Decorative sheet and decorative material, and method for manufacturing decorative sheet and decorative material

The decorative sheet design with a specific layer structure and light-irradiated ridged portions addresses particle fallout and texture complexity, achieving a durable, low-gloss, and tactilely pleasing surface without matting agents or embossing plates.

JP2024155692APending Publication Date: 2024-10-31TOPPAN HOLDINGS INC

Patent Information

Application Number
JP2023197331
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2023-11-21
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Decorative sheets with added matting agents face issues such as particle fallout leading to scratches and changes in surface gloss, and embossing processes require individual embossing plates for texture, which can be cumbersome.

Method used

A decorative sheet design featuring a raw fabric layer, pattern layer, adhesive layer, transparent resin layer, and a surface protective layer with a thickness of 2 μm to 18 μm, a ratio of cutting level difference Rdc to thickness of 0.1 to 0.2, and particles with an average size of 3 μm or more, along with a low gloss of less than 10, achieved through a manufacturing process involving light irradiation to form ridged portions.

Benefits of technology

The solution provides a decorative sheet with excellent design and feel, offering a moist tactile sensation, low gloss, and durability without the need for a matting agent and embossing plates, ensuring long-lasting aesthetic appeal and scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155692000001_ABST
    Figure 2024155692000001_ABST
Patent Text Reader

Abstract

To provide a decorative sheet and a decorative material having excellent designability and touch feeling, and a method for manufacturing a decorative sheet and a decorative material.SOLUTION: A decorative sheet 10 includes a raw fabric layer 2, and a surface protective layer 6 which has an uneven shape formed with a ridge-like part raised into a ridge shape and is provided on an upper side UP of the raw fabric layer 2, wherein the surface protective layer 6 has a thickness of 2 μm or more and 18 μm or less, has a ratio of a cutting level difference Rdc to the thickness of 0.1 or more and 0.2 or less, contains particles having an average particle diameter of 3 μm or more, and has 60-degree reflection glossiness of less than 10.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative sheet and a decorative material, and a method for producing the decorative sheet and the decorative material. [Background technology]

[0002] Conventionally, there are decorative sheets used for the surface decoration of interior materials and fittings for buildings such as houses, building materials such as fittings, furniture and fixtures, housing equipment, home appliances, etc. Decorative sheets are required to have durability such as abrasion resistance, scratch resistance, and stain resistance so that the beauty of the surface is not impaired even after long-term use.

[0003] There are also decorative sheets that have a matte finish imparted by adding a matte agent such as silica or talc to the protective layer provided on the surface of the decorative sheet. The matte finish is imparted to the decorative sheet by using particles of an indefinite shape having irregular corners and edges as the matte agent, and by causing some of these particles to protrude from the average surface of the protective layer to form a fine uneven shape.

[0004] There are also decorative sheets in which a protective layer provided on the surface of the decorative sheet is embossed with an embossing plate to form a concave-convex shape, thereby imparting a desired texture and feel to the surface. An example of a decorative sheet imparted with a matte finish and a concave-convex shape by an embossing plate is the decorative sheet described in Patent Document 1. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-199240 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in a decorative sheet to which a matting agent has been added, when an article or the like comes into contact with the surface of the decorative sheet, there is a risk that the particles added as the matting agent will fall off due to the contact of the article or the like. Furthermore, the fallen particles may rub against the surface of the protective layer, causing scratches on the surface of the decorative sheet and changing the surface shape of the protective layer, which may cause a change in the gloss of the surface of the decorative sheet and a decrease in its aesthetic appearance. In addition, if a large amount of matting agent is added, the protective layer may become cloudy, making it difficult to see the pattern in the pattern layer provided below the protective layer.

[0007] Furthermore, when imparting a tactile feel to a decorative sheet by embossing, an embossing plate must be prepared for each pattern of concave and convex shapes to be embossed.

[0008] In view of the above circumstances, an object of the present invention is to provide a decorative sheet and decorative material having excellent design and feel, and a method for producing the decorative sheet and decorative material. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention proposes the following means. The decorative sheet of the present invention comprises an original fabric layer and a surface protective layer having an uneven shape with ridge-like raised portions formed thereon, the surface protective layer having a thickness of 2 μm or more and 18 μm or less, a ratio of the cut level difference Rdc to the thickness of 0.1 or more and 0.2 or less, containing particles with an average particle size of 3 μm or more, and having a 60-degree reflected gloss of less than 10.

[0010] The decorative sheet further comprises a pattern layer provided on the upper side of the original fabric layer and a primer layer provided on the lower side of the original fabric layer, and the original fabric layer may have a resin layer and a skin layer provided on the upper and lower sides of the resin layer and containing a nucleating agent or inorganic particles.

[0011] The decorative sheet may further include a pattern layer provided on the upper side of the original fabric layer, an adhesive layer provided on the upper side of the pattern layer, a transparent resin layer provided on the upper side of the adhesive layer, and a primer layer provided on the lower side of the original fabric layer.

[0012] In the decorative sheet, the particles may have an average particle size of 11 μm or less.

[0013] In the decorative sheet, the surface protective layer may contain an ionizing radiation curable resin.

[0014] In the decorative sheet, the surface protective layer may contain acrylate.

[0015] In the decorative sheet, the surface protective layer may contain a trifunctional acrylate containing a repeating structure, and the number of repetitions of the repeating structure may be 3 or more and 20 or less.

[0016] In the decorative sheet, the surface protective layer may contain a tetrafunctional acrylate containing a repeating structure, and the number of repetitions of the repeating structure may be 20 or more and 35 or less.

[0017] The decorative material of the present invention comprises any of the decorative sheets described above and a substrate provided below the decorative sheet.

[0018] The method for manufacturing a decorative sheet of the present invention includes a pattern printing step of forming a pattern layer on the upper side of an original layer, a protective layer coating step of forming a surface protective layer on the upper side of the pattern layer, and a light irradiation step of irradiating the surface of the surface protective layer with light having a wavelength of 200 nm or less to form a ridge portion so that the ratio of the cut level difference Rdc to the thickness of the surface protective layer is 0.1 or more and 0.2 or less.

[0019] In the method for producing a decorative sheet, the protective layer coating step may form the surface protective layer so that the thickness of the surface protective layer is 2 μm or more and 18 μm or less.

[0020] The method for producing a decorative material of the present invention comprises the method for producing a decorative sheet described above, and a substrate adhering step of attaching a substrate to the underside of the decorative sheet. Effect of the Invention

[0021] According to the decorative sheet and decorative material, and the manufacturing method of the decorative sheet and decorative material of the present invention, it is possible to provide a decorative sheet and decorative material, and a manufacturing method of a decorative sheet and decorative material, which have excellent design and feel. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic diagram of a decorative sheet according to an embodiment of the present invention. [Diagram 2] 3 is a photograph showing an example of the uneven shape of the decorative sheet. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic view of a surface protective layer of the decorative sheet. [Figure 4] 4 is a flowchart showing an example of a method for producing the decorative sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] An embodiment of the present invention will be described with reference to the drawings.

[0024] FIG. 1 is a cross-sectional view that shows a schematic diagram of a decorative sheet 10 according to this embodiment. In this embodiment, as shown in Figure 1, the thickness direction of the decorative sheet 10 is defined as the "vertical direction V", the direction in which the surface protective layer 6 of the decorative sheet 10 is provided is defined as the "upper side UP" in the vertical direction V, and the opposite direction is defined as the "lower side LO" in the vertical direction V.

