Conductive composition
A conductive composition with specific acrylic monomers and additives improves flexibility and conductivity stability in electronic devices by using a polyhydric phenol derivative and polyisocyanate, addressing issues of air entrainment and prolonged curing times on high mesh screens.
Patent Information
- Application Number
- JP2023070640
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Conductive compositions using acrylic resin as a binder exhibit poor flexibility and increased conductivity loss due to air entrainment during screen printing on high mesh screens, especially when the time from printing to curing is prolonged, leading to reduced performance in flexible electronic devices.
A conductive composition comprising 20 to 100 mol% of structural units derived from a specific acrylic monomer, 0 to 80 mol% of a copolymerizable monomer, a polyhydric phenol derivative, conductive particles, and polyisocyanate, which enhances flexibility and stability over time, even when printed on high mesh screens and cured after a prolonged period.
The composition achieves flexible and conductive films with minimal conductivity change over time, suitable for electronic devices, even when printed on high mesh screens and cured after 2 hours, maintaining excellent conductivity and stability.
Smart Images

Figure 2024156295000001 
Figure 2024156295000002 
Figure 2024156295000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrically conductive composition. [Background technology]
[0002] In fields such as electronic component mounting, attention is being paid to a technology that uses conductive circuits formed by printing a conductive composition whose main component is conductive metal particles such as silver paste or copper paste using a method such as screen printing and then thermally curing the printed circuit board as an alternative to conductive circuits formed by patterning the copper foil, as typified by printed circuit boards, through etching.
[0003] This conductive composition generally contains conductive particles and a binder, and as the binder, a binder resin such as a polyester resin, a urethane resin, a phenolic resin, an epoxy resin, an acrylic resin, etc. Among them, an acrylic resin has an advantage that it is easy to design a binder resin that is endowed with various properties such as impact resistance, thermoplasticity, and photoreactivity depending on the monomer to be combined.
[0004] In recent years, with the development of the metaverse and other technologies, the substrates used in wearable devices are increasingly being made of highly flexible materials, such as polyurethane. On the other hand, it is generally believed that cured films of conductive compositions containing acrylic resins as binders are less flexible than those containing polyester resins or urethane resins as binders, and tend to break easily when bent.
[0005] Patent Document 1 discloses a specific acrylic binder resin, and a conductive composition containing the acrylic binder resin, an organic solvent, and metal particles. It is said that a coating film formed on a copper foil surface using the conductive composition is prevented from peeling off from the copper foil after a mandrel test in which the coating film is bent under specific conditions, and the cured product of the coating film has excellent conductivity. However, there is no disclosure regarding the characteristics of the cured product of the coating film when it is bent.
[0006] In addition, in conductive circuits formed by screen printing from a conductive composition, the printed wiring is becoming thinner as various devices such as wearable devices become more multifunctional, and fine screen plates with meshes of 400 to 500 are used for printing. However, when wiring is printed using a conductive composition (paste) containing an acrylic binder resin with a fine screen plate, the amount of air entrained is greater than with other binder resins, which poses a problem that the metal particles in the cured film after printing may be oxidized, resulting in a decrease in conductivity.
[0007] In addition, it is desirable to heat and cure the printed conductive composition immediately, but in reality, when curing in a batch furnace, it is normal to cure all at once after a certain number of printed sheets have been produced. Therefore, the printed material is left in the atmosphere for about two hours until printing is completed. On the other hand, the printed conductive composition is partially denatured due to the drying of the solvent and exposure to oxygen from the air or air entrained during printing of the binder resin, and a dry-solidified film is formed on the surface of the printed material. If the surface is dried and cured by heating, the volatilization of the solvent in the printed film is hindered, causing many voids in the printed film, which can cause a significant decrease in the conductivity of the cured material. This problem is particularly likely to occur when printing with a fine mesh, as mentioned above, as there is a lot of oxygen entrainment.
[0008] Although it is not used for forming a conductive circuit, Patent Document 2 describes a screen printing ink containing a binder resin including a vinyl chloride copolymer resin and a specific acrylic resin, and an organic solvent including a cyclic ketone organic solvent. It also describes that this screen printing ink can be blended with organic / inorganic pigments, defoamers, leveling agents, and other additives. It is said that such a screen printing ink can provide a printed matter with excellent stability over time at room temperature. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2020-128451 A [Patent Document 2] JP 2022-130777 A Summary of the Invention [Problem to be solved by the invention]
[0010] It was found that the conductive composition containing the binder resin described in Patent Document 1 has good adhesion between the paste and copper foil when folded, but the flexibility of the cured film needs improvement in order to be applied to highly flexible substrates such as wearable devices. Patent Document 2 also describes the use of a defoamer in a screen printing ink containing a specific acrylic resin, but it was confirmed that it is difficult to suppress the influence of air entrained when the paste passes through the screen plate and to suppress the decrease in conductivity, as described above. Furthermore, Patent Documents 1 and 2 do not disclose the decrease in conductivity of the cured film when the screen print is left in the air.
[0011] Thus, even when an acrylic resin is used as a binder, there is currently no conductive composition that produces a cured film that has flexibility, that exhibits conductivity suitable for use in electronic devices even when printed with a high-mesh screen, and that exhibits little change in conductivity even when a long period of time passes between printing and curing, and that has excellent stability over time after printing.
[0012] Therefore, an object of the present invention is to provide a conductive composition that uses an acrylic resin as a binder, which produces a cured film that has flexibility, and which exhibits conductivity that is suitable for use in electronic devices even when printed with a high-mesh screen, and which exhibits little change in conductivity even when a long period of time passes between printing and curing, thereby exhibiting excellent stability over time after printing. [Means for solving the problem]
[0013] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by a conductive composition having a specific composition, and have completed the present invention. That is, the present invention relates to the following conductive composition.
