Article, member, and structure
The article achieves thermal and optical camouflage by manipulating infrared emissivity and visible light reflectance through alternating regions with controlled emissivity and reflectance, addressing the detection challenges of existing technologies.
Patent Information
- Application Number
- JP2024004627
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-01-16
- Publication Date
- 2024-10-30
AI Technical Summary
Existing technologies fail to effectively suppress the reflection of visible light while reducing the emissivity of infrared rays, making objects detectable by both visible light and infrared sensors.
An article with alternating regions having specific emissivity and reflectance characteristics, where the emissivity of infrared rays is 90% or less and reflectance of visible light is 10% or less, with a difference in emissivity and reflectance between adjacent regions of at least 5%, achieved through a metal layer with concavo-convex structures and metal oxide layers.
The article effectively reduces infrared emissivity and visible light reflectance, providing thermal and optical camouflage by minimizing detection from both infrared and visible light sources.
Smart Images

Figure 2024154364000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an article, a component, and a structure. [Background technology]
[0002] Conventionally, techniques for suppressing the reflection of visible light have been known to make vehicles, facilities, people, etc. less discoverable by painting them in a similar color to the background, attaching plants or other objects similar to the background, etc. However, because objects that radiate heat emit a large amount of infrared rays outward, techniques for suppressing the reflection of visible light have been ineffective against radar that captures infrared rays.
[0003] Therefore, Patent Document 1 proposes a plate- or foil-shaped object that has low emissivity for infrared rays and has properties that are adjusted to either absorb most wavelengths of visible light or reflect only light of specific wavelengths at a desired reflectance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-273095 Summary of the Invention [Problem to be solved by the invention]
[0005] The embodiment of Patent Document 1 leaves room for further consideration regarding infrared radiation. Therefore, an object of the present invention is to reduce the infrared emissivity while suppressing the visible light reflectance. [Means for solving the problem]
[0006] The means for solving the above problem is an article having a first region and a second region arranged within the width of the first region, wherein the emissivity of infrared light of a first wavelength in the first region and the second region is 90% or less, the reflectance of visible light of a second wavelength in the first region and the second region is 10% or less, and the difference between the average emissivity (%) for infrared light with a wavelength of 8 μm or more and 13 μm or less in the first region and the average emissivity (%) for infrared light with a wavelength of 8 μm or more and 13 μm or less in the second region is 5% or more. Effect of the Invention
[0007] Provided is a technology that is advantageous in reducing infrared emissivity while suppressing visible light reflectance. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram of an article of the present invention when viewed in plan. [Diagram 2] 1 is a cross-sectional view of a region of an article. [Diagram 3] 1 is a cross-sectional view of a region of a member. [Figure 4] FIG. 1 illustrates a method for manufacturing an article. [Diagram 5] This shows the infrared emissivity spectrum measurement results for each region. [Figure 6] 13 shows the results of measuring the visible light reflectance spectrum of each region. [Figure 7] 1A is an image of the article produced in the example observed in the infrared region, and FIG. 1B is an image of the article produced in the example observed in the visible region. [Figure 8] 1 is a cross-sectional view of a region of a member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiment for carrying out the present invention will be described with reference to the drawings. However, the embodiment described below is one embodiment of the invention, and the present invention is not limited to this. Then, common configurations will be described with mutual reference to multiple drawings, and the description of configurations with common symbols will be omitted as appropriate. Items with the same name but different can be distinguished by adding "No. 0", such as the first item and the second item.
[0010] First Embodiment The article 100 according to this embodiment will be described below with reference to the drawings. FIG. 1 is a schematic diagram of the article 100 according to this embodiment when viewed in plan. The article 100 according to this embodiment is configured to be difficult to radiate infrared rays. For example, by setting the infrared emissivity (hereinafter, high emissivity may be referred to as high heat shielding property) of a certain wavelength (first wavelength) in the entire article 100 to 90% or less, the radiation of infrared rays can be suppressed. If the infrared emissivity exceeds 90%, there is a risk that the infrared rays will be radiated too much and the effect will not be obtained. The article 100 can be applied to any object that radiates infrared rays, and is configured to be able to suppress the radiation of infrared rays well within the above-mentioned range of infrared emissivity. Here, the certain wavelength in the infrared emissivity of a certain wavelength is preferably 6 μm or more, and more preferably a wavelength of 8 μm or more and 13 μm or less.
[0011] The article 100 is composed of a plurality of regions (regions 101, 102, 103, and 104), and each region has a different infrared emissivity. For example, the difference in average emissivity (%) of infrared rays having a wavelength of 8 μm or more and 13 μm or less between the region 101 and the region 102 adjacent to the region 101 is preferably 5% or more. This makes it possible to make the article 100 as a whole less visible to infrared rays, and to create an infrared camouflage state for the article 100 as a whole, thereby enabling an excellent thermal camouflage effect to be exhibited. Furthermore, if it is 10% or more, a greater effect can be exhibited. Also, it is preferably 50% or less, and if it is 30% or less, it is possible to create an infrared camouflage state for the article 100 as a whole, enabling an excellent thermal camouflage effect to be exhibited. The average emissivity of infrared rays having a wavelength of 8 μm or more and 13 μm or less is the average emissivity when infrared rays having wavelengths of 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, and 13 μm are irradiated onto the article 100.
[0012] It is preferable that each region has the same infrared emissivity in a direction different from the vertical and horizontal directions of the article 100. For example, in the case of FIG. 1, it is in a diagonal direction of the article 100. By arranging them in this manner, the article 100 can be made difficult to see, and it is preferable that each region is arranged alternately. In FIG. 1, there are a plurality of regions other than the regions 101 to 104 between each region, but the regions 101 to 104 may be arranged so as to be in contact with each other.
[0013] The shapes of the regions 101 to 104 can be a circle, an ellipse, a polygon such as a rectangle, a diamond, a star, a wave, etc. The shapes of the regions may be the same or may all be different shapes. The area of the regions 101 to 104 is 25 cm 2 More than 10000cm 2 If the shape of the regions 101 to 104 is a rectangle, it is preferable that the vertical length and horizontal length are 5 cm or more and 100 cm or less.
[0014] The article 100 of the present embodiment is preferably configured to be difficult to see with infrared light as well as difficult to see with visible light. For example, by setting the reflectance of visible light of a certain wavelength (second wavelength) in the article 100 (hereinafter, low reflectance may be referred to as high absorbency) to 10% or less, a black-based color scheme that is difficult to see with visible light can be achieved. Furthermore, it is preferable that the reflectance of adjacent regions is different in the visible light region as well as in the infrared region. For example, the difference in the visible light reflectance between the region 101 and the region 102 is preferably 10% or less. Furthermore, the difference in the average reflectance of visible light with a wavelength of 450 nm or more and 650 nm or less is preferably 10% or less. Thereby, the article 100 as a whole can be made difficult to see with visible light, and the article 100 as a whole can be made into a visible light camouflage state. Furthermore, if the reflectance is 5% or less or 3% or less, the article 100 as a whole can be made into a black-based color scheme, and a greater effect can be achieved. The average reflectance of visible light having a wavelength of 450 nm or more and 650 nm or less means the average reflectance when visible light having wavelengths of 450 nm, 500 nm, 550 nm, 600 nm, and 650 nm is irradiated onto the article 100. Here, the certain wavelength in the reflectance of visible light of a certain wavelength (second wavelength) is preferably a visible light wavelength of 400 nm or more and 750 nm or less, more preferably 450 nm or more and 650 nm or less.
[0015] Next, the configuration of the regions 101 to 104 will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view of the region 101. Here, the region 101 will be described as an example, but the regions 102 to 104 can also have a similar configuration.
[0016] The article 100 includes a metal layer 1, one of whose main surfaces includes a relief structure 2. The metal layer 1 further includes a base 11 that forms the surface of the metal layer 1. The material of the metal layer 1 is preferably a metal with high electrical conductivity. Examples of metals with high electrical conductivity include silver, copper, gold, aluminum, magnesium, tungsten, cobalt, zinc, nickel, and chromium, with nickel, zinc, and chromium being preferred, and nickel being particularly preferred. The relief structure 2 provided on the surface of the metal layer 1 is also preferably made of a metal with high electrical conductivity, and more preferably made of the same metal as the base 11 of the metal layer 1.
[0017] The base 11 is a portion in which the metal layer 1 is continuous over the entire region 101, and the concave-convex structure 2 is a portion in which the metal layer 1 is discontinuous over the entire region 101. In Fig. 2, the boundary between the base 11 and the concave-convex structure 2 is indicated by a dashed line.
[0018] The uneven structure 2 includes a first uneven structure 21 and a second uneven structure 22. An object having the uneven structure 2 is an uneven structure, and the uneven structure 2 is a part or the whole of the uneven structure, so the uneven structure 2 can also be called an uneven structure.
