Method for manufacturing printed wiring board, photosensitive resin composition, photosensitive resin film, printed wiring board and semiconductor package

The photosensitive resin composition and manufacturing method create depressions on the interlayer insulating layer surface to enhance adhesive strength with copper plating, addressing the challenge of surface roughness in printed wiring boards and enabling further miniaturization.

JP2024154574APending Publication Date: 2024-10-31RESONAC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023068467
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional methods for manufacturing printed wiring boards face challenges in simultaneously reducing the surface roughness of interlayer insulating layers while maintaining high adhesive strength with copper plating, hindering further miniaturization of wiring.

Method used

A method involving the use of a photosensitive resin composition containing particles that dissolve in sulfuric acid, followed by roughening and dissolving these particles on the interlayer insulating layer surface to create depressions, enhancing adhesive strength while reducing surface roughness.

Benefits of technology

The method achieves high adhesive strength with copper plating while reducing the surface roughness of the interlayer insulating layer, enabling further miniaturization of printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154574000001_ABST
    Figure 2024154574000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a printed wiring board which exhibits high adhesive strength with copper plating while reducing the surface roughness of an interlayer insulation layer, a photosensitive resin composition capable of providing a printed wiring board, a photosensitive resin film, a printed wiring board obtained and a semiconductor package having a printed wiring board.SOLUTION: There is provided a method for manufacturing a printed wiring board which comprises (1) to (4). (1) A photosensitive resin film containing particles, 95 mass% or more of which is dissolved in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L under the conditions of 70°C for 20 minutes, is laminated on one surface or both surfaces of a circuit board. (2) An interlayer insulation layer having vias is formed by exposing and developing the laminated photosensitive resin film. (3-1) The surface of the vias and the interlayer insulation layer is subjected to roughening treatment. (3-2) Particles (X) existing on the surface of the interlayer insulation layer are dissolved by treating the interlayer insulation layer subjected to roughening treatment with an acidic solution. (4) A circuit pattern is formed on the interlayer insulation layer.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a printed wiring board, a photosensitive resin composition, a photosensitive resin film, a printed wiring board, and a semiconductor package. [Background technology]

[0002] In recent years, electronic devices have become smaller and more powerful, and printed wiring boards are becoming denser due to an increase in the number of circuit layers and finer wiring. In particular, the density of semiconductor package substrates such as BGA (ball grid array) and CSP (chip size package) on which semiconductor chips are mounted is increasing significantly, and in addition to finer wiring, there is a demand for thinner insulating layers and smaller diameters of vias (also called via holes) for interlayer connection.

[0003] A conventional method for manufacturing a printed wiring board is a build-up method (see, for example, Patent Document 1) in which an interlayer insulating layer and a conductor circuit layer are sequentially laminated. As wiring becomes finer, the semi-additive method in which circuits are formed by plating has become mainstream for printed wiring boards. In conventional semi-additive processes, for example, (1) a thermosetting resin film is laminated onto a conductor circuit, and then the thermosetting resin film is heated to harden the film and form an "interlayer insulating layer." (2) Next, vias for interlayer connection are formed by laser processing, and then desmearing and roughening are performed by alkaline permanganate treatment or the like. (3) After that, the board is subjected to electroless copper plating, and after a pattern is formed using a resist, a copper circuit layer is formed by electrolytic copper plating. (4) Next, the resist is peeled off, and the electroless layer is flash etched to form the copper circuit.

[0004] As mentioned above, laser processing is the mainstream method for forming vias in an interlayer insulating layer formed by hardening a thermosetting resin film, but the reduction in the diameter of vias by laser irradiation using a laser processing machine is reaching its limit. Furthermore, when forming vias using a laser processing machine, each via hole needs to be formed one by one, and when a large number of vias need to be provided due to high density, it takes a long time to form the vias, which causes a problem of poor manufacturing efficiency.

[0005] Under these circumstances, a method has been proposed as a method capable of forming a large number of vias at once, in which a photosensitive resin composition containing an acid-modified vinyl group-containing epoxy resin, a photopolymerizable compound, a photopolymerization initiator, an inorganic filler, and a silane compound, and in which the inorganic filler content is 10 to 80 mass %, is used to form a plurality of small vias at once by photolithography (see, for example, Patent Document 2). In Patent Document 2, one of the issues is to suppress the decrease in adhesion with copper plating caused by using a photosensitive resin composition instead of a conventional thermosetting resin composition as a material for an interlayer insulating layer or a surface protective layer, and further issues are also identified as via resolution and adhesion with silicon substrates and chip components, and these are claimed to have been resolved. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-304931 [Patent Document 2] JP 2017-116652 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in recent years, the miniaturization of wiring has progressed more and more. One of the means for achieving further miniaturization of wiring is a method for reducing the surface roughness of an interlayer insulating layer. However, reducing the surface roughness of an interlayer insulating layer reduces the adhesion to copper plating, and these are in a trade-off relationship. Therefore, it is difficult to achieve both a reduction in the surface roughness of the interlayer insulating layer and an improvement in the adhesion to copper plating, and it is not easy to achieve further miniaturization of wiring.

[0008] Therefore, an object of the present disclosure is to provide a method for producing a printed wiring board that exhibits high adhesive strength with copper plating while reducing the surface roughness of the interlayer insulating layer, to provide a photosensitive resin composition and a photosensitive resin film that can provide such a printed wiring board, and to provide a printed wiring board obtained by the production method and a semiconductor package having the printed wiring board. [Means for solving the problem]

[0009] As a result of extensive research, the present inventors have found that the above object can be achieved by the present disclosure. The present disclosure includes the following embodiments [1] to

[16] . [1] A method for producing a printed wiring board, comprising the following (1) to (4): (1): A photosensitive resin film containing particles (X) that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes is laminated onto one or both sides of a circuit board. (2): Forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in (1) above. (3-1): Roughening the surfaces of the vias and the interlayer insulating layer. (3-2): Treating the roughened interlayer insulating layer with an acidic solution to dissolve the particles (X) present on the surface of the interlayer insulating layer. (4): Forming a circuit pattern on the interlayer insulating layer. [2] The method for producing a printed wiring board according to the above [1], wherein the roughening treatment in the above (3-1) is carried out using a roughening solution. [3] The method for producing a printed wiring board according to the above [1], wherein the roughening treatment in (3-1) is carried out by dry etching. [4] The method for producing a printed wiring board according to any one of the above [1] to [3], wherein the surface roughness (Ra) of the interlayer insulating layer after the roughening treatment in (3-1) is 0.30 μm or less. [5] The method for producing a printed wiring board according to any one of the above [1] to [4], wherein the acidic solution used in the step (3-2) contains an aqueous sulfuric acid solution. [6] The method for producing a printed wiring board according to any one of the above [1] to [5], wherein the particles (X) have a volume average particle size of 0.1 to 3 μm. [7] The method for producing a printed wiring board according to any one of the above [1] to [6], wherein the photosensitive resin film contains 10 to 70 volume % of the particles (X). [8] A photosensitive resin composition comprising particles (X) that are dissolved at 95% by mass or more in an aqueous sulfuric acid solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes. [9] The photosensitive resin composition according to the above [8], further comprising (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a thermosetting resin.

[10] The photosensitive resin composition according to the above [9], wherein the component (A) contains an alicyclic skeleton represented by the following general formula (A-1): [ka] (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer between 0 and 6. * is a binding site to other structures.)

[11] The photosensitive resin composition according to any one of the above [8] to

[10] , wherein the particles (X) have an average particle size of 0.1 to 3 μm.

[12] The photosensitive resin composition according to any one of the above [8] to

[11] , wherein the content of the particles (X) is 10 to 70% by volume based on the total solid content.

[13] A photosensitive resin composition for forming a photovia, comprising the photosensitive resin composition according to any one of the above [8] to

[12] .

[14] A photosensitive resin film comprising the photosensitive resin composition according to any one of [8] to

[12] above.

[15] A printed wiring board comprising the photosensitive resin composition according to any one of the above [8] to

[12] or the photosensitive resin film according to the above

[14] .

[16] A semiconductor package comprising the printed wiring board according to

[15] above and a semiconductor element. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a method for producing a printed wiring board that exhibits high adhesive strength with copper plating while reducing the surface roughness of an interlayer insulating layer, as well as to provide a photosensitive resin composition and a photosensitive resin film that can provide the printed wiring board, and further to provide a printed wiring board obtained by the production method and a semiconductor package having the printed wiring board. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic diagram showing a lamination step (1). [Diagram 2] FIG. 13 is a schematic diagram showing a photovia forming step (2). [Diagram 3] FIG. 2 is a schematic diagram showing a roughening treatment step (3-1). [Figure 4] FIG. 2 is a schematic diagram showing a particle (X) dissolving step (3-2). [Diagram 5] FIG. 1 is a schematic diagram showing a circuit pattern forming step (4). [Figure 6] FIG. 1 is a schematic diagram of a multilayer printed wiring board. [Figure 7] 1 is a SEM image of a via formed in Example 2. [Figure 8] 13 is an SEM image of a via formed in Example 11. [Figure 9]1 is a SEM image of the surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) in Example 2. [Figure 10] 13 is a SEM image of the surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) in Example 5. [Figure 11] 13 is a SEM image of the surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) in Example 8. [Figure 12] 13 is a SEM image of the surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) in Example 11. [Figure 13] 13 is a SEM image of the surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) in Comparative Example 5. [Figure 14] 13 is a SEM image of the surface of the interlayer insulating layer after the roughening treatment step (3-1) in Example 13. [Figure 15] 13 is a SEM image of the surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) in Example 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the numerical ranges described in the present disclosure, the upper or lower limit of the numerical range may be replaced with the values ​​shown in the examples. In addition, the lower and upper limits of a numerical range may be arbitrarily combined with the lower or upper limit of another numerical range. In the expression of a numerical range "AA to BB", the numerical values ​​AA and BB at both ends are included in the numerical range as the lower and upper limits, respectively. In the present disclosure, for example, the expression "10 or more" means 10 and a numerical value exceeding 10, and the same applies when the numerical values ​​are different. Also, for example, the expression "10 or less" means 10 and a numerical value less than 10, and the same applies when the numerical values ​​are different. In the present disclosure, when there are multiple substances corresponding to each component in the photosensitive resin composition, the content of each component means the total content of the multiple substances present in the photosensitive resin composition, unless otherwise specified. In the present disclosure, the "number of ring carbon atoms" refers to the number of carbon atoms necessary to form a ring, and does not include the number of carbon atoms of the substituents of the ring. For example, both the cyclohexane skeleton and the methylcyclohexane skeleton have 6 ring carbon atoms. The term "XX (meth)acrylate" means one or both of XX acrylate and XX methacrylate, and the term "(meth)acryloyl group" means one or both of acryloyl group and methacryloyl group. In this disclosure, the "resin component" refers to the components (A) and (B) described below, and also includes other components that may be contained as necessary (e.g., components (C), (D), (F), (G), (H), (I), and (J)), but does not include inorganic compounds such as inorganic fillers and pigments. Furthermore, the "solid content" refers to the non-volatile content excluding water and the diluent described below contained in the photosensitive resin composition, and includes liquid, starch syrup, and wax-like substances at room temperature around 25°C. In this disclosure, the "dielectric constant" refers to the dielectric constant in the 10 GHz band unless otherwise specified. Additionally, any combination of the descriptions in this disclosure is also included in this embodiment.

[0013] [Printed wiring board manufacturing method] A method for manufacturing a printed wiring board according to an embodiment of the present disclosure (hereinafter may be simply referred to as the present embodiment) includes the following (1) to (4). (1): Laminating a photosensitive resin film containing particles (X) (hereinafter, sometimes simply referred to as "particles (X)") that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L under conditions of 70°C and 20 minutes, onto one or both sides of a circuit board (hereinafter, referred to as "lamination process (1)"). (2): Forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in (1) above (hereinafter referred to as "photovia forming step (2)"). (3-1): Roughening the surfaces of the vias and the interlayer insulating layer (hereinafter referred to as "roughening treatment step (3-1)"). (3-2): Dissolving the particles (X) present on the surface of the interlayer insulating layer by treating the roughened interlayer insulating layer with an acidic solution (hereinafter referred to as "particle (X) dissolving step (3-2)"). (4): Forming a circuit pattern on the interlayer insulating layer (hereinafter referred to as "circuit pattern forming step (4)"). Here, in this disclosure, as described above, for convenience, a certain operation may be referred to as "XX step", but the XX step is not limited to only the embodiments specifically described in this disclosure.

[0014] In this embodiment, by providing a particle (X) dissolving step (3-2) after the roughening treatment step (3-1), the particles (X) present on the surface of the interlayer insulating layer can be dissolved to create depressions on the surface of the interlayer insulating layer, thereby making it possible to obtain high adhesive strength with the copper plating while reducing the surface roughness of the interlayer insulating layer. Each step will be described below in order.

