Sorption type heat exchange module and method of manufacturing the same
By employing heat transfer fins with a corrosion-resistant film and a sorbent layer of organic polymer particles and a polyamine-epoxy resin binder, the module achieves increased sorbent volume and efficiency, addressing clogging and cracking issues in sorption heat exchange modules.
Patent Information
- Application Number
- JP2023219415
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2023-12-26
- Publication Date
- 2024-10-31
Smart Images

Figure 2024155711000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sorptive heat exchange module including heat transfer fins and heat transfer tubes provided with a sorptive layer having sorptive particles, and a method for manufacturing the same. [Background technology]
[0002] In recent years, from the viewpoint of energy saving in air conditioning, air conditioners that separate and process latent heat and sensible heat have been studied. Among them, the use of a sorbent has been proposed for latent heat treatment, i.e., moisture absorption. For example, the dehumidifying air conditioner disclosed in Patent Document 1 uses a desiccant rotor carrying a sorbent.
[0003] On the other hand, the sorbent has a characteristic that its own temperature rises due to heat generation accompanying moisture absorption, and the moisture absorption rate decreases, so the inherent moisture absorption performance cannot be fully demonstrated. If the heat generated by the sorbent during moisture absorption is removed by cooling, the decrease in the moisture absorption rate is suppressed, leading to an improvement in the efficiency of latent heat treatment, but it is difficult to provide an efficient cooling means for the desiccant rotor.
[0004] One approach to improve this problem is a sorptive heat exchange module that combines a heat transfer fin carrying a sorbent with a heat transfer tube, as disclosed in Patent Document 2. In such a heat exchange module, a refrigerant is passed through the heat transfer tube, thereby cooling and removing heat generated by the moisture absorption of the sorbent.
[0005] In such a heat exchange module, the more the number of heat transfer fins is increased, the larger the sorbent layer area and the amount of sorbent per unit volume of the module, and the latent heat treatment efficiency can be improved. On the other hand, since the heat exchange module is manufactured by immersing the assembled module in a coating liquid containing a sorbent, if the number of heat transfer fins is increased to narrow the gap between the heat transfer fins, the liquid is not sufficiently drained after immersion, and the sorbent is clogged in the gap between the heat transfer fins even after drying, making them prone to clogging. For this reason, there is a limit to increasing the number of heat transfer fins.
[0006] Regarding this point, if the adsorbent is supported on the heat transfer fins before the module is assembled, the problem of poor drainage after immersion can be avoided. However, when the punching process for drilling holes for inserting the heat transfer tubes or the module assembly process is performed on the heat transfer fins supporting the adsorbent layer, the adsorbent layer cracks or peels off, making it difficult to obtain a practical sorptive heat exchange module.
[0007] Regarding the prevention of cracking and peeling of the sorbent layer, Patent Document 3 discloses a method of applying a corrosion-resistant film to the surface of the heat transfer fin and bonding the corrosion-resistant film and the sorbent with a binder. However, this method is only capable of dealing with the volumetric changes of the sorbent due to moisture absorption and release, and is not capable of withstanding processing such as punching. It is possible to improve the effect of preventing cracking and peeling by increasing the amount of binder, but this will increase the degree of coverage of the sorbent with the binder, making it difficult to express the moisture absorption performance, and will result in a decrease in the latent heat treatment efficiency. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 11-262621 [Patent Document 2] JP 2006-200850 A [Patent Document 3] JP 2012-077987 A Summary of the Invention [Problem to be solved by the invention]
[0009] As described above, in a sorptive heat exchange module, there are limitations on the module structure and manufacturing method due to the characteristics of the sorptive layer that cannot withstand clogging between heat transfer fins and machining, and there is a problem that improvement in the efficiency of latent heat treatment is limited. The present invention has been devised in consideration of the current state of the prior art, and its object is to provide a heat exchange module with excellent latent heat treatment efficiency, in which the spacing between heat transfer fins is narrowed and the amount of sorptive agent per unit volume of the module is increased by making the sorptive layer have characteristics that can withstand machining, and enabling punching and module assembly after the sorptive layer is supported. [Means for solving the problem]
[0010] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that the above-mentioned object can be achieved by using a heat transfer fin which is provided on its surface with a corrosion-resistant film containing an epoxy resin, and a sorbent layer which contains sorbent particles made of an organic polymer having a specific amount of carboxy groups, and a binder made of polyamine, a reactive diluent having two or more epoxy groups, and an epoxy resin, and have thus arrived at the present invention.
[0011] That is, the present invention is achieved by the following means. [1] A sorptive heat exchange module comprising a plurality of heat transfer fins provided with a sorptive layer and a heat transfer tube penetrating the plurality of heat transfer fins, The heat transfer fins each have a corrosion-resistant film containing an epoxy resin provided on a surface of a metal plate having excellent thermal conductivity, and a sorbent layer is provided on the corrosion-resistant film, the sorbent layer containing sorbent particles made of an organic polymer having a carboxyl group, and a binder made of polyamine, a reactive diluent having two or more epoxy groups, and an epoxy resin; The organic polymer has a carboxyl group content of 3 to 10 mmol / g and a neutralization degree of 60 to 100%, and 30 to 110 parts by weight of the binder is used per 100 parts by weight of the sorbent particles, and the total amount of the sorbent particles and the binder is 20 to 80 g / m per one side of the metal plate surface. 2 It is supported, The sorptive heat exchange module further comprises: a heat exchanger module that is provided with a heat exchanger that is disposed between adjacent heat transfer fins and that is free of any blocking portion formed by a sorptive layer. [2] The sorptive heat exchange module described in [1], characterized in that the distance between adjacent heat transfer fins is less than 2 mm. [3] The amount of sorbent per unit volume is 20-60 kg / m 3 The sorptive heat exchange module according to [1], [4] A dehumidification system using the sorptive heat exchange module described in any one of [1] to [3]. [5] A method for manufacturing a sorptive heat exchange module according to any one of [1] to [3], comprising the steps of: providing a sorptive layer on the surface of a heat transfer fin provided with a corrosion-resistant film, the sorptive layer containing sorptive particles made of an organic polymer having a carboxyl group, and a binder made of polyamine and epoxy resin; punching out holes in the heat transfer fin provided with the sorptive layer; and inserting heat transfer tubes into the holes. Effect of the Invention
[0012] The heat transfer fins used in the sorptive heat exchange module of the present invention can support the sorbent by line coating on an aluminum plate, and therefore the production speed is significantly improved and the uniformity of the amount of the sorbent supported is also improved compared to the conventional method of repeatedly immersing the module in a coating liquid containing the sorbent and drying it after assembly of the module. The sorptive heat exchange module of the present invention manufactured using such heat transfer fins can narrow the heat transfer fin interval and increase the amount of sorbent per unit volume of the module, making it possible to obtain a heat exchange module that is more compact than conventional ones and has excellent latent heat processing efficiency. The sorptive heat exchange module of the present invention can be used to construct a compact and highly efficient dehumidification system, and therefore can be suitably used in dehumidification systems such as latent heat and sensible heat separation air conditioners and frost-free refrigeration and freezing equipment that suppresses the generation of frost during low-temperature operation. [Brief description of the drawings]
[0013] [Figure 1]FIG. 1 is a diagram showing a representative example of a sorptive heat exchange module of the present invention. [Diagram 2] 1 is a graph showing the change over time in the integrated moisture absorption amount of the sorptive heat exchange modules of Example 1, Example 11, and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The sorptive heat exchange module of the present invention comprises a plurality of heat transfer fins provided with a sorptive layer and a heat transfer tube penetrating the plurality of heat transfer fins, the plurality of heat transfer fins comprising a metal plate having excellent thermal conductivity, a corrosion-resistant film provided on the metal surface, and a sorptive layer containing sorptive particles and a binder, and further, there is no portion between adjacent heat transfer fins where the sorptive layers on the heat transfer fins come into contact with each other to block the gap. Each element will be described below.
