Nickel-zinc-copper ferrite material as well as preparation method and application thereof

By adjusting the content of Fe2O3, NiO, ZnO, CuO and adding auxiliary components, a nickel-zinc copper ferrite material with high magnetic permeability and high Curie temperature was prepared, and the existing nickel-zinc ferrite material was solved at high frequency. The problems of low magnetic permeability and insufficient saturated magnetic induction strength are suitable for high-performance power inductors and common mode inductors.

CN118955110AActive Publication Date: 2024-11-15HENGDIAN GRP DMEGC MAGNETICS CO LTD +1

Patent Information

Application Number
CN202411010712.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing nickel-zinc ferrite materials have low magnetic permeability at high frequencies, and insufficient Curie temperature and saturated magnetic induction strength, resulting in problems such as superimposed current, low energy conversion efficiency and loss during use.

Method used

By adjusting the overall content of Fe2O3, NiO, ZnO, and CuO, and adding auxiliary components such as Bi2O3, Co2O3, CaCO3, and ZrO2, wet ball mill mixing and spray granulation process are used to prepare nickel-zinc copper ferrite materials to control the main components and auxiliary components The proportion of components can achieve high magnetic permeability, high Curie temperature and low specific temperature coefficient.

Benefits of technology

The prepared nickel-zinc copper ferrite material has high saturation magnetic induction strength, high magnetic permeability, high Curie temperature and low residual magnetic induction strength. It is suitable for power inductors and common mode inductors, improving the application of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955110A_ABST
    Figure CN118955110A_ABST
Patent Text Reader

Abstract

The invention relates to a nickel-zinc-copper ferrite material as well as a preparation method and application thereof. The nickel-zinc-copper ferrite material comprises main components and auxiliary components, the main component is prepared from the following components in percentage by weight: 64.5 to 66.5 percent of Fe2O3, 9 to 12 percent of NiO, 13.5 to 18.5 percent of ZnO and 3 to 10 percent of CuO according to the total mass percentage content of 100wt%; the auxiliary components are prepared from the following components in percentage by mass: 0.3 to 1.5 weight percent of Bi2O3, 0.1 to 0.6 weight percent of Co2O3, 0.03 to 0.08 weight percent of CaCO3 and 0.01 to 0.1 weight percent of ZrO2 according to the total mass percent of the main components. The nickel-zinc-copper ferrite material prepared by the invention has high saturation flux density, high magnetic conductivity, high Curie temperature, low residual magnetic flux density and low specific temperature coefficient, and can be better applied to power inductors or common-mode inductors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ferrites, and in particular to a nickel-zinc-copper ferrite material and a preparation method and application thereof. Background Art

[0002] Ferrite materials have been widely used in biomedicine, electromagnetic devices, LED lighting, high computing power computers and other fields due to their high magnetic induction intensity, high coercivity and high magnetic permeability. With the development trend of miniaturization and thinness of components, higher requirements are placed on the magnetoelectric properties of mainstream nickel-zinc materials in ferrite materials.

[0003] The nickel-zinc ferrite material currently under research has a high magnetic permeability, but a low Curie temperature and saturation magnetic induction intensity, which results in products made of nickel-zinc materials having disadvantages such as low inductance after superimposed current, low energy conversion efficiency and high loss during use.

[0004] CN104402428A discloses a nickel-zinc ferrite material with high frequency, high magnetic permeability and high Q value and a preparation method thereof. The ferrite material includes a main component and a doping component, both of which are calculated based on oxide raw materials, wherein the main component is composed of 17-19 mol% NiO, 1-33 mol% ZnO3, and the rest is Fe2O3 in molar percentage; the doping component is composed of 0.2-0.4 wt% SnO2 and 0.002-0.004 wt% Dy2O3 in weight percentage of the total weight of the material. The ferrite material is prepared by the following method: weighing raw materials → pre-sintering once → pre-sintering twice → granulation molding → sintering. The nickel-zinc ferrite material provided by the invention has high frequency and high magnetic permeability, but does not have the performance of high Bs value.

[0005] CN 101169996A discloses a Mn-Zn ferrite magnetic material and a preparation method thereof. The main components and contents of the Mn-Zn ferrite magnetic material are calculated as oxides: Fe2O3 is 52-56 mol%, ZnO is 2-10 mol%, MnO is 38-42 mol%, and the auxiliary components are one or a combination of CaO: 400-800 ppm, Nb2O5: 100-400 ppm, ZrO2: 100-800 ppm, and Co2O3: 1000-5000 ppm. The Mn-Zn ferrite magnetic material has high saturation magnetic induction intensity, low power consumption and excellent electromagnetic characteristics under ultra-high temperature conditions. The patent simultaneously adds a large number of impurities to the main components of ferrite Fe2O3, NiO, ZnO and CuO to achieve the effects of high saturation magnetic induction intensity and high Curie temperature, but the magnetic permeability after sintering is low, and the temperature stability thereof needs to be studied.

