Preparation method of copper green rust pigment that can replace hayeob pigment in traditional dancheong

A method using copper powder and a caustic agent to produce a patina pigment replicates Hayeob's color and composition, addressing the lack of effective production methods for traditional green pigments, ensuring stability and efficiency in cultural heritage applications.

JP2024154353AActive Publication Date: 2024-10-30NAT RESERCH INSTITUE OF CULTURAL PROPERTIES
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023139590
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2023-08-30
Publication Date
2024-10-30
Estimated Expiration
2043-08-30

AI Technical Summary

Technical Problem

There is a lack of detailed methods for producing traditional green pigments like Hayeob, which are used in cultural heritage sites, and existing methods do not accurately replicate their composition or characteristics.

Method used

A method involving the use of copper powder or copper alloys mixed with a caustic agent containing sodium chloride and ammonium chloride to corrode the copper, followed by grinding, wet fractionation, and purification steps to produce a patina pigment that mimics the Hayeob color and composition.

Benefits of technology

The method produces a green pigment that closely resembles Hayeob in terms of color and composition, suitable for traditional Dancheong applications, and enhances stability and efficiency by removing residual caustic agents, improving color uniformity and saturation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154353000005
    Figure 2024154353000005
  • Figure 2024154353000006
    Figure 2024154353000006
  • Figure 2024154353000007
    Figure 2024154353000007
Patent Text Reader

Abstract

To provide a preparation method for a copper green rust pigment, particularly a preparation method for a copper green rust pigment that can replace the traditional Dancheong Hayeob pigment.SOLUTION: A preparation method for a copper green rust pigment comprises the following steps: a step of preparing a copper powder comprising at least one of copper; and a copper alloy comprising copper and at least one of tin (Sn), zinc (Zn), and lead (Pb); and a step of corroding the copper powder by mixing the copper powder with a corrosive agent containing sodium chloride and ammonium chloride. The corrosive agent includes 75 to 90 wt.% of the sodium chloride and 10 to 25 wt.% of the ammonium chloride based on the total weight.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] 2. Background of the Invention 1. Field of the Invention The present invention relates to a method for preparing a patina pigment. 2. Description of Related Art Since ancient times, humans have used pigments of various colors to express beauty in artworks, such as paintings, murals, or architectural Dancheong (traditional multi-colored painting on wooden buildings). Traditionally used pigments are mainly made using natural soil and rocks, but artificial pigments synthetically made from metals, such as mercury, lead, and copper, have also been reported as major coloring materials.

[0002] Traditional artificial pigments include Eunju, Yeonbak, Yeondan, Dongrok, and Hoecheong, among which Dangrok is known as a green pigment mainly composed of copper oxide. In addition, a traditional green pigment is Hayeob, a green pigment used not only in traditional Dancheong of cultural heritage but also in gwaebul (large Buddhist hanging scrolls), temple murals, and paintings, and mentioned in ancient Korean literature records. However, it is only known in literature as a dark green color, there is no record identifying its composition or characteristics, and it is not clear whether it is a natural pigment recovered from nature or an artificial pigment synthesized and fabricated. However, the results of pigment analysis studies conducted on domestic painting cultural heritage suggest that Hayeob pigment is mainly composed of copper (Cu) and (Cl) as the main components, and particle morphology analysis indicates that it is probably an artificially synthesized Dangrok pigment.

[0003] In ancient literature, such as Cheon-Gong-Gae-Mul (Tiangong Kaiwu), Boncho-Gang-Mok (Compendium of Materia Medica), and Imwon-Gyeongje-Ji (Annals of Forestry Economics), it is possible to confirm the method of producing Dongrok (malachite green pigment) by reacting copper plates with vinegar. Kang et al. (2020) conducted research on producing and characterizing malachite green pigment by applying an acid corrosion method using acetic acid to corrode copper plates. According to the investigation results, the copper produced by the acid etching method exhibits a polygonal particle shape and has a copper acetate structure or a copper carbonate structure. In addition, 2· hoganite [Cu(CH3COO)

[0004] H2O], having a monoclinic crystal structure as a secondary copper-based product, was identified as the main constituent inorganic substance. In the research on pigment analysis of painting cultural heritage in Korea, only malachite [Cu2CO3(OH)2], atacamite [Cu2Cl(OH)3], and botallackite [Cu2Cl(OH)3] were reported, while hoganite was not reported at all, suggesting the possibility of a pigment different from those used in painting cultural heritage. On the other hand, according to the results of the investigation of ancient literature records, the production method of Dangrok (malachite green) includes not only the acid corrosion method using vinegar to corrode copper plates but also the chloride corrosion method using chlorine (Cl) compounds or a combination of vinegar and chlorine compounds. This can be found in ancient literature. Shinsu Boncho (Newly Revised Materia Medica) describes a method of mixing copper powder with corrosion agents (sodium chloride, ammonium chloride) and then allowing it to corrode naturally, but there is no detailed description. Furthermore, since there are not many literature records on the chloride corrosion method, further investigation is needed on the production method for replicating Dangrok (malachite green) (see Non-Patent Document 1). 2·

[0004] As a result, the inventors investigated old literature records and research data to produce a Dongrok pigment that can replace the traditional Dancheong Hayeob pigment, sought out the conditions necessary to guarantee the manufacturing technology based on this, and manufactured the Dongrok pigment by applying the guaranteed manufacturing technology, thereby completing the present invention. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Oh, Joonsuk; Lee, Saerom; Hwang, Minyoung; 2020, Review of Copper Trihydroxychloride, a Green Pigment Composed of Copper and Chlorine. MUNHWAJAE, 53(2), pp. 64~87. Summary of the Invention

[0006] SUMMARY OF THE PRESENT APPLICATION It is an object of the present invention to provide a method for preparing a patina pigment. In order to achieve the above object, in one aspect of the present invention, the present invention provides a method for preparing a patina pigment that can replace the traditional Dancheong Hyeob pigment, comprising the steps of: Preparing a copper powder comprising at least one of copper; and a copper alloy comprising copper and at least one of tin (Sn), zinc (Zn), and lead (Pb); and Corroding the copper powder by mixing the copper powder with a corrosive agent containing sodium chloride and ammonium chloride, where the corrosive agent comprises 75-95 wt. % sodium chloride and 10-25 wt. % ammonium chloride based on the total weight. The method further comprises:

[0007] In this case, the caustic agent may include 86 to 90% by weight of sodium chloride and 10 to 14% by weight of ammonium chloride, based on the total weight. In the etching step, the copper powder and the etching agent may be mixed in a weight ratio of 1:2 or more. Corrosion may be performed by artificial corrosion using a corrosion tester.

