Adhesive sheet and optical member with adhesive sheet

The adhesive sheet with a specific acrylic polymer and crosslinking agent addresses contamination and zipping issues, providing easy peelability and maintaining surface quality during high-speed peeling.

JP2024156497AInactive Publication Date: 2024-11-06NITTO DENKO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023071008
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Pressure-sensitive adhesive sheets used for surface protection often cause contamination and zipping during high-speed peeling, leading to noise and adhesive residue on the protected surfaces, and fail to maintain the quality of the object before and after protection.

Method used

A pressure-sensitive adhesive sheet with an acrylic polymer containing alkyl (meth)acrylate monomers having 6 to 17 carbon atoms in the ester end, combined with a crosslinking agent, to achieve high shear force and cohesive strength, reducing contamination and suppressing zipping during high-speed peeling.

Benefits of technology

The adhesive sheet minimizes contamination and zipping, ensuring easy peelability and improved peeling workability, maintaining the integrity of protected surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156497000001_ABST
    Figure 2024156497000001_ABST
Patent Text Reader

Abstract

To provide an adhesive sheet having low staining property to an adherend.SOLUTION: An adhesive sheet has an adhesive layer, and the adhesive layer contains an acrylic polymer. The acrylic polymer is a polymer of a monomer component which contains alkyl(meth)acrylate (m1) having a 6-17C alkyl group in an ester terminal, and the 6-17C alkyl group is a straight-chain alkyl group or a branched 1C alkyl group. A shearing force is 17 N / cm2 or more when sticking 1 cm2 of an adhesive area of the adhesive layer to an optical member, and pulling the product in a shearing direction in a condition of a tensile speed of 0.06 mm / min in an environment of 23°C and 50% RH.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet and an optical member with a pressure-sensitive adhesive sheet. [Background technology]

[0002] Generally, adhesives (also called pressure-sensitive adhesives; the same applies below) are in a soft solid (viscoelastic) state in a temperature range around room temperature, and have the property of easily adhering to an adherend by pressure. Taking advantage of such properties, adhesives are widely used in the form of adhesive sheets for purposes such as joining parts and protecting surfaces. The above adhesive is formed, for example, from an adhesive composition containing an acrylic polymer and a crosslinking agent. Patent documents 1 to 3 are prior art documents disclosing this type of conventional technology. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4682299 [Patent Document 2] International Publication No. 2021 / 125278 [Patent Document 3] International Publication No. 2021 / 125247 Summary of the Invention [Problem to be solved by the invention]

[0004] Adhesive sheets having an adhesive layer are also preferably used as surface protection films that prevent damage (scratches, stains, corrosion, etc.) to the surface of various articles when they are processed or transported. For example, surface protection films are also preferably used to protect the surfaces of optical members such as polarizing plates and displays. Here, as with surface protection films, adhesive sheets that are peeled (re-peeled) from an object to be protected (e.g., an optical member) after achieving the purpose of protecting the object are required to have light peelability so that they can be peeled off from the object to be protected with light force.

[0005] In addition, for adhesive sheets used in a peelable (repeelable) manner, such as surface protection films, it is desirable that the adhesive sheet can be peeled off smoothly from the object to be protected under a constant load without causing a vibratory peeling behavior called zipping when peeling off (repeeling off) from the object to be protected. Zipping in adhesive sheets tends to occur easily, particularly when the adhesive sheet is peeled off at high speed. Zipping during peeling of the adhesive sheet can cause a deterioration of the working environment due to peeling noise (generation of noise) and can also cause streaky peeling marks (glue residue) on the adherend.

[0006] In addition, for a pressure-sensitive adhesive sheet used in a peelable (repeelable) manner like a surface protection film, it is required that the object to be protected is not altered before and after the protection of the object to be protected. For this reason, it is desirable that the surface of the adherend is not contaminated by the pressure-sensitive adhesive after the pressure-sensitive adhesive sheet is peeled off from the adherend. However, for example, when a pressure-sensitive adhesive with a relatively low cohesive strength is used to suppress zipping during high-speed peeling, the adherend tends to be easily contaminated by the pressure-sensitive adhesive.

[0007] The present invention has been created in view of the above circumstances, and the main object is to provide a pressure-sensitive adhesive sheet that is less likely to stain an adherend. In particular, the object is to provide a pressure-sensitive adhesive sheet that can simultaneously reduce the staining of an adherend, suppress zipping during high-speed peeling, and provide easy peeling. Another object is to provide a pressure-sensitive adhesive sheet (surface protection film) used for surface protection of an optical member, and an optical member with a pressure-sensitive adhesive sheet (optical member with a surface protection film) that is composed of an optical member and a pressure-sensitive adhesive sheet. [Means for solving the problem]

[0008] According to this specification, a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer is provided. The pressure-sensitive adhesive layer contains an acrylic polymer, and the acrylic polymer is a polymer of a monomer component containing an alkyl (meth)acrylate (m1) having an alkyl group having 6 to 17 carbon atoms at an ester terminal, where the alkyl group having 6 to 17 carbon atoms is a linear alkyl group or a branched alkyl group having one carbon atom in the branch. The pressure-sensitive adhesive sheet has a pressure-sensitive adhesive layer having an adhesive area of ​​1 cm2. 2 was attached to an optical component and pulled in the shear direction at a pulling speed of 0.06 mm / min in an environment of 23°C and 50% RH, resulting in a shear force of 17 N / cm 2 The above is the result. A pressure-sensitive adhesive sheet using the above-mentioned acrylic polymer and having a shear strength of at least the above-mentioned lower limit is likely to reduce contamination of an adherend. In addition, a pressure-sensitive adhesive sheet having such a configuration is likely to suppress zipping during high-speed peeling.

[0009] In some embodiments, the alkyl (meth)acrylate (m1) includes at least one selected from n-heptyl acrylate and n-octyl acrylate. The use of such an alkyl (meth)acrylate (m1) makes it easier to achieve both reduced contamination of the adherend and suppressed zipping during high-speed peeling.

[0010] In some embodiments, the monomer component further includes (meth)acrylic acid. By using (meth)acrylic acid as a monomer component constituting an acrylic polymer, in an embodiment using a crosslinking agent (e.g., an epoxy-based crosslinking agent), the crosslinking reaction with the crosslinking agent proceeds favorably, increasing the curing property, and a pressure-sensitive adhesive exhibiting easy peelability is easily formed. In addition, since (meth)acrylic acid has a relatively high glass transition temperature, the use of (meth)acrylic acid is advantageous for improving the cohesive strength of the pressure-sensitive adhesive and reducing the contamination of the adherend.

[0011] In some embodiments, the acrylic polymer has a glass transition temperature, calculated based on the composition of the monomer components, of −55° C. or lower. When such an acrylic polymer is used, zipping during high-speed peeling is likely to be suppressed.

[0012] In some embodiments, the pressure-sensitive adhesive layer contains a crosslinking agent. By containing the crosslinking agent, the curing property of the pressure-sensitive adhesive is increased, and a pressure-sensitive adhesive exhibiting easy peeling property is easily formed. From the viewpoint of increasing the cohesive strength of the pressure-sensitive adhesive and reducing the staining property, in some preferred embodiments, an epoxy-based crosslinking agent is used as the crosslinking agent.

