Resin particle, method for producing resin particle, toner, method for producing toner, developer, toner storage unit, image formation device, and image formation method
By controlling the CH rate and BET specific surface area, resin particles with isoindoline pigments achieve improved coloring power and charging stability, overcoming dispersibility and reliability challenges.
Patent Information
- Application Number
- JP2023069549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional resin particles used in electrophotography, particularly those containing isoindoline skeleton pigments, face challenges in achieving high image quality and reliability due to low pigment dispersibility, leading to uneven pigment content and charging instability.
Resin particles are formulated with a specific CH rate (Content Heterogeneity rate) of 20.0% to 30.0% and a BET specific surface area of 0.80 m²/g to 1.60 m²/g, ensuring uniform pigment distribution and improved charging performance.
The formulation results in resin particles with enhanced coloring power and charging stability, addressing the issues of uneven pigment distribution and charging instability.
Smart Images

Figure 2024155119000003 
Figure 2024155119000004 
Figure 2024155119000005
Abstract
Description
[Technical field]
[0001] The present invention relates to resin particles, a method for producing resin particles, a toner, a method for producing a toner, a developer, a toner storage unit, an image forming apparatus, and an image forming method. [Background technology]
[0002] Resin particles are widely used as toner for image forming devices such as multi-function peripherals (MFPs) and printers in various places such as offices.
[0003] There is also a growing demand for high image quality, such as fine lines and color characteristics approaching those of offset printing. Color image formation by full-color electrophotography generally involves layering three color toners, the three primary colors of yellow, magenta, and cyan, or four color toners, including black, to reproduce all colors.
[0004] As resin particles used in full-color electrophotography, a toner master batch containing a resin, a colorant, and a plasticizer is mixed with a binder resin, and the mixture is dispersed and emulsified in an aqueous medium to produce a resin emulsion, and an electrophotographic toner has been disclosed in which the aggregation of pigments is suppressed and the dispersibility of the pigments is improved by aggregating and coalescing the emulsified particles in the resulting resin emulsion (see Patent Document 1).
[0005] However, conventional resin particles cannot fully satisfy the demands for high image quality and high reliability. In particular, a yellow pigment having an isoindoline skeleton is a colorant that has excellent weather resistance and coloring power, but has relatively low dispersibility, so that resin particles containing the pigment may have difficulty in fully utilizing the inherent coloring power of the pigment due to variations in the pigment content per resin particle.
[0006] Furthermore, resin particles containing the pigment may have differences in material composition between resin particles due to issues with the dispersibility of the pigment, which may result in reduced charging stability or weak or reverse charging, which may cause problems in terms of reliability. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of one aspect of the present invention is to provide resin particles having excellent coloring power and electrostatic chargeability. [Means for solving the problem]
[0008] One embodiment of the resin particles according to the present invention is a resin particle including at least a binder resin and a colorant, the colorant including a pigment having an isoindoline skeleton, and a 950 cm -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by the following (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of a CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. CH rate (%)=[(In-Iave) / Iave]×100...(Formula 1) Effect of the Invention
[0009] One aspect of the present invention can provide resin particles having excellent coloring power and electrostatic chargeability. [Brief description of the drawings]
[0010] [Figure 1] FIG. 13 is a diagram for explaining a method for calculating a wave number k. [Diagram 2] FIG. 1 is a diagram illustrating a normalization method in which the intensity at wave number k is set to 1. [Diagram 3] FIG. 1 is a diagram illustrating a method for calculating an average spectral intensity at wave numbers of 2750 cm −1 to 3250 cm −1 . [Figure 4] FIG. 13 is a diagram for explaining a method for calculating a CH ratio from the difference between the average spectrum and the normalized spectrum of a particle (n). [Diagram 5] FIG. 2 is a diagram showing an example of a cross section of a resin particle according to an embodiment. [Figure 6] FIG. 1 is a schematic diagram illustrating an example of an image forming apparatus according to an embodiment. [Figure 7] FIG. 2 is a schematic diagram illustrating an example of a process cartridge according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the embodiments of the present invention will be described in detail. Note that the embodiments are not limited by the following description, and can be appropriately modified without departing from the gist of the present invention. In addition, in this specification, "to" indicating a numerical range means that the numerical values before and after it are included as the lower and upper limits, unless otherwise specified.
[0012] <Resin particles> The resin particles of this embodiment contain at least a binder resin and a colorant. The colorant contains a pigment having an isoindoline skeleton, and the percentage of resin particles having an absolute value of a "CH ratio" described below of 20.0% or more with respect to the total number of resin particles is 1.0% by number or more and 30.0% by number or less. Furthermore, the resin particles have a BET specific surface area of 0.80 m 2 / g or more, 1.60m 2 / g or less.
[0013] (CH rate summary) The CH ratio is an acronym for Content Heterogeneity, and is an index defined to evaluate the heterogeneity of the raw material content in resin particles. It evaluates how much the raw material content of each resin particle deviates from the raw material content at the time of resin particle production, compared with the raw material content at the time of resin particle production. It is naturally preferable that the raw material content of each resin particle does not deviate from the raw material content at the time of resin particle production.
[0014] (Calculation method of CH rate) The CH ratio is calculated from the Raman spectrum of the resin particles. -1 ~3250cm -1 The wave number at which the total intensity of the Raman spectra of the resin particles is maximized is defined as k. When the intensity of the Raman spectrum of each resin particle at wave number k is normalized to 1, the maximum value is obtained at 2750 cm -1 ~3250cm -1 When the integrated intensity of the spectrum of each resin particle obtained in the wave number region is In and the average value of In is Iave, the value is represented by the following formula (1). CH rate (%)=[(In-Iave) / Iave]×100...(Formula 1)
[0015] The Raman spectrum is measured using a Raman microscope. The device used is not particularly limited, but for example, "XploRA PLUS" (manufactured by Horiba, Ltd.) is used for the measurement. The Raman spectrum is measured for each resin particle, and after obtaining spectra for 500 to 600 particles, the CH ratio is calculated by the above-mentioned (Equation 1).
[0016] (Raman spectrum measurement conditions) The Raman spectrum is measured under the following measurement conditions. (1) Selection of excitation laser A laser with an excitation wavelength of 638 nm is used to measure the Raman spectrum. The Raman spectrum is measured by irradiating the laser on each resin particle. The laser intensity is adjusted so that the resin particles do not melt. (2) Number of particles measured Since the spectral shape differs slightly for each resin particle, 500 to 600 resin particles are measured to evaluate the variation. By measuring 500 to 600 resin particles, the measurement variation converges, making it possible to compare different resin particles. (3) Wavenumber range to be measured Analysis is 950cm -1 ~3250cm -1Since the Raman spectrum is measured using the wavelength range of 200 cm, it is necessary to measure the wave number range including this range. Since the fluorescence spectrum is also likely to be measured at the same time when the Raman spectrum is measured, it is preferable to measure in a wave number range wider than the wave number range to be analyzed in order to make it easier to remove the fluorescence spectrum. -1 ~3800cm -1 It is preferable to measure in the region of about 100 nm. (4) Focus adjustment conditions Adjust so that the outermost surface of the resin particles is in focus. (5) Other settings Other measurement conditions related to the resolution of the Raman spectrum were as follows: the objective lens was set at 50x magnification, and the plot interval in the axial direction (X-axis direction) showing the wave number in the Raman spectrum was 3cm. -1 ~4cm -1 Measurements are performed with a resolution setting of approximately 100 kHz.
[0017] (How to make the sample) In order to measure individual resin particles, a sample is prepared by dispersing the resin particles on a glass slide.
[0018] (Raman spectrum correction) Since Raman spectra are affected by fluorescence and noise, it is desirable to perform baseline correction of the spectrum data. Although there are no particular limitations on the method of baseline correction, an example of the correction method is shown below.
[0019] The baseline correction of the spectrum is performed, for example, using the software "Labspec6.0" (manufactured by Horiba, Ltd.). (1) The wavenumber region of the measured Raman spectrum is 200 cm -1 ~3800cm -1 Extract with. (2) Perform baseline correction on (1) above with the following settings: “order: 9,” “maximum score: 57,” and “noise score: 4.” (3) The wave number region of the spectrum of (2) is 950 cm -1 ~3250cm -1 Extract again with.
[0020] (Normalization of Raman spectra) Since the intensity of the Raman spectrum varies depending on the size and shape of the measurement target, the type of raw material, etc., it is not possible to simply compare the Raman spectrum intensities of different resin particles. Therefore, normalization processing is performed on the Raman spectrum so that different resin particles can be compared. Normalization processing is performed using data editing software (such as Excel) on the spectrum whose baseline has been corrected as described above.
[0021] The normalization is performed by the following method: Fig. 1 is a diagram for explaining a method for calculating the wave number k, and Fig. 2 is a diagram for explaining a normalization method for making the intensity at the wave number k 1. (1) As shown in Figure 1, all the Raman spectra are added together to calculate the total spectrum, and the wavenumber k at which the total spectrum shows maximum intensity is determined. (2) As shown in Figure 2, for the Raman spectrum of the nth particle, a correction coefficient X(n) is calculated so that the intensity of wave number k becomes 1, and the spectral intensity is normalized by multiplying the entire wave number range by the correction coefficient X(n). Hereinafter, the normalized Raman spectrum is called the normalized spectrum. This is performed on the Raman spectra of all measured resin particles.
[0022] (Noise data removal process) In measuring Raman spectra, data that becomes noise due to dust or other substances may be obtained. If such data is added to the calculation of the CH ratio, an accurate evaluation may not be possible. Therefore, the noise data is excluded as follows.
[0023] For the normalized spectrum of the nth particle in (2) in the normalization of the Raman spectrum, the spectral area S(n) is calculated. This is performed for all particles measured. The standard deviation σ(S) of S(n) for all particles is calculated, and particles (n) that do not satisfy the following (Equation 2) are treated as error data and excluded from the calculation of the CH rate. S(n)-2×σ(S)≦S(n)≦S(n)+2×σ(S) (Formula 2)
[0024] (Calculation of CH rate) Figure 3 shows the wave number of 2750 cm -1 ~3250cm -1 FIG. 3 is a diagram illustrating a method for calculating the average spectrum intensity at 2750 cm in FIG. -1 ~3250cm -1 The area shown is the area shown in Fig. 1. The average spectrum is calculated using the normalized spectrum of the particle (n) that was not excluded by the noise data elimination process (the normalized spectrum of one particle after the noise data elimination process).
[0025] Fig. 4 is a diagram for explaining a method for calculating the CH ratio from the difference between the average spectrum and the normalized spectrum of a particle (n). Specifically, Fig. 4 shows the average spectrum obtained in Fig. 3 and the normalized spectrum of a particle (n) lined up in the diagram.
[0026] Particle (n) 2750cm -1 ~3250cm -1 The integral intensity In of the normalized spectrum at was calculated, and the average value was calculated using the In of all particles to obtain Iave. The wavenumber of the particle (n) and the average spectrum was 2750 cm -1 ~3250cm -1 The difference in integrated intensity at is In-Iave. The CH rate is calculated as the rate of change relative to the average using the following (Equation 1). CH rate (%)=[(In-Iave) / Iave]×100...(Formula 1) Normalized spectrum of In:n particles at 2750 cm -1 ~3250cm -1 Integral intensity of Iave: Average value of In for all particles
[0027] Since the intensity of the Raman spectrum varies depending on the type of raw material used, the CH ratio is not calculated as the difference between In and Iave, but is calculated as the rate of change as shown in (Equation 1) using the same concept as the coefficient of variation (CV). -1 ~3250cm-1 By performing the analysis using this range, it is possible to accurately evaluate the variation in the content of raw materials other than the colorant.
[0028] As a result of extensive investigations into obtaining excellent coloring power and electrostatic charge performance, the present inventors have found that it is important that the proportion of particles having a CH ratio, which indicates the non-uniformity of the resin component content in resin particles, of particles having an absolute value of 20.0% or more is 1.0% by number or more and 30.0% by number or less, and preferably 5.0% by number or more and 25.0% by number or less.
[0029] If the number of particles having an absolute value of a CH ratio of 20.0% or more exceeds 30.0%, the colorant content among the resin particles will vary, and the resin particles will not be able to exhibit the inherent coloring power of the colorant, and the color development will be insufficient.
[0030] In order to obtain coloring power, it is possible to increase the formulation amount of the colorant itself, but this is not preferable in terms of the particle size distribution of the resin particles, low-temperature fixability, and cost. In addition, if the number of particles having an absolute value of CH ratio of 20.0% or more exceeds 30.0%, this is also not preferable in terms of stabilizing the charge amount of the resin particles.
[0031] On the other hand, if the number of particles having an absolute value of a CH ratio of 20.0% or more is less than 1.0%, the dam of the cleaning blade portion may be insufficient, which may result in poor cleaning.
[0032] The number ratio of resin particles having an absolute value of CH ratio of 35.0% or more to all resin particles is preferably 7.0% or less by number, more preferably 5.0% or less by number. It has been found that in particles having an absolute value of CH ratio of 35.0% or more, deviation from the target physical properties becomes more noticeable due to variation in the content of raw materials among resin particles.
[0033] For example, such particles tend to be weakly or reversely charged, and also cause defects in other physical properties due to deviation from the target central value. By reducing the number ratio of particles with an absolute CH ratio of 35.0% or more, it is possible to increase the uniformity of charging performance, especially between resin particles, and improve reliability.
[0034] Therefore, when the proportion by number of resin particles having an absolute value of a CH ratio of 35.0% or more to all resin particles is 7.0% by number or less, the resin particles can exhibit superior charging performance.
[0035] (Method of measuring BET specific surface area) The BET specific surface area is measured by using a BET specific surface area measuring device for resin particles. There is no particular designation for the device, but for example, a Macsorb model-1201 manufactured by MOUNTECH can be used. Approximately 1 g of resin particles is used, and the measurement is performed after removing impurities and moisture in a pretreatment.
[0036] The BET specific surface area specified in the present invention is that in the state where no external additive treatment is performed. For resin particles to which an external additive has already been attached, the external additive can be released and then measured. As a method for releasing the external additive, for example, the resin particles are dispersed in water using a surfactant, and then ultrasonic waves are applied. Also, the method is not limited to this, and may be performed by a known method.
[0037] The BET specific surface area of the resin particles of this embodiment is 0.80 m 2 / g or more, 1.60m 2 / g or less. The BET specific surface area of the resin particles is 1.60 m 2 If the surface shape of the resin particles is more than 100 μm / g, in an environment in which the resin particles are stirred for a long time in the development section of an image forming apparatus, or in an environment in which stirring stress is high such as in a high-speed machine, the function of the external additive will be reduced due to the embedding of small particle diameter external additives and rolling into recesses, and the charging ability of the resin particles will change, resulting in reduced charging performance.
[0038] When the charging performance of the resin particles is reduced, the transfer efficiency is likely to be reduced. In addition, in terms of suppressing embedding and rolling, the formulation conditions in which the ratio of external additives with large particle diameters is increased are not preferable because the effect of improving the fluidity is insufficient and problems arise in the replenishment of the resin particles.
[0039] The BET specific surface area of the resin particles is 0.80m 2 If it is less than 1 / g, the fluidity is reduced, which reduces the replenishing ability of the resin particles, and the adhesive strength of the external additive is reduced, which causes filming on the photoconductor and reduces the cleaning ability. In addition, the reduced contact area with the carrier and the reduced fluidity may affect the start of charging, and the charging performance is reduced, which is not preferable.
[0040] Therefore, the BET specific surface area of the resin particles is 0.80 m 2 / g or more, 1.60m 2 / g or less, the resin particles can exhibit excellent coloring power and electrostatic charge performance.
[0041] The BET specific surface area of the resin particles is preferably 0.80 m 2 / g or more, 1.40m 2 / g or less, more preferably 1.00m 2 / g or more, 1.40m 2 The BET specific surface area of the resin particles is 0.80 m 2 / g or more, 1.40m 2 / g or less, the resin particles can exhibit excellent coloring power and more excellent electrostatic charge performance.
