Nonaqueous electrical storage device negative electrode material
The graphite-based negative electrode material with a nitrogen-enriched carbon coating layer addresses high charge transfer resistance and input/output issues by enhancing lithium ion affinity, resulting in improved performance of non-aqueous electricity storage elements.
Patent Information
- Application Number
- JP2023067896
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
AI Technical Summary
Non-aqueous electricity storage elements using conventional composite carbon materials as negative electrode materials exhibit high charge transfer resistance and insufficient input/output performance due to low affinity between amorphous carbon and lithium ions.
A negative electrode material comprising a graphite core coated with a carbon layer containing nitrogen atoms, with a specific nitrogen concentration gradient and a D/G ratio in Raman spectroscopy of 0.16 or more, enhancing electron density and affinity for lithium ions.
The proposed electrode material significantly reduces charge transfer resistance and improves input/output performance by increasing the electronegativity near the surface, thereby improving compatibility with lithium ions.
Smart Images

Figure 2024154192000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode material for a non-aqueous electricity storage element. [Background technology]
[0002] Non-aqueous secondary batteries, such as lithium ion batteries, and non-aqueous capacitors, such as lithium ion capacitors, are widely used in applications such as batteries for electric vehicles, personal computers, and mobile terminals; storage batteries for renewable energy; and power sources for streets.
[0003] Both high-crystalline carbon materials and low-crystalline carbon materials are known as negative electrode materials for non-aqueous storage elements such as non-aqueous secondary batteries and non-aqueous capacitors. Storage elements using high-crystalline carbon materials, such as graphite, as the negative electrode material have low resistance and stable cycle characteristics, but low capacity. On the other hand, storage elements using low-crystalline carbon materials, such as amorphous carbon, as the negative electrode material have high initial capacity, but are significantly deteriorated when charge-discharge cycles are repeated.
[0004] Therefore, a composite carbon material in which a core material made of graphite is coated with a coating layer made of amorphous carbon has been proposed as an anode material having both the advantages of crystalline carbon and amorphous carbon. For example, Patent Document 1 describes composite graphite particles having a core material made of graphite and a carbonaceous layer present on the surface thereof, and exhibiting specific parameters by Raman spectroscopy and wide-angle X-ray diffraction analysis. Patent Document 1 explains that exhibiting certain parameters of Raman spectroscopy and wide-angle X-ray diffraction analysis indicates that the coating layer has low crystallinity, and that using such composite graphite particles as an anode material for a lithium-ion battery improves the cycle characteristics, input / output characteristics, etc. of the lithium-ion battery. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2013 / 084506 Summary of the Invention [Problem to be solved by the invention]
[0006] When a composite carbon material such as that described in Patent Document 1 is used as a negative electrode material, there is a problem that the charge transfer resistance of the obtained nonaqueous electricity storage element is high and the input / output performance is insufficient.
[0007] Therefore, an object of the present invention is to provide a negative electrode material that can provide a nonaqueous electricity storage element having sufficiently low charge transfer resistance and excellent input / output performance. [Means for solving the problem]
[0008] The present invention is as follows.