[0013] In some embodiments, the gel fraction of the pressure-sensitive adhesive layer is 70% or more. A pressure-sensitive adhesive layer having a gel fraction of 70% or more is unlikely to be deformed or damaged, such as by dents, by external forces, for example, during production, and is unlikely to change in appearance. A pressure-sensitive adhesive sheet having such a pressure-sensitive adhesive layer is likely to have a smooth surface, and is preferable because it allows for high-precision inspection, for example, when the pressure-sensitive adhesive sheet is formed into a transparent pressure-sensitive adhesive sheet and an adherend is inspected through the pressure-sensitive adhesive sheet. In addition, a pressure-sensitive adhesive layer having a high gel fraction is likely to exhibit light peelability.

[0014] The adhesive sheet disclosed herein tends to have low staining properties on the adherend, suppresses zipping during high-speed peeling, and exhibits easy peeling properties. Therefore, the adhesive sheet can be suitably used as a surface protection film. After a surface protection film is attached to an object to be protected, it is usually peeled off (re-peeled off) from the object to be protected when the protective purpose is achieved. By applying the adhesive sheet disclosed herein to a surface protection application, it is possible to improve the peeling workability during re-peeling and suppress the deterioration of the object to be protected before and after protection. In some preferred embodiments, the adhesive sheet is used for surface protection of optical members.

[0015] Furthermore, according to the technology disclosed herein, there is provided an optical member with an adhesive sheet (or an optical member with a surface protective film) configured by attaching any one of the adhesive sheets (or surface protective films) disclosed herein to at least one surface of an optical member. When an optical member is used as an adherend, the adhesive sheet disclosed herein tends to have low contamination of the adherend, suppresses zipping during high-speed peeling, and exhibits easy peelability. For this reason, an optical member with an adhesive sheet configured by attaching the above-mentioned adhesive sheet to the surface of an optical member tends to have improved peeling workability when peeled again, and suppresses deterioration of the optical member before and after protection. [Brief description of the drawings]

[0016] [Figure 1] 1 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to an embodiment. [Diagram 2] 1 is a cross-sectional view showing a schematic configuration of an optical member with a pressure-sensitive adhesive sheet according to one embodiment. [Diagram 3] FIG. 2 is a schematic diagram for explaining a method for measuring the shear strength of a pressure-sensitive adhesive sheet according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Preferred embodiments of the present invention will be described below. Matters necessary for carrying out the present invention other than those specifically mentioned in this specification can be understood by those skilled in the art based on the teachings on carrying out the invention described in this specification and the common general technical knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general technical knowledge in the relevant field. In the following drawings, the same reference numerals may be used to denote components or parts having the same function, and duplicated descriptions may be omitted or simplified. In addition, the embodiments shown in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the product actually provided.

[0018] In this specification, the term "adhesive" refers to a material that, as mentioned above, is in a soft solid (viscoelastic) state at temperatures near room temperature and easily adheres to an adherend by pressure. The adhesive referred to here is generally a material having a complex tensile modulus E * (1Hz)<10 7 dyne / cm 2 The material may be a material having the properties satisfying the above (typically, a material having the above properties at 25°C).

[0019] In this specification, biomass-derived carbon means carbon (renewable carbon) derived from biomass materials, i.e., materials derived from renewable organic resources. The biomass materials typically refer to materials derived from biological resources (typically plants that perform photosynthesis) that can be continuously reproduced in the presence of sunlight, water, and carbon dioxide. Therefore, materials derived from fossil resources that are depleted by use after mining (fossil resource-based materials) are excluded from the concept of biomass materials here. The biomass carbon ratio of the pressure-sensitive adhesive composition and the pressure-sensitive adhesive, i.e., the proportion of biomass-derived carbon in the total carbon contained in the pressure-sensitive adhesive composition and the pressure-sensitive adhesive, can be estimated from the carbon isotope content with mass number 14 measured in accordance with ASTM D6866.

[0020] <Adhesive sheet> The adhesive sheet disclosed herein comprises an adhesive layer. The adhesive sheet may be an adhesive sheet with a substrate in a form in which the adhesive layer is provided on one or both sides of a non-releasable substrate (support substrate), or may be an adhesive sheet without a substrate (i.e., an adhesive sheet without a non-releasable substrate) in a form in which the adhesive layer is held by a release liner. Hereinafter, the support substrate may be simply referred to as a "substrate". The concept of an adhesive sheet as used herein may include those referred to as adhesive tapes, adhesive labels, adhesive films, and the like. The adhesive sheet may be in the form of a roll or a sheet. It may also be an adhesive sheet processed into various shapes.

[0021] The pressure-sensitive adhesive sheet may have any other appropriate layer other than the substrate and the pressure-sensitive adhesive layer, so long as the effect of the present invention is not impaired. Examples of such other layers include an easy-adhesion layer, an easy-slip layer, an antiblocking layer, an antistatic layer, an antireflection layer, an oligomer prevention layer, and a release liner provided on the surface of the pressure-sensitive adhesive layer opposite the substrate.

[0022] The release liner (also called release film) may be a release liner having a release layer on the surface of a liner substrate such as a resin film or paper, or a release liner made of a low-adhesion material such as a polyolefin resin (e.g., polyethylene, polypropylene) or a fluorine-based resin. The release layer may be formed by surface-treating the liner substrate with a release treating agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based agent. As with the substrate of the pressure-sensitive adhesive sheet described below, a substrate made of a biomass-derived material or a recycled material (e.g., recycled film) may be preferably used as the liner substrate.

[0023] The structure of an adhesive sheet according to an embodiment is shown in FIG. 1. The adhesive sheet 130 is configured as a substrate-attached single-sided adhesive sheet including a sheet-like supporting substrate (e.g., a resin film) 132 having a first surface 132A and a second surface 132B, and an adhesive layer 134 provided on the first surface 132A side. The adhesive layer 134 is fixedly provided on the first surface 132A side of the supporting substrate 132. Such a single-sided adhesive sheet 130 is suitable as a surface protection film that is used by attaching its adhesive surface to the surface of an adherend (an object to be protected, for example, an optical member such as a polarizing plate). As shown in FIG. 1, the adhesive sheet 130 before use can be a component of a release-liner-attached adhesive sheet 100 in a form in which the surface (adhesive surface) 134A of the adhesive layer 134 is protected by a release liner 136, at least the side facing the adhesive layer 134 being a release surface. Alternatively, the release liner 136 may be omitted, and a supporting substrate 132 having a second surface 132B as the release surface may be used, and the adhesive sheet 130 may be rolled up so that the adhesive surface 134A is protected by contact with the second surface (rear surface) 132B of the supporting substrate 132 (roll form).

[0024] <Shear force> The adhesive sheet disclosed herein has an adhesive surface area of ​​the adhesive layer of 1 cm 2 was attached to an optical component and pulled in the shear direction at a pulling speed of 0.06 mm / min in an environment of 23°C and 50% RH, resulting in a shear force of 17 N / cm 2 Herein, when the term "shear force" is used simply in this specification, it refers to the shear force per 1 cm of adhesive area of ​​the adhesive layer, unless otherwise specified. 2 The shear strength is measured when the film is attached to an optical member and pulled in the shear direction at a pulling speed of 0.06 mm / min under an environment of 23°C and 50% RH. The shear strength is measured by the method described in the examples below.

