Preparation method for specimen for observing polymer material and observation method for polymer material
By thinly slicing polymeric materials into a weakly crosslinked state and using a scanning transmission electron microscope, the method allows for direct observation of molecular chains and atoms, addressing the limitations of existing observation methods.
Patent Information
- Application Number
- JP2023070699
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Existing observation methods for polymeric materials, such as vulcanized rubber, do not allow for direct observation of molecular chains and atomic states, limiting understanding of their physical properties.
Prepare specimens by thinly slicing polymeric materials into a weakly crosslinked state with specific crosslinking densities and thicknesses, using a scanning transmission electron microscope to acquire image data that clearly shows molecular chains and atoms.
Enables direct visualization and understanding of molecular chains and atomic states in polymeric materials, enhancing the analysis of their physical properties.
Smart Images

Figure 2024156327000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for preparing a specimen for observation of a polymeric material and a method for observing a polymeric material, and more particularly to a method for preparing a specimen for observation of a polymeric material and a method for observing a polymeric material, which enable direct observation of the state of molecular chains and atoms that constitute the polymeric material. [Background technology]
[0002] It is known that the physical properties of cross-linked polymeric materials such as vulcanized rubber are affected by the state (structure) of the molecular chains that make up the polymeric material. If it were possible to directly observe the state of the molecular chains and atoms of polymeric materials, it would be possible to make great advances in understanding and analyzing the physical properties of cross-linked polymeric materials.
[0003] Conventionally, various observation methods have been proposed for observing the dispersion state of fillers contained in rubber materials using a scanning transmission electron microscope (see Patent Documents 1 and 2). In the proposed observation methods, the three-dimensional structure of a rubber material with a thickness of 200 to 1500 nm is reconstructed by a tomography method. In the three-dimensional image obtained by this observation method, a high-order aggregation structure in which molecular chains of many rubber components (polymers) and particles constituting the filler are aggregated together can be confirmed. However, this observation method does not directly observe the molecular chains or atomic state of polymers. Therefore, there is room for improvement in directly observing the molecular chains and atomic state of polymer materials. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5767477 [Patent Document 1] JP 2013-44607 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a method for preparing a specimen for observation of a polymeric material, which allows direct observation of the molecular chains and atomic state of the polymeric material, and a method for observing the polymeric material. [Means for solving the problem]
[0006] The method for preparing specimens for observation of polymeric materials of the present invention, which achieves the above-mentioned object, comprises slicing a polymeric material in a predetermined crosslinked state into thin pieces to prepare specimens for observation with a scanning transmission electron microscope, the method comprising: preparing samples of the polymeric material, which has been made weakly crosslinked by varying the crosslinking density into a plurality of different thicknesses; obtaining image data of each of the samples under the same predetermined settings with the scanning transmission electron microscope; and setting in advance a crosslinking density reference range and a thickness reference range for the polymeric material, the respective ranges of the crosslinking density and thickness of the samples within which the clarity of the molecular chains or atoms of the polymeric material in each of the obtained image data is within an acceptable range; and preparing a specimen for observation of the polymeric material, the polymeric material is made weakly crosslinked in the crosslinking density reference range, and the weakly crosslinked polymeric material is sliced to a thickness in the thickness reference range.
[0007] The method for observing a polymeric material of the present invention, which achieves the above-mentioned object, comprises using a scanning transmission electron microscope to obtain image data of an observation specimen obtained by slicing a polymeric material in a predetermined crosslinked state into a thin piece, wherein the polymeric material is rendered into a weakly crosslinked state having a crosslink density within a preset crosslink density standard range, and sliced to a thickness of 1 nm or more and 50 nm or less to be used as the observation specimen, and the state of the molecular chains or atoms of the polymeric material is observed in the image data of the observation specimen obtained using the scanning transmission electron microscope. Effect of the Invention
[0008] According to the method for preparing a specimen for observation of a polymeric material of the present invention, when preparing a specimen for observation of the polymeric material, the polymeric material is weakly crosslinked within the preset crosslink density reference range, and the weakly crosslinked polymeric material is sliced to a thickness within the preset thickness reference range, so that the state of the molecular chains or atoms of the polymeric material can be visually confirmed in the image data of the specimen for observation obtained using a scanning transmission electron microscope, which is advantageous for directly observing and understanding the state of the molecular chains or atoms.