[0025] The decorative sheet 10 comprises a primer layer 1 , a base fabric layer 2 , a design layer 3 , an adhesive layer 4 , a transparent resin layer 5 , and a surface protective layer 6 .

[0026] The primer layer 1 is a layer provided on the lower side LO of the decorative sheet 10. As the primer layer 1, a polyester-based resin, a urethane-based resin, an acrylic-based resin, or the like can be used. In particular, it is preferable to use a two-component curing type urethane-based resin for the primer layer 1. The primer layer 1 is formed on the lower side LO of the raw fabric layer 2 by a known printing method such as gravure printing, offset printing, flexographic printing, silk screen printing, or inkjet printing. The primer layer 1 may also be formed using a known coating device.

[0027] An inorganic filler may be added to the primer layer 1. Examples of the inorganic filler that can be added to the primer layer 1 include silica, alumina, magnesia, titanium oxide, and barium sulfate.

[0028] The raw fabric layer 2 is a layer provided on the upper side UP of the primer layer 1. As the raw fabric layer 2, paper such as tissue paper, titanium paper, or resin-impregnated paper, or synthetic resin such as polyethylene, polypropylene, polybutylene, polystyrene, polycarbonate, polyester, polyamide, ethylene-vinyl acetate copolymer, polyvinyl alcohol, or acrylic can be used. As the raw fabric layer 2, a sheet (film) such as an olefin film can also be used.

[0029] Furthermore, rubber such as ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber, styrene-butadiene copolymer rubber, styrene-isoprene-styrene block copolymer rubber, styrene-butadiene-styrene block copolymer rubber, or polyurethane can be used as the raw fabric layer 2. Furthermore, organic or inorganic nonwoven fabric may be used as the raw fabric layer 2, or metal foil using metals such as aluminum, iron, gold, or silver may be used.

[0030] Alternatively, the raw fabric layer 2 may have a three-layer structure having a resin layer formed from an olefin-based resin or the like, and skin layers provided on the upper side UP and lower side LO of the resin layer and containing a nucleating agent or inorganic particles.

[0031] The thickness of the original fabric layer 2 is preferably 20 μm or more and 250 μm or less from the viewpoint of printability and cost. In addition, when an olefin-based resin is used as the original fabric layer 2, the surface of the original fabric layer 2 may be in an inactive state. Therefore, when a substrate such as a wooden board or a metal board (not shown) is provided on the lower side LO of the original fabric layer 2, the adhesion between the original fabric layer 2 and the substrate can be improved by providing a primer layer 1 between the original fabric layer 2 and the substrate.

[0032] Furthermore, the raw fabric layer 2 may be subjected to a surface modification treatment such as a corona treatment, a plasma treatment, an ozone treatment, an electron beam treatment, an ultraviolet treatment, or a dichromate treatment.

[0033] The pattern layer 3 is a layer provided on the upper side UP of the base fabric layer 2. The pattern layer 3 is a layer formed by printing a pattern such as wood grain, stone grain, or sand grain. As a printing method, a known printing method such as gravure printing, offset printing, flexographic printing, silk screen printing, or inkjet printing can be used. Also, for the pattern layer 3, a known printing ink suitable for the printing method to be adopted can be used.

[0034] The binder resin in the ink of the design layer 3 may be nitrocellulose, cellulose, vinyl chloride-vinyl acetate copolymer, polyvinyl butyral, polyurethane, acrylic, polyesters, or modified products thereof, either alone or in combination. The binder resin may be water-based, solvent-based, or emulsion type, and may be a one-component type or a two-component type using a hardener. The design layer 3 may be formed by a method in which a layer formed with a hardening ink is hardened by irradiation with ultraviolet rays, electron beams, or the like. For example, the design layer 3 may be formed by using a urethane-based ink and hardening the ink with isocyanate.

[0035] The ink used to form the design layer 3 may contain various additives such as colorants such as dyes, extender pigments, solvents, light stabilizers, and ultraviolet absorbers in the binder resin of the ink. Examples of pigments used in the design layer 3 include condensed azo, insoluble azo, quinacridone, isoindoline, anthraquinone, imidazolone, cobalt, phthalocyanine, carbon, titanium oxide, iron oxide, and pearl pigments such as mica.

[0036] The adhesive layer 4 is a layer provided on the upper side UP of the pattern layer 3. Known adhesive resins such as polyethylene, acrylic, polyester, and epoxy resins can be used as the adhesive layer 4. Also, ethylene-vinyl acetate copolymer resin adhesives, two-component curing urethane resins, and the like can be used as the adhesive layer 4.

[0037] The adhesive layer 4 is preferably made of a transparent or semi-transparent material that allows the pattern of the pattern layer 3 to be seen through. A melt extrusion molding method can be used to form the adhesive layer 4. The adhesive layer 4 may also be formed by a known printing method such as gravure printing, offset printing, flexographic printing, silk screen printing, or inkjet printing, or by using a known coating device.

[0038] The adhesive layer 4 is a layer intended to improve adhesion between the pattern layer 3 and the transparent resin layer 5. Therefore, if the pattern layer 3 and the transparent resin layer 5 have sufficient adhesion without providing the adhesive layer 4, the decorative sheet 10 does not need to include the adhesive layer 4.

[0039] The transparent resin layer 5 is a layer provided on the upper side UP of the adhesive layer 4. An olefin-based resin is preferably used as the transparent resin layer 5. Examples of the olefin-based resin used for the transparent resin layer 5 include polypropylene, polyethylene, polybutene, and the like, as well as α-olefins (e.g., propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl ... Examples of the polymerizable compound include a homopolymer of α-olefins (e.g., 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, etc.) or a copolymerization of two or more of them, and a copolymerization of ethylene or α-olefins with other monomers such as an ethylene-vinyl acetate copolymer, an ethylene-vinyl alcohol copolymer, an ethylene-methyl methacrylate copolymer, an ethylene-ethyl methacrylate copolymer, an ethylene-butyl methacrylate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-ethyl acrylate copolymer, an ethylene-butyl acrylate copolymer, etc. Furthermore, vinyl chloride resin, acrylic resin, polyester resin, etc. may be used as the transparent resin layer 5.

[0040] In order to improve the surface strength of the decorative sheet 10, it is preferable to use crystalline polypropylene as the transparent resin layer 5. In addition, various additives such as heat stabilizers, light stabilizers, ultraviolet absorbers, antiblocking agents, catalyst scavengers, colorants, light scattering agents, and gloss adjusters may be added to the transparent resin layer 5. As the heat stabilizers, phenol-based, sulfur-based, phosphorus-based, hydrazine-based, and other additives are generally added in any combination. As the light stabilizers, hindered amine-based, and other additives are generally added in any combination. For the transparent resin layer 5, it is preferable to adopt a transparent or semi-transparent material that allows the design of the design layer 3 to be seen through the adhesive layer 4.

[0041] A melt extrusion molding method can be adopted as a method for forming the transparent resin layer 5. The transparent resin layer 5 may be formed by a known printing method such as gravure printing, offset printing, flexographic printing, silk screen printing, or inkjet printing, or by using a known coating device. The transparent resin layer 5 may be formed by laminating a sheet made of crystalline polypropylene or the like by a known lamination method such as dry lamination, wet lamination, non-solvent lamination, wax lamination, or thermal lamination.