[0025] According to the configuration in which the shear strength of the adhesive (layer) is equal to or greater than the lower limit, the staining property of the adhesive to the adherend tends to be reduced (improved). The reason for this should not be interpreted in a particularly restrictive manner, but can be considered as follows. That is, it is considered that the staining components of the adhesive to the adherend are mainly derived from the low molecular weight components contained in the adhesive. For this reason, reducing the proportion of low molecular weight components contained in the adhesive is effective in reducing the staining property of the adherend. On the other hand, since low molecular weight components have the effect of reducing the entanglement between polymers, the inclusion of low molecular weight components in the adhesive is also a factor in reducing the cohesive strength of the adhesive. For this reason, adhesives with high cohesive strength tend to contain less low molecular weight components in the adhesive, and tend to show improved staining properties (low staining properties). And, there is a positive correlation between the cohesive strength and the shear strength of the adhesive, and the higher the cohesive strength, the higher the shear strength tends to be, and the higher the shear strength, the higher the cohesive strength tends to be. From such a relationship between shear strength, cohesive strength and staining property, it is believed that when the shear strength of the adhesive (layer) is equal to or greater than a predetermined value, the staining property of the adhesive tends to be reduced (improved).

[0026] Furthermore, if the shear strength of the adhesive layer is high and the cohesive strength is high, the adhesive tends to have an easy peeling property. Therefore, also from the viewpoint of the easy peeling property of the adhesive, the shear strength of the adhesive layer is preferably equal to or higher than the above lower limit.

[0027] In some preferred embodiments, the shear strength of the adhesive is 18 N / cm 2 More preferably, it is 19 N / cm 2 or more (e.g. 20N / cm 2 or more), and more preferably 22N / cm 2 More preferably, 24N / cm 2 Above 25N / cm 2 It may be 25.5N / cm or more. 2 The upper limit of the shear strength of the adhesive is not particularly limited, but is usually 35 N / cm from the viewpoints of adhesive performance and suppression of zipping during peeling. 2 It is appropriate that the resistance is equal to or less than 30 N / cm 2 Less than or equal to 28N / cm2 Less than 27N / cm 2 The following is also fine.

[0028] Regarding the optical member as the adherend used to measure the shear force of the pressure-sensitive adhesive layer, the optical member refers to a member having optical properties (for example, polarizing property, light refraction property, light scattering property, light reflectivity, light transmittance, light absorption property, light diffraction property, optical rotation property, visibility, etc.). The optical member is not particularly limited as long as it is a member having optical properties, but examples thereof include members constituting devices (optical devices) such as display devices (image display devices) and input devices, or members used in these devices, such as polarizing plates, wave plates, retardation plates, optical compensation films, brightness improvement films, light guide plates, reflective films, anti-reflection films, hard coat (HC) films, impact absorbing films, antifouling films, photochromic films, light control films, transparent conductive films (ITO films), design films, decorative films, surface protection plates, prisms, lenses, color filters, transparent substrates, and further members in which these are laminated (these may be collectively referred to as "functional films"). The above "plate" and "film" each include plate-like, film-like, sheet-like and other forms. For example, a "polarizing plate" includes a "polarizing film", a "polarizing sheet", and the like.

[0029] Examples of the display device include a liquid crystal display device, an organic EL (electroluminescence) display device, a PDP (plasma display panel), electronic paper, etc. Examples of the input device include a touch panel, etc.

[0030] The optical member is not particularly limited, and examples thereof include members (e.g., sheet-shaped, film-shaped, or plate-shaped members) made of glass, acrylic resin, polycarbonate, polyethylene terephthalate, metal thin film, etc. In this specification, the term "optical member" also includes members (design films, decorative films, surface protection films, etc.) that play a role in decoration or protection while maintaining the visibility of a display device or an input device.

[0031] As the optical member as the adherend used to measure the shear force of the pressure-sensitive adhesive layer disclosed herein, for example, an optical member having a non-water-absorbent smooth surface such as a glass plate, a metal plate, a resin plate, etc. is suitable.

[0032] As the optical member as the adherend used to measure the shear force of the adhesive layer disclosed herein, a polarizing plate is particularly preferred. The polarizing plate generally has a structure in which a polarizing film is sandwiched between two triacetyl cellulose (TAC) films. Of the two TAC films, at least the TAC film arranged on the side to which the adhesive sheet is attached is preferably protected on its surface (attached surface) with a hard coat layer. The hard coat layer is preferably made of a urethane acrylate-based material. In addition, the polarizing plate is preferably configured such that an anti-reflection layer is further provided on the hard coat layer. When the shear force is measured using a polarizing plate having such a structure, the adhesive layer is preferably attached to the surface of the polarizing plate that is made of the anti-reflection layer.

[0033] <Adhesive layer> (Acrylic polymer) The adhesive layer disclosed herein contains an acrylic polymer. The adhesive layer is typically an adhesive layer having an acrylic polymer as a base polymer. Such an adhesive layer is also called an acrylic adhesive layer. The base polymer refers to the main component of a rubber-like polymer (a polymer that exhibits rubber elasticity in a temperature range around room temperature) contained in the adhesive layer. In this specification, the term "main component" refers to a component contained in an amount of more than 50% by weight, unless otherwise specified. In addition, the following explanation of the adhesive and the components that may be contained in the adhesive layer are also applicable to the adhesive composition used to form the adhesive (layer) unless otherwise specified.

[0034] In this specification, the term "acrylic polymer" refers to a polymer derived from a monomer component containing more than 50% by weight of a (meth)acrylic monomer. The content of the (meth)acrylic monomer in the monomer component is preferably 70% by weight or more, and may be 80% by weight or more. In some embodiments, the content of the (meth)acrylic monomer in the monomer component may be 90% by weight or more, 95% by weight or more, or 100% by weight. On the other hand, in consideration of the balance of adhesive properties, in some embodiments, the proportion of the (meth)acrylic monomer in the entire monomer component may be, for example, less than 99% by weight, less than 95% by weight, or less than 93% by weight.

[0035] In this specification, the term "(meth)acrylic monomer" refers to a monomer having at least one (meth)acryloyl group in one molecule. Here, "(meth)acryloyl" refers to acryloyl and methacryloyl collectively. Similarly, "(meth)acrylate" refers to acrylate and methacrylate, and "(meth)acrylic" refers to acrylic and methacrylic collectively. Therefore, the concept of a (meth)acrylic monomer here can include both a monomer having an acryloyl group (acrylic monomer) and a monomer having a methacryloyl group (methacrylic monomer).

[0036] The acrylic polymer is typically a polymer of a monomer raw material that contains one or more types of linear alkyl (meth)acrylate as a main monomer and may further contain one or more types of secondary monomers copolymerizable with the main monomer. The main monomer refers to a component that accounts for more than 50% by weight of the entire monomer components. The linear alkyl (meth)acrylate refers to an alkyl (meth)acrylate having a linear alkyl group at the ester end. The linear alkyl group is a concept that includes linear and branched alkyl groups, and does not include cyclic alkyl groups called alicyclic. The secondary monomer refers to a monomer component other than the linear alkyl (meth)acrylate used as the main monomer, and includes functional group-containing monomers such as carboxyl group-containing monomers described later and other copolymerizable monomers. In this specification, the secondary monomer refers to a monomer component other than the alkyl (meth)acrylate (m1) and other linear alkyl (meth)acrylates among the monomer components.

