Method for dividing workpiece
A laser-based method forms a division start point inside the workpiece and uses a low-thermal-conductivity fixing member to achieve reliable and efficient division of silicon chips, ensuring flat end surfaces and reducing processing time and waste.
Patent Information
- Application Number
- JP2023068393
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing methods for dividing silicon chips used as optical waveguides face challenges in achieving near-mirror flatness of end faces due to unevenness and require costly expanding devices or thermally expandable resin sheets, which are less effective and increase processing time and waste.
A method involving a laser beam to form a division start point inside the workpiece, followed by fixing a member with lower thermal conductivity to the opposite surface and heating to propagate cracks along the thickness direction, using a plate material or resin film as a fixing member.
This method enables reliable division with higher performance and reduced mechanical load, resulting in flat end surfaces and decreased processing time and waste, compared to using expanding devices or thermally expandable resin sheets.
Smart Images

Figure 2024154536000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for dividing a plate-shaped workpiece having one surface and another surface located opposite to the one surface. [Background technology]
[0002] Silicon chips are sometimes used as optical waveguides in optical communication devices. For example, silicon chips are manufactured by dividing a disk-shaped workpiece having a silicon single crystal substrate into multiple pieces.
[0003] When a silicon chip is used as an optical waveguide, light enters the inside of the silicon chip from the end face exposed by splitting. Since unevenness on the end face leads to optical loss, it is desirable for the end face of the silicon chip to be as flat as a mirror surface. Therefore, various methods have been devised to split the workpiece so that an end face with a flatness close to that of a mirror surface is formed.
[0004] As a method for dividing a workpiece, a method is known in which a modified layer is formed inside the workpiece, and then the workpiece is divided from the modified layer as a starting point. Specifically, a modified layer is first formed inside the workpiece along a planned dividing line set on one side of the workpiece using a pulsed laser beam having a wavelength that penetrates the workpiece (see, for example, Patent Document 1).
[0005] Next, an expanding device is used to pull the adhesive tape attached to the workpiece to expand the adhesive tape and apply an external force to the workpiece, which divides the workpiece into silicon chips using the modified layer as the starting point for division (see, for example, Patent Document 2).
[0006] However, the use of an expanding device increases the manufacturing cost accordingly. Therefore, a cheaper method for dividing the workpiece has been sought. As an alternative dividing method to the expanding device, a dividing method using a thermally expandable resin sheet has been proposed (for example, see Patent Document 3).
[0007] Specifically, a modified layer is formed inside the workpiece along the planned dividing line, and then an external force is applied to the workpiece to divide it by thermally expanding a thermally expandable resin sheet made of a resin material having a larger thermal expansion coefficient than the workpiece.
[0008] However, when an attempt is made to divide a workpiece by thermally expanding a resin sheet, it is more difficult to divide the workpiece than when an expanding device is used. Therefore, in order to divide the workpiece more reliably, it is necessary to form multiple modified layers in the workpiece so that they overlap in the thickness direction of the workpiece.
[0009] However, in the region where the modified layer is formed, the crystallinity changes (for example, from single crystal phase to amorphous phase) due to multiphoton absorption that occurs during laser processing, so the region where the modified layer is formed does not become a mirror surface on the end face of the above-mentioned silicon chip.
[0010] In other words, the more the number of overlapping modified layers in the thickness direction of the workpiece increases, the smaller the mirror surface area at the end face, i.e., the smaller the area that functions as the light inlet. In addition, the more the number of modified layers increases, the longer the time required for laser processing. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2002-192370 A [Patent Document 2] JP 2011-166002 A [Patent Document 3] JP 2014-086611 A Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention has been made in consideration of these problems, and aims to provide a new dividing method that can divide a workpiece more reliably than when a heat-expandable resin sheet is thermally expanded. [Means for solving the problem]
[0013] According to one aspect of the present invention, there is provided a method for dividing a plate-shaped workpiece having one side and another side located opposite to the one side, the method comprising: a division starting point forming step of forming a division starting point inside the workpiece by positioning a focal point of a laser beam having a wavelength that transmits through the workpiece inside the workpiece closer to the one side than the other side, and relatively moving the focal point and the workpiece along a planned division line set on the one side or the other side; a fixing step of fixing a fixing member having a lower thermal conductivity or linear thermal expansion coefficient than the workpiece to the other side of the workpiece after the division starting point forming step; and a dividing step of heating the workpiece to expand it and propagating a crack from the division starting point along the thickness direction of the workpiece, thereby dividing the workpiece along the planned division line with the fixing member fixed to the other side as a fulcrum.
[0014] Preferably, the fixing member has a plate material, and in the fixing step, the plate material and the workpiece are fixed together via an adhesive layer.