[0009] According to the method for observing a polymeric material of the present invention, the polymeric material is sliced into ultra-thin pieces of 1 nm to 50 nm in a weakly crosslinked state with a crosslink density in a preset crosslink density reference range, and used as the specimen for observation. Therefore, the image data of the specimen for observation obtained using a scanning transmission electron microscope makes it possible to visually confirm the state of molecular chains or atoms of the polymeric material, which is advantageous for directly observing and understanding the state of the molecular chains or atoms. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is an explanatory diagram illustrating an observation system. [Diagram 2] FIG. 1 is an explanatory diagram illustrating a scanning transmission electron microscope. [Diagram 3] FIG. 1 is a flow diagram illustrating the steps of an embodiment of a method for preparing a specimen for observation of a polymer material. [Figure 4] FIG. 1 is a flow chart illustrating the steps of an embodiment of a method for observing a polymer material. [Diagram 5] FIG. 11 is an explanatory diagram illustrating an example of dark-field image data. [Figure 6] FIG. 11 is an explanatory diagram illustrating an example of dark-field image data. [Figure 7] FIG. 1 is an explanatory diagram illustrating bright-field image data. [Figure 8] FIG. 2 is an explanatory diagram illustrating an example of model data. [Figure 9] FIG. 11 is an explanatory diagram illustrating image data generated from dark-field image data. [Figure 10]FIG. 11 is an explanatory diagram illustrating an example of image data generated from bright-field image data. [Figure 11] FIG. 11 is an explanatory diagram illustrating image data generated from dark-field image data. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a method for preparing a specimen for observation of a polymer material and a method for observing a polymer material according to the present invention will be described based on the embodiments shown in the drawings.
[0012] The observation system 1 illustrated in Fig. 1 is used to carry out an embodiment of a method for observing polymeric materials such as rubber and elastomers. In this observation method, image data D1 acquired by a scanning transmission electron microscope 2 (hereinafter referred to as microscope 2) is used to directly observe molecular chains and atoms of a specimen 10 for observation of a polymeric material (hereinafter referred to as specimen 10). In this observation method, a specimen 10 prepared by an embodiment of a method for preparing a specimen for observation of a polymeric material can be used.
[0013] First, the observation system 1 will be described in detail.
[0014] The observation system 1 includes a microscope 2 and a computing device 3. The computing device 3 can be any of various known computers. The computing device 3 includes a central processing unit (CPU), a main storage unit (memory), an auxiliary storage unit (e.g., HDD), an input unit (keyboard, mouse), and an output unit (display). The auxiliary storage unit of the computing device 3 stores image data D1 acquired using the scanning transmission electron microscope 2 and an image simulator D2 (a program that executes an image simulation to generate the image data D1).
[0015] 2 irradiates an electron beam onto a specimen 10, and acquires dark-field image (HAADF-STEM image, LAADF-STEM image) data D1a and bright-field image (BF-STEM image) data D1b, which enable observation of the spatial distribution of electron transmittance inside the specimen 10 from the intensity of the transmitted electron beam. Image data D1 is generated from the dark-field image data D1a and bright-field image data D1b acquired by the microscope 2 by execution of an image simulator D2 by the computing device 3, and the generated image data D1 is stored in an auxiliary storage unit of the computing device 3.
[0016] The microscope 2 may be any of various known scanning transmission electron microscopes, but is preferably one incorporating a spherical aberration corrector 6. Specifically, the microscope 2 has an electron gun 4, a condenser lens 5, a spherical aberration corrector (concave lens) 6, an objective lens (convex lens) 7, and a detector 8 (DF detector 8a and BF detector 8b). By having the spherical aberration corrector 6, the microscope 2 can have a smaller resolution, which is advantageous for identifying structures at the single-atom level and for improving the accuracy of identifying elements.
[0017] The detector 8 is composed of a DF (dark field) detector 8a and a BF (bright field) detector 8b, and the detector 8 acquires dark field image data D1a and bright field image data D1b. The detector 8 may be composed of only one of the DF detector 8a and the BF detector 8b. By configuring the detector 8 with both the DF detector 8a and the BF detector 8b, it becomes possible to simultaneously acquire both the dark field image data D1a and the bright field image data D1b.