[0037] The acrylic polymer used in the technology disclosed herein contains an alkyl(meth)acrylate (m1) having a specific chemical structure as a monomer component. Specifically, the alkyl(meth)acrylate (m1) has an alkyl group having 6 to 17 carbon atoms at the ester terminal, and the alkyl group having 6 to 17 carbon atoms is a linear alkyl group or an alkyl(meth)acrylate having a branched alkyl group with one carbon atom in the branch (also called a branch or a branching group). A pressure-sensitive adhesive containing an acrylic polymer of the above structure is likely to achieve both reduced contamination of the pressure-sensitive adhesive and suppressed zipping during high-speed peeling. The reason for this is not particularly limited, but it is believed that a pressure-sensitive adhesive containing an acrylic polymer synthesized using the above alkyl(meth)acrylate (m1) as a monomer component is likely to have appropriate cohesive strength and glass transition temperature, which is believed to contribute to reduced contamination and suppressed zipping during high-speed peeling. The alkyl (meth)acrylate (m1) is contained as at least a part of the main monomer (chain alkyl (meth)acrylate) in the monomer components of the acrylic polymer. Hereinafter, a chain alkyl (meth)acrylate having a chain alkyl group with a carbon number of X at the ester terminal is referred to as C X In the case of an alkyl (meth)acrylate (for example, a chain alkyl (meth)acrylate having a chain alkyl group having 6 to 17 carbon atoms at the ester end, C 6-17 It is sometimes called alkyl (meth)acrylate.

[0038] The alkyl (meth)acrylate (m1) can also be represented by the following formula (1). CH2=C(R 1 )COOR 2 (1) Here, R in the above formula (1) 1 is a hydrogen atom or a methyl group. 2is an alkyl group having 6 to 17 carbon atoms, and is either a linear alkyl group or a branched alkyl group having one carbon atom in the branch. The number of carbon atoms in the alkyl group of the alkyl (meth)acrylate (m1) is preferably 7 or more, may be 8 or more, may be 9 or more, may be 10 or more, or may be 12 or more, from the viewpoints of reducing contamination, suppressing zipping, and easy peeling. The greater the number of carbon atoms in the alkyl group, the more effectively the effect and characteristics of the alkyl group having a long chain are likely to be exhibited. In addition, from the viewpoints of adhesive formability, adhesive properties, aging speed, etc., the number of carbon atoms is preferably 14 or less, more preferably 12 or less, even more preferably 10 or less, and particularly preferably 8 or less (for example, 7 or 8).

[0039] C used as alkyl (meth)acrylate (m1) 6-17 Specific examples of linear alkyl (meth)acrylates include n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, n-pentadecyl (meth)acrylate, n-hexadecyl (meth)acrylate, and n-heptadecyl (meth)acrylate. C as alkyl (meth)acrylate (m1) 6-17Specific examples of branched alkyl (meth)acrylate include methylheptyl (meth)acrylate, such as 2-octyl (meth)acrylate and isooctyl acrylate, methyloctyl (meth)acrylate, methylnonyl (meth)acrylate, methyldecyl (meth)acrylate, methyldodecyl (meth)acrylate, methyltridecyl (meth)acrylate, methyltetradecyl (meth)acrylate, methylpenta (meth)acrylate, and methylhexadecyl (meth)acrylate. The alkyl (meth)acrylate (m1) can be used alone or in combination of two or more. Although not particularly limited, in some embodiments, alkyl acrylate is preferably used as the alkyl (meth)acrylate (m1).

[0040] In some embodiments, C 6-17 A linear alkyl (meth)acrylate is preferably used. Among them, as the alkyl (meth)acrylate (m1), n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and n-dodecyl (meth)acrylate are more preferable, and n-heptyl (meth)acrylate and n-octyl (meth)acrylate are further more preferable.

[0041] C 6-17 As the branched alkyl (meth)acrylate, either an isoalkyl (meth)acrylate having an isoalkyl group in which a methyl group is branched at the carbon immediately before the end of the branched alkyl group, or a branched alkyl (meth)acrylate having a non-isobranched alkyl group in which a methyl group is branched at the carbon two or more carbons before the end of the branched alkyl group, such as 2-octyl (meth)acrylate, can be used. In some embodiments, however, a branched alkyl (meth)acrylate having a non-isobranched alkyl group in which the side chain end of the acrylic polymer is a relatively long linear alkyl group is preferred. For example, a C 6-17 Branched alkyl (meth)acrylates are preferably used.

[0042] The proportion of the alkyl (meth)acrylate (m1) in the entire monomer components is set according to the purpose of use, required properties, etc. In some embodiments, the proportion of the alkyl (meth)acrylate (m1) in the entire monomer components may be, for example, 10% by weight or more, and is suitably 30% by weight or more. In some preferred embodiments, it is 50% by weight or more (e.g., more than 50% by weight), more preferably 70% by weight or more, even more preferably 80% by weight or more, may be 85% by weight or more, particularly preferably 90% by weight or more, may be 92% by weight or more, or may be 95% by weight or more. By increasing the amount of the alkyl (meth)acrylate (m1) used, the properties based on the alkyl (meth)acrylate (m1) can be effectively expressed. On the other hand, from the viewpoint of copolymerizing a functional group-containing monomer or the like that serves as a crosslinking point, the proportion of the alkyl (meth)acrylate (m1) in the entire monomer components may be, for example, less than 99% by weight, may be less than 98% by weight, or may be less than 97% by weight. In some other embodiments, the upper limit of the proportion of the alkyl (meth)acrylate (m1) in the entire monomer components may be 95% by weight or less, 75% by weight or less, 60% by weight or less, or 50% by weight or less (e.g., less than 50% by weight) from the viewpoint of obtaining the effect of using other monomers.

[0043] The proportion of the alkyl (meth)acrylate (m1) in the total chain alkyl (meth)acrylate contained in the monomer component of the acrylic polymer may be, for example, 10% by weight or more, suitably 30% by weight or more, and in some preferred embodiments, 50% by weight or more (e.g., more than 50% by weight), more preferably 70% by weight or more, even more preferably 80% by weight or more, particularly preferably 90% by weight or more, may be 95% by weight or more, or may be 99% by weight or more. By increasing the amount of the alkyl (meth)acrylate (m1) used, the properties based on the alkyl (meth)acrylate (m1) can be effectively expressed. In some embodiments, an acrylic polymer having a monomer composition containing only the alkyl (meth)acrylate (m1) is used as the chain alkyl (meth)acrylate. Therefore, the upper limit of the proportion of the alkyl (meth)acrylate (m1) in the total chain alkyl (meth)acrylate is 100% by weight. In some other embodiments, the proportion of the alkyl (meth)acrylate (m1) in the entire chain alkyl (meth)acrylate may be 95% by weight or less, 75% by weight or less, 60% by weight or less, or 50% by weight or less (e.g., less than 50% by weight) from the viewpoint of obtaining the effect of using a chain alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1).

[0044] In some preferred embodiments, the alkyl (meth)acrylate (m1) is 7-12 Linear alkyl (meth)acrylates are used. 7-8 It is more preferable to use linear alkyl (meth)acrylate. 7-12 Linear alkyl (meth)acrylate (more preferably C 7-8The proportion of the linear alkyl (meth)acrylate may be, for example, 10% by weight or more, suitably 30% by weight or more, and in some preferred embodiments, 50% by weight or more (e.g., more than 50% by weight), more preferably 70% by weight or more, even more preferably 80% by weight or more, or may be 85% by weight or more, particularly preferably 90% by weight or more, or may be 92% by weight or more, or may be 95% by weight or more. In addition, the proportion of C in the total monomer components may be 7-12 Linear alkyl (meth)acrylate (more preferably C 7-8 The proportion of the linear alkyl (meth)acrylate may be, for example, less than 99% by weight, less than 98% by weight, or less than 97% by weight. 7-12 Linear alkyl (meth)acrylate (more preferably C 7-8 The upper limit of the proportion of the linear alkyl (meth)acrylate may be 95% by weight or less, 75% by weight or less, 60% by weight or less, or 50% by weight or less (for example, less than 50% by weight) from the viewpoint of obtaining the effect of using other monomers.