[0042] The BET specific surface area can be adjusted using various known methods. In the chemical method, for example, the BET specific surface area can be adjusted by heating a resin particle dispersion at a temperature close to the glass transition temperature Tg of the resin. In the aggregation method involving aggregation or coalescence, the BET specific surface area can be adjusted by the temperature and heating time in the fusion step described below, and it is particularly easy to obtain resin particles with a low BET specific surface area.
[0043] (Colorant presence rate on the surface of resin particles) Fig. 5 is a diagram showing an example of a cross section of a resin particle according to an embodiment. As shown in Fig. 1, when the major axis of the cross section of the resin particle 100 is L, and the center 101 of a circle C having a radius r of L / 10 moves along the contour of the cross section of the resin particle 100, the cross section of the resin particle 100 overlaps with the cross section of the resin particle 100 in ...
[0044] Here, the area of the pigment 103 having an isoindoline skeleton in the surface layer 102 of the resin particle relative to the total area of the pigment 103 having an isoindoline skeleton in the cross section of the resin particle 100 means the colorant presence rate in the surface layer 102 of the resin particle.
[0045] With the area of the pigment 103 having an isoindoline skeleton in the surface layer 102 of the resin particle being less than 30.0% of the total area of the pigment 103 having an isoindoline skeleton in the cross section of the resin particle 100, the colorant ratio in the surface layer 102 of the resin particle is reduced and the colorant is dispersed and arranged even inside the resin particle 100, thereby allowing the coloring power and color development properties inherent to the colorant to be fully exhibited. Furthermore, the variation in resistance caused by the uneven distribution of the colorant in the surface layer portion can be suppressed, and the charge distribution can be narrowed and the function can be stabilized.
[0046] In other words, the resin particles can achieve a uniform colorant content among the resin particles, and can also suppress uneven distribution of the colorant per particle, thereby achieving superior coloring power and charging performance.
[0047] (Method of calculating the colorant presence rate on the surface of resin particles) A method for measuring the ratio of a colorant containing a pigment having an isoindoline skeleton present in the surface layer of a resin particle in a cross-sectional image of the resin particle (hereinafter, sometimes referred to as "colorant surface layer uneven distribution ratio") will be described. First, a method for obtaining a cross-sectional image of a resin particle will be described.
[0048] After embedding the resin particles in epoxy resin, a thin section having a thickness of 0.1 μm to 0.2 μm is prepared using a microtome (e.g., a diamond knife (blade angle 45°)), and a cross-sectional image is obtained using a microscope such as an optical microscope, a fluorescent microscope, a scanning electron microscope (SEM), or a transmission electron microscope (TEM). For example, SEM observation can be performed at an acceleration voltage of 50 to 200 kV, and TEM observation can be performed at an acceleration voltage of 0.8 to 2 kV. In this case, the cross section of the resin particles can be obtained by cooling using ion milling in addition to the microtome.
[0049] After obtaining a cross-sectional image of the resin particle, the amount of the pigment having an isoindoline skeleton in the cross-section of the resin particle is measured by the following procedure: The cross-sectional image of the resin particle can be observed by a TEM at a magnification of 10K and an accelerating voltage of 0.8 to 2 kV. (1) Extract 10 resin particles having an average volume particle size Dv±1 μm. (2) Using the image analysis software "Image-Pro Premier," the contours are extracted from the cross-sectional images of the resin particles. (3) As with (2), the contours of the colorants are extracted from the contrast. (4) As shown in FIG. 5, when the major axis of a resin particle 100 is L, the center 101 of a circle C having a radius r (L / 10) is moved along the contour of the cross section of the resin particle 100. (5) The overlapping region where the cross section of the resin particle 100 overlaps with the passing region of the circle C is defined as the resin particle surface layer 102, and the area of the pigment 103 having an isoindoline skeleton in the resin particle surface layer 102 is calculated. (6) The area of all cross sections of the pigment 103 having an isoindoline skeleton present in the cross-sectional image of the resin particle 100 is calculated. (7) The ratio of the area of the pigment 103 having an isoindoline skeleton in the surface layer 102 of the resin particle to the total area of the pigment 103 having an isoindoline skeleton in the cross section of the resin particle is calculated. (8) The above steps (2) to (7) are repeated for 10 resin particles, and the average value obtained is taken as the colorant abundance rate in the surface layer 102 of the resin particle.
[0050] As described above, the resin particles according to this embodiment contain a binder resin and a pigment having an isoindoline skeleton as a colorant, and may contain other components as necessary.
[0051] (Binding resin) The binder resin used in this embodiment may be any resin that is soluble in an organic solvent and insoluble or almost insoluble in water. Examples of the binder resin include polyester resin, polystyrene resin, polyvinyl chloride resin, polyvinyl acetate resin, polyethylene resin, polyurethane resin, polyamide resin, epoxy resin, polyethylene terephthalate (PET), styrene-acrylic acid copolymer, polymethacrylic acid ester resin, polymethyl acrylate (PMA), polyacrylic acid ester, polyacrylonitrile (PAN), paraffin wax, etc. These may be used alone or in combination.
[0052] When the resin particles are used as a toner for developing electrostatic latent images in electrophotography, good fixability can be obtained by using a resin having a polyester skeleton. The resin having a polyester skeleton includes polyester resin and block polymers of polyester and resins having other skeletons, but the polyester resin is preferred because the obtained resin particles are more uniform. As the polyester resin, linear polyester resin is preferred, and unmodified polyester resin is also preferred.
[0053] Here, the unmodified polyester resin is a polyester resin obtained by using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, and is not modified by an isocyanate compound, etc. In addition, it is preferable that the unmodified polyester resin does not have a urethane bond or a urea bond.
[0054] The binder resin is preferably an amorphous polyester resin, which is soluble in tetrahydrofuran (THF) and chloroform, because it provides good fixability.
[0055] ((Amorphous polyester resin)) Examples of amorphous polyester resins include ring-opening polymerization products of lactones, condensation polymerization products of hydroxycarboxylic acids, and polycondensation products of polyols and polycarboxylic acids. From the viewpoint of freedom in design, polycondensation products of polyols and polycarboxylic acids are preferred.
[0056] The weight average molecular weight (Mw) of the amorphous polyester resin is usually 1000 to 30000, preferably 3000 to 15000, and more preferably 5000 to 12000. When the weight average molecular weight (Mw) is 1000 or more, it is possible to suppress a decrease in heat-resistant storage stability. When the weight average molecular weight (Mw) is 30000 or less, it is possible to suppress an increase in the viscoelasticity of the resin particles when melted, and to suppress a decrease in the low-temperature fixability of the resin particles.
[0057] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 35°C to 80°C, more preferably 40°C to 70°C, and even more preferably 45°C to 65°C. When the glass transition temperature (Tg) is 35°C or higher, the resulting resin particles are less likely to deform when placed in a high-temperature environment such as midsummer, or the resin particles are less likely to stick to each other and not be able to behave as intended resin particles. When the glass transition temperature (Tg) is 80°C or lower, deterioration of fixability can be suppressed when the resin particles are used as a toner for developing electrostatic latent images.
[0058] -Polyol- The polyol may be a diol or a trihydric or higher polyol, and a diol alone or a mixture of a diol and a small amount of a trihydric or higher polyol is preferred.
[0059] Examples of diols include alkylene glycols (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, etc.); alkylene ether glycols (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, neopentyl glycol, etc.); alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.); bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.); alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of alicyclic diols; 4,4'-dihydroxybiphenyls (3,3' -difluoro-4,4'-dihydroxybiphenyl, etc.); bis(hydroxyphenyl)alkanes (bis(3-fluoro-4-hydroxyphenyl)methane, 1-phenyl-1,1-bis(3-fluoro-4-hydroxyphenyl)ethane, 2,2-bis(3-fluoro-4-hydroxyphenyl)propane, 2,2-bis(3,5-difluoro-4-hydroxyphenyl)propane (also known as tetrafluorobisphenol A), 2,2-bis(3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, etc.); bis(4-hydroxyphenyl)ethers (bis(3-fluoro-4-hydroxyphenyl)ether, etc.); alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of bisphenols, etc. Among these, the diol is preferably an alkylene glycol having 2 to 12 carbon atoms or an alkylene oxide adduct of a bisphenol, and particularly preferably an alkylene oxide adduct of a bisphenol or a combination of the alkylene oxide adduct and an alkylene glycol having 2 to 12 carbon atoms.
[0060] Examples of trihydric or higher polyols include trihydric to octahydric or higher polyhydric aliphatic alcohols (glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, etc.); trihydric or higher phenols (trisphenol PA, phenol novolac, cresol novolac, etc.); and alkylene oxide adducts of trihydric or higher polyphenols.
[0061] -Polycarboxylic acid- The polycarboxylic acid may be a dicarboxylic acid or a tri- or higher carboxylic acid. A dicarboxylic acid alone or a mixture of a dicarboxylic acid and a small amount of a tri- or higher carboxylic acid is preferred.
[0062] Examples of dicarboxylic acids include alkylene dicarboxylic acids (succinic acid, adipic acid, sebacic acid, etc.); alkenylene dicarboxylic acids (maleic acid, fumaric acid, etc.); aromatic dicarboxylic acids (phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, etc.); 3-fluoroisophthalic acid, 2-fluoroisophthalic acid, 2-fluoroterephthalic acid, 2,4,5,6-tetrafluoroisophthalic acid, 2,3,5,6-tetrafluoroterephthalic acid, 5-trifluoromethylisophthalic acid, Examples of the modified purified rosin include 2,2-bis(4-carboxyphenyl)hexafluoropropane, 2,2-bis(3-carboxyphenyl)hexafluoropropane, 2,2'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 3,3'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 2,2'-bis(trifluoromethyl)-3,3'-biphenyldicarboxylic acid, and hexafluoroisopropylidenediphthalic anhydride. The modified purified rosin is preferably one modified with acrylic acid, fumaric acid, or maleic acid. Of these, the dicarboxylic acid is preferably an alkenylene dicarboxylic acid having 4 to 20 carbon atoms and an aromatic dicarboxylic acid having 8 to 20 carbon atoms.
[0063] Examples of trivalent or higher polycarboxylic acids include aromatic polycarboxylic acids having 9 to 20 carbon atoms (eg, trimellitic acid, pyromellitic acid, etc.).
[0064] As the polycarboxylic acid, an acid anhydride or a lower alkyl ester (methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned polycarboxylic acid may be used to react with the above-mentioned polyol.
[0065] The ratio of polyol to polycarboxylic acid, expressed as the equivalent ratio [OH] / [COOH] of the hydroxyl group [OH] to the carboxyl group [COOH], is usually 2 / 1 to 1 / 2, preferably 1.5 / 1 to 1 / 1.5, and more preferably 1.3 / 1 to 1 / 1.3.
[0066] (Coloring agent) The colorant contained in the resin particles of this embodiment includes a pigment having an isoindoline skeleton. The pigment having an isoindoline skeleton (isoindoline-based pigment) is used as a yellow pigment colorant. As the isoindoline-based pigment, CI Pig.Y-185 or the like having a vivid yellow color can be used.
[0067] Because of their skeleton, isoindoline pigments have excellent weather resistance and high coloring power among azo pigments, and therefore the resin particles containing a pigment having an isoindoline skeleton have excellent coloring power.
[0068] In addition, since isoindoline pigments have high transmittance in the visible range of 500 nm to 700 nm on the long wavelength side, they also have good color development properties for secondary colors.
[0069] As the colorant, known pigments other than isoindoline pigments can be used in combination. For example, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, and mixtures thereof can be used.
[0070] The content of the colorant in the resin particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass to 15 parts by mass, more preferably 3 parts by mass to 10 parts by mass, relative to 100 parts by mass of the resin particles. By having the content of the colorant in the resin particles be 1 part by mass to 15 parts by mass, relative to 100 parts by mass of the resin particles, the resin particles can exhibit better coloring power.
[0071] The colorant can also be used as a masterbatch composited with a resin. The resin to be produced by the masterbatch or kneaded with the masterbatch is not particularly limited and can be appropriately selected according to the purpose. For example, in addition to the above-mentioned amorphous polyester resin, polymers of styrene or its substitutes, styrene-based copolymers, polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resins, epoxy polyol resins, polyurethane, polyamide, polyvinyl butyral, polyacrylic acid resins, rosin, modified rosin, terpene resins, aliphatic or alicyclic hydrocarbon resins, aromatic petroleum resins, chlorinated paraffin, or paraffin wax can be mentioned. These may be used alone or in combination of two or more.
[0072] Polymers of styrene or its substitutes include, for example, polystyrene, poly-p-chlorostyrene, or polyvinyltoluene.
[0073] Examples of styrene-based copolymers include styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-butyl acrylate copolymers, styrene-octyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-acrylonitrile-indene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers.
[0074] The method for producing the masterbatch is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a method in which a resin for the masterbatch and a colorant are mixed and kneaded by applying high shear force. In this case, an organic solvent can be used to enhance the interaction between the colorant and the resin.
[0075] Another method is the so-called flushing method, in which an aqueous paste containing a water-containing colorant is mixed and kneaded with a resin and an organic solvent to transfer the colorant to the resin side and remove the water and organic solvent components. The flushing method is preferable because it does not require drying since the wet cake of the colorant can be used as is. A high-shear dispersion device such as a three-roll mill is preferably used for mixing and kneading.
[0076] The use of the master batch reduces shock during dispersion of the isoindoline pigment in the oil phase, prevents aggregation of the isoindoline pigment, and improves the dispersibility of the isoindoline pigment, so that the resin particles according to this embodiment have better coloring power and charging performance. Furthermore, the resin particles according to this embodiment can be applied to a yellow toner, and a yellow toner containing the resin particles according to this embodiment has better coloring power and charging performance.
[0077] (Other Ingredients) Other components in the resin particles are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include crystalline resins, prepolymers, release agents, charge control agents, or deforming agents, shell agents for forming a core-shell structure, etc. These may be used alone or in combination of two or more.
[0078] (Crystalline Resin) The crystalline resin is not particularly limited as long as it has crystallinity, and can be appropriately selected according to the purpose, and examples thereof include polyester resin, polyurethane resin, polyurea resin, polyamide resin, polyether resin, vinyl resin, and modified crystalline resin. These may be used alone or in combination of two or more. Among these, crystalline resin is preferably crystalline polyester resin.
[0079] -Crystalline polyester resin- Crystalline polyester resins have high crystallinity and exhibit thermal melting properties that cause a sudden change in viscosity near the fixing start temperature. Crystalline polyester resins are polyester resins that are insoluble in tetrahydrofuran (THF) and soluble in chloroform. The resin particles contain crystalline polyester resins with such properties and amorphous polyester resins, and thus have both good heat resistance storage properties and low temperature fixing properties.
[0080] For example, by using a crystalline polyester resin and an amorphous polyester resin in combination, the heat resistance storage stability is good due to the crystallinity of the crystalline polyester resin until just before the melting start temperature, and at the melting start temperature, the viscosity drops sharply (sharp melt property) due to the melting of the crystalline polyester resin. The crystalline polyester resin is compatible with the amorphous polyester resin, and the viscosity of both drops sharply, allowing the resin particles to be fixed well.
[0081] Furthermore, the resin particles also show good results in terms of the release width (the difference between the minimum fixing temperature and the temperature at which high-temperature offset occurs).
[0082] The crystalline polyester resin can be obtained by using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof. These can be used alone or in combination of two or more kinds.
[0083] In this specification, the crystalline polyester resin refers to a resin obtained by using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, as described above, and modified polyester resins, such as prepolymers and resins obtained by subjecting the prepolymers to at least one of a crosslinking reaction and an elongation reaction, do not belong to the crystalline polyester resin category.
[0084] -Polyhydric alcohol- The polyhydric alcohol is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include diols and trihydric or higher alcohols. Examples of the diols include saturated aliphatic diols. Examples of the saturated aliphatic diols include linear saturated aliphatic diols and branched saturated aliphatic diols.