[0018] The DF detector 8a has a circular ring shape in a top view and detects electrons scattered at a high angle. The acceptance angle of the DF detector 8a (the scattering angle of detectable electrons) is, for example, more than 20 mrad and not more than 200 mrad. The DF detector 8a can also be composed of two circular ring-shaped detectors, one large and one small, in which case the larger diameter detector is placed above the smaller diameter detector. The acceptance angle of the larger diameter detector placed at the top is, for example, more than 90 mrad and not more than 200 mrad, and the acceptance angle of the smaller diameter detector placed at the bottom is, for example, more than 20 mrad and not more than 90 mrad.
[0019] The BF detector 8b has a disk shape in a top view, and detects electrons that have passed through the specimen 10 and electrons that have been scattered at small angles. The acceptance angle of the BF detector 8b is, for example, 20 mrad or less. The BF detector 8b can also be configured with two detectors, a detector that is annular in a top view and a detector that is disk-shaped in a top view, in which case the acceptance angle of the annular detector is, for example, more than 10 mrad and 20 mrad or less, and the acceptance angle of the disk-shaped detector is, for example, 10 mrad or less.
[0020] Next, a method for preparing the specimen 10 will be described in detail.
[0021] 3 shows an example of the steps of a method for producing specimen 10. In this method, a polymer material is put into a weakly cross-linked state within a preset cross-link density standard range (S110), and the weakly cross-linked polymer material is sliced to a thickness within a preset thickness standard range (S120). The sliced ultra-thin piece becomes specimen 10. Each step (S110, S120) will be described in detail below.
[0022] In step (S110), a polymer material in a weakly crosslinked state is prepared within a preset crosslink density reference range. The crosslink density reference range will be described later. A weakly crosslinked polymer material is obtained by carrying out known processes including a mixing process for mixing raw materials required for the polymer material and a crosslinking process for crosslinking the uncrosslinked polymer material that has been through the mixing process.
[0023] The rubber component (polymer) that is the raw material of the specimen 10 may be any rubber component that can be crosslinked by a crosslinking agent (vulcanizing agent), and examples of such rubber include natural rubber (NR) and synthetic rubbers such as styrene-butadiene rubber (SBR), butadiene rubber (BR), and isoprene rubber (IR). The crosslinking agent may be any agent that can crosslink polymer molecular chains, and examples of such agents include organic peroxides such as sulfur and peroxide. The raw material of the specimen 10 may contain additives other than the crosslinking agent, such as crosslinking accelerators (vulcanization accelerators), fillers (silica, carbon black, etc.), antioxidants, flame retardants, reinforcing materials, and colorants.
[0024] A weakly crosslinked state is a state in which the degree of crosslinking is weaker (low crosslink density state) than the crosslinked state of a polymer material of normal specifications. The degree of crosslinking can be determined, for example, based on the value of crosslink density, and in a weakly crosslinked state, the value of crosslink density is smaller than that of a crosslinked state of normal specifications. In this step (S110), a polymer material in a weakly crosslinked state may be produced by appropriately setting the blending amounts of raw materials and the conditions of the mixing process and crosslinking process so that the crosslink density falls within the crosslink density reference range. A weakly crosslinked state can be easily achieved by reducing the blending amount of crosslinking agent compared to the case of normal specifications while keeping the manufacturing conditions (conditions of the mixing process and crosslinking process) the same as those for producing a polymer material of normal specifications. The range of crosslinking density that can be said to be a weakly crosslinked state varies slightly depending on the type of polymer material, but is, for example, 1.0×10 -6 mol / cm 3 ~1.0×10 -4 mol / cm 3 The range is slightly wider than this, including
[0025] To check whether the prepared polymeric material is in a weakly crosslinked state within a preset crosslink density standard range, the crosslink density of the prepared polymeric material is measured, and it is judged whether the measurement result satisfies the crosslink density standard range. The crosslink density can be measured by a known measurement method such as the equilibrium lubrication method using the modified Flory-Rehener or the swelling compression method using Flory's logical formula. When measuring the crosslink density, multiple parts of the prepared polymeric material are sampled, and the representative value (average value, median value, etc.) of the crosslink density of each part is used as the crosslink density. When sampling each part, it is preferable to sample from a position that exhibits a representative crosslinked state in a wide range by setting the magnification of the microscope 2 to a lower magnification than when acquiring the image data D1 described later. This allows the polymeric material to eliminate parts that are obviously in a heterogeneous crosslinked state.