[0045] In some preferred embodiments, n-heptyl (meth)acrylate is used as the alkyl (meth)acrylate (m1). By using n-heptyl (meth)acrylate, the effect of the technology disclosed herein can be particularly preferably exhibited. Among them, n-heptyl acrylate is particularly preferred from the viewpoint of adhesive properties.

[0046] The proportion of n-heptyl (meth)acrylate in the entire monomer components is set according to the purpose of use, required properties, etc. In some embodiments, the proportion of n-heptyl (meth)acrylate in the entire monomer components may be, for example, 10% by weight or more, and is suitably 30% by weight or more. In some preferred embodiments, it is 50% by weight or more (e.g., more than 50% by weight), more preferably 70% by weight or more, even more preferably 80% by weight or more, or 85% by weight or more, particularly preferably 90% by weight or more, or 92% by weight or more, or 95% by weight or more. By increasing the amount of n-heptyl (meth)acrylate used, the effect of its use can be effectively expressed. On the other hand, from the viewpoint of copolymerizing functional group-containing monomers that become crosslinking points, the proportion of n-heptyl (meth)acrylate in the entire monomer components may be, for example, less than 99% by weight, or less than 98% by weight, or less than 97% by weight. In some other embodiments, the proportion of n-heptyl (meth)acrylate in the entire monomer components may be 95% by weight or less, 75% by weight or less, 60% by weight or less, or 50% by weight or less (e.g., less than 50% by weight) from the viewpoint of obtaining the effect of using various monomers other than n-heptyl (meth)acrylate.

[0047] The proportion of n-heptyl (meth)acrylate in the total chain alkyl (meth)acrylate contained in the monomer component of the acrylic polymer may be, for example, 10% by weight or more, suitably 30% by weight or more, and in some preferred embodiments, 50% by weight or more (e.g., more than 50% by weight), more preferably 70% by weight or more, even more preferably 80% by weight or more, particularly preferably 90% by weight or more, may be 95% by weight or more, or may be 99% by weight or more. By increasing the amount of n-heptyl (meth)acrylate used, the effect of its use can be effectively expressed. The technology disclosed herein can be preferably implemented in an embodiment using an acrylic polymer having a monomer composition containing only n-heptyl (meth)acrylate as the chain alkyl (meth)acrylate. Therefore, the upper limit of the proportion of n-heptyl (meth)acrylate in the total chain alkyl (meth)acrylate is 100% by weight. In some other embodiments, the proportion of n-heptyl (meth)acrylate in the total amount of the chain alkyl (meth)acrylates may be 95% by weight or less, 75% by weight or less, 60% by weight or less, or 50% by weight or less (e.g., less than 50% by weight) from the viewpoint of obtaining the effect of using other chain alkyl (meth)acrylates.

[0048] In some embodiments, the monomer components constituting the acrylic polymer may contain a chain alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1) within a range that does not significantly impair the effects of the invention. Examples of the chain alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1) include C 1-5 Alkyl (meth)acrylate, alkyl group with 18 or more carbon atoms 18+ Alkyl (meth)acrylate, alkyl group with 2 or more carbon atoms in the branched group 6-17 Branched alkyl (meth)acrylates can be used alone or in combination of two or more. 1-5Specific examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, and isopentyl (meth)acrylate. 18+ Specific examples of alkyl (meth)acrylates include octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. 6-17 A specific example of the branched alkyl (meth)acrylate is 2-ethylhexyl (meth)acrylate.

[0049] The proportion of the chain alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1) in the monomer component is not particularly limited, but may be, for example, approximately 50% by weight or less (e.g., less than 50% by weight), 30% by weight or less, 10% by weight or less, or 1% by weight or less. The technology disclosed herein can be preferably implemented in an embodiment in which the monomer component does not substantially contain a chain alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1). In an embodiment in which the monomer component contains a chain alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1), the proportion of the chain alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1) in the monomer component may be, for example, 1% by weight or more, 10% by weight or more, or 30% by weight or more.

[0050] In this specification, the monomer component being substantially free of monomer A (e.g., a chain alkyl (meth)acrylate other than the above alkyl (meth)acrylate (m1)) means that the monomer A is not used at least intentionally, and it is permissible for the monomer A to be unintentionally included in an amount of, for example, about 0.1% by weight or less.

[0051] In some embodiments, the monomer component may contain, as the linear alkyl (meth)acrylate, an alkyl (meth)acrylate having an alkyl group derived from biomass at the ester end (hereinafter also referred to as "biomass linear alkyl (meth)acrylate"). In recent years, environmental issues such as global warming have come to be emphasized, and it is desired to reduce the amount of fossil resource-based materials such as petroleum used. Under such circumstances, it is also desired to reduce the amount of fossil resource-based materials used in the field of adhesives. By using a biomass linear alkyl (meth)acrylate, it is possible to suitably realize an acrylic adhesive composition that takes into consideration the reduction of dependency on fossil resource-based materials.

[0052] The biomass linear alkyl (meth)acrylate is not particularly limited, and is, for example, an ester of a biomass-derived alkanol and a biomass-derived or non-biomass-derived (meth)acrylic acid. Examples of biomass-derived alkanols include biomass ethanol, alkanols derived from plant materials such as palm oil, palm kernel oil, coconut oil, and castor oil. When the biomass-derived alkanol has 3 or more carbon atoms, the alkanol may be linear or branched. In some embodiments, an ester of a biomass-derived alkanol and a non-biomass-derived (meth)acrylic acid is used as the biomass linear alkyl (meth)acrylate used in the synthesis of an acrylic polymer. In such a biomass linear alkyl (meth)acrylate, the higher the number of carbon atoms of the alkanol, the higher the ratio of the number of biomass-derived carbons to the total number of carbons contained in the biomass linear alkyl (meth)acrylate, that is, the higher the biomass carbon ratio of the linear alkyl (meth)acrylate. Therefore, in the above biomass linear alkyl (meth)acrylate, it is desirable that the linear alkyl group derived from biomass has a large number of carbon atoms in terms of reducing the dependency on fossil resource-based materials. On the other hand, if the linear alkyl group constituting the linear alkyl (meth)acrylate has too many carbon atoms, it tends to be difficult to obtain adhesive properties such as adhesive strength, and it may also be disadvantageous in terms of productivity such as synthesis, handling, and cost. In an embodiment in which an ester of a biomass-derived alkanol and a non-biomass-derived (meth)acrylic acid is used as the biomass linear alkyl (meth)acrylate, it is desirable to use a material that has a good balance between adhesive properties and reduced dependency on fossil resource-based materials (more specifically, the biomass carbon ratio of the above linear alkyl (meth)acrylate).