[0015] (Lamination process (1)) The lamination step (1) is a step of laminating the photosensitive resin film of this embodiment onto one or both sides of a circuit board (substrate 101 having a circuit pattern 102) using a vacuum laminator (see FIG. 1). Examples of the vacuum laminator include a vacuum applicator manufactured by Nichigo-Morton Co., Ltd., a vacuum pressure laminator manufactured by Meiki Co., Ltd., a roll-type dry coater manufactured by Hitachi, Ltd., and a vacuum laminator manufactured by Resonac Co., Ltd.

[0016] When a protective film is provided on the photosensitive resin film, after peeling or removing the protective film, the photosensitive resin film can be laminated to the circuit board by pressing and heating while being in contact with the circuit board. The lamination can be carried out, for example, after preheating the photosensitive resin film and the circuit board as necessary, under reduced pressure at a pressure bonding temperature of 70 to 130°C, a pressure bonding pressure of 0.1 to 1.0 MPa, and an air pressure of 20 mmHg (26.7 hPa) or less, but is not particularly limited to these conditions. The lamination method may be a batch method or a continuous method using a roll. Finally, the photosensitive resin film laminated to the circuit board is cooled to about 25° C. to form the interlayer insulating layer 103. If the photosensitive resin film has a carrier film, the carrier film may be peeled off at this point, or may be peeled off after exposure, as described below.

[0017] (Photovia formation process (2)) In the photovia forming process (2), at least a part of the photosensitive resin film laminated to the circuit board is exposed to light, and then developed. The exposed portion is photocured to form a pattern. There is no particular limitation on the exposure method, and for example, a method of irradiating the active light in an image-wise manner by passing the active light through a negative or positive mask pattern called artwork (mask exposure method) may be adopted, or a method of irradiating the active light in an image-wise manner by a direct writing exposure method such as LDI (Laser Direct Imaging) exposure method or DLP (Digital Light Processing) exposure method may be adopted. Known light sources can be used as the light source of the actinic rays. Specific examples of light sources include carbon arc lamps, mercury vapor arc lamps, high-pressure mercury lamps, xenon lamps, gas lasers such as argon lasers, solid-state lasers such as YAG lasers, and semiconductor lasers that effectively radiate ultraviolet rays or visible light. The exposure dose is appropriately selected depending on the light source used and the thickness of the photosensitive layer, and for example, in the case of ultraviolet irradiation from a high-pressure mercury lamp, the exposure dose is usually 10 to 1,000 mJ / cm for a photosensitive layer with a thickness of 1 to 100 μm. 2 The preferred range is 50 to 700 mJ / cm 2 More preferably, 150 to 550 mJ / cm 2 is more preferred.

[0018] In the development, the uncured portions of the photosensitive layer are removed from the substrate, and the photocured portions are formed on the substrate as an interlayer insulating layer. When a carrier film is present on the photosensitive layer, the carrier film is removed before removing (developing) the unexposed portion. The developing method includes wet development and dry development, either of which may be adopted, but wet development is widely used and can be adopted in this embodiment as well. In the case of wet development, a developer corresponding to the photosensitive resin composition is used to develop the photosensitive resin composition by a known development method. Examples of the development method include a dip method, a battle method, a spray method, brushing, slapping, scraping, and a method using a swing immersion. Among these, from the viewpoint of improving the resolution of the via, the spray method is preferred, and among the spray methods, the high-pressure spray method is more preferred. The development may be performed by one method, or may be performed by combining two or more methods. The composition of the developer is appropriately selected depending on the composition of the photosensitive resin composition. Examples of the developer include an alkaline aqueous solution, a water-based developer, and an organic solvent-based developer, and among these, an alkaline aqueous solution is preferred.

[0019] In the photovia forming process (2), after exposure and development, 0.2 to 10 J / cm 2 (preferably 0.5 to 5 J / cm 2 The interlayer insulating layer may be further cured, and preferably is further cured, by performing a post-UV cure with an exposure amount of about 1000 nm, and a post-thermal cure at a temperature of about 60 to 250° C. (preferably 120 to 200° C.) as necessary. By the above method, an interlayer insulating layer having vias 104 is formed (see FIG. 2). There are no particular limitations on the shape of the vias, and examples of the cross-sectional shape include a rectangle and an inverted trapezoid (the upper side is longer than the lower side), and examples of the shape seen from the front (the direction from which the via bottom is visible) include a circle and a rectangle. In the formation of vias by photolithography in this embodiment, a via having a cross-sectional shape of an inverted trapezoid (the upper side is longer than the lower side) can be formed, which is preferable because it increases the adhesion of copper plating to the via wall surface.

[0020] The size (diameter) of the via 104 formed by this process can be less than 40 μm, and can also be 35 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less, and can be smaller than the size of a via created by laser processing. There is no particular lower limit to the size (diameter) of the via formed by this process, but it may be 5 μm or more, 10 μm or more, or 15 μm or more. However, the size (diameter) of the vias 104 formed in this process is not limited to less than 40 μm, and may be selected arbitrarily within the range of, for example, 5 to 300 μm, or may be 15 to 100 μm, or may be 20 to 80 μm.

[0021] (Roughening treatment step (3-1)) In the roughening treatment step (3-1), the surfaces of the via and the interlayer insulating layer are roughened (see FIG. 3). The roughening treatment forms finely uneven anchors on the surfaces of the via and the interlayer insulating layer. From the viewpoint of finer wiring, the surface roughness (Ra) of the interlayer insulating layer after the roughening treatment is preferably 0.30 μm or less, more preferably 0.25 μm or less, even more preferably 0.01 to 0.12 μm, particularly preferably 0.02 to 0.10 μm, and most preferably 0.02 to 0.09 μm. In the present disclosure, the surface roughness (Ra) is a result of measurement using a high-performance non-contact three-dimensional surface roughness measurement system (Wyko NT9100, manufactured by Bruker Japan Co., Ltd.), and more specifically, a value measured by the method described in the examples.

[0022] The roughening method is not particularly limited, and a known roughening method for vias and interlayer insulating layers can be adopted. The roughening method is not particularly limited, but includes a method using a roughening liquid, a method using dry etching, etc. Here, the method using a roughening liquid is also called wet etching.

[0023] An oxidizing agent can be used as the roughening liquid. Examples of the oxidizing agent include an alkaline permanganate solution in which potassium permanganate, sodium permanganate, or the like is dissolved in an aqueous solution of sodium hydroxide, dichromate, ozone, hydrogen peroxide-sulfuric acid, nitric acid, and the like. The concentration of permanganate in the alkaline permanganate solution is preferably 5 to 10 mass %. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as Concentrate Compact CP and Dosing Solution Securigans (registered trademark) P (both manufactured by Atotech Japan Co., Ltd.). In addition, when a smear occurs in the photovia forming step (2), the smear may be removed by the roughening liquid. The roughening treatment and the removal of the smear (desmear) can be performed simultaneously.

[0024] When the roughening liquid is used, preferably, the via surface and the interlayer insulating layer surface are swelled, and then the via surface and the interlayer insulating layer surface are roughened. Here, a commercially available swelling liquid can be used for the swelling treatment. Examples of the swelling liquid include an alkaline solution, a surfactant solution, and the like, and preferably an alkaline solution. Examples of the alkaline solution include a sodium hydroxide solution and a potassium hydroxide solution. Examples of commercially available swelling liquids include Swelling Dip Securigance (registered trademark) P and Swelling Dip Securigance (registered trademark) SBU (both manufactured by Atotech Japan Co., Ltd.). The time and temperature of the swelling treatment are not particularly limited, but are preferably 50 to 90°C, more preferably 60 to 80°C, and are preferably 1 to 20 minutes, more preferably 3 to 15 minutes, and even more preferably 3 to 8 minutes.

[0025] After the swelling treatment and the roughening treatment, a water washing treatment may be performed as necessary. The time and temperature of the water washing treatment are not particularly limited, but are preferably 5 to 40°C, more preferably 15 to 30°C, and are preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes. The water washing treatment may be a combination of so-called "pooled water washing" in which water is simply pooled and so-called "running water washing" in which water is flowed, or only one of them may be performed, but it is preferable to perform at least running water washing, and it is more preferable to perform both pooled water washing and running water washing.

[0026] The dry etching includes RIE (Reactive Ion Etching), and the RIE includes dry etching using reactive gas and dry etching using plasma. Among these, dry etching using plasma is preferable. For dry etching using plasma, a commercially available plasma etching device may be used. The conditions for dry etching using plasma are not particularly limited, but preferably oxygen plasma is used, and the output is preferably 100 to 500 W, more preferably 200 to 400 W. There are no particular limitations on the time and temperature of the dry etching, but the temperature is preferably 5 to 40° C., more preferably 15 to 30° C., and the time is preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes.

[0027] 3, the roughening treatment step (3-1) causes some of the particles (X) to protrude from the surface of the interlayer insulating layer 103. The particles (X) will be described later.

[0028] (Particle (X) dissolution process (3-2)) In the particle (X) dissolving step (3-2), the roughened interlayer insulating layer is treated with an acidic solution to dissolve the particles (X) present on the surface of the interlayer insulating layer (see FIG. 4). The acidic solution is not particularly limited, and examples thereof include an aqueous sulfuric acid solution, an aqueous hydrochloric acid solution, an aqueous sodium persulfate solution, an aqueous ammonium persulfate solution, an aqueous potassium persulfate solution, etc. The acidic solution preferably contains an aqueous sulfuric acid solution or an aqueous hydrochloric acid solution, more preferably contains an aqueous sulfuric acid solution, and further preferably is an aqueous sulfuric acid solution. From the viewpoint of the solubility of the particles (X), the concentration of the aqueous sulfuric acid solution is preferably 5 to 100 ml / L, more preferably 10 to 80 ml / L, and even more preferably 15 to 50 ml / L, and may be 10 to 30 ml / L, 35 to 80 ml / L, or 35 to 60 ml / L. From the viewpoint of the solubility of the particles (X), the concentration of the hydrochloric acid aqueous solution is preferably 5 to 100 g / L, more preferably 10 to 80 g / L, and even more preferably 15 to 50 g / L, and may be 10 to 30 ml / L, 35 to 80 ml / L, or 35 to 60 ml / L. Although not particularly limited, it is preferable that the acid solution is not toxic (for example, hydrofluoric acid).

[0029] The particle (X) dissolving step (3-2) may be performed before or during the circuit pattern forming step (4) described below. Furthermore, the particle (X) dissolving step (3-2) can be regarded as a neutralization step after the roughening treatment when a roughening liquid is used in the roughening treatment step (3-1), or as a pretreatment for forming a seed layer when a semi-additive process is performed in the circuit pattern forming step (4) described later when a dry etching treatment is performed in the roughening treatment step (3-1). In any case, it is important that the particle (X) present on the interlayer insulating layer surface is dissolved by the particle (X) dissolving step (3-2) to form a depression 2 as shown in FIG.

[0030] The temperature when treating the interlayer insulating layer with the acidic solution is, from the viewpoint of the solubility of the particles (X), preferably 15 to 80°C, more preferably 20 to 75°C, and even more preferably 25 to 70°C, and may be 40 to 70°C, 50 to 70°C, or 60 to 70°C. The time for treatment with the acidic solution is not particularly limited, but from the viewpoint of the solubility of the particles (X), it is preferably 0.1 to 40 minutes, more preferably 0.3 to 35 minutes, even more preferably 3 to 30 minutes, particularly preferably 5 to 25 minutes, and most preferably 15 to 25 minutes. The method for treating the interlayer insulating layer with an acidic solution is not particularly limited, and examples thereof include (1) a method of immersing a substrate having an interlayer insulating layer in an acidic solution and, if necessary, rocking the substrate having an interlayer insulating layer, (2) a method of immersing a substrate having an interlayer insulating layer in an acidic solution and, if necessary, stirring the acidic solution, and (3) a method of spraying the acidic solution onto the interlayer insulating layer, etc. From the viewpoint of the solubility of the particles (X), the method (1) or (2) is preferred.

[0031] After the treatment with the acidic solution, a water washing treatment may be carried out as necessary. The time and temperature of the water washing treatment are not particularly limited, but are preferably 5 to 40°C, more preferably 15 to 30°C, and are preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes. The water washing treatment may involve both stored water washing and running water washing, or only one of them may be carried out, but it is preferable to carry out at least running water washing, and it is more preferable to carry out both stored water washing and running water washing.