[0009] Aspect 1: A negative electrode material for a non-aqueous storage element, comprising a core made of graphite and a coating layer containing a carbon material other than graphite and nitrogen atoms, The negative electrode material for a nonaqueous electricity storage element has a D / G ratio of 0.16 or more in a Raman spectroscopic analysis, the coating layer has a nitrogen concentration distribution in its thickness direction, and the nitrogen concentration at the outer surface of the coating layer is higher than the nitrogen concentration inside the coating layer; Negative electrode material. <Embodiment 2> Nitrogen concentration C of the outer surface of the coating layer N0 and the nitrogen concentration C at a point 1 nm from the outer surface in the thickness direction of the coating layer. N1 Difference from C N0 -C N1 is greater than or equal to 0.1 and less than or equal to 3.0. <Embodiment 3> Nitrogen concentration C of the outer surface of the coating layer N0 and the nitrogen concentration C at a point 5 nm from the outer surface in the thickness direction of the coating layer. N5 Difference from C N0 -C N5 is greater than or equal to 0.1 and less than or equal to 5.0. Aspect 4: The negative electrode material according to any one of Aspects 1 to 3, wherein the particle size of the negative electrode material is 1 to 20 μm. Aspect 5: The negative electrode material according to any one of Aspects 1 to 3, wherein the carbon material in the coating layer is a non-crystalline carbon material. Aspect 6: The negative electrode material for a nonaqueous storage element according to any one of Aspects 1 to 3, wherein the negative electrode material for a nonaqueous storage element has a D / G ratio of 0.30 or less in Raman spectroscopic analysis. Aspect 7: A negative electrode of a nonaqueous electricity storage element, comprising the negative electrode material according to any one of aspects 1 to 3. Aspect 8: The negative electrode according to aspect 7, wherein the nonaqueous storage element is a nonaqueous secondary battery or a nonaqueous capacitor. A nonaqueous electricity storage element comprising the negative electrode according to Aspect 8. Aspect 10: The nonaqueous electricity storage element according to Aspect 9, which is a nonaqueous secondary battery or a nonaqueous capacitor. A method for producing the negative electrode material according to any one of Aspects 1 to 3, comprising the steps of: A negative electrode material precursor having a core made of graphite and a coating layer containing a carbon material other than graphite is heated in the presence of a nitrogen source. A method for producing anode materials. Aspect 12: The method for producing a negative electrode material according to aspect 11, wherein the nitrogen source is selected from urea, thiourea, cyanamide, dicyandiamide, guanidine salts, triazine, triazine derivatives, and nitrogen-containing organic polymers. Effect of the Invention
[0010] According to the present invention, there is provided a negative electrode material which can provide a nonaqueous electricity storage element having sufficiently low charge transfer resistance and excellent input / output performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Non-aqueous negative electrode material for energy storage devices> The negative electrode material for a nonaqueous storage element of the present invention is A negative electrode material for a non-aqueous storage element having a core made of graphite and a coating layer containing a carbon material other than graphite and nitrogen atoms, The negative electrode material for a nonaqueous electricity storage element has a D / G ratio of 0.16 or more in a Raman spectroscopic analysis, the coating layer has a nitrogen concentration distribution in its thickness direction, and the nitrogen concentration at the outer surface of the coating layer is higher than the nitrogen concentration inside the coating layer; It is a negative electrode material.
[0012] The present inventors have carried out a detailed study on the reason why, when a composite carbon material in the prior art is used as a negative electrode material, the resulting nonaqueous electricity storage element has high charge transfer resistance and insufficient input / output performance.
[0013] As a result, it was found that in the composite carbon materials of the prior art, the affinity between the amorphous carbon that constitutes the coating layer and lithium ions is low, making it difficult for lithium ions to reach the negative electrode material, resulting in high charge transfer resistance.
[0014] In the present invention, therefore, the affinity between the negative electrode material and lithium ions is improved by arranging nitrogen atoms having high electronegativity near the outer surface of the coating layer of the composite carbon material to increase the electron density of the outer surface of the coating layer. At this time, a nitrogen concentration distribution is provided in the thickness direction of the coating layer, and the nitrogen atoms are concentrated on the outer surface of the coating layer to increase the electron density of the outer surface of the coating layer.
[0015] In addition, the negative electrode material for a nonaqueous storage element of the present invention has a D / G ratio of 0.16 or more in Raman spectroscopy. If the D / G ratio in Raman spectroscopy is in this range, the advantage of high capacity due to the amorphous carbon material in the coating layer can be effectively enjoyed.
[0016] The elements constituting the negative electrode material of the present invention will be described below in order.
[0017] <Core> The core of the negative electrode material of the present invention is graphite. The graphite may be natural graphite or artificial graphite. The natural graphite as the core of the negative electrode material of the present invention may be graphite obtained by processing, for example, flake graphite, lump (scale) graphite, or clay graphite into a spherical shape, and the artificial graphite may be graphite obtained by, for example, heating (graphitizing) petroleum coke in an inert atmosphere at a temperature of about 2,500°C to 3,500°C for 10 minutes to 100 hours.
[0018] The particle size of the core, calculated as the particle size when the cumulative volume fraction in the particle size distribution obtained by a light scattering method using laser light is 50% (D50), may be, for example, 1 μm or more, 3 μm or more, 5 μm or more, 7 μm or more, or 10 μm or more, and may be, for example, 50 μm or less, 40 μm or less, 30 μm or less, 20 μm or less, or 15 μm or less.