[0014] (A) 5 to 30 mass% of a polymer which is composed of 20 to 100 mol% of structural units derived from a monomer (a1) represented by the following formula (1) and 0 to 80 mol% of structural units derived from a monomer (a2) copolymerizable with the monomer (a1), and has a weight average molecular weight of 1,000 to 1,000,000, (B) 0.1 to 20 mass% of a polyhydric phenol derivative represented by the following formula (2): (C) Conductive particles 50-94% by mass, (D) 0.5 to 20 mass% polyisocyanate, A conductive composition comprising:
[0015] [ka]
[0016] (In formula (1), R 1 is a hydrogen atom or a methyl group, R 2 is a single bond, an amide group, or an ester group.
[0017] [ka]
[0018] (In formula (2), R 3 ~R 7 are each independently a hydrogen atom, a hydroxyl group, or a hydrocarbon group having 1 to 6 carbon atoms, and at least one of them is a hydroxyl group.) Effect of the Invention
[0019] According to the present invention, it is possible to provide a conductive composition using an acrylic resin as a binder, which gives a cured film having flexibility, exhibits conductivity suitable for electronic devices even when printed using a high-mesh screen, and exhibits little change in conductivity even when a long time passes between printing and curing, resulting in excellent stability over time after printing. The effects of the present invention are particularly pronounced when printing using a high-mesh screen having a mesh number of 300 or more. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto. In this specification, a numerical range defined using the symbol "to" includes both the upper and lower limits of the symbol "to". For example, "2 to 5" means 2 or more and 5 or less. Furthermore, when a concentration or amount is specified, any higher concentration or amount can be associated with any lower concentration or amount. For example, when "2 to 10% by mass" and "preferably 4 to 8% by mass" are stated, the descriptions "2 to 4% by mass", "2 to 8% by mass", "4 to 10% by mass", and "8 to 10% by mass" are also included.
[0021] The conductive composition according to an embodiment of the present invention contains (A) 5 to 30 mass % of a polymer which is composed of 20 to 100 mol % of structural units derived from monomer (a1) represented by formula (1) below and 0 to 80 mol % of structural units derived from monomer (a2) copolymerizable with monomer (a1), and has a weight average molecular weight of 1,000 to 1,000,000, (B) 0.1 to 20 mass % of a polyhydric phenol derivative represented by formula (2) below, (C) 50 to 94 mass % of conductive particles, and (D) 0.5 to 20 mass % of a polyisocyanate.
[0022] [ka]
[0023] (In formula (1), R 1 is a hydrogen atom or a methyl group, R 2is a single bond, an amide group, or an ester group.
[0024] [ka]
[0025] (In formula (2), R 3 ~R 7 are each independently a hydrogen atom, a hydroxyl group, or a hydrocarbon group having 1 to 6 carbon atoms, and at least one of them is a hydroxyl group.)
[0026] Each component contained in the conductive composition will be described below.
[0027] [Component (A): Polymer] The component (A) used in the embodiment of the present invention is a polymer (hereinafter, sometimes referred to as polymer (A)) that is composed of 20 to 100 mol % of structural units derived from the monomer (a1) represented by the above formula (1) and 0 to 80 mol % of structural units derived from the monomer (a2) copolymerizable with the monomer (a1), and has a weight average molecular weight of 1,000 to 1,000,000. This polymer (A) acts as a binder in the conductive composition according to the embodiment of the present invention.
[0028] The monomer (a1) is not particularly limited as long as it is a compound represented by formula (1). 1 R may be any of the above, but is preferably a methyl group from the viewpoint of hydrolysis resistance. 2 may be any of the above, but from the viewpoint of electrical conductivity, an ester group is preferred. Specific examples of the monomer (a1) include 4-hydroxyphenyl methacrylate, 4-hydroxystyrene, N-(4-hydroxyphenyl) methacrylamide, and 4-hydroxyphenyl acrylate. The compound represented by formula (1) may be used alone or in combination of two or more.
[0029] The polymer (A) may be a polymer composed of only the monomer (a1), or may be a copolymer of the monomer (a1) and a monomer (a2) copolymerizable therewith. By forming a copolymer with the monomer (a2), it is possible to impart properties based on the monomer (a2). The monomer (a2) is not particularly limited as long as it is a vinyl monomer copolymerizable with the monomer (a1), and examples of the monomer (a2) include known substances such as anionic and cationic ionic monomers, nonionic monomers, (meth)acrylic acid ester compounds, aromatic alkenyl compounds such as styrene, vinyl cyanide compounds, acrylamide compounds, vinyl esters, vinyl ethers, maleates, fumarates, and α-olefins. From the viewpoint of electrical conductivity, methacrylic acid ester compounds are preferred, and those having a primary hydroxyl group are preferred. Specific examples of methacrylic acid ester compounds include methyl methacrylate, hydroxyethyl methacrylate, polyethylene glycol monomethacrylate, polypropylene glycol monomethacrylate, and polyethylene glycol-tetramethylene glycol monomethacrylate. Monomer (a2) may be used alone or in combination of two or more. From the viewpoint of electrical conductivity, it is preferable to use at least one type having a primary hydroxyl group. In addition, the structure of monomer (a2) having a primary hydroxyl group is not particularly limited, but from the viewpoint of electrical conductivity during screen printing and stationary stability after screen printing, the linker part between the (meth)acrylic acid moiety and the hydroxyl group moiety preferably has 1 to 6 carbon atoms in the case of an alkylene skeleton, and preferably has 1 to 10 repeating units in the case of an alkylene oxide skeleton. Specifically, an ester of (meth)acrylic acid and a polyhydric alcohol having two or more hydroxyl groups including at least one primary hydroxyl group is preferred, and as the polyhydric alcohol, one having an alkylene skeleton or one having an alkylene oxide skeleton is more preferred, and in the case of an alkylene skeleton, one having 1 to 6 carbon atoms in the skeleton is more preferred, and in the case of an alkylene skeleton, one having 1 to 10 repeating units in the skeleton is even more preferred.