[0019] The first uneven structure 21 includes a plurality of convex portions (e.g., convex portion 211 and convex portion 212). The first uneven structure 21 also includes a plurality of concave portions (e.g., concave portion 210 between convex portions 211 and 212). Due to the presence of the first uneven structure 21, the article 100 has an increased infrared emissivity and has a heat-shielding effect. Note that the convex portions 211 and 212 of the first uneven structure 21 are part of the metal layer 1, and the concave portion 210 of the first uneven structure 21 does not necessarily need to have the metal layer 1, and is a space in which a substance other than the metal layer 1 may be present.
[0020] The second uneven structure 22 includes a plurality of convex portions (e.g., convex portion 221 and convex portion 222). The second uneven structure 22 also includes a plurality of concave portions (e.g., concave portion 220 between convex portions 221 and 222). Due to the presence of the second uneven structure 22, the article 100 has a reduced reflectance of visible light, and has a light absorbing effect. Note that the convex portions 221 and 222 of the second uneven structure 22 are part of the metal layer 1, and the concave portion 220 of the first uneven structure 21 does not necessarily need to have the metal layer 1, and is a space in which a substance other than the metal layer 1 may be present.
[0021] The second uneven structure 22 is preferably formed on the upper surface of the first uneven structure 21. In this way, the article 100 has an enhanced light absorbing effect. That is, the second uneven structure 22 is provided on the upper surface of each of a plurality of convex portions (e.g., convex portions 211 and 212) included in the first uneven structure 21. It is preferable that the main components of the metal materials of the first uneven structure 21 and the second uneven structure 22 are the same. By forming the base 11, the first uneven structure 21, and the second uneven structure 22 from a common metal material (i.e., a single-layer metal layer 1), superior light absorbing properties and heat shielding properties can be achieved compared to forming them from different metal materials (i.e., multiple metal layers).
[0022] The metal layer 1, which is the uneven structure in the article 100, has a base 11 made of a metal material having the same main component as the first uneven structure 21 and the second uneven structure 22 under the first uneven structure 21. The base 11 extends continuously under a plurality of convex portions (e.g., convex portions 211 and 212) included in the first uneven structure 21. In contrast, the metal layer 1 of the uneven structure 2 is discontinuous due to the concave portions (e.g., concave portions 210) of the first uneven structure 21 or the concave portions 220 of the second uneven structure 22. That is, the convex portions (e.g., convex portions 211 and 212) of the first uneven structure 21 are discontinuous due to the concave portions 210. Furthermore, the convex portions (e.g., convex portions 221 and 222) of the second uneven structure 22 are discontinuous due to the concave portions 220. Note that the main component in this specification refers to the component having the highest molar content among the components when the material is composed of a plurality of components.
[0023] The average roughness Ra of the first uneven structure 21 is preferably 0.1 μm or more and 5 μm or less, and the average roughness Ra of the second uneven structure 22 is preferably 1 nm or more and 50 nm or less. This makes the effect of providing the first uneven structure 21 and the second uneven structure 22 more remarkable. Here, the first uneven structure 21 and the second uneven structure 22 in the region 101 are described, but it is preferable that the same uneven structure 2 is also provided in the regions 102 to 104. By making the arithmetic mean roughness Ra of at least one of the first uneven structure 21 and the second uneven structure 22 different, the infrared emissivity and the visible light reflectance between the regions 101 to 104 can be changed.
[0024] Here, the average roughness of the concave-convex structure 2, or the average roughness of the concave-convex structure 2 to which a transparent metal oxide described later is attached, refers to the arithmetic average roughness defined in JIS-B-0601, "Definition and display of surface roughness." When only a reference length is cut out from the roughness curve in the direction of the average line, the X-axis is taken in the direction of the average line of the cut-out portion, and the Y-axis is taken in the direction of the longitudinal magnification, and the roughness curve is expressed as y=f(x), it can be calculated by the following formula (1).
[0025]
number
[0026] In formula (1), Ra is the average roughness (nm), L is the reference length, and F(X,Y) is the height at the measurement point (X,Y) where the X coordinate is X and the Y coordinate is Y.
[0027] Furthermore, in the article 100 according to this embodiment, the maximum height Rz of the first uneven structure 21 on the surface of the metal layer 1 is preferably 1 μm or more and 10 μm or less, and the maximum height Rz of the second uneven structure 22 is preferably 100 nm or more and 800 nm or less. In this way, the effects of providing the first uneven structure 21 and the second uneven structure 22 become more pronounced.
[0028] Here, the maximum height of the uneven structure 2, or the maximum height of the uneven structure 2 to which a transparent metal oxide described later is attached, refers to the maximum height specified in "Definition and Display of Surface Roughness" of JIS-B-0601. Only a reference length is cut out from the roughness curve in the direction of the average line, and the distance between the peak line and the valley line of the cut-out portion is measured in the direction of the longitudinal magnification of the roughness curve and calculated. This valley line may correspond to the boundary between the base 11 and the uneven structure 2, shown by the dashed line in FIG. 2. The average roughness Ra and maximum height Rz of the uneven structure 2 can be obtained by observing the cross section of the article 100 of this embodiment with a scanning electron microscope or the like.
[0029] The article 100 of this embodiment includes metal oxide layers 3 and 4 provided on one main surface of a metal layer 1. The metal oxide layers 3 and 4 are not necessarily required to be provided.
[0030] It is preferable that a transparent metal oxide layer 3 is attached to the surface of the concave-convex structure 2. In other words, it is preferable that the article 100 includes a transparent metal oxide layer 3 on the surface of the concave-convex structure, which is the metal layer 1. The metal oxide layer 3 is preferably provided on the entire surface of the concave-convex structure, but it is sufficient that it is provided on at least the convex parts (for example, the convex parts 221 and 222). It is preferable that the metal component of the metal oxide layer 3 attached to the surface of the concave-convex structure 2 is different from the metal component of the metal layer 1. That is, for example, if the material of the metal layer 1 is mainly nickel, the metal oxide layer 3 attached to the surface of the concave-convex structure 2 is mainly an oxide of a metal other than nickel. Therefore, the metal oxide layer 3 attached to the surface of the concave-convex structure 2 can be distinguished from a metal oxide having the same metal component as the metal component of the metal layer 1, which is formed by natural oxidation of the metal layer 1, etc.
[0031] In this specification, the metal oxide layers 3 and 4 may be referred to as metal oxide. The metal oxide layer 3 is provided between a plurality of convex portions (e.g., convex portions 221 and 222) included in the second concave-convex structure 22. In other words, the metal oxide layer 3 is preferably formed in a film shape, filling in the concave portions (e.g., concave portions 220 between convex portions 221 and 222) of the second concave-convex structure 22.
[0032] Furthermore, the article 100 of the present invention may further include a transparent metal oxide layer 4 that covers the surface of the metal oxide layer 3 that is not in contact with the relief structure 2. It is preferable that the metal oxide layer 4 covers the relief structure 2, and that the metal oxide layer 3 is provided between the metal oxide layer 4 and the metal layer 1.
[0033] The material of the metal oxide layer 3 is not particularly limited, but it is preferable that the main component is aluminum oxide, and more preferable that the metal oxide layer 3 contains plate-shaped crystals (hereinafter referred to as plate-shaped crystals) mainly composed of aluminum oxide. The plate-shaped crystals mainly composed of aluminum oxide are formed of crystals mainly composed of aluminum oxide or hydroxide or hydrates thereof, and boehmite is a particularly preferable crystal. Here, the plate-shaped crystals mainly composed of aluminum oxide may be plate-shaped crystals made of aluminum oxide alone, or may be plate-shaped crystals containing aluminum oxide plate-shaped crystals and trace amounts of zirconium, silicon, titanium, zinc, etc.
[0034] In this way, the article 100 can protect the concave-convex structure 2 by including the metal oxide layer 3. When the metal oxide layer 3 is a plate-like structure of plate-like crystals mainly composed of aluminum oxide, it is preferable that the plate-like crystals mainly composed of aluminum oxide are arranged in a direction perpendicular to the plane direction of the metal layer 1, and that their spatial occupancy rate changes continuously.
[0035] The material of the metal oxide layer 4 is not particularly limited, but preferably contains an amorphous gel of aluminum oxide. The metal oxide layer 4 increases the hardness of the surface of the article 100 of the present embodiment while decreasing the light absorbency. Therefore, the thickness of the metal oxide layer 4 may be appropriately determined so as to satisfy the required hardness and light absorbency.
