3 Ti 1.7 P3O 12, Li3PO4 (LiPON), Li4SiO4-Li3PO4, Li4SiO4, or Li3BO3. In addition, a molten salt can be used as the solid electrolyte or the electrolyte solution. In the case of a thermoelectric generating element used at a relatively low temperature, an ionic liquid can also be used. As the ionic liquid, a deep eutectic solvent (DES) can be used.

[0029] The molten salt may include at least one cation selected from the group consisting of imidazolium cation, pyridinium cation, piperidinium cation, pyrrolidinium cation, phosphonium cation, morpholinium cation, sulfonium cation, and ammonium cation, and at least one anion selected from the group consisting of carboxylate anion, sulfonate anion, halogen anion, tetrafluoroborate, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, and bis(fluorosulfonyl)imide. The electrolyte in the present invention functions as a hole transporting material.

[0030] The electrolyte layer is not limited as long as it can transport holes generated in the thermoelectric conversion material, and may contain components other than the solid electrolyte or the electrolyte solution. Examples of the components include, but are not limited to, a solvent (water, methanol, toluene, tetrahydrofuran, etc.) that dissolves or disperses the electrolyte when preparing the second layer, a binder (polyvinyl alcohol, methyl cellulose, acrylic resin, agar, etc.) that binds the electrolyte, and a sintering aid (magnesium oxide, yttrium oxide, calcium oxide, etc.) that helps form the hole transport material. The second layer used in the present invention essentially functions as a hole transport layer. The electrolyte layer contains a resin, which may be, but is not limited to, the binder or metal salt (ion source), the separator (made of resin), or an insulating ceramic.

[0031] The electrolyte layer can be prepared by, for example, a squeegee method, a screen printing method, a sputtering method, a vacuum deposition method, a sol-gel method, or a spin coating method. For example, CuZr2(PO4)3 described later was prepared by a sol-gel method, and the obtained sol was used by a squeegee method to prepare a layered electrolyte layer. Furthermore, when the electrolyte is an electrolyte solution (liquid electrolyte), the second layer is in a liquid phase. When the second layer is in a liquid phase, the second layer in the thermoelectric power generation element is preferably prepared when the thermoelectric power generation device, thermobattery, or thermoelectric power generation module is produced. That is, the second layer can be produced by providing a tank for holding the electrolyte solution (liquid electrolyte).

[0032] Conductive polymer layer The conductive polymer layer includes an electron transport material. Examples of the electron transport material include polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyaniline-based conductive polymers, and polypyrrole-based conductive polymers. Specific examples of the electron transport material include polyacetylene, poly(p-phenylene), poly(p-phenylenevinylene), and polyaniline.

[0033] The conductive polymer layer may contain components other than the electron transport material, so long as it can transport thermally excited electrons generated by the thermoelectric conversion material. The components include, but are not limited to, binders (polyvinyl alcohol, methyl cellulose, acrylic resin, agar, etc.) that bind the electron transport material, and sintering aids (magnesium oxide, yttrium oxide, calcium oxide, etc.) that help mold the electron transport material. In addition, the solvent used in the manufacturing process may remain. The third layer used in the present invention essentially functions as an electron transport layer. In the thermoelectric generating element of the present invention, the electron transport material has an electron conduction potential that is the same as or positive to the conduction potential of the semiconductor in the semiconductor layer, and therefore the electron transport material can transport thermally excited electrons.

[0034] The conductive polymer layer can be prepared by, for example, a squeegee method, a screen printing method, a sputtering method, a vacuum deposition method, a single crystal growth method, or a spin coating method. When using the spin coating method, the conductive polymer layer can be prepared by dissolving the oxadiazole derivative in a polar solvent such as acetone, and spin coating the solution onto the substrate or the first layer.