[0015] (1) Metal plates with excellent thermal conductivity The metal plate having excellent thermal conductivity (hereinafter, simply referred to as the substrate) in the present invention corresponds to the substrate portion of the heat transfer fin. Examples of the type of metal to be used include silver, copper, gold, aluminum, steel, etc., and metals with a thermal conductivity of 50 (W / m·K) or more are preferable because they can perform highly efficient heat exchange. Among them, aluminum, aluminum alloys, copper, and copper alloys are more preferable from the practical viewpoint of cost. There is no particular restriction on the shape of the substrate, and it can be appropriately selected according to the purpose, such as flat, wavy, corrugated, or partially perforated.
[0016] The thickness of the substrate (hereinafter also referred to as plate thickness) is preferably 0.03 to 1.0 mm, more preferably 0.04 to 0.6 mm, and even more preferably 0.05 to 0.4 mm. If the plate thickness is less than 0.03 mm, it is likely to be easily cracked, broken, deformed, etc. by external forces, and thus it may be difficult to handle in each process of processing into a heat exchange module. If the plate thickness exceeds 1.0 mm, it is difficult to transfer the cold heat of the heat transfer tube to the sorption agent layer, and therefore it may be difficult to obtain sufficient performance.
[0017] (2) Corrosion-resistant film The corrosion-resistant film in the present invention is provided on the surface of the substrate for the purpose of preventing corrosion of the substrate and improving adhesion between the adsorbent layer and the substrate. The primer component forming such a corrosion-resistant film is an epoxy resin having good adhesion to the substrate and the adsorbent layer, and among them, an acrylic-modified epoxy resin is preferable. In addition, when the substrate is an aluminum-based material, the substrate is usually subjected to a surface treatment such as a phosphoric acid chromate treatment, and then the primer component is applied to form the corrosion-resistant film.
[0018] (3) About the sorbent layer The sorbent layer in the present invention is mainly composed of sorbent particles and a binder (hereinafter also referred to as binder) made of a reactive diluent having two or more epoxy groups, a polyamine, and an epoxy resin.
[0019] (3-1) Sorbent particles The sorbent particles are composed of an organic polymer having a carboxyl group. Since the carboxyl group has a property of reversibly adsorbing water vapor in the air, the sorbent particles made of the organic polymer have moisture absorbing and releasing ability. The lower limit of the total amount of carboxyl groups contained in the organic polymer is preferably 3 mmol / g, more preferably 4 mmol / g. If the amount of carboxyl groups is less than 3 mmol / g, the moisture absorbing and releasing properties required by the present invention cannot be obtained sufficiently. The upper limit is preferably 10 mmol / g, more preferably 7 mmol / g. If the amount of carboxyl groups exceeds 10 mmol / g, the sorbent particles will absorb more moisture than necessary and swell, resulting in a loss of water resistance.
[0020] In addition, the carboxyl groups are at least partially neutralized to improve moisture absorption performance. In this case, the counter cation may be, for example, an alkali metal such as Li, Na, K, Rb, or Cs, an alkaline earth metal such as Mg, Ca, Sr, or Ba, or an organic cation such as NH4 or amine. From the viewpoint of moisture absorption and desorption speed, it is preferable that the counter ion is an alkali metal or an alkaline earth metal cation, and sodium or potassium is more preferable. In this case, the ratio of the counter ion to the total carboxyl groups that is the above cation, that is, the degree of neutralization, is 60% as a lower limit, and 65% is preferable. If the degree of neutralization is below the lower limit, the sorbent particles cannot obtain sufficient moisture absorption performance. In addition, there is no particular limit as to the upper limit, but from the definition of the degree of neutralization described above, the degree of neutralization does not exceed 100%.
[0021] The weight average particle diameter of the sorbent particles is preferably 3 μm, more preferably 10 μm, and even more preferably 20 μm as a lower limit. If the weight average particle diameter is less than 3 μm, the particles are buried in the binder and cannot exhibit sufficient moisture absorption performance. The upper limit is preferably 100 μm, and more preferably 50 μm. If the weight average particle diameter exceeds 100 μm, the film-forming property is reduced, which is undesirable because it leads to cracking and peeling of the coating film.
[0022] The swelling ratio of the adsorbent particles in water is preferably 5 times or less, and more preferably 3 times or less. If the swelling ratio in water exceeds 5 times, the adsorbent layer containing the adsorbent particles is likely to peel off from the substrate, which is not preferable.
[0023] The above-mentioned sorbent particles can be produced by a conventional method of polymerizing a monomer to form a polymer. At this time, the monomer is not particularly limited, and can be appropriately selected, including vinyl monomers. In addition, there is no particular limit to which method is adopted, and examples thereof include a method of obtaining a polymer by homopolymerizing a monomer having a salt-type carboxyl group or copolymerizing it with another monomer that can be copolymerized (method 1), a method of obtaining a polymer having a carboxyl group and then converting it to a salt type (method 2), a method of polymerizing a monomer having a functional group that can be derived to a carboxyl group, converting the functional group of the obtained polymer to a carboxyl group by chemical modification, and then converting it to a salt type (method 3), or a method of carrying out the above three methods by graft polymerization.
[0024] Examples of the method for polymerizing a monomer having a salt-type carboxyl group in the above-mentioned method 1 include a method in which a salt-type monomer corresponding to a monomer containing a carboxyl group, such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinylpropionic acid, etc., is polymerized alone, or two or more of these monomers are polymerized, or a mixture of a carboxylic acid type and a corresponding salt type of the same type of monomer is polymerized, and further a method in which these monomers are copolymerized with other monomers that are copolymerizable therewith.