[0042] The transparent resin layer 5 may have an embossed shape (pattern) on the surface on the upper side UP. When the transparent resin layer 5 has an embossed shape, the unevenness of the embossed shape can give the decorative sheet 10 a visual three-dimensional effect and a three-dimensional effect by touch. For example, when the transparent resin layer 5 has an embossed shape that is in harmony with the picture layer 3, the picture of the picture layer 3 in the decorative sheet 10 can be given a three-dimensional effect.

[0043] The surface protective layer 6 is a layer provided on the upper side UP of the transparent resin layer 5. The surface protective layer 6 has an uneven shape on the surface of the upper side UP of the surface protective layer 6, in which ridge-like raised portions are formed. FIG. 2 is a photograph showing an example of the uneven shape of the surface protective layer 6 when viewed from the upper side UP.

[0044] 3 is a cross-sectional view showing a schematic diagram of the surface protective layer 6. The surface protective layer 6 has a core portion 6a and a ridge portion 6b that protrudes in a ridge shape from the surface of the upper side UP of the core portion 6a. As a result, an uneven shape is formed on the surface of the upper side UP of the surface protective layer 6.

[0045] The ridge portion 6b is formed by irradiating the upper surface UP of the surface protection layer 6 with light of a specific wavelength described below, thereby shrinking the surface of the resin (e.g., ionizing radiation curable resin) that forms the surface protection layer 6.

[0046] Here, "ridge-like" refers to a shape that rises in a long, thin manner upward and is connected linearly when viewed from the upper side UP. The ridge-like raised ridge portions 6b may have a curved or linear shape when viewed from the upper side UP, but a curved shape is preferable from the viewpoint of the fingerprint resistance of the decorative sheet 10. The linear shapes of the ridge portions 6b may or may not be branched when viewed from the upper side UP.

[0047] The ridge portion 6b is a portion of the uneven shape provided on the surface of the upper side UP of the surface protection layer 6, ranging from the lowest point to the highest point in the up-down direction V. The core portion 6a is the portion of the surface protection layer 6 other than the ridge portion 6b.

[0048] The ridge portions 6b are curved and at least some of them are adjacent to each other in the width direction, as shown in Fig. 2. At a position where at least some of the ridge portions 6b are adjacent to each other in the width direction, the cross section of the surface protective layer 6 parallel to the width direction and the thickness direction (vertical direction V) of the surface protective layer 6 has a wave shape such as a sine wave shape in the portion where the uneven shape is provided, as shown in Fig. 3.

[0049] The uneven shape of the surface protective layer 6 has a ratio Rdc / t (hereinafter simply referred to as "ratio Rdc / t") of 0.1 to 0.2 of the cut level difference Rdc to the thickness t of the surface protective layer 6. The ratio Rdc / t is preferably 0.11 to 0.19.

[0050] "Cut level difference Rdc" is a surface quality parameter defined in JIS B 0601. The cut level difference Rdc indicates the cut level difference of the load curve, and expresses the steepness of the uneven shape. The ratio Rdc / t of the cut level difference Rdc to the thickness t of the surface protective layer 6 indicates the steepness of the uneven shape per unit thickness of the surface protective layer 6.

[0051] When the ratio Rdc / t is 0.1 or more and 0.2 or less, the slope of the uneven shape is relatively gentle. In this case, when the surface of the decorative sheet (the upper UP surface) is pressed with a finger and the finger is slid over the surface, the pressing resistance due to contact between the finger and the surface of the decorative sheet is small, and the contact area between the finger and the convex surface of the uneven shape gradually increases, resulting in a tactile sensation as if the surface of the decorative sheet is sticking to the finger. This tactile sensation can be associated with a "moist tactile sensation."

[0052] On the other hand, when the ratio Rdc / t is greater than 0.2, the slope of the uneven shape becomes steep. In this case, when a finger is pressed against the surface of the decorative sheet and then slid across the surface, the resistance to pressure caused by contact between the finger and the surface of the decorative sheet is large, and the presence of the unevenness is felt. This tactile sensation can be associated with a "rough tactile sensation."

[0053] Furthermore, when the ratio Rdc / t is smaller than 0.1, the slope of the uneven shape is very gentle. In this case, when the surface of the decorative sheet is pressed with a finger and slid over the surface, the pressing resistance due to contact between the finger and the surface of the decorative sheet is small, and the contact area between the finger and the convex surface of the uneven shape is large from the start of the pressing action, and the increase in this contact area accompanying the pressing action is very gentle. In this case, the surface of the decorative sheet feels as if it is sticking to the finger, while the slope of the uneven shape is very gentle, resulting in a smooth feel compared to the above-mentioned "moist feel", and overall the impression of a smooth feel is stronger. This feel can be associated with a "smooth feel".

[0054] The thickness t of the surface protective layer 6 is 2 μm or more and 18 μm or less. The thickness t of the surface protective layer 6 is preferably 3 μm or more and 10 μm or less. When the thickness of the surface protective layer 6 is increased, the value of the ratio Rdc / t tends to increase. For this reason, if the thickness of the surface protective layer 6 is too small or too large, it becomes difficult to achieve a "moist touch."

[0055] Furthermore, if the thickness of the surface protective layer 6 is reduced, it becomes difficult to achieve a low glossiness. Here, the thickness of the surface protective layer 6 is determined by observing the cross section with a scanning electron microscope and averaging 25 points. Specifically, the thickness of the surface protective layer 6 can be determined as described in the examples below. Note that, when the resin (coating liquid for surface protective layer) forming the surface protective layer 6 does not contain a solvent, the thickness of the coating film made of the coating liquid for surface protective layer is equal to the thickness of the surface protective layer 6.

[0056] The 60-degree reflected gloss of the surface protective layer 6 is less than 10. The 60-degree reflected gloss of the surface protective layer 6 is preferably 5 or less. Here, the reflected gloss in this embodiment refers to the specular gloss defined in JIS Z 8741. The 60-degree reflected gloss refers to the 60-degree specular gloss in the above-mentioned JIS standard, and refers to the gloss of reflected light of light with an incident angle α of 60 degrees in the case of light with an incident angle α shown in FIG. 3. By making the 60-degree reflected gloss less than 10, the decorative sheet 10 can have an excellent low-gloss design. The gloss of reflected light can be measured by a measuring instrument such as a surface gloss meter.

[0057] Ionizing radiation curable resins such as (meth)acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, and epoxy resins can be used as the surface protective layer 6. It is preferable to use a transparent or semi-transparent material for the surface protective layer 6 so that the pattern of the pattern layer 3 can be seen through the adhesive layer 4 and the transparent resin layer 5.

[0058] Here, "ionizing radiation" refers to a charged particle beam such as an electron beam. Ionizing radiation curable resins are cured by irradiation with ionizing radiation. Ionizing radiation curable resins can also be cured by ultraviolet light irradiation. The ionizing radiation curable resins used here are cured by irradiation with light having a wavelength of 200 nm or less, and have a large absorption coefficient for this light.