[0085] Among these, the saturated aliphatic diol is preferably a linear saturated aliphatic diol, and more preferably a linear saturated aliphatic diol having 2 to 12 carbon atoms. If the saturated aliphatic diol is a linear type, the crystallinity of the crystalline polyester resin is high, and the melting point is high. If the carbon number of the saturated aliphatic diol exceeds 12, it becomes difficult to obtain a practical material. It is more preferable that the carbon number of the saturated aliphatic diol is 12 or less.
[0086] Specific examples of saturated aliphatic diols include ethylene glycol, butylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosandecanediol. These may be used alone or in combination of two or more.
[0087] Among these, the saturated aliphatic diol is preferably ethylene glycol, butylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, or 1,12-dodecanediol, in that the crystalline polyester resin has high crystallinity and excellent sharp melting properties.
[0088] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. These polyhydric alcohols may be used alone or in combination of two or more.
[0089] -Polycarboxylic acids- The polycarboxylic acid is not particularly limited and may be appropriately selected depending on the purpose, and examples of the polycarboxylic acid include dicarboxylic acids, such as saturated aliphatic dicarboxylic acids, unsaturated aliphatic dicarboxylic acids, and aromatic dicarboxylic acids.
[0090] Examples of saturated aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, sebacic acid, adipic acid, and dodecanedioic acid. Examples of unsaturated aliphatic dicarboxylic acids include fumaric acid and maleic acid. Examples of aromatic dicarboxylic acids include terephthalic acid. These may be used alone or in combination of two or more.
[0091] The derivative of the polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. For example, a polycarboxylic acid anhydride or a polycarboxylic acid ester can be mentioned.
[0092] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms. This allows the crystalline polyester resin to have high crystallinity and excellent sharp melting properties, and therefore can exhibit excellent low-temperature fixing properties.
[0093] In addition, as a method for controlling the crystallinity and softening point of a crystalline polyester resin, there can be mentioned a method for designing and using a non-linear polyester by condensation polymerization in which a polyhydric alcohol having a valence of three or more, such as glycerin, is added to the alcohol component during polyester synthesis, or a polyvalent carboxylic acid having a valence of three or more, such as trimellitic anhydride, is added to the acid component.
[0094] The melting point of the crystalline polyester resin is not particularly limited and can be appropriately selected according to the purpose, but is preferably 60° C. or more and 80° C. or less. When the melting point of the crystalline polyester resin is 60° C. or more, the crystalline polyester resin can be prevented from melting at a low temperature and the heat-resistant storage stability of the resin particles can be prevented from decreasing. When the melting point of the crystalline polyester resin is 80° C. or less, the melting of the crystalline polyester resin due to heating during fixing can be improved, and the decrease in low-temperature fixability can be prevented.
[0095] The molecular weight of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. However, from the viewpoint that a low molecular weight resin with a sharp molecular weight distribution has excellent low-temperature fixability, and a large amount of components with a large molecular weight improves heat-resistant storage stability, the molecular weight of the crystalline polyester resin is preferably within the following range when measured by gel permeation chromatography (GPC) of the orthodichlorobenzene-soluble portion thereof.
[0096] The weight average molecular weight (Mw) of the crystalline polyester resin is preferably from 3,000 to 30,000, and more preferably from 5,000 to 25,000.The number average molecular weight (Mn) of the crystalline polyester resin is preferably from 1,000 to 10,000, and more preferably from 2,000 to 10,000.
[0097] The molecular weight ratio (Mw / Mn) of the crystalline polyester resin is preferably from 1.0 to 10, and more preferably from 1.0 to 5.0.
[0098] The acid value of the crystalline polyester resin is not particularly limited and can be appropriately selected according to the purpose, but the lower limit of the oxidation is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, in order to achieve the desired low-temperature fixability from the viewpoint of the affinity between the recording medium and the resin particles. Also, the upper limit of the acid value of the crystalline polyester resin is preferably 45 mgKOH / g or less, in order to improve the high-temperature offset resistance.
[0099] The oxidation of the crystalline polyester resin can be measured in accordance with the measurement method described in JIS K0070-1992.
[0100] The hydroxyl value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. In order to achieve the desired low-temperature fixability and good charging characteristics, the hydroxyl value is preferably more than 0 mgKOH / g and not more than 50 mgKOH / g, and more preferably more than 0 mgKOH / g and not more than 10 mgKOH / g.
[0101] The hydroxyl value of the crystalline polyester resin can be measured in accordance with the measurement method described in JIS K0070-1966.
[0102] The molecular structure of the crystalline polyester resin can be confirmed by measurement using nuclear magnetic resonance spectroscopy (NMR) in a solution or solid, as well as by measurement using X-ray diffraction, gas chromatography / mass spectrometry (GC / MS), liquid chromatography / MS, or infrared absorption spectroscopy (IR). -1 and 990±10cm -1 A simple method is to detect a crystalline polyester resin that has absorption due to olefin δCH (out-of-plane bending vibration).
[0103] The content of the crystalline polyester resin in the resin particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 3 parts by mass or more and 20 parts by mass or less, and more preferably 5 parts by mass or more and 15 parts by mass or less, per 100 parts by mass of the resin particles.
[0104] When the content of the crystalline polyester resin in the resin particles is 3 parts by mass or more, the sharp melting property due to the crystalline polyester resin can be improved, and the low-temperature fixing property can be improved. When the content of the crystalline polyester resin in the resin particles is 20 parts by mass or less, the deterioration of the heat-resistant storage stability can be suppressed, and the occurrence of fogging of the image can be suppressed.
[0105] When the content of the crystalline polyester resin in the resin particles is from 5 parts by mass to 15 parts by mass, it is advantageous in that both high image quality and low-temperature fixability are excellent.
[0106] ((Release Agent)) The release agent is not particularly limited and can be appropriately selected from known ones, for example, waxes, fatty acid amides, homopolymers or copolymers of polyacrylate, or crystalline polymers having long alkyl groups on the side chains. These may be used alone or in combination of two or more. These release agents are soluble in chloroform.
[0107] Examples of waxes include natural waxes, synthetic hydrocarbon waxes, and synthetic waxes other than synthetic hydrocarbon waxes.
[0108] Examples of natural waxes include vegetable waxes, animal waxes, mineral waxes, and petroleum waxes. Examples of vegetable waxes include carnauba wax, cotton wax, and wood wax. Examples of animal waxes include beeswax and lanolin. Examples of mineral waxes include ozokerite and cerusine. Examples of petroleum waxes include paraffin, microcrystalline, and petrolatum.
[0109] Examples of synthetic hydrocarbon waxes include Fischer-Tropsch wax and polyethylene wax. Examples of synthetic waxes other than synthetic hydrocarbon waxes include esters, ketones, and ethers.
[0110] Examples of fatty acid amides include 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride imide, and chlorinated hydrocarbons.
[0111] Examples of polyacrylates include poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins. Examples of polyacrylate homopolymers or copolymers include n-stearyl acrylate-ethyl methacrylate copolymers.
[0112] The melting point of the release agent is not particularly limited and can be appropriately selected according to the purpose, but is preferably 60° C. or more and 80° C. or less. When the melting point of the release agent is 60° C. or more, it is possible to prevent the release agent from melting at a low temperature, and to prevent the deterioration of heat-resistant storage stability. When the melting point of the release agent is 80° C. or less, it is possible to prevent the release agent from melting sufficiently when the resin is melted and in the fixing temperature range, and thus prevent the occurrence of fixing offset, and prevent the occurrence of image defects.
[0113] The content of the release agent in the resin particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2 parts by mass or more and 10 parts by mass or less, and more preferably 3 parts by mass or more and 8 parts by mass or less, per 100 parts by mass of the resin particles.
[0114] When the content of the releasing agent is 2 parts by mass or more, the deterioration of high-temperature offset resistance and low-temperature fixing property during fixing can be suppressed.When the content of the releasing agent is 10 parts by mass or less, the deterioration of heat-resistant storage stability can be suppressed, and the occurrence of image fogging can be suppressed.
[0115] When the content of the releasing agent is 3 parts by mass or more and 8 parts by mass or less, it is advantageous in terms of improving image quality and fixing stability.
[0116] ((Charge Control Agent)) The charge control agent is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, salicylic acid metal salts, salicylic acid derivative metal salts, oxynaphthoic acid metal salts, phenol-based condensates, azo-based pigments, boron complexes, or polymeric compounds having functional groups (e.g., sulfonic acid groups, carboxyl groups, or quaternary ammonium salts, etc.). These may be used alone or in combination of two or more.
[0117] Specific examples of charge control agents include the nigrosine dye Bontron (registered trademark) 03, the quaternary ammonium salt Bontron (registered trademark) P-51, the metal-containing azo dye Bontron (registered trademark) S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), LRA-901, the boron complex LR-147 (all manufactured by Nippon Carlit Co., Ltd.), copper phthalocyanine, perylene, quinacridone, and azo pigments.
[0118] The content of the charge control agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass to 10 parts by mass, more preferably 0.2 parts by mass to 5 parts by mass, per 100 parts by mass of the resin particles.
[0119] When the content of the charge control agent is 10 parts by mass or less per 100 parts by mass of resin particles, the chargeability of the toner containing the resin particles can be prevented from becoming too high, the effect of the charge control agent can be maintained, an increase in the electrostatic attraction force with the developing roller can be prevented, and a decrease in the fluidity of the developer and a decrease in image density can be suppressed.
[0120] These charge control agents can be melt-kneaded together with the master batch and the resin and then dissolved and dispersed, or of course they can be added when directly dissolved or dispersed in an organic solvent, or they can be fixed to the surface of the resin particles after the resin particles are produced.
[0121] ((Deformation Agent)) The deforming agent is added to deform the shape of the resin particles. The deforming agent is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable to contain a layered inorganic mineral in which at least a part of the interlayer ions of the layered inorganic mineral are modified with organic ions.
[0122] The layered inorganic mineral in which at least a portion of the interlayer ions of the layered inorganic mineral have been modified with organic ions is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include those having a basic smectite crystal structure modified with organic cations.
[0123] Smectite clay minerals have layers that carry a negative charge, and to compensate for this, they have cations between the layers, and can form intercalation compounds by ion exchange of these cations or adsorption of polar molecules. Metal ions can also be introduced by replacing part of the divalent metal of the layered inorganic mineral with a trivalent metal. However, since the introduction of metal anions increases hydrophilicity, layered inorganic compounds in which at least part of the metal anions is modified with organic anions are preferred.
[0124] A layered inorganic mineral in which at least a part of the interlayer ions of the layered inorganic mineral are modified with organic ions can be obtained by using an organic cation modifier or an organic anion modifier.
[0125] The organic cation modifier is not particularly limited as long as it can be modified with organic ions as described above, and examples thereof include quaternary alkyl ammonium salts, phosphonium salts, and imidazolium salts. These may be used alone or in combination of two or more. Among these, quaternary alkyl ammonium salts are preferred as the organic cation modifier.
[0126] The quaternary alkyl ammonium is not particularly limited, and examples thereof include trimethylstearyl ammonium, dimethylstearylbenzyl ammonium, and oleylbis(2-hydroxyethyl)methyl ammonium.
[0127] The organic anion modifier is not particularly limited as long as it can be modified with organic ions as described above, and examples thereof include branched, unbranched, or cyclic alkyl groups (having 1 to 44 carbon atoms), branched, unbranched, or cyclic alkenyl groups (having 1 to 22 carbon atoms), branched, unbranched, or cyclic alkoxy groups (having 8 to 32 carbon atoms), branched, unbranched, or cyclic hydroxyalkyl groups (having 2 to 22 carbon atoms), sulfates, sulfonates, carboxylates, or phosphates having an ethylene oxide skeleton or a propylene oxide skeleton. These may be used alone or in combination of two or more. Among these, the organic anion modifier is preferably a carboxylic acid having an ethylene oxide skeleton.
[0128] When the resin particles are produced by the method for producing resin particles described later, the non-spherical agent is preferably added in the oil phase preparation step described later.
[0129] By modifying at least a part of the ions between layers of the layered inorganic mineral with organic ions, the oil phase containing the resin particle material has a non-Newtonian viscosity and the resin particles can be deformed. In this case, the content of the deformer is preferably 0.05% by mass to 10% by mass, more preferably 0.05% by mass to 5% by mass, based on the total amount of the resin particle material.
[0130] The layered inorganic mineral is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include montmorillonite, bentonite, hectorite, attapulgite, sepiolite, and mixtures thereof.
[0131] Among these, organically modified montmorillonite or organically modified bentonite is preferred because layered inorganic minerals in which at least a portion of the interlayer ions of the layered inorganic minerals have been modified with organic ions do not affect the toner properties when the resin particles are used in a toner, the viscosity can be easily adjusted, and the amount added can be reduced.
[0132] Examples of commercially available products of layered inorganic minerals in which at least a part of the interlayer ions of the layered inorganic minerals are modified with organic ions include quaternium-18 bentonites such as Bentone (registered trademark) 3, Bentone 38, Bentone 38V (all manufactured by Rheox Corporation), Thixogel (registered trademark) VP (manufactured by United Catalyst Corporation), Clayton (registered trademark) 34, Clayton 40, and Clayton XL (all manufactured by Southern Clay Corporation); stearalkonium bentonites such as Bentone 27 (manufactured by Rheox Corporation), Thixogel LG (manufactured by United Catalyst Corporation), Clayton AF, and Clayton APA (all manufactured by Southern Clay Corporation); and quaternium-18 / benzalkonium bentonites such as Clayton HT and Clayton PS (all manufactured by Southern Clay Corporation). Among these, Clayton AF and Clayton APA are preferred.
[0133] In addition, as a layered inorganic mineral in which at least a part of the ions between layers of the layered inorganic mineral is modified with an organic ion, a layered inorganic mineral modified with an organic anion modifier represented by the following general formula (I) is more preferable. An example of the organic anion modifier represented by the following general formula (I) is Hitenol (registered trademark) 330T (Dai-ichi Kogyo Seiyaku Co., Ltd.). R1(OR2) n OSO3M···(I) (In general formula (I), R1 represents an alkyl group having 13 carbon atoms, R2 represents an alkylene group having 2 to 6 carbon atoms, n represents an integer of 2 to 10, and M represents a monovalent metal element.)
[0134] The resin particles may have a core-shell structure. The shell resin constituting the shell layer is not particularly limited, but is preferably an amorphous polyester resin, and the binder resin contained in the core is preferably an amorphous polyester, as described above.
[0135] In this specification, "having a core-shell structure" means a structure having a core layer and a shell layer. The "shell layer" means a layer made of a resin present in the outermost layer of a resin particle, and the "core layer" means a region inside a resin particle excluding the shell layer. The core layer and the shell layer are not completely compatible with each other and are formed inhomogeneously.
[0136] In the core-shell structure, the surface of the core layer is preferably covered by the shell layer. In the core-shell structure, the surface of the core layer may be completely covered by the shell layer, or may not be completely covered by the shell layer. Examples of the form in which the surface of the core layer is not completely covered by the shell layer include a form in which the core layer is covered by the shell layer in a mesh-like shape, and a form in which the core layer is partially exposed from the shell layer. Among these, from the viewpoint of filming resistance, it is preferable that the surface of the core layer is completely covered by the shell layer.
[0137] <Method of manufacturing resin particles> The method for producing resin particles according to the present embodiment is a method for producing resin particles containing at least a binder resin and a colorant. The method for producing resin particles according to the present embodiment includes a step of aggregating particles in a dispersion of at least the binder resin and the colorant, the colorant containing a pigment having an isoindoline skeleton, and a Raman spectroscopy of the resin particles at 950 cm -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. Details of (Formula 1) are the same as those explained for resin particles, and therefore will be omitted.
[0138] The method for producing the resin particles of the present embodiment is an example of the aggregation method. There are also various methods for the aggregation method, but in the resin particles of the present embodiment that contain the pigment having an isoindoline skeleton, a method in which the pigment is dispersed in an organic solvent together with the binder resin to form an oil phase, and then the phase is inverted and emulsified, is preferable in terms of improving the pigment dispersibility, compared to a method in which an aqueous dispersion containing a colorant and an aqueous dispersion containing a binder resin such as amorphous polyester are separately prepared and then aggregated.