[0006] CN109279886A discloses a nickel-zinc-copper soft magnetic ferrite material, which is composed of the following components by mass: 40-60 parts of iron oxide powder, 10-20 parts of nickelous oxide, 5-10 parts of zinc sulfate, 5-10 parts of antimony trioxide, 3-6 parts of sodium dodecylbenzenesulfonate, 2-5 parts of sodium hypophosphite, 2-5 parts of expanded perlite powder, 2-5 parts of methyl methacrylate, 1-3 parts of sodium benzoylsulfonimide, 1-3 parts of tungsten trioxide, and the balance of deionized water. The nickel-zinc-copper soft magnetic ferrite material provided by the invention can meet the requirements of low loss under high frequency, but the other magnetic properties need to be improved.

[0007] Therefore, in view of the shortcomings of the prior art, there is an urgent need to provide a nickel-zinc-copper ferrite material with high magnetic permeability, high Curie temperature, high saturation magnetic induction intensity and low specific temperature coefficient. Summary of the invention

[0008] The purpose of the present invention is to provide a nickel-zinc-copper ferrite material and a preparation method and application thereof. By limiting the reasonable ratio of raw materials, the prepared nickel-zinc-copper ferrite material has the characteristics of high magnetic permeability, high Curie temperature, high saturation magnetic induction intensity, low residual magnetic induction intensity and low specific temperature coefficient.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In the first aspect, the present invention provides a nickel-zinc-copper ferrite material, which includes a main component and an auxiliary component; based on the total mass percentage of 100wt%, the main component includes: Fe2O364.5-66.5wt%, NiO 9-12wt%, ZnO 13.5-18.5wt%, CuO 3-10wt%; based on the total mass percentage of the main component, the auxiliary component includes: Bi2O3 0.3-1.5wt%, Co2O3 0.1-0.6wt%, CaCO3 0.03-0.08wt%, ZrO2 0.01-0.1wt%.

[0011] The present invention can obtain a nickel-zinc-copper ferrite material with higher magnetic permeability and Curie temperature by controlling the content range of the main component; in order to ensure high saturation magnetic induction intensity and low specific temperature coefficient characteristics, it is necessary to adjust the overall content of Fe2O3, ZnO, NiO and CuO; by adjusting the auxiliary component Ca 2+ and Bi 3+ The combined substitution of can improve the magnetic permeability and achieve high-frequency charging efficiency; 2+ 、Co 3+ A small amount of substitution can reduce the imaginary part of the magnetic permeability to achieve low loss characteristics; through Ca 2+ 、Co 3+and Bi 3+ or Zr 4+ The combined substitution can adjust the saturation magnetic induction intensity to achieve the applicability of the device in extreme environments. The nickel-zinc-copper ferrite material prepared by the present invention has high saturation magnetic induction intensity, high magnetic permeability, high Curie temperature, low residual magnetic induction intensity and low specific temperature coefficient, and can be better applied to power inductors or common-mode inductors.

[0012] The mass percentage of Fe2O3 in the main component is 64.5-66.5wt%, for example, it can be 64.5wt%, 65wt%, 65.5wt%, 66wt% or 66.5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] The mass percentage of NiO in the main component is 9-12wt%, for example, it can be 9wt%, 9.5wt%, 10.3wt%, 11.5wt% or 12wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0014] The mass percentage of ZnO in the main component is 13.5-18.5wt%, for example, it can be 13.5wt%, 14.5wt%, 15.5wt%, 16.5wt% or 18.5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] The mass percentage of CuO in the main component is 3-10wt%, for example, it can be 3wt%, 5wt%, 6wt%, 8wt% or 10wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] The mass percentage of Bi2O3 in the auxiliary component is 0.3-1.5wt% of the total mass percentage of the main component, for example, it can be 0.3wt%, 0.5wt%, 0.8wt%, 1.2wt% or 1.5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] The mass percentage of Co2O3 in the auxiliary component is 0.1-0.6wt% of the total mass percentage of the main component, for example, it can be 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt% or 0.6wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] The mass percentage of CaCO3 in the auxiliary component is 0.03-0.08wt% of the total mass percentage of the main component, for example, it can be 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt% or 0.08wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] The mass percentage of ZrO2 in the auxiliary component is 0.01-0.1wt% of the total mass percentage of the main component, for example, it can be 0.01wt%, 0.03wt%, 0.05wt%, 0.08wt% or 0.1wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the total mass percentage of ZnO+CuO in the main component is 22-26wt%, for example, it can be 22wt%, 23wt%, 23.5wt%, 24wt% or 26wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] In the present invention, the total amount of ZnO and CuO needs to be controlled within a reasonable range. If the total amount exceeds the limited range, even if the content of each main component is within the required range, the magnetic permeability and saturation magnetic induction intensity Bs of the prepared nickel-zinc-copper ferrite material will be reduced.

[0022] Preferably, the total mass percentage of Bi2O3+ZrO2 in the auxiliary components is 0.35-1.55wt% of the total mass percentage of the main components, for example, it can be 0.35wt%, 0.5wt%, 0.8wt%, 1wt% or 1.55wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] In the present invention, the total amount of Co2O3 and CaCO3 needs to be controlled within a reasonable range. If the total amount exceeds the limited range, the magnetic permeability of the prepared nickel-zinc-copper ferrite material will be reduced even if the content of each auxiliary component is within the required range.