[0026] In the next step (S120), the weakly crosslinked polymer material having a predetermined crosslink density standard range is sliced to a thickness within a predetermined thickness standard range. The thickness standard range will be described later. For this slicing, for example, a known ultramicrotome is used.
[0027] The above-mentioned crosslink density standard range and thickness standard range are grasped by conducting tests in advance. This test can be conducted for each type of polymer material, but if the polymer materials are of the same type, it is sufficient to conduct the test for one representative type and apply the test results to the polymer materials of the same type. For example, if the main polymer type of rubber is the same or the main polymer type of resin is the same, this test is conducted for one representative type of the same type. Alternatively, a crosslink density standard range and thickness standard range that can be applied to the majority of types of polymer materials may be set based on the test results conducted for multiple different types of polymer materials.
[0028] In the test for setting the crosslink density standard range and the thickness standard range, the polymer material to be tested is prepared in a weakly crosslinked state with a plurality of different crosslink densities, and sliced into a plurality of different thicknesses to prepare samples 10A. Next, image data D1 of each sample 10A is obtained by the microscope 2 under the same predetermined settings (accelerating voltage, magnification, etc.). Next, the ranges of the crosslink density and thickness of the sample 10A in which the degree of clarity of the molecular chains or atoms of the polymer material in each of the obtained image data D1 is within an acceptable range are set in advance as the crosslink density standard range and the thickness standard range. The test for setting the crosslink density standard range and the thickness standard range is the same process as the procedure of the observation method illustrated in FIG. 4 described later.
[0029] The degree of clarity of the molecular chains or atoms of the polymeric material in the image data D1 is the degree of clarity of the molecular chains or atoms that affects the visibility of their state (degree of suitability for observation). In the image data D1 (image data of the dark-field image data D1a and the bright-field image data D1b) acquired by the microscope 2, the molecular chains and atoms of the polymeric material are represented by contrast (difference in light and dark) that shows the difference between the atoms that make up each of them.
[0030] In the image data D1, when the density of molecular chains in sample 10A is high, the contrast of molecular chains and atoms becomes less clear, and when the density of molecular chains is low, the contrast becomes clearer. In addition, in the image data D1, the thicker the sample 10A, the higher the density of molecular chains. Therefore, the higher the crosslink density of sample 10A and the thicker it is, the lower the clarity of molecular chains and atoms in the image data D1, making it unsuitable for observation. On the other hand, the lower the crosslink density of sample 10A and the thinner it is, the higher the clarity of molecular chains and atoms in the image data D1, making it suitable for observation.
[0031] The crosslink density standard range and thickness standard range may be appropriately set based on the above-mentioned test results, and are set so as to exclude those in which the contrast in the image data D1 becomes unclear. Therefore, when this clarity is within the allowable range, the density of the molecular chains of the polymer material is appropriately low, and the contrast in the image data D1 becomes clear. In the sample 10A made from a normal crosslinked polymer material (a polymer material in a normal crosslinked state), the molecular chains of the polymer material are highly dense because of the strong crosslinking state, and are not suitable for observation with the image data D1.
[0032] However, if the crosslink density of the sample 10A is too low (close to an uncrosslinked state), the molecular structure is weak and is easily damaged when sliced, making it impossible to obtain a specimen 10 suitable for observation. Also, if the sample 10 is too thin, defects will occur and it will be impossible to obtain a specimen 10 suitable for observation. Therefore, the crosslink density standard range and thickness standard range are set so that the sample 10 is in an appropriately weakly crosslinked state and has an appropriate thickness.
[0033] Although the optimal crosslink density standard range and thickness standard range vary slightly depending on the type of polymer material, taking into account the test results, the following ranges are considered to be effective for most types of polymer materials. Therefore, the crosslink density standard range is 1.0 x 10 -6 mol / cm 3 Above 1.0×10 -4 mol / cm 3The thickness standard range is preferably 1 nm or more and 50 nm or less, and more preferably 1 nm or more and 20 nm or less.