[0053] In the technology disclosed herein, a biomass linear alkyl (meth)acrylate can be used for both the above-mentioned alkyl (meth)acrylate (m1) and the linear alkyl (meth)acrylate other than the alkyl (meth)acrylate (m1). In an embodiment in which two or more compounds are used as the linear alkyl (meth)acrylate used in the synthesis of an acrylic polymer, at least a part of them (for example, one or two types, or all, i.e., all types) can be a biomass linear alkyl (meth)acrylate. In some preferred embodiments, by using a biomass linear alkyl (meth)acrylate as the alkyl (meth)acrylate (m1), the effect of the technology disclosed herein can be preferably realized while reducing the dependency on fossil resource materials.

[0054] From the viewpoints of adhesive formability, adhesive properties, and aging speed, the number of carbon atoms in the alkyl group of the biomass linear alkyl (meth)acrylate is preferably 14 or less, more preferably 12 or less, even more preferably 10 or less, and particularly preferably 8 or less (e.g., 7 or 8). Moreover, the above-mentioned number of carbon atoms is preferably 7 or more. For example, in an embodiment in which an ester of a biomass-derived alkanol and a non-biomass-derived (meth)acrylic acid is used as the biomass linear alkyl (meth)acrylate, the biomass carbon ratio of the synthesized acrylic polymer can be increased by increasing the number of carbon atoms in the alkyl group.

[0055] In some preferred embodiments, n-heptyl(meth)acrylate having an n-heptyl group derived from biomass (hereinafter also referred to as "biomass heptyl(meth)acrylate") is used as the alkyl(meth)acrylate (m1). By using biomass heptyl(meth)acrylate, the effect of the technology disclosed herein can be particularly favorably exhibited while reducing the dependency on fossil resource-based materials. Among them, biomass heptyl acrylate is particularly preferable from the viewpoint of adhesive properties.

[0056] The proportion of the biomass linear alkyl (meth)acrylate (e.g., biomass n-heptyl (meth)acrylate) in the total linear alkyl (meth)acrylate used in the monomer component of the acrylic polymer may be, for example, 1% by weight or more, suitably 10% by weight or more, preferably 30% by weight or more, more preferably 50% by weight or more (e.g., more than 50% by weight), 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, or 99% by weight or more. By increasing the proportion of the biomass linear alkyl (meth)acrylate used, the biomass carbon ratio of the acrylic polymer can be improved while effectively exerting the effect of its use. The technology disclosed herein can be preferably implemented in an embodiment in which an acrylic polymer having a monomer composition containing only a biomass linear alkyl (meth)acrylate is used as the linear alkyl (meth)acrylate. Therefore, the upper limit of the proportion of the biomass chain alkyl (meth)acrylate in the entire chain alkyl (meth)acrylate is 100% by weight. In some other embodiments, the proportion of the biomass chain alkyl (meth)acrylate in the entire chain alkyl (meth)acrylate may be 95% by weight or less, 70% by weight or less, 50% by weight or less (e.g., less than 50% by weight), 30% by weight or less, 10% by weight or less, or 1% by weight or less.

[0057] In some embodiments, the monomer components forming the acrylic polymer contain, in addition to the above-mentioned chain alkyl (meth)acrylate, other monomers (copolymerizable monomers) that are copolymerizable with the above-mentioned chain alkyl (meth)acrylate. The copolymerizable monomers can be used alone or in combination of two or more. The above-mentioned copolymerizable monomers can be useful for introducing crosslinking points into the acrylic polymer or for increasing the cohesive strength of the acrylic polymer. The copolymerizable monomers may be derived from biomass or non-biomass.

[0058] In some preferred embodiments, a carboxyl group-containing monomer is used as the copolymerizable monomer. By using a carboxyl group-containing monomer as a copolymerizable monomer component for introducing a crosslinking point into an acrylic polymer in combination with a crosslinking agent (e.g., an epoxy-based crosslinking agent), the cohesive strength is improved, and it is easy to adjust the adhesive strength to a good level that allows re-peeling, and the staining of the adherend is reduced, so that it is easy to form a pressure-sensitive adhesive suitable for surface protection applications that can be peeled off.

[0059] Examples of the carboxyl group-containing monomer include ethylenically unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl-2-hydroxyethyl-phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, carboxypolycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl tetrahydrophthalic acid, crotonic acid, and isocrotonic acid; and ethylenically unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, and citraconic acid. The carboxyl group-containing monomer may also be a monomer having a metal salt (e.g., an alkali metal salt) of a carboxyl group. Among these, acrylic acid and methacrylic acid are preferred, and acrylic acid is more preferred.The above carboxyl group-containing monomers may be used alone or in combination of two or more.

[0060] The content of the carboxyl group-containing monomer (preferably (meth)acrylic acid) in the monomer components forming the acrylic polymer may be, for example, 0.01% by weight or more, 0.1% by weight or more, or more than 0.5% by weight, and in some preferred embodiments, 1% by weight or more (for example, more than 1% by weight), 2% by weight or more, or 3% by weight or more. The content of the carboxyl group-containing monomer (preferably (meth)acrylic acid) in the entire monomer components is, for example, less than 15% by weight, and is preferably 10% by weight or less, and in some preferred embodiments, may be 8% by weight or less, 6% by weight or less, or 5% by weight or less. By using an appropriate amount of the carboxyl group-containing monomer (preferably (meth)acrylic acid) within the above range, the cohesive strength is improved, and it is easy to adjust the adhesive strength to a good level that allows re-peeling, and it is easy to form a pressure-sensitive adhesive suitable for surface protection applications that can be re-peeled.

[0061] The monomer component forming the acrylic polymer is the above-mentioned alkyl (meth)acrylate. The copolymer may contain other copolymerizable monomers that are copolymerizable with (m1). The other copolymerizable monomers are defined as monomers that are different from the above-mentioned chain alkyl (meth)acrylate (m1), the chain alkyl (meth)acrylates other than the above-mentioned alkyl (meth)acrylate (m1), and the above-mentioned carboxyl group-containing monomers. The other copolymerizable monomers may be used alone or in combination of two or more.

[0062] Non-limiting examples of other copolymerizable monomers include the following: Hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc.; unsaturated alcohols such as vinyl alcohol, allyl alcohol, etc. Monomers containing a sulfonic acid group or a phosphoric acid group: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethyl acryloyl phosphate, etc. Epoxy group-containing monomers: for example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl ether (meth)acrylate, allyl glycidyl ether, and glycidyl ether (meth)acrylate. Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile, etc. Isocyanate group-containing monomers: for example, 2-isocyanatoethyl (meth)acrylate. Amide group-containing monomers: for example, (meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide; N-alkyl(meth)acrylamides such as N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and Nn-butyl(meth)acrylamide. N-vinyl carboxylic acid amides such as N-vinyl acetamide; monomers having a hydroxyl group and an amide group, for example, N-hydroxyalkyl (meth)acrylamides such as N-(2-hydroxyethyl)(meth)acrylamide; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl (meth)acrylamides such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, etc.; and others, such as N,N-dimethylaminopropyl (meth)acrylamide, N-(meth)acryloylmorpholine, etc. Monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc. (for example, lactams such as N-vinyl-2-caprolactam). Monomers having a succinimide skeleton: for example, N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, N-(meth)acryloyl-8-oxyhexamethylene succinimide, and the like. Maleimides: for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, and the like. Itaconimides: for example, N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, N-laurylitaconimide, and the like. Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate. Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; alkoxyalkylene (meth)acrylates such as methoxyethylene glycol (meth)acrylate and methoxypolypropylene glycol (meth)acrylate. Vinyl esters: for example, vinyl acetate, vinyl propionate, etc. Vinyl ethers: for example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether. Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc. Olefins: For example, ethylene, butadiene, isoprene, isobutylene, etc. (Meth)acrylates having an alicyclic hydrocarbon group: for example, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and the like. (Meth)acrylates having an aromatic hydrocarbon group: for example, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, and the like. Other examples include heterocyclic ring-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, halogen atom-containing (meth)acrylates such as vinyl chloride and fluorine atom-containing (meth)acrylates, silicon atom-containing (meth)acrylates such as silicone (meth)acrylate, and (meth)acrylates obtained from terpene compound derivative alcohols.

