Method for separating molybdenum from copper, zinc and iron
By extracting the molybdenum reagent MP136 from copper smoke leaching liquid prepared by sodium cellulose, glycerol and EDC, combined with stirring extraction and separation steps, the high impurity content of molybdenum separation in copper smoke was successfully solved, and efficient molybdenum separation and recovery were achieved. The rate reaches 95-99%.
Patent Information
- Application Number
- CN202411085173.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the molybdenum separation method in copper smoke dust has failed to effectively solve the problem of high impurity content, especially in the sulfuric acid leaching system with high acidity, and lacks effective molybdenum extraction reagents and recycling methods.
The copper smoke leaching solution prepared with sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carboyldiimide (EDC) were used as raw materials to extract molybdenum reagent MP136. The extraction and separation steps were carried out by stirring and extraction and separation. It is added to the copper smoke leaching liquid, and anionic composite extractant is used to combine with Mo ions to form a molybdenum-amino chelate, thereby achieving the separation of molybdenum from copper, zinc and iron.
The extraction rate of molybdenum is achieved to reach 95-99%, and the stable performance of the extractant is maintained under high acid and high temperature conditions, effectively reducing the impurity content.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and chemical engineering, and specifically relates to a method for separating molybdenum from copper, zinc and iron. Background Art
[0002] The composition of molybdenum in copper smoke after leaching with sulfuric acid is as follows: In this system, the impurity content is relatively high, such as molybdenum, copper, zinc and iron. The acidity reaches 100-300g / L, and the acidity is high. There is no similar method for separating molybdenum in this system in the literature. Therefore, it is very necessary to develop a molybdenum extraction reagent and recovery method that can solve the above technical problems. Summary of the invention
[0003] The object of the present invention is to provide a method for separating molybdenum from copper, zinc and iron.
[0004] The object of the present invention is achieved in that the method for separating molybdenum from copper, zinc and iron is to add the copper fume leaching solution to extract the molybdenum reagent MP136 to the copper fume leaching solution for stirring, extraction and separation steps, specifically comprising: A. Stirring extraction: adding copper dust leachate extraction molybdenum reagent MP136 to the copper dust leachate to be treated, stirring at a temperature of 20-25°C for 10-30 minutes to obtain material a; the copper dust leachate extraction molybdenum reagent MP136 is prepared from sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) as raw materials; B. Separation: Transfer material a into a separatory funnel and let it stand for 5 to 15 minutes for separation. The aqueous phase and the organic phase are separated to separate molybdenum from copper, zinc and iron.
[0005] The specific operations are as follows: Accurately measure 200ml of copper fume leaching solution with a volume fraction of 20-30% molybdenum extraction reagent (MP136) and 600ml copper fume leaching solution (Mo100mg-5g / L, Zn20g-120g / L, Fe5-30g / L, Cu2-5g / L), transfer them into a 1000ml beaker, stir at 500r / min for 20min at 20-25℃, pour into a separatory funnel, let stand for 10min for separation, separate the aqueous phase and the organic phase, analyze the aqueous phase, the Mo content is 10mg|L, the (Cu, Zn, Fe) content remains unchanged, and the molybdenum extraction rate reaches 95-99%.
[0006] The specific operation of preparing the molybdenum reagent (MP136) extracted from copper dust leaching solution is as follows: Sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl) carbodiimide (EDC) are reacted under pressure at an oxygen pressure of 1.2-1.5 kPa and a temperature of 150-200°C for 1-4 hours, and then filtered and separated to obtain a composite extractant MP136 for extracting molybdenum; wherein the molar ratio of sodium cellulose, glycerol and EDC is 1:2-50:1-15. The extractant has stable extraction performance for molybdenum under high acid and high temperature conditions.
[0007] The technical principle of extracting molybdenum reagent MP136 from copper fume leaching solution of the present invention is: under the dispersing effect of sodium cellulose, -OH in glycerol combines with propyl in 1-ethyl-(3-dimethylaminopropyl)carbodiimide to form anionic valence bonds, i.e. MP136 anionic composite extractant, and Mo ions in the solution combine with anions of MP136 to form molybdenum-amino chelates, thereby achieving separation of molybdenum from copper, zinc, arsenic and antimony in the solution. DETAILED DESCRIPTION
[0008] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0009] The method for separating molybdenum from copper, zinc and iron of the present invention is to add the copper fume leaching solution molybdenum extraction reagent MP136 into the copper fume leaching solution for stirring, extraction and separation steps, which specifically include: A. Stirring extraction: adding copper dust leachate extraction molybdenum reagent MP136 to the copper dust leachate to be treated, stirring at a temperature of 20-25°C for 10-30 minutes to obtain material a; the copper dust leachate extraction molybdenum reagent MP136 is prepared from sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) as raw materials; B. Separation: Transfer material a into a separatory funnel and let it stand for 5 to 15 minutes for separation. The aqueous phase and the organic phase are separated to separate molybdenum from copper, zinc and iron.