[0024] In a second aspect, the present invention provides a method for preparing the nickel-zinc-copper ferrite material as described in the first aspect, the preparation method comprising the following steps:

[0025] (1) weighing the main components according to the proportion, and then wet ball milling and mixing, and the obtained ball milled material is pre-calcined after the first spray granulation to obtain a pre-calcined material;

[0026] (2) weighing auxiliary components according to the ratio, and then sequentially subjecting the auxiliary components, the liquid medium, the additives and the pre-sintered material obtained in step (1) to a first grinding and a second grinding, and the obtained ground material is subjected to a second spray granulation and then molded and sintered to obtain the nickel-zinc-copper ferrite material.

[0027] The preparation method of the nickel-zinc-copper ferrite material provided by the present invention is beneficial to the magnetic domain refinement of the nickel-zinc-copper ferrite material obtained by subsequent sintering by selecting reasonable process parameters, thereby ensuring the high saturation magnetic induction intensity, high magnetic permeability, high Curie temperature, low residual magnetic induction intensity and low specific temperature coefficient of the nickel-zinc-copper ferrite material, thereby meeting the high performance requirements as a soft magnetic ferrite material.

[0028] Preferably, the mass ratio of the main component, the ball milling medium and the liquid medium in the wet ball milling mixing in step (1) is 1:(4-8):(0.5-1.2), for example, it can be 1:4:0.5, 1:5:0.6, 1:6:0.8, 1:7:1 or 1:8:1.2, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the ball milling media comprises zirconium balls.

[0030] Preferably, the liquid medium comprises deionized water.

[0031] Preferably, the wet ball milling mixing time in step (1) is 20-60 min, for example, 20 min, 30 min, 40 min, 50 min or 60 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the pre-burning temperature in step (1) is 780-950°C, for example, 780°C, 800°C, 820°C, 850°C, 880°C, 900°C or 950°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the pre-burning time in step (1) is 2-4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the additives in step (2) include a binder, a dispersant and a defoaming agent.

[0035] Preferably, the mass ratio of the pre-burned material, liquid medium, binder, dispersant and defoamer in step (2) is 100:(40-150):(4-20):(0.1-2):(0.001-0.0025), for example, it can be 100:40:4:0.1:0.001, 100:70:7:0.5:0.0012, 100:100:10:1:0.0015, 100:120:15:1.5:0.002 or 100:150:20:2:0.0025, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0036] Preferably, the liquid medium in step (2) comprises deionized water.

[0037] Preferably, the binder comprises any one of polyvinyl alcohol, polyvinyl butyral, hydroxy cellulose or polyacrylate or a combination of at least two thereof, typical but non-limiting combinations comprising a combination of polyvinyl alcohol and polyvinyl butyral, a combination of polyvinyl butyral, hydroxy cellulose and polyacrylate, or a combination of polyvinyl alcohol, polyvinyl butyral, hydroxy cellulose and polyacrylate.

[0038] Preferably, the dispersant includes any one of amine citrate, sodium stearate, polyacrylic acid or triethanolamine, or a combination of at least two of them. Typical but non-limiting combinations include a combination of amine citrate and sodium stearate, a combination of sodium stearate and polyacrylic acid, or a combination of amine citrate, sodium stearate, polyacrylic acid and triethanolamine.

[0039] Preferably, the defoaming agent includes any one of n-octanol, tributyl phosphate, stearic acid or polyethylene glycol, or a combination of at least two of them. Typical but non-limiting combinations include a combination of n-octanol and tributyl phosphate, a combination of stearic acid and polyethylene glycol, or a combination of n-octanol, tributyl phosphate, stearic acid and polyethylene glycol.

[0040] Preferably, the rotation speed of the first grinding in step (2) is 145-265 rpm, for example, it can be 145 rpm, 180 rpm, 200 rpm, 220 rpm or 265 rpm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] Preferably, the first grinding time in step (2) is 5-10 min, for example, 5 min, 6 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the rotation speed of the second grinding in step (2) is 270-320 rpm, for example, it can be 270 rpm, 290 rpm, 300 rpm, 310 rpm or 320 rpm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0043] Preferably, the second grinding time in step (2) is 0.5-2 h, for example, 0.5 h, 0.8 h, 1 h, 1.5 h or 2 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the median particle size X50 of the grinding material in step (2) is 0.5-0.8 μm, and the particle size X90 with a cumulative percentage of 90% is 1.25-1.8 μm.

[0045] The median particle size X50 of the abrasive is 0.5-0.8 μm, for example, 0.5 μm, 0.6 μm, 0.7 μm or 0.8 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] The lower median particle size X50 of the abrasive is beneficial to the magnetic domain refinement of the nickel-zinc-copper ferrite material obtained by subsequent sintering, thereby improving the magnet strength.

[0047] The particle size X90 of the abrasive at a cumulative percentage of 90% is 1.25-1.8 μm, for example, 1.25 μm, 1.5 μm, 1.6 μm, 1.7 μm or 1.8 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, the average particle size of the particles obtained by the second spray granulation in step (2) is 30-200 μm, for example, 30 μm, 60 μm, 100 μm, 150 μm or 200 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0049] Preferably, the forming in step (2) includes forming a standard sample ring blank.