[0015] Preferably, the fixing member has a resin film, and in the fixing step, the film is fixed to the workpiece by closely contacting the other surface of the workpiece without an adhesive layer. Preferably, the fixing member has heat shrinkability.
[0016] Also, preferably, in the dividing step, the workpiece is heated and the fixing member is cooled. Effect of the Invention
[0017] In a method for dividing a workpiece according to one aspect of the present invention, a dividing start point is first formed inside the workpiece closer to one surface than the other surface (dividing start point forming step), and then a fixing member having a smaller thermal conductivity or linear thermal expansion coefficient than the workpiece is fixed to the other surface of the workpiece (fixing step).
[0018] After the fixing process, the workpiece is heated and expanded to cause a crack to propagate from the starting point of the division along the thickness direction of the workpiece, thereby dividing the workpiece along the intended division line using the fixing member fixed to the other surface as a fulcrum (division process).
[0019] Therefore, the workpiece can be divided more reliably than when an external force is applied to the workpiece by thermally expanding a thermally expandable resin sheet. Furthermore, by using this dividing method, even though no mechanical load is applied to the workpiece, a higher dividing performance can be achieved than when an expanding device that applies a mechanical load is used. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a flow diagram of a method for dividing a workpiece. [Diagram 2] FIG. 11 is a perspective view showing a division start point forming step. [Diagram 3] FIG. 11 is a partial cross-sectional side view showing a division start point forming step. [Figure 4] FIG. [Diagram 5] FIG. 11 is a partial cross-sectional side view showing heating of the workpiece in a dividing step. [Figure 6] 11 is a partial cross-sectional side view showing a state in which a crack has propagated to a second surface in a dividing step. FIG. [Figure 7] 1 is a partially sectional side view showing the workpiece divided in a dividing step. FIG. [Figure 8] Figure 8(A) is a photograph showing the end surface of a silicon chip obtained by dividing a workpiece on which two modified regions have been formed using the dividing method of this embodiment, and Figure 8(B) is a photograph showing the end surface of a silicon chip obtained by dividing a workpiece on which six modified regions have been formed using an expanding device. [Figure 9] FIG. 11 is a partial cross-sectional side view showing a modified example of the division start point forming step. [Figure 10] FIG. 11 is a partial cross-sectional side view showing a modified example of the dividing step. [Figure 11] 13 is a partial cross-sectional side view showing a fixing step according to the second embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] (First embodiment) An embodiment according to one aspect of the present invention will be described with reference to the accompanying drawings. Fig. 1 is a flow diagram of a method for dividing a workpiece 11 (see Fig. 2). In this embodiment, each step is performed in the order of a division start point forming step S10, a fixing step S20, and a dividing step S30.
[0022] First, a disk-shaped (i.e., plate-shaped) workpiece 11 to be processed in the division starting point forming step S10 will be described with reference to Fig. 2. The workpiece 11 in this embodiment is a silicon single crystal substrate (i.e., a silicon wafer), and in particular, is a mirror wafer on which no devices or the like are formed.
[0023] However, the workpiece 11 is not limited to a silicon single crystal substrate. One or more thin films and / or one or more layers may be formed on the workpiece 11 to the extent that they do not hinder cleavage of the workpiece 11. A device may be formed on the workpiece 11.
[0024] The workpiece 11 has a first surface (i.e., one surface) 11a and a second surface (i.e., the other surface) 11b, each of which is substantially circular. The first surface 11a and the second surface 11b are located on opposite sides in a thickness direction 11c of the workpiece 11.
[0025] The thickness direction 11c is, for example, a direction perpendicular to the first surface 11a and the second surface 11b under normal temperature and pressure. However, when the workpiece 11 is heated by a heat source disposed at a position closer to the first surface 11a than to the second surface 11b, the thickness direction 11c may be regarded as a direction perpendicular to the second surface 11b, which has a relatively small amount of thermal deformation.
[0026] A plurality of planned division lines 15 (see FIG. 3) are set on the first surface 11a, each arranged along a predetermined direction. In FIG. 3, the planned division lines 15 are indicated by black dots. Note that the planned division lines 15 in this embodiment are not drawn on the first surface 11a, but are imaginary straight lines that are appropriately determined according to the shape, size, etc. of the workpiece 11.
[0027] However, the planned division lines 15 may be drawn on the first surface 11a. The planned division lines 15 may be set on the second surface 11b instead of the first surface 11a. In this embodiment, ten planned division lines 15 are arranged parallel to each other along a predetermined direction (X-axis direction in FIG. 3). In another example, the multiple planned division lines 15 may be arranged in a lattice pattern on the first surface 11a.
[0028] The diameter of the workpiece 11 in this embodiment is, for example, about 200 mm to 300 mm, and the thickness from the first surface 11a to the second surface 11b is, for example, about 300 μm. However, the diameter and thickness of the workpiece 11 are not limited to this example.