[0010] The volume percentage concentration of the molybdenum reagent MP136 extracted from the copper fume leaching solution is 20-30%.
[0011] The amount of the molybdenum reagent MP136 added to the copper fume leaching solution for extracting the molybdenum is 25-35% by volume of the copper fume leaching solution.
[0012] The molar ratio of sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) described in step A is 1:(2-50):(1-15).
[0013] The copper fume leaching solution molybdenum extraction reagent MP136 is prepared by subjecting sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a formulated ratio to a pressure reaction under an oxygen atmosphere.
[0014] The oxygen pressure of the pressurized reaction is 1.2~1.5KPa.
[0015] The temperature of the pressurized reaction is 150-200°C.
[0016] The time of the pressurized reaction is 1 to 4 hours.
[0017] The present invention is further described below with specific implementation cases: Example 1 Cellulose sodium, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:25:8 were pressurized and reacted at an oxygen pressure of 1.2-1.5 KPa and a temperature of 180-200°C for 1 hour, and the copper fume leaching solution molybdenum extraction reagent MP136 was prepared by filtration and separation.
[0018] Example 2 Sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:2:1 were pressurized and reacted for 4 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 150-180°C. The copper fume leaching solution molybdenum extraction reagent MP136 was prepared by filtration and separation.
[0019] Example 3 Sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:50:15 were pressurized and reacted at an oxygen pressure of 1.2-1.5 KPa and a temperature of 160-180°C for 3 hours, and the copper fume leaching solution molybdenum extraction reagent MP136 was prepared by suction filtration and separation.
[0020] Example 4 Sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:10:10 were pressurized and reacted for 2 hours at an oxygen pressure of 1.2-1.5 KPa and a temperature of 170-190°C. The copper fume leaching solution molybdenum extraction reagent MP136 was prepared by suction filtration and separation.
[0021] Example 5 Cellulose sodium, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a molar ratio of 1:35:7 were pressurized and reacted at an oxygen pressure of 1.2-1.5 KPa and a temperature of 170-180°C for 2.5 hours, and the copper fume leaching solution molybdenum extraction reagent MP136 was prepared by filtration and separation.
[0022] Example 6 Accurately measure 200 ml of copper fume leaching solution molybdenum extraction reagent (MP136) prepared in Example 1 with a volume fraction of 20%, and 600 ml of copper fume leaching solution (Mo103.2 mg / L, Zn22.4 g / L, Fe5.6 g / L, Cu2.3 g / L) are transferred into a 1000 ml beaker, stirred at 500 r / min for 10 min at 20-25 ° C, poured into a separatory funnel, and allowed to stand for 5 min for separation. The aqueous phase and the organic phase are separated, and the aqueous phase is analyzed. The Mo content is 8.8 mg|L, the (Cu, Zn, Fe) content remains unchanged, and the molybdenum extraction rate reaches 96.76%.
[0023] Example 7 Accurately measure 100 ml of molybdenum reagent (MP136) for extracting copper fume leaching solution prepared in Example 2 with a volume fraction of 30%, and 350 ml of copper fume leaching solution (Mo4.89 g / L, Zn117.8 g / L, Fe28.87 g / L, Cu4.3 g / L) are transferred into a 1000 ml beaker, stirred at 400 r / min for 30 min at 20-25 ° C, poured into a separatory funnel, and allowed to stand for 15 min for separation. The aqueous phase and the organic phase are separated, and the aqueous phase is analyzed. The Mo content is 13.24 mg|L, the (Cu, Zn, Fe) content remains unchanged, and the molybdenum extraction rate reaches 98.23%.