[0025] The method of converting a polymer having a carboxyl group into a salt form after obtaining it in the second method is, for example, a method of obtaining a homopolymer of an acid monomer containing a carboxyl group as described above, or a copolymer of two or more of the monomers, or a copolymer with another copolymerizable monomer by polymerization, and then converting it into a salt form. There is no particular limitation on the method of converting a carboxyl group into a salt form, and the conversion can be performed by a method such as reacting the obtained acid polymer with a solution containing an alkali metal ion such as Li, Na, K, Rb, Cs, etc., an alkaline earth metal ion such as Mg, Ca, Sr, Ba, etc., or an organic cation such as NH4 or an amine to perform ion exchange.
[0026] The method of introducing a carboxyl group by the chemical modification method of the third method includes, for example, a method of polymerizing a homopolymer of a monomer having a functional group that can be modified to a carboxyl group by chemical modification treatment, or a copolymer consisting of two or more kinds, or a copolymer with another copolymerizable monomer, and modifying the resulting polymer to a carboxyl group by hydrolysis. If the resulting state is not a salt type, the above-mentioned method of converting the modified carboxyl group to a salt type is applied. Examples of monomers that can be used in this manner include monomers having a nitrile group such as acrylonitrile and methacrylonitrile; anhydrides, ester derivatives, amide derivatives, and crosslinkable ester derivatives of monomers having a carboxylic acid group such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, and vinylpropionic acid.
[0027] Examples of the anhydride of a monomer having a carboxylic acid group include maleic anhydride, acrylic anhydride, methacrylic anhydride, itaconic anhydride, phthalic anhydride, N-phenylmaleimide, and N-cyclomaleimide.
[0028] Examples of the ester derivatives of monomers having a carboxylic acid group include alkyl ester derivatives such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, lauryl, pentadecyl, cetyl, stearyl, behenyl, 2-ethylhexyl, isodecyl, and isoamyl; methoxyethylene glycol, ethoxyethylene glycol, methoxypolyethylene glycol, ethoxypolyethylene glycol, polyethylene glycol, methoxypropylene glycol, propylene glycol, methoxypolypropylene glycol, polypropylene glycol, methoxypolytetraethylene glycol, polytetraethylene glycol, polyethylene glycol-polypropylene glycol, polyethylene glycol-polytetraethylene glycol, polyethylene glycol-polypropylene glycol, polypropylene glycol-polytetraethylene glycol, butoxyethylene glycol, alkyl ether ester derivatives such as cyclohexyl, tetrahydrofurfuryl, benzyl, phenoxyethyl, phenoxypolyethylene glycol, isobornyl, neopentyl glycol benzoate, and other cyclic compound ester derivatives; hydroxyalkyl ester derivatives such as hydroxyethyl, hydroxypropyl, hydroxybutyl, hydroxyphenoxypropyl, hydroxypropylphthaloylethyl, and chlorohydroxypropyl; aminoalkyl ester derivatives such as dimethylaminoethyl, diethylaminoethyl, and trimethylaminoethyl; carboxylic acid alkyl ester derivatives such as (meth)acryloyloxyethyl succinate and (meth)acryloyloxyethyl hexahydrophthalate; alkyl ester derivatives containing a phosphoric acid group or a phosphoric acid ester group such as (meth)acryloyloxyethyl acid phosphate and (meth)acryloyloxyethyl acid phosphate; Ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,6-hexanediol (meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, glycerin dimethacrylate, 2-hydroxy-3-acryloyloxypropyl (meth)acrylate Examples of crosslinkable alkyl esters include ethylene oxide adduct di(meth)acrylate of bisphenol A, propylene oxide adduct di(meth)acrylate of bisphenol A, neopentyl glycol di(meth)acrylate, 1,10-decanediol di(meth)acrylic, dimethylol tricyclodecane di(meth)acrylate, and ethylene oxide modified trimethylolpropane tri(meth)acrylate; and fluorinated alkyl ester derivatives such as trifluoroethyl, tetrafluoropropyl, hexafluorobutyl, and perfluorooctylethyl.
[0029] Examples of amide derivatives of monomers having a carboxylic acid group include amide compounds such as (meth)acrylamide, dimethyl(meth)acrylamide, monoethyl(meth)acrylamide, normal-t-butyl(meth)acrylamide, etc. Other methods for introducing a carboxyl group by chemical modification include oxidation of alkenes, alkyl halides, alcohols, aldehydes, etc.
[0030] There is no particular limitation on the method of introducing salt-type carboxyl groups by hydrolysis of the polymer in the above-mentioned third method, and known hydrolysis conditions can be used. For example, a method of introducing salt-type carboxyl groups into a polymer crosslinked by polymerizing the above-mentioned monomers using a basic aqueous solution of an alkali metal hydroxide, such as sodium hydroxide, lithium hydroxide, potassium hydroxide, or ammonia, or a method of reacting the polymer with a mineral acid, such as nitric acid, sulfuric acid, or hydrochloric acid, or an organic acid, such as formic acid or acetic acid, to form a carboxylic acid group, and then mixing it with an alkali metal salt to introduce a salt-type carboxyl group by ion exchange. Among them, the hydrolysis method using potassium hydroxide is preferred, which can easily obtain potassium salt-type carboxyl groups with excellent moisture absorption rate. The conditions for 3 to 10 mmol / g can be determined by clarifying the relationship between reaction factors such as reaction temperature, concentration, and time and the amount of salt-type carboxyl groups introduced through experiments.
[0031] In addition, the sorbent particles used in the present invention preferably have a crosslinked structure. Such a crosslinked structure reduces swelling of the particles that occurs when the particles absorb moisture or water. There is no particular limitation on the crosslinked structure, so long as it is not physically or chemically modified by moisture absorption or release, and any structure such as crosslinking by covalent bonds, ionic crosslinking, crosslinking by polymer molecular interactions or crystalline structures may be used. There is also no particular limitation on the method of introducing crosslinks, and examples include a crosslinking introduction method in which a crosslinking monomer is copolymerized in the polymerization stage of the monomer in each of the above-mentioned first, second, and third methods, or a post-crosslinking method in which the above-mentioned monomer is first polymerized and then a crosslinking structure is introduced by a chemical reaction or physical energy. In particular, the method of using a crosslinking monomer in the polymerization stage of the monomer, or the method of chemical post-crosslinking after obtaining a polymer, is preferable in that it is possible to introduce strong crosslinks by covalent bonds and is less susceptible to physical and chemical modifications associated with moisture absorption and release.