[0029] A protective tape 13 for protecting the first surface 11a is attached to the first surface 11a of the workpiece 11. The protective tape 13 has a laminated structure of, for example, a resin base layer and an adhesive layer (glue layer) formed of a resin adhesive.
[0030] The adhesive layer side of protective tape 13 is attached to first surface 11a of workpiece 11. First surface 11a side of workpiece 11 is suction-held by chuck table 4 via protective tape 13.
[0031] Next, the laser processing device 2 will be described with reference to Fig. 2. Note that the X-axis direction (processing feed direction), Y-axis direction (indexing feed direction), and Z-axis direction (height direction, vertical direction) shown in Fig. 2 are mutually orthogonal.
[0032] The chuck table 4 has a disk-shaped frame made of metal. A disk-shaped recess having a smaller diameter than the frame is formed in the upper part of the frame, and a disk-shaped porous plate made of porous ceramics is fixed in the recess.
[0033] The frame has a predetermined flow path (not shown) for supplying negative pressure to the porous plate. A suction source (not shown) such as a vacuum pump is connected to the frame via a pipe (not shown), and negative pressure is transmitted from the suction source to the porous plate via the predetermined flow path.
[0034] The upper surface of the porous plate and the upper surface of the frame are substantially flush with each other, and function as a holding surface that suction-holds the workpiece 11. A rotation drive mechanism (not shown) that rotates the chuck table 4 around a rotation axis substantially parallel to the Z-axis direction is provided below the chuck table 4.
[0035] The rotary drive mechanism includes, for example, a rotor and a stator. In this case, the chuck table 4 is fixed to the rotor and rotates together with the rotor. Alternatively, the rotary drive mechanism may include a motor, a driving pulley, a driven pulley, and an endless belt wound around the driving pulley and the driven pulley. In this case, the chuck table 4 is fixed to the driven pulley and rotates together with the driven pulley.
[0036] The chuck table 4 and the rotation drive mechanism are configured to be moved along the X-axis direction by a ball screw type X-axis direction moving mechanism (not shown), and to be moved along the Y-axis direction by a ball screw type Y-axis direction moving mechanism (not shown).
[0037] A laser beam irradiation unit 6 for irradiating a laser beam L toward a workpiece 11 held on the holding surface is provided above the chuck table 4. The laser beam irradiation unit 6 has a cylindrical housing 8 whose longitudinal direction is arranged along the Y-axis direction.
[0038] The housing 8 is configured to move along the Z-axis direction by a ball screw type Z-axis direction moving mechanism (not shown). The inside of the housing 8 forms a path through which the pulsed laser beam L passes.
[0039] The laser beam L is emitted from a laser oscillator (not shown) having a laser medium such as an Nd:YAG crystal. The laser oscillator includes an excitation light source such as a lamp that irradiates the laser medium with excitation light, and a Q switch that controls the timing at which the laser beam L is emitted.
[0040] The laser beam L has a wavelength that transmits through the workpiece 11, and in this embodiment where the workpiece 11 is a silicon single crystal substrate, the wavelength of the laser beam L is 1342 nm. However, the wavelength used is appropriately changed depending on the material constituting the workpiece 11.
[0041] A head unit 10 is fixed to the tip of the housing 8. Inside the head unit 10, a mirror (not shown) and a condenser lens (not shown) are arranged along the Z-axis direction.
[0042] The laser beam L has its traveling direction changed by a mirror, passes through a condenser lens, and is then irradiated onto the workpiece 11. At this time, the laser beam L is condensed by the condenser lens so as to be condensed to approximately one point inside the workpiece 11.
[0043] A microscope camera unit 12 for taking an image of the first surface 11a side and setting a planned division line 15 (see FIG. 3) is provided on the side of the housing 8. The microscope camera unit 12 has an objective lens, a light source, and an image sensor, all of which are not shown.
[0044] For example, the light source has an LED (Light Emitting Diode) capable of emitting infrared light, and the imaging element has an image sensor (a CCD (Charge-Coupled Device) image sensor or a CMOS (Complementary Metal-Oxide-Semiconductor) image sensor) capable of photoelectrically converting infrared light reflected by the first surface 11a.
[0045] In addition, when the planned dividing line 15 is set on the second surface 11b of the workpiece 11, an LED capable of emitting light having a wavelength in the visible light band instead of infrared light is used as the light source, and an image sensor capable of photoelectrically converting visible light is used as the imaging element.
[0046] Fig. 2 is a perspective view showing the division start point forming step S10. Fig. 3 is a partially sectional side view showing the division start point forming step S10, in which the workpiece 11 and the protective tape 13 are shown in a cross section taken along line AA in Fig. 2.