[0036] The aluminum element, silicon element, etc. in the uneven structure 2, the metal oxide layer 3, and the metal oxide layer 4 can be detected by surface measurement using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). They can also be detected by energy dispersive X-ray analysis (EDX) or X-ray photoelectron spectroscopy (XPS) during cross-sectional observation. Similarly, metal elements such as silver, copper, gold, aluminum, magnesium, tungsten, cobalt, zinc, nickel, and chromium in the metal layer 1 can be detected by surface measurement using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). Similarly, silicon element, fluorine element, etc. in the coating layer can be detected by surface measurement using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). They can also be detected by energy dispersive X-ray analysis (EDX) or X-ray photoelectron spectroscopy (XPS) during cross-sectional observation. When the concave-convex structure 2, the metal oxide layer 3, or the metal oxide layer 4 is provided, the proportion of metal oxides such as aluminum elements decreases relatively from the surface (metal oxide layer 4) toward the inside (metal layer 1) in the direction perpendicular to the surface direction of the metal layer 1. Conversely, the proportion of metal elements constituting the metal layer 1 and the concave-convex structure 2 increases relatively from the surface (metal oxide layer 4) toward the inside (metal layer 1), and ultimately only metal elements are detected.
[0037] The article 100 of the present invention includes a coating layer 40 provided on the metal oxide layers 3, 4 and made of a material different from that of the metal oxide layers 3, 4. The metal oxide layer 4 may not be required. As the coating layer 40 that is in contact with the metal oxide layers 3, 4 and made of a material different from that of the metal oxide layers 3, 4, the coating layer 40 preferably contains Si and O, more preferably contains siloxane, and further preferably contains silsesquioxane. In addition to having the coating layer 40 made of the inorganic material described above, the article 100 of the present invention preferably further has a coating layer 40 made of an organic material. As an organic material, the coating layer 40 preferably contains a fluororesin or an acrylic resin. The material of the metal oxide layers 3, 4 is, as described above, for example, aluminum oxide. The coating layer 40 being made of a different material from the metal oxide layers 3, 4 means that the materials are different in that, for example, the metal oxide layers 3, 4 mainly contain Al (aluminum), whereas the coating layer 40 mainly contains Si (silicon) in the inorganic material and mainly contains C (carbon) in the organic material. In this case, it is not that the coating layer 40 does not contain any Al, but rather that when the material of the metal oxide layers 3, 4 is mainly Al, the material of the coating layer 40 is not mainly Al. In this way, it is possible to provide the article 100 with abrasion resistance and weather resistance.
[0038] Silsesquioxane is a compound having a T3 unit structure represented by the formula [R1(SiO1.5)n] (R1 is a functional group, e.g., at least one selected from the group consisting of a polymerizable group, a hydroxyl group, a chlorine atom, an alkyl group having 1 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms), and is a hybrid material of silicon oxide and an organic substance.
[0039] Silsesquioxane (hereinafter sometimes abbreviated as SQ) is a siloxane-based compound whose main chain skeleton is composed of Si-O bonds, and is represented by the composition formula [R1(SiO1.5)n]. In this case, it is preferable that R1 is a polymerizable group, and it is more preferable that R1 is at least one polymerizable group selected from the group consisting of an acryloyl group, a methacryloyl group, an oxetanyl group, and an epoxy group. In this way, it is possible to impart excellent abrasion resistance to the article 100.
[0040] When silsesquioxane plays a role of binding particles composed of a large number of solid substances, it is possible to realize a superior strength while maintaining a high porosity. The silsesquioxane is not particularly limited in the form of a polymer, and examples thereof include known linear polysiloxanes, cage polysiloxanes, and ladder polysiloxanes. The structure of silsesquioxane is a structure in which each silicon atom is bonded to three oxygen atoms, and each oxygen atom is bonded to two silicon atoms (the number of oxygen atoms relative to the number of silicon atoms is 1.5). From the viewpoint of cost, linear polysiloxanes, cage polysiloxanes, and ladder polysiloxanes may be mixed. The suitable thickness of the silsesquioxane layer is 20 nm or more and 180 nm or less, preferably 30 nm or more and 150 nm or less.
[0041] The silsesquioxane is preferably a compound having a polymerizable group (R1 in the above formula) in the molecule and curing by radical polymerization or cationic polymerization. The R1 is preferably at least one polymerizable group selected from the group consisting of an acryloyl group, a methacryloyl group, an oxetanyl group, and an epoxy group. In the silsesquioxane curing by radical polymerization, the R1 may be an acryloyl group or a methacryloyl group. On the other hand, in the type curing by cationic polymerization, the R1 may be an oxetanyl group or an epoxy group. Specifically, the silsesquioxane derivative SQ series (AC-SQ, MAC-SQ, OX-SQ) manufactured by Toa Gosei Co., Ltd. may be mentioned.
[0042] As described above, the article 100 of the present invention preferably has a coating layer 40 of an organic material in addition to having an inorganic coating layer 40 (e.g., a silsesquioxane layer). Examples of materials used for the organic coating layer 40 include fluororesins and acrylic resins. The organic coating layer 40 is preferably formed on the inorganic coating layer 40 (e.g., a silsesquioxane layer) described above. In this way, weather resistance can be imparted to the article 100.
[0043] The coating layer 40 preferably contains a fluoroolefin copolymer (fluoroolefin polymer) as a fluororesin. The fluoroolefin copolymer is a copolymer of a fluoroolefin and another copolymerizable monomer that can be copolymerized with the fluoroolefin. Examples of the fluoroolefin constituting the fluoroolefin copolymer include fluoroolefins having 2 to 3 carbon atoms, such as tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene, vinylidene fluoride, and vinyl fluoride. The ratio of the polymerization unit based on the fluoroolefin in the fluoroolefin copolymer is preferably 20 to 70 mol % in order to provide the coating film with sufficient weather resistance. As the other copolymerizable monomer constituting the fluoroolefin copolymer, a vinyl monomer, that is, a compound having a carbon-carbon double bond, is preferable. Examples of the vinyl monomer include vinyl ether, allyl ether, vinyl carboxylate, allyl carboxylate, and olefin. As the acrylic resin, a known one can be used.
[0044] The coating layer 40 may contain an acrylic resin. The acrylic resin is a resin containing a (meth)acrylic polymer. The content of the (meth)acrylic polymer in the acrylic resin is usually 30% by mass or more, preferably 50% by mass or more, more preferably 70% by mass or more, particularly preferably 90% by mass or more, and most preferably 95% by mass or more. The (meth)acrylic polymer has excellent optical properties such as high light transmittance and low wavelength dependency of the refractive index. The (meth)acrylic polymer is a polymer having a structural unit ((meth)acrylic acid ester unit) derived from a (meth)acrylic acid ester monomer. The content of the (meth)acrylic acid ester unit in the (meth)acrylic polymer is usually preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and particularly preferably 70% by mass or more.
[0045] The (meth)acrylic polymer may have a structural unit other than the (meth)acrylic acid ester unit. Such a structural unit is, for example, a structural unit derived from each monomer of styrene, vinyltoluene, α-methylstyrene, α-hydroxymethylstyrene, α-hydroxyethylstyrene, acrylonitrile, methacrylonitrile, ethylene, propylene, 4-methyl-1-pentene, vinyl acetate, 2-hydroxymethyl-1-butene, methyl vinyl ketone, N-vinylpyrrolidone, and N-vinylcarbazole. The (meth)acrylic polymer may have two or more of these structural units.
[0046] The organic material used for the coating layer 40 is not limited to fluororesin or acrylic resin, and any material having transparency and weather resistance may be used.
[0047] As shown in Fig. 8, the article 100 of the present invention preferably has an ink layer 41 on the metal oxide layer 3. The ink layer 41 is preferably disposed on the outermost layer of the article 100. The ink layer 41 is capable of controlling the infrared emissivity and the visible light reflectance, and also has the function of improving the design of the article 100 by coloring it.
[0048] 8, the ink layer 41 is provided in contact with the metal oxide layer 3, but at least one of the metal oxide layer 4, the coating layer 40 made of an inorganic material, and the coating layer 40 made of an organic material may be provided between the metal oxide layer 3 and the ink layer 41. The ink layer 41 may be provided without the metal oxide 3 therebetween. It is sufficient that the ink layer 41 is provided above at least one of the concave-convex structures 2 in the regions 101, 102, 103, and 104.
[0049] The thickness of the ink layer 41 is preferably smaller than the arithmetic mean roughness Ra of the first uneven structure 21. This makes it easier to achieve both the design provided by the ink layer 41 and the heat insulation property of the first uneven structure 21. The thickness of the ink layer 41 is preferably in the range of 100 nm or more and 1 μm or less.
[0050] The ink layer 41 can be formed using various inkjet inks such as water-based inks, solvent inks, and UV-curable inks, and the embodiment is not limited thereto. Among them, it is preferable to use UV-curable inks. Each component contained in the ink that forms the ink layer 41 will be described in detail below.
[0051] The ink contains a polymerizable compound, a photopolymerization initiator, a colorant, and a solvent, and may contain other desired components.
[0052] [Polymerizable compound] The polymerizable compound (A) contained in the ink is a compound that reacts with a polymerization factor (radical, etc.) generated from the photopolymerization initiator (B) described below, and becomes a cured product formed from a high molecular compound (polymer) through a chain reaction (polymerization reaction).