[0059] The amount of the cured ionizing radiation curable resin in the surface protective layer 6 is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. As the ionizing radiation curable resin, known resins such as various monomers and commercially available oligomers can be used. The ionizing radiation curable resin forming the surface protective layer 6 may be either an aqueous resin or a non-aqueous (organic solvent-based) resin.

[0060] The main component of the ionizing radiation curable resin is preferably an acrylate. Here, the main component of the ionizing radiation curable resin means a component that accounts for 60 mass% or more of the ionizing radiation curable resin. The ionizing radiation curable resin preferably contains 70 mass parts or more of acrylate, more preferably 80 mass parts or more. The ionizing radiation curable resin in the surface protective layer 6 is more preferably an acrylate.

[0061] The acrylate contained in the surface protective layer 6 is preferably a bifunctional or higher acrylate, and more preferably a trifunctional or higher acrylate. In order to obtain a surface protective layer 6 having excellent scratch resistance, the acrylate is preferably a trifunctional or higher acrylate. There is no upper limit to the number of functional groups of the acrylate, but according to one example, it is 6-functional or lower.

[0062] The acrylate contained in the surface protective layer 6 preferably contains a repeating structure. This repeating structure is, for example, any one of an ethylene oxide (EO) structure, a propylene oxide (PO) structure, and an ε-caprolactone (CL) structure. The repeating structure is preferably ethylene oxide or propylene oxide. In the acrylate, the repeating structure may be present between the acryloyl group and the methylol group in a ring-opened state.

[0063] The number of repetitions of the repeating structure in the acrylate contained in the surface protective layer 6 is preferably 3 or more. If an acrylate with a large number of repetitions is used, the cured film is more likely to expand in the in-plane direction in the light irradiation step described below, and wrinkles corresponding to the ridge-like portions 6b are more likely to appear on the coating film surface. In addition, if an acrylate with a large number of repetitions is used, the ratio Rdc / t tends to be larger. However, if the number of repetitions is increased, the crosslink density decreases, and the scratch resistance of the surface protective layer decreases.

[0064] The ionizing radiation curable resin forming the surface protective layer 6 is preferably a trifunctional acrylate containing a repeating unit. The trifunctional acrylate containing a repeating unit is, for example, EO-modified, PO-modified or CL-modified trimethylolpropane triacrylate, glycerin triacrylate, isocyanurate triacrylate or pentaerythritol triacrylate. In the trifunctional acrylate containing a repeating unit, the number of repeats of the repeating unit is preferably 3 or more, more preferably 3 to 30, and even more preferably 3 to 20.

[0065] Moreover, the ionizing radiation curable resin forming the surface protective layer 6 is preferably a tetrafunctional acrylate containing a repeating unit. The tetrafunctional acrylate containing a repeating unit is, for example, EO-modified, PO-modified or CL-modified pentaerythritol tetraacrylate. In the tetrafunctional acrylate containing a repeating unit, the number of repeats of the repeating unit is preferably 12 or more, more preferably 12 to 50, even more preferably 20 to 50, and even more preferably 20 to 35.

[0066] The number of repetitions of the repeating structure can be analyzed by using MALDI-TOF-MS (matrix-assisted laser desorption / ionization time-of-flight mass spectrometry). Ionizing radiation curable resins may have a molecular weight distribution. When there is a molecular weight distribution, the number of repetitions is the number of repetitions corresponding to the molecular weight having the strongest peak in the MALDI-TOF-MS mass spectrum.

[0067] The surface protective layer 6 contains particles having an average particle size of 3 μm or more. Examples of the particles contained in the surface protective layer 6 include particles made of an organic material such as polyethylene (PE) wax, polypropylene (PP) wax, and resin beads, and particles made of an inorganic material such as silica, glass, alumina, titania, zirconia, calcium carbonate, and barium sulfate.

[0068] The average particle size (D50) of the particles contained in the surface protective layer 6 is preferably 3 μm or more and 11 μm or less, and more preferably 4 μm or more and 10 μm or less.

[0069] By including particles in the surface protective layer 6, wrinkles can be more uniformly generated on the coating surface in the light irradiation step described below. As the average particle size (D50) of the particles increases, the ratio Rdc / t tends to decrease. For this reason, if the average particle size (D50) is too small or too large, it becomes difficult to achieve a "moist tactile feel." In addition, when particles with a large particle size are used, the particles are likely to fall off from the surface protective layer 6, making it difficult to achieve high scratch resistance. If the particle size is small, the effect of generating wrinkles uniformly is small.

[0070] Here, the "average particle size (D50)" is the median size (D50) measured by a laser diffraction / scattering type particle size distribution analyzer. When the coating liquid for the surface protective layer contains particles, the surface protective layer 6 obtained from this coating liquid also contains particles. The average particle size of the particles contained in the surface protective layer 6 can be determined by observing the cross section of the layer and averaging the particle sizes of a plurality of particles. The value obtained in this manner is substantially the same as the median size (D50) measured by a laser diffraction / scattering type particle size distribution analyzer.

[0071] The amount of particles added to the surface protective layer 6 is preferably 3 parts by mass or more and 11 parts by mass or less relative to 100 parts by mass of the resin forming the surface protective layer 6. The amount of particles added is more preferably 4 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the resin forming the surface protective layer 6. Note that "100 parts by mass of resin" refers to the parts by mass of the solid content of the resin.

[0072] When the amount of particles added is within the above range, the effect of generating wrinkles uniformly is particularly large. When the amount of particles added is large, the value of the ratio Rdc / t tends to decrease. Therefore, when the amount of particles added is too small or too large, it becomes difficult to achieve a "moist touch." In addition, when the amount of particles added is large, the particles are likely to fall off from the surface protective layer 6, and it may be difficult to achieve high scratch resistance. When the amount of particles added is small, the effect of generating wrinkles uniformly is small.

[0073] A known printing method such as gravure printing, offset printing, flexographic printing, silk screen printing, or inkjet printing can be used as a method for forming the surface protective layer 6. The surface protective layer 6 may also be formed using a known coating device.

[0074] The decorative sheet 10 may include a substrate on the lower side LO of the decorative sheet 10. By providing a substrate on the lower side LO of the decorative sheet 10, a decorative material (decorative board) can be obtained.

[0075] The substrate to be laminated on the lower side LO of the decorative sheet 10 may be a wood substrate such as particle board or medium density fiberboard (MDF), a metal plate-shaped component such as aluminum or stainless steel, or a composite board in which a metal such as aluminum is attached to both sides of a core material made of a resin such as polyethylene.

[0076] Next, an example of a method for producing the decorative sheet 10 will be described. 4 is a flow chart showing an example of a manufacturing method for manufacturing the decorative sheet 10 by a decorative sheet manufacturing system. Here, the decorative sheet manufacturing system is a system that carries out the manufacture of the decorative sheet 10 according to this embodiment.

[0077] First, the decorative sheet manufacturing system performs step S1 (pattern printing step). In step S1, an arbitrary pattern is printed on the surface of the upper side UP of the raw fabric layer 2 to form a pattern layer 3. At this time, the pattern layer 3 may be printed after a surface treatment such as a corona treatment is performed on the surface of the upper side UP of the raw fabric layer 2. In addition, a primer layer 1 is printed and formed on the surface of the lower side LO of the raw fabric layer 2.