[0034] The crosslink density of a polymeric material is affected by the manufacturing conditions of the mixing process and the crosslinking process (vulcanization process), but when these manufacturing conditions are the same, it is greatly affected by the amount of the crosslinking agent blended. Therefore, when preparing a sample 10 in a weakly crosslinked state within the crosslink density standard range, it is advisable to blend 0.1 parts by mass to 2 parts by mass, more preferably 0.2 parts by mass to 1 part by mass, of the crosslinking agent per 100 parts by mass of the polymer of the uncrosslinked polymeric material, and then perform the mixing process and the crosslinking process.
[0035] The results of the test for setting the crosslink density standard range and thickness standard range described above revealed that as the amount of filler in the sample 10A increases, the contrast of the molecular chains and atoms of the polymer material in the image data D1 becomes unclear. The atoms constituting the filler are heavier than the atoms constituting the remaining additives excluding the filler from among the rubber components and additives. Therefore, as the amount of filler in the polymer material increases, the contrast of the molecular chains and atoms is buried in the contrast of the atoms of the filler. Therefore, when preparing the specimen 10, the amount of filler is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, per 100 parts by mass of the polymer of the uncrosslinked polymer material. In this way, by limiting the amount of filler, the contrast of the molecular chains and atoms of the polymer material in the image data D1 becomes clear, which is advantageous for obtaining a specimen 10 suitable for observation.
[0036] Next, a method for observing a polymer material will be described.
[0037] 4 shows an example of the procedure of an embodiment of the observation method. In this observation method, the specimen 10 prepared by the procedure described above is used. The thickness of the specimen 10 may be 1 nm or more and 50 nm or less, which is considered to be effective for most types of polymer materials. That is, in this observation method, a polymer material in a weakly crosslinked state, whose crosslink density is within a preset crosslink density reference range, is sliced to a thickness of 1 nm or more and 50 nm or less and used as the specimen 10.
[0038] In this observation method, image data D1 of the specimen 10 is obtained using the microscope 2 (S210, S220). Next, the state of the molecular chains and atoms of the polymer material is observed using the obtained image data D1 (S230). The contents of each step (S210 to S230) are described in detail below, but these steps are similar to the above-mentioned test for setting the crosslink density reference range and thickness reference range of the specimen 10, and basically the microscope 2 is set in the same settings (accelerating voltage, magnification, etc.) as in this test to obtain image data D1 of each specimen 10.
[0039] In step (S210), the specimen 10 is set in the microscope 2, and the microscope 2 acquires dark-field image data D1a and bright-field image data D1b of the specimen 10. The microscope 2 may acquire both the dark-field image data D1a and the bright-field image data D1b, or may acquire only one of the image data. By the microscope 2 acquiring both the dark-field image data D1a and the bright-field image data D1b, it becomes possible to compare the respective images.
[0040] 5 is a HAADF-STEM image (high-angle scattering annular dark-field image). The acceptance angle of the DF detector 8a is 90 mrad or more and 170 mrad or less.
[0041] 6 is a LAADF-STEM image (low-angle scattering annular dark-field image). The acceptance angle of the DF detector 8a is 40 mrad or more and 90 mrad or less.
[0042] The bright-field image data D1b shown in Fig. 7 is a BF-STEM image. The acceptance angle of the BF detector 8b is 23 mrad or less.
[0043] In each image data, dot-like areas with relatively high contrast (difference between light and dark) represent the atoms of the polymer material, while line-like areas with relatively low contrast represent the molecular chains of the polymer material.
[0044] In step (S220), the image simulator D2 is executed to perform data processing for generating image data D1 from the acquired dark-field image data D1a and bright-field image data D1b using image simulation by the arithmetic unit 3. The image simulator D2 is a program that causes the arithmetic unit 3 to execute various known image simulations, and is used to generate the image data D1. Examples of image simulations include simulations using various known methods such as the multi-slice method, the Bloch wave method, and the Bethe method. In the generated image data D1, molecular chains and atoms of the polymer material in the dark-field image data D1a and the bright-field image data D1b are identified by the image simulation, and the contrast of each is clearer than that of the image data.
[0045] The procedure of an example of the image simulation will be described. In this image simulation, first, model data D3 showing the aggregate structure of the specimen 10 is generated using molecular dynamics simulation. Next, the dispersion state of the molecular chains and atoms of the polymer material in the generated model data D3 and the intensities of the transmitted waves and diffracted waves are calculated. Next, the calculated dispersion state and intensity are compared with the contrast in the image data D1. Through this comparison, the molecular chains and atoms of the polymer material in the dark-field image data D1a and the bright-field image data D1b are identified based on the dispersion state, and image data D1 is generated in which the contrast of the identified molecular chains and atoms of the polymer material is simulated based on the intensity. In the molecular dynamics simulation, various parameters showing the state of the specimen 10, such as the compounding amount of the raw materials (rubber components and additives) of the specimen 10, the manufacturing conditions (mixing conditions and crosslinking conditions), the crosslinking density and thickness of the specimen 10, etc. are input as input parameters.