[0032] (Circuit pattern formation process (4)) The circuit pattern forming step (4) is a step of forming a circuit pattern on the interlayer insulating layer after the particle (X) dissolving step (3-2) (see FIG. 5). From the viewpoint of forming fine wiring, it is preferable to form the circuit pattern by a semi-additive process, which forms the circuit pattern and also provides electrical continuity through the vias. In the semi-additive process, first, the via bottom, via wall and the entire surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) are subjected to electroless copper plating using a palladium catalyst or the like to form a seed layer 105. The seed layer 105 is for forming a power supply layer for electrolytic copper plating, and is preferably formed to a thickness of about 0.1 to 2.0 μm. If the seed layer 105 has a thickness of 0.1 μm or more, there is a tendency to suppress a decrease in connection reliability during electrolytic copper plating, and if it is 2.0 μm or less, there is no need to increase the amount of etching when flash etching the seed layer between wirings, and there is a tendency to suppress damage to wiring during etching.

[0033] As pretreatment before the formation of the seed layer, a cleaner treatment (also called a conditioner treatment) and a water washing treatment, or soft etching and a water washing treatment may be performed, if necessary. The cleaner treatment may be carried out with a commercially available alkaline cleaner (conditioner solution) at preferably 40 to 80° C., more preferably 50 to 70° C., for preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes. The water washing treatment after the cleaner treatment is explained in the same manner as the water washing treatment described above, and the preferred embodiments are also the same. Soft etching can be performed by treating with sodium persulfate and sulfuric acid, or ammonium persulfate and sulfuric acid, at preferably 10 to 40°C, more preferably 20 to 35°C, for preferably 0.1 to 3 minutes, more preferably 0.3 to 1 minute. The water washing treatment after soft etching is explained in the same manner as the water washing treatment described above, and the preferred embodiments are also the same. The soft etching can also be performed as the particle (X) dissolving step (3-2).

[0034] The electroless copper plating process is carried out by depositing metallic copper on the surface of the vias and the interlayer insulating layer through a reaction between copper ions and a reducing agent. The electroless plating method and the electrolytic plating method may be any known method and are not particularly limited. As the electroless copper plating solution, a commercially available product can be used, and examples of the commercially available product include "MSK-DK" manufactured by Atotech Japan KK and "ThruCup (registered trademark) PEA series" manufactured by Uemura Kogyo Co., Ltd.

[0035] After the electroless copper plating process, a dry film resist is thermocompressed onto the electroless copper plating using a roll laminator. The thickness of the dry film resist must be greater than the wiring height after electrolytic copper plating, and from this viewpoint, a dry film resist having a thickness of 5 to 30 μm is preferred. As the dry film resist, the "Photec (registered trademark)" series manufactured by Resonac Corporation and the like are used. After the dry film resist is thermocompression bonded, the dry film resist is exposed to light, for example, through a mask on which a desired wiring pattern is drawn. The exposure can be performed using the same device and light source as those that can be used when forming vias in the photosensitive resin film. After the exposure, the dry film resist is developed using an alkaline aqueous solution, and the unexposed parts are removed to form a resist pattern 106. Thereafter, if necessary, a process of removing development residues of the dry film resist using plasma or the like may be performed. After development, electrolytic copper plating is performed to form a copper circuit layer (circuit pattern) 107 and to fill vias.

[0036] After the electrolytic copper plating, the dry film resist is stripped using an alkaline aqueous solution or an amine-based stripper. After the dry film resist is stripped, the seed layer between the wirings is removed (flash etching). The flash etching is performed using an acidic solution such as sulfuric acid and hydrogen peroxide, and an oxidizing solution. After the flash etching, palladium and the like attached to the portions between the wirings is removed as necessary. Palladium can be removed preferably using an acidic solution such as nitric acid or hydrochloric acid.

[0037] After the dry film resist is peeled off or after the flash etching process, a post-baking process is preferably performed. The post-baking process can sufficiently heat-cure unreacted thermosetting components, and thus tends to improve insulation reliability, curing characteristics, and adhesive strength with copper plating. Although the heat-curing conditions vary depending on the type of resin composition, etc., it is preferable that the curing temperature is 150 to 240°C and the curing time is 15 to 100 minutes. The post-baking process completes a series of steps for manufacturing the printed wiring board 100A by the photovia method, and the multi-layered printed wiring board 100A is manufactured by repeating this process according to the number of required interlayer insulating layers (see FIG. 6). Then, a solder resist layer 108 is preferably formed on the outermost layer.

[0038] [Photosensitive resin composition] The photosensitive resin composition of the present embodiment is a photosensitive resin composition containing particles (X) that dissolves at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L under conditions of 70° C. and 20 minutes. By using the photosensitive resin composition as a material for an interlayer insulating layer of a printed wiring board, it becomes possible to dissolve the particles (X) in the particle (X) dissolving step (3-2).

[0039] The photosensitive resin composition of the present embodiment is suitable for via formation by photolithography (also referred to as photovia formation), and is therefore suitable for the formation of one or more selected from the group consisting of photovias and interlayer insulating layers. Here, in the present disclosure, when the term "layer" is used, for example, as in the case of an interlayer insulating layer, the term "layer" includes not only a solid layer, but also a layer that is not a solid layer but at least a part of which is island-like, a layer that has holes, and a layer in which the interface with an adjacent layer is unclear. The solid layer refers to a sheet-like layer that has not been subjected to any particular processing. The photosensitive resin composition of the present embodiment is suitable as a negative type photosensitive resin composition. Hereinafter, the particles (X) will be described in detail, and then other components that may be contained in the photosensitive resin composition of the present embodiment will be described in detail.

[0040] <Particle(X)> As described above, the particles (X) are particles that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L under conditions of 70° C. and 20 minutes. The particles (X) are particles that are easily dissolved in the particle (X) dissolving step (3-2). The concentration of the sulfuric acid aqueous solution is preferably 10 to 80 ml / L, more preferably 15 to 50 ml / L, from the viewpoint of the solubility of the particles (X) in the particle (X) dissolving step (3-2). The particles (X) are preferably 97% by mass or more soluble in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L under conditions of 70°C and 20 minutes, more preferably 99% by mass or more soluble, and may be 100% by mass soluble. Here, the dissolution amount is the amount of dissolution when the particles (X) are submerged in the sulfuric acid aqueous solution and stirred at 70°C for 1 hour. The amount of dissolution of the particles (X) can be calculated from the weight of the particles (X) obtained by filtering the particles (X) after submerging them in the sulfuric acid aqueous solution having the predetermined concentration under conditions of 70°C and 20 minutes. It should be noted that if no solid content is obtained upon filtration, it can be said that the particles (X) are 100% dissolved.

[0041] The particles (X) may be inorganic particles or organic particles. The inorganic particles are not particularly limited, and examples thereof include magnesium-containing inorganic particles such as magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium peroxide, magnesium diboride, magnesium nitride, magnesium sulfide, calcium magnesium carbonate, magnesium nitrate, magnesium sulfate, magnesium sulfite, trimagnesium phosphate, magnesium phosphate, spinel, talc, and serpentine; calcium oxide, calcium hydroxide, calcium sulfide, calcium sulfate, calcium hydrogen sulfate, calcium thiosulfate, calcium sulfite, calcium selenide, calcium selenate, calcium nitrite, calcium phosphate, calcium carbonate, calcium hydrogen carbonate, calcium metasilicate, calcium tetraborate, calcium chromate, and calcium dichromate; and zinc-containing inorganic particles such as zinc oxide, zinc hydroxide, zinc sulfate, zinc nitrate, and zinc carbonate. Among these, magnesium-containing inorganic particles and zinc-containing inorganic particles are preferred from the viewpoint of solubility in the particle (X) dissolving step (3-2), magnesium hydroxide, magnesium carbonate, and zinc oxide are more preferred, and magnesium hydroxide and magnesium carbonate are even more preferred. The organic particles are not particularly limited, and examples thereof include melamine resin, benzoguanamine, polyadamantyl(meth)acrylate, polyt-butyl(meth)acrylate, polyacrylic acid, etc. Among these, polyadamantyl(meth)acrylate and polyt-butyl(meth)acrylate are preferred from the viewpoint of solubility in the particle (X) dissolving step (3-2).

[0042] The volume average particle diameter of the particles (X) is not particularly limited, but from the viewpoint of peel strength with copper plating, it is preferably 0.1 to 3 μm, more preferably 0.2 to 2.0 μm, even more preferably 0.3 to 1.7 μm, and particularly preferably 0.3 to 1.5 μm, and may be 0.5 to 1.5 μm or 0.7 to 1.5 μm. In this disclosure, the volume average particle diameter is determined by measuring particles dispersed in a solvent with a refractive index of 1.38 using a submicron particle analyzer (manufactured by Beckman Coulter, Inc., product name: N5) in accordance with ISO13321, and determining the volume average particle diameter as the particle diameter equivalent to an integrated value of 50% (volume basis) in the particle size distribution.

[0043] In the photosensitive resin composition of the present embodiment, the content of the particles (X) is not particularly limited, but is preferably 10 to 70 volume %, more preferably 15 to 60 volume %, and even more preferably 20 to 55 volume %, and may be 25 to 50 volume %, or may be 25 to 40 volume %, based on the total solid content. When the content of the particles (X) is equal to or more than the lower limit, there is a tendency for high adhesive strength with copper plating to be exhibited while reducing the surface roughness of the interlayer insulating layer, and when it is equal to or less than the upper limit, there is a tendency for good resolution to be maintained. In addition, by making the content of the particles (X) 15% by volume or more based on the total solid amount, the effect of improving the high adhesive strength with the copper plating tends to be further enhanced.

[0044] The photosensitive resin composition of the present embodiment preferably further contains (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a thermosetting resin. Hereinafter, the (A) component and the (B) component will be described in detail in that order, and then the other components will be described in detail.

[0045] <(A) Photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent> The component (A) is a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent. The component (A) may be used alone or in combination of two or more types.

[0046] The component (A) is a compound that exhibits photopolymerizability, particularly radical polymerizability, due to the presence of an ethylenically unsaturated group. Examples of the ethylenically unsaturated group contained in component (A) include photopolymerizable functional groups such as vinyl groups, allyl groups, propargyl groups, butenyl groups, ethynyl groups, phenylethynyl groups, maleimide groups, nadimide groups, (meth)acryloyl groups, etc. Among these, (meth)acryloyl groups are preferred from the viewpoints of reactivity and via resolution.

[0047] The component (A) has an acidic substituent so as to enable alkaline development. Examples of the acidic substituent contained in the component (A) include a carboxy group, a sulfonic acid group, a phenolic hydroxyl group, etc. Among these, from the viewpoint of via resolution, a carboxy group is preferred. The acid value of component (A) is preferably 20 to 200 mgKOH / g, more preferably 40 to 180 mgKOH / g, further preferably 70 to 150 mgKOH / g, and particularly preferably 90 to 120 mgKOH / g. When the acid value of component (A) is equal to or more than the lower limit, the solubility of the photosensitive resin film in a dilute alkaline solution tends to be excellent, and when it is equal to or less than the upper limit, the relative dielectric constant tends to be excellent. The acid value of component (A) can be measured by the method described in the Examples. Two or more types of (A) components having different acid values ​​may be used in combination. In that case, it is preferable that the weighted average acid value of the two or more types of (A) components falls within any of the above ranges.

[0048] The weight average molecular weight (Mw) of the (A) component is preferably 600 to 30,000, more preferably 800 to 25,000, even more preferably 1,000 to 18,000, even more preferably 1,000 to 8,000, particularly preferably 1,200 to 5,000, and most preferably 1,200 to 3,500. When the weight average molecular weight (Mw) of the (A) component is within the above range, the adhesive strength to the copper plating, heat resistance, and insulation reliability tend to be excellent. Here, in the present disclosure, the weight average molecular weight is a value determined by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent and converted into standard polystyrene, and in detail, is a value measured according to the method described in the examples.

[0049] From the viewpoint of relative dielectric constant, the component (A) preferably contains an alicyclic skeleton, but does not necessarily have to contain an alicyclic skeleton. From the viewpoints of via resolution, adhesive strength to copper plating, and electrical insulation reliability, the alicyclic skeleton of component (A) is preferably an alicyclic skeleton having 5 to 20 ring carbon atoms, more preferably an alicyclic skeleton having 5 to 18 ring carbon atoms, even more preferably an alicyclic skeleton having 6 to 18 ring carbon atoms, particularly preferably an alicyclic skeleton having 8 to 14 ring carbon atoms, and most preferably an alicyclic skeleton having 8 to 12 ring carbon atoms. Moreover, from the viewpoints of via resolution, adhesive strength with copper plating, and electrical insulation reliability, the alicyclic skeleton preferably comprises two or more rings, more preferably comprises two to four rings, and even more preferably comprises three rings. Examples of alicyclic skeletons having two or more rings include a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton, and a saturated dicyclopentadiene skeleton. Among these, from the viewpoints of via resolution, adhesive strength with copper plating, and electrical insulation reliability, a saturated dicyclopentadiene skeleton is preferred. From the same viewpoint, the component (A) preferably contains an alicyclic skeleton represented by the following general formula (A-1).

[0050] [ka] (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer between 0 and 6. * is a binding site to other structures.)