[0053] The polymerizable compound (A) has a polymerizable functional group. In this specification, the polymerizable functional group refers to a functional group that can be polymerized. The polymerizable functional group of the polymerizable compound (A) is preferably a radically polymerizable polymerizable functional group, and more preferably an ethylenically unsaturated group. Specifically, the polymerizable functional group of the polymerizable compound (A) is particularly preferably an acryloyl group, a methacryloyl group, a vinyl group, an allyl group, or a vinyl ether group.
[0054] The polymerizable compound (A) contained in the ink may be one type of polymerizable compound or multiple types of polymerizable compounds. When multiple types of polymerizable compounds are contained, the blending ratio of the polymerizable compound in the ink is calculated based on the total mass of the multiple types of polymerizable compounds.
[0055] The polymerizable compound (A) is not particularly limited as long as it is a compound having a polymerizable functional group, and can be a monomer, an oligomer, a polymer, a mixture thereof, etc. When a solid polymerizable compound is used, it is preferable to mix it with a liquid polymerizable compound and dissolve the solid polymerizable compound in the liquid polymerizable compound before use.
[0056] The blending ratio of the polymerizable compound (A) in the ink is preferably 30% by mass or more and 90% by mass or less, when the total mass of the ink is 100% by mass. Also, it is more preferably 40% by mass or more and 80% by mass or less. By making the blending ratio of the polymerizable compound (A) in the ink 30% by mass or more relative to the total mass of the ink, the mechanical strength of the formed cured product can be increased.
[0057] [Photopolymerization initiator] The photopolymerization initiator (B) contained in the ink is a compound that senses light (active energy rays) of a predetermined wavelength and generates a polymerization factor (radicals, etc.). Specifically, the photopolymerization initiator is a polymerization initiator that generates a polymerization factor by active energy rays such as light (infrared rays, visible light, ultraviolet rays, far ultraviolet rays, X-rays, charged particle rays such as electron beams, radiation, etc.). More specifically, the photopolymerization initiator (B) preferably contains a polymerization initiator that generates a polymerization factor by light of a wavelength of 150 nm or more and 400 nm or less.
[0058] The photopolymerization initiator contained in the ink may be one type of photopolymerization initiator or multiple types of photopolymerization initiators. When multiple types of photopolymerization initiators are contained, the blending ratio of the photopolymerization initiator in the ink is calculated based on the total mass of the multiple types of photopolymerization initiators.
[0059] The blending ratio of the photopolymerization initiator is preferably from 0.01% to 15% by mass, and more preferably from 0.1% to 10% by mass, when the total mass of the ink is taken as 100% by mass.
[0060] By making the blending ratio of the photopolymerization initiator 0.01% by mass or more based on the total mass of the ink, the ink curing speed can be increased and the reaction efficiency can be improved, and by making the blending ratio 15% by mass or less based on the total mass of the ink, the mechanical strength of the formed cured product can be improved.
[0061] [Coloring Agent] The ink according to the present invention may contain a colorant for achieving a desired reflectance. Examples of the colorant include known pigments and dyes. Examples of the pigment include known pigments such as carbon black, cyan, yellow, and magenta.
[0062] [solvent] Examples of the solvent contained in the ink include organic solvents and water. Specific examples of the solvent include, but are not limited to, water; alcohols such as ethanol, 2-propanol, and butanol; various aliphatic or alicyclic hydrocarbons such as n-hexane, n-octane, cyclohexane, and cyclopentane; various aromatic hydrocarbons such as toluene; various esters such as ethyl formate and ethyl acetate; various ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; various ethers such as dimethoxyethane, tetrahydrofuran, dioxane, and diisopropyl ether; and various chlorinated hydrocarbons such as chloroform, methylene chloride, and carbon tetrachloride. These low-boiling point solvents may be used alone or in combination of two or more.
[0063] The solvent is preferably a liquid that is compatible with the polymerizable compound (A) and the photopolymerization initiator (B). The blending ratio of the solvent in the ink is preferably 10% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 40% by mass or less, when the total mass of the ink is 100% by mass.
[0064] [Other added ingredients] The ink may contain further additive components according to various purposes, within the scope of not impairing the effects of the present invention. Examples of such additive components include surfactants and conductive materials. When the ink contains a surfactant, it is possible to improve the dispersion stability of the colorant dispersed in the ink. When the ink contains a conductive material, it is possible to control the electrical conductivity, thermal conductivity, and electromagnetic wave absorption functions of the article 100.
[0065] The surfactant may be composed of one type of surfactant or may be composed of multiple types of surfactants.
[0066] Examples of the hydrocarbon surfactant include polyoxyalkylene alkyl ethers in which an alkylene oxide having 2 to 4 carbon atoms is added to an alkyl alcohol having 1 to 50 carbon atoms.
[0067] Examples of polyoxyalkylene alkyl ethers include methyl alcohol ethylene oxide adducts, decyl alcohol ethylene oxide adducts, lauryl alcohol ethylene oxide adducts, cetyl alcohol ethylene oxide adducts, oleyl alcohol ethylene oxide adducts, and stearyl alcohol ethylene oxide adducts. When the ink contains a surfactant, the content of the surfactant is preferably, for example, 0.001% by mass or more and 20% by mass or less with respect to the total amount of the ink. More preferably, it is 0.01% by mass or more and 10% by mass or less, and even more preferably, it is 0.1% by mass or more and 10% by mass or less. By setting the content of the surfactant within the above range, the dispersion stability of the droplets 101 can be improved.
[0068] The conductive material may be composed of one type of conductive material, or may be composed of multiple types of conductive materials.
[0069] Examples of the conductive material include carbon nanotubes, carbon nanofibers, graphene, graphite, conductive carbon black, and metal particles or fibers of gold, silver, nickel, aluminum, iron, or the like.
[0070] The means for imparting the electrical conductivity, thermal conductivity, and electromagnetic wave absorption functions to the article 100 is not particularly limited. For example, a layer made of a conductive material or a layer containing a conductive material can be provided on the surface layer of the article 100 within a range that does not impair the effects of the present invention. Also, a layer made of a conductive material or a layer containing a conductive material can be provided on the back surface of the article 100, or a sheet having electrical conductivity can be attached.
[0071] When a layer made of a conductive material or a layer containing a conductive material is provided on the surface layer of the article 100, the thickness of the layer made of the conductive material is preferably in the range of 100 nm to 1 μm inclusive. In this range, it is possible to simultaneously achieve the effect of suppressing the reflectance of visible light, the function of reducing the emissivity of infrared light, and the conductive function.
[0072] In addition, when a layer made of a conductive material or a layer containing a conductive material is provided on the back surface of the article 100, the thickness of the article 100 is preferably in the range of 100 nm to 5 μm. In addition, the thickness of the layer made of a conductive material or the layer containing a conductive material and the conductive sheet-like material is preferably in the range of 50 μm to 5 mm. In this range, it is possible to simultaneously achieve the effect of suppressing the reflectance of visible light, the function of reducing the emissivity of infrared light, and the conductive function.
[0073] [Physical properties of photocurable ink] The viscosity of the ink at 25°C is preferably 1 mPa·s or more and 75 mPa·s or less. Also, the viscosity of the ink is more preferably 1 mPa·s or more and 30 mPa·s or less. By making the ink viscosity 1 mPa·s or more and 75 mPa·s or less, the ejection stability when the ink is ejected by the inkjet method can be improved.
[0074] [Preparation method of photocurable ink] Although the method for preparing the ink is not particularly limited, an example of the method for preparing the ink is shown below. The ink is prepared by stirring and mixing the polymerizable compound (A), the photopolymerization initiator (B), and the colorant.
[0075] When stirring and mixing, a homogenizer, an ultrasonic disperser, an agitator, or the like can be used. Among these, from the viewpoint of preparing a homogenous ink, it is preferable to use a homogenizer or an ultrasonic disperser. As shown in FIG. 3, an embodiment of the member 200 of the present invention is a member 200 in which a substrate 5 is provided on the surface of the metal layer 1 of the article 100 of this embodiment opposite to the uneven structure 2. The member 200 includes the substrate 5 and the article 100 provided on the substrate 5. The shape of the substrate 5 may be any shape that can be formed according to the purpose of use, and may be, for example, a molded product, and may be, for example, a flat plate shape, a film shape, a sheet shape, or the like, but is not limited thereto.
[0076] Materials for the substrate 5 include, but are not limited to, metal, glass, ceramics, wood, paper, and resin. Examples of resins include thermoplastic resins such as polyester, triacetyl cellulose, cellulose acetate, polyethylene terephthalate, polypropylene, polystyrene, polycarbonate, and polymethyl methacrylate. Other examples of thermoplastic resins include ABS resin, polyphenylene oxide, polyurethane, polyethylene, and polyvinyl chloride. Other examples of thermosetting resins include unsaturated polyester resin, phenolic resin, crosslinked polyurethane, crosslinked acrylic resin, and crosslinked saturated polyester resin.