[0035] <<Laminated all-resin heat-utilizing power generation element>> The all-resin heat-utilizing power generating element of the present invention can be used as a laminated all-resin heat-utilizing power generating element by stacking two or more all-resin heat-utilizing power generating elements. As shown in FIG. 3A, a conventional laminated heat-utilizing power generating element has a metal layer between the laminated heat-utilizing power generating elements and the heat-utilizing power generating elements. In contrast, as shown in FIG. 3B or C, the laminated all-resin heat-utilizing power generating element of the present invention does not have a metal layer between the laminated heat-utilizing power generating elements and the heat-utilizing power generating elements. As shown in FIG. 3B, the laminated all-resin heat-utilizing power generating element may have a metal layer as a current collector on the outside of one semiconductor layer and on the outside of the other conductive polymer layer. Furthermore, instead of the metal layer, a metal wire, a carbon sheet, graphene, or a conductive fiber can be used as a current collector.

[0036] [2] Manufacturing method of semiconductor layer The all-resin thermal power generation element of the present invention does not have a metal layer. Therefore, in the manufacturing method of the semiconductor layer, the semiconductor layer is peeled off from the metal foil that is the substrate. The conventional manufacturing method is a coating and drying method, and as shown in FIG. 4A, the adhesion area between the semiconductor layer and the metal foil is large, and the adhesive force between the semiconductor film and the metal foil is strong. Therefore, it is difficult to peel off the semiconductor layer from the metal foil. According to the manufacturing method of the semiconductor layer of the present invention, the adhesion area between the semiconductor layer and the metal foil is small, as shown in FIG. 4B, and the semiconductor film can be easily peeled off from the metal foil.

[0037] The method for manufacturing a semiconductor layer includes the steps of (1) mixing a semiconductor material with a binder solution to obtain a semiconductor binder mixture, (2) mixing a solvent that cannot dissolve the binder to obtain a gel mixture, (3) applying the gel mixture to metal foil and further sandwiching the metal foil, (4) applying pressure to the gel mixture sandwiched between the metal foils, and (5) peeling off the metal foils.

[0038] In the mixing step (1), a semiconductor material is mixed into the binder solution. As the semiconductor material, any of the semiconductor materials described in the "Semiconductor Layer" section above can be used without limitation. The binder includes, but is not limited to, PVDF, PVA, PEC, PEG, PMMA, PA, PE, PPG, PP, PAI, PU, ​​PI, or PPC. Examples of the solvent that dissolves the binder include, but are not limited to, an NMP solution, a DMSO solution, a DMF solution, a pyridine solution, a toluene solution, an acetone solution, or an acetonitrile solution.

[0039] In the step (2) of obtaining the semi-solid mixture, a solvent that cannot dissolve the binder is mixed to obtain the semi-solid mixture. By adding a solvent that cannot dissolve the binder, the semi-solid mixture can be obtained. Solvents that cannot dissolve the binder include acetone, alcohol (eg, methanol, ethanol propanol, etc.), water, ether, or THF. The amount of the solvent that cannot dissolve the binder to be added is not particularly limited as long as a semi-solid mixture is obtained, but for example, 1 to 50 parts by volume, preferably 5 to 30 parts by volume, and more preferably 10 to 15 parts by volume can be added, assuming that the semiconductor binder mixture is 100 parts by volume.

[0040] In the step (3), the semi-solid mixture is applied to a metal foil and then sandwiched between two metal foils, that is, the semi-solid mixture is sandwiched between two metal foils. The metal foil is not particularly limited, and examples thereof include stainless steel foil, copper foil, aluminum foil, titanium foil, gold foil, silver foil, platinum foil, nickel foil, zinc foil, and brass foil. However, without using a metal foil, the semi-solid mixture may be placed in a hydraulic press or the like in the following pressure application step (4) and pressure may be applied. Although the hydraulic press or the like may be soiled by the semi-solid mixture, the present invention can be sufficiently implemented.

[0041] In the pressure application step (4), pressure is applied to the semi-solid mixture. The pressure applied to the semi-solid mixture is not particularly limited as long as the effects of the present invention can be obtained, but is, for example, within the range of 0.01 to 200 MPa, preferably 0.1 to 20 MPa, and more preferably 1 to 10 MPa. The method of applying pressure is not particularly limited, but pressure can be applied using a hydraulic press or a hand press.

[0042] When a metal foil is used in the step (3), the metal foil is peeled off in the metal foil peeling step (5). In detail, the upper metal foil is slowly peeled off so as not to tear the film, and the film is vacuum dried, for example, at 25° C. to 80° C., preferably 50° C. to 70° C. After vacuum drying, the lower metal foil is slowly peeled off so as not to tear the free-standing film.