[0008] The method for preparing the patina pigment further comprises the steps of grinding and wet fractionating the corrosion product prepared in the corrosion step. The method for preparing the patina pigment further comprises removing residual caustic by mixing the milled and wet fractionated powder with distilled water and removing the supernatant. The method for preparing the patina pigment further includes purifying the powder from which residual caustic agents have been removed.

[0009] In another aspect of the present invention, the present invention provides a green-blue pigment prepared using the above-described preparation method. The verdigris pigment can be a green pigment for traditional coloring.

[0010] Beneficial Effects The present invention has the significant advantage of providing a green-blue pigment that can replace Hayeob, a traditional green pigment that has been widely used in various pictorial cultural heritages, such as Dancheong, Buddhist paintings, temple murals, and portraits of the Joseon Dynast. The preparation method of the present invention can be extended and applied to various painting cultural heritages, and also contribute greatly to the continuation of traditional techniques by providing a springboard for research into alternative pigments to expensive natural pigments required both at home and abroad. [Brief description of the drawings]

[0011] BRIEF DESCRIPTION OF THE DRAWINGS [Figure 1] FIG. 1 is a series of photographs showing the results of observing the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT). [Diagram 2] FIG. 2 is a series of photographs showing the results of observing the colors of pigments prepared by naturally corroding the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT). [Diagram 3] FIG. 3 is a series of photographs showing the results of observing the pigment color of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT) before they were artificially corroded by mixing them with a corroding agent. [Figure 4] FIG. 4 is a series of photographs showing the results of observing the pigment color after the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT) were artificially corroded by mixing them with a corrosive agent.

[0012] [Figure 5A] FIG. 5A is a series of graphs showing the results of evaluating the weight change over the period of artificial corrosion of the copper powders CU of Preparation Examples 1 to 5. [Figure 5B] FIG. 5B is a series of graphs showing the results of evaluating the weight change over the period of artificial corrosion of the copper powders CS of Preparation Examples 1 to 5. [Figure 5C] FIG. 5C is a series of graphs showing the results of evaluating the weight change over the period of artificial corrosion of the copper powders CZS of Preparation Examples 1 to 5. [Figure 5D] FIG. 5D is a series of graphs showing the results of evaluating the weight change over the period of artificial corrosion of the copper powders CP of Preparation Examples 1 to 5. [Figure 5E] FIG. 5E is a series of graphs showing the results of evaluating the weight change over the period of artificial corrosion of the copper powders CT of Preparation Examples 1 to 5.

[0013] [Figure 6] 6 to 10 are photographs showing the results of observing the colors of pigments prepared by varying the artificial corrosion periods of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT). [Figure 7]6 to 10 are photographs showing the results of observing the colors of pigments prepared by varying the artificial corrosion periods of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT). [Figure 8] 6 to 10 are photographs showing the results of observing the colors of pigments prepared by varying the artificial corrosion periods of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT). [Figure 9] 6 to 10 are photographs showing the results of observing the colors of pigments prepared by varying the artificial corrosion periods of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT). [Figure 10] 6 to 10 are photographs showing the results of observing the colors of pigments prepared by varying the artificial corrosion periods of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT).

[0014] [Figure 11] FIG. 11 is a series of photographs showing the results of observing the colors of pigments prepared by artificial corrosion of copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1 to 5, where the ratios of sodium chloride and ammonium chloride in the corrosion agent are 0:1, 1:2, 1:1, 2:1, and 1:0. [Figure 12] FIG. 12 is a series of photographs showing the results of observing the color of pigments prepared by artificial corrosion of copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1 to 5, where the ratios of sodium chloride and ammonium chloride in the corrosion agent are 3:1, 4:1, 9:1, and 19:1. [Figure 13] FIG. 13 is a series of photographs showing the results of observing the color of pigments prepared by artificial corrosion of copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1 to 5, where the ratio of sodium chloride and ammonium chloride in the corrosion agent is 19:1.

[0015] [Figure 14A]FIG. 14A is a graph showing the results of measuring the concentration of chloride ions following a wet sieving process in the method for preparing a green-blue pigment of the present invention. [Figure 14B] FIG. 14B is a graph showing the results of measuring the reduction rate of chloride ions following a wet sieving process in the method for preparing a patina pigment of the present invention. [Figure 15A] FIG. 15A is a series of graphs showing the results of evaluating the concentration of chloride ions according to elution time in the dilution process in the method for preparing a green-blue pigment of the present invention. [Figure 15B] FIG. 15B is a series of graphs showing the results of evaluating the rate of increase in chloride ions according to elution time in the dilution process in the method for preparing a green-blue pigment of the present invention.

[0016] [Figure 16A] FIG. 16A is a graph showing the results of evaluating the removal rate of residual corrosion for a pigment having a particle size of 75 to 100 μm in the dilution process in the method for preparing a patina pigment of the present invention. [Figure 16B] FIG. 16B is a graph showing the results of evaluating the removal rate of residual corrosion for pigments having particle sizes of 45 to 75 μm in the dilution process in the method for preparing the patina pigment of the present invention. [Figure 16C] FIG. 16C is a graph showing the results of evaluating the removal rate of residual corrosion for pigments having particle sizes of 0 to 34 μm in the dilution process in the method for preparing the patina pigment of the present invention.

[0017] [Figure 17] FIG. 17 is a series of photographs showing a comparison of pigment color before and after the refining process in the method for preparing the patina pigment of the present invention. [Figure 18] FIG. 18 is a diagram showing a process chart of a method for preparing a patina pigment of the present invention. [Figure 19]FIG. 19 is a series of photographs showing a comparison of the color of pigments prepared by varying the ratio of sodium chloride and ammonium chloride in the caustic when the pigments are prepared by carrying out the method for preparing a patina pigment of the present invention according to the process chart of FIG. [Figure 20] FIG. 20 is a series of graphs showing the results of evaluating the colors of FIG. 19 in comparison to the colors of Hayeob.

[0018] [Figure 21] FIG. 21 is a series of photographs showing green pigments prepared by the method of preparing a patina pigment of the present invention. [Figure 22] FIG. 22 is a graph showing the yield of green pigment prepared by the method for preparing a patina pigment of the present invention. [Figure 23A] FIG. 23A is a series of graphs showing the chromaticity of a medium size green pigment prepared by the method of preparing a patina pigment of the present invention. [Figure 23B] FIG. 23B is a series of graphs showing the chromaticity of a small size green pigment prepared by the method for preparing a patina pigment of the present invention. [Figure 24] FIG. 24 is a series of graphs showing particle size distribution of a green pigment prepared by the method of preparing a patina pigment of the present invention.