[0139] Therefore, the method for producing resin particles of this embodiment can make the content of the material containing the pigment having an isoindoline skeleton among the resin particles more uniform than other methods, and also suppresses uneven distribution of the pigment having an isoindoline skeleton on the surface layer of the resin particles, thereby providing excellent pigment dispersibility inside the resin fine particles. As described above, the method for producing resin particles of this embodiment can provide resin particles having excellent coloring power and charging performance.
[0140] A method for producing resin particles according to another embodiment includes a step of preparing an oil phase by dissolving or dispersing at least a binder resin and a colorant in an organic solvent (hereinafter, this step may be referred to as an "oil phase preparation step"); a step of adding water to the oil phase to invert the phase from a water-in-oil dispersion to an oil-in-water dispersion (hereinafter, this step may be referred to as a "phase inversion emulsification step"); and a step of aggregating particles in the oil-in-water dispersion (hereinafter, this step may be referred to as an "aggregation step"). The colorant includes a pigment having an isoindoline skeleton, and the resin particles are analyzed by Raman spectroscopy to determine whether the pigment has an isoindoline skeleton or not. -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. Details of (Formula 1) are the same as those explained for resin particles, and therefore will be omitted.
[0141] The method for producing resin particles according to the present embodiment can more uniformly distribute the content of the material containing the pigment having an isoindoline skeleton among the resin particles than other methods, and can suppress uneven distribution of the pigment having an isoindoline skeleton on the surface layer of the resin particles, thereby providing excellent pigment dispersibility inside the resin fine particles. Thus, the method for producing resin particles according to the present embodiment can provide resin particles having excellent coloring power and charging performance.
[0142] The method for producing resin particles according to another embodiment may include other steps, such as an aqueous phase preparation step, a solvent removal step, a fusion step, a washing step, a drying step, a classification step, an annealing step, etc. Next, each step will be described in detail.
[0143] (Oil phase preparation process) The oil phase preparation step is a step of preparing an oil phase by dissolving or dispersing at least a binder resin and a colorant in an organic solvent. The binder resin preferably contains an amorphous polyester resin, and the colorant contains at least a pigment having an isoindoline skeleton. As described above, the colorant is preferably used as a master batch from the viewpoint of ensuring dispersibility. The oil phase may further contain a crystalline resin, a release agent, a charge control agent, a deforming agent, etc., as necessary.
[0144] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, but an organic solvent having a boiling point of less than 150° C. is preferred in terms of ease of removal.
[0145] The organic solvent having a boiling point of less than 150° C. is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, and methyl isobutyl ketone. These may be used alone or in combination of two or more. Among these, the organic solvent is preferably ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, or carbon tetrachloride, and more preferably ethyl acetate.
[0146] The amount of organic solvent used is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 40 parts by mass to 300 parts by mass, more preferably 60 parts by mass to 140 parts by mass, and even more preferably 80 parts by mass to 120 parts by mass, per 100 parts by mass of the raw material for the resin particles.
[0147] The method for preparing the oil phase is not particularly limited and can be appropriately selected depending on the purpose. For example, there is a method in which the materials for the oil phase are gradually added to an organic solvent with stirring to dissolve or disperse them.
[0148] For dispersion, known devices can be used, such as a bead mill, a disk mill, a rotor-stator type disperser, etc., and the material is finely dispersed by shearing force or collision force. At this time, multiple devices that generate shearing force or collision force may be used in combination, which can efficiently reduce resin particles with a non-uniform composition having an absolute value of CH ratio of 20.0% or more.
[0149] The dispersion method is not particularly limited, but the preferred method for fine dispersion by shear is to crush the material with high shear force generated in the narrow gap between the rotor and stator, while the preferred method for fine dispersion by collision is to fill a vessel with beads such as zirconia and rotate the vessel to crush the material by collision between the beads or between the beads and the vessel.
[0150] When microdispersion by shear and microdispersion by collision are performed, the order is not particularly limited, but when undissolved residue remains in the oil phase in which the material is merely dissolved in an organic solvent, it is preferable to first perform microdispersion by shear using a rotor and stator type, etc. In the case of microdispersion by collision using a media disperser such as a bead mill, there is a possibility that unsolvented materials may become clogged in the screen mesh, which is likely to be a problem in efficient dispersion.
[0151] In order to efficiently disperse the material, in the case of dispersing by shearing, the rotor circumferential speed is preferably more than 12 m / s, and in the case of dispersing by collision, the disk circumferential speed is preferably 6 m / s or more, more preferably 10 m / s to 12 m / s.
[0152] By setting the disk speed to 6m / s or more, sufficient crushing energy can be obtained through collisions, and the uneven distribution of beads can be suppressed, resulting in sufficient dispersion. By setting the disk speed to 12m / s or less, re-agglomeration due to an increase in liquid temperature or over-dispersion can be suppressed.
[0153] The media (beads) diameter is preferably 0.5 mm or less, and more preferably 0.3 mm or less. By making the media diameter 0.5 mm or less, the dispersion efficiency can be improved. The smaller the media diameter, the greater the total surface area of the beads, increasing the opportunities for dispersion through collision and improving the dispersion efficiency. If the media diameter is too small, the openings of the screen separating the beads and the process liquid must be narrowed, which means that the flow rate cannot be achieved and the liquid temperature rises, which creates the risk of re-agglomeration.
[0154] (Aqueous phase preparation process) The aqueous phase preparation step is a step of preparing an aqueous phase (aqueous medium). The aqueous medium is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include water, a solvent miscible with water, and a mixture thereof. These may be used alone or in combination of two or more. Among these, water is preferred.
[0155] The water-miscible solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include alcohol, dimethylformamide, tetrahydrofuran, ethyl acetate, cellosolves, and lower ketones.
[0156] The alcohol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include methanol, isopropanol, and ethylene glycol. The lower ketone is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include acetone and methyl ethyl ketone.
[0157] (Phase inversion emulsification process) The phase inversion emulsification process is a process in which an aqueous medium is added to the oil phase to invert the phase from a water-in-oil dispersion to an oil-in-water dispersion, thereby obtaining a fine particle dispersion (oil droplets).
[0158] The method for phase inversion emulsification of the oil phase in the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose. For example, there is a method in which the oil phase is neutralized with a base or the like, and then an aqueous phase is added thereto, thereby obtaining a microparticle dispersion by phase inversion emulsification in which a water-in-oil dispersion is inverted into an oil-in-water dispersion.
[0159] In the phase inversion emulsification process, when the oil phase is neutralized with a base, it is preferable to carry out an additional dispersion process after adding the base to the oil phase. This is expected to have the effect of redispersing the aggregates of materials that have been generated by the neutralization process, and can efficiently reduce the number of resin particles with a non-uniform composition in which the absolute value of the CH ratio is 20.0% or more.
[0160] As the base for neutralizing the oil phase, either a basic inorganic compound or a basic organic compound may be used. Examples of the basic inorganic compound include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, potassium hydrogen carbonate, and ammonia. Examples of the basic organic compound include N,N-dimethylethanolamine, N,N-diethylethanolamine, triethanolamine, tripropanolamine, tributanolamine, triethylamine, n-propylamine, n-butylamine, isopropylamine, monomethanolamine, morpholine, methoxypropylamine, pyridine, vinylpyridine, and isophoronediamine.
[0161] Neutralization is performed while uniformly mixing and dispersing using a normal stirrer or dispersing device. The dispersing device is not particularly limited, and examples thereof include ultrasonic dispersers, bead mills, ball mills, roll mills, homomixers, ultra mixers, dispersing mixers, penetrating type high pressure dispersing devices, collision type high pressure dispersing devices, multi-hole type high pressure dispersing devices, ultra-high pressure homogenizers, and ultrasonic homogenizers. A normal stirrer and a dispersing device may be used in combination.
[0162] The amount of the aqueous medium used when the oil phase containing the resin particle material is inverted and emulsified is not particularly limited and can be appropriately selected depending on the purpose. The amount of the aqueous medium used is preferably 50 parts by mass or more and 2,000 parts by mass or less, more preferably 100 parts by mass or more and 1,000 parts by mass or less, relative to 100 parts by mass of the resin particle material.
[0163] When the amount of the aqueous medium used is 50 parts by mass or more relative to 100 parts by mass of the resin particle material, the dispersion state of the resin particle material is prevented from becoming poor, and the resin particles having the desired particle size can be prevented from being unable to be obtained. Also, when the amount of the aqueous medium used is 2,000 parts by mass or less relative to 100 parts by mass of the resin particle material, the production cost can be prevented from increasing.
[0164] When the oil phase containing the resin particle material is subjected to phase inversion emulsification, it is preferable to use a dispersant from the viewpoints of stabilizing the dispersion of oil droplets, etc., forming a desired shape, and sharpening the particle size distribution.
[0165] The dispersant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, and polymer-based protective colloids. These may be used alone or in combination of two or more. Among these, surfactants are preferred as dispersants.
[0166] The surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the surfactant include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants.
[0167] The anionic surfactant is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include alkylbenzenesulfonates, α-olefinsulfonates, and phosphates. Among these, the anionic surfactant having a fluoroalkyl group is preferred.
[0168] Phase inversion emulsification can be carried out using a stirring blade. The stirring blade is not particularly limited and can be appropriately selected depending on the viscosity of the solution, and examples thereof include an anchor blade, a turbine blade, a Pfaudle blade, a full zone blade, a Max Blend blade, and a half-moon blade.
[0169] The volume average particle size of the dispersed matter (oil droplets) in the fine particle dispersion is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50 nm to 2,000 nm, more preferably 50 nm to 500 nm.
[0170] (Solvent removal process) The solvent removal step is a step in which the organic solvent is removed from the fine particle dispersion obtained in the phase inversion emulsification step to obtain fine particles.
[0171] The method for removing the organic solvent from the microparticle dispersion is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include a method of gradually increasing the temperature of the entire reaction system to evaporate the organic solvent in the microparticle dispersion (oil droplets); a method of spraying the microparticle dispersion in a dry atmosphere to remove the organic solvent in the microparticle dispersion (oil droplets); a method of decompressing the microparticle dispersion to evaporate and remove the organic solvent, etc. These methods may be used alone or in combination of two or more.
[0172] The drying atmosphere into which the microparticle dispersion is sprayed is not particularly limited and can be appropriately selected depending on the purpose. Examples include air, nitrogen, carbon dioxide, heated combustion gas, etc., and various air streams heated to a temperature equal to or higher than the boiling point of the highest boiling point solvent used are generally used.
[0173] The solvent removal step can be carried out using equipment such as a spray dryer, a belt dryer, or a rotary kiln, and the desired quality can be obtained sufficiently with a short treatment period.
[0174] (Agglutination process) The aggregation step is a step of aggregating particles in an oil-in-water dispersion to obtain aggregated particles. The method of aggregating oil droplets or particles is not particularly limited and can be appropriately selected from known methods according to the purpose, for example, a method of adding an aggregating agent, a method of adjusting pH, etc.
[0175] In the aggregation step, by uniformly progressing the aggregation, it is possible to efficiently reduce the number of resin particles having a non-uniform composition with an absolute value of CH ratio of 20.0% or more. It is preferable to thoroughly stir the inside of the reaction vessel, and it is also preferable to adjust the solution concentration of the components to be added, such as the flocculant, according to the aggregation properties. This makes it possible to uniformize the material content of the aggregated particles.
[0176] The flocculant is not particularly limited and can be appropriately selected depending on the purpose. For example, aluminum chloride, zinc sulfate, magnesium sulfate, aluminum sulfate, potassium aluminum sulfate, sodium chloride, sodium bromide, sodium iodide, sodium fluoride, sodium acetate, sodium acetoacetate, lithium chloride, lithium bromide, lithium iodide, lithium fluoride, lithium acetate, lithium acetoacetate, potassium chloride, potassium bromide, potassium iodide, potassium fluoride, potassium acetoacetate, magnesium bromide, magnesium chloride, magnesium iodide, and magnesium fluoride. Examples of the coagulant include magnesium, magnesium acetate, magnesium acetoacetate, calcium chloride, calcium bromide, barium bromide, barium chloride, barium iodide, barium fluoride, barium acetate, barium acetoacetate, strontium bromide, strontium chloride, strontium iodide, strontium fluoride, strontium acetate, strontium acetoacetate, zinc bromide, zinc chloride, zinc iodide, zinc fluoride, zinc acetate, zinc acetoacetate, copper bromide, copper chloride, copper iodide, copper fluoride, copper acetate, copper acetoacetate, iron bromide, iron chloride, iron iodide, iron fluoride, iron acetate, or iron acetoacetate. These may be used alone or in combination of two or more. Among these, divalent metal salts are preferable as the coagulant, and trivalent metal salts are more preferable. By using a divalent or higher metal salt, a three-dimensional structure can be formed by metal cross-linking with the carboxyl groups contained in the amorphous polyester resin, thereby increasing the strength of the resin particles and improving the filming resistance.
[0177] When adding the flocculant, it may be added as is, but it is preferable to add the flocculant in the form of an aqueous solution, since this can avoid localized high concentration. Also, it is preferable to add the flocculant salt gradually while monitoring the particle size of the flocculant particles.
[0178] The temperature of the reaction system in which the aggregation step is carried out (the temperature of the dispersion liquid during aggregation) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably near the glass transition temperature (Tg) of the amorphous polyester resin. If the temperature is too low, the aggregation does not proceed very well, which may result in poor efficiency, and if the temperature is too high, the aggregation speed increases, which may result in the generation of coarse particles and a deterioration in particle size distribution.
[0179] In the aggregation step, aggregation is stopped after the aggregated particles reach a target particle size. There is no particular limitation on the method for stopping aggregation, and it can be appropriately selected according to the purpose. For example, a method of adding a salt or a chelating agent having a lower ionic valence than the aggregated salt; a method of adjusting the pH; a method of lowering the temperature of the reaction system (dispersion liquid) during aggregation; a method of adding a large amount of an aqueous medium to dilute the concentration of the reaction system (dispersion liquid) during aggregation; a method of adding a dispersant, etc. can be used. These may be used alone or in combination of two or more.
[0180] The volume average particle size of the aggregated particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 3.0 μm to 6.0 μm, and more preferably 4.0 μm to 6.0 μm.
[0181] In the aggregation step, a release agent may be added, or a crystalline resin may be added for low-temperature fixability. When a release agent or a crystalline resin is added in the aggregation step, a dispersion liquid in which the release agent is dispersed in an aqueous medium or a dispersion liquid of a crystalline polyester resin is prepared, and the dispersion liquid is mixed with a fine particle dispersion liquid (oil droplets) and then aggregated to obtain aggregated particles in which the release agent or the crystalline resin is uniformly dispersed.
[0182] The aggregation step may also include a step of forming a shell layer on the aggregated particles (hereinafter, sometimes referred to as a "shelling step"). In the shelling step, by forming a shell layer on the aggregated particles, a crystalline resin or a release agent that deteriorates filming properties can be encapsulated, thereby improving filming resistance.
[0183] The method for forming the shell layer is not particularly limited and can be appropriately selected depending on the purpose. For example, after preparing aggregated particles by the above-mentioned method, a dispersion of a shell agent can be added to the aggregated particles that have reached a desired particle size. In this case, the shell agent and the aggregating agent can be added stepwise to laminate the shell layer, or the shell agent can be added after the fusion step described below, and the process corresponding to the aggregating step can be repeated again. In addition, when the manufacturing method of resin particles includes a desolvation step, the dispersion of the shell agent can be added after obtaining the aggregated particles obtained in the desolvation step.
[0184] (fusion process) The fusion step is a step in which the aggregated particles are fused to reduce unevenness and obtain spherical resin particles. In addition, when a resin is added to the aggregated particles in the aggregation step to form a shell layer, the fusion step can form a shell layer on the surface of the aggregated particles.
[0185] The method for fusing the aggregated particles is not particularly limited and may be appropriately selected depending on the purpose. For example, a method in which a dispersion of the aggregated particles is heated while being stirred may be mentioned.