[0043] [3] Method for manufacturing conductive polymer layer A conductive polymer dispersion is dropped onto a metal foil. After uniformly dispersing to the required thickness, it is dried at high temperature. The dried polymer metal foil is left under an inert gas atmosphere. A conductive polymer layer is obtained. The metal foil is not particularly limited, but examples thereof include stainless steel foil, copper foil, aluminum foil, titanium foil, gold foil, silver foil, platinum foil, nickel foil, zinc foil, and brass foil. The conductive polymer may be a polythiophene-based conductive polymer, a polyacetylene-based conductive polymer, a polyaniline-based conductive polymer, or a polypyrrole-based conductive polymer.Specific examples of the electron transport material include polyacetylene, poly(p-phenylene), poly(p-phenylenevinylene), and polyaniline.

[0044] [4] Power generation method The power generation method of the present invention further comprises: 15 / cm 3 In the power generation method of the present invention, the thermally excited electron density is preferably 10 15 / cm 3 More preferably, it is 10 18 / cm 3 More preferably, 10 20 / cm 3 More preferably, 10 22 / cm 3 The higher the thermally excited electron density, the higher the power generation efficiency that can be obtained. The temperature applied to the semiconductor can be appropriately selected so that each semiconductor generates a sufficient number of thermally excited electrons and holes for power generation. In other words, in the present invention, a voltage can be generated in the thermoelectric power generation element by applying to the semiconductor a temperature at which the semiconductor generates a sufficient number of thermally excited electrons and holes for power generation. The number of thermally excited electrons and holes sufficient for power generation is actually expressed as electron density, and may be approximately the same as the number of photoexcited electrons in the semiconductor used in the solar cell, for example, 10, which is the number of photoexcited electrons in amorphous silicon used in solar cells. 15 / cm 3 That is, in the thermoelectric conversion material used in the present invention, the thermally excited electron density is 10 15 / cm 3 At a temperature equal to or higher than this, it is possible to generate a sufficient number of thermally excited electrons and holes for power generation, and power generation can be performed at temperatures equal to or higher than this temperature.

[0045] [5] Thermoelectric power generation devices, thermobatteries, and thermoelectric power generation modules The thermoelectric power generation device of the present invention includes the thermoelectric power generation element of the present invention, and preferably includes a positive electrode and / or a negative electrode. The thermobattery of the present invention includes the thermoelectric power generation element of the present invention, and preferably includes a positive electrode and / or a negative electrode. Furthermore, the thermoelectric power generation module of the present invention includes the thermoelectric power generation element of the present invention, and preferably includes a positive electrode and / or a negative electrode. In this specification, the term "thermoelectric battery" refers to a battery that includes the thermoelectric power generation element of the present invention and generates electricity by applying a temperature to the semiconductor (thermoelectric conversion material) of the thermoelectric power generation element at which thermally excited electrons and holes can be generated. In other words, a thermoelectric battery is a "battery that generates electricity if there is a heat source" and is different from conventional "batteries that generate electricity by using high-temperature and low-temperature parts."

[0046] "electrode" The positive and negative electrodes are not limited as long as they can transport electrons, but examples thereof include titanium, gold, platinum, silver, copper, tin, tungsten, niobium, tantalum, stainless steel, aluminum, graphene, molybdenum, indium, vanadium, rhodium, niobium, chromium, nickel, carbon, alloys thereof, and combinations thereof. The same material may be used for the positive and negative electrodes. The positive and negative electrodes may be provided in the form of conductors, or may be provided as a positive electrode layer or a negative electrode layer. In the case of a positive electrode layer or a negative electrode layer, it can be manufactured by a vacuum deposition method, a spin coating method, or the like. By providing a negative electrode on the third layer side of the thermoelectric generating element and a positive electrode on the second layer side, electrons can move from the negative electrode to the positive electrode, generating electricity.

[0047] [6] Thermoelectric power generation method The thermoelectric power generation method of the present invention includes the steps of placing the thermoelectric power generation module at a heat generation location, and heating the thermoelectric power generation module with heat to generate electric power.