[0019] [Diagram 25] FIG. 25 is a series of photographs showing the results of observing a green pigment prepared by the method of preparing a patina pigment of the present invention using a magnification microscope. [Figure 26] FIG. 26 is a series of photographs showing the results of observing a green pigment prepared by the method for preparing a patina pigment of the present invention using a scanning electron microscope (SEM). [Figure 27] FIG. 27 is a graph showing the results of evaluating the oil absorption of a green pigment prepared by the method for preparing a patina pigment of the present invention. [Figure 28] FIG. 28 is a graph showing the results of X-ray fluorescence analysis using a green pigment prepared by the method for preparing a patina pigment of the present invention. [Figure 29] FIG. 29 is a graph showing the results of an X-ray diffraction analysis using a green pigment prepared by the method for preparing a patina pigment of the present invention.

[0020] [Diagram 30] FIG. 30 is a graph showing the results of calculating the color difference (ΔE) according to the accumulated amount of UV irradiation on the pigment to evaluate the stability of the green pigment prepared by the method for preparing a patina pigment of the present invention. [Diagram 31] FIG. 31 is a series of photographs showing a comparison of color before and after accelerated weathering tests to evaluate the stability of a green pigment prepared by the method for preparing a patina pigment of the present invention. [Diagram 32] FIG. 32 is a graph showing the results of comparative evaluation of the chromaticity of the green pigment prepared by the method for preparing a patina pigment of the present invention before and after aging with the chromaticity of the traditional Dancheong Hayeob pigment measured at a cultural heritage site.

[0021] Description of the Preferred Embodiments Below, preferred embodiments of the present invention will be described. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. It is well understood by those skilled in the art with average knowledge in this field that the embodiments of the present invention are given to more precisely describe the present invention. In addition, throughout this specification, the "comprise" of an element does not exclude other elements, but may include other elements, unless otherwise specifically specified.

[0022] In one aspect of the present invention, the present invention provides a method for preparing a patina pigment that can replace the traditional Dancheong Hyeob pigment, comprising the steps of: Preparing a copper powder comprising at least one of copper; and a copper alloy comprising copper and at least one of tin (Sn), zinc (Zn), and lead (Pb); and Corroding the copper powder by mixing the copper powder with a corrosive agent containing sodium chloride and ammonium chloride, where the corrosive agent comprises 75-95 wt. % sodium chloride and 10-25 wt. % ammonium chloride based on the total weight. The method further comprises:

[0023] Hereinafter, the preparation method of the patina pigment according to the embodiment will be described in greater detail. A method for preparing a patina pigment according to an embodiment is a method for making a patina pigment using a traditional chlorine etch method. In a method for preparing a patina pigment according to an embodiment, a step is carried out of preparing at least one copper powder of copper; and copper alloys including copper and at least one of tin (Sn), zinc (Zn), and lead (Pb). In this case, the copper powder may be pure copper or a copper alloy containing copper and at least one of tin (Sn), zinc (Zn), and lead (Pb).

[0024] For example, the copper alloy may be an alloy of copper and tin (Sn) and include 70-80% by weight of copper (Cu) and 20-30% by weight of tin (Sn). In addition, the copper alloy may be an alloy of copper (Cu) and zinc (Zn) and include 75-85% by weight of copper (Cu) and 25-35% by weight of zinc (Zn). In addition, the copper alloy may be an alloy of copper (Cu), tin (Sn) and zinc (Zn) and include 75-85% by weight of copper (Cu) and 5-15% by weight of each of tin (Sn) and zinc (Zn). Additionally, the copper alloy may be an alloy of copper (Cu), tin (Sn), zinc (Zn) and lead (Pb) and may include 80-90% by weight copper (Cu) and 3-7% by weight each of tin (Sn), zinc (Zn), and lead (Pb).

[0025] Next, in the method for preparing a patina pigment according to the embodiment, a step of corroding the copper powder by mixing the copper powder with a corrosive agent containing sodium chloride and ammonium chloride is carried out. A method for preparing a patina pigment according to an embodiment is a method for producing a patina pigment, Dangrok, by corroding copper powder using a chlorine corroding method that uses a chlorine compound as a corroding agent. The caustic agent contains sodium chloride and ammonium chloride, and is characterized in that it contains 75 to 90% by weight of sodium chloride and 10 to 25% by weight of ammonium chloride based on the total weight.

[0026] This is because the caustic is used to produce a green-blue pigment having the color Hayeob. When copper powder is causticized using a caustic containing sodium chloride and ammonium chloride, the greenness of the produced pigment increases with increasing sodium chloride content. When sodium chloride is included at less than 75% by weight and ammonium chloride is included at more than 25% by weight, the blueness of the prepared pigment increases, resulting in a problem of not showing green color. On the other hand, when sodium chloride is included at more than 90% by weight and more than 95% by weight, and ammonium chloride is included at less than 10% by weight and less than 5% by weight, there is a problem of the copper powder not being properly causticized.

[0027] Consequently, to produce a patina pigment having a similar or identical green color to the color of Hayeob, it is preferred to include 75-90% by weight sodium chloride and 10-25% by weight ammonium chloride, based on the total weight of the caustic. It may be more preferred to include 86-90% by weight sodium chloride and 10-14% by weight ammonium chloride, based on the total weight of the caustic. In the step of corroding the copper powder, the copper powder and the corroding agent are preferably mixed in a weight ratio of 1:2 or more, and more preferably mixed in a weight ratio of 1:2 to 1:4 or 1:2 to 1:3.

[0028] This is to improve the corrosion rate and subsequent removal efficiency of the corrosive agent by the corrosive agent.If the corrosive agent is included in an amount less than the amount of copper powder, the production time for the pigment may be too long, or the copper powder may not be corroded properly, because the corrosion rate by the corrosive agent is slow.If the corrosive agent is included in an amount more than three times the amount of copper powder, the corrosive agent remaining after the completion of corrosion is large, and therefore a large amount of energy may be consumed in the additional process to remove the corrosive agent.

[0029] At this time, corrosion may be carried out naturally in the air, but from the viewpoint of corrosion efficiency, it is preferable to carry out artificial corrosion using a corrosion tester. For example, in the etching step, copper powder and the etching agent may be mixed in a weight ratio of 1:2 and may be etched by artificial etching method for a total of 72 hours (9 cycles of 8 hours each).