[0050] The density of the standard sample ring blank is 3.1-3.25g / cm 3 , size is H25*15*10mm.

[0051] Preferably, the sintering in step (2) is carried out in a push plate kiln.

[0052] Preferably, the sintering in step (2) includes a first heat treatment, a second heat treatment, a first cooling treatment and a second cooling treatment performed in sequence.

[0053] Preferably, the specific steps of the first heat treatment include: heating from room temperature to 550-750° C. at a heating rate of 0.5-2° C. / min in an air atmosphere, and keeping the temperature for 2-7 hours.

[0054] The heating rate of the first heat treatment is 0.5-2°C / min, for example, it can be 0.5°C / min, 0.8°C / min, 1°C / min, 1.5°C / min or 2°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] The normal temperature refers to a temperature of 20-25°C.

[0056] The temperature endpoint of the first heat treatment is 550-750°C, for example, 550°C, 600°C, 650°C, 700°C or 750°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] The holding time of the first heat treatment is 2-7 hours, for example, 2 hours, 3 hours, 5 hours, 6 hours or 7 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0058] Preferably, the specific steps of the second heat treatment include: continuing to heat up to 950-1050° C. at a heating rate of 1-3° C. / min, and keeping the temperature for 2-5 hours.

[0059] The heating rate of the second heat treatment is 1-3°C / min, for example, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min or 3°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] The temperature endpoint of the second heat treatment is 950-1050°C, for example, it can be 950°C, 980°C, 1000°C, 1020°C or 1050°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] The holding time of the second heat treatment is 2-5 hours, for example, 2 hours, 2.5 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0062] Preferably, the specific step of the first cooling treatment includes: cooling to 595-605° C. at a cooling rate of 2-6° C. / min in an air atmosphere.

[0063] The cooling rate of the first cooling treatment is 2-6°C / min, for example, it can be 2°C / min, 3°C / min, 4°C / min, 5°C / min or 6°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0064] The temperature endpoint of the first cooling treatment is 595-605°C, for example, it can be 595°C, 598°C, 600°C, 602°C or 605°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0065] Preferably, the specific step of the second cooling treatment includes: continuing to cool to 45-55°C at a cooling rate of 1-5°C / min.

[0066] The cooling rate of the second cooling treatment is 1-5°C / min, for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] The temperature end point of the second cooling treatment is 45-55°C, for example, 45°C, 48°C, 50°C, 52°C or 55°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0068] The sintering adopts the sintering method in the air atmosphere of the push plate kiln, which can mass-produce magnetic core samples and achieve low-cost production; at the same time, through two-stage heat treatment and two-stage cooling treatment, the magnetic permeability can be significantly improved, the magnet densification can be improved, and then the saturation magnetic induction intensity Bs of the magnetic core can be improved.

[0069] In a third aspect, the present invention provides an application of the nickel-zinc-copper ferrite material as described in the first aspect, wherein the nickel-zinc-copper ferrite material is used in a power inductor or a common-mode inductor.

[0070] The nickel-zinc-copper ferrite material provided by the present invention solves the problem of magnetic permeability stability at low and high temperatures and the problem of low saturation magnetic induction intensity and high residual magnetic induction intensity of the material, thereby improving the applicability of power magnetic products such as common-mode inductors and laminated magnetic beads / inductors, and can be better applied to product industries such as avionics, automotive electronics, and communications electronics.

[0071] Compared with the prior art, the present invention has the following beneficial effects:

[0072] The present invention can obtain a nickel-zinc-copper ferrite material with higher magnetic permeability and Curie temperature by controlling the content range of the main component; in order to ensure high saturation magnetic induction intensity and low specific temperature coefficient characteristics, it is necessary to adjust the overall content of Fe2O3, ZnO, NiO and CuO; by adjusting the auxiliary component Ca 2+ and Bi 3+ The combined substitution of can improve the magnetic permeability and achieve high-frequency charging efficiency; 2+ 、Co 3+ A small amount of substitution can reduce the imaginary part of the magnetic permeability to achieve low loss characteristics; through Ca 2+ 、Co 3+ and Bi 3+ or Zr 4+ The combined substitution can adjust the saturation magnetic induction intensity to achieve the applicability of the device in extreme environments. The nickel-zinc-copper ferrite material prepared by the present invention has high saturation magnetic induction intensity, high magnetic permeability, high Curie temperature, low residual magnetic induction intensity and low specific temperature coefficient, and can be better applied to power inductors or common-mode inductors. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 This is a SEM image of the nickel-zinc-copper ferrite material provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0074] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0075] Example 1

[0076] The present embodiment provides a nickel-zinc-copper ferrite material, which includes a main component and an auxiliary component; based on the total mass percentage of 100wt%, the main component includes: Fe2O365.5wt%, NiO 11wt%, ZnO16.5wt%, CuO 7wt%; based on the total mass percentage of the main component, the auxiliary component includes: Bi2O3 0.5wt%, Co2O3 0.3wt%, CaCO3 0.05wt%, ZrO20.05wt%;

[0077] The total mass percentage of ZnO+CuO in the main component is 23.5wt%; the total mass percentage of Bi2O3+ZrO2 in the auxiliary component is 0.55wt% of the total mass percentage of the main component.