[0030] The molar percentages of the constituent units derived from the monomer (a1) and the monomer (a2) in the polymer (A) may be the above-mentioned respective ratios. That is, the constituent units derived from the monomer (a1) in the polymer (A) are 20 to 100 mol %, and the constituent units derived from the monomer (a2) are 0 to 80 mol %. The ratio of the constituent units derived from the monomers contained in the polymer (A) can be measured by GC / MS analysis. It can also be calculated from the blending ratio during synthesis. The preferred molar ratios of each constituent unit are 30 to 100 mol % of the monomer (a1) and 0 to 70 mol % of the monomer (a2). When the monomer (a2) is contained, the preferred molar ratios of each constituent unit are 30 to 80 mol % of the monomer (a1) and 20 to 70 mol % of the monomer (a2). If the molar ratio of the component (a2) is more than 80%, the dispersibility of the conductive particles decreases, and it may be difficult to obtain a cured film exhibiting excellent conductivity.
[0031] The polymer (A) may contain structural units derived from monomers other than the monomers (a1) and (a2). In this case, the content is preferably such that the physical properties are not impaired, and is, for example, preferably 0 to 40 mol % of the entire polymer (A).
[0032] The weight average molecular weight of the polymer (A) is 1,000 to 1,000,000, preferably 2,000 to 800,000, more preferably 3,000 to 300,000. If the weight average molecular weight of the polymer (A) is lower than 1,000, the strength and viscosity of the polymer (A) may be insufficient, and if the weight average molecular weight is higher than 1,000,000, the solvent solubility and printability may be reduced. The weight average molecular weight can be determined in terms of polystyrene using gel permeation chromatography (GPC).
[0033] When the polymer (A) is a copolymer, the copolymer may have a random or block structure, but is preferably a random copolymer.
[0034] The above-mentioned polymer (A) can be obtained, for example, by radical polymerization of a monomer solution containing the monomer (a1) or the monomer (a1) and the monomer (a2). The polymerization can be carried out by a known method. For example, solution polymerization, suspension polymerization, emulsion polymerization, etc. can be mentioned, but solution polymerization and suspension polymerization are preferred in terms of ease of adjusting the weight average molecular weight of the polymer (A) within the above-mentioned desired range. In the solution polymerization and suspension polymerization, for example, the above-mentioned monomer (a1) or the monomer (a1) and the monomer (a2) (including the case where other monomers are used as necessary) can be obtained by polymerizing the monomer (a1) in a polymerization solvent in the presence of a polymerization initiator under predetermined conditions.
[0035] The polymerization initiator usable in the above-mentioned radical polymerization can be a known one. For example, di(4-t-butylcyclohexyl)peroxydicarbonate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-butylperoxycarbonate, and other organic peroxides, and 2,2'-azobisisobutyronitrile, and other azo-based polymerization initiators can be mentioned. These polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used can be appropriately set according to the type and combination of monomers used, reaction conditions, and the like. When the polymerization initiator is added, for example, the entire amount may be charged at once, a part of the polymerization initiator may be charged at once and the rest may be dripped, or the entire amount may be dripped. In addition, it is preferable to drip the polymerization initiator together with the monomer, since it is easy to control the reaction, and it is also preferable to add the polymerization initiator after the monomer is dripped, since it is possible to reduce the remaining monomer.
[0036] In addition, in the radical polymerization, a chain transfer agent can be used as necessary. Known chain transfer agents can be used, and examples of such agents include mercaptans such as n-dodecyl mercaptan, lauryl mercaptan, thioglycolic acid, and octyl thioglycolate; mercaptocarboxylic acids and their esters such as mercaptoacetic acid and mercaptopropynic acid; mercaptoethanol; halogenated compounds; dimeric alpha-methylstyrene; and the like.
[0037] As the polymerization solvent usable in the solution polymerization, one capable of dissolving the monomer and the polymerization initiator can be used, and specific examples thereof include methanol, ethanol, 1-propanol, acetone, methyl ethyl ketone, propylene glycol monomethyl ether, etc. The concentration of all monomers (total amount) relative to the polymerization solvent is preferably 10 to 60% by mass, more preferably 20 to 50% by mass, from the viewpoints of adjusting the weight average molecular weight of the polymer (A) and controlling heat generation during the polymerization reaction.
[0038] The method of charging the monomers into a reaction vessel when reacting them by solution polymerization is not particularly limited, and for example, the entire amount may be charged at once, a portion may be charged at once and the remainder may be added dropwise, or the entire amount may be added dropwise. From the viewpoint of ease of controlling heat generation, it is preferable to charge a portion at once and the remainder may be added dropwise, or to add the entire amount dropwise.
[0039] The polymerization temperature can be appropriately set depending on the type of polymerization solvent, and is, for example, 50° C. to 110° C. The polymerization time can be appropriately set depending on the type of polymerization initiator and the polymerization temperature. For example, when di(4-t-butylcyclohexyl)peroxydicarbonate is used as the polymerization initiator, the polymerization temperature is set to 70° C., and the polymerization time is suitably about 6 hours.