[0051] In the general formula (A-1), R A1 Examples of the alkyl group having 1 to 12 carbon atoms represented by include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferable, an alkyl group having 1 to 3 carbon atoms is more preferable, and a methyl group is further preferable. m 1represents an integer of 0 to 6, preferably an integer of 0 to 2, and more preferably 0. m 1 When is an integer between 2 and 6, multiple R A1 may be the same or different. A1 may be substituted on the same carbon atom or on different carbon atoms, to the extent possible. * denotes a bonding site to another structure, and may be bonded to any carbon atom on the alicyclic skeleton. However, it is preferable that the bond is formed at a carbon atom at a site represented by 1 or 2 in the following general formula (A-1'), and at a carbon atom at a site represented by 3 or 4.

[0052] [ka] (In the formula, R A1 , m 1 and * are the same as those in general formula (A-1).

[0053] From the viewpoint of via resolution and adhesive strength with copper plating, the component (A) is preferably an acid-modified vinyl group-containing resin obtained by reacting (a1) an epoxy resin with (a2) an ethylenically unsaturated group-containing organic acid (hereinafter sometimes referred to as component (A')) with (a3) ​​a saturated or unsaturated group-containing polybasic acid anhydride. Here, the term "acid-modified" in the acid-modified vinyl group-containing resin means having an acidic substituent, and the "vinyl group" means an ethylenically unsaturated group. Hereinafter, preferred embodiments of the component (A) obtained from (a1) an epoxy resin, (a2) an ethylenically unsaturated group-containing organic acid, and (a3) ​​a saturated or unsaturated group-containing polybasic acid anhydride will be described.

[0054] ((a1) Epoxy resin) The (a1) epoxy resin is preferably an epoxy resin having two or more epoxy groups. The (a1) epoxy resin may be used alone or in combination of two or more kinds. (a1) Epoxy resins are classified into glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferred.

[0055] (a1) Epoxy resins can be classified into various epoxy resins according to the difference in the main skeleton, and can be classified into epoxy resins having an alicyclic skeleton, novolac epoxy resins, bisphenol epoxy resins, aralkyl epoxy resins, other epoxy resins, etc. Among these, epoxy resins having an alicyclic skeleton and novolac epoxy resins are preferred. Although not particularly limited, it is preferred that novolac epoxy resins, bisphenol epoxy resins, aralkyl epoxy resins, and other epoxy resins have an alicyclic skeleton.

[0056] -Epoxy resin with alicyclic skeleton- The alicyclic skeleton of the epoxy resin having an alicyclic skeleton is explained in the same manner as the alicyclic skeleton of the component (A) described above, and preferred embodiments are also the same. As the epoxy resin having an alicyclic skeleton, an epoxy resin represented by the following general formula (A-2) is preferable.

[0057] [ka] (In the formula, R A1 R represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. A2 represents an alkyl group having 1 to 12 carbon atoms. 1 is an integer between 0 and 6, m 2 is an integer between 0 and 3. n is a number between 0 and 50.)

[0058] In general formula (A-2), R A1 R in general formula (A-1) A1 The preferred embodiments are also the same. R in general formula (A-2)A2 Examples of the alkyl group having 1 to 12 carbon atoms represented by include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferable, an alkyl group having 1 to 3 carbon atoms is more preferable, and a methyl group is further preferable. m in general formula (A-2) 1 m in general formula (A-1) 1 The preferred embodiments are also the same. m in general formula (A-2) 2 represents an integer of 0 to 3, preferably 0 or 1, and more preferably 0. In the general formula (A-2), n represents the repeating number of the structural unit in the parentheses, and is a number from 0 to 50. Usually, an epoxy resin is a mixture of structural units in the parentheses that have different repeating numbers, so in this case, n represents the average value of the mixture. n is preferably a number from 0 to 30.

[0059] As the epoxy resin having an alicyclic skeleton, a commercially available product may be used, and examples of the commercially available product include XD-1000 (trade name, manufactured by Nippon Kayaku Co., Ltd.) and EPICLON (registered trademark) HP-7200 (trade name, manufactured by DIC Corporation).

[0060] -Novolac type epoxy resin- Examples of novolac type epoxy resins include bisphenol novolac type epoxy resins such as bisphenol A novolac type epoxy resins, bisphenol F novolac type epoxy resins, and bisphenol S novolac type epoxy resins; phenol novolac type epoxy resins, cresol novolac type epoxy resins, biphenyl novolac type epoxy resins, naphthol novolac type epoxy resins, etc. The novolac type epoxy resin is not particularly limited, but cresol novolac type epoxy resins are preferred. Moreover, the novolac type epoxy resin is preferably an epoxy resin having a structural unit represented by the following general formula (A-3).

[0061] [ka] (In the formula, R A3 represents a hydrogen atom or a methyl group, Y A1 Each of R independently represents a hydrogen atom or a glycidyl group. A3 may be the same or different. A1 At least one of the groups represents a glycidyl group.

[0062] R A3 From the viewpoints of via resolution and adhesive strength with copper plating, it is preferable that Y be a hydrogen atom. A1 is preferably a glycidyl group. The number of structural units in the epoxy resin (a1) having a structural unit represented by general formula (A-3) is a number equal to or greater than 1, and is preferably a number from 10 to 100, more preferably a number from 15 to 80, and even more preferably a number from 15 to 70. When the number of structural units is within the above range, adhesive strength with copper plating, heat resistance, and insulation reliability tend to be improved. In general formula (A-3), R A3 are all hydrogen atoms, and Y A1 In the case where R is a glycidyl group, it is commercially available as the EXA-7376 series (trade name, manufactured by DIC Corporation). A3 are all methyl groups, and Y A1 However, those having glycidyl groups are commercially available as the EPON SU8 series (product name, manufactured by Mitsubishi Chemical Corporation).

[0063] Examples of bisphenol type epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, and 3,3',5,5'-tetramethyl-4,4'-diglycidyloxydiphenylmethane. Examples of the aralkyl type epoxy resin include phenol aralkyl type epoxy resin, biphenyl aralkyl type epoxy resin, and naphthol aralkyl type epoxy resin. Other epoxy resins include stilbene type epoxy resins, naphthalene skeleton-containing epoxy resins, biphenyl type epoxy resins, dihydroanthracene type epoxy resins, cyclohexanedimethanol type epoxy resins, trimethylol type epoxy resins, alicyclic epoxy resins, aliphatic linear epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, and rubber-modified epoxy resins.

[0064] ((a2) Ethylenically unsaturated group-containing organic acid) The (a2) ethylenically unsaturated group-containing organic acid is preferably an ethylenically unsaturated group-containing monocarboxylic acid. Examples of the ethylenically unsaturated group contained in the component (a2) include the same ethylenically unsaturated groups as those exemplified as the ethylenically unsaturated group contained in the component (A). Examples of the component (a2) include acrylic acid, acrylic acid dimers, methacrylic acid, acrylic acid derivatives such as β-furfurylacrylic acid, β-styrylacrylic acid, cinnamic acid, crotonic acid, and α-cyanocinnamic acid; half-ester compounds which are reaction products of hydroxyl group-containing acrylates and dibasic acid anhydrides; and half-ester compounds which are reaction products of vinyl group-containing monoglycidyl ethers or vinyl group-containing monoglycidyl esters and dibasic acid anhydrides. The component (a2) may be used alone or in combination of two or more types.

[0065] The half-ester compound is obtained by reacting one or more ethylenically unsaturated group-containing compounds selected from the group consisting of hydroxyl group-containing acrylates, vinyl group-containing monoglycidyl ethers, and vinyl group-containing monoglycidyl esters with a dibasic acid anhydride. The reaction is preferably carried out by reacting the ethylenically unsaturated group-containing compound with the dibasic acid anhydride in equimolar amounts.

[0066] Examples of the hydroxyl group-containing acrylate used in the synthesis of the semi-ester compound include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate. Examples of vinyl group-containing monoglycidyl ethers include glycidyl (meth)acrylate.

[0067] The dibasic acid anhydride used in the synthesis of the half ester compound may contain a saturated group or an unsaturated group, and examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.

[0068] In the reaction between the (a1) component and the (a2) component, the amount of the (a2) component used is preferably 0.6 to 1.05 equivalents, more preferably 0.7 to 1.02 equivalents, and even more preferably 0.8 to 1.0 equivalents relative to 1 equivalent of the epoxy group of the (a1) component. By reacting the (a1) component and the (a2) component in the above ratio, the photopolymerizability of the (A) component is improved, and the resolution of the vias in the obtained photosensitive resin composition tends to be improved.

[0069] The components (a1) and (a2) are preferably dissolved in an organic solvent and reacted with each other. Examples of organic solvents include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. One type of organic solvent may be used alone, or two or more types may be used in combination.

[0070] In the reaction between the (a1) component and the (a2) component, it is preferable to use a catalyst for promoting the reaction. Examples of the catalyst include amine-based catalysts such as triethylamine and benzylmethylamine; quaternary ammonium salt catalysts such as methyltriethylammonium chloride, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide and benzyltrimethylammonium iodide; and phosphine-based catalysts such as triphenylphosphine. Among these, phosphine-based catalysts are preferable, and triphenylphosphine is more preferable. The catalyst may be used alone or in combination of two or more kinds. When a catalyst is used, the amount of the catalyst used is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total of the components (a1) and (a2), in order to obtain an appropriate reaction rate.

[0071] In the reaction between the (a1) component and the (a2) component, it is preferable to use a polymerization inhibitor to prevent polymerization during the reaction. Examples of the polymerization inhibitor include hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, pyrogallol, etc. The polymerization inhibitor may be used alone or in combination of two or more kinds. When a polymerization inhibitor is used, the amount used is preferably 0.01 to 1 part by mass, more preferably 0.02 to 0.8 parts by mass, and even more preferably 0.1 to 0.5 parts by mass, per 100 parts by mass of the total of the components (a1) and (a2).

[0072] The reaction temperature between the components (a1) and (a2) is preferably 60 to 150°C, more preferably 80 to 120°C, and even more preferably 90 to 110°C, from the viewpoint of ensuring sufficient reactivity and proceeding with the reaction homogeneously.

[0073] As described above, when an ethylenically unsaturated group-containing monocarboxylic acid is used as the (a2) component, the (A') component obtained by reacting the (a1) component with the (a2) component has a hydroxyl group formed by a ring-opening addition reaction between the epoxy group of the (a1) component and the carboxyl group of the (a2) component. Next, by further reacting the (A') component with the (a3) ​​component, an acid-modified vinyl group-containing resin can be obtained in which the hydroxyl group of the (A') component (including the hydroxyl group originally present in the (a1) component) and the acid anhydride group of the (a3) ​​component are half-esterified.

[0074] ((a3) Polybasic acid anhydride) The (a3) ​​component may contain a saturated group or an unsaturated group. Examples of the (a3) ​​component include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride. Among these, tetrahydrophthalic anhydride is preferred from the viewpoint of via resolution. The (a3) ​​component may be used alone or in combination of two or more.

[0075] In the reaction between the (A') component and the (a3) ​​component, for example, the acid value of the acid-modified vinyl group-containing resin can be adjusted by reacting 0.1 to 1.0 equivalent of the (a3) ​​component with 1 equivalent of the hydroxyl group in the (A') component.

[0076] The reaction temperature between the component (A') and the component (a3) ​​is preferably 50 to 150°C, more preferably 60 to 120°C, and even more preferably 70 to 100°C, from the viewpoint of ensuring sufficient reactivity and proceeding with the reaction homogeneously.

[0077] The content of the component (A) in the photosensitive resin composition of the present embodiment is not particularly limited, but from the viewpoints of heat resistance, dielectric constant, and chemical resistance, it is preferably 10 to 80 mass %, more preferably 15 to 75 mass %, even more preferably 25 to 70 mass %, particularly preferably 35 to 70 mass %, and most preferably 45 to 70 mass %, based on the total amount of resin components in the photosensitive resin composition.

[0078] <(B) Thermosetting resin> The component (B) is a thermosetting resin. The component (B) does not include the component (A). By including the thermosetting resin (B) in the photosensitive resin composition of the present embodiment, the adhesive strength with copper plating and the insulation reliability are improved, and in addition, the heat resistance tends to be improved. Examples of the thermosetting resin include epoxy resin, phenol resin, unsaturated imide resin, cyanate resin, isocyanate resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin, silicone resin, triazine resin, melamine resin, etc. Also, the thermosetting resin is not particularly limited to these, and any known thermosetting resin can be used. Among these, epoxy resin is preferred from the viewpoints of adhesive strength with copper plating, insulation reliability, and heat resistance. The component (B) may be used alone or in combination of two or more types.

[0079] The epoxy resin is preferably an epoxy resin having two or more epoxy groups. Epoxy resins are classified into glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferred.