[0063] The monomer component constituting the acrylic polymer may or may not contain the other copolymerizable monomer. The amount of the other copolymerizable monomer is not particularly limited and may be appropriately selected according to the purpose and application. The content of the other copolymerizable monomer in the monomer component is, for example, appropriately less than 50% by weight (e.g., less than 30% by weight), preferably less than 10% by weight, more preferably less than 5% by weight, and may be less than 3% by weight (e.g., less than 1% by weight). The technology disclosed herein can be preferably implemented in an embodiment in which the monomer component does not substantially contain other copolymerizable monomer.

[0064] The biomass carbon ratio of the monomer components constituting the acrylic polymer (the biomass carbon ratio of the acrylic polymer) may be, for example, 1% or more, suitably 10% or more, preferably 30% or more, more preferably 50% or more (e.g., more than 50%), may be 60% or more, may be 65% or more, may be 70% or more, may be 80% or more, or may be 90% to 100%. By designing in this way, an acrylic pressure-sensitive adhesive that takes into consideration the reduction of dependency on fossil resource-based materials can be obtained.

[0065] The composition of the monomer components constituting the acrylic polymer may be set so that the glass transition temperature Tg calculated by the Fox formula based on the composition of the monomer components is −75° C. or more and 10° C. or less. In some embodiments, from the viewpoint of adhesive strength and the like, the Tg is suitably 0° C. or less, preferably −10° C. or less, and may be −20° C. or less or −30° C. or less. From the viewpoint of suppressing zipping during high-speed peeling, the Tg is preferably −55° C. or less, more preferably −60° C. or less, and even more preferably −62° C. or less (e.g., −64° C. or less).

[0066] Here, the Fox formula is a relational expression between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below. 1 / Tg=Σ(Wi / Tgi) In the above Fox formula, Tg is the glass transition temperature of the copolymer (unit: K), Wi is the weight fraction of monomer i in the copolymer (copolymerization ratio based on weight), and Tgi is the glass transition temperature of a homopolymer of monomer i (unit: K). The glass transition temperature of the homopolymer used to calculate Tg is the value described in a publicly known document, specifically, "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989). When multiple values ​​are described in this document, the highest value is used.

[0067] Although not particularly limited, the weight average molecular weight (Mw) of the acrylic polymer is usually about 10 × 10 4 It is appropriate that the Mw of the acrylic polymer is 30×10 or more. By using an acrylic polymer having such Mw, a pressure-sensitive adhesive exhibiting good cohesiveness is easily obtained. In some embodiments, the Mw of the acrylic polymer is, for example, 30×10 4 It is appropriate that the ratio is equal to or greater than 50×10 4 That's it, 70 x 10 4 It may be 100 x 10 or more. 4 Ultra-fine, 110x10 4 More than 120 x 10 is fine. 4 More than 130 x 10 is fine. 4 By setting the Mw of the acrylic polymer to a predetermined value or more, the cohesive force of the pressure-sensitive adhesive is improved, and it is easy to prevent the occurrence of contamination on the surface of the adherend. In addition, from the viewpoint of adhesion to the adherend, the Mw of the acrylic polymer is usually about 500 × 10 4 It is appropriate that the value is less than 300×10 4 It may be less than or equal to 100 x 10 4 Less than or equal to (e.g. 100×10 4It may be less than 100%. By setting the Mw to a predetermined value or less, the pressure-sensitive adhesive has an appropriate fluidity and tends to easily obtain wettability (adhesion) to the adherend. By having good wettability, the pressure-sensitive adhesive sheet does not peel off from the adherend during use, and can preferably fulfill its protective function. In the acrylic polymer obtained by the solution polymerization method, it is particularly significant that the Mw is in the above-mentioned preferred range.

[0068] The Mw of the acrylic polymer can be measured by gel permeation chromatography (GPC) and calculated as a standard polystyrene equivalent. Specifically, it can be measured under the following conditions using a GPC measuring device (trade name: "HLC-8220GPC" manufactured by Tosoh Corporation). The same applies to the examples described below. [GPC measurement conditions] Sample concentration: 0.1% by weight (tetrahydrofuran solution) Sample injection volume: 10 μL Eluent: tetrahydrofuran (THF) Flow rate (flow rate): 1.0mL / min Column temperature (measurement temperature): 40℃ column: Sample column: 1 "TSKguardcolumn SuperHZ-H" + 2 "TSKgel SuperHZM-H" (manufactured by Tosoh Corporation) Reference column: 1 "TSKgel SuperH-RC" (manufactured by Tosoh Corporation) Detector: Differential refractometer (RI) Standard sample: polystyrene

[0069] From the viewpoint of reducing contamination of the adherend, the low molecular weight components contained in the acrylic polymer (e.g., molecular weights of 10 × 10 4 In some preferred embodiments, the content of the acrylic polymer contained in the pressure-sensitive adhesive layer is preferably low. 4The weight fraction is 13% or less, more preferably 12% or less, even more preferably 11% or less, still more preferably 9% or less, and particularly preferably 8% or less. From the viewpoint of further reducing the staining property, the molecular weight of the acrylic polymer contained in the pressure-sensitive adhesive layer is 10×10 4 The weight fraction of the acrylic polymer contained in the pressure-sensitive adhesive layer may be 7% or less, 6% or less, or 5% or less. 4 The lower limit of the weight fraction below is not particularly limited, but from the viewpoint of increasing the polymerization rate and improving the yield, it is usually appropriate to set the lower limit to 3% or more, preferably 4% or more, and may be 5% or more.

[0070] The molecular weight of the acrylic polymer is 10 × 10 4 The following weight fractions are based on the results of GPC measurement of the acrylic polymer under the above-mentioned GPC measurement conditions, and are calculated based on the molecular weight of 10 × 10 4 It can be determined by fractionating and calculating the following. The same applies to the examples described later.

[0071] The method for obtaining an acrylic polymer is not particularly limited, and various polymerization methods known as a synthesis method for an acrylic polymer, such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and photopolymerization, can be appropriately adopted. For example, a solution polymerization method can be preferably adopted. The embodiment adopting the solution polymerization method can be advantageous from the viewpoint of transparency, adhesive performance, and the like. As a monomer supply method when carrying out solution polymerization, a lump-sum charging method in which all monomer raw materials are supplied at once, a continuous supply (dropping) method, a divided supply (dropping) method, and the like can be appropriately adopted. The polymerization temperature when carrying out solution polymerization can be appropriately selected depending on the type of monomer and solvent used, the type of polymerization initiator, and the like, and can be, for example, about 20°C to 170°C (typically about 40°C to 140°C). In some embodiments, the polymerization temperature is about 45°C to 75°C.