[0078] Next, the decorative sheet manufacturing system performs step S2 (melt extrusion step). In step S2, the resin forming the adhesive layer 4 and the resin forming the transparent resin layer 5 are co-extruded using a melt extruder to form the adhesive layer 4 and the transparent resin layer 5.

[0079] Next, the decorative sheet manufacturing system performs step S3 (extrusion lamination process). In step S3, an adhesive for dry lamination is applied to the upper UP surface of the pattern layer 3 formed in step S1. Next, the surface of the pattern layer 3 to which the adhesive for dry lamination is applied is bonded to the transparent resin layer 5 formed in step S2 by extrusion lamination via the adhesive layer 4 formed in step S2. Here, an embossed pattern (shape) may be applied to the upper UP surface of the bonded transparent resin layer 5 by pressing with a mold roll or the like. By applying an embossed pattern to give the transparent resin layer 5 an uneven shape, the decorative sheet 10 can obtain a three-dimensional effect. In addition, as the embossed pattern applied to the transparent resin layer 5, a pattern in harmony with the pattern of the pattern layer 3 may be embossed.

[0080] Next, the decorative sheet manufacturing system performs step S4 (protective layer coating step). In step S4, a resin (surface protective layer coating liquid) that forms the surface protective layer 6 is coated on the upper side UP of the transparent resin layer 5. Here, the surface protective layer coating liquid is an ionizing radiation curable resin.

[0081] Next, the decorative sheet manufacturing system performs step S5 (light irradiation step). In step S5, the upper surface UP of the coating liquid for the surface protective layer applied in step S4 is irradiated with excimer VUV light having a wavelength of 172 nm. By irradiating with excimer VUV light having a wavelength of 200 nm or less, the surface of the ionizing radiation curable resin shrinks, and ridge portions 6b in the surface protective layer 6 are formed.

[0082] Here, the ionizing radiation curable resin contained in the coating liquid for surface protective layer has a large absorption coefficient for excimer VUV light. Therefore, the excimer VUV light incident on the coating film of the coating liquid for surface protective layer can only reach a position that is several tens to several hundreds of nm away from the outermost surface. Therefore, in step S5, the crosslinking reaction proceeds in the surface region of the coating film of the coating liquid for surface protective layer, forming an extremely thin cured film. Meanwhile, in other regions, the crosslinking reaction does not proceed and the coating liquid for surface protective layer remains uncured.

[0083] Next, the decorative sheet manufacturing system performs step S6 (protective layer curing step). In step S6, ionizing radiation is irradiated onto the surface of the coating liquid for surface protective layer on which the ridges 6b have been formed in step S5. By irradiating the ionizing radiation curable resin in which the ridges 6b have been formed by the excimer VUV light with ionizing radiation, the entire ionizing radiation curable resin is cured, and a surface protective layer 6 having an uneven shape with cores 6a and ridges 6b is formed is formed. With the surface protective layer 6 formed, the manufacturing process for the decorative sheet 10 is completed.

[0084] When manufacturing a decorative material having a substrate on the lower LO of the decorative sheet 10, a manufacturing method for the decorative material can include a substrate bonding process for bonding the substrate to the lower LO of the decorative sheet 10 after step S6, thereby manufacturing a decorative material using the decorative sheet 10.

[0085] According to the decorative sheet 10 and decorative material and the manufacturing method of the decorative sheet 10 and decorative material of this embodiment, the surface protective layer 6 has an uneven shape with ridge-like raised portions 6b formed therein and a 60-degree reflected gloss of less than 10, a thickness t of 2 μm or more and 18 μm or less, and a ratio of the cut level difference Rdc to the thickness t of 0.1 or more and 0.2 or less. The surface protective layer 6 also contains particles having an average particle size of 3 μm or more.

[0086] Therefore, when a user slides his / her finger over the surface of the surface protective layer 6 while pressing the surface with the skin, the decorative sheet 10 gives the user a moist feel and has an excellent touch. Furthermore, the decorative sheet 10 is excellent in design and durability because it can realize a low gloss design without containing a matting agent. Furthermore, it is possible to provide a concave-convex shape in the surface protective layer 6 without embossing with an embossing plate, so an embossing plate for embossing is not required.

[0087] As a result, it is possible to provide a decorative sheet 10 and a decorative material having excellent design and feel, as well as a method for manufacturing the decorative sheet 10 and the decorative material.

[0088] Although one embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and design modifications and the like within the scope of the present invention are also included. In addition, the components shown in the above-mentioned embodiment and the modified examples shown below can be appropriately combined to form a configuration.

[0089] (Variation 1) In the above embodiment, the decorative sheet 10 includes a transparent resin layer 5, but the aspect of the decorative sheet 10 is not limited to this. The decorative sheet does not have to include a transparent resin layer 5. The decorative sheet 10 includes a transparent resin layer 5, and an embossed pattern is applied to the transparent resin layer 5, thereby imparting a visual three-dimensional effect to the decorative sheet 10. If there is no need to impart a visual three-dimensional effect to the decorative sheet by an embossed pattern, the decorative sheet does not have to include a transparent resin layer 5. Furthermore, even if the decorative sheet includes a transparent resin layer 5, the transparent resin layer 5 does not have to be embossed with a pattern.

[0090] (Variation 2) In the above embodiment, the decorative sheet 10 includes an adhesive layer 4 and a primer layer 1, but the aspect of the decorative sheet 10 is not limited to this. The decorative sheet does not have to include the adhesive layer 4 or the primer layer 1. The adhesive layer 4 and the primer layer 1 can improve the adhesion between the layers laminated with the adhesive layer 4 or the primer layer 1 in between. If each layer of the decorative sheet can have sufficient adhesion without improving the adhesion with the adhesive layer 4 or the primer layer 1, the decorative sheet does not have to include the adhesive layer 4 or the primer layer 1.

[0091] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples.

[0092] Example 1 (Pattern printing process S1) As the base layer 2, an olefin film (manufactured by RIKEN TECHNOS CORPORATION) having a thickness of 55 μm was prepared, and the surface of the upper side UP of the base layer 2 was subjected to a corona treatment. A pattern was printed on the surface of the upper side UP of the base layer 2 that had been subjected to the corona treatment to form a pattern layer 3. For the pattern layer 3, a two-component urethane ink (V180 manufactured by Toyo Ink Co., Ltd.) was used, to which 0.5 parts by mass of a hindered amine-based light stabilizer (Chimasorb 944 manufactured by BASF) was added relative to the binder resin content of the ink. In addition, a two-component urethane ink similar to the ink used for the pattern layer 3 was printed on the surface of the lower side LO of the base layer 2 to form a primer layer 1.

[0093] (Melt extrusion process S2) A mixture of 100 parts by mass of crystalline polypropylene resin (pentad fraction 97.8%, molecular weight distribution 2.3, MFR 18g / 10min) as the resin for forming the transparent resin layer 5, 0.5 parts by mass of a hindered amine light stabilizer (BASF's Chimassorb 944) and 0.5 parts by mass of a benzotriazole UV absorber (BASF's Tinuvin 328) was co-extruded with the resin for forming the adhesive layer 4 using a melt extruder to produce a 60 μm thick transparent resin layer 5 and a 10 μm thick adhesive layer 4.