[0186] The heating temperature is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from Tg to Tg+20° C. of the amorphous polyester resin, and more preferably from Tg to Tg+10° C. When the heating temperature is from Tg+20° C. of the amorphous polyester resin, the amorphous polyester resin and the crystalline resin are appropriately compatible with each other, and the heat-resistant storage stability is improved.
[0187] When resin particles are applied to toner, the average circularity is preferably a specific shape, and the average circularity is preferably 0.940 or more and less than 0.980. A toner having an average circularity of less than 0.940 and an indefinite shape that is too far from a sphere cannot obtain a high-quality image with satisfactory transferability and no dust. If the average circularity is 0.980 or more, in a system that employs blade cleaning, cleaning failure occurs on the photoreceptor and transfer belt, causing stains on the image.
[0188] -Measurement of average circularity- In this embodiment, the average particle size and the average circularity can be measured, for example, by using a flow type particle image analyzer (FPIA-3000, manufactured by Sysmex Corporation).
[0189] In a specific measurement method, 0.1 to 0.5 mL of a surfactant, preferably an alkylbenzene sulfonate, is added as a dispersant to 100 to 150 mL of water from which solid impurities have been removed in advance in a container, and about 0.1 to 0.5 g of the measurement sample is further added. The suspension in which the sample is dispersed is subjected to a dispersion treatment for about 1 to 3 minutes with an ultrasonic disperser, and the average particle size, average circularity, and standard deviation (SD) of the circularity are measured with an apparatus with a dispersion concentration of 3,000 particles / μL to 10,000 particles / μL.
[0190] However, the particle diameter is the equivalent circle diameter, the average particle diameter is calculated based on the equivalent circle diameter (number basis), and the analysis conditions for the flow type particle image analyzer are as follows: [Analysis conditions] Particle size limit: 0.5μm≦circle equivalent diameter (number basis)≦200.0μm Particle shape limit: 0.93<circularity≦1.00 In the present embodiment, the average circularity is defined as follows. (Average circularity) = (perimeter of a circle equal to the projected area of a particle) / (perimeter of a projected image of a particle)
[0191] (Annealing process) The annealing step is a step carried out when a crystalline resin is added, and is a step for causing phase separation between the crystalline resin and the amorphous polyester resin.
[0192] The method of performing the annealing treatment is not particularly limited and can be appropriately selected depending on the purpose, but examples include a method of storing the resin at a temperature near the glass transition temperature (Tg) of the crystalline resin for 10 hours or more. This step is often performed after the fusion step, and can be performed at any desired timing, such as before washing, before drying, or after drying.
[0193] In the fusion step, when heating is performed at a temperature near the glass transition temperature (Tg) of the resin used, the crystalline resin and the amorphous polyester resin become in a compatible state, and it may become impossible to achieve both heat-resistant storage stability and low-temperature fixability. However, when an annealing treatment is performed, phase separation between the crystalline resin and the amorphous resin proceeds, and the compatible state is eliminated, which is advantageous.
[0194] (Cleaning process) The washing step is a step of washing the resin particles obtained in the aggregation step or fusion step. Since the dispersion of resin particles obtained by the above-mentioned method may contain sub-materials such as a flocculant in addition to the resin particles, it is preferable to perform washing in order to extract only the resin particles from the dispersion of resin particles.
[0195] The method for washing the resin particles is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include centrifugation, reduced pressure filtration, and filter press. Any of the washing methods can obtain a cake of resin particles, but if the resin particles cannot be sufficiently washed in one operation, the obtained cake may be dispersed again in an aqueous solvent to form a slurry, and the step of extracting the resin particles by at least one of the washing methods may be repeated.
[0196] When washing is carried out by vacuum filtration or filter press, a method may be used in which an aqueous solvent is passed through the cake body to wash away the secondary materials embraced by the resin particles.
[0197] The aqueous solvent used in the washing step is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include water and a mixed solvent of water and alcohol. Examples of the alcohol include methanol and ethanol. Among these, the aqueous solvent is preferably water from the viewpoint of cost and environmental load due to wastewater treatment.
[0198] (drying process) The drying step is a step of washing the resin particles obtained in the washing step. Since the resin particles washed in the washing step contain a large amount of the aqueous medium, the resin particles are dried in the drying step to remove the aqueous medium, thereby obtaining only the resin particles.
[0199] The drying method is not particularly limited and can be appropriately selected depending on the purpose. For example, a method using a dryer such as a spray dryer, a vacuum freeze dryer, a reduced pressure dryer, a stationary shelf dryer, a mobile shelf dryer, a fluidized bed dryer, a rotary dryer, or an agitator dryer can be included.
[0200] The final moisture content of the dried resin particles is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the moisture content is less than 1% by mass.
[0201] The resin particles dried in the drying step are in the form of soft agglomeration, and if this causes inconvenience during use, the soft agglomeration may be broken down by crushing. The method for crushing is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a method using a device such as a jet mill, a Henschel mixer, a super mixer, a coffee mill, an Oster blender, or a food processor.
[0202] (Classification process) The classification step is a step of classifying the resin particles obtained in the washing step or the drying step. The classification method is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a method of removing fine particles in a liquid using a cyclone, a decanter, centrifugal separation, etc., and a method of performing a known classification operation after drying.
[0203] <Toner> The toner of the present embodiment contains the resin particles of the present embodiment. The toner of the present embodiment contains the resin particles of the present embodiment, and therefore has excellent coloring power and charging performance.
[0204] The toner of the present embodiment preferably further contains an external additive, and further contains other components as necessary. The content of the resin particles in the toner is not particularly limited and can be appropriately selected depending on the purpose. The toner may be the resin particles themselves.
[0205] (External additives) The external additive is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include inorganic fine particles, oxide fine particles, fatty acid metal salts, or hydrophobized versions of these, etc. These may be used alone or in combination of two or more.
[0206] The average particle size of the primary particles of the inorganic fine particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 100 nm or less, more preferably 1 nm or more and 100 nm or less, even more preferably 3 nm or more and 70 nm or less, and particularly preferably 5 nm or more and 70 nm or less.
[0207] When the average particle size of the primary particles of the inorganic fine particles is 1 nm or more, the inorganic fine particles can be prevented from being embedded in the toner and not functioning effectively, and when it is 100 nm or less, uneven damage to the photoreceptor surface can be suppressed.
[0208] The inorganic fine particles preferably contain at least one type of inorganic fine particles having an average primary particle size of 20 nm or less, and at least one type of inorganic fine particles having an average primary particle size of 30 nm or more.
[0209] The specific surface area of the inorganic fine particles as measured by the BET method is not particularly limited and can be appropriately selected depending on the purpose. 2 / g or more 500m 2 It is preferable that the molecular weight is not more than 1 / g.
[0210] The inorganic fine particles are not particularly limited and can be appropriately selected according to the purpose, and examples thereof include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, red iron oxide, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride. These may be used alone or in combination of two or more. Among these, silica or titanium dioxide is preferred.
[0211] The oxide fine particles are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include titania, alumina, tin oxide, and antimony oxide.
[0212] Examples of fatty acid metal salts include zinc stearate and aluminum stearate.
[0213] Among these, hydrophobically treated silica, titania, titanium oxide, or alumina fine particles are preferred as the external additive.
[0214] Examples of silica fine particles include R972, R974, RX200, RY200, R202, R805, and R812 (all manufactured by Nippon Aerosil Co., Ltd.).
[0215] Examples of titania fine particles include P-25 (manufactured by Nippon Aerosil Co., Ltd.), STT-30, STT-65C-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-140 (manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-150W, MT-500B, MT-600B, and MT-150A (all manufactured by Teika Corporation).
[0216] Examples of hydrophobically treated titanium oxide microparticles include T-805 (manufactured by Nippon Aerosil Co., Ltd.), STT-30A, STT-65S-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-500T, TAF-1500T (all manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-100S, MT-100T (all manufactured by Teika Corporation), and IT-S (manufactured by Ishihara Sangyo Co., Ltd.).
[0217] Hydrophobized oxide particles, hydrophobized silica particles, hydrophobized titania particles, or hydrophobized alumina particles can be obtained by treating hydrophilic particles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, or octyltrimethoxysilane. Silicone oil-treated oxide particles and inorganic particles are also suitable, which are treated with silicone oil by heating if necessary to form inorganic particles. External additives can also be surface-treated with a flowability improver.
[0218] The silicone oil is not particularly limited and can be appropriately selected depending on the purpose. Examples of the silicone oil include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methylhydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, methacryl-modified silicone oil, and α-methylstyrene-modified silicone oil.
[0219] The content of the external additive is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass to 5 parts by mass, more preferably 0.3 parts by mass to 3 parts by mass, relative to 100 parts by mass of the toner.
[0220] The method for producing the toner is not particularly limited and can be appropriately selected from known methods, but it is preferable to produce the toner by the method for producing the toner of the present invention described below.
[0221] <Toner manufacturing method> The toner manufacturing method of the present embodiment includes a step of adding at least an external additive to the resin particles of the present embodiment (hereinafter, may be referred to as a "mixing step"). The toner manufacturing method of the present embodiment may further include other steps as necessary.
[0222] (Mixing process) The mixing step is a step of mixing the toner resin particles as the toner base particles with the external additive. At this time, it is preferable to apply a mechanical impact force in order to prevent the external additive particles from being detached from the surfaces of the toner base particles.
[0223] The method of applying the mechanical impact force is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method of applying an impact force to a mixture of resin particles and external additives using a blade rotating at high speed; and a method of introducing a mixture of resin particles and external additives into a high-speed air stream and accelerating it to cause the particles to collide with each other or with an appropriate collision plate.
[0224] The device used in the method of applying a mechanical impact force is not particularly limited and can be appropriately selected depending on the purpose. Examples of the device include an Angmill (manufactured by Hosokawa Micron Corporation), a device obtained by modifying an I-type mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.) to reduce the grinding air pressure, a Hybridization System (manufactured by Nara Machinery Works, Ltd.), a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar.
[0225] <Developer> The developer of the present embodiment contains the toner of the present embodiment. The developer of the present embodiment may further contain other components, such as a carrier, which are appropriately selected as necessary.
[0226] Since the toner contained in the developer of the present embodiment contains the resin particles of the present embodiment, the developer has excellent coloring power and charge stability. The developer has excellent coloring power, transferability, chargeability, etc., and can stably form high-quality images.
[0227] The developer may be a one-component developer or a two-component developer. However, when used in high-speed printers that correspond to the recent improvements in information processing speed, a two-component developer is preferred because it has a longer life.
[0228] When the developer is used as a one-component developer, even if the toner is balanced, there is little fluctuation in the particle size of the toner, there is little filming of the toner on the developing roller, and there is little fusion of the toner to components such as blades that thin the toner layer, and good and stable developability and images can be obtained even with long-term stirring in the developing device.
[0229] When the developer is used as a two-component developer, even if the toner is replenished over a long period of time, there is little fluctuation in the particle size of the toner, and good and stable developability and images can be obtained even with long-term stirring in the developing device.
[0230] (Career) The carrier is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the carrier has a core material and a resin layer that covers the core material.
[0231] The material of the core material is not particularly limited and can be appropriately selected according to the purpose. For example, manganese-strontium-based material of 50 emu / g to 90 emu / g or manganese-magnesium-based material of 50 emu / g to 90 emu / g can be mentioned. In order to ensure image density, it is preferable to use high magnetization materials such as iron powder of 100 emu / g or more, magnetite of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetization materials such as copper-zinc-based materials of 30 emu / g to 80 emu / g because it can reduce the impact of the developer in a standing state on the photoconductor and is advantageous for high image quality. These materials may be used alone or in combination of two or more.
[0232] The volume average particle size of the core material is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 10 μm to 150 μm, and more preferably from 40 μm to 100 μm.
[0233] When the core material has a volume average particle size of 10 μm or more, it is possible to prevent the carrier from containing a large amount of fine powder, and to suppress the carrier from scattering due to a decrease in magnetization per particle. Also, when the core material has a volume average particle size of 150 μm or less, it is possible to prevent the specific surface area from decreasing, and to suppress the toner from scattering, and in full color toners with many solid areas, it is possible to suppress the reproduction of the solid areas from becoming poor.
[0234] When the toner is used in a two-component developer, it may be mixed with a carrier. The content of the carrier in the two-component developer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 90 parts by mass or more and 98 parts by mass or less, more preferably 93 parts by mass or more and 97 parts by mass or less, relative to 100 parts by mass of the two-component developer.
[0235] The developer can be suitably used for image formation by various known electrophotographic methods, such as a magnetic one-component development method, a non-magnetic one-component development method, or a two-component development method.
[0236] <Toner storage unit> The toner storage unit in the present embodiment stores the toner of the present embodiment. The toner storage unit refers to a unit having a function of storing toner and storing the toner. The toner storage unit in the present embodiment stores the toner containing the resin particles of the present embodiment, and therefore can exhibit excellent coloring power and charging performance.
[0237] Examples of the toner storage unit include a toner storage container, a developing device, and a process cartridge. A toner storage container is a container that stores toner. A developing device is a device that stores toner and has a means for developing the toner. A process cartridge is a device that integrates at least an image carrier and a developing device, stores toner, and is detachable from an image forming device. The process cartridge may further include at least one selected from a charging device, an exposure device, and a cleaning device.
[0238] <Image forming device> The image forming apparatus of the present embodiment includes an electrostatic latent image carrier, an electrostatic latent image forming section that forms an electrostatic latent image on the electrostatic latent image carrier, a developing section that develops the electrostatic latent image with toner to form a visible image, a transfer section that transfers the visible image to a recording medium, and a fixing section that fixes the transferred image transferred to the recording medium, and the toner is the toner of the present embodiment. Thus, the image forming apparatus of the present embodiment can exhibit excellent coloring power and charging performance.
[0239] Next, one aspect of the method for forming an image by the image forming apparatus of the present embodiment will be described with reference to Fig. 6. Although a printer is shown as an example of the image forming apparatus of the present embodiment, the image forming apparatus is not particularly limited as long as it is capable of forming an image using toner, such as a copier, facsimile, or multifunction machine.
[0240] 6 is a schematic diagram showing an example of an image forming apparatus according to an embodiment. As shown in FIG. 6, an electrophotographic image forming apparatus (printer) 1 includes a paper feed section 10, a conveyance section 20, an image forming section 30, a transfer section 40, a fixing section 50, and a toner cartridge 60.
[0241] The paper feed section 10 includes a paper feed cassette 11 in which paper P to be fed is stacked, and a paper feed roller 12 that feeds the paper P stacked in the paper feed cassette 11 one sheet at a time.
[0242] The paper feed cassettes 11 are disposed below the exposure unit 32. Each paper feed cassette 11 contains a stack of transfer paper P, which is a recording medium.
[0243] The paper feed roller 12 is disposed so as to come into contact with the topmost sheet of transfer paper P in the paper feed cassette 11 .
[0244] In the paper feed section 10, when the paper feed roller 12 is driven to rotate counterclockwise in the figure by the driving means, the topmost transfer sheet P in the paper feed cassette 11 is discharged from the right side of the paper feed cassette 11 in Figure 6 toward the conveying section 20. The discharged transfer sheet P is sandwiched between the rollers of the conveying roller 21 and conveyed from the bottom to the top in Figure 6.
[0245] The conveying section 20 includes a conveying roller 21 that conveys the transfer paper P fed by the paper feed roller 12 toward the transfer section 40, a pair of timing rollers 22 that hold the leading edge of the transfer paper P conveyed by the conveying roller 21 and wait, and send the paper to the transfer section 40 at a predetermined timing, a paper discharge roller 23 that discharges the paper P with the fixed color toner image onto a paper discharge tray 24, and the paper discharge tray 24 onto which the paper P discharged from the paper discharge roller 23 is fed.
[0246] The transport rollers 21 are disposed so as to sandwich the transfer sheet P, and transport the transfer sheet P from the lower side to the upper side in FIG.
[0247] The timing roller 22 is disposed at the downstream end in the transport direction of the transport roller 21. As soon as the timing roller 22 sandwiches the transfer paper P sent from the transport roller 21 between the rollers, the timing roller 22 temporarily stops the rotation of both rollers. Then, the timing roller 22 sends the transfer paper P sandwiched between the rollers toward the secondary transfer nip at a timing that allows the transfer paper P to be synchronized with the four-color toner image on the intermediate transfer belt 43.