[0032] In the method of using a crosslinkable monomer in the polymerization stage of the monomer, particularly in the case of an organic polymer-based sorbent having a salt-type carboxyl group, a crosslinkable monomer that has the above-mentioned carboxyl group or that can be copolymerized with a monomer that can be modified to a carboxyl group is used, and a crosslinked polymer having a crosslinked structure based on a covalent bond can be obtained by copolymerization. However, in this case, the crosslinkable monomer must be one that is not or is not easily affected by the acidic conditions exhibited by the monomer acrylic acid, or by chemical influences (such as hydrolysis) when modifying the polymer to a carboxyl group.
[0033] The crosslinkable monomer that can be used in the method of using a crosslinkable monomer in the monomer polymerization stage is not particularly limited, and examples thereof include crosslinkable vinyl compounds such as glycidyl methacrylate, N-methylol acrylamide, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, hydroxyethyl methacrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and methylene bisacrylamide. Among these, crosslinked structures using triallyl isocyanurate, triallyl cyanurate, divinylbenzene, and methylene bisacrylamide are preferable because they are chemically stable even during hydrolysis or the like for introducing a carboxyl group into a crosslinked polymer containing them.
[0034] In addition, the post-crosslinking method is not particularly limited, and for example, the post-crosslinking method can be mentioned in which the nitrile group contained in the nitrile polymer containing 50% by weight or more of vinyl monomer having a nitrile group is reacted with a hydrazine compound or formaldehyde. Among them, the crosslinked structure introduced by the hydrazine compound is stable against acids and alkalis, and the formed crosslinked structure itself is hydrophilic, so it can contribute to improving hygroscopicity, and it is extremely excellent in that it can introduce a strong crosslink that can maintain the shape of the porosity or the like given to the polymer. The crosslinked structure obtained by the reaction has not been identified in detail, but it is presumed to be based on a triazole ring or tetrazole ring structure.
[0035] The vinyl monomer having a nitrile group is not particularly limited as long as it has a nitrile group, and specific examples thereof include acrylonitrile, methacrylonitrile, ethacrylonitrile, α-chloroacrylonitrile, α-fluoroacrylonitrile, vinylidene cyanide, etc. Among them, acrylonitrile is most preferable because it is cost-effective and has a large amount of nitrile groups per unit weight.
[0036] The method of introducing crosslinking by reaction with a hydrazine compound is not particularly limited as long as the desired crosslinked structure can be obtained, and the concentration of the acrylonitrile polymer and the hydrazine compound during the reaction, the solvent used, the reaction time, the reaction temperature, etc. can be appropriately selected as necessary. Regarding the reaction temperature, if it is too low, the reaction rate will be slow and the reaction time will be too long, and if it is too high, the raw acrylonitrile polymer will be plasticized, and the shape given to the polymer will be destroyed. Therefore, the preferred reaction temperature is 50 to 150°C, more preferably 80°C to 120°C. In addition, there is no particular limit to the part of the acrylonitrile polymer to be reacted with the hydrazine compound, and it can be appropriately selected according to the application and the shape of the polymer. Specifically, it can be appropriately selected to react only on the surface of the polymer, or to react all over the polymer to the core, or to react only in a specific part. The hydrazine compounds used herein include hydrazine salts such as hydrazine hydrate, hydrazine sulfate, hydrazine hydrochloride, hydrazine nitrate, hydrazine bromate, and hydrazine carbonate, as well as hydrazine derivatives such as ethylenediamine, guanidine sulfate, guanidine hydrochloride, guanidine nitrate, guanidine phosphate, and melamine.
[0037] The sorbent particles having a crosslinked structure used in the present invention can be produced as described above, but commercially available products may also be used. An example of such a sorbent particle having a crosslinked structure is "Ecopod (registered trademark) HU-750P" manufactured by Toyobo Co., Ltd.
[0038] In addition, after producing the sorbent particles as described above, it is also preferable to further impart a basic polymer such as polyethyleneimine to the surface of the sorbent particles. In this way, when a urethane-modified epoxy resin is used as the binder described later, the adhesion between the sorbent particles and the binder is increased, and the strength of the sorbent layer can be improved. Examples of the sorbent particles to which a basic polymer is imparted include the functional fine particles disclosed in International Publication No. 2014 / 188908.
[0039] (3-2) About binders The binder is composed of an epoxy resin, a polyamine, and a reactive diluent having two or more epoxy groups. First, the epoxy resin serves to support the sorbent particles on the substrate, and among them, urethane-modified epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, and chelate-modified epoxy resin are preferred, and urethane-modified bisphenol A type epoxy resin and urethane-modified bisphenol F type epoxy resin are more preferred, and these resins may be used in combination. Specifically, ADEKA RESIN (registered trademark) EPU-11F (urethane-modified bisphenol A type epoxy resin) and EPU-1001 (urethane-modified bisphenol F type epoxy resin) manufactured by ADEKA CORPORATION can be mentioned.
[0040] Next, the polyamine functions as a curing agent, and by crosslinking the resin, the strength of the sorbent layer is increased and cracking can be suppressed. Examples of such polyamines include polyallylamine, polyethyleneimine, polydimethyldiallylammonium chloride, xylylenediamine, and isophoronediamine. Only one type of polyamine may be used, or multiple types may be used in combination. In addition, commercially available polyamines may be used, such as jER Cure (registered trademark) LV11 manufactured by Mitsubishi Chemical Corporation and Daitoclar (registered trademark) D6293 manufactured by Daito Sangyo Co., Ltd.
[0041] The content of the polyamine in the binder is not particularly limited and may be appropriately selected depending on the epoxy equivalent and content of the epoxy resin. When a commercially available polyamine is used, the blending amount specified by the manufacturer may be appropriately adopted.
[0042] A reactive diluent having two or more epoxy groups can suppress a decrease in the concentration of epoxy groups in a coating liquid containing the binder component, while reducing the viscosity of the coating liquid to prevent thick coating or unevenness when applied to a substrate, and can also form a crosslinked structure within the binder to increase its strength.
[0043] The viscosity of the reactive diluent at 25°C is not particularly limited in terms of its lower limit, and the lower the better. The upper limit is preferably 500 mPa·s, and more preferably 400 mPa·s. If the viscosity exceeds 500 mPa·s, the viscosity of the coating liquid may not be sufficiently reduced.
[0044] The molecular weight of the reactive diluent is not particularly limited as a lower limit, and there is no problem if it is, for example, 174 or more, which is the molecular weight of ethylene glycol diglycidyl ether, which has the simplest structure among the reactive diluents commonly used. The upper limit is preferably 500, and more preferably 300. In general, since there is a positive correlation between molecular weight and viscosity, when the molecular weight of the reactive diluent exceeds 500, the viscosity also increases, and there is a risk that the viscosity of the coating liquid cannot be sufficiently reduced.