[0040] The content of component (A) is 5 to 30 mass% based on the solid content in the conductive composition, and preferably 5 to 20 mass%. If the content of component (A) is less than 5 mass%, the conductive composition tends to have a problem of not being fluid enough when printed, resulting in blurring during printing. If the content of component (A) is more than 30 mass%, the conductive particles of component (C) in the conductive composition are less likely to come into contact with each other, and a cured film exhibiting excellent conductivity may not be obtained.
[0041] [Component (B): Polyphenol derivative] The component (B) used in the embodiment of the present invention is a polyhydric phenol derivative represented by the above formula (2) (hereinafter, may be simply referred to as "polyhydric phenol derivative"). The polyhydric phenol derivative is represented by the formula (2) R 3 ~R 7 may be any of the above and at least one of them may be a hydroxyl group. From the viewpoint of electrical conductivity and rate of change of electrical conductivity, the more hydroxyl groups there are, the better. On the other hand, from the viewpoint of printability, in the case of a printing plate with a high mesh number, a large number of hydroxyl groups increases the viscosity and causes clogging. 3 ~R 7 The number of hydroxyl groups in the hydroxyl group is preferably 1 to 3, and more preferably 2. The substitution site of the hydroxyl group is not particularly limited, but from the viewpoint of the electrical conductivity and the rate of change in electrical conductivity, the ortho position (i.e., R 3 and R 7 ) rather than the para-position (i.e. R 5 ) is preferably introduced.
[0042] The hydrocarbon group having 1 to 6 carbon atoms is not particularly limited and can be appropriately selected. From the viewpoint of electrical conductivity and rate of change of electrical conductivity, the number of carbon atoms in the hydrocarbon group is preferably small, and is preferably 1 to 3. Examples of the hydrocarbon group include an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. When the aliphatic hydrocarbon group has 2 or more carbon atoms, it may be saturated or unsaturated, and when the aliphatic hydrocarbon group has 3 or more carbon atoms, it may be linear or branched. Of these, from the viewpoint of electrical conductivity and rate of change of electrical conductivity, an aliphatic hydrocarbon group is preferred. The substitution site of the hydrocarbon group having 1 to 6 carbon atoms is not particularly limited, but it is preferable that the ortho position (i.e., R 3 and R 7 From the viewpoint of the electrical conductivity and the rate of change of the electrical conductivity, the number of substitutions is preferably small, and is preferably 0 or 1.
[0043] Specific examples of polyhydric phenol derivatives include pyrogallol, 1,2-dihydroxybenzene, 1,3-dihydroxybenzene, 1,4-dihydroxybenzene, 2,5-dihydroxytoluene, tert-butylhydroquinone, 2,5-dihydroxy-m-xylene, 2,5-di-tert-butylhydroquinone, 1,2,3-trihydroxybenzene, and 1,2,4-trihydroxybenzene.
[0044] The content of the polyhydric phenol derivative in the conductive composition may be 0.1 to 20 mass % based on the solid content, but from the viewpoint of suppressing drying of the surface of the coating film and improving flexibility, 0.3 to 18 mass % is preferable.
[0045] [Component (C): Conductive particles] The component (C) used in the embodiment of the present invention is a conductive particle, and inorganic conductive particles such as silver, nickel, gold, and copper can be used. From the viewpoint of conductivity, silver and copper are preferable, and from the viewpoint of migration resistance and use in a high applied voltage region such as driving a device, copper is preferable. The copper particles may be composed of only copper, but may further contain metals other than copper such as silver and platinum, metal oxides, and metal sulfides. When the copper particles further contain metals other than copper, metal oxides, and metal sulfides, the mass ratio of copper in the copper particles is preferably 50 mass% or more. In addition, the copper particles may have a shape in which a surface layer or protrusions are formed.
[0046] Although commercially available conductive particles may be used as they are, it is preferable to use surface-coated conductive particles whose surfaces are coated for the purpose of improving oxidation resistance, etc. Among them, it is preferable to use surface-coated conductive particles whose surfaces are coated with an amine compound, and it is more preferable to use surface-coated conductive particles whose surfaces are coated with an amine compound represented by the following formula (3).
[0047] [ka]
[0048] (In formula (3), m is an integer of 0 to 3, n is an integer of 0 to 2, and when n=0, m is any of 0 to 3, and when n=1 or n=2, m is any of 1 to 3.)
[0049] From the viewpoint of obtaining better oxidation resistance, it is preferable that the surface-coated conductive particles whose surfaces are coated with an amine compound such as the amine compound represented by the above formula (3) are further coated with an aliphatic monocarboxylic acid to form surface-coated conductive particles. As a result, the conductive particle surface is coated with a first coating layer formed with the amine compound and a second coating layer formed with the aliphatic monocarboxylic acid. Preferably, the first coating layer is formed on the conductive particle surface, and the second coating layer is formed on the first coating layer.
[0050] The aliphatic monocarboxylic acid forming the second coating layer is preferably an aliphatic monocarboxylic acid having a carbon number of 8 to 24. Examples of the aliphatic monocarboxylic acid include linear saturated aliphatic monocarboxylic acids, linear unsaturated aliphatic monocarboxylic acids, branched saturated aliphatic monocarboxylic acids, and branched unsaturated aliphatic monocarboxylic acids.