[0248] The paper discharge roller 23 is a roller that discharges the transfer paper P to the outside of the printer 1 after the fixing process.
[0249] The paper discharge tray 24 is provided on the upper surface of the housing of the main body of the printer 1, and stacks the transfer paper P discharged to the outside of the printer 1 by the paper discharge roller 23.
[0250] The image forming section 30 includes four imaging units 31Y, 31C, 31M and 31K for yellow, magenta, cyan and black (hereinafter referred to as Y, C, M and K, respectively), and an exposure device 32 which is a latent image forming section.
[0251] The imaging units 31Y, 31C, 31M, and 31K are arranged in order from left to right in the drawing at a predetermined interval, and are arranged side by side so as to face the intermediate transfer belt 43. The imaging units 31Y, 31C, 31M, and 31K form images using developers containing Y toner, C toner, M toner, and K toner, respectively. The developers contain toner and carrier. The four imaging units 31Y, 31C, 31M, and 31K each use a different type of developer.
[0252] The configurations of the imaging units 31Y, 31C, 31M, and 31K will be described. Note that the imaging units 31Y, 31C, 31M, and 31K are similar except for the toner colors, so only the configuration of the imaging unit 31Y will be described, and the configurations of the other imaging units 31C, 31M, and 31K will not be described.
[0253] The imaging unit 31Y incorporates a drum-shaped photoconductor 311Y, a charging device 312Y, a developing device 313Y, a photoconductor cleaning device 314Y, a lubricant application device (not shown), a cleaning roller, a static electricity removal lamp, etc. into one unit as a process cartridge, which is detachable from the image forming apparatus 1. Around the photoconductor 311Y, the charging device 312Y, the developing device 313Y, the photoconductor cleaning device 314Y, a lubricant application device (not shown), a cleaning roller, a static electricity removal lamp, etc. are arranged.
[0254] Although the photoconductor 311Y is shown to have a drum shape, it may also be in the form of a sheet or an endless belt.
[0255] The charging device 312Y may be a known device such as a corotron, a scorotron, or a solid-state charger. Of these charging methods, the contact charging method and the non-contact close-by arrangement method are more preferable, and have the advantages of increasing charging efficiency, reducing the amount of ozone generated, and enabling the device to be made smaller. In this embodiment, the charging device 312Y includes a charging roller 3121Y, which is a charging member, and uses a non-contact close-by arrangement method in which the charging roller 3121Y is placed close to the photoconductor 311Y at a predetermined distance and in a non-contact manner. The charging roller 3121Y is placed in a non-contact manner with the photoconductor 311Y, and charges the photoconductor 311Y to a predetermined polarity and a predetermined potential. The surface of the photoconductor 311Y, which is uniformly charged by the charging roller 3121Y, is irradiated with laser light L from the exposure device 32 based on image information, and an electrostatic latent image is formed.
[0256] The developing device 313Y converts the latent image formed on the surface of the photoconductor 311Y into a toner image. The developing device 313Y has a developing roller 3131Y as a developer carrier. A developing bias is applied to the developing roller 3131Y from a power source.
[0257] In the developing device 313Y, the toner in the developer is charged to a predetermined polarity. Then, the developer is pumped up onto the surface of the developing roller 3131Y, and the toner of the pumped up developer adheres to the latent image on the photoconductor 311Y in a development area facing the photoconductor 311Y.
[0258] The photoconductor cleaning device 314Y cleans the toner remaining on the photoconductor 311Y after the toner image is transferred to the intermediate transfer belt 43 included in the transfer unit 40. The photoconductor cleaning device 314Y may have a fur brush, a cleaning blade, or the like.
[0259] A lubricant application device (not shown) applies a lubricant onto the surface of the photoconductor 311Y after it has been cleaned by the photoconductor cleaning device 314Y.
[0260] The cleaning roller (not shown) cleans the charging roller 3121Y.
[0261] A charge removing lamp (not shown) removes the surface potential of the photoconductor 311Y after cleaning.
[0262] The exposure device 32 is disposed below the imaging units 31Y, 31C, 31M, and 31K. The exposure device 32 irradiates the photoconductors 311Y, 311C, 311M, and 311K with laser light L generated based on image information. As a result, electrostatic latent images for Y, C, M, and K are formed on the photoconductors 311Y, 311C, 311M, and 311K.
[0263] The exposure unit 32 includes a polygon mirror 321 that is rotated by a motor to irradiate laser light L emitted from a light source onto photoconductors 311Y, 311C, 311M, and 311K via a plurality of optical lenses and mirrors while deflecting the laser light L by the polygon mirror 321. Note that the exposure unit 32 may include an LED array for optical scanning instead of the above configuration.
[0264] The light source for the laser light L of the exposure device 32 and the light source for the charge removal lamp can be any light-emitting material such as a fluorescent lamp, a tungsten lamp, a halogen lamp, a mercury lamp, a sodium lamp, a light-emitting diode (LED), a semiconductor laser (LD), an electroluminescence (EL), etc.
[0265] In order to irradiate only light in a desired wavelength range, various filters such as a sharp cut filter, a band pass filter, a near infrared cut filter, a dichroic filter, an interference filter, and a color temperature conversion filter can be used.
[0266] Of these light sources, light emitting diodes and semiconductor lasers are preferably used since they have high irradiation energy and emit light with a long wavelength of 600 to 800 nm.
[0267] The transfer section 40 is disposed above the four image forming units 31Y, 31C, 31M, and 31K. The transfer section 40 includes a drive roller 41, a driven roller 42, an intermediate transfer belt 43 that is an intermediate transfer body that can rotate counterclockwise in the figure as the drive roller 41 is driven, primary transfer rollers 44Y, 44C, 44M, and 44K that are provided facing the photoconductors 311Y, 311C, 311M, and 311K across the intermediate transfer belt 43, and a secondary opposing roller 45 and a secondary transfer roller 46 that are provided facing each other across the intermediate transfer belt 43 at a transfer position of the toner image to paper. The transfer section 40 transfers the toner images of each color formed on the surfaces of the photoconductors 311Y, 311C, 311M, and 311K onto the surface of the intermediate transfer belt 43 in a superimposed manner.
[0268] The driving roller 41 is a roller that drives the intermediate transfer belt 43 to rotate.
[0269] The driven roller 42 is disposed inside the intermediate transfer belt 43 and is a roller for moving the intermediate transfer belt 43 endlessly.
[0270] The intermediate transfer belt 43 is an endless belt that is stretched around seven rollers arranged on the inside, and is designed to be endlessly movable in the direction of the arrow by the rotational drive of the drive roller 41.
[0271] The primary transfer rollers 44Y, 44C, 44M, and 44K are primary transfer members provided in a primary transfer device that is a primary transfer section that transfers the toner images on the surfaces of the photoconductors 311Y, 311C, 311M, and 311K to the intermediate transfer belt 43. The primary transfer rollers 44Y, 44C, 44M, and 44K sandwich the intermediate transfer belt 43 between the photoconductors 311Y, 311C, 311M, and 311K to form primary transfer nips, respectively. The primary transfer rollers 44Y, 44C, 44M, and 44K apply a transfer bias of the opposite polarity (e.g., positive) to that of the toner to the back surface (inner peripheral surface of the loop) of the intermediate transfer belt 43. As the intermediate transfer belt 43 moves endlessly, the Y, C, M, and K toner images on the photoconductors 311Y, 311C, 311M, and 311K are sequentially passed through the primary transfer nips for Y, C, M, and K, and are primarily transferred in a superimposed manner onto the surface of the intermediate transfer belt 43. As a result, a four-color superimposed toner image (hereinafter referred to as a four-color toner image) is formed on the intermediate transfer belt 43.
[0272] The secondary opposing roller 45 sandwiches the intermediate transfer belt 43 with a secondary transfer roller 46 disposed outside the loop of the intermediate transfer belt 43 to form a secondary transfer nip.
[0273] A secondary transfer bias is applied to the secondary transfer roller 46. The secondary transfer roller 46 is a secondary transfer member that performs secondary transfer of the four-color toner image on the intermediate transfer belt 43 all at once onto the transfer paper P. The four-color toner image on the intermediate transfer belt 43 is secondarily transferred all at once onto the transfer paper P in the secondary transfer nip due to the influence of the secondary transfer electric field and nip pressure formed between the secondary transfer roller 46 and the secondary opposing roller 45. This results in a color toner image.
[0274] After passing through the secondary transfer nip, residual toner that has not been transferred to the transfer paper P adheres to the intermediate transfer belt 43. The residual toner is cleaned by a belt cleaning unit (not shown).
[0275] When forming a monochrome image, the printer 1 revolves the primary transfer rollers 44Y, 44C, 44M, and 44K for Y, C, and M counterclockwise around the rotation axis of the driven roller 42 to separate the intermediate transfer belt 43 from the photoconductors 311Y, 311C, and 311M for Y, C, and M. Then, of the four imaging units 31Y, 31C, 31M, and 31K, only the imaging unit 31K for K is driven to form a monochrome image. This makes it possible to avoid wear and tear on the members constituting the imaging units due to unnecessary driving of the imaging units 31Y, 31C, and 31M when forming a monochrome image.
[0276] The fixing section 50 is disposed above the secondary transfer nip in the drawing. The fixing section 50 includes a fixing belt unit 51 that contains a heat source such as a halogen lamp and heats the transfer paper P, and a pressure roller 52 that rotatably presses the fixing belt unit 51 to form a fixing nip in contact with the fixing belt 621.
[0277] The transfer paper P that has passed through the secondary transfer nip described above is separated from the intermediate transfer belt 43 and then sent into the fixing section 50. Then, in the process of being conveyed from the bottom to the top in the figure while being sandwiched in the fixing nip inside the fixing section 50, the transfer paper P is heated and pressed by the fixing belt unit 51, so that heat and pressure are applied to the color toner image on the transfer paper P, and the color toner image is fixed to the transfer paper P.
[0278] The transfer paper P which has been subjected to the fixing process in this manner passes between the rollers of the paper discharge roller 23, and is then discharged onto the paper discharge tray 24. This completes a series of image forming processes.
[0279] The toner cartridge 60 is provided above the transfer unit 40 and includes toner cartridges 60Y, 60C, 60M, and 60K. The toner cartridges 60Y, 60C, 60M, and 60K accommodate Y, C, M, and K toners, respectively. The Y, C, M, and K toners in the toner cartridges 60Y, 60C, 60M, and 60K are appropriately supplied to the developing devices 313Y, 313C, 313M, and 313K of the image forming units 31Y, 31C, 31M, and 31K. These toner cartridges 60Y, 60C, 60M, and 60K are detachable from the printer body independently of the image forming units 31Y, 31C, 31M, and 31K.
[0280] <Process cartridge> The process cartridge according to one embodiment is molded so as to be detachably attached to various image forming devices, and has an electrostatic latent image carrier that carries an electrostatic latent image, and a developing unit that develops the electrostatic latent image carried on the electrostatic latent image carrier with a developer according to the above-mentioned one embodiment to form a toner image, and may have other configurations as necessary.
[0281] The electrostatic latent image carrier is the same as the electrostatic latent image carrier of the image forming apparatus described above, and therefore details thereof will be omitted.
[0282] The developing unit includes a developer container that contains the developer according to an embodiment, and a developer carrier that carries and transports the developer contained in the developer container. The developing unit may further include a regulating member or the like to regulate the thickness of the developer carried.
[0283] FIG. 7 shows an example of a process cartridge according to an embodiment. As shown in FIG. 7, the process cartridge 200 has a photoconductor drum 210, a corona charger 220 as a charging unit, a developing device 230, a transfer roller 240, and a cleaning device 250. An exposure device 260 is provided above the process cartridge 200. These members constituting the process cartridge 200 are the same as the photoconductors 311Y, 311C, 311M, and 311K, the charging devices 312Y, 312C, 312M, and 312K, the developing devices 313Y, 313C, 313M, and 313K, the photoconductor cleaning devices 314Y, 314C, 314M, and 314K, and the primary transfer rollers 44Y, 44C, 44M, and 44K shown in FIG. 5, so details are omitted.
[0284] In the process cartridge 200, the surface of the photosensitive drum 210 is uniformly charged using a corona charger 220, and after the surface of the photosensitive drum 210 is uniformly charged, the exposure device 260 is used to expose the photosensitive drum 210 to exposure light L to form an electrostatic latent image. The electrostatic latent image formed on the photosensitive drum 210 is then developed with toner supplied from a developing device 230 to form a toner image. The toner image formed on the photosensitive drum 210 is then transferred to the transfer paper P conveyed by the transfer roller 240 by a transfer bias applied by the roller.
[0285] <Image forming method> The image forming method of the present embodiment includes an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier, a developing step of developing the electrostatic latent image with a toner to form a toner image, a transfer step of transferring a visible image to a recording medium, and a fixing step of fixing the transferred image transferred to the recording medium, in which the toner is the toner of the present embodiment. Thus, the image forming method of the present embodiment can exhibit excellent coloring power and charging performance.
[0286] The image forming method of the present embodiment may further include other steps as necessary. The image forming method of the present embodiment may be suitably performed by the image forming apparatus of the present embodiment, the electrostatic latent image forming step may be suitably performed by the electrostatic latent image forming unit, the developing step may be suitably performed by the developing unit, and the other steps may be suitably performed by the other units.
[0287] Furthermore, the image forming method according to one embodiment more preferably includes, in addition to the electrostatic latent image forming process and the developing process described above, a transfer process of transferring the toner image onto a recording medium, and a fixing process of fixing the transferred image onto the surface of the recording medium.
[0288] In the developing step, the toner according to an embodiment is used. Preferably, a developer containing the toner according to an embodiment and, if necessary, other components such as a carrier may be used to form a toner image.
[0289] The electrostatic latent image forming process is a process of forming an electrostatic latent image on an electrostatic latent image carrier, and includes a charging process of charging the surface of the electrostatic latent image carrier and an exposure process of exposing the charged surface of the electrostatic latent image carrier to light to form an electrostatic latent image. Charging can be performed, for example, by applying a voltage to the surface of the electrostatic latent image carrier using a charger. Exposure can be performed, for example, by exposing the surface of the electrostatic latent image carrier to light in an imagewise manner using an exposure device. The electrostatic latent image can be formed, for example, by uniformly charging the surface of the electrostatic latent image carrier and then exposing it to light in an imagewise manner, and can be performed by an electrostatic latent image forming unit.
[0290] The developing process is a process of sequentially developing the electrostatic latent image with toners of multiple colors to form a visible image. The formation of the visible image can be performed, for example, by developing the electrostatic latent image with toners, and can be performed by a developing device.
[0291] In the developing device, for example, toner and carrier are mixed and stirred, and the toner becomes charged by friction during this process and is held in a standing state on the surface of the rotating magnet roller, forming a magnetic brush. Since the magnet roller is disposed near an electrostatic latent image carrier (photoconductor), a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the electrostatic latent image carrier (photoconductor) by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image made of the toner is formed on the surface of the electrostatic latent image carrier (photoconductor).
[0292] The transfer step is a step of transferring a visible image to a recording medium. The transfer step is preferably performed using an intermediate transfer body, and after the visible image is primarily transferred onto the intermediate transfer body, the visible image is secondarily transferred onto the recording medium. The transfer step is more preferably performed using toner of two or more colors, preferably full-color toner, and includes a primary transfer step of transferring the visible image onto the intermediate transfer body to form a composite transfer image, and a secondary transfer step of transferring the composite transfer image onto the recording medium. The transfer can be performed, for example, by charging an electrostatic latent image carrier (photoconductor) with a transfer charger, and can be performed by a transfer section.
[0293] The fixing process is a process in which the visible image transferred to the recording medium is fixed using a fixing device, and may be performed for each color developer each time it is transferred to the recording medium, or may be performed simultaneously for each color developer in a stacked state.
[0294] The image forming method according to the first embodiment may further include other steps appropriately selected as necessary, such as a static elimination step, a cleaning step, a recycling step, and the like.