[0030] The method for preparing a patina pigment according to an embodiment of the present invention may further comprise the steps of grinding and wet fractionating the corrosion product prepared in the corroding step. Grinding is performed to improve the color uniformity of the produced pigment by reducing the particle size of the corrosion products to 100 μm or less. The grinding can be carried out using any method, so long as the method is capable of grinding the powder, and can be carried out, for example, using a mortal mill, without limitation.

[0031] In addition, fractionation is performed to classify the powder ground to 100 μm or less based on particle size, which can be, for example, classified into three groups: 45 μm or less, 45 μm to 75 μm, and 75 μm to 100 μm. Fractionation is preferably a wet fractionation, and may be carried out preferably by a wet sieving method using distilled water, through which it has the advantage of classifying the pigments by particle size and at the same time removing residual caustic agents.

[0032] In addition, the method of preparing a patina pigment according to an embodiment of the present invention may further include removing residual caustic agents by mixing the milled and wet fractionated powder with distilled water and removing the supernatant. This step is to reduce the content of residual caustic agents in the pigment prepared by grinding and wet fractionation to 10 ppm or less. By removing the residual caustic agents in the pigment through the above steps, the stability of the pigment can be further improved by preventing further corrosion caused by the residual caustic agents. As an example, the above steps can be carried out by mixing the target pigment with distilled water, allowing it to settle, and then removing the supernatant.

[0033] Additionally, the method of preparing a patina pigment according to an embodiment of the present invention may further include purifying the powder from which residual caustic agents have been removed. During the process of making the pigment, fine powders of white, grey or brown may be produced in the grinding step, which float on the surface during application and may be less than green in colour. Consequently, the refining step is a step for removing fines in the pigment, specifically fines less than 5 μm.

[0034] The refining step may be carried out on the pigment powder having a small particle size which is classified in the fractionating step, and in particular may be carried out by an elutriation method. At this time, the elutriation method is a method in which the pigment is mixed with distilled water, and then it is left to stand and the supernatant of the distilled water is removed to remove the fine powder present in the supernatant. As an example, the purification process according to the elutriation method can be carried out separately in the first and second stages. The first stage is carried out by placing the pigment in a 600 ml beaker filled with distilled water, mixing it, leaving it for 15 minutes, and removing the supernatant except for the precipitated particles. The second stage can be carried out by thoroughly mixing the decanted supernatant, leaving it for 30 minutes, and then removing the supernatant except for the precipitate. After this, the purified pigment can be obtained by drying the precipitate at 60° C. for 24 hours using a desiccator.

[0035] In another aspect of the present invention, the present invention provides a green-blue pigment prepared using the above-described preparation method. Verdigris pigment is the green pigment for traditional Dancheong coloring. The pigments have the advantage of being able to substitute for Hayeob pigments, as they are similar or identical in terms of color, physical properties and components to the traditional Dancheong Hayeob pigments analyzed in actual cultural heritage sites.

[0036] Hereinafter, the present invention will be described in detail by the following examples and experimental examples. However, the following examples and experimental examples are only intended to illustrate the present invention, and the content of the present invention is not limited thereto.

[0037] <Material> Among the methods for producing patina pigments confirmed through old literature records, the materials used in the chlorine corrosion method in which copper powder is reacted with a chlorine compound are copper powder and a corrosive agent such as sodium chloride and ammonium chloride. Although copper powder is presented as the main material in the literature, there are not many documents related to the chlorine corrosion method, and considering the difficulty of producing copper powder, copper plate can be used as a material for investigation in the production method together with copper powder.

[0038] (1)Copper powder On the other hand, copper utensils commonly used in daily life are likely to have been used as a source of copper for the manufacture of patina pigments in the past. Copper utensils commonly used after the Three Kingdoms period are made from bronze or brass, which are representative copper alloys. Bronze is composed of copper (Cu), tin (Sn) and lead (Pb), while brass is composed of copper (Cu) and zinc (Zn). Bronze and brass were widely used in daily utensils, such as vessels and spoons, as well as in utensils used in ancestral ceremonies and decorative items, and the proportions of the main components varied depending on the purpose of use, the manufacturing method, and the demand and supply of materials.

[0039] The composition ratio of the main components of the copper powder used to produce the patina pigment with Hayeob color was selected based on the analysis results of the bronze vessels, Bangjja items, and Sangpyeong Tongbo among the excavated relics, as well as the analysis results of the pigments of the pictorial cultural heritage. The copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1 to 5 were prepared by producing pure copper or copper alloys in the ratios shown in Table 1 below through a domestic manufacturer. The prepared copper powders are shown in Figure 1.

[0040] [Table 1]

[0041] (2) Corrosive agents According to the literature records, Kwangmyeong salt and Nyosa were used as corroding agents to corrode copper powder. Kwangmyeong salt is an inorganic salt of a halide compound, and its main component is sodium chloride (NaCl), while Nyosa is a natural ammonium chloride (NH4Cl) found in volcano or hot spring areas. To fabricate a patina pigment with Hayeob color by applying the chlorine corrosion method according to an embodiment of the present invention, 99.5% sodium chloride (SAMCHUN, Korea) and 99.0% ammonium chloride (SAMCHUN, Korea) were purchased and used from a domestic company. At this time, sodium chloride and ammonium chloride were mixed in the mixing ratio shown in Tables 2 and 3 below to prepare the corrosive agent.

[0042] [Table 2]

[0043] [Table 3]

[0044] <Experimental Example 1> Preparation of pigments by natural corrosion The pigment was prepared by mixing the corroding agent and copper powder in a weight ratio of 2:1, and then naturally corroding it, and the color during the natural corroding process was confirmed by the following method. The results are shown in Table 2. - Pigment preparation method: The caustic agent of Preparation Example 8 was mixed with each of the copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1 to 5 in an amount of 200% by weight based on the weight of the copper powder, and then exposed to air at room temperature for 20 days to prepare a pigment.

[0045] FIG. 2 is a series of photographs showing the color of the copper powder for 0, 1, 3, 6, 10, 16, and 21 days after natural corrosion of a mixture obtained by mixing each of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT) with the corrosive agent of Preparation Example 8 (NA11). As shown in Figure 2, after 3 days, regardless of the type of copper powder, the color of all the copper powders changed completely due to corrosion, and after 21 days, it was visually confirmed that the copper powders were completely corroded. The completely corroded pigments were blue and did not show the green color of Hayeob.