[0045] The epoxy equivalent of the reactive diluent is preferably 50 g / eq as a lower limit, more preferably 70 g / eq. If the epoxy equivalent is less than 50 g / eq, the crosslinked structure may become excessively dense and hard and brittle. The upper limit is preferably 200 g / eq, more preferably 150 g / eq. If the epoxy equivalent is more than 200 g / eq, the epoxy groups are less relative to the amount of reactive diluent added to the coating liquid, and the effect of increasing the strength of the binder by the crosslinking described above may not be sufficiently obtained.
[0046] Examples of such reactive diluents include ethylene glycol diglycidyl ether, cyclohexanedimethanol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, etc. Commercially available products may also be used, such as Denacol (registered trademark) EX810 and Adeka Glycirol (registered trademark) ED523T manufactured by ADEKA CORPORATION.
[0047] The content of the reactive diluent in the binder is preferably 100 parts by weight or less, and more preferably 70 parts by weight or less, based on 100 parts by weight of the epoxy resin.
[0048] The lower limit of the binder content is preferably 30 parts by weight, more preferably 50 parts by weight, and even more preferably 60 parts by weight, per 100 parts by weight of the sorbent particles. If the binder content is too small, the adhesion between the corrosion-resistant film and the sorbent and between the sorbents themselves decreases, making them more likely to peel off. The upper limit is preferably 110 parts by weight, more preferably 100 parts by weight, per 100 parts by weight of the sorbent particles. If the binder content is too high, the binder will cover too much of the surface of the sorbent particles, making it difficult to fully exert the function of the sorbent.
[0049] (3-3) Loading amount and moisture absorption amount of the adsorbent layer In the present invention, the amount of the sorbent layer supported on the surface of one side of the substrate is 20 g / m 2 It is preferable that the thickness is 30 g / m 2 If the amount of the adsorbent layer is too small, it becomes difficult to exhibit sufficient moisture absorption capacity. 2 It is preferable that the thickness is 70 g / m 2 If the amount of the sorbent layer loaded is too large, the sorbent layer becomes prone to peeling off from the substrate, resulting in a decrease in durability.
[0050] The moisture absorption amount of the adsorbent layer is, in the measurement method described later, limited to 10 g / m 2 is preferred, and 15 g / m 2 If the moisture absorption amount is below the lower limit, sufficient moisture absorption performance may not be obtained.
[0051] (4) Heat transfer fins with adsorbent layers The heat transfer fin provided with the adsorbent layer employed in the present invention can be obtained by coating the surface of a metal plate having excellent thermal conductivity provided with a corrosion-resistant film containing the above-mentioned epoxy resin with a coating liquid containing adsorbent particles made of an organic polymer having a carboxyl group, polyamine, a reactive diluent having two or more epoxy groups, an epoxy resin, and a solvent, and baking the coating liquid. Examples of the coating method include a method of immersing a substrate in the coating liquid and then draining the liquid using a centrifugal separator or a squeeze roller, a method of applying the coating liquid to the substrate using a bar coder, a blade, or the like, and a method of spraying the coating liquid onto the substrate.
[0052] In addition to the above components, other components such as antibacterial agents and preservatives may be added to the coating liquid as necessary. In addition, it is preferable to use an organic solvent as the solvent for the coating liquid, since the volume change caused by the water swelling of the sorbent particles can be suppressed. Among them, when a ketone is used as the solvent, a part of it reversibly generates ketimine with the polyamine during the baking reaction, suppressing the rate of the crosslinking reaction between the polyamine and the epoxy resin, and therefore it is more preferable to reduce unevenness in the reaction. Examples of such ketones include acetone, methyl ethyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, diethyl ketone, benzyl methyl ketone, diisopropyl ketone, cyclopentanone, and cyclohexanone.
[0053] When preparing the coating liquid, it is preferable to first prepare a solution containing an epoxy resin, a reactive diluent having two or more epoxy groups, an organic solvent, and sorbent particles made of an organic polymer having a carboxyl group, and then add a polyamine to the solution. If the polyamine is added prior to the addition of other components other than the epoxy resin, the epoxy resin will begin to harden at that point, which may cause problems in the subsequent preparation and application of the coating liquid.
[0054] The heat transfer fins provided with the sorbent layer employed in the present invention described above have high strength and adhesion of the sorbent layer, so that the sorbent layer is unlikely to crack or peel off and can withstand machining. Therefore, even if the heat transfer fins are subjected to burring (a process of punching holes and attaching raised portions (flanges) around the holes) and a heat transfer tube is inserted and assembled into a sorption-type heat exchange module (hereinafter referred to as a pre-coating method), a sorption-type heat exchange module without cracks or peeling of the sorbent layer can be obtained. In other words, there is no need to use the conventional method of impregnating a pre-assembled module with a sorbent-containing liquid to form a sorbent layer (hereinafter referred to as an impregnation coating method).
[0055] (5) Sorption-type heat exchange module The sorptive heat exchange module of the present invention has a shape as shown in FIG. 1, for example, and is manufactured by a precoat method using a heat transfer fin provided with the above-mentioned sorptive layer. Specifically, the module can be manufactured through a process of providing a sorptive layer containing sorptive particles made of an organic polymer having a carboxyl group, and a binder made of polyamine, a reactive diluent having two or more epoxy groups, and an epoxy resin on the surface of the heat transfer fin provided with a corrosion-resistant film, a process of punching the heat transfer fin provided with the sorptive layer to form holes, and a process of inserting heat transfer tubes into the holes. That is, after obtaining the heat transfer fin provided with the sorptive layer, the module can be manufactured in the same manner as the manufacturing method of a normal heat exchange module. The material of the heat transfer tube can be the same as the material of the metal plate having excellent thermal conductivity described above.
[0056] In the precoat method, unlike the impregnation coating method, poor drainage of the sorbent-containing liquid does not occur, so that even if the interval between the heat transfer fins is narrowed, the problem of blockage between the heat transfer fins does not occur. Therefore, in the sorptive heat exchange module of the present invention, the interval between adjacent heat transfer fins can be preferably less than 2 mm, more preferably 1.5 mm or less, and even more preferably 1.3 mm or less. On the other hand, the lower limit of the interval between adjacent heat transfer fins is preferably 0.3 mm or more from the viewpoint of air circulation. In the present invention, the "interval between adjacent heat transfer fins" refers to the distance between the substrates constituting the heat transfer fins, and is controlled by the burring height in the burring process described later.