[0295] The charge removing step is a step of removing electricity by applying a charge removing bias to the electrostatic latent image bearing member, and can be suitably performed by the charge removing unit.
[0296] The cleaning step is a step of removing the toner remaining on the electrostatic latent image carrier, and can be suitably performed by a cleaning unit.
[0297] The recycling step is a step in which the toner removed in the cleaning step is recycled to the developing unit, and can be suitably carried out by the recycling unit. EXAMPLES
[0298] The present invention will be described in more detail below based on examples, but the technical scope of the present invention is not limited to the following examples. In the following description, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0299] [Example 1] <Synthesis of amorphous polyester resin A-1 for core> Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 2 mol ethylene oxide adduct of bisphenol A / 3 mol propylene oxide adduct of bisphenol A (molar ratio 40 / 60) as a diol component, terephthalic acid / adipic acid (molar ratio 85 / 15) as a dicarboxylic acid component, and 3.5 mol% of trimethylolpropane relative to the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.2.
[0300] Furthermore, 1,000 ppm of tetrabutyl orthotitanate was added as a condensation catalyst based on the total monomer amount, and the mixture was heated to 230°C over 2 hours under a nitrogen stream, and reacted for 5 hours while distilling off the water produced. After that, the mixture was reacted for 4 hours under a reduced pressure of 5mmHg to 15mmHg, and cooled to 180°C. Then, 1.0 mol% of trimellitic anhydride based on the total monomer amount and 200 ppm of tetrabutyl orthotitanate based on the total monomer amount were added, and the mixture was reacted at 180°C under normal pressure for 1 hour, and then further reacted for 3 hours under a reduced pressure of 5mmHg to 20mmHg to obtain [Amorphous polyester resin A-1 for core] with an acid value of 18.
[0301] <Synthesis of amorphous polyester resin 1 for shell> A 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was charged with 122 parts of an ethylene oxide 2 mol adduct of bisphenol A, 199 parts of a propylene oxide 2 mol adduct of bisphenol A, 133 parts of terephthalic acid, 22 parts of adipic acid, and 4.7 parts of trimethylolpropane. 1000 ppm of tetrabutyl orthotitanate relative to the total monomer amount was added as a condensation catalyst. The temperature was raised to 230°C over 2 hours under a nitrogen stream, and the reaction was carried out for 5 hours while distilling off the generated water.
[0302] After that, the mixture was reacted for 4 hours under a reduced pressure of 5 mmHg to 15 mmHg and cooled to 180°C. After that, 0.21 parts of trimellitic anhydride and 200 ppm of tetrabutyl orthotitanate relative to the total monomer amount were added and reacted at normal pressure at 180°C for 1 hour, and then further reacted for 3 hours under a reduced pressure of 5 mmHg to 20 mmHg to obtain [Amorphous Polyester Resin 1 for Shell] with an acid value of 27.
[0303] <Preparation of Crystalline Polyester Resin Dispersion C-1a> (Synthesis of crystalline polyester resin C-1) 1,6-hexanediol and sebacic acid were charged into a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple so that the ratio of hydroxyl groups to carboxylic acid groups (OH / COOH) was 1.1. The mixture was reacted while discharging water together with 500 ppm of titanium tetraisopropoxide relative to the mass of the charged raw materials, and finally heated to 235°C and reacted for 1 hour. Then, the mixture was reacted for 6 hours under reduced pressure of 10 mmHg or less. Then, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio to the carboxylic acid group was 0.053, and the mixture was reacted for 2 hours with stirring to obtain [Crystalline polyester resin C-1].
[0304] (Preparation of crystalline polyester resin dispersion C-1a) A container equipped with a stirring rod and a thermometer was charged with 45 parts of [crystalline polyester resin C-1] and 450 parts of ethyl acetate. The temperature was raised to 80 °C under stirring and held at 80 °C for 5 hours. Then, it was cooled to 30 °C in 1 hour. Using a media disperser bead mill (Ultraviscomill, manufactured by IMAX Co., Ltd.), with a liquid feeding rate of 5 kg / hr and a disk peripheral speed of 6 m / s, 80% by volume of zirconia beads with a diameter of 0.5 mm were filled, and dispersion was carried out under the condition of 3 passes to obtain [crystalline polyester resin dispersion C-1a]. The solid content concentration of the obtained [crystalline polyester resin dispersion C-1a] was 10%.
[0305] <Preparation of WAX dispersion 1> A container equipped with a stirring rod and a thermometer was charged with 42 parts of carnauba wax (RN-5, plant-based wax, melting point 82 °C, manufactured by Noda Cerica Co., Ltd.) as a mold release agent and 420 parts of ethyl acetate. The temperature was raised to 80 °C under stirring and held at 80 °C for 5 hours. Then, it was cooled to 30 °C in 1 hour. Using a media disperser bead mill (Ultraviscomill, manufactured by IMAX Co., Ltd.), with a liquid feeding rate of 5 kg / hr and a disk peripheral speed of 6 m / s, 80% by volume of zirconia beads with a diameter of 0.5 mm were filled, and dispersion was carried out under the condition of 3 passes to obtain [WAX dispersion 1]. The solid content concentration of the obtained [WAX dispersion 1] was 10%.
[0306] <Preparation of colorant masterbatch 1> Pigment Yellow185 (PY185) and [amorphous polyester resin A-1 for core] were preliminarily mixed at a mass ratio of 1:1 using a Henschel mixer (FM20B, manufactured by Mitsui Miike Chemical Machinery Co., Ltd.), and then melted and kneaded at a temperature of 130 °C using a twin-screw kneader (PCM30, manufactured by Ikegai Corporation). The obtained kneaded product was rolled to a thickness of 2.7 mm using a roller and then cooled to room temperature using a belt cooler, and coarsely pulverized to a particle size of 200 μm to 300 μm using a hammer mill to obtain [colorant masterbatch 1].
[0307] <Preparation of core emulsion 1> (Oil phase preparation process) [Core amorphous polyester resin A-1] 790 parts, [Crystalline polyester resin dispersion C-1a] 59 parts, [WAX dispersion 1] 59 parts, [Colorant master batch 1] 75 parts were placed in a container and mixed with a shear disperser TK Homomixer (manufactured by Primix Corporation) at a peripheral speed of 12 m / s for 60 minutes to obtain [Oil phase 1]. The above blend amounts indicate the blend amounts of solids in each raw material. The solid concentration of the obtained [Oil phase 1] was 48%.
[0308] (Aqueous phase preparation process) 990 parts of water, 20 parts of sodium dodecyl sulfate, and 90 parts of ethyl acetate were mixed and stirred to obtain a milky white liquid, which was designated as [aqueous phase 1].
[0309] (Phase inversion emulsification process) While stirring 703 parts of [Oil phase 1] with a stirrer, 28% ammonia water, which corresponds to a neutralization rate of 100% relative to the acid value of [Amorphous polyester resin A-1 for core], was added and mixed for 10 minutes to perform a neutralization treatment, thereby obtaining [Oil phase 1 after neutralization treatment].
[0310] While stirring 708.1 parts of [neutralized oil phase 1] with a stirrer, 1197 parts of [water phase 1] was gradually added dropwise to obtain [core emulsion slurry 1]. Furthermore, [core emulsion slurry 1] was placed in a container equipped with a stirrer and a thermometer, and the solvent was removed at 30°C or less, and then ion-exchanged water was added to obtain [core emulsion 1] with a solid content concentration of 25%.
[0311] <Preparation of shell emulsion 1> (Preparation of amorphous polyester resin solution 1s for shell) 200 parts of [shell amorphous polyester resin 1] and 200 parts of methyl ethyl ketone were placed in a container and mixed for 60 minutes at a peripheral speed of 8 m / s using a TK homomixer (manufactured by Primix Corporation) to obtain [shell amorphous polyester resin solution 1]. The solid content of the obtained [shell amorphous polyester resin solution 1s] was 50%.
[0312] (Preparation of aqueous phase 2) 468 parts of water and 132 parts of methyl ethyl ketone were mixed and stirred. This was designated as [aqueous phase 2].
[0313] (Phase inversion emulsification process) While stirring 400 parts of [Shell Amorphous Polyester Resin Solution 1s] with a stirrer, 28% ammonia water equivalent to a neutralization rate of 100% for the acid value of [Shell Amorphous Polyester Resin 1] was added, and after mixing for 10 minutes, 600 parts of [Water Phase 2] was gradually added dropwise to obtain [Shell Emulsion 1]. Furthermore, [Shell Emulsion Slurry 1] was placed in a container equipped with a stirrer and a thermometer, and the solvent was removed at 30°C or less, and ion-exchanged water was added to obtain [Shell Emulsion 1] with a solid content concentration of 25%.
[0314] <Aggregation process and shell formation process> 100 parts of [Core Emulsion 1] and 25 parts of ion-exchanged water were placed in a container and stirred for 1 minute at 25° C. Then, 6.3 parts of a 20% aqueous magnesium sulfate solution was added dropwise and stirred for an additional 5 minutes, and the temperature was then raised to 55° C.
[0315] After that, when the particle size reached 5.0 μm, 18 parts of [Shell Emulsion 1] diluted with 27 parts of water was added, and 15 parts of a 20% aqueous magnesium sulfate solution was added dropwise and stirred for another 10 minutes, after which the temperature was raised to 65° C. and stirring was continued for 30 minutes. The temperature rise rate associated with the aggregation and shell formation was 2° C. / min.
[0316] <Fusing process and stopping process> Further, 30 parts of 20% sodium sulfate was added, and the mixture was heated to 70° C., and cooled when the desired circularity of 0.957 to 0.962 was reached, to obtain [Resin Particle Dispersion 1].
[0317] <Annealing process, washing process, and drying process> 100 parts of [Resin Particle Dispersion 1] was stored at 45° C. for 10 hours, filtered under reduced pressure, and washed and dried as follows. (1) [Resin particle dispersion 1] was filtered under reduced pressure, and 100 parts of ion-exchanged water was added to the filter cake obtained, and the mixture was mixed with a TK homomixer (at a peripheral speed of 8 m / s for 10 minutes) and then filtered. (2) 900 parts of ion-exchanged water was added to the filter cake of (1), and ultrasonic vibration was applied and mixed with a TK homomixer (circumferential speed 8 m / s for 30 minutes), and then the mixture was filtered under reduced pressure. This operation was repeated until the electrical conductivity of the reslurry liquid became 10 μC / cm or less, and then the mixture was filtered to obtain [Filter cake 1]. (3) [Filter cake 1] was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a 75 μm mesh to obtain [resin particle base 1].
[0318] <External attachment> 2.5 parts of inorganic fine particles, TS530 manufactured by Cabosil Corporation, were added to 100 parts of [Resin particle base 1], and mixed for 10 minutes at 40 m / s in a Henschel mixer to obtain [Resin particle 1].
[0319] [Examples 2 to 6 and Comparative Examples 1 to 3] Resin particles 2 to 6 and 15 to 17 were obtained by preparing resin particles in the same manner as resin particle 1, except that the peripheral speed of the shear disperser in the oil phase preparation process, the heating rate in the aggregation process and the shell formation process, and the temperature in the fusion process were changed as shown in Table 1.
[0320] [Examples 7 to 10] The peripheral speed of the shear disperser in the oil phase preparation step, the heating rate in the aggregation step and the shell formation step, and the temperature in the fusion step were changed as shown in Table 1, and furthermore, in the neutralization treatment in the phase inversion emulsification step, an additional dispersion treatment was carried out using a shear machine as shown below. The rest of the procedure was the same as for resin particle 1, and resin particles 7 to 10 were obtained.
[0321] As an example, the neutralization treatment of Example 7 is shown below. The neutralization treatments of Examples 8 to 10 were carried out in the same manner as in Example 7, except that the peripheral speed of shear dispersion was set to the peripheral speeds shown in Table 1.
[0322] (Neutralization treatment) While stirring 703 parts of [oil phase 7] obtained in the same manner as in Example 1 with a stirrer, 5.1 parts of 28% ammonia water, which corresponds to a neutralization rate of 100% for an acid value of 18 of [core amorphous polyester resin A-1], was added and mixed for 10 minutes, and further mixed with a shear disperser TK Homomixer (manufactured by Primix Corporation) at a peripheral speed of 12 m / s for 30 minutes to obtain [neutralized oil phase 7].
[0323] [Examples 11 to 14] The peripheral speed of the shear disperser in the oil phase preparation step, the temperature rise rate in the aggregation step and the shell formation step, and the temperature in the fusion step were changed as shown in Table 1, and furthermore, in the neutralization treatment in the phase inversion emulsification step, an additional dispersion treatment was carried out using a media disperser as shown below. The rest of the procedure was the same as for resin particle 1, and resin particles 11 to 14 were obtained.
[0324] As an example, the neutralization treatment of Example 11 is shown below. The neutralization treatments of the other Examples 12 to 14 were carried out in the same manner as Example 11, except that the peripheral speed or bead diameter of the media dispersion shown in Table 1 was used.
[0325] (Neutralization treatment) While stirring 703 parts of [oil phase 11] obtained in the same manner as in Example 1 with a stirrer, 5.1 parts of 28% ammonia water, which corresponds to a neutralization rate of 100% for an acid value of 18 for the [core amorphous polyester resin A-1], was added and mixed for 10 minutes. Further, using a media dispersing bead mill (Ultraviscomill, manufactured by Imex), the mixture was dispersed under conditions of a liquid feed rate of 5 kg / hr, a disk peripheral speed of 10 m / s, and 80% by volume of zirconia beads having a diameter of 0.5 mm, and 3 passes to obtain [oil phase 11 after neutralization treatment].
[0326] [Comparative Example 4] Unlike resin particles 1 to 17, which are produced by aggregating an oil phase inversion emulsion containing a binder resin and a colorant, the resin particles were produced by aggregating particles in an aqueous dispersion of a binder resin, etc. and an aqueous dispersion of a colorant.
[0327] <Preparation of amorphous polyester resin aqueous dispersion A-1w> (Preparation of amorphous polyester resin solution A-1s) 200 parts of [Amorphous polyester resin for core A-1] and 200 parts of methyl ethyl ketone were placed in a container and mixed for 60 minutes at a peripheral speed of 8 m / s using a TK homomixer (manufactured by Primix Corporation) to obtain [Amorphous polyester resin solution A-1s]. The solid content of the obtained [Amorphous polyester resin solution A-1s] was 50%.
[0328] While stirring 400 parts of [amorphous polyester resin solution A-1s] with a stirrer, 28% ammonia water corresponding to a neutralization rate of 100% for the acid value of [core amorphous polyester resin A-1] was added, and after mixing for 10 minutes, 600 parts of [water phase 2] was gradually added dropwise to obtain [emulsion slurry 2]. Furthermore, [emulsion slurry 2] was placed in a container equipped with a stirrer and a thermometer, and the solvent was removed at 30°C or less, and ion-exchanged water was added to obtain [amorphous polyester resin aqueous dispersion A-1w] with a solid content concentration of 25%.
[0329] <Preparation of crystalline polyester resin aqueous dispersion C-1w> (Crystalline polyester resin solution C-1s preparation) 200 parts of [Crystalline polyester resin C-1] and 200 parts of methyl ethyl ketone were placed in a container and mixed for 60 minutes at a peripheral speed of 8 m / s using a TK homomixer (manufactured by Primix Corporation) to obtain [Crystalline polyester resin solution C-1s]. The solid content of the obtained [Crystalline polyester resin solution C-1s] was 50%.
[0330] (Phase inversion emulsification process: Preparation of emulsified slurry and emulsion) While stirring 400 parts of the solution of [Crystalline polyester resin solution C-1s] with a stirrer, 28% ammonia water corresponding to a neutralization rate of 100% for the acid value of [Crystalline polyester resin C-1] was added, and after mixing for 10 minutes, 600 parts of [Water phase 2] was gradually added dropwise to obtain [Emulsion slurry 3]. Furthermore, [Emulsion slurry 3] was placed in a container equipped with a stirrer and a thermometer, and the solvent was removed at 30°C or less, and ion-exchanged water was added to obtain [Crystalline polyester resin aqueous dispersion C-1w] with a solid content concentration of 25%.