[0046] <Experimental Example 2> Preparation of pigments by artificial corrosion The pigment was prepared by mixing the corroding agent and copper powder in a weight ratio of 2:1, and then artificially corroding it according to the following method, and the color during the artificial corroding process was confirmed. The results are shown in Figures 3 and 4. - Pigment preparation method: Each of the corrosive agents of Preparation Examples 6-10 (NA10, NA01, NA11, NA21, and NA12) was mixed with each of the copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1-5 in an amount of 200% by weight based on the weight of the copper powder, and the mixture was artificially corroded according to KS Standard D ISO 14993 (Corrosion of metals and alloys - Accelerated test involving cyclic exposure to salt mist, dry and wet conditions), in which distilled water was sprayed in the spraying process during the corrosion tester operation, and a total of three cycles (24 hours, one day) with one cycle of 8 hours were performed to prepare the pigment.

[0047] FIG. 3 is a series of photographs showing the color of the copper powder and corroding agent mixture before artificial corrosion, and FIG. 4 is a series of photographs showing the color one day after artificial corrosion. As shown in Figures 3 and 4, it was found that as a result of artificial etching, generally green or blue etching products were produced, except for the pigments produced by artificial etching by applying the etching agent of Preparation Example 6 (NA10). In the case of natural corrosion, corrosion was completed after 21 days (see Experimental Example 1), whereas in the case of artificial corrosion, corrosion was confirmed to be completed in one day. From the above results, it can be concluded that the method using artificial corrosion is more suitable for the production of patina pigments in terms of labor time efficiency.

[0048] <Experimental Example 3> Evaluation of corrosion period In order to set a suitable corrosion period for producing Dongrok, a green-blue pigment with Hayeob color, by artificial corrosion using a corrosion tester, each of the corrosion agents of Preparation Examples 6 to 10 (NA10, NA01, NA11, NA21, and NA12) was mixed with each of the copper powders (CU, CS, CZ, CP, and CT) and then artificially corroded in the same manner as in Experimental Example 2. A total of 11 cycles of artificial corrosion were performed for each of them, and the weight change of the copper powder according to the corrosion period was analyzed, and the results are shown in Figures 5A to 5E. In addition, the color change was analyzed, and the results are shown in Figures 6 to 10.

[0049] 5A-5E are a series of graphs showing the weight changes according to the artificial corrosion period of the copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1-5. As a result of the analysis, in most conditions, the weight increased rapidly at the beginning of corrosion and remained constant or rather tended to decrease in weight after about 5 cycles. 6 to 10 are photographs showing the colors of the copper powders of Preparation Examples 1 to 5 (CU, CS, CZ, CP, and CT) subjected to an artificial corrosion period.

[0050] As shown in Figure 6, in the case of copper powder (CU) of Preparation Example 1, there was a tendency for the amount of green products to increase overall as the artificial corrosion progressed. When the corrosion agent of Preparation Example 6 was used, the sample turned black and the state was maintained, resulting in no green color appearing. In the other conditions except for the condition using the corrosion agent of Preparation Example 6 (NA10), the color was stable after 7 cycles, but the shape showed a gradual expansion up to 11 cycles. As shown in Figure 7, in the case of the copper powder of Example 2 (CS), as corrosion progressed under all conditions, the blue color tended to decrease and the number of samples that turned green tended to increase. Unlike the other copper powders, a dark green oxide was produced under conditions using the etchant of Example 6 (NA10). In general, a stable corrosion morphology was observed after 7 cycles.

[0051] As shown in Figure 8, in the case of copper powder (CZ) of Preparation Example 3, generally, bluish corrosion products were produced. Under the conditions using the corrosive agent (NA10) of Preparation Example 6, only a small amount of blue corrosion products were produced, but the overall state was dark red corrosion. In general, a stable corrosion morphology was observed after 7 cycles, and under the conditions using the corrosive agent (NA21) of Preparation Example 9, the expansion state gradually increased. As shown in Figure 9, in the case of copper powder (CP) of Preparation Example 4, under the conditions using the corrosive agent (NA10) of Preparation Example 6, only a small amount of green products were produced, but under other conditions, green oxides were produced overall. As the corrosion progressed, the phenomenon of changing from blue to green was clearly observed, generally indicating a stable corrosion state after 9 cycles.

[0052] As shown in Figure 10, in the case of copper powder of Preparation Example 5 (CT), blue or green corrosion products were generally produced, except for the condition using NA10. Under the conditions using the corrosives of Preparation Example 8 (NA11) and Preparation Example 9 (NA21), green corrosives were rapidly produced, while under the condition using the corrosive of Preparation Example 2 (NA01), a lot of blue corrosives remained. Generally, a stable corrosion state was shown after 5 cycles. From the above results, it was confirmed that the artificial corrosion period during which a stable patina is produced through complete corrosion is at least 7 cycles (i.e., 56 hours or more), and preferably 9 cycles or more (i.e., 72 hours or more).

[0053] <Experimental Example 4> Evaluation according to corrosive agent ratio After mixing each of the copper powders (CU, CS, CZ, CP, and CT) and each of the corrodents (mixtures of sodium chloride and ammonium chloride in weight ratios of 0:1, 1:2, 1:1, 2:1, and 1:0) in a 1:2 weight ratio, artificial corrosion was carried out for 7 cycles in the same manner as in Example 2. The results are shown in FIG. As shown in Fig. 11, when the ratio of ammonium chloride in the corrosive agent was increased, blue corrosion products were produced, but when the ratio of sodium chloride was increased, green corrosion products tended to be produced. However, when there was no ammonium chloride, corrosion did not proceed smoothly. As a result, it was confirmed that when the corrosive agent of Preparation Example 9 containing sodium chloride and ammonium chloride in a weight ratio of 2:1 was used, the green color closest to Hayeob color appeared.

[0054] On the other hand, a higher percentage of ammonium chloride would result in a more blue color. To confirm the optimal content ratio of sodium chloride and ammonium chloride to produce Hayeob color, the copper powders (CU, CS, CZ, CP, and CT) of Preparation Examples 1 to 5 were artificially corroded (7 cycles) using the corrosives of Preparation Examples 11, 12, 15, and 16, which contained sodium chloride and ammonium chloride in weight ratios of 3:1, 4:1, 9:1, and 19:1 (containing 5, 10, 20, and 25 wt. % ammonium chloride, based on the total weight of the corrosive), to prepare pigments and confirm their respective colors. The results are shown in FIG. 12. As shown in FIG. 12, in the case of the pigment prepared using the copper powder of Preparation Example 3 (CZ), as the ratio of sodium chloride increased, the blue color disappeared and green corrosion products were produced, while in the cases of the other copper powders, the green color tended to become darker.