[0080] Epoxy resins are also classified into various epoxy resins according to the difference in the main skeleton, and each of the above types of epoxy resins is further classified as follows: Specifically, bisphenol-based epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol S-type epoxy resins; bisphenol-based novolac-type epoxy resins such as bisphenol A-type epoxy resins and bisphenol F-type epoxy resins; novolac-type epoxy resins other than the above bisphenol-based novolac-type epoxy resins, such as phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, and biphenyl novolac-type epoxy resins; phenol aralkyl-type epoxy resins; stilbene-type epoxy resins; naphtha-type epoxy resins; They are classified into naphthalene skeleton-containing epoxy resins such as novolac type epoxy resins, naphthol type epoxy resins, naphthol aralkyl type epoxy resins, and naphthylene ether type epoxy resins; biphenyl type epoxy resins; biphenyl aralkyl type epoxy resins; xylylene type epoxy resins; dihydroanthracene type epoxy resins; alicyclic epoxy resins such as saturated dicyclopentadiene type epoxy resins; heterocyclic epoxy resins; spiro ring-containing epoxy resins; cyclohexane dimethanol type epoxy resins; trimethylol type epoxy resins; aliphatic chain epoxy resins; and rubber-modified epoxy resins.

[0081] Among these, the epoxy resin preferably contains at least one selected from the group consisting of bisphenol-based epoxy resins, naphthalene skeleton-containing epoxy resins, and biphenylaralkyl-type epoxy resins, particularly from the viewpoints of heat resistance, electrical insulation reliability, developability, and adhesive strength with copper plating, and more preferably contains at least one selected from the group consisting of naphthalene skeleton-containing epoxy resins and biphenylaralkyl-type epoxy resins.

[0082] The equivalent ratio of the acidic substituent in the (A) component to the epoxy group in the (B) component in the photosensitive resin composition of the present embodiment [epoxy group / acidic substituent] is not particularly limited, but from the viewpoints of insulation reliability, relative dielectric constant, heat resistance, and adhesive strength with copper plating, it is preferably 0.5 to 6.0, more preferably 0.7 to 4.0, even more preferably 0.8 to 2.0, and particularly preferably 0.9 to 1.8.

[0083] The content of the component (B) in the photosensitive resin composition of the present embodiment is not particularly limited, but from the viewpoints of insulation reliability, relative dielectric constant, heat resistance, and adhesive strength with copper plating, it is preferably 1 to 50 mass %, more preferably 5 to 30 mass %, even more preferably 10 to 25 mass %, and most preferably 15 to 25 mass %, based on the total amount of resin components in the photosensitive resin composition.

[0084] <(C) Crosslinking agent> The photosensitive resin composition of the present embodiment preferably further contains a crosslinking agent as component (C). The crosslinking agent is preferably a crosslinking agent having two or more ethylenically unsaturated groups and no acidic substituent. The crosslinking agent reacts with the ethylenically unsaturated groups of component (A) to increase the crosslinking density of the photosensitive resin film after curing. Therefore, the photosensitive resin composition of the present embodiment tends to further improve the heat resistance and the relative dielectric constant by containing a crosslinking agent. The component (C) may be used alone or in combination of two or more types.

[0085] Examples of the component (C) include a bifunctional monomer having two ethylenically unsaturated groups and a polyfunctional monomer having three or more ethylenically unsaturated groups. The component (C) preferably contains the polyfunctional monomer. Examples of the ethylenically unsaturated group contained in the component (C) include the same as the ethylenically unsaturated group contained in the component (A), and the preferred examples are also the same.

[0086] Examples of the bifunctional monomer include aliphatic di(meth)acrylates such as trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; di(meth)acrylates having an alicyclic skeleton such as dicyclopentadiene di(meth)acrylate and tricyclodecane dimethanol di(meth)acrylate; and aromatic di(meth)acrylates such as 2,2-bis(4-(meth)acryloxypolyethoxypolypropoxyphenyl)propane and bisphenol A diglycidyl ether di(meth)acrylate. Among these, from the viewpoint of obtaining a lower relative dielectric constant, di(meth)acrylates having an alicyclic skeleton are preferred, and tricyclodecane dimethanol diacrylate is more preferred.

[0087] Examples of the polyfunctional monomer include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from ditrimethylolpropane, such as ditrimethylolpropane tetra(meth)acrylate; and (meth)acrylate compounds having a skeleton derived from diglycerin. Among these, from the viewpoints of via resolution and adhesive strength with copper plating, a (meth)acrylate compound having a skeleton derived from trimethylolpropane is preferred, and trimethylolpropane tri(meth)acrylate is more preferred. Here, the "(meth)acrylate compound having a skeleton derived from XXX" (wherein XXX is the name of the compound) means an esterification product of XXX and (meth)acrylic acid, and the esterification product also includes a compound modified with an alkyleneoxy group.

[0088] When the photosensitive resin composition of the present embodiment contains a crosslinking agent (C), the content of the crosslinking agent (C) is not particularly limited, but from the viewpoints of heat resistance and relative dielectric constant, it is preferably 1 to 85 parts by mass, more preferably 5 to 70 parts by mass, even more preferably 10 to 50 parts by mass, and particularly preferably 10 to 40 parts by mass, relative to 100 parts by mass of the component (A).

[0089] <(D) Elastomer> The photosensitive resin composition of this embodiment preferably further contains an elastomer as component (D). The photosensitive resin composition of this embodiment contains the elastomer (D), which tends to further improve the adhesive strength with the copper plating. In addition, the photosensitive resin composition of this embodiment contains the elastomer (D), which tends to suppress the "reduction in flexibility and adhesive strength with the copper plating" caused by distortion (internal stress) that may occur due to the cure shrinkage of the component (A). The (D) elastomer may be used alone or in combination of two or more kinds.

[0090] The (D) elastomer may have a reactive functional group at the molecular end or in the molecular chain. Examples of the reactive functional group include an acid anhydride group, an epoxy group, a hydroxyl group, a carboxyl group, an amino group, an amide group, an isocyanato group, an acrylic group, a methacrylic group, a vinyl group, etc. Among these, from the viewpoint of the resolution of the via and the adhesive strength with the copper plating, an acid anhydride group, an epoxy group, a hydroxyl group, a carboxyl group, an amino group, and an amide group are preferred, an acid anhydride group and an epoxy group are more preferred, and an acid anhydride group is even more preferred. The acid anhydride group is preferably an acid anhydride group derived from phthalic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylnadic anhydride, nadic anhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, or the like, and more preferably an acid anhydride group derived from maleic anhydride. When the (D) elastomer has acid anhydride groups, the number of acid anhydride groups in one molecule is preferably 1 to 10, more preferably 3 to 10, and even more preferably 6 to 10, from the viewpoints of via resolution and relative dielectric constant.

[0091] The photosensitive resin composition of the present embodiment preferably contains, as the elastomer (D), an elastomer having an ethylenically unsaturated group and an acidic substituent. Examples of the acidic substituent and the ethylenically unsaturated group include the same as those of the acidic substituent and the ethylenically unsaturated group of the component (A). Among these, the elastomer (D) preferably has the above-mentioned acid anhydride group as the acidic substituent and the below-mentioned 1,2-vinyl group as the ethylenically unsaturated group.

[0092] (D) Examples of the elastomer include polybutadiene-based elastomers, polyester-based elastomers, styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, polyamide-based elastomers, acrylic-based elastomers, silicone-based elastomers, derivatives of these elastomers, etc. Among these, polybutadiene-based elastomers are preferred from the viewpoints of improving the adhesive strength with the copper plating and further improving compatibility and solubility with the resin component.

[0093] Suitable examples of the polybutadiene-based elastomer include those containing 1,2-vinyl groups and having 1,4-trans structural units and 1,4-cis structural units. As described above, from the viewpoint of via resolution, the polybutadiene-based elastomer is preferably a polybutadiene-based elastomer having an acid anhydride group that has been modified with an acid anhydride, and more preferably a polybutadiene-based elastomer having an acid anhydride group derived from maleic anhydride. Polybutadiene-based elastomers are commercially available, and specific examples thereof include "POLYVEST (registered trademark) MA75" and "POLYVEST (registered trademark) EP MA120" (all of which are product names manufactured by Evonik), "Ricon (registered trademark) 100", "Ricon (registered trademark) 130MA8", "Ricon (registered trademark) 131MA5", "Ricon (registered trademark) 131MA17", and "Ricon (registered trademark) 184MA6" (all of which are product names manufactured by Cray Valley Corporation).

[0094] From the viewpoint of adhesive strength with copper plating, the polybutadiene-based elastomer may be polybutadiene having an epoxy group (hereinafter, may be referred to as epoxidized polybutadiene). From the viewpoints of adhesive strength to copper plating and flexibility, the epoxidized polybutadiene is preferably an epoxidized polybutadiene represented by the following general formula (D-1).

[0095] [ka] (In the formula, a, b, and c each represent a ratio of the structural units in the parentheses, a is 0.05 to 0.40, b is 0.02 to 0.30, and c is 0.30 to 0.80, and further, a+b+c=1.00 and (a+c)>b are satisfied. y represents the number of structural units in the square brackets and is an integer of 10 to 250.)

[0096] In the general formula (D-1), the structural units in the square brackets may be bonded in any order. In other words, the structural unit shown on the left, the structural unit shown in the center, and the structural unit shown on the right may be interchanged, and if they are represented as (a), (b), and (c), respectively, various bonding orders are possible, such as -[(a)-(b)-(c)]-[(a)-(b)-(c)-]-, -[(a)-(c)-(b)]-[(a)-(c)-(b)-]-, -[(b)-(a)-(c)]-[(b)-(a)-(c)-]-, -[(a)-(b)-(c)]-[(c)-(b)-(a)-]-, -[(a)-(b)-(a)]-[(c)-(b)-(c)-]-, and -[(c)-(b)-(c)]-[(b)-(a)-(a)-]-. From the viewpoints of adhesive strength to copper plating and flexibility, a is preferably 0.10 to 0.30, b is preferably 0.10 to 0.30, and c is preferably 0.40 to 0.80. From the same viewpoints, y is preferably an integer of 30 to 180.

[0097] Examples of polyester-based elastomers include those obtained by polycondensation of a dicarboxylic acid or a derivative thereof with a diol compound or a derivative thereof. Examples of dicarboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and aromatic dicarboxylic acids in which the hydrogen atoms of the aromatic nuclei are substituted with methyl groups, ethyl groups, phenyl groups, or the like; aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. Examples of the diol compound include aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols such as bisphenol A, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3-methylphenyl)propane, and resorcin. As a polyester-based elastomer, a multiblock copolymer having an aromatic polyester (e.g., polybutylene terephthalate) portion as a hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) portion as a soft segment component is preferably used. Multiblock copolymers are available in various grades depending on the type, ratio, and molecular weight of the hard and soft segments.

[0098] The number average molecular weight of the (D) elastomer is not particularly limited, but is preferably 10,000 to 80,000, and may be 20,000 to 70,000, 30,000 to 65,000, or 40,000 to 60,000. The number average molecular weight of the (D) elastomer is determined by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent, and is converted into standard polystyrene.

[0099] When the photosensitive resin composition of the present embodiment contains an elastomer (D), the content of the elastomer (D) is not particularly limited, but from the viewpoints of heat resistance and adhesive strength with copper plating, it is preferably 0.5 to 15 mass %, more preferably 1 to 10 mass %, even more preferably 1 to 8 mass %, and particularly preferably 3 to 8 mass %, based on the total amount of the resin components in the photosensitive resin composition.

[0100] <(E) Inorganic filler> The photosensitive resin composition of the present embodiment may further contain an inorganic filler as component (E). The component (E) does not contain the particles (X). In other words, the component (E) is an inorganic filler other than the particles (X). When the photosensitive resin composition of the present embodiment contains the inorganic filler (E), the low thermal expansion coefficient, heat resistance, and flame retardancy tend to be further improved. The (E) component is not particularly limited, but includes silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, aluminum hydroxide, aluminum silicate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (calcined clay, etc.), molybdic acid compounds such as zinc molybdate, aluminum borate, silicon carbide, etc. The (E) component may be used alone or in combination of two or more. Among these, the inorganic filler is preferably silica, alumina, or mica, more preferably silica or alumina, and even more preferably silica, from the viewpoints of thermal expansion coefficient, heat resistance, and flame retardancy. Examples of silica include crushed silica, fumed silica, and fused silica (fused spherical silica).

[0101] There are no particular limitations on the volume average particle size of component (E), but it is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, even more preferably 0.2 to 1 μm, and particularly preferably 0.3 to 0.8 μm.

[0102] ((E) Component Content) When the photosensitive resin composition of the present embodiment contains the component (E), the content of the component (E) is preferably 20 mass % or less, more preferably 15 mass % or less, further preferably 10 mass % or less, and particularly preferably 5 mass % or less based on the total solid content of the photosensitive resin composition, from the viewpoint of not impairing the effect of the particles (X). The photosensitive resin composition of the present embodiment does not need to contain the component (E).