[0078] The preparation method of the nickel-zinc-copper ferrite material comprises the following steps:

[0079] (1) weighing the main components according to the ratio, and then wet ball milling for 40 minutes, wherein the mass ratio of the main components, zirconium balls and deionized water in the wet ball milling is 1:6:0.8; the obtained ball mill material is pre-calcined at 850° C. for 3 hours after the first spray granulation to obtain a pre-calcined material;

[0080] (2) weighing auxiliary components according to the proportion, and then grinding the auxiliary components, hydroxycellulose, sodium stearate, tributyl phosphate, deionized water and the pre-burned material obtained in step (1) at a rotation speed of 200 rpm for 8 minutes and a rotation speed of 300 rpm for 1.5 hours to obtain a grinding material with a median particle size X50 of 0.7 μm and a cumulative percentage of 90% of the particle size X90 of 1.5 μm; the obtained grinding material is subjected to a second spray granulation to obtain particles with an average particle size of 100 μm, and then formed and sintered in a push-plate kiln to obtain the nickel-zinc-copper ferrite material;

[0081] The mass ratio of the pre-burned material, deionized water, hydroxy cellulose, sodium stearate and tributyl phosphate is 100:100:10:1:0.002;

[0082] The sintering includes a first heat treatment, a second heat treatment, a first cooling treatment and a second cooling treatment performed in sequence; the specific steps of the first heat treatment include: heating from room temperature to 650°C at a heating rate of 1°C / min in an air atmosphere, and keeping the temperature for 5 hours; the specific steps of the second heat treatment include: continuing to heat to 1000°C at a heating rate of 2°C / min, and keeping the temperature for 3 hours; the specific steps of the first cooling treatment include: cooling to 600°C at a cooling rate of 4°C / min in an air atmosphere; the specific steps of the second cooling treatment include: continuing to cool to 50°C at a cooling rate of 3°C / min;

[0083] The molding includes molding of a standard sample ring blank; the density of the standard sample ring blank is 3.2g / cm 3 , size is H25*15*10mm.

[0084] The SEM image of the nickel-zinc-copper ferrite material prepared in this example is as follows: Figure 1 As shown in the figure, it can be seen that the morphology and particle size are uniform and the grains are relatively dense.

[0085] Example 2

[0086] The present embodiment provides a nickel-zinc-copper ferrite material, which includes a main component and an auxiliary component; based on the total mass percentage of 100wt%, the main component includes: Fe2O364.5wt%, NiO 9.5wt%, ZnO 16wt%, CuO 10wt%; based on the total mass percentage of the main component, the auxiliary component includes: Bi2O30.3wt%, Co2O3 0.1wt%, CaCO3 0.03wt%, ZrO20.05wt%;

[0087] The total mass percentage of ZnO+CuO in the main component is 26wt%; the total mass percentage of Bi2O3+ZrO2 in the auxiliary component is 0.35wt% of the total mass percentage of the main component.

[0088] The preparation method of the nickel-zinc-copper ferrite material comprises the following steps:

[0089] (1) weighing the main components according to the ratio, and then wet ball milling for 20 minutes, wherein the mass ratio of the main components, zirconium balls and deionized water in the wet ball milling is 1:4:0.5; the obtained ball mill material is pre-calcined at 780° C. for 4 hours after the first spray granulation to obtain a pre-calcined material;

[0090] (2) weighing auxiliary components according to the proportion, and then grinding the auxiliary components, polyvinyl alcohol, triethanolamine, n-octanol, deionized water and the pre-sintered material obtained in step (1) at a rotation speed of 265 rpm for 5 min and at a rotation speed of 320 rpm for 0.5 h, to obtain a grinding material with a median particle size X50 of 0.5 μm and a cumulative percentage of 90% particle size X90 of 1.25 μm; the obtained grinding material is subjected to a second spray granulation to obtain particles with an average particle size of 30 μm, and then formed and sintered in a push-plate kiln to obtain the nickel-zinc-copper ferrite material;

[0091] The mass ratio of the pre-sintered material, deionized water, polyvinyl alcohol, triethanolamine and n-octanol is 100:40:4:0.1:0.001;

[0092] The sintering includes a first heat treatment, a second heat treatment, a first cooling treatment and a second cooling treatment performed in sequence; the specific steps of the first heat treatment include: heating from room temperature to 550°C at a heating rate of 0.5°C / min in an air atmosphere, and keeping the temperature for 7 hours; the specific steps of the second heat treatment include: continuing to heat to 950°C at a heating rate of 1°C / min, and keeping the temperature for 5 hours; the specific steps of the first cooling treatment include: cooling to 605°C at a cooling rate of 2°C / min in an air atmosphere; the specific steps of the second cooling treatment include: continuing to cool to 55°C at a cooling rate of 1°C / min;

[0093] The molding includes molding of a standard sample ring blank; the density of the standard sample ring blank is 3.2g / cm 3 , size is H25*15*10mm.