[0055] In addition, a large color change was observed in the pigment prepared using the caustic agent of Preparation Example 6 (sodium chloride:ammonium chloride = 19:1) among all the pigments. To confirm this, each of the pigments was ground into a powder size of 100 μm or less using a mortar, and sieved into 45 μm or less, 45 to 75 μm, and 75 to 100 μm by wet sieving using distilled water, and the color according to size was analyzed. The results are shown in Figure 13. As shown in FIG. 13, in the case of using the corrosion agent of Preparation Example 16, a large change in color was found according to the particle size range, confirming that there were more red or black corrosion products rather than green corrosion products.

[0056] From the above results, it was found that as the percentage of sodium chloride in the etching agent increases, the green pigment increases, so a higher percentage of sodium chloride is suitable for producing a green-blue pigment with Hayeob color, but if the percentage of sodium chloride exceeds 95%, the etching is not fully achieved, so it should be contained at a maximum of less than 95%. As a result, the caustic used to prepare the patina pigment having Hayeob color may include sodium chloride and ammonium chloride, where sodium chloride is preferably included at 75% to 95% by weight, more preferably at 86% to 93% by weight, and most preferably at 90% by weight, to ensure that Hayeob color appears in all five types of copper powder. In addition, to ensure that the Hayeob color appears in all five types of copper powder, ammonium chloride is preferably included in an amount of 5 wt% to 25 wt%, more preferably in an amount of 7 wt% to 14 wt%, and most preferably in an amount of 10 wt%.

[0057] <Experimental Example 5> Evaluation of the removal rate of residual caustic agent following the wet screening process In order to evaluate the removal rate of residual etchant following the wet sieving process after etching during the pigment fabrication process, mixtures of copper powder and etchant in a weight ratio of 1:2 (CU 3:1, 19:1 (CU copper powder, sodium chloride:ammonium chloride = 3:1, 19:1), CP 3:1, 19:1 (CP copper powder, sodium chloride:ammonium chloride = 3:1, 19:1)) were artificially etched (7 cycles) by the method of Experimental Example 2. The powder was then crushed to a size of 100 μm or less using a mortar, and sieved to 45 μm or less, 45-75 μm, and 75-100 μm through wet sieving using distilled water. The discharged water was collected at the beginning, middle, and end of the wet sieving process, diluted 100 times, and the chloride ions (Cl - ) was measured and the results are shown in Figures 14A and 14B, through which the change in the content of residual caustic during the wet sieving process was analyzed.

[0058] As shown in Figures 14A and 14B, the analysis results showed that the initial chloride ion concentration was 205-876 ppm, and in the latter half, it was 1.66-33.1 ppm, indicating a reduction rate of about 91.9-99.1%. In other words, it was confirmed that almost 90% or more of the remaining corrosive agent was removed by wet sieving. However, the chloride ion concentration was measured in the water sample diluted 100 times, so additional dilution was required for the remaining corrosive agent in the corrosion product.

[0059] <Experimental Example 6> Evaluation of the removal rate of residual caustic agent following the wet dilution process Although the removal of residual caustic agents by wet sieving is highly effective, the amount of residual caustic agents is large, in the range of 100-1000 ppm, so additional measures are required to remove these residual caustic agents. As a result, for each particle size of the target pigments selected by wet sieving, a dilution process was additionally carried out to evaluate the removal rate of residual caustic agents, and the results are shown in Figures 16A-16C.

[0060] Each of the copper powders (CU, CS, CZ, CP, and CT) from Preparation Examples 1 to 5 and the corroding agent (sodium chloride:ammonium chloride=3:1) from Preparation Example 11 were mixed in a weight ratio of 1:2, followed by artificial corroding (7 cycles) by the method of Experimental Example 2. The powders were then crushed to a size of 100 μm or less using a mortar, and sieved into sizes of 45 μm or less, 45-75 μm, and 75 μm-100 μm through wet sieving using distilled water. The classified powders were used as target pigments. The dilution process was carried out by repeated exchanges of distilled water by mixing the target pigment with distilled water, allowing it to stand for a given period of time, and then decanting the distilled water.

[0061] After the pigment was mixed with distilled water in the dilution process, the caustic agent in the pigment was dissolved during the process of settling and removed together with the distilled water. In order to improve the efficiency of the process of removing the caustic agent, the elution time of the caustic agent was measured, and the chloride ion concentration and the increase rate were measured every 10 minutes. As a result, as shown in Figures 15A and 15B, the chloride ion concentration increased rapidly in the early stage of the analysis and stabilized to some extent after 60 minutes. The increase rate of the chloride ion concentration was analyzed, and the increase rate was 0.7% and 0.9% at 80 minutes and 90 minutes, respectively, indicating an increase rate of less than 1%. Based on the above results, the state in which the increase rate of the chloride ion concentration was maintained at 1% or less was regarded as reaching a constant weight, and the elution time of the caustic agent was set to 90 minutes.

[0062] Based on the calculated elution time, the target pigments prepared according to particle size were diluted. As a result, as shown in Figures 16A-16C, in the case of the second and third stage pigments with large pigment particles, most of them were found to have chloride ion concentrations below 10 ppm after 3 to 5 dilutions. In the case of the first stage with small pigment particles, the chloride ion concentration reached below 10 ppm through 7 to 8 dilutions. Through the above results, it was confirmed that the content of caustic agent in the pigment can be reduced to below 10 ppm through the dilution process.

[0063] <Experimental Example 7> Color evaluation following the refining process for removing fine powder Pigments have different colors when they are in their own powder state and when they are actually applied using a fixing agent such as glue. Through wet sieving, pigments are classified into particles below 45μm and between 45μm and 100μm, and the produced pigments may have low chroma when actually applied using water glue. This is because the white, gray, and brown fine particles are generated in the process of grinding the corrosive materials for pigment production, and these particles float on the surface when applied. Therefore, in order to improve the problem of low chroma of the produced verdigris pigment, a refining process was added and the fine powder contained in the verdigris pigment was removed using the water elutriation method. The refining process was a process of removing fine particles using an elutriation method, which was carried out on pigments selected for particles below 45 μm during the wet sieving process.

[0064] Specifically, the purification process according to the elutriation method was carried out in the first and second stages separately. The first stage was carried out by putting the pigment into a 600ml beaker, filling it with both running water, mixing it, leaving it for 15 minutes, and removing the supernatant except for the precipitated particles. The second stage was carried out by mixing the watered-down supernatant well, leaving it for 30 minutes, and then removing the supernatant except for the precipitate. After that, the purified pigment was obtained by drying the precipitate at 60°C for 24 hours using a dryer. The pigment without the purification process and the purified pigment were applied and the colors were compared, and the results are shown in Figure 17 (5S7C corrosion conditions: 5:1 NA corrode, 7 cycles of artificial corrosion / 6S7C: 6:1 NA corrode, 7 cycles of artificial corrosion).