[0103] <(F)Organic filler> The photosensitive resin composition of the present embodiment may further contain an organic filler as component (F). The component (F) does not contain the particles (X). In other words, the component (F) is an organic filler other than the particles (X). The photosensitive resin composition of the present embodiment contains an organic filler (F), so that the photosensitive resin composition and the photosensitive resin film tend to have a low specific gravity, and depending on the material, the relative dielectric constant tends to be further reduced. The (F) component preferably contains resin particles formed from at least one selected from the group consisting of a resin having fluorine atoms, polyethylene, polypropylene, polystyrene, polyphenylene ether, and silicone. Among these, from the viewpoint of the effect of reducing the relative dielectric constant, the (F) component preferably contains resin particles formed from a resin having fluorine atoms, and more preferably contains resin particles formed from a polytetrafluoroethylene (PTFE) resin. The volume average particle diameter of the resin particles is not particularly limited, but is preferably 20 to 1,000 nm, more preferably 30 to 800 nm, further preferably 50 to 500 nm, and particularly preferably 100 to 300 nm. The method for measuring the volume average particle diameter is as described above.

[0104] When the photosensitive resin composition of the present embodiment contains an organic filler (F), the content of the organic filler (F) is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the total amount of the resin components of the photosensitive resin composition, from the viewpoint of not impairing the effect of the particles (X). The photosensitive resin composition of the present embodiment does not need to contain the component (F).

[0105] <(G) Hardener> The photosensitive resin composition of the present embodiment preferably further contains a curing agent as component (G). By containing the curing agent (G), the photosensitive resin composition of the present embodiment tends to be able to further improve the heat resistance, the relative dielectric constant, and the like. The (G) curing agent may be used alone or in combination of two or more kinds.

[0106] As the (G) curing agent, the curing agent for the (B) thermosetting resin may be used. For example, when the (B) thermosetting resin is an epoxy resin, it is preferable to use an epoxy resin curing agent, and examples of the epoxy resin curing agent include guanamines such as acetoguanamine and benzoguanamine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylylenediamine, diaminodiphenylsulfone, dicyandiamide, urea, urea derivatives, melamine, and polybasic hydrazides; organic acid salts and / or epoxy adducts thereof; amine complexes of boron trifluoride; triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, and 2,4-diamino-6-xylyl-S-triazine; polyphenols such as polyvinylphenol, polyvinylphenol bromide, phenol novolac, alkylphenol novolac, and triazine ring-containing phenol novolac resin. The polyphenol may be, for example, a modified polyphenol modified with melamine, benzoguanamine, etc. The hydroxyl equivalent of the polyphenol is not particularly limited, but is preferably 40 to 300 g / eq, may be 40 to 250 g / eq, may be 60 to 200 g / eq, may be 80 to 160 g / eq, or may be 100 to 140 g / eq. Here, the hydroxyl equivalent (g / eq) can be determined by titration using an acetylation method using acetic anhydride.

[0107] When the photosensitive resin composition of the present embodiment contains a (G) curing agent, the content of the (G) curing agent is not particularly limited, but from the viewpoint of further improving the heat resistance and the relative dielectric constant, it is preferably 0.01 to 10 mass %, more preferably 0.05 to 5 mass %, and even more preferably 0.1 to 1 mass %, based on the total amount of the resin components of the photosensitive resin composition.

[0108] <(H) Curing accelerator> The photosensitive resin composition of the present embodiment preferably further contains a curing accelerator as component (H). By containing the curing accelerator (H), the photosensitive resin composition of the present embodiment tends to be able to further improve the heat resistance, the relative dielectric constant, and the like. The (H) curing accelerator may be used alone or in combination of two or more kinds.

[0109] (H) Curing accelerators include imidazole compounds such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, 2-phenyl-1-benzyl-1H-imidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and isocyanate masked imidazole (addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole); trimethylamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylamine, ... tertiary amines such as tylguanidine and m-aminophenol; organic phosphines such as tributylphosphine, triphenylphosphine and tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the above-mentioned polybasic acid anhydrides; diphenyliodonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, 2,4,6-triphenylthiopyrylium hexafluorophosphate, and the like. Among these, imidazole compounds are preferred from the viewpoint of obtaining an excellent curing effect.

[0110] When the photosensitive resin composition of the present embodiment contains the curing accelerator (H), the content of the curing accelerator (H) is not particularly limited, but from the viewpoint of further improving the heat resistance and the relative dielectric constant, it is preferably 0.01 to 10 mass %, more preferably 0.05 to 5 mass %, and even more preferably 0.1 to 2 mass % based on the total amount of the resin components of the photosensitive resin composition.

[0111] <(I) Photopolymerization initiator> The photosensitive resin composition of the present embodiment preferably further contains a photopolymerization initiator as component (I). By containing the photopolymerization initiator (I), the photosensitive resin composition of the present embodiment tends to further improve the resolution of the vias. The photopolymerization initiator (I) may be used alone or in combination of two or more. From the viewpoint of via resolution, the photosensitive resin composition of the present embodiment preferably contains two or more types of the component (I).

[0112] (I) The photopolymerization initiator is not particularly limited as long as it can photopolymerize an ethylenically unsaturated group, and can be appropriately selected from commonly used photopolymerization initiators. (I) Photopolymerization initiators include benzoin-based compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone-based compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane, and N,N-dimethylaminoacetophenone; 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, 2 ketal compounds such as acetophenone dimethyl ketal and benzyl dimethyl ketal; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; acylphosphine oxide compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; and oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime].

[0113] Among these, oxime ester compounds and acylphosphine oxide compounds are preferred, and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime) and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide are more preferred. Oxime ester compounds have the advantage of improving photocurability, and acylphosphine oxide compounds have the advantage of improving the degree of curing of the bottom of the cured product obtained by curing the photosensitive resin film, and suppressing undercut. By using an oxime ester compound and an acylphosphine oxide compound in combination, the resolution of the via tends to be further improved.

[0114] When the photosensitive resin composition of the present embodiment contains a photopolymerization initiator (I), the content of the photopolymerization initiator (I) is not particularly limited, but is preferably 0.01 to 20 mass%, more preferably 0.05 to 10 mass%, further preferably 0.05 to 3 mass%, and particularly preferably 0.05 to 1.0 mass%, based on the total amount of the resin components of the photosensitive resin composition. If the content of the photopolymerization initiator (I) is equal to or more than the lower limit, there is a tendency that the elution of the exposed portion during development can be reduced, and if it is equal to or less than the upper limit, there is a tendency that the heat resistance is improved.

[0115] <(J) Photosensitizer> The photosensitive resin composition of this embodiment may contain a photosensitizer as the component (J) as necessary. The photosensitizer (J) may be used alone or in combination of two or more. From the viewpoint of via resolution, the photosensitive resin composition of the present embodiment may contain two or more types of component (J). Examples of (J) photosensitizers include thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; tertiary amines such as trialkylamines and triethanolamine; dialkylaminobenzoic acid alkyl esters such as ethyl N,N-dimethylaminobenzoate and amyl N,N-dimethylaminobenzoate; bis(dialkylamino)benzophenones such as 4,4'-bis(dimethylamino)benzophenone and 4,4'-bis(diethylamino)benzophenone; phosphine compounds such as triphenylphosphine; toluidine compounds such as N,N-dimethyltoluidine; anthracene compounds such as 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, and 2-ethyl-9,10-diethoxyanthracene; perylene compounds; and coumarin compounds. As the (J) photosensitizer, from the viewpoint of improving the resolution and shape of the vias, bis(dialkylamino)benzophenone is preferred, and 4,4'-bis(diethylamino)benzophenone is more preferred.

[0116] When the photosensitive resin composition of the present embodiment contains a photosensitizer (J), the content of the photosensitizer (J) is not particularly limited, but is preferably 0.01 to 5 mass%, more preferably 0.05 to 3 mass%, further preferably 0.1 to 1.5 mass%, and particularly preferably 0.1 to 1.0 mass%, based on the total amount of the resin components of the photosensitive resin composition. If the content of the photosensitizer (J) is equal to or more than the lower limit, the degree of cure of the bottom of the cured product obtained by curing the photosensitive resin film tends to be sufficiently high, and if it is equal to or less than the upper limit, the degree of cure of the bottom of the cured product tends to be appropriately low.

[0117] <(K) Additives> The photosensitive resin composition of the present embodiment may contain, as necessary, various known and commonly used additives, such as pigments such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black; adhesion aids such as melamine; foam stabilizers such as silicone compounds; polymerization inhibitors; thickeners; and flame retardants. The content of these (K) additives may be appropriately adjusted depending on each purpose, but each content is preferably 0.01 to 5 mass %, alternatively 0.05 to 3 mass %, or alternatively 0.1 to 1 mass % based on the total amount of the resin components in the photosensitive resin composition.

[0118] <Diluent> The photosensitive resin composition of the present embodiment may contain a diluent as necessary. As the diluent, an organic solvent or the like can be used. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. The diluent may be used alone or in combination of two or more.

[0119] When the photosensitive resin composition of the present embodiment contains a diluent, the content of the diluent may be appropriately selected for the purpose of adjusting the concentration of the total solid content in the photosensitive resin composition to a range of preferably 40 to 90 mass%, more preferably 50 to 85 mass%, and further preferably 60 to 80 mass%. By adjusting the amount of the diluent used to the above range, the coatability of the photosensitive resin composition is improved, and a more precise pattern can be formed.

[0120] The photosensitive resin composition of the present embodiment can be obtained by kneading and mixing the components using a roll mill, a bead mill, or the like. Here, the photosensitive resin composition of the present embodiment may be used in a liquid state (liquid form) or in a film state (film form). When used in a liquid state, the method for applying the photosensitive resin composition of the present embodiment is not particularly limited, and examples of the application method include printing, spin coating, spray coating, jet dispensing, inkjet, dip coating, etc. Among these, printing and spin coating are preferred from the viewpoint of more easily forming the photosensitive layer. When used in the form of a film, it can be used in the form of a photosensitive resin film described later, for example, and in this case, a photosensitive layer of a desired thickness can be formed by laminating it on a carrier film using a laminator, etc. Note that using it in the form of a film is preferable because it increases the production efficiency of printed wiring boards.

[0121] Since the photosensitive resin composition of this embodiment is suitable for via formation by photolithography (also referred to as photovia formation), the present disclosure also provides a photosensitive resin composition for photovia formation comprising the photosensitive resin composition of this embodiment. The photosensitive resin composition of the present embodiment is useful as an interlayer insulating layer for printed wiring boards, and is also useful for solder resist applications.

[0122] [Photosensitive resin film] The photosensitive resin film of the present embodiment contains the photosensitive resin composition of the present embodiment, in other words, is formed using the photosensitive resin composition of the present embodiment. The photosensitive resin film is useful as a photosensitive layer for forming an interlayer insulating layer. The photosensitive resin film of this embodiment is formed using the photosensitive resin composition of this embodiment, and therefore contains 10 to 70 volume % of the particles (X). The components and their contents in the photosensitive resin film are as described for the components and their contents in the photosensitive resin composition of this embodiment.

[0123] The photosensitive resin film of the present embodiment may be provided on a carrier film. The photosensitive resin film of the present embodiment can be formed, for example, by applying the photosensitive resin composition of the present embodiment onto a carrier film using a known coating device such as a comma coater, a bar coater, a kiss coater, a roll coater, a gravure coater, or a die coater, and then drying the applied composition. Examples of the carrier film include polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polyolefins such as polypropylene and polyethylene. The thickness of the carrier film is preferably 5 to 100 μm, more preferably 10 to 60 μm, and further preferably 15 to 45 μm.

[0124] In addition, the photosensitive resin film of this embodiment may have a protective film on the surface opposite to the surface in contact with the carrier film. As the protective film, a polymer film such as polyethylene or polypropylene may be used. The same polymer film as the carrier film described above may be used, or a different polymer film may be used.

[0125] The coating film formed by applying the photosensitive resin composition can be dried using a dryer using hot air drying, far infrared rays, or near infrared rays. The drying temperature is preferably 60 to 150°C, more preferably 70 to 120°C, and even more preferably 80 to 110°C. The drying time is preferably 1 to 60 minutes, more preferably 2 to 30 minutes, and even more preferably 5 to 20 minutes. The content of the remaining diluent in the photosensitive resin film after drying is preferably 3 mass% or less, more preferably 2 mass% or less, and even more preferably 1 mass% or less, from the viewpoint of preventing the diluent from diffusing in the manufacturing process of the printed wiring board.

[0126] The thickness (thickness after drying) of the photosensitive resin film (photosensitive layer) is not particularly limited, but from the viewpoint of thinning the printed wiring board, it is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 5 to 40 μm.