[0051] Examples of linear saturated aliphatic monocarboxylic acids having 8 to 24 carbon atoms include caprylic acid, pelargonic acid, capric acid, undecylic acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, nonadecylic acid, and arachidic acid. Examples of linear unsaturated aliphatic monocarboxylic acids having 8 to 24 carbon atoms include myristoleic acid, palmitoleic acid, petroselinic acid, and oleic acid. Examples of branched saturated aliphatic monocarboxylic acids having 8 to 24 carbon atoms include 2-ethylhexanoic acid. As the aliphatic monocarboxylic acids, one selected from the above compounds may be used alone, or two or more may be used in combination.
[0052] The method for producing the surface-coated conductive particles is not particularly limited. For example, the method for obtaining the surface-coated conductive particles whose surface is coated with an amine compound includes washing the conductive particles with an aqueous ammonium chloride solution, adding the washed conductive particles to a solution of an amine compound, and heating as required, or adding the conductive particles to a solution containing, for example, ammonium chloride and an amine compound, and heating as required.
[0053] As a method for producing the surface-coated conductive particles coated with a first coating layer formed by an amine compound and a second coating layer formed by an aliphatic monocarboxylic acid, for example, a method of adding the surface-coated conductive particles coated with an amine compound to a solution of an aliphatic monocarboxylic acid can be mentioned. After adding to the solution of the aliphatic monocarboxylic acid, heating may be performed as necessary.
[0054] The average particle size (D50) of the conductive particles is not particularly limited, but in order to enable the conductive composition containing the conductive particles as component (C) to be printed well by various printing methods such as dispenser printing and screen printing, it is preferable to control the average particle size (D50) of the conductive particles. Specifically, the average particle size (D50) of the conductive particles is preferably 5 nm to 20 μm, and more preferably 10 nm to 10 μm. The average particle size (D50) of the conductive particles can be measured by a laser diffraction / scattering type particle size distribution measuring device (for example, Microtrack MT3000II manufactured by Microtrack Bell Co., Ltd.).
[0055] The BET specific surface area of the conductive particles is 0.05 to 400 m 2 / g, and 0.1 to 200m 2 / g It is more preferable that the BET specific surface area of the conductive particles can be measured by a BET single point method using a specific surface area measuring device (for example, Monosorb, manufactured by Yuasa Ionics Co., Ltd.).
[0056] There are no particular limitations on the shape or aspect ratio (ratio of the long axis to the short axis) of the conductive particles, and various shapes such as spherical, polyhedral, flat, plate, flake, thin plate, rod, dendritic, fibrous, etc. The conductive particles may be used alone or in combination of two or more types selected from those differing in components, average particle size, shape, aspect ratio, etc.
[0057] The content of component (C) is 50 to 94 mass% based on the solid content in the conductive composition, and from the viewpoint of achieving both fluidity and conductivity, 55 to 94 mass% is preferable. If the content of component (C) is less than 50 mass%, it becomes difficult for the conductive particles to come into contact with each other during curing, and a cured film exhibiting excellent conductivity may not be obtained.
[0058] [Component (D): Polyisocyanate] The component (D) used in the embodiment of the present invention is a polyisocyanate. Examples of polyisocyanates include aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, and derivatives thereof, as well as compounds containing terminal isocyanate groups. From the viewpoint of flexibility of the cured film, aliphatic diisocyanates and derivatives thereof are preferred. Examples of derivatives include those which have been converted into biuret, isocyanurate, or adduct, but from the viewpoint of adhesion, those in which a part of the isocyanate forms a trimer and has an isocyanurate skeleton (triisocyanurate) are more preferred.
[0059] The polyisocyanate may also be blocked with a blocking agent. Blocking extends the usable time and also works favorably on print stability. Any blocking agent may be used as long as it contains active hydrogen (hydrogen bonded to oxygen, sulfur, or nitrogen) that reacts with isocyanate and the product is reversible, i.e., unblocked by heat. Representative blocking agents include oximes, lactams, phenols, active methylenes, pyrazoles, mercaptans, imidazoles, amines, imines, triazoles, hydroxylamines, and derivatives selected from aliphatic, alicyclic, or aromatic alkyl monoalcohols. Among them, pyrazoles have a relatively low dissociation temperature and work favorably on plastic substrates such as polyethylene terephthalate (PET) that cannot be heated to high temperatures. Examples of pyrazoles include 2,2-dimethylpyrazole and 3,5-dimethylpyrazole. An example of a commercially available polyisocyanate having an isocyanurate skeleton and three isocyanate groups derived from hexamethylene diisocyanate and blocked with 3,5-dimethylpyrazole is Duranate SBN-70D manufactured by Asahi Kasei Corporation, but is not limited thereto.
[0060] The polyisocyanates may be used alone or in combination of two or more. From the viewpoint of electrical conductivity, the content of component (D) is 0.5 to 20 mass %, preferably 1 to 18 mass %, more preferably 2 to 18 mass %, based on the solid content in the conductive composition.
[0061] [Other ingredients] In addition to the above components (A) to (D), the conductive composition according to the embodiment may contain various additives such as solvents, antioxidants, lubricants, dispersants, curing agents, curing accelerators, viscosity modifiers, foaming agents, and defoamers, as necessary, within the range that does not impair the effects of the present invention. The conductive composition may also contain impurities that may be inevitably mixed in from raw material components and equipment in the manufacturing process. When any of these components is contained, the content of the components in the conductive composition may be more than 0 mass% and 50 mass% or less, and preferably 30 mass% or less, based on the solid content. The content of the solvent will be described later.