[0094] Example 3

[0095] The present embodiment provides a nickel-zinc-copper ferrite material, which includes a main component and an auxiliary component; based on the total mass percentage of 100wt%, the main component includes: Fe2O3 66wt%, NiO 12wt%, ZnO18.5wt%, CuO 3.5wt%; based on the total mass percentage of the main component, the auxiliary component includes: Bi2O31.45wt%, Co2O3 0.6wt%, CaCO3 0.08wt%, ZrO2 0.1wt%;

[0096] The total mass percentage of ZnO+CuO in the main component is 22wt%; the total mass percentage of Bi2O3+ZrO2 in the auxiliary component is 1.55wt% of the total mass percentage of the main component.

[0097] The preparation method of the nickel-zinc-copper ferrite material comprises the following steps:

[0098] (1) weighing the main components according to the ratio, and then wet ball milling for 60 minutes, wherein the mass ratio of the main components, zirconium balls and deionized water in the wet ball milling is 1:8:1.2; the obtained ball mill material is pre-calcined at 950° C. for 2 hours after the first spray granulation to obtain a pre-calcined material;

[0099] (2) weighing auxiliary components according to the proportion, and then grinding the auxiliary components, polyvinyl butyral, polyacrylic acid, polyethylene glycol, deionized water and the pre-sintered material obtained in step (1) at a rotation speed of 145 rpm for 10 min and at 270 rpm for 2 h to obtain a grinding material with a median particle size X50 of 0.8 μm and a cumulative percentage of 90% particle size X90 of 1.8 μm; the obtained grinding material is subjected to a second spray granulation to obtain particles with an average particle size of 200 μm, and then formed and sintered in a push-plate kiln to obtain the nickel-zinc-copper ferrite material;

[0100] The mass ratio of the pre-sintered material, deionized water, polyvinyl butyral, polyacrylic acid and polyethylene glycol is 100:150:20:2:0.0025;

[0101] The sintering includes a first heat treatment, a second heat treatment, a first cooling treatment and a second cooling treatment performed in sequence; the specific steps of the first heat treatment include: heating from room temperature to 750°C at a heating rate of 2°C / min in an air atmosphere, and keeping the temperature for 2 hours; the specific steps of the second heat treatment include: continuing to heat to 1050°C at a heating rate of 3°C / min, and keeping the temperature for 2 hours; the specific steps of the first cooling treatment include: cooling to 595°C at a cooling rate of 6°C / min in an air atmosphere; the specific steps of the second cooling treatment include: continuing to cool to 45°C at a cooling rate of 5°C / min;

[0102] The molding includes molding of a standard sample ring blank; the density of the standard sample ring blank is 3.2g / cm 3 , size is H25*15*10mm.

[0103] Example 4

[0104] This embodiment provides a nickel-zinc-copper ferrite material, which is different from Embodiment 1 in that, based on the total mass percentage of 100wt%, the main components are adjusted to: Fe2O3 64.5wt%, NiO 9wt%, ZnO16.5wt%, CuO10wt%, and the total mass percentage of ZnO+CuO is 26.5wt%, and the rest is the same as Embodiment 1.

[0105] Example 5

[0106] This embodiment provides a nickel-zinc-copper ferrite material, which is different from Embodiment 1 in that, based on the total mass percentage of 100wt%, the main components are adjusted to: Fe2O3 66.5wt%, NiO 12wt%, ZnO18.5wt%, CuO3wt%, and the total mass percentage of ZnO+CuO is 21.5wt%, and the rest is the same as Embodiment 1.

[0107] Example 6

[0108] This embodiment provides a nickel-zinc-copper ferrite material, which differs from Embodiment 1 in that, based on the total mass percentage of the main components, the auxiliary components are adjusted to: Bi2O3 0.3wt%, Co2O3 0.1wt%, CaCO3 0.03wt%, ZrO2 0.01wt%, and the total mass percentage of Bi2O3+ZrO2 is adaptively obtained to be 0.31wt% of the total mass percentage of the main components, and the rest are the same as Embodiment 1.

[0109] Example 7

[0110] This embodiment provides a nickel-zinc-copper ferrite material, which differs from Embodiment 1 in that, based on the total mass percentage of the main components, the auxiliary components are adjusted to: Bi2O3 1.5wt%, Co2O3 0.6wt%, CaCO3 0.08wt%, ZrO2 0.1wt%, so that the total mass percentage of Bi2O3+ZrO2 is 1.6wt% of the total mass percentage of the main components, and the rest are the same as Embodiment 1.

[0111] Example 8

[0112] The present embodiment provides a nickel-zinc-copper ferrite material. The preparation method of the nickel-zinc-copper ferrite material is different from that of embodiment 1 in that the sintering in step (2) is adjusted to a heat treatment and a cooling treatment performed sequentially. The specific steps of the heat treatment include: heating from room temperature to 1000° C. at a heating rate of 1.5° C. / min in an air atmosphere, and keeping the temperature for 8 hours; the specific steps of the cooling treatment include: cooling to 50° C. at a cooling rate of 3.5° C. / min in an air atmosphere. The rest are the same as those in embodiment 1.