[0048] <<Thermoelectric power generation module installation process>> In the thermoelectric power generation module installation step, the thermoelectric power generation module of the present invention is installed at a heat generation location. The heat generating location is not particularly limited as long as it is a location that generates heat at a temperature equal to or higher than the temperature at which a sufficient number of excited electrons and holes are generated in the thermoelectric conversion material for power generation. However, a location with a relatively high temperature is preferable because it allows efficient power generation, and therefore examples of the heat generating location include a geothermal generating location and a waste heat generating location such as a factory. Geothermal energy is not limited to heat in the soil, but also includes hot water or steam heated by geothermal energy, and further includes hot water or steam from the sea, lakes, rivers, etc., heated by geothermal energy. The waste heat is not particularly limited, but examples thereof include waste heat from steel furnaces, waste incineration plants, substations, subways, automobiles, etc. In particular, the waste heat from steel furnaces and waste incineration plants, which have large amounts of energy, is discharged without being utilized, and it is preferable to reuse the energy by the thermoelectric power generation method of the present invention.

[0049] <Electricity generation process> In the power generation step, the thermoelectric power generation module of the present invention is heated to generate power. The heat generated from the heat generation location heats the thermoelectric conversion material of the thermoelectric power generation module to a temperature at or above the temperature at which a sufficient number of excited electrons and holes are generated for power generation, whereby power can be generated from the thermoelectric power generation module. EXAMPLES

[0050] The present invention will be specifically described below with reference to examples, but the scope of the present invention is not limited thereto.

[0051] Example 1 (Creating a free-standing PEDOT:PSS film) A conductive polymer layer was created by applying 1 mL of PEDOT / PSS dispersion onto a mirror-finished copper foil and drying at 120°C. It was then left in an argon gas atmosphere for several hours, and the PEDOT / PSS free-standing film was peeled off.

[0052] (Electrolyte Creation) An electrolyte layer was created. 5% polyvinylidene fluoride (PVDF) was dissolved in N-methyl-2-pyrrolidone (NMP) by heating at 60°C to create a PVDF (5%) solution. 166 mg of lithium chloride (LiCl) was dissolved in 8 g of this solvent by heating at 60°C. 68 mg of copper chloride (I) and 94 mg of copper chloride (II) were added and dissolved by heating at 60°C. The obtained electrolyte solution was dropped onto the separator. Once the separator was immersed in the electrolyte solution, it was heated at 60°C and vacuum dried.

[0053] (Creating free-standing semiconductor films) A semiconductor layer was created. 200 mg of Ge was put into a mortar and ground. 2.0 g of binder solution (PVDF in NMP) was added and stirred. Next, 1 mL of acetone, a solvent that cannot dissolve the binder, was added to make the semiconductor mixture semi-solid. A piece of stainless steel foil was laid down, and the semiconductor mixture was placed on top of it and sandwiched between another piece of stainless steel foil. The mixture was clamped at room temperature for 1 hour in a vice (universal angle vice, Palmgren) at a pressure of 2 MPa. The mixture was removed from the pressure machine, the upper and lower stainless steel foils were peeled off, and the mixture was vacuum dried at 60°C to obtain a semiconductor free-standing film.

[0054] The "conductive polymer layer", "electrolyte layer", and "semiconductor layer" obtained in the above steps were laminated as follows to obtain an all-resin heat-utilizing power generating element of the present invention. The power generating unit of the all-resin heat-utilizing power generation element was obtained by stacking the "conductive polymer layer" (positive electrode), "electrolyte layer" and "semiconductor layer" (negative electrode) in that order (Figure 2). Furthermore, multiple units of the above can be stacked to create an all-resin heat-utilizing power generation element.

[0055] Example 2 In this example, the procedure of Example 1 was repeated except that PVA was used instead of PVDF as the binder, to obtain an all-resin heat-utilizing power generating element of the present invention. In the preparation of the free-standing semiconductor film, the stainless steel foil could be easily peeled off from the semiconductor layer.

[0056] Example 3 In this example, the procedure of Example 1 was repeated except that PEC was used as the binder instead of PVDF, to obtain an all-resin heat-utilizing power generating element of the present invention. In the preparation of the free-standing semiconductor film, the stainless steel foil could be easily peeled off from the semiconductor layer.