[0065] As shown in FIG. 17, it was confirmed that the green color of Hayeob was more pronounced when colored using the verdigris pigment produced by the refining process. Based on the above results, the method for preparing a green-blue pigment having Hayeob color according to an embodiment of the present invention may be carried out in the steps of corrosion, grinding, wet sieving, salt removal, purification, and drying, as shown in FIG. 18. More preferably, it may be carried out by a method carrying out the following process. Copper powder (including at least one of copper; and copper alloys including copper and at least one of tin (Sn), zinc (Zn), and lead (Pb)) was mixed with a corroding agent containing sodium chloride and ammonium chloride in a certain ratio to corrode the copper powder. The corroding agent included 75-95% by weight of sodium chloride and 5-25% by weight of ammonium chloride. Then, the corrosion product was crushed and screened, and a dilution process for removing residual corroding agent and a purification process for removing fine particles were carried out.

[0066] <Experimental Example 8> Evaluation according to corrosive agent ratio (2) As in Experimental Example 7, the patina pigment was prepared by carrying out the steps of etch, grinding, wet sieving, desalting, refining, and drying. As etchants, sodium chloride and ammonium chloride were used in different weight ratios of 3:1, 4:1, 5:1, 6:1, and 9:1. The color of the produced pigment was checked, and the results are shown in FIG. 19, and the results of comparison with the traditional Dancheong Hayeob color selected by Dancheong experts are shown in FIG. 20.

[0067] As a result of color measurement in Figure 19 and evaluation in Figure 20, all five types of produced pigments showed green or greenish blue close to Hayeob color. However, it was found that the case with the lowest ammonium chloride ratio of 10 wt% was closest to Hayeob color. As a result, the preparation method of the patina pigment which can replace the traditional Dancheong Hayeob pigment can be most preferably carried out by the method shown in Table 4 below.

[0068] [Table 4]

[0069] Specifically, copper powder was mixed with twice the weight of the caustic agent, and the caustic agent was a mixture of sodium chloride and ammonium chloride in a ratio of 9:1, and then artificial corrosion was carried out using a corrosion tester. The corrosion was carried out in 9 cycles (total 72 hours), and the corrosion products were crushed to 100 μm or less using a mortar. The crushed samples were screened into particles of 45 μm or less and 45-100 μm by sieving using distilled water through a wet sieving method, and more than 90% of the residual caustic agent was removed in this process. The caustic agent contained in the pigment was removed through a dilution process in which the process of stirring for 1 hour, removing the supernatant, and settling for 1 hour was repeated more than 5 times to improve the color stability. Fine particles were removed through a purification process using a water elutriation method, and the saturation of the pigment was increased. The final pigment was prepared through a drying process in which the pigment was dried at 60° C. for 24 hours using a dryer.

[0070] <Experimental Example 9> Evaluation of color and yield of prepared patina pigment A green-blue pigment was prepared by the method shown in Table 5 using five types of copper powders of Preparation Examples 1 to 5. According to the particle size of each copper powder, it was divided into M (45 to 100 μm) and S (45 μm or less) (S is the state in which fine particles are removed from particles of 45 μm or less by a purification process). Two types of pigment were prepared for each copper powder, and a total of 10 types of green-blue pigments were produced. The color and yield of the 10 prepared pigments were confirmed, and the results are shown in Figures 21 and 22.

[0071] As shown in FIG. 21, all the prepared patina pigments were generally light to dark green, indicating a Hayeob color, with the pigments with larger particle sizes showing relatively darker colors. As shown in FIG. 22, about 60 g of copper powder was used to produce the patina pigment at one time, and four sets were produced at one time, generally using 241-243 g of copper powder to produce 267-299 g of patina pigment, resulting in a yield of 110.7-123.6%.

[0072] <Experimental Example 10> Evaluation of the physical properties of the prepared patina pigment The chromaticity, particle size distribution, microstructure and oil absorption were measured for the 10 types of patina pigments prepared in Experimental Example 8, and the results are shown in Figures 23-27. 23A and 23B are a series of graphs showing the results of measuring the chromaticity of 10 types of prepared pigments. As shown in FIG. 23A, the M size green-blue pigment has an a of -9.71 to -23.05. * Value, b from -1.35 to 1.64 * value, and L of 40.84 to 48.97 * As shown in FIG. 23B, the S-size green-blue pigment had a value of -7.61 to -20.76. * Value, b of 0.90 to 4.95 * value, and 43.33 to 53.24 * In general, the brightness (L * value) and greenness (-a * The blueness (b value) is higher than that of the M-size verdigris pigment, but * Depending on the type of copper powder, the greenness of CS, CP, and CT was higher than that of CU and CZ, and the greenness of CS was the highest.

[0073] Figure 24 is a series of graphs showing the results of measuring the particle size distribution of 10 types of prepared pigments. As shown in Figure 24, generally, similar distribution patterns were shown regardless of the type of copper powder below 100 μm. The M size patina pigment with large particles showed a relatively narrow normal distribution with a particle size of 66.9 μm as the center, and an average particle size of 63.0 to 66.9 μm. The S size patina pigment with small particles showed a shape close to a normal distribution centered on a particle size of 21.2, but slightly broadened with a relatively large number of particles below 10 μm, and an average particle size of 19.6 to 29.4 μm (Figure 61). In the case of the S pigment prepared below 45 μm, small particles below 5 μm accounted for less than 1% of each section, which is likely due to the removal of fine particles during the refining process.

[0074] FIG. 25 is a series of photographs showing the results of observing the 10 types of pigments prepared using a magnification microscope, and FIG. 26 is a series of photographs showing the results of observing the pigments using a scanning electron microscope. As shown in Figure 25, as a result of magnification microscopic analysis, blue-green or green particles were observed in all 10 pigments, and dark red particles existed among the green particles. Especially a large number of dark red particles were observed in the patina pigment prepared with CU copper powder. This is attributed to the fact that particles separated from the surface of the corrosion product appear in the process of grinding the corrosion product. This is probably due to the nature of corrosion, where the corrosion occurs from the surface of the raw material, and once the corrosion layer is formed, there may be copper or copper oxide remaining inside that is not fully corroded. In the case of pure copper, this feature is stronger than that of the alloy mixed with tin, zinc, and lead sugar, so it is determined that there are relatively more dark red particles.