[0113] Comparative Example 1

[0114] This comparative example provides a nickel-zinc-copper ferrite material, which is different from Example 1 in that, based on the total mass percentage of 100wt%, the main components are adjusted to: Fe2O3 64wt%, NiO 8wt%, ZnO20wt%, CuO 8wt%, and the total mass percentage of ZnO+CuO is 28wt%, and the rest is the same as Example 1.

[0115] Comparative Example 2

[0116] This comparative example provides a nickel-zinc-copper ferrite material, which is different from Example 1 in that, based on the total mass percentage of 100wt%, the main components are adjusted to: Fe2O3 67wt%, NiO 13wt%, ZnO12wt%, CuO 8wt%, and the total mass percentage of ZnO+CuO is 20wt%, and the rest is the same as Example 1.

[0117] Comparative Example 3

[0118] This comparative example provides a nickel-zinc-copper ferrite material, which differs from Example 1 in that, based on the total mass percentage of the main components, the auxiliary components are adjusted to: Bi2O3 0.25wt%, Co2O3 0.05wt%, CaCO3 0.02wt%, ZrO2 0.005wt%, and the total mass percentage of Bi2O3+ZrO2 is adaptively obtained to be 0.255wt% of the total mass percentage of the main components, and the rest are the same as Example 1.

[0119] Comparative Example 4

[0120] This comparative example provides a nickel-zinc-copper ferrite material, which differs from Example 1 in that, based on the total mass percentage of the main components, the auxiliary components are adjusted to: Bi2O3 1.55wt%, Co2O3 0.65wt%, CaCO3 0.1wt%, ZrO2 0.15wt%, and the total mass percentage of Bi2O3+ZrO2 is adaptively obtained to be 1.7wt% of the total mass percentage of the main components, and the rest are the same as Example 1.

[0121] Performance Testing

[0122] The nickel-zinc-copper ferrite materials provided in Examples 1-8 and Comparative Examples 1-4 were tested for inductance using Agilent E4991, and the real and imaginary parts of the magnetic permeability μi were calculated based on the size coefficient. The Curie temperature Tc and the magnetic permeability of each temperature zone were tested using an LCR magnetic material tester and a high and low temperature controllable oven, and the specific temperature coefficient at each temperature was calculated. The results are shown in Table 1.

[0123] The saturation magnetic flux density Bs and residual magnetic flux density Br were tested using the SY8218 instrument produced by Iwasaki Corporation of Japan. The results are shown in Table 1.

[0124] Table 1

[0125]

[0126]

[0127] It can be seen from Table 1 that the nickel-zinc-copper ferrite material provided by the present invention has the advantages of high Curie temperature, high saturation magnetic induction intensity, low residual magnetic induction intensity, low specific temperature coefficient, etc., and can be better applied to power inductors or common-mode inductors;

[0128] By comparing Example 1 with Examples 4-7, it can be seen that when the contents of each main component and auxiliary component are within the specified range, but the total amount of ZnO+CuO or Bi2O3+ZrO2 exceeds the specified range, the magnetic properties of the nickel-zinc-copper ferrite material will be reduced as a whole; by comparing Example 1 with Example 8, it can be seen that sintering as a single heat treatment and cooling treatment will result in a lower magnetic permeability compared to two heat treatments and cooling treatments;

[0129] By comparing Example 1 with Comparative Examples 1-4, it can be seen that when the content of the main component or the auxiliary component exceeds the specified range, and the total amount of ZnO+CuO or Bi2O3+ZrO2 also exceeds the specified range, the saturation magnetic induction intensity and Curie temperature of the nickel-zinc-copper ferrite material will be greatly reduced, and the residual magnetic induction intensity and the specific temperature coefficient will be increased; in addition, the present invention can uniformly grow FeBi2O4 with a spinel structure by adding Bi2O3. 3+ The K1 value is large, so the content of CoFe2O4 in the composition determines the imaginary part of the complex permeability of the nickel-zinc-copper ferrite material to a large extent. Controlling the CoFe2O4 content within a reasonable range can reduce the loss of the ferrite and ensure high permeability performance at high frequencies; when Bi-Ca and nickel-zinc-copper ferrite materials undergo solid-phase reaction, they mainly grow on the grain boundaries, and the Bi2O3 content of the solution is higher than 1.5wt%, which will cause crystallization on the surface of the magnet, thereby causing the magnetic permeability to decrease and the residual magnetic induction intensity to increase.

[0130] In summary, the present invention can obtain a nickel-zinc-copper ferrite material with higher magnetic permeability and Curie temperature by controlling the content range of the main component; in order to ensure high saturation magnetic induction intensity and low specific temperature coefficient characteristics, it is necessary to adjust the overall content of Fe2O3, ZnO, NiO and CuO; by adjusting the auxiliary component Ca 2+ and Bi 3+ The combined substitution of can improve the magnetic permeability and achieve high-frequency charging efficiency; 2+ 、Co 3+ A small amount of substitution can reduce the imaginary part of the magnetic permeability to achieve low loss characteristics; through Ca 2+ 、Co 3+ and Bi 3+ or Zr 4+ The combined substitution can adjust the saturation magnetic induction intensity to achieve the applicability of the device in extreme environments. The nickel-zinc-copper ferrite material prepared by the present invention has high saturation magnetic induction intensity, high magnetic permeability, high Curie temperature, low residual magnetic induction intensity and low specific temperature coefficient, and can be better applied to power inductors or common-mode inductors.