[0094] (Extrusion lamination process S3) A dry lamination adhesive (Takelac A540 manufactured by Mitsui Chemicals, Inc.) was applied in an amount of 2 g / m to the upper surface UP of the pattern layer 3 formed in the pattern printing process S1. 2 The upper UP surface of the design layer 3 coated with the adhesive for dry lamination and the lower LO surface of the transparent resin layer 5 formed in the melt extrusion step S2 were bonded together by extrusion lamination via the adhesive layer 4 formed in the melt extrusion step S2. Furthermore, the upper UP surface of the transparent resin layer 5 bonded to the design layer 3 was pressed using an embossing die roll to form a pear-shaped embossed pattern.

[0095] (Protective layer coating process S4) A coating liquid for forming a surface protective layer 6 was applied to the upper surface UP of the transparent resin layer 5 on which the embossed pattern had been formed in the extrusion lamination step S3 to a layer thickness of 6 μm.

[0096] As the coating liquid for the surface protective layer, a coating liquid containing the following ionizing radiation curable resin, the following particles, and a photopolymerization initiator was used. ·Ionizing radiation curable resin Type: Trimethylolpropane EO modified triacrylate (EO 15 moles added) Product name: SR9035 (Sartomer) Blend: 100 parts by mass ·particle Product name: Silica 250N (manufactured by Fuji Silysia Chemical) Particle size: 6μm Blend: 5 parts by mass Photopolymerization initiator Product name: Omnirad184 (IGM Resins) Blend: 3 parts by mass

[0097] (Light irradiation process S5) The upper surface UP of the coating liquid for the surface protective layer applied in the protective layer coating process S4 was irradiated with excimer VUV light using a Xe excimer lamp to shrink the surface of the coating liquid for the surface protective layer. At this time, the ultraviolet light with a wavelength of 172 nm was irradiated at an integrated light intensity of 30 mJ / cm in a nitrogen gas atmosphere with an oxygen concentration of 100 ppm under atmospheric pressure. 2 The irradiation was performed so that

[0098] (Protective layer curing step S6) In the light irradiation process S5, the coating liquid for the surface protective layer shrunk by the excimer VUV light was irradiated with 200 mJ / cm using a high-pressure mercury lamp. 2 The coating liquid for surface protective layer was entirely cured to form a surface protective layer 6. In this way, a decorative sheet 10 of Example 1 having a total thickness of 131 μm was obtained.

[0099] Example 2 A decorative sheet 10 of Example 2 was obtained in the same manner as in Example 1, except that the thickness of the coating liquid for the surface protective layer was set to a layer thickness of 8 μm.

[0100] Comparative Example 1 A decorative sheet of Comparative Example 1 was obtained by forming a surface protective layer using a resin obtained by blending the following particles with the following ionizing radiation curable resin, and by using the same method as in Example 1, except that the light irradiation step S5 was not performed. In addition, a matting agent was added to the ionizing radiation curable resin forming the surface protective layer so that the 60-degree reflective gloss on the upper surface of the surface protective layer was 4.5. ·Ionizing radiation curable resin Type: Trimethylolpropane triacrylate Product name: NK Ester A-TMPT (manufactured by Shin-Nakamura Chemical Co., Ltd.) Blend: 100 parts by mass ·particle Product name: Silica 250N (manufactured by Fuji Silysia Chemical)

[0101] Comparative Example 2 The decorative sheet of Comparative Example 2 was obtained in the same manner as Comparative Example 1, except that the embossed pattern applied to the upper side of the transparent resin layer in the extrusion lamination process S3 was a sand-grained pattern, and a matting agent was added to the ionizing radiation curable resin so that the 60-degree reflective gloss on the upper surface of the surface protection layer was 4.6.

[0102] Comparative Example 3 No embossing was applied to the upper surface of the transparent resin layer, and the coating amount of the surface protection layer was 5 g / m 2 A decorative sheet of Comparative Example 3 was obtained in the same manner as in Comparative Example 1, except that a matting agent was added to the ionizing radiation curable resin so that the 60 degree reflective gloss on the upper surface of the surface protective layer was 5.3.

[0103] Comparative Example 4 The surface protection layer is applied at a rate of 5 g / m 2 A decorative sheet of Comparative Example 4 was obtained in the same manner as in Comparative Example 1, except that a matting agent was added to the ionizing radiation curable resin so that the 60 degree reflective gloss on the upper surface of the surface protective layer was 4.3.

[0104] Comparative Example 5 The surface protection layer is applied at a rate of 5 g / m 2 A decorative sheet of Comparative Example 5 was obtained in the same manner as in Comparative Example 1, except that no matting agent was added to the surface protective layer.

[0105] Comparative Example 6 Paper base material with a basis weight of 23g / m 2 A mixed paper (TP23 manufactured by Tenma Tokushu Seishi Co., Ltd.) with a thickness of 33 μm was prepared, and a pattern was printed on the surface (upper surface) of the paper using nitrocellulose ink (PCNT ink manufactured by Toyo Ink Mfg. Co., Ltd.) and urethane ink (PCRNT ink manufactured by Toyo Ink Mfg. Co., Ltd.) to form a pattern layer. As a surface protection layer, a transparent coating liquid made of a base agent mainly composed of acrylic polyol to which an isocyanate hardener was added was applied at a dry weight of 5 g / m2 on the upper surface of the pattern layer. 2 A decorative sheet of Comparative Example 6 was obtained. A matting agent was added to the surface protective layer so that the 60 degree reflected gloss on the upper surface of the surface protective layer was 5.3.

[0106] Comparative Example 7 No embossing was applied to the upper surface of the transparent resin layer, and the coating amount of the surface protection layer was 5 g / m 2 A decorative sheet of Comparative Example 7 was obtained in the same manner as in Comparative Example 1, except that no matting agent was added to the surface protective layer.

[0107] Comparative Example 8 A decorative sheet of Comparative Example 8 was obtained in the same manner as in Comparative Example 6, except that no matting agent was added to the coating liquid for forming the surface protective layer.

[0108] Comparative Example 9 A matting agent was added to the coating liquid forming the surface protective layer so that the 60-degree reflective gloss on the upper surface of the surface protective layer was 3.2, and the coating amount of the coating liquid forming the surface protective layer was set to 10 g / m2 in terms of dry weight. 2 A decorative sheet of Comparative Example 9 was obtained in the same manner as in Comparative Example 6, except that:

[0109] Comparative Example 10 A matting agent was added to the coating liquid forming the surface protective layer so that the 60-degree reflective gloss on the upper surface of the surface protective layer was 13.2, and the coating amount of the coating liquid forming the surface protective layer was set to 10 g / m2 in terms of dry weight. 2A decorative sheet of Comparative Example 10 was obtained in the same manner as in Comparative Example 6, except that:

[0110] Comparative Example 11 No embossing was applied to the upper surface of the transparent resin layer, and the coating amount of the surface protection layer was set to 10 g / m 2 The decorative sheet of Comparative Example 11 was obtained in the same manner as Comparative Example 1, except that a matting agent was added to the coating liquid for forming the surface protective layer so that the 60-degree reflected gloss on the upper surface of the surface protective layer was 5.7.

[0111] Comparative Example 12 In the extrusion lamination process S3, the embossed pattern on the top of the transparent resin layer is rough and sand-like, and the coating amount of the surface protective layer is 10 g / m 2 A decorative sheet of Comparative Example 12 was obtained in the same manner as in Comparative Example 1, except that a matting agent was added to the ionizing radiation curable resin so that the 60-degree reflective gloss on the upper surface of the surface protective layer was 4.1.