[0127] The photosensitive resin film of the present embodiment is excellent in via resolution and adhesive strength with copper plating, and is therefore suitable primarily as an interlayer insulating layer for printed wiring boards, but is also useful as a solder resist.

[0128] [Printed wiring board] The printed wiring board of the present embodiment is obtained by the above-mentioned manufacturing method, and contains the photosensitive resin composition of the present embodiment or the photosensitive resin film of the present embodiment. In other words, it contains an interlayer insulating layer formed using the photosensitive resin composition of the present embodiment or the photosensitive resin film of the present embodiment. Here, the expression "containing an interlayer insulating layer" includes a case where the interlayer insulating layer is contained as it is, and a case where the interlayer insulating layer is contained in a state after, for example, processing such as via formation, various treatments such as roughening treatment, and wiring formation are performed on the interlayer insulating layer. The printed wiring board of this embodiment allows the formation of fine wiring and has excellent adhesion to copper plating, so it can also be used as an interposer for a semiconductor package.

[0129] [Semiconductor package] The present disclosure also provides a semiconductor package including the printed wiring board of the present embodiment and a semiconductor element. The semiconductor package of the present embodiment can be manufactured by mounting a semiconductor element such as a semiconductor chip or memory at a predetermined position on the printed wiring board of the present embodiment, and then sealing the semiconductor element with a sealing resin or the like. EXAMPLES

[0130] The present embodiment will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples. The acid value and weight average molecular weight of component (A) were measured according to the following method. The photosensitive resin compositions obtained in each example were used to evaluate the properties according to the following method.

[0131] <Acid value measurement method> The acid value of component (A) was calculated from the amount of potassium hydroxide aqueous solution required to neutralize component (A).

[0132] <Method for measuring weight average molecular weight> The weight average molecular weight of component (A) was measured using the following GPC measuring device and measuring conditions, and the value converted using the calibration curve of standard polystyrene was used as the weight average molecular weight. The calibration curve was created using a 5-sample set ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) as standard polystyrene. (GPC measurement device) Equipment: High-speed GPC equipment "HCL-8320GPC", detector is differential refractometer or UV, manufactured by Tosoh Corporation Column: TSKgel SuperMultipore HZ-H (column length: 15 cm, column inner diameter: 4.6 mm), manufactured by Tosoh Corporation (Measurement conditions) Solvent: Tetrahydrofuran (THF) Measurement temperature: 40℃ Flow rate: 0.35ml / min Sample concentration: 10mg / THF5ml Injection volume: 20μl

[0133] [1. Surface roughness (Ra)] In each of the Examples and Comparative Examples, the surface of the evaluation laminate A after the desmear treatment was measured for the surface roughness (Rz) of the prepreg surface produced in each Example using a white light interferometry method with a high-performance non-contact three-dimensional surface profile roughness measurement system (Wyko NT9100, manufactured by Bruker Japan Co., Ltd.).

[0134] [2. Evaluation of adhesive strength with copper plating] For the evaluation laminate B produced in each of the Examples and Comparative Examples, the perpendicular peel strength was measured at 23° C. in accordance with JIS C6481 (1996).

[0135] Synthesis Example 1: Synthesis of photopolymerizable compound (A1) having an ethylenically unsaturated group and an acidic substituent 350 parts by mass of dicyclopentadiene type epoxy resin ("XD-1000" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 252 g / eq, softening point 74.2°C, component (a1), number of ring carbon atoms in alicyclic skeleton: 10), 70 parts by mass of acrylic acid (component (a2)), 0.5 parts by mass of methylhydroquinone, and 120 parts by mass of carbitol acetate were charged and reacted by heating to 90°C and stirring, thereby dissolving the mixture. Next, the obtained solution was cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the solution was heated to 100°C and reacted until the acid value of the solution reached 1 mgKOH / g. To the solution after the reaction, 98 parts by mass of tetrahydrophthalic anhydride (component (a3)) and 85 parts by mass of carbitol acetate were added, and the solution was heated to 80°C and reacted for 6 hours. Thereafter, it was cooled to room temperature to obtain a photopolymerizable compound (A1) having an ethylenically unsaturated group and an acidic substituent and a solid content concentration of 73 mass % [acid value: 60 mg KOH / g, weight average molecular weight: 2,000].

[0136] <Synthesis Example 2> Synthesis of photopolymerizable compound (A2) having an ethylenically unsaturated group and an acidic substituent 350 parts by mass of a cresol novolac epoxy resin (EOCN-104S, manufactured by Nippon Kayaku Co., Ltd.; component (a1)), 70 parts by mass of acrylic acid (component (a2)), 0.5 parts by mass of methyl hydroquinone, and 120 parts by mass of carbitol acetate were charged and reacted by heating to 90° C. and stirring to dissolve the mixture. Next, the obtained solution was cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the solution was heated to 100°C and reacted until the acid value of the solution reached 1 mgKOH / g. To the solution after the reaction, 98 parts by mass of tetrahydrophthalic anhydride (component (a3)) and 85 parts by mass of carbitol acetate were added, and the solution was heated to 80°C and reacted for 6 hours. Thereafter, it was cooled to room temperature to obtain a photopolymerizable compound (A2) having an ethylenically unsaturated group and an acidic substituent and a solid content concentration of 73 mass % [acid value: 60 mg KOH / g, weight average molecular weight: 6,500].

[0137] Examples 1 to 12 and Comparative Examples 1 to 6 (1) Production of photosensitive resin composition A composition was formulated according to the formulation shown in Table 1 (the units of values ​​in the table are parts by mass, and in the case of a solution, the amounts are calculated as solid contents) (note that the particles (X) were mixed with the component (A) in advance), and then kneaded with a three-roll mill. Methyl ethyl ketone was then added so that the solid content concentration became 65% by mass, to obtain a photosensitive resin composition. (2) Manufacture of photosensitive resin films A polyethylene terephthalate film having a thickness of 16 μm (manufactured by Teijin Limited, product name "G2-16") was used as a carrier film. The photosensitive resin composition prepared in each example was applied onto the carrier film while adjusting the film thickness after drying to 25 μm, and dried at 100° C. for 10 minutes using a hot air convection dryer to form a photosensitive resin film (photosensitive layer). Next, a polyethylene film (manufactured by Tamapoly Corporation, product name "NF-15") was laminated as a protective film onto the surface of the photosensitive resin film (photosensitive layer) opposite to the side in contact with the carrier film, to produce a photosensitive resin film in which the carrier film and the protective film were laminated together.

[0138] (Lamination process (1)) While peeling off the protective film from the "photosensitive resin film having a carrier film and a protective film laminated thereto" produced by the above method, lamination was performed on a copper-clad laminate substrate having a thickness of 1.0 mm using a press-type vacuum laminator (manufactured by Meiki Seisakusho Co., Ltd., product name "MVLP-500") at a pressure of 0.4 MPa, a press hot plate temperature of 75°C, a vacuum drawing time of 25 seconds, a lamination press time of 25 seconds, and an air pressure of 4 kPa or less to obtain a laminate. The obtained laminate was exposed to 200 mJ / cm 2 using a parallel light exposure machine (manufactured by Oak Manufacturing Co., Ltd., product name "EXM-1201") using an ultra-high pressure mercury lamp as a light source. 2 (wavelength 365 nm). Then, using an ultraviolet exposure device, the entire surface was exposed to 2,000 mJ / cm 2 After exposure to light at a wavelength of 365 nm, the copper-clad laminate was heated at 170° C. for 1 hour to obtain a cured product on the copper-clad laminate, which was then used as a “laminate for evaluation.”

[0139] (Photovia formation process (2)) The laminate for evaluation was irradiated with 210 mJ / cm 2 from above the carrier film using an i-line stepper (UX-7, manufactured by Ushio Inc.) using a step tablet and a via evaluation mask. 2 The film was exposed to a 365 nm wavelength. After the carrier film was peeled off, a spray developer was used to perform development at 30° C. for 40 seconds in a 1% by mass aqueous solution of sodium carbonate, forming a via having a size of approximately 60 μm. For Examples 2 and 11, images of the vias obtained by scanning electron microscope (SEM) measurement (magnification: 2,500 times) are shown in FIGS. 7 and 8, respectively. In FIG. 7 (Example 2), the opening diameter of the via top was 55.6 μm, and the opening diameter of the via bottom was 53.6 μm. In FIG. 8 (Example 11), the opening diameter of the via top was 56.0 μm, and the opening diameter of the via bottom was 53.8 μm. In both cases, it can be seen that the resolution of the vias is excellent.

[0140] (Roughening treatment step (3-1); roughening treatment using a roughening solution) Next, first, 2 L of "Swelling Dip Securigant MV" (trade name, manufactured by Atotech Japan Co., Ltd.) [sodium hydroxide concentration: 3 g / L] containing sodium hydroxide was heated to 70° C., and the laminate for evaluation was immersed in the solution for 5 minutes. Thereafter, the laminate was washed in stored water at 25° C. for 1 minute, and then washed in running water at 25° C. for 3 minutes. Next, 2 L of "Dosing Securigant PMV" (trade name, manufactured by Atotech Japan Co., Ltd.) containing sodium hydroxide as a roughening solution (sodium hydroxide concentration: 40 g / L) was heated to 60°C, and the evaluation laminate was immersed in the solution for 5 minutes. After that, the laminate was washed with pure water at 70°C for 1 minute.

[0141] (Particle (X) dissolving step (3-2); although particles (X) were not used in each comparative example, this step was carried out in the same manner as in the examples.) Next, "Reduction Solution Securigant MV" (product name, manufactured by Atotech Japan Co., Ltd.) (total volume: 2,000 ml) to which an aqueous sulfuric acid solution was added so that the sulfuric acid concentration was 48 ml / L was heated to the temperature shown in Table 1, and the evaluation laminate was then immersed in it for the time shown in Table 1. Thereafter, it was washed in stored water at 25°C for 1 minute, and then washed with running water at 25°C for 3 minutes. This evaluation laminate after the particle (X) dissolving step (3-2) is referred to as evaluation laminate A. Here, in Examples 2, 5, 8, and 11 and Comparative Example 5, scanning electron microscope (SEM) measurements were performed on the surfaces of the evaluation laminate A, and surface images were taken. The results are shown in Figures 9 to 13.

[0142] (Circuit pattern formation process (4)) Next, the laminate was treated with an alkaline cleaner "Cleaner Securigant 902" (trade name, manufactured by Atotech Japan Co., Ltd.) at 60°C for 5 minutes, and then degreased and washed. After washing, the evaluation laminate was treated with a pre-dip liquid "Pre-dip Neoganth B" (trade name, manufactured by Atotech Japan Co., Ltd.) at 23°C for 1 minute. Thereafter, the evaluation laminate was treated with an activator liquid "Activator Neoganth 834" (trade name, manufactured by Atotech Japan Co., Ltd.) at 35°C for 5 minutes, and then the evaluation laminate was treated with a reducing liquid "Reducer Neoganth WA" (trade name, manufactured by Atotech Japan Co., Ltd.) at 30°C for 5 minutes. The evaluation laminate thus obtained was placed in a chemical copper solution (Basic Printganth MV-TP1, Copper Printganth MV-TP1, Moderator Printganth MV-TP1, Stabilizer Printganth MV-TP1, Reducer Cu (all trade names manufactured by Atotech Japan Co., Ltd.) and sodium hydroxide) and electroless plating was performed until the plating thickness reached about 0.5 μm. After the electroless plating, an annealing treatment was performed at a temperature of 120 ° C for 30 minutes to remove the remaining hydrogen gas. Thereafter, copper sulfate electrolytic plating was performed, and an annealing treatment was performed at 180 ° C for 60 minutes to form a conductor layer with a thickness of 25 μm. This evaluation laminate is referred to as Evaluation Laminate B. Thereafter, a circuit pattern was formed by a semi-additive process on the evaluation laminate B. The measurement and evaluation results are shown in Table 1.

[0143] [Table 1]

[0144] The components used in Table 1 are as follows: [(A) Photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent] · A1: the photopolymerizable compound (A1) having an ethylenically unsaturated group and an acidic substituent obtained in Synthesis Example 1, which contains an alicyclic skeleton. A2: the photopolymerizable compound (A2) having an ethylenically unsaturated group and an acidic substituent obtained in Synthesis Example 2, which does not contain an alicyclic skeleton.