[0046] FIG. 8 shows an enlarged view of an example of the model data D3 used in the image simulation. In this enlarged view, linear polymeric molecular chains and point-like atoms are present. This model data D3 generally shows the aggregate structure of the molecular chains and atoms of the polymeric material in the specimen 10. That is, the aggregate structure shown by the model data D3 can be regarded as the aggregate structure in the actual specimen 10. The contrast of the molecular chains and atoms in the dark-field image data D1a and bright-field image data D1b acquired by the microscope 2 may not simply depend on the number of atoms and atomic number in the aggregate structure of the crosslinked material. Therefore, for observation on a more microscopic scale, it is preferable to generate image data D1 by image simulation using an image simulator D2.
[0047] Fig. 9 shows an example of image data D1 generated from the dark-field image data D1a. In the image data D1 shown in Fig. 9, the molecular chains and atoms of the polymer material are shown in white, and it can be seen that the contrast of the molecular chains and atoms of the polymer material (Zn and S3 in Fig. 9) is clearer than that in the dark-field image data D1a.
[0048] Fig. 10 shows an example of image data D1 generated from bright-field image data D1b. In the image data D1 shown in Fig. 10, molecular chains and atoms of the polymeric material are shown in black, and it can be seen that the contrast of the molecular chains and atoms of the polymeric material (Zn and S3 in Fig. 10) is clearer than that in the bright-field image data D1b.
[0049] In step (S220), the arithmetic unit 3 executes data processing to calculate the thickness of the specimen 10 in the image data D1 based on the contrast in the image data D1. A known through-focus method can be used as a method for calculating this thickness. In the above-mentioned Figs. 9 and 10, the thickness of the specimen 10 in the image data D1 is 4 nm.
[0050] In step (S230), the image data D1 is used to visually observe the state of molecular chains and atoms of the polymeric material present in the image data D1. As illustrated in Fig. 9 and Fig. 10 above, the image data D1 provides clear contrast due to the molecular chains and atoms of the polymeric material, making it possible to visually recognize the state of the molecular chains and atoms of the polymeric material.
[0051] Fig. 11 shows an example of image data D1 generated from dark-field image data D1b. The thickness of the specimen 10 in the image data D1 shown in Fig. 11 is 1 nm. The image data D1 shown in Fig. 11 shows clearer contrast due to molecular chains and atoms of polymer materials than the image data D1 of the specimen 10 having a thickness of 4 nm shown in Fig. 9 above. In this way, the smaller the thickness of the specimen 10 in the image data D1, the more suitable it is for observation.
[0052] As described above, according to the embodiment of the method for producing specimen 10, the produced specimen 10 is in a weakly crosslinked state within the crosslink density reference range and has a thickness within the thickness reference range, so that the state of molecular chains or atoms of the polymer material can be visually confirmed in image data D1 acquired using microscope 2. As a result, it is advantageous to directly observe and understand the state of these molecular chains or atoms using image data D1.
[0053] According to the embodiment of the observation method described above, a polymeric material is in a weakly crosslinked state in which the crosslink density is within a preset crosslink density reference range, and is sliced into ultra-thin pieces of 1 nm to 50 nm to be used as specimen 10. Therefore, in image data D1 of specimen 10 acquired using microscope 2, the state of molecular chains or atoms of the polymeric material becomes visible, which is advantageous for directly observing and understanding the state of these molecular chains or atoms.
[0054] Conventional observations of polymeric materials have used thin slices of ordinary vulcanized rubber (strongly cross-linked, not weakly cross-linked) sliced to a thickness of, for example, about 100 nm as specimens. In specimens with strong cross-linking, the density of molecular chains is high, and in specimens with a thickness of about 100 nm, the degree of overlap of molecular chains in the thickness direction is high. Therefore, image data D1 of conventional specimens is not suitable for directly observing the state of molecular chains and atoms of polymeric materials.