[0057] Comparative Example 1 In this example, a hydrothermal power generation element having a metal layer was produced according to a conventional method. (Creation of PEDOT:PSS film) A conductive polymer layer was created. 1 mL of PEDOT / PSS dispersion was applied and dispersed on a mirror-finished copper foil and dried at 120°C. It was then left to stand for several hours under an argon gas atmosphere. A PEDOT / PSS film with a mirror-finished copper foil was obtained.

[0058] (Electrolyte Creation) An electrolyte layer was created. 5% polyvinylidene fluoride (PVDF) was dissolved in N-methyl-2-pyrrolidone (NMP) by heating at 60°C to create a PVDF (5%) solution. 166 mg of lithium chloride (LiCl) was dissolved in 8 g of this solvent by heating at 60°C. 68 mg of copper chloride (I) and 94 mg of copper chloride (II) were added and dissolved by heating at 60°C. The obtained electrolyte solution was dropped onto the separator. Once the separator was immersed in the electrolyte solution, it was heated at 60°C and vacuum dried.

[0059] (Preparation of Semiconductor Layer with Metal Foil) A semiconductor layer was created. 200 mg of Ge was placed in a mortar and ground. 2.0 g of binder solution (PVDF in NMP) was added and stirred. The solution was dropped onto stainless steel foil and a film was created using an applicator. The coated metal foil was vacuum dried at 60°C. The metal foil could not be peeled off from the semiconductor layer.

[0060] The "conductive polymer layer," "electrolyte layer," and "semiconductor layer" obtained in the above steps were stacked as follows to obtain a conventional heat-utilizing power generation element. The power generation unit of a conventional heat-utilizing power generation element was obtained by stacking the "conductive polymer layer" (positive electrode) / "electrolyte layer" / "semiconductor layer" (negative electrode) in that order (Figure 1). [Industrial Applicability]

[0061] The all-resin heat-utilizing power generation element of the present invention is highly flexible because it does not have metal foil, and can be applied to places where bending is required, and can also be made compact.

Claims

1. A semiconductor layer that generates thermally excited electrons and holes; an electrolyte layer comprising a solid electrolyte or an electrolyte solution in which charge-transporting ion pairs can migrate; a conductive polymer layer comprising an electron transport material; An all-resin heat-utilizing power generation element comprising: An all-resin heat-utilizing power generation element that does not include any metal layers on the outside of either the semiconductor layer or the conductive polymer layer.

2. A laminated all-resin heat-utilizing power generation element comprising two or more all-resin heat-utilizing power generation elements according to claim 1 stacked together.

3. 3. The laminated all-resin heat-utilizing power generating element according to claim 2, further comprising a metal layer on the outer side of one of the semiconductor layers and on the outer side of the other of the conductive polymer layers of the laminated all-resin heat-utilizing power generating element.

4. The thermal energy generating element according to claim 1, wherein the thermally excited electron density of the semiconductor generating thermally excited electrons and holes in the semiconductor layer is 10 15 / m 3 This method generates electricity by placing the device in an environment where the temperature is above the limit.

5. A thermoelectric power generating device comprising the thermal power generating element according to claim 1 .

6. A thermobattery comprising the thermoelectric power generation element according to claim 1.

7. A thermoelectric power generation module comprising the thermoelectric power generation element according to claim 1 .

8. A step of installing the thermoelectric power generation module according to claim 7 at a heat generation location; and Heating the thermoelectric power generation module with heat to generate electricity; A thermoelectric power generation method comprising:

9. The thermoelectric power generation method according to claim 8 , wherein the heat is geothermal heat or exhaust heat.

Citation Information

Patent Citations

  • Method and device for cutting work with wire saw

    JP1997262826A

  • Inspection method and inspection device for semiconductor ingot and laser processing apparatus

    JP2018147928A

  • Power generation module utilizing heat and thermoelectric power generation device including the same

    JP2021005649A

  • PROCESSING METHOD AND LASER PROCESSING APPARATUS FOR SiC INGOT

    JP2021068819A

  • Si SUBSTRATE GENERATION METHOD

    JP2022025566A