[0057] As described above, in the sorptive heat exchange module of the present invention, the distance between adjacent heat transfer fins can be narrowed to increase the area of the sorbent layer per unit volume, so that the amount of sorbent per unit volume can be increased. In particular, a major advantage of the present invention is that clogging of the spaces between the heat transfer fins by the sorbent can be avoided even if the amount of sorbent per unit volume is increased more than in the past.
[0058] The amount of sorbent per unit volume is 20 to 60 kg / m 3 is preferably 22 to 55 kg / m 3 More preferably, it is 60 kg / m 3 If it exceeds 20kg / m, the adsorbent layer becomes too thick and the gap between the heat transfer fins becomes narrow, which may cause excessive pressure loss when air passes through. 3 If it is less than this, there is a risk that sufficient moisture absorption performance will not be obtained.
[0059] The above-mentioned sorptive heat exchange module of the present invention has a narrow heat transfer fin spacing and a large amount of sorbent per unit volume of the module, and therefore has a higher latent heat treatment efficiency than conventional modules. The sorptive heat exchange module of the present invention can be used to construct a compact, highly efficient dehumidification system, and is therefore suitable for use in dehumidification systems such as latent heat and sensible heat separation air conditioners and frost-free refrigeration and freezing equipment that suppresses the formation of frost during low-temperature operation. EXAMPLES
[0060] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following examples. In the examples, parts and percentages are by weight unless otherwise specified. First, the evaluation method for each characteristic will be described.
[0061] [Total amount of carboxyl groups] Approximately 1 g of the sorbent sample is dried at 105°C for 16 hours and the weight is measured (X [g]). 200 ml of water is added to this, and then 1N hydrochloric acid is added while heating to 50°C to adjust the pH to 2, converting all of the carboxyl groups contained in the sample to H-type carboxyl groups. A titration curve is then obtained using a 0.1N sodium hydroxide aqueous solution according to the usual method. The amount of sodium hydroxide aqueous solution consumed by the H-type carboxyl groups (V [ml]) is obtained from the titration curve, and the total amount of carboxyl groups contained in the sample is calculated using the following formula. [Formula] Total amount of carboxyl groups [mmol / g] = 0.1V / X
[0062] [Neutralization level] A titration curve is similarly obtained without adjusting the pH to 2 by adding 1N hydrochloric acid during the above-mentioned total carboxyl group measurement procedure, and the amount of H-type carboxyl groups contained in the sample is calculated. From these results, the degree of neutralization is calculated using the following formula. [Formula] Degree of neutralization = {(total amount of carboxyl groups) - (amount of H-type carboxyl groups)} / (total amount of carboxyl groups)
[0063] [Weight average particle diameter] Measurements are taken using a Shimadzu SALD-200V laser diffraction particle size distribution analyzer using water as the dispersion medium, and the average particle size is calculated from the particle size distribution expressed on a volume basis.
[0064] [Swelling ratio] After drying 20 g of sorbent particles at 120°C for 2 hours, place it in a 100 mL graduated cylinder and read its volume (A [mL]). After that, add ion-exchanged water up to the 100 mL mark on the test tube and leave it to stand for 2 hours, then read the volume of the sample again (B [mL]). From these results, calculate the swelling ratio of the sorbent particles using the following formula: [Formula] Swelling ratio [times] = B / A
[0065] [Method for measuring viscosity of reactive diluents] The viscosity at 25° C. is measured using a viscometer (manufactured by BROOKFIELD, LVDV-II+).
[0066] [Method for measuring epoxy equivalent] Measured according to JIS K7236.
[0067] [Moisture absorption amount of the adsorbent layer on the heat transfer fin] The heat transfer fins (area A [m 2 The weight (W0[g]) after drying at 105°C for 16 hours and the weight (W s From these results, calculate the amount of moisture absorbed per unit area of the heat transfer fin using the following formula. [Formula] Moisture absorption per unit area of heat transfer fin [g / m 2 ]=(W s -W0) / A
[0068] [Difficulty in peeling] The measurement is performed in accordance with the Japanese Industrial Standard JIS-K5600-5-6. Specifically, the adsorbent layer of the heat transfer fin prepared in each of the following examples is first cut into a lattice shape with a cutter knife, and 100 square pieces with sides of 2 mm are formed on the adsorbent layer. These square pieces are attached with Cellophane Tape (registered trademark) CT-24S (width 24 mm), which is an adhesive tape manufactured by Nichiban Co., Ltd. Thereafter, the cellophane tape is peeled off at an angle of 60° to the heat transfer fin, and the state of the square pieces remaining on the substrate is evaluated according to the following criteria. [Evaluation Criteria] 0: The edges of the cut are completely smooth and there are no peeling marks on any of the grids. 1: Small separations of the coating at the intersections of cuts. The cross-cut area affected is not significantly more than 5%. 2: The coating has delaminated along the edges of cuts and / or at intersections. Clearly more than 5% but not more than 15% of the cross-cut area is affected. 3: The coating has partially or completely peeled off significantly along the edges of the cuts and / or has partially or completely peeled off various areas of the mesh. Cross-cut areas are affected by significantly more than 15% but not more than 35%. 4: The coating has partially or completely peeled off significantly along the edges of the cuts and / or has partially or completely peeled off in several sections. The cross-cut area is clearly more than 35% affected but not more than 65% affected. 5: When the degree of peeling exceeds classification 4. From the viewpoint of adhesion between the sorbent layer and the substrate, the above evaluation is preferably 0 to 1.
[0069] [Sorbent layer condition] The condition of the sorbent layer on the burred heat transfer fin is visually evaluated according to the following criteria. [Evaluation Criteria] ◎: The average number of cracks and peeling around the holes is 0 per hole (no cracks or peeling) ○: The average number of cracks and peeling points around the holes per hole is greater than 0 and less than 1. △: The average number of cracks and peeling points around the holes is more than 1 and less than 2 per hole. ×: The average number of cracks / peelings around the holes per hole exceeds 2.
[0070] [Amount of sorbent per unit volume] The amount of sorbent per unit volume is calculated by the following formula. [Formula] Amount of sorbent per unit volume [kg / m 3 ] = {(area of one heat transfer fin × coating amount per side × 2) × (sorbent ratio in coating amount)} / {area of one heat transfer fin × (thickness of substrate with corrosion-resistant film + distance between adjacent heat transfer fins)} = (amount of coating per side × 2 × sorbent ratio in amount of coating) / (thickness of substrate with corrosion-resistant film + distance between adjacent heat transfer fins)
[0071] [Moisture absorption performance of the sorptive heat exchange module] While 35°C brine is passed through the heat transfer tubes of the sorptive heat exchange module, air with a temperature of 35°C and an absolute humidity of 3.47 g / kg (relative humidity of 10%) is blown in at a speed of 1 m / s. After a steady state is reached, the circulation of the brine is stopped and the air being blown is simultaneously switched to air with a temperature of 35°C and an absolute humidity of 21.44 g / kg (relative humidity 60%), which is blown in at a speed of 1 m / s. From the start of blowing, sensors are used to continuously measure the absolute humidity difference and air volume between the air inlet and outlet of the sorptive heat exchange module, the amount of moisture absorption is calculated from these measurements, and the change in the accumulated amount of moisture absorption over time is observed.