[0055] In the above-described embodiment, the specimen 10 is made of a chemically crosslinked polymeric material using a crosslinking agent such as sulfur vulcanization or non-sulfur vulcanization (peroxide vulcanization), but the specimen 10 can also be made of a polymeric material that is physically crosslinked by hydrogen bonding (such as maleic anhydride modified polypropylene). In the physically crosslinked polymeric material, the hydrogen bonding action between the polymers is reduced by adding an appropriate amount of alkyl alcohols, and the crosslink density is made into a weakly crosslinked state that is within a preset crosslink density reference range. In the physically crosslinked polymeric material, if the specimen 10 is in a weakly crosslinked state and is an ultra-thin specimen that satisfies the thickness reference range (1 nm or more and 50 nm or less), it becomes possible to visually confirm the molecular chains and atomic state of the polymeric material from the image data D1 acquired by the microscope 2.
[0056] The microscope 2 only needs to be capable of photographing the specimen 10 and acquiring two-dimensional image data as the dark-field image data D1a and the bright-field image data D1b, but may also acquire three-dimensional image data as these image data.
[0057] The image simulation performed by the image simulator D2 can use measurement results obtained by energy dispersive X-ray analysis (EDX) instead of the model data D3. In this way, the image simulation is not particularly limited.
[0058] The present invention is not limited to a specific embodiment, and various modifications and variations are possible within the scope of the gist of the present invention. EXAMPLES
[0059] Using 10 types of specimen samples (Comparative Examples 1 and 2, Examples 1 to 8) differing in the type and amount of raw materials (polymer and additive), the molecular chains and atomic states of the polymeric materials were observed according to the following procedure using a system similar to the observation system illustrated in Figures 1 and 2, and the results are shown in Table 1. In Table 1, the amount of additive is shown as parts by mass relative to 100 parts by mass of polymer.
[0060] [Table 1]
[0061] Each specimen was cooled to a low temperature using liquid nitrogen to solidify below the glass transition temperature, and then cut into ultrathin sections using an ultramicrotome. The scanning transmission electron microscope was set to an accelerating voltage of 200 kV and a magnification of 20 million times, and dark-field image data D1a and bright-field image data D1b of each specimen were taken. The acceptance angle of the DF detector was set to more than 40 mrad and less than 90 mrad, and the acceptance angle of the BF detector was set to less than 14 mrad.
[0062] Next, image data D1 was generated by image simulation using a computing device. In the image simulation, the image data D1 was simulated by a multi-slice method or the like using model data D3 showing the aggregate structure of the specimen 10 using molecular dynamics simulation.
[0063] The crosslink densities shown in Table 1 were measured using a known equilibrium lubrication method.
[0064] In the image data D1 of each of Examples 1 to 8, the molecular chains and atomic states of the polymeric material could be visually observed. In Comparative Example 1, which is unvulcanized rubber, image data could not be obtained because an observable specimen sample could not be prepared. In Comparative Example 2, the molecular chains and atomic states of the polymeric material could not be visually observed in the obtained image data.