[0062] (Antioxidants) The conductive composition according to the embodiment may contain an antioxidant for the purpose of maintaining the performance of each component during storage. The type of antioxidant is not particularly limited, and various antioxidants can be used depending on the application. For example, nitrogen-containing heterocyclic compounds such as 2,2-bipyridyl and 1,10-phenanthroline; Schiff bases such as N,N'-bis(salicylidene)ethylenediamine (generic name: Salen), N,N'-bis(salicylidene)-1,2-propanediamine, N,N'-bis(salicylidene)-1,3-propanediamine, and N,N'-bis(salicylidene)-1,2-phenylenediamine; 1,2-phenylenediamine, 1,3-phenylenediamine, 1,4-phenylenediamine, 2,5-dimethyl-1,4-phenylenediamine, etc. Examples of the antioxidant include, but are not limited to, aromatic diamines such as amine, 2,3,5,6-tetramethyl-1,4-phenylenediamine, N,N-dimethyl-1,4-phenylenediamine, N,N,N'N'-tetramethyl-1,4-phenylenediamine, and N,N'-diphenyl-1,4-phenylenediamine; p-methoxyphenol; ascorbic acids such as L-ascorbic acid, 6-O-palmitoyl-L-ascorbic acid, 6-O-stearoyl-L-ascorbic acid, and tetra-2-hexyldecanoic acid ascorbyl. The antioxidant may be used alone or in combination of two or more. When two or more types are used in combination, the mixing ratio is not particularly limited.
[0063] (solvent) The conductive composition according to the embodiment may contain a solvent for the purpose of improving the coatability and adjusting the viscosity. Examples of the solvent include ether alcohols such as ethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol monoethyl ether acetate, propylene glycol diacetate, dipropylene glycol monomethyl ether, ethylene glycol monobutyl ether acetate, triethylene glycol monomethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol, and dipropylene glycol; non-ether alcohols such as propylene glycol and 1,4-butanediol; esters such as cyclohexanol acetate, methyl methoxypropionate, ethyl ethoxypropionate, and 1,6-hexanediol acetate; ketones such as isophorone and cyclohexanone; terpenes such as terpineol, dihydroterpineol, dihydroterpinyl acetate, and isobornylcyclohexanol; and other hydrocarbons such as octane, decane, dodecane, tetradecane, hexadecane, and propylene carbonate, but are not limited thereto. The solvent may be used alone or in combination of two or more. When two or more types are used in combination, the mixing ratio is not particularly limited.
[0064] The type of solvent is preferably one or more selected from the above ether alcohols, esters, and terpenes. When two or more of these solvents are mixed, the mixing ratio is not particularly limited.
[0065] When the conductive composition according to the embodiment contains a solvent, the content of the solvent is preferably 1 to 30 mass % and more preferably 1 to 15 mass % in the entire conductive composition. In addition, when other components contain a solvent, this includes the solvent.
[0066] (lubricant) A lubricant may be appropriately added to the conductive composition according to the embodiment in order to adjust the dispersibility of the conductive particles of the component (C). Examples of the lubricant include fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid; fatty acid metal salts formed from metals such as sodium, potassium, barium, magnesium, calcium, aluminum, iron, cobalt, manganese, zinc, and tin and the fatty acids; fatty acid amides such as stearic acid amide, oleic acid amide, behenic acid amide, palmitic acid amide, and lauric acid amide; fatty acid esters such as butyl stearate; waxes such as paraffin wax and liquid paraffin; alcohols such as ethylene glycol and stearyl alcohol; polyethers made of polyethylene glycol, polypropylene glycol, and modified products thereof; polysiloxanes such as silicone oil; and fluorine compounds such as fluorine-based oil. The lubricant may be used alone or in combination of two or more kinds. When two or more kinds are used, the mixing ratio is not particularly limited. In the present invention, lauric acid is highly effective, and examples of commercially available products include, but are not limited to, NAA-122 manufactured by NOF Corporation.
[0067] Among these lubricants, from the viewpoint of dispersibility, it is preferable to use one or more types selected from fatty acids and fatty acid metal salts, and it is more preferable to use at least one type selected from magnesium stearate and lauric acid.
[0068] When the conductive composition according to the embodiment contains a lubricant, the content of the lubricant in the conductive composition is preferably 0.01 to 10 mass %, more preferably 0.1 to 5 mass %, and even more preferably 0.2 to 3 mass %, based on the solid content.
[0069] The conductive composition as described above can be obtained by mixing and kneading the above-mentioned components according to a standard method. The form of the conductive composition can be appropriately determined depending on the application, etc., and in particular, when a high-mesh screen plate (high-mesh plate) is used, a liquid form is preferable. In addition, a conductive cured film (metal film) can be obtained by heating a coating film formed according to a standard method using the conductive composition. The coating film can be formed by a known coating machine, and in the formation of a conductive circuit, patterning can be easily performed using various coating machines such as a die coater, an inkjet printer, a screen printing machine, a gravure offset printing machine, and a pad printing machine. In particular, a screen printing machine is capable of printing a thick film of 10 μm or more, and is suitable as a method requiring a highly conductive circuit. When applying by screen printing, the viscosity at 25 ° C. is preferably, for example, 500 mPa·s or more and 300 Pa·s or less. It is preferable that the composition is liquid and uniform at 25 ° C.
[0070] The conductive composition can form a cured film having flexibility that allows it to be applied to flexible substrates. The flexibility of the cured film can be evaluated by its 180° bending property, as described in the Examples section below.
[0071] By using the conductive composition, even if the printed matter is formed by screen printing using a high mesh screen plate such as 400 mesh, the cured film has good conductivity, and it is considered that air entrainment is suppressed even when an acrylic binder resin is used. This conductivity can be evaluated, for example, by the volume resistivity measured in the Examples section described later. From the viewpoint of driving a general electronic device, for example, the volume resistivity is preferably 100 μΩ·cm or less, more preferably 30 μΩ·cm or less.