[0077] The article 100 and the base material 5 may be bonded to each other by an adhesive layer. The adhesive layer of the member 200 may be any layer capable of bonding the article 100 and the base material 5 to each other, and examples of the adhesive layer include a layer made of a cured product of an adhesive resin (e.g., an epoxy resin) and a double-sided tape.
[0078] The article according to the present embodiment includes the article 100. The article 100 according to the present embodiment can be provided on the surface of various members or articles. The article 100 according to the present embodiment is preferably used as a heating element having a heating means as a member or article. Examples of articles including such a heating element include a battery, an engine, a motor, and a vehicle. The engine is a reciprocating engine, a rotary engine, a diesel engine, a gas turbine engine, a jet engine, a rocket engine, and the like. The motor is a DC motor, an AC motor, a PM motor, a brush motor, a stepping motor, an induction motor, a servo motor, an ultrasonic motor, an in-wheel motor, a linear motor, and the like. A transport device including at least one of an engine and a motor may include the article 100. The transport device including at least one of an engine and a motor is not limited to various vehicles such as automobiles and trains, but also includes ships, aircraft such as drones, and various robots such as AGVs. The transport device is not limited to passenger transport, but may be for cargo transport, and may be unmanned by remote control or autonomous guidance. A hybrid car is a vehicle including a battery, an engine, and a motor. The article 100 and the member 200 of the present embodiment can be used as a stray light prevention and heat shielding member inside an optical device, or as an interior and exterior member of space-related equipment such as an artificial satellite, and can also be used as an exterior film, a solar collector, etc. In addition, the article 100 of the present embodiment can be used for clothing, etc. The article 100 of the present embodiment may also be used as a heat-shielding decorative film. For example, the article 100 of the present embodiment can be attached as a heat-shielding decorative film to the interior and exterior of a vehicle, a mobile device, a home appliance, a parasol, and a tent. When the article 100 of the present embodiment is provided on the surface of a member or an article, various adhesives can be used. Therefore, the article 100 of the present embodiment can be provided on the surface of a member or an article according to the purpose of use, and the surface of the member and the article is not limited to being smooth, and may have a two-dimensional or three-dimensional curved surface.
[0079] Next, a method for manufacturing the article 100 of this embodiment will be described with reference to FIG. 4. As a method for forming the plurality of regions 101-104 of the article 100 having different infrared emissivity, for example, there is a method for forming the regions by applying an optical camouflage colorant on a sheet having a uniformly controlled infrared emissivity. As the optical camouflage colorant, for example, a pigment such as green, brown, gray, or black having a hue that blends with a natural environment or an artificial environment is preferably used. The optical camouflage colorant is applied to the surface of the sheet having a uniformly controlled emissivity by a method such as inkjet, coating, spray, sublimation transfer, or printing using electrolysis. As a method for forming the plurality of regions 101-104 of the article 100 having different infrared emissivity, a method for forming regions having different roughness on the surface of a base substrate may also be used.
[0080] The manufacturing method described below is one example, and any manufacturing method that can form a plurality of regions 101 to 104 of article 100 with different infrared emissivity can be applied.
[0081] (Step of forming metal oxide layer 3) First, a base substrate 500 is prepared. The base substrate 500 may be a mirror-polished substrate or a substrate surface having a micro-order uneven structure, and may be, for example, ground glass roughened with an abrasive or an etching solution such as acid or alkali, or a substrate processed with an electron beam, but is not limited thereto. A micro-order structure may be formed on a film applied to the surface to form the substrate.
[0082] Thereafter, regions 1001-1004 corresponding to regions 101-104 of article 100 are formed as shown in Fig. 4(a). Regions 1001-1004 are regions with different roughnesses, and are rougher than the surface of base substrate 500. Sandblasting is preferably used as a method for forming regions 1001-1004. The roughness of each region is preferably an average roughness Ra of 0.1 µm or more and 5 µm or less.
[0083] Next, as shown in FIG. 4(b), a film 105 containing aluminum is formed on the surface of the base substrate 500 on which the regions 1001-1004 are formed. Therefore, an uneven structure reflecting the roughness of the regions 1001-1004 is formed on the surface of the film 105. The uneven structure of the film 105 has a plurality of recesses and a plurality of protrusions between the plurality of recesses. The plurality of recesses of the film 105 reflect the plurality of recesses of the substrate 500, and the plurality of protrusions of the film reflect the plurality of protrusions of the substrate 500. Thereafter, the film 105 is altered, so that a metal oxide layer having an uneven structure can be formed on the substrate 500.
[0084] The material of the metal oxide is not particularly limited, but it is preferable that the main component is aluminum oxide. The uneven structure can be formed by a known gas phase method such as chemical vapor deposition (CVD) or physical vapor deposition (PVD), or a liquid phase method using sol-gel. By these methods, it is possible to provide an uneven structure of a metal oxide containing plate-like crystals mainly composed of aluminum oxide. Among them, a method in which an aluminum-containing film is treated with hot water to grow aluminum oxide plate-like crystals is preferable.
[0085] Examples of the aluminum-containing film include an aluminum oxide gel film formed by applying a sol-gel coating liquid containing an aluminum compound, and a film containing metallic aluminum formed by dry film formation such as vacuum deposition or sputtering. From the viewpoints of reactivity and ease of adjusting the height of the metal oxide unevenness structure, it is preferable to form the metal oxide unevenness structure using an aluminum oxide gel film.
[0086] As the raw material for the aluminum oxide gel film, aluminum compounds such as aluminum alkoxides, aluminum halides, aluminum salts, etc. can be used. From the viewpoint of film formability, it is preferable to use aluminum alkoxides.
[0087] Examples of aluminum compounds include aluminum alkoxides such as aluminum ethoxide, aluminum isopropoxide, aluminum n-butoxide, aluminum sec-butoxide, and aluminum tert-butoxide, as well as their oligomers, aluminum halides such as aluminum chloride, aluminum salts such as aluminum nitrate, aluminum acetate, aluminum phosphate, and aluminum sulfate, aluminum acetylacetonate, and aluminum hydroxide.
[0088] The aluminum oxide gel film may also contain other compounds. Examples of the other compounds include alkoxides, halides, and salts of zirconium, silicon, titanium, and zinc, and combinations thereof. By including other compounds in the aluminum oxide gel film, the height of the metal oxide relief structure formed can be increased compared to when the aluminum oxide gel film does not include these compounds.
[0089] The aluminum oxide gel film is formed on the base substrate 500 by applying a sol-gel coating liquid containing an aluminum compound as described below. The sol-gel coating liquid is prepared by dissolving the aluminum compound in an organic solvent. The amount of the organic solvent relative to the aluminum compound is preferably about 20 times by molar ratio.
[0090] As the organic solvent, alcohol, carboxylic acid, aliphatic hydrocarbon, alicyclic hydrocarbon, aromatic hydrocarbon, ester, ketone, ether, or a mixture of these can be used. As the alcohol, for example, methanol, ethanol, 2-propanol, butanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, etc. can be mentioned. Furthermore, 1-propoxy-2-propanol, 4-methyl-2-pentanol, 2-ethylbutanol, 3-methoxy-3-methylbutanol, ethylene glycol, diethylene glycol, glycerin, etc. can be mentioned. As the carboxylic acid, for example, n-butyric acid, α-methylbutyric acid, iso-valeric acid, 2-ethylbutyric acid, 2,2-dimethylbutyric acid, 3,3-dimethylbutyric acid, 2,3-dimethylbutyric acid, 3-methylpentanoic acid, 4-methylpentanoic acid, etc. can be mentioned. Further examples include 2-ethylpentanoic acid, 3-ethylpentanoic acid, 2,2-dimethylpentanoic acid, 3,3-dimethylpentanoic acid, 2,3-dimethylpentanoic acid, 2-ethylhexanoic acid, and 3-ethylhexanoic acid. Examples of aliphatic or alicyclic hydrocarbons include n-hexane, n-octane, cyclohexane, cyclopentane, and cyclooctane. Examples of aromatic hydrocarbons include toluene, xylene, and ethylbenzene. Examples of esters include ethyl formate, ethyl acetate, n-butyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, and ethylene glycol monobutyl ether acetate. Examples of ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Examples of ethers include dimethoxyethane, tetrahydrofuran, dioxane, and diisopropyl ether. Among these, it is preferable to use alcohol in terms of the stability of the sol-gel coating liquid.
[0091] When aluminum alkoxide is used as the aluminum compound, it is highly reactive to water, and therefore the aluminum alkoxide may be rapidly hydrolyzed by the addition of moisture in the air or water, causing the sol-gel coating liquid to become cloudy and precipitate. In order to prevent these, it is preferable to add a stabilizer to the sol-gel coating liquid to stabilize it. As the stabilizer, β-diketone compounds, β-ketoester compounds, alkanolamines, etc. can be used. Examples of β-diketone compounds include acetylacetone, trifluoroacetylacetone, hexafluoroacetylacetone, benzoylacetone, 3-methyl-2,4-pentanedione, 3-ethyl-2,4-pentanedione, etc. Examples of β-ketoester compounds include methyl acetoacetate, ethyl acetoacetate, butyl acetoacetate, hexyl acetoacetate, allyl acetoacetate, benzyl acetoacetate, iso-propyl acetoacetate, etc. Furthermore, examples of acetoacetate-2-methoxyethyl, acetoacetate-sec-butyl, acetoacetate-tert-butyl, acetoacetate-iso-butyl, etc. can be used. Examples of alkanolamines include monoethanolamine, diethanolamine, triethanolamine, etc. The amount of the stabilizer relative to the aluminum alkoxide is preferably about 1:1 in molar ratio.