[0065] The present disclosure includes the following inventions. Invention (1): A method for preparing a specimen for observation of a polymeric material, comprising slicing a polymeric material in a predetermined crosslinked state into thin slices to prepare a specimen for observation under a scanning transmission electron microscope, comprising: The polymer material having a weak crosslinking state with a crosslinking density of a plurality of different types is sliced into samples having a plurality of different thicknesses, acquiring image data of each of the samples under the same predetermined settings by the scanning transmission electron microscope, and presetting the ranges of the crosslink density and thickness of the sample in which the degree of clarity of the molecular chains or atoms of the polymer material in each of the acquired image data is within an acceptable range as a crosslink density reference range and a thickness reference range of the polymer material; When preparing a specimen for observation of the polymer material, the polymer material is brought into a weakly cross-linked state within the cross-link density standard range, and the weakly cross-linked polymer material is sliced to a thickness within the thickness standard range. Invention (2): A method for preparing a specimen for observation of a polymeric material according to invention (1), wherein the standard thickness range is 1 nm or more and 50 nm or less. Invention (3): The crosslink density reference range is 1.0 × 10 -6 mol / cm 3 Above 1.0×10 -4 mol / cm 3 A method for preparing a specimen for observation of a polymeric material according to the following invention (1) or (2). Invention (4): A method for preparing an observation specimen of a polymeric material according to any one of inventions (1) to (3), comprising mixing 0.1 to 2 parts by mass of a crosslinking agent per 100 parts by mass of the uncrosslinked polymer of the polymeric material to bring the polymeric material into a weakly crosslinked state within the crosslink density range. Invention (5): A method for observing a polymeric material, comprising the steps of: obtaining image data of a specimen for observation, which is a thin slice of a polymeric material in a predetermined crosslinked state, using a scanning transmission electron microscope; A method for observing a polymer material, comprising: rendering the polymer material in a weakly crosslinked state in which the crosslink density is within a preset crosslink density standard range; slicing the polymer material to a thickness of 1 nm or more and 50 nm or less to use as the specimen for observation; and observing the state of the molecular chains or atoms of the polymer material in the image data of the specimen for observation obtained using the scanning transmission electron microscope. Invention (6): A method for observing a polymeric material according to invention (5), comprising using the scanning transmission electron microscope to capture at least one of dark-field image data and bright-field image data of the specimen for observation, and generating the image data by processing the captured image data using image simulation by a computing device. Invention (7): A method for observing a polymeric material according to invention (5) or (6), comprising data processing for calculating the thickness of the specimen for observation by the arithmetic device based on the contrast of the image data. [Explanation of symbols]
[0066] 1 Observation System 2. Scanning Transmission Electron Microscopy 3 Computing device 10. Observation specimens 10A Sample D1a dark field image data D1b Brightfield image data D1 Image data D2 Statue Simulator
Claims
1. A method for preparing a specimen for observation of a polymer material, comprising slicing a polymer material in a predetermined crosslinked state into thin slices to prepare a specimen for observation under a scanning transmission electron microscope, comprising the steps of: The polymer material having a weak crosslinking state with a crosslinking density of a plurality of different types is sliced into samples having a plurality of different thicknesses, acquiring image data of each of the samples under the same predetermined settings by the scanning transmission electron microscope, and presetting the ranges of the crosslink density and thickness of the sample in which the degree of clarity of the molecular chains or atoms of the polymer material in each of the acquired image data is within an acceptable range as a crosslink density reference range and a thickness reference range of the polymer material; When preparing a specimen for observation of the polymer material, the polymer material is brought into a weakly cross-linked state within the cross-link density standard range, and the weakly cross-linked polymer material is sliced to a thickness within the thickness standard range.
2. 2. The method for preparing a specimen for observation of a polymer material according to claim 1, wherein the thickness standard range is 1 nm or more and 50 nm or less.
3. The crosslink density reference range is 1.0×10 -6 mol / cm 3 Above 1.0 x 10 -4 mol / cm 3 3. A method for preparing a specimen for observation of a polymer material according to claim 1 or 2, which comprises the following steps:
4. 4. A method for preparing an observation specimen of a polymer material as described in claim 3, wherein when preparing the observation specimen, a crosslinking agent is mixed in an amount of 0.1 parts by mass or more and 2 parts by mass or less per 100 parts by mass of polymer of the uncrosslinked polymer material, thereby bringing the polymer material into a weakly crosslinked state within the crosslink density range.
5. A method for observing a polymer material, comprising the steps of: obtaining image data of a specimen for observation, the specimen being a thin slice of a polymer material in a predetermined crosslinked state, using a scanning transmission electron microscope; A method for observing a polymer material, comprising: rendering the polymer material in a weakly crosslinked state in which the crosslink density is within a preset crosslink density standard range; slicing the polymer material to a thickness of 1 nm or more and 50 nm or less to use as the specimen for observation; and observing the state of the molecular chains or atoms of the polymer material in the image data of the specimen for observation obtained using the scanning transmission electron microscope.
6. 6. The method for observing a polymer material according to claim 5, further comprising the steps of: capturing at least one of dark-field image data and bright-field image data of the specimen for observation using the scanning transmission electron microscope; and generating the image data by processing the captured image data using image simulation by a computing device.
7. The method for observing a polymer material according to claim 6, further comprising the step of: carrying out data processing to calculate a thickness of the specimen for observation by the arithmetic unit based on the contrast of the image data.
Citation Information
Patent Citations
Automatic broadcasting device for man conveyor
JP1982067477A
Method of observing rubber material
JP2013044607A