[0019] <Coating layer> The coating layer of the negative electrode material of the present invention contains a carbon material and nitrogen atoms.
[0020] The carbon material in the coating layer may be the same as that in the coating layers of composite carbon materials in the prior art, and typically may be an amorphous carbon material.
[0021] In the Raman spectroscopic analysis of the negative electrode material for a non-aqueous storage element of the present invention, a Raman shift of 1,350 cm -1 The peak intensity D of the "D band" near 1,580 cm -1 The ratio of the peak intensity G to that of the "G band" nearby (D / G ratio) is 0.16 or more. The D band is a peak derived from amorphous carbon, and the G band is a peak derived from the sp 2This peak is derived from the planar structure of carbon. Therefore, the larger the D / G ratio in Raman spectroscopy, the thicker the coating layer, and the smaller this value, the thinner the coating layer. The D / G ratio in Raman spectroscopy of the negative electrode material is 0.16 or more. By having a D / G ratio of 0.16 or more, the coating layer becomes sufficiently thick, and the capacity of the obtained nonaqueous storage element can be increased. On the other hand, from the viewpoint of showing stable input / output characteristics without the coating layer becoming excessively thick and therefore without excessively increasing the resistance when lithium ions pass through the coating layer, the D / G ratio may be 0.30 or less.
[0022] In view of the above, the D / G ratio is 0.16 or more, and may be 0.18 or more, 0.20 or more, 0.22 or more, 0.24 or more, or 0.26 or more. Similarly, the D / G ratio may be 0.30 or less, 0.29 or less, 0.25 or less, 0.23 or less, 0.22 or less, or 0.20 or less.
[0023] The coating layer contains nitrogen atoms in addition to the carbon material described above.
[0024] The coating layer in the present invention has a nitrogen concentration distribution in the thickness direction, and is configured so that the nitrogen concentration on the outer surface of the coating layer is higher than the nitrogen concentration inside the coating layer. Such a nitrogen concentration distribution effectively increases the electronegativity near the outer surface of the coating layer, increasing the affinity between the negative electrode material and lithium ions, and reducing the charge transfer resistance.
[0025] Nitrogen concentration on the outer surface of the coating layer C N0 From the viewpoint of imparting an appropriate electronegativity to the negative electrode material, the nitrogen concentration C N0 is the mass ratio of nitrogen atoms to the total mass of nitrogen atoms, carbon atoms, and oxygen atoms, and may be, for example, 0.5 mass% or more, 1.0 mass% or more, 1.5 mass% or more, 2.0 mass% or more, 3.0 mass% or more, or 4.0 mass% or more, and may be, for example, 10.0 mass% or less, 8.0 mass% or less, 6.0 mass% or less, 4.0 mass% or less, 3.0 mass% or less, or 2.0 mass% or less.
[0026] Nitrogen concentration C at a point 1 nm from the outer surface of the coating layer in the thickness direction of the coating layer N1 is C N0 It is small compared to C. N1 is the mass ratio of nitrogen atoms to the total mass of nitrogen atoms, carbon atoms, and oxygen atoms, and may be, for example, 0.3 mass% or more, 0.8 mass% or more, 1.2 mass% or more, 1.5 mass% or more, or 3.0 mass% or more, and may be, for example, 8.0 mass% or less, 6.0 mass% or less, 4.0 mass% or less, 3.0 mass% or less, 2.0 mass% or less, or 1.8 mass% or less.
[0027] Nitrogen concentration C at a point 5 nm from the outer surface of the coating layer in the thickness direction of the coating layer N5 is C N1 It can be smaller than C. N5 is the mass ratio of nitrogen atoms to the total mass of nitrogen atoms, carbon atoms, and oxygen atoms, and may be, for example, 0.2 mass% or more, 0.5 mass% or more, 1.0 mass% or more, 1.2 mass% or more, 1.5 mass% or more, or 2.0 mass% or more, and may be, for example, 5.0 mass% or less, 4.0 mass% or less, 3.0 mass% or less, 2.0 mass% or less, 1.8 mass% or less, or 1.5 mass% or less.