[0092] A catalyst may be used to promote the hydrolysis reaction of the aluminum alkoxide, and examples of the catalyst include nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, and ammonia.
[0093] In addition, a water-soluble organic polymer compound can be added to the aluminum oxide gel film as necessary. The water-soluble organic polymer compound is easily dissolved from the aluminum oxide gel film by immersion in warm water, which increases the reaction surface area between the aluminum compound and warm water, making it possible to form a concave-convex structure at a low temperature and in a short time. In addition, by changing the type and molecular weight of the organic polymer added, it becomes possible to control the height of the concave-convex structure formed. As the organic polymer, polyether glycols such as polyethylene glycol and polypropylene glycol are preferred because they are easily dissolved from the aluminum oxide gel film by immersion in warm water. The amount of polyether glycols relative to the weight of the aluminum compound in the aluminum oxide gel film is preferably in the range of 0.1 to 10 times by weight.
[0094] (Step of forming metal layer 1) By forming the metal layer 10 on the aluminum-containing film 105 on which the uneven structure is formed, the metal layer 10 having the uneven structure transferred thereto is formed. With reference to FIG. 4(c), the process of forming the metal layer 10 on the film 105 will be described below. As a method for forming the metal layer 10, metal plating is preferred, and electroless plating is more preferred. In the electroless plating process, an aqueous solution in which a palladium compound such as palladium chloride, a gold compound such as gold chloride, a silver compound such as silver chloride, a tin compound such as tin chloride, or the like is dissolved is applied to the film 105 on which the uneven structure is formed, thereby performing activation. The activation may be performed by immersing the uneven structure together with the substrate in an aqueous solution in which a palladium compound is dissolved. Thereafter, the metal layer 10 is deposited on the film 105 on which the uneven structure is formed using an electroless plating solution. The metal layer 10 corresponds to the metal layer 1 of the article 100 of this embodiment, and is preferably an electroless plating solution containing nickel ions, chromium ions, and zinc ions, and particularly preferably a nickel plating solution containing nickel ions. The nickel plating solution may contain phosphorus and boron components in addition to the nickel component. Examples of commercially available nickel plating solutions include the Top Nicoron series from Okuno Chemical Industries. The temperature of the plating solution in the electroless plating process is preferably 30°C or higher and 98°C or lower, more preferably 50°C or higher and 90°C or lower. The time for performing the electroless plating process can be adjusted according to the thickness of the metal layer 10 to be formed, and is usually 30 seconds to 1 hour. In this way, the metal layer 10 is formed so as to fill the gaps in the uneven structure of the film 105, and the metal layer 10 including the uneven structure to which the uneven structure of the film 105 is transferred is formed. At this time, the part located above the apex of the convex part of the uneven structure corresponds to the base 11, and the part located below the apex of the convex part of the uneven structure corresponds to the uneven structure 2. In other words, the metal layer 1 having the base 11, the first uneven structure 21, and the second uneven structure 22 is formed. The metal layer 1 is preferably a plating layer. Moreover, it is preferable that the main component of the metal material of the metal layer 1 including the base 11, the first uneven structure 21, and the second uneven structure 22 is the same.
[0095] It is preferable to perform electroless plating so that the thickness of the metal layer 10 including the uneven structure is 200 nm or more and 15000 nm or less. The metal layer 10 is formed so as to cover the apexes of the convex portions of the uneven structure, and this portion becomes the base 11, so the thickness of the base 11 can be 200 nm or more and 15000 nm or less. In addition, the average height of the second uneven structure 22 in the uneven structure corresponds to the average height of the uneven structure of the film 105, and is 100 nm or more and 1000 nm or less. When the thickness of the metal layer 10 including the uneven structure is 200 nm or more, the article 100 of this embodiment exhibits excellent light absorbing and heat shielding properties.
[0096] After the electroless plating process described above, in order to increase the thickness of the metal layer 10, an electroplating process may be performed on the opposite side of the metal layer 10 from the side on which the concave-convex structure is provided. A known electroplating solution may be used for the electroplating process, and for example, an electroplating solution containing nickel ions, iron ions, copper ions, etc. may be used as metal ions. When the same metal as the metal layer 10 is used for the electroplating process, the thickness of the metal layer 10 can be increased by the electroplating process. When a metal different from the metal layer 10 is used for the electroplating process on the metal layer 10, the metal layer 10 provided by the electroplating process becomes a base material. In addition to inorganic salts that are raw materials for metal ions, conductive salts, salts for adjusting counter ions, carboxylic acid additives for increasing the homogeneity of the plating film, gloss agents, etc. may be added to the electroplating solution as necessary. In addition, in the electroplating process, the temperature, current density, and plating time of the electroplating solution may be adjusted to make the metal layer 10 have a desired thickness. If necessary, prior to the electroplating step, the surface of the metal layer 10 opposite to the surface on which the concave-convex structure is formed may be activated with an aqueous solution containing an acid or the like. Furthermore, in order to improve the quality of the film formed by the electroplating step, a step of removing foreign matter from the electroplating solution may be provided in addition to stirring the electroplating solution during the electroplating step.
[0097] (Etching process) Next, the base substrate 500 is removed to obtain the article 100. FIG. 4(d) shows the state of the base substrate 500 after etching. The surface of the metal layer 10 is provided with a film 105 containing aluminum. When the film 105 is a film containing metallic aluminum, it is necessary to further remove the film containing metallic aluminum by etching because metallic aluminum reflects visible light. When the film 105 is a metal oxide layer (a layer containing amorphous gel of aluminum oxide), the layer containing amorphous gel of aluminum oxide is a metal oxide layer of the light absorbing and heat shielding member. Therefore, the layer containing amorphous gel of aluminum oxide may be removed by etching so as to satisfy the required surface hardness and light absorbing property. As an etching method, wet etching in which a film containing metallic aluminum or a metal oxide layer is dissolved using an acid or an alkaline solution is preferable. Examples of acids include hydrochloric acid, nitric acid, and sulfuric acid. Examples of alkalis include sodium hydroxide and potassium hydroxide. From the viewpoint of work efficiency, an etching method using an alkaline solution is more preferable. The etching concentration is preferably in the range of several percent to several tens of percent, and the etching time is preferably in the range of several hours to several days. The metal layer 10 having the metal oxide attached to the uneven structure also has excellent light absorption properties, and since the strength of the uneven structure can be improved, it also has excellent durability and environmental resistance.
[0098] Residual metal oxide such as aluminum oxide after etching (metal oxide adhering to the concave-convex structure 2) can be detected by EDX or XPS measurement during surface or cross-sectional observation with SEM or TEM.
[0099] As described above, the degree of etching may be adjusted depending on the desired balance between the light absorption performance and surface hardness of the article 100. If necessary, a surface treatment may be performed on the outermost surface of the article 100 for the purpose of improving the mechanical strength. Examples of surface treatment agents include silsesquioxane and fluororesin.
[0100] The article 100 of the present embodiment is preferably used as a heating element as a member or structure. Examples of articles having such a heating element include a battery, an engine, a motor, and a vehicle. The engine is a reciprocating engine, a rotary engine, a diesel engine, a gas turbine engine, a jet engine, a rocket engine, and the like. The motor is a DC motor, an AC motor, a PM motor, a brush motor, a stepping motor, an induction motor, a servo motor, an ultrasonic motor, an in-wheel motor, a linear motor, and the like. A transport device having at least one of an engine and a motor may be provided with an infrared radiation amount control member. The transport device having at least one of an engine and a motor is not limited to various vehicles such as automobiles and trains, but may also be a ship, an aircraft such as a drone, or various robots such as an AGV. The transport device is not limited to passenger transport, but may be for cargo transport, and may be unmanned by remote control or autonomous guidance. A hybrid car is a vehicle equipped with a battery, an engine, and a motor. The article 100 and component 200 of this embodiment can be used as stray light prevention and heat shielding components inside optical equipment, or as interior and exterior components for space-related equipment such as artificial satellites, and can also be used as exterior films, solar collectors, etc.