[0145] [(B) Thermosetting resin] B1: "YX-4000" (Mitsubishi Chemical Corporation, biphenyl aralkyl type epoxy resin, epoxy equivalent: 180-192g / eq)

[0146] [(C) Crosslinking agent] · C1; "DPHA" (Dipentaerythritol hexaacrylate) · C2; "TMPTA" (trimethylolpropane triacrylate)

[0147] [(D) Elastomer] D1: "Ricon (registered trademark) 131MA17" (Cray Valley Corporation, maleic acid modified polybutadiene, number average molecular weight 54,000 (catalog value))

[0148] [(X) Particles (particles that dissolve at 95% by mass or more in a sulfuric acid aqueous solution with a concentration of 5 to 100 ml / L at 70°C for 20 minutes)] X1: Magnesium hydroxide 1: "ECOMAG (registered trademark) Z-10" (magnesium hydroxide, volume average particle size 1.2 μm, manufactured by Tateho Chemical Industries Co., Ltd.) ·X2: "Magthermo MS-S" (magnesium carbonate, volume average particle size 1.2 μm, manufactured by Konoshima Chemical Co., Ltd.) ·X3; "LPZINC-KS-2" (zinc oxide, volume average particle size 2 μm, manufactured by Sakai Chemical Industry Co., Ltd.) ·X4: Magnesium hydroxide 2: "Magseeds (registered trademark) V-6F" (magnesium hydroxide, volume average particle size 0.9 μm, manufactured by Konoshima Chemical Co., Ltd.)

[0149] [(E) Inorganic filler] E1: Spherical fused silica (volume average particle size 0.5 μm)

[0150] [(I) Photopolymerization initiator] I1; Photopolymerization initiator 1: 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, acetophenone-based compound I2: Photopolymerization initiator 2: 2,4-diethylthioxanthone, thioxanthone compounds

[0151] It can be seen from Table 1 that in Examples 1 to 12, the adhesive strength with the copper plating was successfully increased while keeping the surface roughness of the interlayer insulating layer small. This is presumably because the particles (X) present on the surface of the interlayer insulating layer were dissolved to form depressions, as shown in Figures 9 to 12. On the other hand, in Comparative Examples 1 to 3 in which particles (X) were used, the surface roughness was small due to the absence of particles, but in this case, the peel strength with the copper plating was extremely small. Also, in Comparative Examples 4 to 6 in which an inorganic filler other than particles (X) was used instead of particles (X), the peel strength with the copper plating was low when the surface roughness was small. As shown in FIG. 13, it is presumed that this is due to the presence of an inorganic filler on the surface of the interlayer insulating layer.

[0152] Example 13 and Comparative Example 7 In the same manner as in Example 1 and Comparative Example 4, each photosensitive resin film was produced, and a cured product was formed on a copper-clad laminate substrate through the lamination step (1) to obtain a "laminate for evaluation." Thereafter, the following operations were performed. (Roughening treatment step (3-1); dry etching) The surface of the laminate for evaluation obtained above was subjected to a plasma treatment using oxygen plasma under conditions of an output of 300 W, a temperature of 25° C., and a treatment time of 5 minutes. (Particle (X) Dissolving Process (3-2) and Circuit Pattern Forming Process (4)) Next, the sample was treated with an alkaline cleaner "Cleaner Securigant 902" (product name, manufactured by Atotech Japan Co., Ltd.) at 60°C for 5 minutes, then washed with stored water at 25°C for 1 minute, and then washed with running water at 25°C for 3 minutes. Here, in Example 13, the surface of the obtained evaluation laminate was measured with a scanning electron microscope (SEM) (magnification: 10,000 times), and a surface image was taken. The results are shown in Figure 14. Next, the surface of the evaluation laminate was treated with a mixed solution of sodium persulfate and an aqueous sulfuric acid solution (sulfuric acid concentration: 18.5 ml / L) at 27° C. for 30 seconds to perform soft etching and dissolve the particles (X). This treatment was carried out not only in Example 13 but also in Comparative Example 7, which did not use particles (X). Thereafter, the laminate was washed with stored water at 25° C. for 1 minute, and then washed with running water at 25° C. for 3 minutes. Here, in Example 13, the surface of the obtained evaluation laminate was measured with a scanning electron microscope (SEM) (magnification: 10,000 times), and a surface image was taken. The results are shown in FIG. 15. After the above treatment, the evaluation laminate was treated for 1 minute with a pre-dip liquid "Pre-dip Neoganth B" (trade name, manufactured by Atotech Japan Co., Ltd.) at 25° C. Then, the evaluation laminate was treated for 5 minutes with an activator liquid "Activator Neoganth 834" (trade name, manufactured by Atotech Japan Co., Ltd.) at 40° C., and then washed with stored water at 25° C. for 1 minute, and then washed with running water at 25° C. for 3 minutes. Next, the evaluation laminate was treated with a reducing solution "Reducer Neogant WA" (product name, manufactured by Atotech Japan Co., Ltd.) at 30°C for 5 minutes, rinsed in standing water at 25°C for 1 minute, and then rinsed in running water at 25°C for 3 minutes. The evaluation laminate thus obtained was placed in a chemical copper solution ("Basic Printganth MV-TP1", "Copper Printganth MV-TP1", "Moderator Printganth MV-TP1", "Stabilizer Printganth MV-TP1", "Reducer Cu" (all trade names manufactured by Atotech Japan Co., Ltd.) and sodium hydroxide) and electroless plating was performed until the plating thickness reached about 0.5 μm. After the electroless plating, an annealing treatment was performed at a temperature of 120 ° C for 30 minutes to remove the remaining hydrogen gas. Thereafter, copper sulfate electrolytic plating was performed, and an annealing treatment was performed at 180 ° C for 60 minutes to form a conductor layer with a thickness of 25 μm. This evaluation laminate is referred to as evaluation laminate C. Thereafter, a circuit pattern was formed by a semi-additive process on the evaluation laminate C. The measurement and evaluation results are shown in Table 2.

[0153] [Table 2]

[0154] From Table 2, it can be seen that in Example 13, as can be seen from the change in the surface of the interlayer insulating layer from FIG. 14 to FIG. 15, the particles (X) were dissolved after the particle (X) dissolving step (3-2), and as a result, it can be seen that it was possible to successfully increase the adhesive strength with the copper plating while keeping the surface roughness of the interlayer insulating layer small. On the other hand, in Comparative Example 7 in which an inorganic filler not corresponding to particles (X) was used instead of particles (X), the peel strength with the copper plating was low when the surface roughness was small.

[0155] Example 14 and Comparative Example 8 In the same manner as in Example 2 and Comparative Example 5, each photosensitive resin film was produced, and a cured product was formed on a copper-clad laminate substrate through the lamination step (1) to obtain a "laminate for evaluation." Thereafter, the following operations were performed. (Roughening treatment step (3-1); dry etching) The surface of the laminate for evaluation obtained above was subjected to a plasma treatment using oxygen plasma under conditions of an output of 300 W, a temperature of 25° C., and a treatment time of 5 minutes. (Particle (X) dissolution process (3-2)) The surface of the evaluation laminate that had been subjected to the plasma treatment was immersed in "Reduction Solution Securigant MV" (product name, manufactured by Atotech Japan K.K.) (total amount: 2,000 ml) to which an aqueous sulfuric acid solution had been added so that the sulfuric acid concentration was 49 ml / L, and the solution was heated to the temperature shown in Table 3, and the evaluation laminate was then immersed for the time shown in Table 3. This treatment was carried out not only in Example 14, but also in Comparative Example 8, which did not use particles (X). (Circuit pattern formation process (4)) Next, the substrate was treated with an alkaline cleaner "Cleaner Securigant 902" (product name, manufactured by Atotech Japan Co., Ltd.) at 60°C for 5 minutes, then washed with stored water at 25°C for 1 minute, and then washed with running water at 25°C for 3 minutes. Next, the surface of the evaluation laminate was treated with a mixed solution of sodium persulfate and an aqueous sulfuric acid solution (sulfuric acid concentration: 18.5 ml / L) at 27° C. for 0.5 minutes to perform soft etching. After that, it was washed with stored water at 25° C. for 1 minute, and then washed with running water at 25° C. for 3 minutes. After the above treatment, the evaluation laminate was treated for 1 minute with a pre-dip liquid "Pre-dip Neoganth B" (trade name, manufactured by Atotech Japan Co., Ltd.) at 25° C. Then, the evaluation laminate was treated for 5 minutes with an activator liquid "Activator Neoganth 834" (trade name, manufactured by Atotech Japan Co., Ltd.) at 40° C., and then washed with stored water at 25° C. for 1 minute, and then washed with running water at 25° C. for 3 minutes. Next, the evaluation laminate was treated with a reducing solution "Reducer Neogant WA" (product name, manufactured by Atotech Japan Co., Ltd.) at 30°C for 5 minutes, rinsed in standing water at 25°C for 1 minute, and then rinsed in running water at 25°C for 3 minutes. The evaluation laminate thus obtained was placed in a chemical copper solution ("Basic Printganth MV-TP1", "Copper Printganth MV-TP1", "Moderator Printganth MV-TP1", "Stabilizer Printganth MV-TP1", "Reducer Cu" (all trade names manufactured by Atotech Japan Co., Ltd.) and sodium hydroxide) and electroless plating was performed until the plating thickness reached about 0.5 μm. After the electroless plating, an annealing treatment was performed at a temperature of 120 ° C for 30 minutes to remove the remaining hydrogen gas. Thereafter, copper sulfate electrolytic plating was performed, and an annealing treatment was performed at 180 ° C for 60 minutes to form a conductor layer with a thickness of 25 μm. This evaluation laminate is referred to as evaluation laminate C. Thereafter, a circuit pattern was formed by a semi-additive process on the evaluation laminate C. The measurement and evaluation results are shown in Table 2.

[0156] [Table 3]

[0157] As can be seen from Table 3, in Example 14, the particles (X) were dissolved after the particle (X) dissolving step (3-2), and as a result, it can be said that the adhesion strength with the copper plating was successfully increased while keeping the surface roughness of the interlayer insulating layer small. On the other hand, in Comparative Example 8, in which an inorganic filler not corresponding to particles (X) was used instead of particles (X), the peel strength with the copper plating was low when the surface roughness was small. [Explanation of symbols]

[0158] 100A Printed Wiring Board 1 particle (X) 2. Depression 101 Substrate 102 Circuit Pattern 103 Interlayer insulation layer 104 Beer (Beer Hall) 105 Seed Layer 106 Resist Pattern 107 Copper circuit layer 108 Solder resist layer

Claims

1. A method for producing a printed wiring board, comprising the following (1) to (4): (1): A photosensitive resin film containing particles (X) that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70° C. for 20 minutes is laminated onto one or both sides of a circuit board. (2) Forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in (1) above. (3-1): Roughening the surfaces of the vias and the interlayer insulating layer. (3-2): Treating the roughened interlayer insulating layer with an acidic solution to dissolve the particles (X) present on the surface of the interlayer insulating layer. (4): Forming a circuit pattern on the interlayer insulating layer.

2. The method for producing a printed wiring board according to claim 1, wherein the roughening treatment in the step (3-1) is carried out using a roughening liquid.

3. The method for producing a printed wiring board according to claim 1, wherein the roughening treatment in the step (3-1) is carried out by dry etching.

4. 2. The method for producing a printed wiring board according to claim 1, wherein the surface roughness (Ra) of the interlayer insulating layer after the roughening treatment in (3-1) is 0.30 μm or less.

5. The method for producing a printed wiring board according to claim 1, wherein the acidic solution used in the step (3-2) contains an aqueous sulfuric acid solution.

6. The method for producing a printed wiring board according to claim 1, wherein the particles (X) have a volume average particle diameter of 0.1 to 3 μm.

7. 2. The method for producing a printed wiring board according to claim 1, wherein the photosensitive resin film contains 10 to 70 volume % of the particles (X).

8. A photosensitive resin composition comprising particles (X) that are soluble in an aqueous sulfuric acid solution having a concentration of 5 to 100 ml / L at 70° C. for 20 minutes at a rate of 95% by mass or more.

9. The photosensitive resin composition according to claim 8, further comprising (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a thermosetting resin.

10. The photosensitive resin composition according to claim 9, wherein the component (A) contains an alicyclic skeleton represented by the following general formula (A-1): [Formula 1] (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer from 0 to 6. * is a binding site to other structures.)

11. The photosensitive resin composition according to claim 8, wherein the particles (X) have an average particle size of 0.1 to 3 μm.

12. The photosensitive resin composition according to claim 8, wherein the content of the particles (X) is 10 to 70 volume % based on the total solid content.

13. A photosensitive resin composition for forming a photovia, comprising the photosensitive resin composition according to claim 8.

14. A photosensitive resin film comprising the photosensitive resin composition according to claim 8.

15. A printed wiring board comprising the photosensitive resin composition according to claim 8 or the photosensitive resin film according to claim 14.

16. A semiconductor package comprising the printed wiring board according to claim 15 and a semiconductor element.

Citation Information

Patent Citations

  • Thermosetting resin composition, multilayered printed wiring board, and preparation thereof

    JP1995304931A

  • Photosensitive additive adhesive composition

    JP2000104034A

  • Photosensitive resin composition and method for forming resin pattern using the composition

    JP2004233835A

  • Photosensitive resin composition, and dry film, printed wiring board and method for manufacturing printed wiring board using the composition

    JP2017116652A

  • Photosensitive resin film laminate

    JP2019061224A