[0028] The coating layer in the present invention has a nitrogen concentration of C N0 and the nitrogen concentration C at a point 1 nm from the outer surface of the coating layer in the thickness direction of the coating layer. N1 Difference from C N0 -C N1 may be 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, or 0.6 or more, and may be 3.0 or less, 2.5 or less, 2.0 or less, 1.5 or less, 1.2 or less, 1.0 or less, or 0.8 or less.
[0029] In addition, the coating layer in the present invention has a nitrogen concentration C N0 and the nitrogen concentration C at a point 5 nm from the outer surface of the coating layer in the thickness direction of the coating layer. N5 Difference from C N0 -C N5may be 0.1 or more, 0.2 or more, 0.3 or more, 0.5 or more, 0.7 or more, 1.0 or more, or 1.2 or more, and may be 5.0 or less, 4.5 or less, 4.0 or less, 3.0 or less, 2.5 or less, 2.0 or less, or 1.5 or less.
[0030] The nitrogen concentration distribution in the thickness direction of the coating layer may be measured by X-ray photoelectron spectroscopy (XPS) using an argon monomer ion gun.
[0031] <Particle size of negative electrode material> The particle size of the negative electrode material of the present invention, as determined as the particle size (D50) at which the cumulative volume fraction in a particle size distribution obtained by a light scattering method using laser light is 50%, may be, for example, 1 μm or more, 2 μm or more, 5 μm or more, 7 μm or more, or 10 μm or more, and may be, for example, 20 μm or less, 18 μm or less, 15 μm or less, 12 μm or less, or 10 μm or less.
[0032] <<Method for producing negative electrode material>> The negative electrode material of the present invention may be produced by any method so long as it has the above-mentioned configuration.
[0033] The negative electrode material of the present invention may be produced, for example, by a method including heating a negative electrode material precursor having a core made of graphite and a coating layer containing a carbon material other than graphite in the presence of a nitrogen source.
[0034] The negative electrode material precursor may be produced, for example, by mixing graphite for the core with a carbon source for forming the coating layer, and then heating the mixture to carbonize the carbon source.
[0035] The graphite core may be appropriately selected depending on the form of the core in the desired negative electrode material. For example, natural graphite or artificial graphite having a particle size of 1 μm or more and 50 μm or less may be used.
[0036] The carbon source may be, for example, isotropic pitch, anisotropic pitch, synthetic resin, natural polymer, etc. The synthetic resin may be selected from, for example, phenolic resin, polyvinyl alcohol resin, polystyrene resin, polyimide resin, etc. The natural polymer may be selected from, for example, sucrose, amylose, alginic acid, etc.
[0037] Here, the thickness of the coating layer can be controlled by appropriately adjusting the ratio of the graphite to the carbon source used. As a non-limiting example, 0.05 parts by mass or more and 1 part by mass or less of the carbon source may be used per 100 parts by mass of graphite.
[0038] The graphite and the carbon source may be mixed by dry mixing or wet mixing. When wet mixing is performed, the solvent used may be removed before the heating in the next step.
[0039] The heating may be carried out, for example, at a temperature of 500° C. or more or 900° C. or more and 2,000° C. or less or 1,500° C. or less for a period of 30 minutes or more or 45 minutes or more and 120 minutes or less or 90 minutes or less. The heating may be carried out in an inert atmosphere.
[0040] After heating, the heated product may be crushed to adjust the particle size to a desired size, for example, from 1 μm to 20 μm.
[0041] The negative electrode material precursor can be produced by the above method. However, a commercially available composite carbon material may be used as the negative electrode material precursor in the present invention. Examples of such commercially available products include "SG-10 coated product" (manufactured by Da Sheng Graphite New Materials Co., Ltd.).
[0042] The negative electrode material precursor is then heated in the presence of a nitrogen source.
[0043] The nitrogen source may be selected from, for example, urea, thiourea, cyanamide, dicyandiamide, guanidine salt, triazine, triazine derivative, nitrogen-containing organic polymer, etc. The guanidine salt may be, for example, guanidine carbonate, guanidine hydrochloride, etc. The triazine derivative may be, for example, melamine, trimethylhexahydrotriazine, 2,4,6-trihydroxy-1,3,5-triazine, etc. The nitrogen-containing organic polymer may be, for example, polyimide, polypyrrole, polyacrylonitrile, polyalkylenepolyamine, etc.