[0101] In addition, the infrared radiation amount control member of this embodiment can be used for clothing, etc. The infrared radiation amount control member of this embodiment can also be used as a heat-shielding decorative film. For example, the infrared radiation amount control member of this embodiment can be attached as a heat-shielding decorative film to the surface of the interior of a vehicle, a mobile device, a home appliance, a parasol, or a tent. When providing the infrared radiation amount control member of this embodiment on the surface of a member or an article, various adhesives can be used. Therefore, the infrared radiation amount control member of this embodiment can be provided on the surface of a member or an article according to the purpose of use, and the surface of the member or the article is not limited to being smooth, and may have a two-dimensional or three-dimensional curved surface.
[0102] If the thermal camouflage and optical camouflage effects deteriorate significantly due to harsh usage environments, the infrared radiation amount control member of the present invention is in sheet form and can be easily replaced by peeling off the sheet.
[0103] <Example> EXAMPLES Hereinafter, examples of the present invention will be described, but the present invention is not limited to the following examples.
[0104] The infrared emissivity of the examples was evaluated by measuring the reflectance spectrum in the infrared region. A Fourier transform infrared spectrophotometer (FT / IR-6600, manufactured by JASCO Corporation) was used as the measuring device. The emissivity of the product of the present invention was calculated from the reflectance according to the relational equation of the law of conservation of energy and Kirchhoff's law. Since the transmittance of the product of the present invention is about 0%, the emissivity % is a value obtained by subtracting the reflectance % from 100%.
[0105] The evaluation of the reflectance in the visible light region in the examples was carried out by measuring the reflectance spectrum in the visible light region using a lens reflectance measuring device (product name: USPM-RU III, manufactured by Olympus Corporation).
[0106] Example 1 (Preparation of base substrate 500) The surface of the base material 500 made of quartz glass was sandblasted to form elliptical regions 101-104 with different roughness. The elliptical regions 101-104 each have a different roughness. The difference in roughness depends on the type of sand used, and is conventionally expressed by a number called the grit number. For example, grit number 1000 is expressed as #1000. In this embodiment, the grit numbers #800, #600, #400, and #220 were used for the roughness of the regions 101-104, respectively.
[0107] (Production of article 100 and member 200) Aluminum sec-butoxide (hereinafter referred to as "Al(O-sec-Bu) 3An aluminum oxide sol solution was prepared by dissolving ethyl acetoacetate (hereinafter, also referred to as "EtOAcAc") in 2-propanol (hereinafter, also referred to as "IPA") and stirring at room temperature for about 3 hours. The molar ratio of each component in the aluminum oxide sol solution was as follows: Al(O-sec-Bu) 3 : EtOAcAc:IPA = 1:1:20. 0.01M dilute hydrochloric acid aqueous solution was added to the aluminum oxide sol solution, and the additive amount of hydrochloric acid was Al(O-sec-Bu) 3 The aluminum oxide gel film was then added to the aluminum oxide film in a molar ratio of twice that of the aluminum oxide film, and refluxed for about 6 hours to prepare a sol-gel coating liquid. The sol-gel coating liquid was applied by spin coating onto the base material 500, on whose surface elliptical regions 101 to 104 had been formed by sandblasting, to form a coating film. The coating film was then heat-treated at 100°C for 1 hour to obtain a transparent aluminum oxide gel film. Next, the aluminum oxide gel film was immersed in warm water at 80°C for 30 minutes and then dried at 100°C for 10 minutes to form an aluminum oxide layer having an uneven structure.
[0108] An aqueous palladium chloride solution was applied by spin coating onto the aluminum oxide layer having the uneven structure, and then dried at 100°C. Thereafter, the aluminum oxide layer was immersed in a nickel-phosphorus plating solution (phosphorus content: about 1-2 wt%) set at 80°C for 20 minutes to form a nickel layer as the metal layer 1 having the uneven structure and the base 11 therebelow. Thereafter, the article 100 was peeled off from the quartz glass substrate, and an etching process was performed using a 3M aqueous sodium hydroxide solution at room temperature for 50 hours to produce the article 100. The overall thickness of the obtained article 100 was about 10 μm.
[0109] Example 2 A UV ink was prepared by mixing and stirring predetermined amounts of the polymerizable compound (A), photopolymerization initiator (B), solvent, and colorant.
[0110] The UV-curable ink was dropped onto a PET film (Tetron HL92W, manufactured by Teijin DuPont Films) using a micropipette, and then the article obtained in Example 1 was placed on top of the dropwise dropwise dropwise dropwise and filled with ink.
[0111] Next, light emitted from a UV light source equipped with an ultra-high pressure mercury lamp was irradiated for 20 seconds through a diffusion plate and then through the PET film, thereby curing the ink sandwiched between the PET film and the article obtained in Example 1. The irradiated light used had a wavelength of 365 nm and an illuminance of 15 mW / cm. 2 The UV light was used.
[0112] After the light irradiation, the PET film was peeled off, and then the article was left standing at room temperature (25° C.) to form an ink layer on the article obtained in Example 1.
[0113] (Optical properties) FIG. 5 shows the results of infrared emissivity spectrum measurement in the regions 101-104, and FIG. 6 shows the results of visible light reflectance spectrum measurement in the regions 101-104.
[0114] As shown in FIG. 5, article 100 has an infrared emissivity of 90% or less when the wavelength is 6 μm or more, and the difference in emissivity between the respective regions is 5% or more when the wavelength is 6 μm or more.
[0115] As shown in FIG. 6, the article 100 has a visible light reflectance of 10% or less when the wavelength is 400 nm or more and 750 nm or less, and the difference in reflectance between the respective regions is 5% or less when the wavelength is 400 nm or more and 750 nm or less.
[0116] The article on which the ink layer was formed had an infrared emissivity of 90% or less when the wavelength was 6 μm or more, and the difference in emissivity between the respective regions was 5% or more when the wavelength was 6 μm or more.
[0117] Furthermore, the article on which the ink layer was formed had a visible light reflectance of 10% or less when the wavelength was 400 nm or more and 750 nm or less, and the difference in reflectance between the respective regions was 5% or less when the wavelength was 400 nm or more and 750 nm or less.
[0118] (Infrared and visible light visibility by article 100) Fig. 7(a) shows an image of the member 200 of the present invention (Fig. 3) placed on a heater set at 40°C, photographed with an infrared thermography device (model: H2640, manufactured by Nippon Avionics Co., Ltd.). The photographing environment was at room temperature, and the distance between the member 200 and the measuring device was about 40 cm. Since the infrared emissivity of adjacent regions differs, the difference in black and white shading is clearly visible, and it can be seen that the sheet member as a whole exhibits an infrared camouflage effect.
[0119] FIG. 7(b) shows an image of the member 200 of the present invention observed visually (with visible light) in a dark room. The member blended in with the surrounding environment, making it difficult to visually distinguish the pattern of the member.
[0120] The above-described embodiments may be modified as appropriate without departing from the scope of the technical concept. For example, a plurality of embodiments may be combined. In addition, some of the features of at least one embodiment may be deleted or replaced.
[0121] In addition, new matters may be added to at least one embodiment. The disclosure of this specification includes not only what is explicitly described in this specification, but also all matters that can be understood from this specification and the drawings attached to this specification.
[0122] Furthermore, the disclosure of this specification includes the complement of each concept described in this specification. In other words, if this specification contains a statement that "A is greater than B," for example, even if the statement that "A is not greater than B" is omitted, this specification can be said to disclose that "A is not greater than B." This is because when a statement that "A is greater than B" is made, it is assumed that the case in which "A is not greater than B" is taken into consideration.
[0123] The disclosure of the present invention is given below.
[0124] (Configuration 1) An article comprising a first region and a second region disposed within the width of the first region from the first region, wherein the emissivity of infrared light of a first wavelength in the first region and the second region is 90% or less, the reflectance of visible light of a second wavelength in the first region and the second region is 10% or less, and the difference between the average emissivity of infrared light with a wavelength of 8 μm or more and 13 μm or less in the first region and the average emissivity of infrared light with a wavelength of 8 μm or more and 13 μm or less in the second region is 5% or more.
[0125] (Configuration 2) The article described in configuration 1, characterized in that the difference between the average reflectance of the first region for visible light with a wavelength of 450 nm or more and 650 nm or less and the average reflectance of the second region for visible light with a wavelength of 8 μm or more and 13 μm or less is 5% or more.
[0126] (Configuration 3) 3. The article according to claim 1 or 2, wherein a difference between an average reflectance of the first region for visible light having a wavelength of 450 nm or more and 650 nm or less and an average reflectance of the second region for visible light having a wavelength of 450 nm or more and 650 nm or less is 5% or more.
[0127] (Configuration 4) 4. The article according to any one of claims 1 to 3, wherein the first wavelength is 6 μm or longer.
[0128] (Configuration 5) 5. The article according to any one of claims 1 to 4, wherein the first wavelength is greater than or equal to 8 μm and less than or equal to 13 μm.
[0129] (Configuration 6) 6. The article according to any one of claims 1 to 5, wherein the second wavelength is not less than 400 nm and not more than 750 nm.
[0130] (Configuration 7) 7. The article according to any one of claims 1 to 6, wherein the second wavelength is not less than 450 nm and not more than 650 nm.