[0331] <Preparation of WAX Dispersion 2> 50 parts of carnauba wax (RN-5, plant-based wax, melting point 82°C, manufactured by Noda Cerica Co., Ltd.), 5 parts of cationic surfactant (Sanisol B50), and 200 parts of ion-exchanged water were heated to 95°C, dispersed using a homogenizer, and then dispersed using a pressure discharge type homogenizer to obtain an aqueous dispersion [WAX Dispersion 2] containing release agent fine particles. The solid content concentration of the obtained [WAX Dispersion 2] was 20%.
[0332] <Preparation of Colorant Dispersion 1> 50 parts of Pigment Yellow 185 (PY185), 5 parts of nonionic surfactant (Emulgen 150), and 200 parts of ion-exchanged water were mixed and dissolved, and dispersed using a homogenizer to obtain an aqueous dispersion [Colorant Dispersion 1] containing colorant fine particles. The solid content concentration of the obtained [Colorant Dispersion 1] was 20%.
[0333] <Agglomeration Step and Shelling Step> 790 parts of [Amorphous Polyester Resin Aqueous Dispersion A-1w], 59 parts of [Crystalline Polyester Resin Aqueous Dispersion C-1w], 59 parts of [WAX Dispersion 2], 75 parts of [Colorant Dispersion 1], and 845 parts of ion-exchanged water were placed in a container and stirred at 25°C for 1 minute. The above blending amounts indicate the blending amounts of the solid content in each raw material. The solid content concentration during stirring before agglomeration was 20%.
[0334] Next, 92 parts of a 20% magnesium sulfate aqueous solution was added dropwise and stirred for an additional 5 minutes, and then the temperature was raised to 55°C. Thereafter, when the particle size reached 5.0 μm, a diluted solution of 263 parts of [Shell Emulsion 1] with 395 parts of water was added. Further, 219 parts of a 20% magnesium sulfate aqueous solution was added dropwise and stirred for an additional 10 minutes, and then the temperature was raised to 65°C and stirred for 30 minutes. The heating rate associated with agglomeration and shelling was set at 2°C / min.
[0335] <Fusing Step and Stopping Step> Furthermore, 439 parts of 20% sodium sulfate were added, heated to 70 °C, cooled when the desired circularity reached 0.957 to 0.962, and [Resin Particle Dispersion Liquid 18] was obtained.
[0336] As described above, it was prepared in the same manner as Resin Particle 1 except for the changes, and [Resin Particle 18] was obtained.
[0337] The production conditions of the resin particles obtained as above are shown in Table 1.
Table 1
[0338] Next, each of the obtained resin particles was evaluated as follows. The results are shown in Table 2.
[0339] <CH Ratio> Using a Raman microscope "XploRA PLUS" (manufactured by Horiba, Ltd.), Raman spectra of 500 to 600 particles per resin particle 1 were measured with a laser having an excitation wavelength of 638 nm. The CH ratio was calculated from the obtained Raman spectra, and the number ratio of resin particles having an absolute value of the CH ratio of 20.0% or more to all resin particles, and the number ratio of resin particles having an absolute value of 35.0% or more to all resin particles were determined.
[0340] <BET Specific Surface Area> Using Macsorb model-1201 manufactured by MOUNTECH, 1 g of the resin particle matrix that had been degassed at 30 °C for 30 minutes was used for measurement. The resin particle matrix is the resin particles in the state before external addition.
[0341] <Coloring Agent Surface Layer Distribution Ratio> After embedding the resin particles in an epoxy resin, thin slices with a thickness of 0.1 μm to 0.2 μm were prepared with a microtome (diamond knife (blade angle 45°)), observed with a TEM at a magnification of 10,000 times and an acceleration voltage of 0.8 to 2 kV, and a cross-sectional image was obtained.
[0342] After obtaining the cross-sectional image of the resin particles, the amount of the pigment having an isoindoline skeleton in the cross-section of the resin particles is measured according to the following procedure. (1) Ten resin particles with an average volume particle size Dv ± 1 μm were extracted. (2) Using the image analysis software "Image-Pro Premier", the contour was extracted from the cross-sectional image of the resin particles. (3) For the colorant as well, the contour was extracted from the contrast in the same manner as in (2). (4) When the major axis of the resin particle is L, the center of a circle with a radius r (L / 10) was moved along the contour of the cross-section of the resin particle. (5) The overlapping region where the passing region through which the circle passed overlapped with the cross-section of the resin particle was defined as the resin particle surface layer, and the area of the pigment having an isoindoline skeleton in the resin particle surface layer was calculated. (6) The areas of all the cross-sections of the pigment having an isoindoline skeleton present in the cross-sectional image of the resin particles were measured. (7) The ratio of the area of the pigment having an isoindoline skeleton in the resin particle surface layer to the total area of the pigment having an isoindoline skeleton in the cross-section of the resin particle was calculated. (8) For ten resin particles, the average value of the values obtained by repeating the operations (2) to (7) above was defined as the colorant presence rate of the resin particle surface layer.
[0343] <WST rate> The charge amount distribution of the resin particles was measured for the Q / d distribution (fC / μm) using a charge amount distribution measuring device, Easpart Analyzer (manufactured by Hosokawa Micron), and the percentage of the number of positive charge regions was calculated as the WST (Wrong Sign Toner) rate. (Evaluation criteria) A: The WST rate is less than 8.0%. B: The WST rate is 8.0% or more and less than 9.5%. C: The WST rate is 9.5% or more and less than 11.0%. D: The WST rate is 11.0% or more.
[0344] <Charge stability> The developer was set in a modified imageo MP C5503 (manufactured by Ricoh Co., Ltd.), and a running evaluation was performed on 300,000 sheets of an image chart with a 50% image area in monochrome mode.Then, the charge stability was evaluated based on the evaluation criteria using the charge amount change of the carrier after this running.
[0345] The amount of change in charge was as follows: That is, the sample was prepared by conditioning the humidity in an open system for 30 minutes or more in an environment of 23°C temperature and 50% relative humidity (M / M environment), adding 6,000 g of the initial carrier and 0.452 g of resin particles to a stainless steel container, sealing it, and operating a shaker (YS-LD, Yayoi) at 150 for 5 minutes, shaking it about 1,100 times to triboelectrically charge the sample.
[0346] The charge amount of the sample measured by the blow-off method (Toshiba Chemical: TB-200) was defined as Q1, and the charge amount of the carrier obtained by removing the resin particles in the developer after running with a blow-off device was measured in the same manner as above and defined as Q2. The charge amount change was defined as the absolute value (|Q1-Q2|) of the charge amount Q1 minus the charge amount Q2. (Evaluation Criteria) A: Charge change is less than 10 μc / g B: Charge change is 10 μc / g or more and less than 15 μc / g C: Charge change is 15 μc / g or more and less than 20 μc / g D: Charge change is 20μc / g or more
[0347] <Coloring power> The carrier used in imageo MP C5503 (manufactured by Ricoh Company, Ltd.) and the resin particles obtained above were mixed so that the concentration of the resin particles was 5% by mass, to obtain a two-component developer.
[0348] Using each two-component developer, resin particles were deposited on an aluminum substrate in a cascade development process with a resin particle adhesion of 0.3 mg / cm 2 After developing the image, the image was electrostatically transferred from the aluminum substrate to Tokubishi Art double-sided paper and fixed with a belt fixing machine (linear speed 282 mm / sec, nip time 40.1 msec, nip pressure 37 N / cm 2) and a fixed image was created at a fixing temperature of 180°C.
[0349] The ID of the obtained image was measured using a Model 938 (manufactured by X-Rite), and the coloring strength was evaluated based on the following evaluation criteria: If the ID of the relevant color was 1.55 or more, it was rated as very good (A), if it was 1.50 or more and less than 1.55, it was rated as good (B), if it was 1.45 or more and less than 1.50, it was rated as fair (C), and if it was less than 1.45, it was rated as poor (D). (Evaluation Criteria) A: The color ID is 1.55 or higher. B: The color ID is between 1.50 and 1.55. C: The color ID is between 1.45 and 1.50 D: The ID of the color is less than 1.45
[0350] <Overall Judgment> Based on the individual evaluation results of WST rate, charge stability, and coloring power, an overall evaluation was determined according to the following criteria. (Evaluation Criteria) AA: All three evaluation items are rated A A: 2 evaluation items are A (and the remaining 1 evaluation item is B) B: No C or D evaluation items, A is 0~1 evaluation items C: There is at least one C evaluation item D: D is given to one or more evaluation items
[0351] [Table 2]
[0352] From the results in Table 2, it can be seen that Examples 1 to 14 of the present invention exhibit excellent coloring power and excellent charging performance. Comparative Examples 1 to 3 have problems with at least either coloring power or charging performance due to an increase in the CH ratio or colorant surface layer presence ratio caused by insufficient material dispersion during the oil phase preparation process or neutralization treatment before phase inversion emulsification, or an increase in the BET specific surface area caused by insufficient surface smoothing due to fusion.
[0353] In the method of Comparative Example 4, a colorant aqueous dispersion is prepared and then aggregated to form resin particles. However, compared to a method in which an oil phase containing an organic solvent is prepared from a binder resin and a colorant, and this is then subjected to phase inversion emulsification and aggregated, the dispersibility of the pigment having an isoindoline skeleton is low, and the coloring power and charging performance are reduced.
[0354] (Embodiments of the present invention) The present invention includes the following aspects. <Aspect 1> Resin particles containing at least a binder resin and a colorant, the colorant containing a pigment having an isoindoline skeleton, and the resin particles having a Raman spectroscopy -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by the following (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of a CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. CH rate (%)=[(In-Iave) / Iave]×100...(Formula 1) <Aspect 2> The BET specific surface area of the resin particles is 0.80 m 2 / g or more, 1.40m 2 / g or less. <Aspect 3> In the resin particles according to embodiment 1 or 2, the proportion of the resin particles having an absolute value of the CH ratio of 35.0% or more to the total number of resin particles is 7.0% or less by number. <Aspect 4> The resin particle is described in any one of aspects 1 to 3, in which when the major axis of the cross-section of the resin particle is L, and the area through which a circle with a radius of L / 10 passes when the center of the circle moves along the contour of the cross-section of the resin particle overlaps with the cross-section of the resin particle, the area of the pigment having the isoindoline skeleton in the surface layer of the resin particle is less than 30.0% of the total area of the pigment having the isoindoline skeleton in the cross-section of the resin particle. <Aspect 5> A method for producing resin particles including at least a binder resin and a colorant, comprising the steps of: a step of aggregating particles in a dispersion of at least the binder resin and the colorant, The colorant contains a pigment having an isoindoline skeleton, and the resin particles have a Raman spectrum of 950 cm -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by the following (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of a CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. CH rate (%)=[(In-Iave) / Iave]×100...(Formula 1) <Aspect 6> A method for producing resin particles including at least a binder resin and a colorant, comprising the steps of: A step of preparing an oil phase by dissolving or dispersing at least a binder resin and a colorant in an organic solvent; adding water to the oil phase to invert the water-in-oil dispersion into an oil-in-water dispersion; aggregating particles in the oil-in-water dispersion, The colorant contains a pigment having an isoindoline skeleton, and the resin particles have a Raman spectrum of 950 cm -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by the following (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of a CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. CH rate (%)=[(In-Iave) / Iave]×100...(Formula 1) <Aspect 7> A toner comprising the resin particles according to any one of the first to fourth aspects. <Aspect 8> A method for producing a toner, comprising the step of adding at least an external additive to the resin particles according to any one of the first to fourth aspects. <Aspect 9> A developer comprising the toner according to embodiment 7. <Aspect 10> A toner storage unit containing the toner according to aspect 7. <Aspect 11> An electrostatic latent image carrier; an electrostatic latent image forming unit for forming an electrostatic latent image on the electrostatic latent image carrier; a developing section for developing the electrostatic latent image with toner to form a visible image; a transfer section for transferring the visible image onto a recording medium; a fixing unit that fixes the transferred image on the recording medium, The image forming apparatus according to claim 7, wherein the toner is the toner according to claim 7. <Aspect 12> an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with a toner to form a visible image; a transfer step of transferring the visible image onto a recording medium; A fixing step of fixing the transferred image transferred onto the recording medium, The image forming method according to claim 7, wherein the toner is the toner according to claim 7.
[0355] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0356] 1. Image forming device 100 resin particles 101 Center of the circle 102 Resin particle surface layer 103 Pigments with isoindoline skeleton 200 Process Cartridge 311Y, 311C, 311M, 311K photoreceptor 312Y, 312C, 312M, 312K Charging device 313Y, 313C, 313M, 313K developing device (developing section) 40 Transcription section 50 Fixing unit [Prior art documents] [Patent documents]
[0357] [Patent Document 1] JP 2008-70466 A
Claims
1. Resin particles containing at least a binder resin and a colorant, the colorant containing a pigment having an isoindoline skeleton, and the resin particles having a Raman spectroscopy -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by the following (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of a CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. CH rate (%) = [(In-Iave) / Iave] x 100... (Formula 1)
2. The BET specific surface area of the resin particles is 0.80 m 2 / g or more, 1.40m 2 The resin particles according to claim 1, characterized in that the molecular weight of the resin particles is 1 / g or less.
3. 3. The resin particles according to claim 2, wherein the number ratio of the resin particles having an absolute value of the CH ratio of 35.0% or more to the total number of the resin particles is 7.0% or less.
4. 4. The resin particle according to claim 3, wherein when the long axis of the cross section of the resin particle is L, and the overlapping area where the cross section of the resin particle overlaps with the area through which the center of a circle with a radius of L / 10 passes when moved along the contour of the cross section of the resin particle, the area of the pigment having the isoindoline skeleton on the surface layer of the resin particle is less than 30.0% of the total area of the pigment having the isoindoline skeleton on the cross section of the resin particle.
5. A method for producing resin particles including at least a binder resin and a colorant, comprising the steps of: a step of aggregating particles in a dispersion of at least the binder resin and the colorant, The colorant contains a pigment having an isoindoline skeleton, and the resin particles have a Raman spectrum of 950 cm -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by the following (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of a CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. CH rate (%) = [(In-Iave) / Iave] x 100... (Formula 1)
6. A method for producing resin particles including at least a binder resin and a colorant, comprising the steps of: A step of preparing an oil phase by dissolving or dispersing at least a binder resin and a colorant in an organic solvent; adding water to the oil phase to invert the water-in-oil dispersion into an oil-in-water dispersion; aggregating particles in the oil-in-water dispersion, The colorant contains a pigment having an isoindoline skeleton, and the resin particles have a Raman spectrum of 950 cm -1 ~3250cm -1 When the intensity of the Raman spectrum at wave number k of each resin particle obtained in the wave number region is normalized to 1, -1 ~3250cm -1 The integral intensity of the spectrum of each resin particle obtained in the wave number region is In, the average value of In is Iave, and the value calculated by the following (Equation 1) is the CH ratio. The number ratio of resin particles having an absolute value of a CH ratio of 20.0% or more to all resin particles is 1.0 number% or more and 30.0 number% or less, and the BET specific surface area is 0.80 m 2 / g or more, 1.60m 2 / g or less. CH rate (%) = [(In-Iave) / Iave] x 100... (Formula 1)
7. A toner comprising the resin particles according to any one of claims 1 to 4.
8. A method for producing a toner, comprising the step of adding at least an external additive to the resin particles according to any one of claims 1 to 4.
9. A developer comprising the toner according to claim 7.
10. A toner storage unit containing the toner according to claim 7.
11. An electrostatic latent image carrier; an electrostatic latent image forming unit for forming an electrostatic latent image on the electrostatic latent image carrier; a developing section for developing the electrostatic latent image with toner to form a visible image; a transfer section for transferring the visible image onto a recording medium; a fixing unit that fixes the transferred image on the recording medium, An image forming apparatus, wherein the toner is the toner according to claim 7.
12. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with a toner to form a visible image; a transfer step of transferring the visible image onto a recording medium; A fixing step of fixing the transferred image transferred onto the recording medium, The image forming method according to claim 7 , wherein the toner is the toner according to claim 7 .