[0044] Nitrogen-containing organic compounds synthesized using the above-listed nitrogen sources as raw materials may also be used as the nitrogen source in the present invention. Examples of such nitrogen-containing organic compounds include melam, melem, melon, graphitic carbon nitride (g-C3N4), melamine resin, and urea resin.
[0045] The thickness of the coating layer can be controlled by appropriately adjusting the ratio of the negative electrode material precursor to the nitrogen source, which varies depending on the type of nitrogen source used.
[0046] When a nitrogen-containing organic polymer is used as a nitrogen source, in order to introduce a sufficient amount of nitrogen, the ratio of the nitrogen source to 100 parts by mass of the negative electrode material precursor is 0.1 parts by mass or more, 0.3 parts by mass or more, 0.5 parts by mass or more, 1.0 parts by mass or more, or 2.0 parts by mass or more. In addition, if an excessive amount of the nitrogen-containing organic polymer is used as a nitrogen source, carbon atoms in the polymer may be deposited on the negative electrode material precursor, resulting in an excessive thickness of the coating layer. To avoid this, the ratio of the nitrogen source to 100 parts by mass of the negative electrode material precursor may be 5.0 parts by mass or less, 4.0 parts by mass or less, 3.5 parts by mass or less, 3.0 parts by mass or less, 2.5 parts by mass or less, or 2.0 parts by mass or less.
[0047] On the other hand, when a low molecular weight compound other than a nitrogen-containing organic polymer is used as a nitrogen source, a part of the nitrogen source may evaporate during the heating process, and the desired amount of nitrogen may not be introduced into the coating layer. In addition, since a part of the low molecular weight compound evaporates during the heating process, even if a relatively large amount of the nitrogen source is used, there is little concern that the thickness of the coating layer will be excessively large. In consideration of these, when a low molecular weight compound is used as a nitrogen source, in order to introduce an appropriate amount of nitrogen, the ratio of the nitrogen source to 100 parts by mass of the negative electrode material precursor may be, for example, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, or 20 parts by mass or more, and may be, for example, 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, or 20 parts by mass or less.
[0048] The negative electrode material precursor and the nitrogen source may be mixed by dry mixing or wet mixing. When wet mixing is performed, the solvent used may be removed before the heating in the next step.
[0049] The heating may be carried out, for example, at a temperature of 500° C. or more or 650° C. or more and 1,500° C. or less or 1,000° C. or less for a period of 30 minutes or more or 45 minutes or more and 120 minutes or less or 90 minutes or less. The heating may be carried out in an inert atmosphere.
[0050] After heating, the heated product may be crushed as necessary to adjust the particle size to a desired size, for example, from 1 μm to 20 μm.
[0051] By the above method, the negative electrode material of the present invention can be obtained.
[0052] <Negative electrode of non-aqueous electricity storage element> According to another aspect of the present invention, there is provided a negative electrode for a non-aqueous storage element, comprising the negative electrode material of the present invention. The negative electrode of the present invention may have the same structure as a known negative electrode, except that the negative electrode material of the present invention is used as a negative electrode active material.
[0053] The negative electrode of the present invention has, for example, a negative electrode current collector and a negative electrode active material layer disposed on one or both sides of the negative electrode current collector, and the negative electrode material of the present invention is used as the negative electrode active material contained in the negative electrode active material layer.
[0054] The negative electrode current collector may be a metal foil having high electrical conductivity, such as an aluminum foil, a copper foil, or a nickel foil.
[0055] The negative electrode active material layer contains the negative electrode material of the present invention, and may further contain, as necessary, for example, a conductive filler, a thickener, a binder, a dispersion stabilizer, and the like.
[0056] <Non-aqueous energy storage element> The negative electrode of the present invention is suitable as a negative electrode for a nonaqueous electricity storage element. Therefore, according to yet another aspect of the present invention, there is provided a nonaqueous electricity storage element comprising the negative electrode of the present invention.
[0057] The nonaqueous storage element of the present invention may be, for example, a nonaqueous secondary battery or a nonaqueous capacitor. The nonaqueous secondary battery may be, for example, a lithium ion battery, and the nonaqueous capacitor may be, for example, a lithium ion capacitor.