[0047] In the division start point forming step S10, first, the workpiece 11 is suction-held on the holding surface of the chuck table 4 via the protective tape 13. At this time, the second surface 11b of the workpiece 11 is exposed upward. Then, the orientation of the chuck table 4 is adjusted so that the planned division line 15 is approximately parallel to the X-axis direction.
[0048] Next, with the focal point P (see Figure 3) of the laser beam L positioned at a depth position closer to the first surface 11a than the second surface 11b (i.e., inside the workpiece 11), the focal point P and the workpiece 11 are moved relatively at a predetermined speed along each planned division line 15.
[0049] In this embodiment, with the focal point P on the workpiece 11 fixed at a first depth, the chuck table 4 is moved along the X-axis direction at a predetermined processing feed speed so that the focal point P moves from one end of one planned division line 15 in the X-axis direction to the other end (first pass).
[0050] As a result, a modified region 17 is formed along one of the planned division lines 15 inside the workpiece 11. The crystallinity of the modified region 17 has changed due to multiphoton absorption. The modified region 17 is a weaker region than a region not irradiated with the laser beam L, and functions as a division starting point in the division step S30.
[0051] Next, the chuck table 4 is indexed and moved along the Y-axis direction by a predetermined index amount, and the laser beam L is similarly irradiated along another planned division line 15 adjacent to the scanned planned division line 15 in the Y-axis direction to form a modified region 17.
[0052] In this manner, modified regions 17 are formed at the first depth along all of the planned division lines 15. Thereafter, the light focusing point P is positioned at a second depth that is closer to the second surface 11b than the first depth, and modified regions 17 are formed similarly along all of the planned division lines 15 (second pass).
[0053] However, when first forming a modified region 17 at the second depth and then forming a modified region 17 at the first depth, when forming the modified region 17 at the first depth, the laser beam L is scattered by the modified region 17 at the second depth that was previously formed, making it difficult to form the modified region 17 at the first depth.
[0054] In contrast, in the present embodiment, first, the modified region 17 is formed at a first depth, and then the modified region 17 is formed at a second depth that is closer to the head portion 10 than the first depth, thereby reducing scattering of the laser beam L when forming the modified region 17 at the first depth.
[0055] A crack 19 extends from each modified region 17 along the thickness direction 11c of the workpiece 11. In the example shown in Fig. 3, a crack 19 is formed from the modified region 17 at the first depth to reach the first surface 11a.
[0056] The modified region 17 of the first depth and the modified region 17 of the second depth are connected by a crack 19. Furthermore, a crack 19 is formed from the modified region 17 of the second depth, which does not reach the second surface 11b and stops extending inside the workpiece 11. An example of processing conditions used in the split start point forming step S10 of this embodiment is shown below.
[0057] Wavelength: 1342nm Average power output: 1.0W Repetition frequency: 90kHz Machining feed speed: 600mm / s Number of passes: 2 Focus point depth position: the first depth is 40 μm from the first surface 11a (first pass) The second depth is 100 μm from the first surface 11a (second pass)
[0058] The number of passes means the number of times that the light-collecting point P moves from one end to the other end (or from the other end to one end) of one of the planned division lines 15. In this embodiment, the number of passes is set to 2 as described below, but the number of passes may be set to 1.
[0059] The depth position at which the modified region 17 is formed is closer to the first surface 11a than to the second surface 11b, that is, is set between a position halfway through the thickness of the workpiece 11 and the first surface 11a.
[0060] More preferably, in order to start the division from the first surface 11a, the depth position at which the modified region 17 is formed is set between a depth position that is 1 / 3 of the thickness of the workpiece 11 starting from the first surface 11a and the first surface 11a.
[0061] After the division starting point forming step S10, a fixing step S20 is performed in which a plate material (fixing member) 23 is fixed to the second surface 11b of the workpiece 11 via an adhesive layer 21 (see FIG. 4). FIG. 4 is a partially cross-sectional side view showing the fixing step S20. The plate material 23 has a square shape with one side longer than the diameter of the workpiece 11.
[0062] In the fixing step S20, first, the workpiece 11 is placed on the support table 18 so that the protective tape 13 is in contact with the substantially flat support surface 18a. Next, the first surface 23a of the plate material 23 having the resin adhesive layer 21 provided on the first surface 23a is pressed against the second surface 11b of the workpiece 11.
[0063] This forms a workpiece unit 25 in which the protective tape 13, the workpiece 11, and the plate material 23 are integrated together. The adhesive layer 21 is formed of an ultraviolet curing resin, wax, etc. The ultraviolet curing resin has adhesiveness before being irradiated with ultraviolet rays, but almost loses its adhesiveness after being irradiated with ultraviolet rays.
[0064] Since the plate material 23 is eventually removed from the workpiece 11 after division, it is preferable to use an ultraviolet curing resin in order to reduce the residue of the adhesive layer 21 on the workpiece 11. However, the material of the adhesive layer 21 is not particularly limited as long as the present embodiment can be implemented.