[0075] As shown in FIG. 26, the results of FE-SEM analysis showed that the 10 pigments generally had rough surface particles, many porous ellipsoidal particles were observed, and they showed polygonal particle shapes, which were different from the natural inorganic pigments that showed inorganic specific particle shapes. Figure 27 is a graph showing the results of evaluating the oil absorption of the 10 types of pigments prepared. Oil absorption is one of the basic characteristics of pigments, and is affected by particle shape, particle size, and particle size distribution, and is a criterion for estimating the mixing ratio of fixative when using pigments. The oil absorption of the patina pigments was measured. As a result, as shown in Figure 27, the M size pigments with larger particle size showed relatively higher oil absorption than the S size pigments with smaller particle size. The M size pigments showed oil absorption of 44.82-54.97ml / 100g, and the patina pigments made of CZ showed the highest oil absorption. The S size pigments showed oil absorption of 36.62-43.97ml / 100g, and the patina pigments made of CU showed the highest oil absorption.

[0076] <Experimental Example 11> Evaluation of the components of the prepared patina pigment X-ray fluorescence and X-ray diffraction analyses were conducted to analyze the constituents of the ten patina pigments prepared in Example 8. The results are shown in Figures 28 and 29. FIG. 28 is a graph showing the results of X-ray fluorescence analysis for 10 pigments. As shown in Figure 28, the constituent elements of the patina pigments showed no significant difference between the S-size and M-size pigments classified by particle size, and the main elements detected were copper (Cu), zinc (Zn), tin (Sn), and lead (Pb). Since it is a patina pigment made of pure copper and copper alloy containing tin, zinc, and lead, the main elements detected may be due to the influence of copper and copper alloy, raw materials.

[0077] FIG. 29 is a series of graphs showing the results of X-ray diffraction analysis for 10 pigments. As shown in FIG. 29, there is no significant difference between S-size pigments and M-size pigments classified by particle size, and the main constituent inorganic substance of the verdigris pigment was identified as atacamite (Cu2Cl(OH)3). In addition, elements such as copper (Cu), zinc (Zn), tin (Sn), and lead (Pb) contained in the raw copper powder were detected (in FIG. 29, Ata is atacamite, Cla is clinoatacamite, Cu is copper, Cpr is cuprite, Kps is kapellasite, Zin is zincite, Ana is anatacamite, and Sal is salammonite).

[0078] <Experimental Example 12> Evaluation of the stability of the prepared patina pigment Accelerated weathering tests were carried out to evaluate the stability of the green-blue pigment. The stability was evaluated by measuring the chromaticity of the colored samples at regular intervals in the accelerated weathering test process and calculating the color difference (ΔE) according to the accumulated UV irradiation. The results are shown in Figures 30 and 31.

[0079] As shown in Figure 30, CU, CZ, CP, and CT patina pigments, excluding CS patina pigment, showed a similar trend. From the start of the test, the color difference was 11.9 MJ / m 2 The color difference increased rapidly until the UV exposure reached 100 nm, and then increased gradually thereafter. In the case of CS patina pigment, the color difference tended to increase rapidly from the beginning to the end of the test. As a result, CU and CZ patina pigments showed color difference values ​​of 3.81 and 4.97, respectively, indicating relatively good color change, while CS, CP, and CT patina pigments showed color differences of 8 or more, indicating relatively high color change. In addition, when examining the color change of the verdigris pigment before and after the stability evaluation test through Figure 31, a color change from bluish green before the test to dark green with increased yellowness after the test was found.

[0080] <Experimental Example 13> Comparative evaluation with traditional Dancheong Hayeob pigments The patina pigment prepared according to an embodiment of the present invention was compared with Hayeob pigment, which is presumed to be the patina pigment in traditional Dancheong. To compare the color of Hayeob, a traditional Dancheong pigment, with the color of the prepared verdigris pigment, the results of the traditional Dancheong survey and the chromaticity before and after aging of Dangrok pigment were compared, and the results are shown in Figure 32.

[0081] As shown in FIG. 32, the prepared patina pigment exhibited similar values ​​for greenness compared to the remaining Hayeob pigment, while being significantly less yellow. On the other hand, it was confirmed that the color of the patina pigment after aging had a similar color to that of the traditional Dancheong Hayeob color due to a significant increase in yellowness. Regarding the investigation into the reproduction of the traditional Dancheong pigment, it was encountered that the prepared patina pigment, when aged, exhibited a color similar to that of the traditional Dancheong Hayeob color remaining today. In addition, the results of the characteristic analysis of the prepared patina pigments and the traditional Danhcheong Hayeob pigments were compared. As a result, it was confirmed that the patina pigments replicated by the chlorine etching method using pure copper and copper alloy powders (five types) had similar color and composition, as well as similar particle shape, to the traditional Danhcheong Hayeob in the cultural heritage.

Claims

1. A method for preparing a patina pigment that can replace the traditional Dancheong Hyeob pigment, comprising the steps of: Preparing a copper powder comprising at least one of copper and a copper alloy comprising copper and at least one of tin (Sn), zinc (Zn), and lead (Pb); and Corroding the copper powder by mixing the copper powder with a caustic containing sodium chloride and ammonium chloride, where the caustic comprises 75-95 wt. % sodium chloride and 10-25 wt. % ammonium chloride based on the total weight; The method comprising:

2. 2. The method for preparing a patina pigment according to claim 1, wherein the caustic comprises 86-90% by weight sodium chloride and 10-14% by weight ammonium chloride, based on the total weight.

3. 2. The method for preparing a patina pigment according to claim 1, wherein in the corroding step, the copper powder and the corroding agent are mixed in a weight ratio of 1:2 to 1:

4.

4. 2. The method for preparing the patina pigment according to claim 1, wherein the etching is carried out by artificial etching using a corrosion tester.

5. 2. The method for preparing the patina pigment of claim 1, wherein the method further comprises the steps of grinding and wet fractionating the corrosion product prepared in the corrosion step.

6. 6. The method for preparing the patina pigment of claim 5, wherein the method further comprises the step of removing residual caustic agent by mixing the milled and wet fractionated powder with distilled water and removing the supernatant.

7. 7. The method for preparing the patina pigment of claim 6, wherein the method further comprises purifying the powder to remove residual caustic agent.

8. A patina pigment prepared by the process of claim 1.

9. 9. The patina pigment according to claim 8, wherein the patina pigment is an artificial patina pigment which can replace Hayeob pigment for traditional Dancheong coloring.

Citation Information

Patent Citations

  • Formation of greenish blue film

    JP1986042378A

  • Production of verdigris-like substance of organic dibasic acid composite type

    JP1987124154A

  • Patina pattern-forming agent

    JP1990118082A

  • Surface treated copper sheet

    JP1997225395A

  • Producing method for artificial copper plate

    KR1020100082542A