[0058] The nonaqueous electricity storage element of the present invention may have the same configuration as a known nonaqueous electricity storage element, except that the negative electrode of the present invention is used as the negative electrode.
[0059] A lithium ion secondary battery may include, for example, the negative electrode of the present invention, as well as a positive electrode, a separator, and a non-aqueous electrolyte solution.
[0060] The positive electrode may have a positive electrode current collector and a positive electrode active material layer disposed on one or both sides of the positive electrode current collector. The positive electrode current collector may be, for example, an aluminum foil. The positive electrode active material layer may contain an appropriate positive electrode active material, such as a transition metal oxide, and may further contain, for example, a conductive filler, a thickener, a binder, a dispersion stabilizer, etc., as necessary. The separator may be, for example, a porous film made of a resin selected from polyolefin, cellulose, aramid resin, etc. The non-aqueous electrolyte may be a non-aqueous solution containing a lithium salt and a non-aqueous solvent. The lithium salt may be, for example, LiPF6, LiBF4, etc., and the non-aqueous solvent may be, for example, selected from a cyclic carbonate and a chain carbonate.
[0061] In the lithium ion secondary battery, the negative electrode, the positive electrode, the separator, and the non-aqueous electrolyte may be entirely enclosed in a suitable exterior body.
[0062] The lithium ion capacitor may have the same configuration as the lithium ion secondary battery, except that a suitable carbon material, for example, activated carbon, is used as the positive electrode active material. EXAMPLES
[0063] Example 1 (1) Anode material precursor The negative electrode precursor used was a commercially available composite carbon material with a core made of graphite particles and a coating layer made of amorphous carbon (manufactured by Dashen Graphite New Materials Co., Ltd., product name "SG-10 coating product"). The average diameter of this composite carbon material was 10.2 μm.
[0064] (2) Manufacturing of anode materials 100 parts by mass of the negative electrode material precursor obtained above and 20 parts by mass of melamine as a nitrogen source were mixed and heated at 800°C for 1 hour in an inert atmosphere to introduce nitrogen atoms into the coating layer of the negative electrode material precursor, thereby obtaining a negative electrode material.
[0065] (3) Analysis of anode materials (i) Measurement of particle size of negative electrode material The particle size of the negative electrode material was determined as the particle size (D50) when the cumulative volume fraction in the particle size distribution obtained by the light scattering method using a laser beam was 50%. As a result, the particle size (D50) of the negative electrode material was 10.2 μm.
[0066] (ii) Raman spectroscopy The negative electrode material was subjected to Raman spectroscopic analysis under the following measurement conditions to examine the D / G ratio, and the D / G ratio of the negative electrode material of Example 1 was found to be 0.19. [Raman spectroscopic analysis measurement conditions] Measurement equipment: Renishaw Plc., inVia Reflex confocal Raman microscope Objective lens magnification: 20x Excitation laser: 532 nm (100 mW) Laser power: 1% Irradiation time: 60 seconds Number of times accumulated: 1
[0067] (iii) Nitrogen concentration distribution in the thickness direction of the coating layer The nitrogen concentration distribution in the thickness direction of the coating layer of the negative electrode material was measured by X-ray photoelectron spectroscopy (XPS) using an argon monomer ion gun under the following measurement conditions. The nitrogen concentration was calculated as the mass ratio (mass%) of N atoms to the total mass of N atoms, C atoms, and O atoms. [XPS measurement conditions] Measuring device: PHI5000 Versa-Probe, manufactured by Ulvac-Phi Inc. Equipment vacuum degree: 1.0×10 -5 Pa or less X-ray source: Monochromated AlKα X-ray output: 25W, 15kV Beam diameter: 100μmφ Measurement element / measurement range: C 1s 278eV~298eV, N 1s 391eV~411eV, O 1s 523eV~543eV Pass Energy: C 1s 23.5 eV, N 1s 187.85 eV, O 1s 117.4eV Energy step interval: C 1s 0.05 eV, N 1s 0.2 eV, O 1s 0.25eV Energy axis correction: C 1s 284.8eV Sample preparation method: Sample powder is fixed on carbon tape Ion gun: Ar monomer ion gun Gas used: PAr (G1) Sputter output: 2kV Raster area: 2mm x 2mm Sputtering rate: 0.14 min / nm @ SiO2 conversion (standard sample ULVAC 100 nm SiO2 / Si) Sputtering time, number of sputters: 0.14 min x 5 times @ SiO2 equivalent 5 nm
[0068] As a result, the nitrogen concentration C N0 is 1.8% by mass, Nitrogen concentration C at a point 1 nm in the thickness direction from the outer surface of the coating layer N1 is 1.4% by mass, Nitrogen concentration C at a point 5 nm in the thickness direction from the outer surface of the coating layer N5 The content was 1.5 mass %.