[0131] (Configuration 8) 8. The article according to any one of claims 1 to 7, wherein the first region and the second region have different shapes.
[0132] (Configuration 9) 9. The article of any one of configurations 1 to 8, wherein a difference between the emissivity of infrared light of the first wavelength in the first region and the emissivity of infrared light of the first wavelength in the second region is 10% or more.
[0133] (Configuration 10) 10. The article of any one of claims 1 to 9, wherein a difference between the emissivity of infrared light of the first wavelength in the first region and the emissivity of infrared light of the first wavelength in the second region is 50% or less.
[0134] (Configuration 11) The area of the first region and the second region is 25 cm 2 More than 10000cm 2 An article according to any one of claims 1 to 10, characterized in that:
[0135] (Configuration 12) 12. The article of any one of configurations 1 to 11, further comprising a third region disposed within a width of the second region, wherein a difference between an average emissivity of the second region for infrared rays having a wavelength of 8 μm or more and 13 μm or less and an average emissivity of the third region for infrared rays having a wavelength of 8 μm or more and 13 μm or less is 5% or more.
[0136] (Configuration 13) The article described in configuration 12, further comprising a fourth region disposed within the width of the third region, wherein the difference between the average emissivity of the third region for infrared rays having a wavelength of 8 μm or more and 13 μm or less and the average emissivity of the fourth region for infrared rays having a wavelength of 8 μm or more and 13 μm or less is 5% or more.
[0137] (Configuration 14) 14. The article according to any one of claims 1 to 13, wherein the arithmetic mean roughness Ra of the first region is different from the arithmetic mean roughness Ra of the second region.
[0138] (Configuration 15) The article described in any one of configurations 1 to 14, characterized in that the first region has a first uneven structure and a second uneven structure on a surface of the first uneven structure and having a smaller arithmetic mean roughness Ra than the first uneven structure, and the second region has a third uneven structure and a fourth uneven structure on a surface of the third structure and having a smaller arithmetic mean roughness Ra than the third uneven structure, and the arithmetic mean roughness Ra of the first uneven structure is different from the arithmetic mean roughness Ra of the third uneven structure and / or the arithmetic mean roughness Ra of the second uneven structure is different from the arithmetic mean roughness Ra of the fourth uneven structure.
[0139] (Configuration 16) The article described in configuration 15, characterized in that the arithmetic mean roughness Ra of the first uneven structure and the third uneven structure is 0.1 μm or more and 5 μm or less.
[0140] (Configuration 17) An article described in structure 15 or 16, characterized in that the arithmetic mean roughness Ra of the second uneven structure and the fourth uneven structure is 1 nm or more and 50 nm or less.
[0141] (Configuration 18) 18. The article of any one of claims 15 to 17, wherein the article has an ink layer on the first region and the second region.
[0142] (Configuration 19) 19. The article of claim 18, wherein the thickness of the ink layer is smaller than the arithmetic mean roughness Ra of the first uneven structure and the arithmetic mean roughness Ra of the third uneven structure.
[0143] (Configuration 20) 20. The article according to claim 18 or 19, wherein the thickness of the ink layer is in the range of 100 nm to 1 μm.
[0144] (Configuration 21) An article described in any one of structures 15 to 20, characterized in that the first uneven structure, the second uneven structure, the third uneven structure, and the fourth uneven structure are formed on the surface of a metal layer containing a metal.
[0145] (Configuration 22) 22. The article of claim 21 further comprising a metal oxide layer overlying the metal layer.
[0146] (Configuration 23) The article according to any one of configurations 1 to 22, characterized in that the article is formed in a film shape.
[0147] (Configuration 24) A member comprising the article according to any one of configurations 1 to 23, the article being provided with a substrate.
[0148] (Configuration 25) A structure comprising a heating element and the article according to any one of configurations 1 to 23, wherein the article insulates against heat from the heating element. [Explanation of symbols]
[0149] 100 goods 101 First area 102 Second area
Claims
1. An article including a first region and a second region disposed within a width of the first region from the first region, the emissivity of infrared light having a first wavelength in the first region and the second region is 90% or less; the reflectance of visible light having a second wavelength in the first region and the second region is 10% or less; An article characterized in that the difference between the average emissivity (%) of the first region for infrared rays with a wavelength of 8 μm or more and 13 μm or less and the average emissivity (%) of the second region for infrared rays with a wavelength of 8 μm or more and 13 μm or less is 5% or more.
2. 2. The article of claim 1, wherein a difference between a reflectance of visible light of the second wavelength in the first region and a reflectance of visible light of the second wavelength in the second region is 10% or less.
3. The article according to claim 1, characterized in that the difference between the average reflectance (%) of the first region for visible light with a wavelength of 450 nm or more and 650 nm or less and the average reflectance (%) of the second region for visible light with a wavelength of 450 nm or more and 650 nm or less is 5% or more.
4. 2. The article of claim 1, wherein the first wavelength is greater than or equal to 6 μm.
5. 2. The article of claim 1, wherein the first wavelength is greater than or equal to 8 μm and less than or equal to 13 μm.
6. The article of claim 1 , wherein the second wavelength is greater than or equal to 400 nm and less than or equal to 750 nm.
7. 2. The article of claim 1, wherein the second wavelength is greater than or equal to 450 nm and less than or equal to 650 nm.
8. The article of claim 1 , wherein the first region and the second region have different shapes.
9. The article of claim 1, wherein the difference between the emissivity (%) of infrared radiation of the first wavelength in the first region and the emissivity (%) of infrared radiation of the first wavelength in the second region is 10% or more.
10. The article of claim 1, wherein a difference between the emissivity (%) of infrared light of the first wavelength in the first region and the emissivity (%) of infrared light of the first wavelength in the second region is 50% or less.
11. The area of the first region and the second region is 25 cm 2 More than 10000cm 2 2. The article of claim 1, wherein:
12. a third region provided within a width of the second region from the second region, The article described in claim 1, characterized in that the difference between the average emissivity (%) of the second region for infrared rays with a wavelength of 8 μm or more and 13 μm or less and the average emissivity (%) of the third region for infrared rays with a wavelength of 8 μm or more and 13 μm or less is 5% or more.
13. a fourth region provided within a width of the third region from the third region; The article described in claim 12, characterized in that the difference between the average emissivity (%) of the third region for infrared rays having a wavelength of 8 μm or more and 13 μm or less and the average emissivity (%) of the fourth region for infrared rays having a wavelength of 8 μm or more and 13 μm or less is 5% or more.
14. 2. The article of claim 1, wherein the arithmetic mean roughness Ra of the first region is different from the arithmetic mean roughness Ra of the second region.
15. The first region includes a first uneven structure and a second uneven structure on a surface of the first uneven structure, the second uneven structure having an arithmetic mean roughness Ra smaller than that of the first uneven structure, the second region is provided with a third uneven structure and a fourth uneven structure on a surface of the third uneven structure, the fourth uneven structure having an arithmetic mean roughness Ra smaller than that of the third uneven structure; An article as described in claim 1, characterized in that the arithmetic mean roughness Ra of the first uneven structure is different from the arithmetic mean roughness Ra of the third uneven structure, and / or the arithmetic mean roughness Ra of the second uneven structure is different from the arithmetic mean roughness Ra of the fourth uneven structure.
16. The article according to claim 15, wherein the first uneven structure and the third uneven structure have an arithmetic mean roughness Ra of 0.1 μm or more and 5 μm or less.
17. The article described in claim 15, characterized in that the arithmetic mean roughness Ra of the second uneven structure and the fourth uneven structure is such that the arithmetic mean roughness Ra of the second uneven structure 22 is 1 nm or more and 50 nm or less.
18. The article of claim 15, wherein the article has an ink layer over the first region and the second region.
19. The article according to claim 18, wherein a thickness of the ink layer is smaller than an arithmetic mean roughness Ra of the first uneven structure and an arithmetic mean roughness Ra of the third uneven structure.
20. 20. The article of claim 18, wherein the ink layer has a thickness in the range of 100 nm to 1 μm.
21. The article according to claim 15, wherein the first uneven structure, the second uneven structure, the third uneven structure, and the fourth uneven structure are formed on a surface of a metal layer containing a metal.
22. 22. The article of claim 21, further comprising a metal oxide layer overlying the metal layer.
23. The article according to claim 1 , wherein the article is formed into a film.
24. A member comprising the article according to any one of claims 1 to 23, the article being provided with a substrate.
25. A heating element and an article according to any one of claims 1 to 23, A structure in which the article insulates against heat from the heat generating body.
Citation Information
Patent Citations
Infrared ray radiation suppressor, using method thereof and infrared ray stealthy device
JP1994273095A
Cited By
Colored heat shielding member, article, and method for manufacturing colored heat shielding member
WO2026221019A1
Light-absorbing heat-shielding film, colored heat-shielding member, article, and method for manufacturing colored heat-shielding member
WO2026221021A1