[0065] The plate material 23 has a smaller thermal conductivity than the workpiece 11, or a smaller linear thermal expansion coefficient than the workpiece 11. The plate material 23 of the present embodiment is made of polyethylene terephthalate (hereinafter abbreviated as PET), and has a smaller thermal conductivity than the workpiece 11 which is made of a silicon single crystal substrate.
[0066] The thermal conductivity of PET is 0.2 [Wm -1 K -1 ] to 0.3 [Wm -1 K -1 In contrast, the thermal conductivity of a silicon single crystal substrate is approximately 160 [Wm -1 K -1 ] and 80 [Wm -1 K -1 ].
[0067] That is, PET is less resistant to heat transfer than a silicon single crystal substrate. Therefore, when workpiece unit 25 is heated in a state in which workpiece 11 is disposed closer to the heat source than plate material 23, workpiece 11 begins to expand before plate material 23 begins to thermally expand.
[0068] However, the linear thermal expansion coefficient of PET is approximately 6.5×10 at 300K. -5 [K -1 ], and the linear thermal expansion coefficient of a silicon single crystal substrate is approximately 2.6 × 10 at 300 K. -6 [K -1 ], approximately 3.6 × 10 at 500 K -6 [K -1 In other words, the linear thermal expansion coefficient of PET is greater than that of the silicon single crystal substrate.
[0069] However, in the subsequent dividing step S30, the workpiece 11 is disposed closer to the heat source than the plate material 23. Furthermore, since the resin adhesive layer 21 is provided between the workpiece 11 and the plate material 23, the temperature rise rate of the plate material 23 becomes slower than when the plate material 23 is in direct contact with the workpiece 11.
[0070] Therefore, if the thermal conductivity of the plate material 23 is smaller than that of the workpiece 11, the thermal expansion of the workpiece 11 begins sufficiently earlier than the start of thermal expansion of the plate material 23, and cleavage of the workpiece 11 proceeds starting from the modified region 17.
[0071] The plate material 23 may be made of diamond. The thermal conductivity of diamond is about 1000 [Wm -1 K -1 ] to about 2000 [Wm -1 K -1 ], which is significantly greater than the thermal conductivity of a silicon single crystal substrate, so heat is transferred more easily through it than through a silicon single crystal substrate.
[0072] However, the linear thermal expansion coefficient of diamond is about 1.0×10 at 300K. -6 [K -1], which is smaller than the linear thermal expansion coefficient of the silicon single crystal substrate. Therefore, no matter how much heat is transferred to the diamond plate 23 through the silicon single crystal substrate, the thermal expansion of the plate 23 does not pose any problem.
[0073] In contrast, if the plate material 23 has a thermal conductivity greater than that of the workpiece 11 and a linear thermal expansion coefficient greater than that of the workpiece 11, the plate material 23 may thermally expand to the same extent as the workpiece 11 or greater than that of the workpiece 11.
[0074] The plate material 23 is positioned on the second surface 11b side of the workpiece 11, and the modified region 17 is formed on the first surface 11a side rather than the second surface 11b. Therefore, if the plate material 23 undergoes thermal expansion equal to or greater than that of the workpiece 11, cleavage of the workpiece 11 starting from the modified region 17 is unlikely to proceed.
[0075] Therefore, when the plate material 23 is made of a material such as silver (Ag), copper (Cu), or gold (Au), which has a higher thermal conductivity and a higher linear thermal expansion coefficient than a silicon single crystal substrate, the plate material 23 is less able to perform the function of fixing the workpiece 11.
[0076] In contrast, in the present embodiment, deformation of the plate material 23 is substantially suppressed, so that the plate material 23 fixes the second surface 11b side of the workpiece 11, and spontaneous cleavage due to thermal expansion of the workpiece 11 can proceed starting from the modified region 17, which is relatively close to the heat source.
[0077] The above-mentioned materials are merely examples, and the material for the plate material 23 may be selected based on the relative magnitude relationship between the thermal expansion coefficient and linear thermal expansion coefficient of the workpiece 11 and the thermal expansion coefficient and linear thermal expansion coefficient of the plate material 23.
[0078] After the fixing step S20, a dividing step S30 is performed. In the dividing step S30, first, as shown in FIG. 5, the workpiece unit 25 is placed on the hot plate 20 so that the protective tape 13 is in contact with the substantially flat supporting surface 20a.
[0079] The support surface 20a of the hot plate 20 is formed of ceramics, aluminum alloy, stainless steel, etc., and is heated by a heating element provided inside the hot plate 20. The temperature of the support surface 20a is controlled, for example, within a range from room temperature to approximately 400°C.