[0112] Comparative Example 13 In the extrusion lamination process S3, the embossed pattern on the top of the transparent resin layer is rough and sand-like, and the coating amount of the surface protective layer is 10 g / m 2 A decorative sheet of Comparative Example 13 was obtained in the same manner as in Comparative Example 1, except that no matting agent was added to the surface protective layer.

[0113] Comparative Example 14 The decorative sheet of Comparative Example 14 was obtained in the same manner as Comparative Example 1, except that the embossing pattern applied to the upper side of the transparent resin layer in the extrusion lamination process S3 was the same sand-grained shape as in Comparative Example 2, and a matting agent was added to the coating liquid forming the surface protective layer so that the 60-degree reflected gloss on the upper surface of the surface protective layer was 2.2.

[0114] Comparative Example 15 In the extrusion lamination process S3, the embossed pattern on the top of the transparent resin layer is rough and sand-like, and the coating amount of the surface protective layer is 3 g / m 2The decorative sheet of Comparative Example 15 was obtained in the same manner as in Comparative Example 1, except that a matting agent was added to the coating liquid for forming the surface protective layer so that the 60-degree reflected gloss on the upper surface of the surface protective layer was 7.9.

[0115] Comparative Example 16 In the extrusion lamination process S3, the embossed pattern on the top of the transparent resin layer is rough and sand-like, and the coating amount of the surface protective layer is 5 g / m 2 A decorative sheet of Comparative Example 16 was obtained in the same manner as in Comparative Example 1, except that no matting agent was added to the surface protective layer.

[0116] (Comparative Example 17) In the extrusion lamination process S3, the embossed pattern on the top of the transparent resin layer is rough and sand-like, and the coating amount of the surface protective layer is 10 g / m 2 A decorative sheet of Comparative Example 17 was obtained in the same manner as in Comparative Example 1, except that no matting agent was added to the surface protective layer.

[0117] (Comparative Example 18) In the extrusion lamination process S3, the embossed pattern on the top of the transparent resin layer is rough and sand-like, and the coating amount of the surface protective layer is 5 g / m 2 The decorative sheet of Comparative Example 18 was obtained in the same manner as in Comparative Example 1, except that a matting agent was added to the coating liquid for forming the surface protective layer so that the 60-degree reflected gloss on the upper surface of the surface protective layer was 4.5.

[0118] Comparative Example 19 In the extrusion lamination process S3, the embossed pattern on the top of the transparent resin layer is rough and sand-like, and the coating amount of the surface protective layer is 5 g / m 2 A decorative sheet of Comparative Example 19 was obtained in the same manner as in Comparative Example 1, except that no matting agent was added to the surface protective layer.

[0119] Comparative Example 20 A decorative sheet of Comparative Example 20 was obtained in the same manner as in Example 1, except that the thickness of the coating liquid for surface protection layer was set to 20 μm.

[0120] Comparative Example 21 A decorative sheet of Comparative Example 21 was obtained in the same manner as in Example 1, except that the thickness of the coating liquid for surface protection layer was set to a layer thickness of 0.7 μm.

[0121] Comparative Example 22 A decorative sheet of Comparative Example 22 was obtained in the same manner as in Example 1, except that the thickness of the coating liquid for surface protection layer was set to 1 μm.

[0122] (Experiment 1) For the decorative sheets of Example 1 and Comparative Example 1, the following were measured: "reflective gloss (20 degrees, 60 degrees, 85 degrees)," "cut level difference Rdc," "ratio Rdc / t of cut level difference Rdc to thickness t of surface protective layer," "arithmetic mean roughness Ra," and "maximum height Rz." Here, the 20-degree reflected gloss and the 85-degree reflected gloss are specular gloss values ​​defined in JIS Z 8741, similar to the 60-degree reflected gloss, and indicate the gloss of reflected light when the incident angle α shown in FIG. 3 is 20 degrees or 85 degrees, respectively.

[0123] The arithmetic mean roughness Ra and maximum height Rz are surface quality parameters conforming to JIS B 0601, and are surface quality parameters indicating the surface roughness in the thickness direction of the uneven surface shape of the surface protective layer.

[0124] The reflected gloss (at 20 degrees, 60 degrees, and 85 degrees) was measured using a gloss meter (Rhopoint IQ, manufactured by Konica Minolta).

[0125] The thickness t of the surface protective layer was measured by the following method. First, the decorative sheet was embedded in a resin such as a cold-curing epoxy resin or a UV-curing resin and fully cured, and then cut so that the cross section of the decorative sheet appeared, and mechanically polished to obtain a measurement surface. Next, the thickness of the surface protective layer was measured using a scanning electron microscope SIGMA500 manufactured by Carl Zeiss Microscopy. The thickness was measured at any 25 points, and the average measurement value of the 25 points was defined as the "thickness t of the surface protective layer". The measurement conditions were an acceleration voltage of 0.5 keV (low acceleration voltage), an imaging mode of SE2 mode, and a magnification of 2000 times.

[0126] (Experiment 2) For the decorative sheets of Example 1 and Comparative Example 1, a "pencil hardness test," a "steel wool rubbing test," a "Hoffman scratch test," and a "stain resistance test" were carried out.

[0127] The pencil hardness test was conducted in accordance with JIS K 5600-5-4 (scratch hardness (pencil method)) with a load of 750g from pencil hardness B to 6B, and the hardness was confirmed to be sufficient to cause no scratches or changes in gloss.

[0128] In the steel wool rubbing test, a wooden substrate was attached to the underside of the decorative sheet, and then a load of 500 g was applied to the steel wool, which was rubbed back and forth across the surface of the decorative sheet 20 times, and the surface of the decorative sheet was visually inspected for scratches and changes in gloss. The evaluation criteria were on a five-point scale. 5: Good condition with no change in gloss. 4: Slight scratches, but almost no change in gloss. 3: Items with significant scratches or changes in gloss in some areas. 2: Significant scratches or changes in gloss all over the surface. 1: The surface protective layer is completely peeled off.

[0129] In the Hoffman scratch test, a cylindrical blade was placed on the surface of the decorative sheet at a 45° angle, and a load was applied to the blade from 200g to 2000g in 200g increments while moving the blade across the surface of the decorative sheet at a constant speed. The upper limit of the load at which the surface of the decorative sheet was not scratched was confirmed.

[0130] In the stain resistance test, 1% NaOH, 5% sulfuric acid, ethanol, and lacquer thinner were dropped onto the surface of the decorative sheet and covered with a watch glass. After 24 hours, the surface of the decorative sheet was washed with water and the appearance of the decorative sheet was then checked. The evaluation criteria were three-level. ○: No change in appearance. △: Gloss changed. ×: bleached.