[0072] By using the conductive composition described above, even if the printed matter is formed by screen printing using a high mesh screen such as 400 mesh, even if the time from printing to curing is long, 2 hours, the conductivity of the cured film is suppressed from decreasing compared to the cured film cured immediately after printing, and it is practically usable and has excellent stability over time after printing. The change in conductivity after standing for a long time can be evaluated by the change rate of volume resistivity measured in the Examples section described later. EXAMPLES
[0073] Hereinafter, the embodiments of the present invention will be described more specifically based on examples, but the present invention is not limited to these.
[0074] (Production Example 1: Production of Polymer 1) A 1L separable flask equipped with a stirrer, a thermometer, a condenser, a dropping funnel and a nitrogen inlet tube was charged with 100g of diethylene glycol monoethyl ether, and the atmosphere in the separable flask was replaced with nitrogen to create a nitrogen atmosphere. A monomer solution in which 280g of 4-hydroxyphenyl methacrylate (monomer (a1-1)) as monomer (a1) was dissolved in 277g of diethylene glycol monoethyl ether, and a polymerization initiator solution in which 43g of t-butyl peroxide carbonate was dissolved in 43g of diethylene glycol monoethyl ether were prepared. Next, the temperature in the separable flask was raised to 75°C, and the monomer solution and the polymerization initiator solution were simultaneously dropped over 2 hours. After that, the mixture was reacted at 75°C for 4 hours to obtain polymer 1.
[0075] (Production Example 2: Production of Polymer 2) Polymer 2 was obtained in the same manner as in Polymerization Example 1, except that 42 g of n-dodecyl mercaptan was added as a chain transfer agent.
[0076] (Production Example 3: Production of Polymer 3) Polymer 3 was obtained in the same manner as in Polymerization Example 2, except that the atmosphere in the separable flask was not replaced with nitrogen and the amount of t-butyl peroxide carbonate used was changed to 14 g.
[0077] (Production Examples 4 to 12: Production of Polymers 4 to 12) Polymers 4 to 12 were obtained in the same manner as in Example 1, except that monomer solutions prepared using monomer (a1) shown in Table 1 and monomer (a2) shown in Table 2 in the amounts shown in Table 3 were used.
[0078] (Measurement of weight average molecular weight) The weight average molecular weights of Copolymers 1 to 12 were determined by gel permeation chromatography (GPC) under the following conditions. The measurement results are shown in Table 3. Equipment: Tosoh Corporation, HLC-8220 Column: Shodex, LF-804 Standard material: polystyrene Eluent: THF (tetrahydrofuran) Flow rate: 1.0ml / min Column temperature: 40℃ Detector: RI (Differential Refractive Index Detector)
[0079] [Table 1]
[0080] [Table 2]
[0081] [Table 3]
[0082] (Production Example 13: Production of Surface-Treated Conductive Particles) An aqueous solution of ammonium chloride was prepared by dissolving 5 g of ammonium chloride in 100 g of water. Copper particles [Mitsui Mining & Smelting Co., Ltd. "1400YP"; particle size (D50) 6 μm, BET specific surface area 0.60 m 2 / g, Shape: Plate 2 μm, BET specific surface area 0.40 m 250 g of ammonium chloride solution (100 g / g, shape: spherical) was added to an aqueous ammonium chloride solution and stirred at 30°C for 60 minutes under nitrogen bubbling. Stirring was performed using a mechanical stirrer at a rotation speed of 150 rpm. The following stirring was performed at the same rotation speed using a similar stirring device. After stirring was completed, the copper particles were filtered out by vacuum filtration using a Kiriyama funnel with 5C filter paper, and then the copper particles were washed twice with 150 g of water on the Kiriyama funnel. The washed copper particles were added to 250 g of a 40% by mass aqueous solution of diethylenetriamine, and the mixture was heated and stirred at 60° C. for 1 hour while bubbling with nitrogen. After stopping the stirring and leaving it to stand for 5 minutes, about 200 g of the supernatant was removed. Next, 200 g of isopropanol was added to the precipitate as a cleaning solvent, and the mixture was stirred at 30° C. for 3 minutes. After stopping the stirring and leaving it to stand for 5 minutes, about 200 g of the supernatant was removed, and then 250 g of a 2% by mass lauric acid isopropanol solution was added, followed by stirring at 30° C. for 30 minutes. After the stirring was completed, the copper particles were filtered out by vacuum filtration using a Kiriyama funnel with 5C filter paper, and the obtained copper particles were dried under reduced pressure at 25° C. for 3 hours to obtain surface-treated copper particles.
[0083] Example 1 [Production of Conductive Composition] As component (A), 19.2 g (40% solids) of polymer 1 was used, as component (B), 4.8 g of 1,4-dihydroxybenzene (polyhydric phenol derivative (b-2)) was used as component (B) as shown in Table 4, 79.3 g of surface-coated copper particles from Production Example 13 was used as component (C), 7.1 g of blocked polyisocyanate [Asahi Kasei Corporation, Duranate SBN-70D, solids 70% by mass, solvent: dipropylene glycol monomethyl ether] was used as component (D), 2.0 g of lauric acid (NOF Corporation, NAA-122) was used as a lubricant, 1.3 g of N,N'-bis(salicylidene)ethylenediamine (Salen) was used as an antioxidant, and 2.0 g of diethylene glycol monoethyl ether acetate was used as a solvent. Next, the mixture was stirred at room temperature for 120 seconds at a rotation speed of 2000 rpm using a planetary mixer [Thinky Corporation, ARV-310], and primary kneading was performed. Next, a three-roll mill [EXAKT-M80S, Nagase Screen Printing Laboratory Co., Ltd.] was used to perform secondary mixing by passing the mixture five times at room temperature with a roll distance of 5 μm. The mixture obtained by the secondary mixing was stirred and degassed for 90 seconds at 1000 rpm under vacuum conditions at room temperature using a planetary mixer [ARV-310, Thinky Corporation] to produce a conductive composition. The composition of each component of the conductive composition (based on solid content) is shown in Table 5.