[0080] In this embodiment, the first surface 11a, not the plate material 23, is disposed adjacent to the support surface 20a, and the support surface 20a is heated to approximately 200° C. Fig. 5 is a partial cross-sectional side view showing the heating of the workpiece 11 in the dividing step S30.
[0081] 5, the heat supplied to the workpiece 11 is indicated by an arrow B. When the workpiece 11 is heated, the workpiece 11 thermally expands. As described above, if the thermal expansion of the first surface 11a progresses faster in time, the workpiece 11 is deformed such that the central portion of the first surface 11a protrudes more than the outer periphery.
[0082] The internal stress of the workpiece 11 caused by thermal expansion (see the arrows going left and right from the modified region 17) is released as a result of the workpiece 11 cleaving as a result of a crack 19 propagating from the modified region 17 (i.e., the starting point of the split) along the thickness direction 11c of the workpiece 11.
[0083] In addition, the linear region 17a of the second surface 11b located directly above the modified region 17 is fixed by the plate material 23 and therefore remains substantially fixed even as the cleavage of the workpiece 11 progresses. In other words, the cleavage of the workpiece 11 progresses so as to split from the first surface 11a side with the plate material 23 as a fulcrum.
[0084] In this manner, the workpiece 11 is divided into rectangular pieces along each of the intended division lines 15. Fig. 6 is a partial cross-sectional side view showing a state in which the crack 19 has propagated to the second surface 11b in the dividing step S30.
[0085] When the crack 19 propagates to the second surface 11b, the workpiece 11 is divided into a plurality of rectangular silicon chips. After a predetermined period of heating, the heating of the workpiece 11 by the hot plate 20 is stopped. Figure 7 is a partial cross-sectional side view showing the workpiece 11 divided in the dividing step S30.
[0086] In this embodiment, the workpiece 11 can be divided more reliably than in the case where a thermally expandable resin sheet is placed between the hot plate 20 and the workpiece 11 and an external force is applied to the workpiece 11 by thermally expanding this resin sheet.
[0087] That is, rather than using an external force applied to the workpiece 11 due to thermal expansion of the resin sheet, it is easier to split the workpiece 11 by fixing the second surface 11b with the plate material 23 and allowing cleavage to proceed from the modified region 17 as the splitting starting point. Moreover, the end faces after splitting are cleavage surfaces, and therefore are flat surfaces close to mirror surfaces.
[0088] In addition, since the workpiece 11 can be divided even if the number of modified regions 17 in the thickness direction 11c is reduced, the number of passes in the division start point forming step S10 can be reduced, compared to when a thermally expandable resin sheet is used. Furthermore, since the number of modified regions 17 can be reduced, the amount of processing waste generated in the division step S30 can also be reduced.
[0089] Furthermore, when the dividing method of the present embodiment is used, even though no mechanical load is applied to the workpiece 11, it is possible to exhibit higher dividing performance than when an expanding device that applies a mechanical load is used.
[0090] Fig. 8(A) is a photograph showing an end face of a silicon chip obtained by dividing a workpiece 11 having two layers of modified regions 17 by the dividing method of this embodiment. Fig. 8(B) is a photograph showing an experimental result of a comparative example, showing an end face of a silicon chip obtained by dividing a workpiece 11 having six layers of modified regions 17 by an expanding device.
[0091] In both Figures 8(A) and 8(B), the thickness of the silicon chip is the same, 300 μm. In the experiment shown in Figure 8(A), a rectangular silicon single crystal substrate measuring 20 mm square was used as the workpiece 11, and the workpiece 11 was divided into strips.
[0092] 8(A), there is a long and narrow black region between the two layers of modified regions 17, but in this black region, cracks 19 are not completely connected in the thickness direction 11c. Note that a mirror surface region 11e is formed over a wide area between the modified region 17 on the second surface 11b side and the second surface 11b.
[0093] In the photograph shown in Figure 8 (B), two layers of modified regions 17 near the first surface 11a of the workpiece 11 are formed approximately continuously along the planned division line 15, while four layers of modified regions 17 closer to the second surface 11b than these two layers are formed at a predetermined interval 11d along the planned division line 15.
[0094] A mirror area 11e is formed in a rectangular area having a predetermined interval 11d on one side, but the width of the mirror area 11e in Figure 8(B) (i.e., the predetermined interval 11d) is approximately 1 / 5 of the width of the mirror area 11e in Figure 8(A).
[0095] In the example shown in FIG. 8(B), six layers of modified regions 17 are required in order to divide the workpiece 11 by the expanding device so that cleavage planes are formed on the end faces of the silicon chips after division.
[0096] As a result, in the example shown in Fig. 8(B), the width of the mirror surface region 11e is narrower than that in the example shown in Fig. 8(A). In other words, in the example shown in Fig. 8(A), the number of passes and processing waste can be reduced, and the area of the cleavage plane can be increased, compared to the example shown in Fig. 8(B).