[0131] (Experiment 3) The decorative sheets of Examples 1-2 and Comparative Examples 1-22 were subjected to a tactile evaluation test. In the tactile evaluation test, first, advance preparation was carried out to ensure that the evaluation criteria were consistent between evaluators. In advance preparation, three standard test pieces with different surface properties were prepared. Next, five blindfolded evaluators pressed and slid their fingers over the surface of the standard test pieces, and classified the tactile sensation into the following three groups. Group 1: Almost no resistance was felt when pushing, but the surface of the decorative sheet felt as if it was sticking to the fingers, and it also felt smooth to the touch. Overall, the impression of a smooth texture was strong. In other words, a "smooth texture" was obtained. Group 2: Almost no resistance was felt when pushing, but the surface of the decorative sheet felt as if it was sticking to the fingers. However, there was no impression of a smooth feel. In other words, a "moist feel" was felt. Group 3: They felt resistance to pressure and also felt the presence of unevenness. In other words, they felt a "rough texture."

[0132] Next, five blindfolded evaluators pressed and slid their fingers over the surfaces of the decorative sheets of Examples 1-2 and Comparative Examples 1-22 to evaluate the feel of the decorative sheets of Examples 2 and Comparative Examples 1-22 relative to the feel of the decorative sheet 10 of Example 1. The evaluation criteria were three-level. ◯: The feel is similar to that of Example 1. △: The texture is different from that of Example 1, but the smoothness is similar. ×: The touch is clearly different from that of Example 1.

[0133] (Experimental Results) The results of Experiment 1 are shown in Table 1. The 60-degree reflected gloss and ratio Rdc / t were comparable for the decorative sheet 10 of Example 1, in which an uneven shape was realized by the ridge shapes (ridge portions 6b) formed on the surface protective layer 6, and the decorative sheet of Comparative Example 1, which did not have ridge shapes.

[0134] The results of Experiment 2 are shown in Table 2. The decorative sheet 10 of Example 1, in which the uneven shape was realized by the ridge shapes formed in the surface protective layer 6, was found to have the same or greater durability (scratch resistance and stain resistance) as the decorative sheet of Comparative Example 1, which did not have the ridge shapes.

[0135] The results of Experiment 3 are shown in Tables 3 and 4. Here, Tables 3 and 4 also show the reflective gloss (20 degrees, 60 degrees, and 85 degrees) and the ratio Rdc / t measured in the same manner as in Experiment 1. Note that, regarding the tactile evaluation results in Tables 3 and 4, the evaluation results of the tactile feel of Example 2 and Comparative Examples 1-22 relative to Example 1 are shown, and therefore the results for Example 1 are not shown.

[0136] In addition, Tables 3 and 4 show the "coat application amount (g / m 2 )" is the coating amount of the coating liquid for surface protective layer. In Tables 3 and 4, the coating amount is shown only in the examples and comparative examples having a surface protective layer formed by irradiating the coating liquid for surface protective layer with excimer VUV light. In addition, since the coating amount shown in Tables 3 and 4 is the dry weight of the coating liquid for surface protective layer, the coating amount of the coating liquid for surface protective layer and the thickness of the surface protective layer are numerically the same.

[0137] First, in the touch evaluation test, the touch of Example 1, which was classified using a standard test piece, was "Group 2: moist touch". As shown in Tables 3 and 4, similar to Example 1, the decorative sheet 10 of Example 2, in which the uneven shape is realized by the ridge shape formed on the surface protective layer 6, the thickness (coat application amount) of the surface protective layer 6 is 2 μm or more and 18 μm or less, and the ratio Rdc / t is 0.1 or more and 0.2 or less, had a touch similar to that of Example 1. In addition, compared to the decorative sheet 10 of Example 1, the decorative sheets of Comparative Example 1 and Comparative Example 6-9, which do not have a ridge shape and have a ratio Rdc / t of 0.1 or more and 0.2 or less, had a touch similar to that of Example 1. That is, Examples 1-2, Comparative Example 1, and Comparative Example 6-9 had a "moist touch". Furthermore, as shown in Tables 3 and 4, Comparative Example 2 and Comparative Examples 13-19, in which the ratio Rdc / t was greater than 0.2, had a feel that was clearly different from that of Example 1.

[0138] Furthermore, even though the decorative sheet had an uneven shape achieved by forming ridges on the surface protective layer, Comparative Examples 20-22, in which the coating amount was less than 2 μm or greater than 18 μm and the ratio Rdc / t was greater than 0.2, had a different feel to the touch from Example 1.

[0139] [Table 1]

[0140] [Table 2]

[0141] [Table 3]

[0142] [Table 4] [Explanation of symbols]

[0143] 10 Decorative Sheet 1 Primer layer 2 Original layer 3. Picture layer 4 Adhesive layer 5 Transparent resin layer 6 Surface protective layer 6a Core section 6b Ridged part S1 Pattern printing process S2 Melt extrusion process S3 Extrusion Lamination Process S4 Protective layer coating process S5 Light irradiation process S6 Protective layer curing process V vertical direction UP upper side LO Lower

Claims

1. The original layer and A surface protective layer having an uneven shape with ridge-like raised portions formed thereon and provided on the upper side of the raw fabric layer; Equipped with The surface protective layer is The thickness is 2 μm or more and 18 μm or less, a ratio of the cut level difference Rdc to the thickness is 0.1 or more and 0.2 or less, Contains particles with an average particle size of 3 μm or more, 60 degree reflected gloss is less than 10; Decorative sheet.

2. A pattern layer provided on the upper side of the raw fabric layer; A primer layer provided under the base layer; Further equipped with The raw fabric layer is A resin layer; a skin layer provided on the upper side and the lower side of the resin layer and containing a nucleating agent or inorganic particles; having The decorative sheet according to claim 1 .

3. A pattern layer provided on the upper side of the raw fabric layer; an adhesive layer provided on the upper side of the design layer; a transparent resin layer provided on the upper side of the adhesive layer; A primer layer provided under the base layer; Further comprising: The decorative sheet according to claim 1 .

4. The average particle size of the particles is 11 μm or less. The decorative sheet according to claim 1 .

5. The surface protective layer contains an ionizing radiation curable resin. The decorative sheet according to claim 1 .

6. The surface protective layer contains an acrylate. The decorative sheet according to claim 1 .

7. the surface protective layer contains a trifunctional acrylate having a repeating structure, and the number of repeats of the repeating structure is 3 or more and 20 or less; The decorative sheet according to claim 1 .

8. the surface protective layer contains a tetrafunctional acrylate having a repeating structure, and the number of repeats of the repeating structure is 20 or more and 35 or less; The decorative sheet according to claim 1 .

9. The decorative sheet according to any one of claims 1 to 8, A substrate provided on the lower side of the decorative sheet; Equipped with Cosmetic materials.

10. A pattern printing process for forming a pattern layer on the upper side of the raw fabric layer; a protective layer coating step of forming a surface protective layer on the upper side of the design layer; a light irradiation step of irradiating a surface of the surface protective layer with light having a wavelength of 200 nm or less to form a ridge portion so that a ratio of a cut level difference Rdc to a thickness of the surface protective layer is 0.1 or more and 0.2 or less; Equipped with A method for producing a decorative sheet.

11. The protective layer coating step forms the surface protective layer so that the thickness of the surface protective layer is 2 μm or more and 18 μm or less. A method for producing the decorative sheet according to claim 10.

12. A method for producing a decorative sheet according to claim 10 or 11, a substrate adhering step of adhering a substrate to the underside of the decorative sheet; Equipped with A method for manufacturing a cosmetic material.

Citation Information

Patent Citations

  • Decorative sheet

    JP2018199240A

Cited By

  • Method for producing a decorative surface

    WO2026099706A1