[0069] Therefore, the difference C N0 -C N1 is 0.4 mass%, and the difference C N0 -C N5 The content was 0.3 mass%.
[0070] (4) Evaluation of anode materials (i) Manufacture of the negative electrode 98.8 parts by mass of the negative electrode material obtained above, 0.5 parts by mass of carboxymethyl cellulose (CMC) as a thickener, and water as a solvent were kneaded together, and 0.7 parts by mass of styrene butadiene rubber (SBR) as a binder was further added and kneaded to obtain a negative electrode slurry.
[0071] The obtained negative electrode slurry was applied onto a copper foil, dried at 70° C., and then roll-pressed to produce a negative electrode. The negative electrode weight (amount of coating on the copper foil) was 3.8 mg / cm. 2 It was.
[0072] (ii) Manufacturing of cells for battery evaluation The negative electrode obtained above was used as the working electrode, with a diameter of 15.96 mm (area of 2.00 cm). 2 ) punched into a circular shape; as counter electrode, lithium metal foil; The electrolyte was a 1.1 mol / L LiPF6 solution (solvent: ethylene carbonate: dimethyl carbonate: ethyl methyl carbonate (30:40:30 (volume%) mixed solvent); As a separator, a porous polypropylene membrane; As a battery evaluation container, a three-electrode test cell manufactured by Toyo Systems Co., Ltd. was used; Each of these was used to manufacture a cell for battery evaluation.
[0073] (iii) Measurement of charge transfer resistance The battery evaluation cell obtained above was subjected to pretreatment and measurement of charge transfer resistance at 25° C. according to the following procedures.
[0074] <Pretreatment> As a pretreatment, two discharge-charge cycles consisting of the first CCCV discharge and CC charge described below were performed, and then a second CCCV discharge was performed. First CCCV discharge: Discharge the battery at a fixed current rate of 0.2C until the voltage reached 0.01V. After reaching 0.01V, discharge the battery at a fixed voltage of 0.01V until the current reached 1 / 20C. CC charging: The current was fixed at 0.2C rate and the voltage was charged to 1.5V. Second CCCV discharge: Discharge the battery at a fixed current rate of 0.2C until the voltage reached 0.1V. After reaching 0.1V, discharge the battery at a fixed voltage of 0.1V until the current reached 1 / 20C.
[0075] <measurement> For the pretreated battery evaluation cells, constant current type AC impedance measurements were performed under conditions of a starting frequency of 100 kHz, an ending frequency of 0.1 Hz, a set current of 0 A, and an amplitude of 0.3 mA, and the charge transfer resistance was read from the diameter of the semicircle in the Cole-Cole plot.
[0076] The charge transfer resistance is shown in Table 1 as a relative value, with the charge transfer resistance value of the battery evaluation cell of Comparative Example 1 described below taken as 100%.
[0077] Example 2 and Comparative Examples 1 and 2 In "(2) Production of negative electrode material", the type and amount of nitrogen source were changed as shown in Table 1, but other than that, negative electrode materials were produced in the same manner as in Example 1, and battery evaluation cells were produced and evaluated using the negative electrode materials. In Comparative Example 1, "(2) Production of negative electrode material" was not performed, and the negative electrode material precursor described in "(1) Negative electrode material precursor" was used as it is as the negative electrode material. In Example 2 and Comparative Example 2, the material after heating in an inert atmosphere in "(2) Production of negative electrode material" was crushed and then used as the negative electrode material.
[0078] The results are shown in Table 1.