[0097] (First Modification) Next, a modification of the splitting start point forming step S10 will be described. Fig. 9 is a partial cross-sectional side view showing a modification of the splitting start point forming step S10. In this modification, the crack 19 extending from the modified region 17 of the first layer to the first surface 11a does not reach the first surface 11a.
[0098] Depending on the processing conditions during laser processing, the crack 19 may not have reached the first surface 11a during the splitting start point formation step S10, but after the splitting step S30, the crack 19 reaches the first surface 11a and the workpiece 11 is split into silicon chips.
[0099] (Second Modification) Next, a modification of the dividing step S30 will be described. Fig. 10 is a partial cross-sectional side view showing a modification of the dividing step S30. In this modification, in the dividing step S30, the workpiece 11 is heated by the hot plate 20 and the plate material 23 is cooled.
[0100] 10, a blower (not shown) is used to send room temperature air toward the second surface 23b side of the plate material 23 to cool the plate material 23. In Fig. 10, the air is indicated by arrow C. Note that the plate material 23 may be cooled with air at a temperature lower than room temperature, or by placing a heat sink in contact with the plate material 23 or in the vicinity of the plate material 23 through which cold water circulates.
[0101] By cooling the plate material 23, the thermal expansion of the plate material 23 can be more reliably suppressed, and the function of the plate material 23 to fix the second surface 11b of the workpiece 11 can be more reliably achieved. In some cases, such as when the heating temperature of the workpiece 11 in the dividing step S30 is relatively high or when the heating time is relatively long, it may be preferable to cool the plate material 23.
[0102] Second embodiment Next, a second embodiment will be described. Fig. 11 is a partially sectional side view showing a fixing step S20 according to the second embodiment. In the fixing step S20 of the second embodiment, a resin film 27 having a smaller thermal conductivity or linear thermal expansion coefficient than the workpiece 11 is used as a fixing member.
[0103] The film 27 is formed of a polyolefin such as polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc. However, the film 27 is not limited to polyolefin, and may be made of other thermoplastic resins.
[0104] Specific examples of other thermoplastic resin materials that can be used include acrylic resins, methacrylic resins, vinyl resins, polyacetal, natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyamides such as nylon-6, nylon-66 and polymethaxylene adipamide, polyacrylates, polymethacrylates, polyvinyl chloride, polyetherimides, polyacrylonitrile, polycarbonates, polystyrenes, polysulfones, polyethersulfones, polyphenylenes, ether polybutadiene resins, polycarbonate resins, thermoplastic polyimide resins, thermoplastic polyurethane resins, phenoxy resins, polyamideimide resins, fluororesins, ethylene-unsaturated carboxylic acid copolymers, ethylene-vinyl acetate copolymers, ionomers, ethylene-vinyl acetate-maleic anhydride terpolymers, saponified ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, and the like.
[0105] Examples of the unsaturated carboxylic acid constituting the ethylene-unsaturated carboxylic acid copolymer include acrylic acid, methacrylic acid, maleic acid, itaconic acid, monomethyl maleate, monoethyl maleate, maleic anhydride, itaconic anhydride, etc. Here, the ethylene-unsaturated carboxylic acid copolymer includes not only a binary copolymer of ethylene and an unsaturated carboxylic acid, but also a multi-component copolymer in which other monomers are further copolymerized.
[0106] Examples of the other monomers that may be copolymerized with the ethylene-unsaturated carboxylic acid copolymer include vinyl esters such as vinyl acetate and vinyl propionate, and unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, isobutyl acrylate, n-butyl acrylate, methyl methacrylate, isobutyl methacrylate, dimethyl maleate, and diethyl maleate.
[0107] Film 27 has a storage modulus, which is an index of hardness, of 1×10 at room temperature. 6 Pa or more 1×10 9Pa or less, and when heated for application, it is 1×10 6 Pa or more 1×10 7 It is preferable that the storage modulus is equal to or less than Pa. However, the storage modulus when heated for application is lower than the storage modulus at room temperature (that is, it is softer when heated).
[0108] When the film 27 is made of polyolefin, the film 27 is heated to a predetermined temperature of 80° C. or more and 100° C. or less when it is applied. At this time, the storage modulus is 1×10 6 Pa or more 1×10 7 Pa or less.
[0109] Film 27 is circular and has approximately the same diameter as workpiece 11, but may have a larger diameter than workpiece 11. In fixing step S20, film 27 is pressed against second surface 11b of workpiece 11 without adhesive layer 21 (see FIG. 4) therebetween while being heated to the above-mentioned predetermined temperature.