[0072] [Example 1] 71 parts by weight of ADEKA RESIN (registered trademark) EPU-11F (epoxy equivalent: 280 g / eq), a urethane-modified bisphenol A-type epoxy resin manufactured by ADEKA CORPORATION, was diluted with 29 parts by weight of DENACOL (registered trademark) EX810 (epoxy equivalent: 113 g / eq, viscosity: 20 mPa·s, molecular weight: 174), an epoxy-based reactive diluent manufactured by Nagase ChemteX Corporation, and then methyl ethyl ketone (20 parts by weight) was added. Next, 133.3 parts by weight of Ecopod (registered trademark) HU-750P (total carboxyl group amount: 6.45 mmol / g, neutralization degree: 80%, weight average particle size: 30 μm, swelling ratio: 2.5 times), an organic polymer-based sorbent particle manufactured by Toyobo Co., Ltd., was added and dispersed by stirring. To this was added 33.3 parts by weight of polyamine jER Cure (registered trademark) LV11 (amine value: 545 mgKOH / g) manufactured by Mitsubishi Chemical Corporation to prepare a coating liquid. The coating amount per side of the coating solution after drying (i.e., the amount of the adsorbent layer carried) was 40 g / m on an aluminum fin material (plate thickness 0.1 mm, 255 mm x 45 mm) that had been treated with phosphoric acid chromate and then provided with a corrosion-resistant film containing epoxy resin. 2 The coating was then baked at 120°C for 60 minutes to obtain a heat transfer fin.
[0073] The obtained heat transfer fins were subjected to burring to create 20 circular holes with a diameter of 9.88 mm so that the distance between the fins when stacked would be 1.5 mm. Next, 120 of the obtained heat transfer fins were stacked and a copper heat transfer tube with an outer diameter of 9.52 mm was inserted into them to produce a sorptive heat exchange module as shown in Figure 1 according to a known method.
[0074] [Example 2] In Example 1, 61 parts by weight of ADEKA RESIN (registered trademark) EPU-1001 (epoxy equivalent: 220 g / eq), a chelate-modified bisphenol F type epoxy resin manufactured by ADEKA CORPORATION, was used as the epoxy resin, and 39 parts by weight of ADEKA Glysilol (registered trademark) ED523T (epoxy equivalent: 140 g / eq, viscosity: 15 mPa s, molecular weight: 216) manufactured by ADEKA CORPORATION was used as the reactive diluent. The coating amount per one side after drying of the coating liquid was 41 g / m 2 A heat transfer fin and a sorptive heat exchange module of Example 2 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0075] [Example 3] In Example 1, 66 parts by weight of EPU-1001 was used as the epoxy resin, and 34 parts by weight of EX810 was used as the reactive diluent. The coating amount per side after drying of the coating liquid was 40 g / m 2 A heat transfer fin and a sorptive heat exchange module of Example 3 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0076] [Example 4] In Example 1, 66.7 parts by weight of EPU-11F was used as the epoxy resin, and 33.3 parts by weight of ED523T was used as the reactive diluent. The coating amount per side after drying of the coating liquid was 39.5 g / m 2A heat transfer fin and a sorptive heat exchange module of Example 4 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0077] [Example 5] In Example 4, 25 parts by weight of LV11 was used as the polyamine, 166.7 parts by weight of HU-750P as the sorbent particles, and 50 parts by weight of methyl ethyl ketone were used, and the coating amount per side after drying of the coating liquid was 45 g / m 2 A heat transfer fin and a sorptive heat exchange module of Example 5 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0078] [Example 6] In Example 5, 166.5 parts by weight of HU-750P and 53.3 parts by weight of methyl ethyl ketone were used as the sorbent particles, and the coating amount per side after drying of the coating liquid was 39.5 g / m 2 The heat transfer fin and the sorptive heat exchange module of Example 6 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0079] [Example 7] In Example 6, the coating amount per side after drying of the coating liquid was 50.4 g / m 2 The heat transfer fin and the sorptive heat exchange module of Example 7 were obtained in the same manner except for applying the coating so as to give the following:
[0080] [Example 8] In Example 1, 50 parts by weight of Daitoclar (registered trademark) D6293 (amine value: 262 mgKOH / g), a modified aliphatic polyamine manufactured by Daito Sangyo Co., Ltd., were used as the polyamine, 150 parts by weight of HU-750P (pH 8) (total amount of carboxyl groups: 6.45 mmol / g, degree of neutralization: 65%, weight average particle size: 30 μm, swelling ratio: 2.0 times) were used as the sorbent particles, and 35.1 parts by weight of methyl ethyl ketone were used. The coating amount per one side after drying of the coating liquid was 40.5 g / m 2The heat transfer fin and the sorptive heat exchange module of Example 8 were obtained in the same manner, except that the coating was performed so that the pH of the dispersion was 8. Here, HU-750P (pH 8) is obtained by dispersing HU-750P in ion-exchanged water to prepare a dispersion, adding dilute nitric acid so that the pH of the dispersion becomes 8, and then filtering, washing with water, and drying.
[0081] [Example 9] In Example 1, 61 parts by weight of EPU-11F was used as the epoxy resin, 39 parts by weight of ED523T as the reactive diluent, 50 parts by weight of D6293 as the polyamine, 159.7 parts by weight of HU-750P as the sorbent particles, and 53.9 parts by weight of methyl ethyl ketone were used, and the coating amount per one side after drying of the coating liquid was 40.6 g / m 2 A heat transfer fin and a sorptive heat exchange module of Example 9 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0082] [Example 10] In Example 1, 133.3 parts by weight of HU-720SF (total carboxyl group amount: 6.45 mmol / g, neutralization degree: 65%, weight average particle size: 4 μm, swelling ratio: 2.5 times) which is a moisture absorptive and desorptive particle manufactured by Nippon Exlan Kogyo Co., Ltd. was used as the sorbent particles, and the coating amount per one side after drying of the coating liquid was 39.8 g / m 2 The heat transfer fin and the sorptive heat exchange module of Example 10 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0083] [Example 11] In Example 1, burring was performed so that the distance between the heat transfer fins when stacked was 1.2 mm, and the coating amount per side after drying of the coating liquid was 40.6 g / m 2 A heat transfer fin and a sorptive heat exchange module of Example 11 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0084] [Example 12] In Example 1, instead of HU-750P, organic polymer-based sorbent particles to which a basic polymer is added as disclosed in Example 1 of WO 2014 / 188908 (total amount of carboxyl groups: 6.6 mmol / g, degree of neutralization: 94%, weight average particle size: 40 μm, swelling ratio: 2.3 times) were used as the organic polymer-based sorbent particles, and the coating amount per one side after drying of the coating liquid was 45 g / m 2 The heat transfer fin and the sorptive heat exchange module of Example 12 were obtained in the same manner except that the coating was performed so that the above-mentioned organic polymer-based sorptive agent particles having the basic polymer added thereto were produced as follows.