[0084] [180° bending ability of cured film] The obtained conductive composition was applied onto a release film using a metal mask in a size of 1 cm wide, 3 cm long, and 50 μm thick, and then cured on a hot plate at 150° C. for 30 minutes. The cured film peeled off from the release film was folded 180° along a curved surface with R=1φmm, and the folding property was evaluated according to the following evaluation criteria. ◎: No breaks, no bending marks ○: No breakage, bending marks remain ×: Breakage present
[0085] (Conductivity of the cured film from 400 mesh screen printing) The obtained conductive composition was printed on a PET substrate using a 400 mesh screen (400 mesh) as a 2.5 cm square solid film with a wet target film thickness of 30 μm using a screen printer (Micro-Tech Co., Ltd., MT-320T). The obtained print was immediately heated in a convection oven at 150° C. for 30 minutes under atmospheric pressure to obtain a cured film. The volume resistivity of the cured film was measured using a low resistivity meter (Nitto Seiko Analytech Co., Ltd., Loresta-GP MCP-T610), and the conductivity of the cured film was evaluated according to the following evaluation criteria. The smaller the volume resistivity value, the easier it is for current to flow through the cured film, indicating superior conductivity. ◎: The volume resistivity value is less than 50 μΩ·cm. ○: The volume resistivity value is 50 μΩ·cm or more and less than 100 μΩ·cm. ×: The volume resistivity value is 100 μΩ·cm or more.
[0086] (Stability of 400 mesh screen prints over time) A cured film was prepared in the same manner as in the above-mentioned "Conductivity of the cured film of 400 mesh screen printing" except that the printed matter was left to stand in the air for 2 hours at 23°C and then heated, and its volume resistivity was measured. The volume resistivity of the cured film left to stand for 2 hours (volume resistivity after standing for 2 hours) and the volume resistivity of the cured film cured without standing in the same manner as in the above-mentioned "Conductivity of the cured film of 400 mesh screen printing" (volume resistivity without standing) were used to evaluate the increase rate using the following formula (A). The smaller the increase rate, the smaller the change, and the stability over time of the printed matter (paste film) was evaluated according to the following criteria.
[0087]
number
[0088] ◎: Increase rate ≦30% ○:30<Increase rate≦100 ×:100<increase rate
[0089] (Examples 2 to 19, Comparative Examples 1 to 3) A conductive composition was produced, and a cured film was formed and evaluated in the same manner as in Example 1, except that the component (B) shown in Table 4 was used and the composition of each component was as shown in Tables 5 to 7. The evaluation results are shown in Tables 5 to 7.
[0090] [Table 4]
[0091] [Table 5]
[0092] [Table 6]
[0093] [Table 7]
[0094] In Examples 1 to 19, the cured films were bent at 180° without any breakage and had sufficient flexibility. Additionally, the volume resistivity of the cured films of the 400-mesh screen-printed products was all 32-85 μΩ·cm, less than 100 μΩ·cm, proving that they have good conductivity suitable for use in a variety of electronic devices. Furthermore, after screen-printing using the 400-mesh screen, the prints were left to stand for two hours, and then the cured films showed an increase in volume resistivity of 15-65%, all of which were less than 100%, compared to those cured immediately after printing, proving that they have stability over time suitable for practical production. On the other hand, Comparative Example 1 does not contain polyhydric phenol derivative (B), so the bendability of the cured film after screen printing on a 400 mesh plate is poor, and the conductivity of the cured film cured after leaving the printed material still for 2 hours does not meet the requirements. In Comparative Example 2, the polymer (A) used does not contain monomer (a1) represented by the formula (1), and the 180° bendability of the cured film, the conductivity of the cured film of the 400 mesh screen printing film, and the conductivity of the cured film cured after leaving the printed material still for 2 hours do not meet the requirements. Comparative Example 3 does not contain polymer (A), and although the bendability of the cured film is excellent, the conductivity of the cured film of the 400 mesh screen printing film and the conductivity of the cured film cured after leaving the printed material still for 2 hours do not meet the requirements.
Claims
[Claim 1] (A) 5 to 30 mass% of a polymer which is composed of 20 to 100 mol% of structural units derived from a monomer (a1) represented by the following formula (1) and 0 to 80 mol% of structural units derived from a monomer (a2) copolymerizable with the monomer (a1), and has a weight average molecular weight of 1,000 to 1,000,000: (B) 0.1 to 20% by mass of a polyhydric phenol derivative represented by the following formula (2), (C) conductive particles 50 to 94% by mass, (D) polyisocyanate 0.5 to 20 mass% A conductive composition comprising: [Formula 1] (In formula (1), R 1 is a hydrogen atom or a methyl group, R 2 is a single bond, an amide group, or an ester group. [chemical 2] (In formula (2), R 3 ~R 7 are each independently a hydrogen atom, a hydroxyl group, or a hydrocarbon group having 1 to 6 carbon atoms, and at least one of them is a hydroxyl group.
Citation Information
Patent Citations
Binder resin and conductive paste composition
JP2020128451A
Ink for screen printing and printed matter
JP2022130777A