[0110] In this manner, film 27 is fixed to workpiece 11 by closely contacting film 27 with second surface 11b of workpiece 11. Film 27 is attached to workpiece 11 without adhesive layer 21, which is advantageous in that no adhesive remains even when film 27 is peeled off from workpiece 11.
[0111] When film 27 is made of polyolefin, film 27 is heated to a predetermined temperature of 70°C or more and 100°C or less, more preferably, to a predetermined temperature of 70°C or more and 90°C or less, and the pressure applied to film 27 is set to a predetermined value of 0.08 MPa or more and 0.15 MPa or less (e.g., 0.1 MPa), and film 27 is pressed against workpiece 11.
[0112] Thereafter, the heating and pressing are stopped and the workpiece is cooled to room temperature, thereby forming a workpiece unit 25 in which a film 27 is attached to the second surface 11b of the workpiece 11 and a protective tape 13 is attached to the first surface 11a of the workpiece 11.
[0113] The thermal conductivity of the above-mentioned thermoplastic resins is sufficiently lower than that of the silicon single crystal substrate, and in addition, they have heat shrinkability. For example, polyethylene, polypropylene, polystyrene, polyvinyl chloride, PET, etc., undergo heat shrinkage at a certain temperature in the range of 150°C to 200°C.
[0114] If the film 27 has heat shrinkability, the film 27 can be heat-shrunk in the dividing step S30 to apply a force from the outer periphery to the center of the second surface 11b. This can further promote cleavage of the workpiece 11.
[0115] In addition, the structures, methods, etc. according to the above-described embodiments can be appropriately modified and implemented without departing from the scope of the present invention. The above-described first and / or second modified examples can also be applied to the second embodiment.
[0116] A GaN single crystal substrate, a SiC single crystal substrate, or a sapphire single crystal substrate can also be used as the workpiece 11. In this case, the wavelength of the laser beam L used in the splitting start point forming step S10 is appropriately selected so as to transmit the workpiece 11. The material of the plate material 23 or the film 27 is also appropriately selected depending on the thermal expansion coefficient or thermal conductivity of each individual workpiece 11.
[0117] In the above-described embodiment and modified example, the workpiece 11 is divided into rectangular strips, but the workpiece 11 may be divided into a lattice shape. When the workpiece 11 is divided into a lattice shape, a plurality of planned division lines 15 are set in a lattice shape on the first surface 11a. In the division start point forming step S10, one or more layers of modified regions 17 are formed along each of the planned division lines 15. [Explanation of symbols]
[0118] 2: Laser processing device, 4: Chuck table 6: Laser beam irradiation unit, 8: Housing, 10: Head part 11: Workpiece, 11a: 1st surface (one side), 11b: 2nd surface (other side), 11c: Thickness direction 11d: Predetermined interval, 11e: Mirror surface area 12: Microscope camera unit 13: Protective tape, 15: Dividing line 17: modified region, 17a: linear region, 19: crack 18: Support stand, 18a: Support surface 20: hot plate, 20a: support surface 21: adhesive layer, 23: plate material (fixing member), 23a: first surface, 23b: second surface 25: Workpiece unit 27: Film (fixing member) B, C: Arrows, L: Laser beam, P: Focus point S10: Division starting point formation process, S20: Fixing process, S30: Division process
Claims
1. A method for dividing a plate-shaped workpiece having one surface and another surface located opposite to the one surface, comprising the steps of: a division starting point forming step of forming a division starting point inside the workpiece by relatively moving the focus point and the workpiece along a planned division line set on the one surface or the other surface while positioning the focus point of a laser beam having a wavelength that transmits the workpiece inside the workpiece closer to the one surface than the other surface; a fixing step of fixing a fixing member having a thermal conductivity or a linear thermal expansion coefficient smaller than that of the workpiece to the other surface of the workpiece after the dividing start point forming step; a dividing step of dividing the workpiece along the intended dividing line using the fixing member fixed to the other surface as a fulcrum by heating and expanding the workpiece after the fixing step to cause a crack to propagate from the dividing starting point along the thickness direction of the workpiece; A method for dividing a workpiece, comprising:
2. The fixing member has a plate material, 2. The method for dividing a workpiece according to claim 1, wherein in the fixing step, the plate material and the workpiece are fixed via an adhesive layer.
3. The fixing member has a resin film, The method for dividing a workpiece as described in claim 1, characterized in that in the fixing step, the film is fixed to the workpiece by closely adhering the film to the other surface of the workpiece without using an adhesive layer.
4. 4. The method for dividing a workpiece according to claim 3, wherein the fixing member has heat shrinkability.
5. 4. The method for dividing a workpiece according to claim 1, wherein in the dividing step, the workpiece is heated and the fixing member is cooled.
Citation Information
Patent Citations
Laser beam machining method
JP2002192370A
Method for processing wafer
JP2011166002A
Method for dividing plate-like object
JP2014086611A