[0131] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A nickel-zinc-copper ferrite material, characterized in that: The nickel-zinc-copper ferrite material includes a main component and an auxiliary component; based on the total mass percentage of 100wt%, the main component includes: Fe2O3 64.5-66.5wt%, NiO 9-12wt%, ZnO 13.5-18.5wt%, CuO 3-10wt%; based on the total mass percentage of the main component, the auxiliary component includes: Bi2O3 0.3-1.5wt%, Co2O3 0.1-0.6wt%, CaCO3 0.03-0.08wt%, ZrO2 0.01-0.1wt%.

2. The nickel-zinc-copper ferrite material according to claim 1, characterized in that: The total mass percentage of ZnO+CuO in the main component is 22-26wt%.

3. The nickel-zinc-copper ferrite material according to claim 1 or 2, characterized in that: The total mass percentage of Bi2O3+ZrO2 in the auxiliary components is 0.35-1.55wt% of the total mass percentage of the main components.

4. A method for preparing the nickel-zinc-copper ferrite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) weighing the main components according to the proportion, and then wet ball milling and mixing, and the obtained ball milled material is pre-calcined after the first spray granulation to obtain a pre-calcined material; (2) weighing auxiliary components according to the ratio, and then sequentially subjecting the auxiliary components, the liquid medium, the additives and the pre-sintered material obtained in step (1) to a first grinding and a second grinding, and the obtained ground material is subjected to a second spray granulation and then molded and sintered to obtain the nickel-zinc-copper ferrite material.

5. The preparation method according to claim 4, characterized in that: The mass ratio of the main component, the ball milling medium and the liquid medium in the wet ball milling mixing of step (1) is 1:(4-8):(0.5-1.2); Preferably, the wet ball milling mixing time in step (1) is 20-60 min; Preferably, the pre-burning temperature in step (1) is 780-950°C; Preferably, the pre-burning time in step (1) is 2-4 hours.

6. The preparation method according to claim 4 or 5, characterized in that: The additives in step (2) include a binder, a dispersant and a defoamer; Preferably, the mass ratio of the pre-burned material, the liquid medium, the binder, the dispersant and the defoamer in step (2) is 100:(40-150):(4-20):(0.1-2):(0.001-0.0025); Preferably, the liquid medium in step (2) comprises deionized water.

7. The preparation method according to any one of claims 4 to 6, characterized in that: Step (2) the first grinding speed is 145-265 rpm; Preferably, the first grinding time in step (2) is 5-10 min; Preferably, the rotation speed of the second grinding in step (2) is 270-320 rpm; Preferably, the second grinding time in step (2) is 0.5-2h; Preferably, the median particle size X50 of the grinding material in step (2) is 0.5-0.8 μm, and the particle size X90 with a cumulative percentage of 90% is 1.25-1.8 μm; Preferably, the average particle size of the particles obtained by the second spray granulation in step (2) is 30-200 μm.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The sintering in step (2) is carried out in a push plate kiln; Preferably, the sintering in step (2) includes a first heat treatment, a second heat treatment, a first cooling treatment and a second cooling treatment performed in sequence.

9. The preparation method according to claim 8, characterized in that: The specific steps of the first heat treatment include: heating to 550-750°C at a heating rate of 0.5-2°C / min in an air atmosphere, and keeping the temperature for 2-7h; Preferably, the specific steps of the second heat treatment include: continuing to heat up to 950-1050°C at a heating rate of 1-3°C / min, and keeping the temperature for 2-5h; Preferably, the specific steps of the first cooling treatment include: cooling to 595-605°C at a cooling rate of 2-6°C / min in an air atmosphere; Preferably, the specific step of the second cooling treatment includes: continuing to cool to 45-55°C at a cooling rate of 1-5°C / min.

10. An application of the nickel-zinc-copper ferrite material according to any one of claims 1 to 3, characterized in that: The nickel-zinc-copper ferrite material is used in power inductors or common-mode inductors.

Citation Information

Patent Citations

  • A NiZnCu ferrite material and preparing method thereof

    CN101552074A

  • Nickel-zinc ferrite material, and preparation method and use thereof

    CN110357610A

  • Nickel-zinc high-permeability material with wide temperature range and low specific temperature coefficient and preparation method of nickel-zinc high-permeability material

    CN112079633A

  • Manganese-zinc ferrite material with wide temperature range, high Bs and low temperature coefficient and preparation method thereof

    CN112194480A

  • Manganese-zinc ferrite material with wide temperature range and low power consumption and preparation method thereof

    CN112408969A

Cited By

  • Nickel-zinc ferrite material as well as preparation method and application thereof

    CN119638396A

  • A nickel-zinc ferrite material and its preparation method and use

    CN119638396B