[0079] Comparative Examples 3 and 4 As the negative electrode material precursor, graphite particles (manufactured by Da Sheng Graphite New Materials Co., Ltd., product name "SG-10", particle size 10.2 μm) were used as the negative electrode material precursor, and the type and amount of nitrogen source used were as shown in Table 1, respectively. Except for this, "(2) Production of negative electrode material" was carried out in the same manner as in Example 1 to prepare the negative electrode materials of Comparative Examples 3 and 4. Except for using the obtained negative electrode material, a battery evaluation cell was produced and evaluated in the same manner as in Example 1. In Comparative Example 4, the material after heating under an inert atmosphere in "(2) Production of negative electrode material" was crushed and then used as the negative electrode material. The results are shown in Table 1.
[0080] [Table 1]
[0081] In the "Nitrogen source" type column of Table 1, "PAN" stands for polyacrylonitrile.
[0082] From Table 1 above, the following was found.
[0083] The battery manufactured using the anode material of Comparative Example 3, in which the D / G ratio in Raman spectroscopy was less than 0.16, had a higher charge transfer resistance than the battery of the prior art of Comparative Example 1. In addition, the battery manufactured using the anode material of Comparative Example 4, in which the D / G ratio was 0.16 or more but the nitrogen concentration on the outer surface of the coating layer was not higher than the nitrogen concentration inside the coating layer, also had a higher charge transfer resistance than the battery of Comparative Example 1.
[0084] In contrast, the batteries manufactured using the negative electrode materials of Examples 1 and 2, in which the D / G ratio was 0.16 or more and the nitrogen concentration on the outer surface of the coating layer was higher than the nitrogen concentration inside the coating layer, had a smaller charge transfer resistance than the battery of Comparative Example 1.
[0085] From the above, it was verified that the charge transfer resistance is reduced in an electricity storage device manufactured using the negative electrode material of the present invention.
Claims
1. A negative electrode material for a non-aqueous storage element having a core made of graphite and a coating layer containing a carbon material other than graphite and nitrogen atoms, The negative electrode material for a nonaqueous storage element has a D / G ratio of 0.16 or more in a Raman spectroscopic analysis, the coating layer has a nitrogen concentration distribution in its thickness direction, and the nitrogen concentration at the outer surface of the coating layer is higher than the nitrogen concentration inside the coating layer; Negative electrode material.
2. The nitrogen concentration C of the outer surface of the coating layer N0 and the nitrogen concentration C at a point 1 nm from the outer surface in the thickness direction of the coating layer N1 Difference C N0 -C N1 is 0.1 or more and 3.0 or less, The negative electrode material according to claim 1 .
3. The nitrogen concentration C of the outer surface of the coating layer N0 and the nitrogen concentration C at a point 5 nm from the outer surface in the thickness direction of the coating layer N5 Difference C N0 -C N5 is 0.1 or more and 5.0 or less, The negative electrode material according to claim 1 .
4. The negative electrode material according to any one of claims 1 to 3, wherein the particle size of the negative electrode material is 1 to 20 µm.
5. The negative electrode material according to any one of claims 1 to 3, wherein the carbon material in the coating layer is an amorphous carbon material.
6. The negative electrode material according to any one of claims 1 to 3, wherein the D / G ratio measured by Raman spectroscopic analysis of the negative electrode material for non-aqueous storage elements is 0.30 or less.
7. A negative electrode for a non-aqueous electricity storage element, comprising the negative electrode material according to any one of claims 1 to 3.
8. The negative electrode according to claim 7 , wherein the nonaqueous storage element is a nonaqueous secondary battery or a nonaqueous capacitor.
9. A non-aqueous electricity storage element comprising the negative electrode according to claim 8 .
10. The nonaqueous electricity storage element according to claim 9 , which is a nonaqueous secondary battery or a nonaqueous capacitor.
11. A method for producing the negative electrode material according to any one of claims 1 to 3, comprising the steps of: A negative electrode material precursor having a core made of graphite and a coating layer containing a carbon material other than graphite is heated in the presence of a nitrogen source. A method for producing anode materials.
12. The method for producing a negative electrode material according to claim 11, wherein the nitrogen source is selected from urea, thiourea, cyanamide, dicyandiamide, guanidine salts, triazines, triazine derivatives, and nitrogen-containing organic polymers.
Citation Information
Patent Citations
Composite graphite particles and use of same
WO2013084506A1