[0085] 700 parts by weight of water was charged into a 2L reaction tank, and a mixture of 210 parts by weight of acrylonitrile and 90 parts by weight of divinylbenzene was additionally charged. While stirring the reaction tank, 3 parts by weight of ammonium persulfate (polymerization initiator) was added and dissolved. Then, the reaction tank was heated to 70°C and reacted for 3 hours. After the reaction was completed, the mixture was cooled to about 20°C while continuing to stir, and crosslinked acrylonitrile-based polymer particles with an average particle size of 40 μm were obtained. Next, 800 g of water, 100 g of NaOH, and 100 g of the crosslinked acrylonitrile-based polymer particles were charged into a 2L reaction tank, and a hydrolysis reaction was carried out at 90°C for 60 hours to obtain salt-type carboxyl group-containing particles. Furthermore, 900 g of water and 100 g of the salt-type carboxyl group-containing particles were charged into a 2 L reaction tank, and 0.5 g of polyethyleneimine (average molecular weight 70,000) was added with stirring to react at 50°C for 30 minutes. After that, washing and drying treatment were performed to obtain organic polymer-based sorbent particles with a basic polymer attached.
[0086] [Comparative Example 1] In Example 1, 50 parts by weight of D6293 was used as the polyamine, 150 parts by weight of HU-750P and 16.8 parts by weight of methyl ethyl ketone were used as the sorbent particles, and JIS A1050, which is industrially pure aluminum, was used as the aluminum plate. The coating amount per side after drying of the coating liquid was 40 g / m 2 A heat transfer fin and a sorptive heat exchange module of Comparative Example 1 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0087] [Comparative Example 2] In Example 1, 533.2 parts by weight of HU-750P and 70 parts by weight of methyl ethyl ketone were used as the sorbent particles, and the coating amount per side after drying of the coating liquid was 40.6 g / m 2 A heat transfer fin and a sorptive heat exchange module of Comparative Example 2 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0088] [Comparative Example 3] In Example 1, 90 parts by weight of HU-750P and 10 parts by weight of methyl ethyl ketone were used as the sorbent particles, and the coating amount per side after drying of the coating liquid was 39.7 g / m 2 A heat transfer fin and a sorptive heat exchange module of Comparative Example 3 were obtained in the same manner, except that the coating was performed so that the thickness of the coating film was 100 μm.
[0089] [Comparative Example 4] The aluminum fin material (plate thickness 0.1 mm, width 110 mm, length 360 mm) was treated with phosphoric acid chromate and provided with a corrosion-resistant film containing epoxy resin. The heat transfer fins obtained were subjected to burring processing with 20 circular holes having a diameter of 9.88 mm so that the interval between the heat transfer fins when stacked was 1.5 mm. Next, 120 sheets of the obtained heat transfer fins were stacked, and a copper heat transfer tube having an outer diameter of 9.52 mm was inserted into the stack, and a heat exchange module was produced according to a known method. The heat exchange module was immersed in the coating liquid prepared in Example 1, pulled up, and drained by blowing compressed air five times, and then baked at 120 ° C for 60 minutes to obtain a sorption-type heat exchange module of Comparative Example 4.
[0090] The heat transfer fins of each Example and Comparative Example were subjected to the above-mentioned evaluation test, and the results are shown in Table 1. In addition, Fig. 2 shows the change over time in the moisture absorption amount of the sorptive heat exchange modules of Examples 1 and 11 and Comparative Example 3.
[0091] [Table 1]
[0092] As shown in Table 1, the heat transfer fins described in each example all maintain the hygroscopicity of the adsorbent layer, are not easily peeled off, and hardly crack when burred. In addition, due to this property, in the sorptive heat exchange module of the present invention that employs such heat transfer fins, a heat transfer fin spacing of less than 2 mm, which is narrower than conventional fin spacing, can be achieved without clogging, and the amount of adsorbent per unit volume can be increased, and as shown in Figure 2, more moisture can be removed from the air when the air temperature, humidity, and amount are all the same.
Claims
1. A sorptive heat exchange module including a plurality of heat transfer fins each having a sorptive layer thereon and a heat transfer tube penetrating the plurality of heat transfer fins, The heat transfer fins each have a corrosion-resistant film containing an epoxy resin provided on a surface of a metal plate having excellent thermal conductivity, and a sorbent layer is provided on the corrosion-resistant film, the sorbent layer containing sorbent particles made of an organic polymer having a carboxyl group, and a binder made of polyamine, a reactive diluent having two or more epoxy groups, and an epoxy resin; The organic polymer has a carboxyl group content of 3 to 10 mmol / g and a neutralization degree of 60 to 100%, and 30 to 110 parts by weight of the binder is used per 100 parts by weight of the sorbent particles, and the total amount of the sorbent particles and the binder is 20 to 80 g / m per one side of the metal plate surface. 2 It is supported, The sorptive heat exchange module further comprises: a heat exchanger module that is provided with a heat exchanger that is disposed between adjacent heat transfer fins and that is free of any blocking portion formed by a sorptive layer.
2. 2. The sorptive heat exchange module according to claim 1, wherein the distance between adjacent heat transfer fins is less than 2 mm.
3. The amount of sorbent per unit volume is 20 to 60 kg / m 3 2. The sorptive heat exchange module according to claim 1,
4. A dehumidification system using the sorptive heat exchange module according to any one of claims 1 to 3.
5. 4. A method for manufacturing a sorptive heat exchange module according to any one of claims 1 to 3, comprising the steps of: providing a sorptive layer on a surface of a heat transfer fin provided with a corrosion-resistant film, the sorptive layer containing sorptive particles made of an organic polymer having a carboxyl group in its molecule, and a binder made of polyamine, a reactive diluent having two or more epoxy groups, and an epoxy resin; punching out holes in the heat transfer fin provided with the sorptive layer; and inserting heat transfer tubes into the holes.
Citation Information
Patent Citations
Dehumidifying air conditioner
JP1999262621A
Sorption type heat exchange module, and its manufacturing method
JP2006200850A
Heat transfer fin, and heat exchanger
JP2012077987A