[0024] Example 8 Accurately measure 150 ml of copper fume leaching solution molybdenum extraction reagent (MP136) prepared in Example 3 with a volume fraction of 25%, and 600 ml of copper fume leaching solution (Mo650 mg / L, Zn60.3 g / L, Fe25.6 g / L, Cu3.84 g / L) are transferred into a 1000 ml beaker, stirred at 600 r / min for 20 min at 20-25 ° C, poured into a separatory funnel, and allowed to stand for 10 min for separation. The aqueous phase and the organic phase are separated, and the aqueous phase is analyzed. The Mo content is 7.65 mg|L, the (Cu, Zn, Fe) content remains unchanged, and the molybdenum extraction rate reaches 96.88%.
[0025] Example 9 Accurately measure 250 ml of copper fume leaching solution molybdenum reagent (MP136) prepared in Example 4 with a volume fraction of 28%, and 500 ml of copper fume leaching solution (Mo3.34 g / L, Zn67.8 g / L, Fe15.6 g / L, Cu3.34 g / L) are transferred into a 1000 ml beaker, stirred at 450 r / min for 25 min at 20-25 ° C, poured into a separatory funnel, and allowed to stand for 30 min for separation. The aqueous phase and the organic phase are separated, and the aqueous phase is analyzed. The Mo content is 9.34 mg|L, the (Cu, Zn, Fe) content remains unchanged, and the molybdenum extraction rate reaches 97.23%.
[0026] Example 10 Accurately measure 200 ml of copper fume leaching solution molybdenum extraction reagent (MP136) prepared in Example 1 with a volume fraction of 26%, and 500 ml of copper fume leaching solution (Mo2.48 g / L, Zn83.3 g / L, Fe17.56 g / L, Cu3.48 g / L) are transferred into a 1000 ml beaker, stirred at 500 r / min for 26 min at 20-25 ° C, poured into a separatory funnel, and allowed to stand for 20 min for separation. The aqueous phase and the organic phase are separated, and the aqueous phase is analyzed. The Mo content is 8.87 mg|L, the (Cu, Zn, Fe) content remains unchanged, and the molybdenum extraction rate reaches 98.24%.
Claims
1. A method for separating molybdenum from copper, zinc and iron, characterized in that: The method for separating molybdenum from copper, zinc and iron is to add the copper dust leaching solution molybdenum extraction reagent MP136 into the copper dust leaching solution for stirring extraction and separation steps, specifically comprising: A. Stirring extraction: adding copper dust leachate extraction molybdenum reagent MP136 to the copper dust leachate to be treated, stirring at a temperature of 20-25°C for 10-30 minutes to obtain material a; the copper dust leachate extraction molybdenum reagent MP136 is prepared from sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) as raw materials; B. Separation: Transfer material a into a separatory funnel and let it stand for 5 to 15 minutes for separation. The aqueous phase and the organic phase are separated to separate molybdenum from copper, zinc and iron.
2. The method for separating molybdenum from copper, zinc and iron according to claim 1, characterized in that: The volume percentage concentration of the molybdenum reagent MP136 extracted from the copper fume leaching solution is 20-30%.
3. The method for separating molybdenum from copper, zinc and iron according to claim 1 or 2, characterized in that: The amount of the molybdenum reagent MP136 added to the copper fume leaching solution for extracting the molybdenum is 25-35% by volume of the copper fume leaching solution.
4. The method for separating molybdenum from copper, zinc and iron according to claim 1, characterized in that: The molar ratio of sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) described in step A is 1:(2-50):(1-15).
5. The method for separating molybdenum from copper, zinc and iron according to claim 1, characterized in that: The copper fume leaching solution molybdenum extraction reagent MP136 is prepared by subjecting sodium cellulose, glycerol and 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) in a formulated ratio to a pressure reaction under an oxygen atmosphere.
6. The method for separating molybdenum from copper, zinc and iron according to claim 5, characterized in that: The oxygen pressure of the pressurized reaction is 1.2~1.5KPa.
7. The method for separating molybdenum from copper, zinc and iron according to claim 5, characterized in that: The temperature of the pressurized reaction is 150-200°C.
8. The method for separating molybdenum from copper, zinc and iron according to claim 5, characterized in that: The time of the pressurized reaction is 1 to 4 hours.
Citation Information
Cited By
A method for recovering molybdenum-containing iron hydroxide and by-product ammonium sulfate from coal direct liquefaction oil residue acid system leach liquor
CN122748722A
A method for recovering molybdenum from coal direct liquefaction oil residue acid system leach liquor
CN122879527A