[0072] The solvent (polymerization solvent) used in the solution polymerization can be appropriately selected from conventionally known organic solvents (toluene, ethyl acetate, etc.). The initiator used in the polymerization can be appropriately selected from conventionally known polymerization initiators (for example, azo-based polymerization initiators such as 2,2'-azobisisobutyronitrile (AIBN), peroxide-based initiators, etc.) depending on the type of polymerization method. The amount of the polymerization initiator used is not particularly limited, and can usually be selected from the range of about 0.005 to 1 part by weight (typically about 0.01 to 1 part by weight) relative to 100 parts by weight of the monomer component.

[0073] When the amount of polymerization initiator used is reduced, the amount of radical generation is reduced, and the polymer growth reaction is promoted, and the reaction product tends to have a high molecular weight. By increasing the molecular weight of the polymer, the generation of relatively low molecular weight components is suppressed, and it is expected that the contamination of the adhesive is reduced. From this viewpoint, in some embodiments, the amount of polymerization initiator used is preferably 0.3 parts by weight or less (e.g., 0.2 parts by weight or less) relative to 100 parts by weight of the monomer component, more preferably 0.15 parts by weight or less, even more preferably 0.1 parts by weight or less, even more preferably 0.08 parts by weight or less, and particularly preferably 0.06 parts by weight or less. The lower limit of the amount of polymerization initiator used is not particularly limited, but is suitably 0.005 parts by weight or more relative to 100 parts by weight of the monomer component, and may be 0.01 parts by weight or more.

[0074] In addition, the reaction time in solution polymerization is not particularly limited. In solution polymerization, relatively high molecular weight components tend to be generated in the early stage of the polymerization reaction, and relatively low molecular weight components tend to be generated in the later stage of the polymerization reaction. Therefore, from the viewpoint of suppressing the generation of low molecular weight components and reducing the contamination of the adhesive, it is advantageous to shorten the polymerization reaction time. From this viewpoint, in some embodiments, it is preferable to set the reaction time to less than 7 hours. By shortening the reaction time, it is possible to suppress the generation of low molecular weight components that tend to be generated in the later stage of polymerization. In some preferred embodiments, the reaction time in solution polymerization is 6 hours or less, more preferably 5.5 hours or less (e.g. 5 hours or less). Note that the reaction time here does not include the maturation time in the process of maturing the polymerization product at a temperature higher than the polymerization temperature (e.g., a temperature about 5 to 15°C higher than the polymerization temperature) in the post-polymerization process. From the viewpoint of preventing an excessive decrease in the yield due to an excessive decrease in the polymerization rate, it is usually appropriate to set the reaction time to 1 hour or more, preferably 1.5 hours or more, and more preferably 2 hours or more (e.g. 2.5 hours or more).

[0075] The solid concentration of the monomer components in the reaction solution in solution polymerization (hereinafter also referred to as "polymerization concentration") is not particularly limited. By increasing the polymerization concentration, the probability of encounter between monomers increases, and the reaction product tends to have a higher molecular weight. From the viewpoint of suppressing the generation of low molecular weight components and reducing the contamination of the adhesive, in some preferred embodiments, the polymerization concentration is 20% by weight or more, may be 25% by weight or more, may be 30% by weight or more, or may be 33% by weight or more. It is usually appropriate for the polymerization concentration to be about 45% by weight or less, and may be 40% by weight or less.

[0076] (Crosslinking agent) The adhesive composition disclosed herein includes a crosslinking agent. The crosslinking agent can be useful for increasing the cohesive strength of the adhesive. The crosslinking agent can be selected from various crosslinking agents known in the field of adhesives. Examples of such crosslinking agents include epoxy-based crosslinking agents, isocyanate-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, and amine-based crosslinking agents. The crosslinking agent can be used alone or in combination of two or more. The crosslinking agent may be derived from biomass or non-biomass. From the viewpoint of producing an acrylic adhesive that takes into consideration the reduction of dependency on fossil resource-based materials, a biomass-derived crosslinking agent is preferably used. The technology disclosed herein can be preferably implemented in an embodiment in which both the acrylic polymer and the crosslinking agent contained in the adhesive composition are derived from biomass.

[0077] The amount of the crosslinking agent used is not particularly limited. The amount of the crosslinking agent used may be selected from the range of, for example, 0.1 to 20 parts by weight relative to 100 parts by weight of the acrylic polymer. From the viewpoint of achieving a good balance between improving the cohesive force and adhesion to the adherend, the amount of the crosslinking agent used relative to 100 parts by weight of the acrylic polymer is usually preferably 15 parts by weight or less, may be 10 parts by weight or less, may be 8 parts by weight or less, may be 7 parts by weight or less, and may be 0.5 parts by weight or more, and may be 1 part by weight or more. By setting the amount of the crosslinking agent used within an appropriate range, the cohesive force of the adhesive can be increased, the occurrence of adhesive residue on the adherend can be prevented, and adhesion to the adherend can be obtained.

[0078] In some embodiments, the crosslinking agent preferably contains at least an epoxy-based crosslinking agent. The epoxy-based crosslinking agent may be used alone or in combination of two or more. The epoxy-based crosslinking agent may be derived from biomass or may be derived from non-biomass. From the viewpoint of producing an acrylic adhesive that takes into consideration the reduction of dependency on fossil resource-based materials, a biomass-derived epoxy-based crosslinking agent is preferably used. The epoxy-based crosslinking agent may also be used in combination with other crosslinking agents, such as an isocyanate-based crosslinking agent.

[0079] As the epoxy crosslinking agent, a compound having two or more epoxy groups in one molecule can be used without any particular limitation. An epoxy crosslinking agent having 3 to 5 epoxy groups in one molecule is preferred. The epoxy crosslinking agent can be used alone or in combination of two or more. Specific examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, and the like. Examples of commercially available epoxy crosslinking agents include Mitsubishi Gas Chemical Company, Inc.'s product name "TETRAD-C" and product name "TETRAD-X", DIC Corporation's product name "Epicron CR-5L", Nagase ChemteX Corporation's product name "Denacol EX-512", Nissan Chemical Industries, Ltd.'s product name "TEPIC-G", and the like.

[0080] The amount of the epoxy crosslinking agent used may be, for example, about 0.1 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, or more than 1.5 parts by weight, relative to 100 parts by weight of the acrylic polymer. From the viewpoint of obtaining a higher use effect, the amount of the epoxy crosslinking agent used relative to 100 parts by weight of the acrylic polymer may be, for example, more than 2.0 parts by weight, 2.5 parts by weight or more, 3.0 parts by weight or more, or 3.5 parts by weight or more. In addition, the amount of the epoxy crosslinking agent used relative to 100 parts by weight of the acrylic polymer is usually appropriate to be 20 parts by weight or less, 10 parts by weight or less, 8 parts by weight or less, 6 parts by weight or less, or 5 parts by weight or less (for example, less than 5 parts by weight). By setting the amount of the epoxy crosslinking agent used within an appropriate range, the cohesive strength of the pressure-sensitive adhesive can be increased, it is easy to adjust the adhesive strength to a good level that allows re-peelability, it is possible to prevent the occurrence of contamination of the adherend, and it is also possible to obtain adhesion to the adherend. Furthermore, by limiting the amount of the epoxy crosslinking agent used, a transparent adhesive can be easily formed.

[0081] In some embodiments, from the viewpoint of reducing contamination, the amount of the epoxy-based crosslinking agent used may be more than 4 parts by weight, 4.5 parts by weight or more, more than 5 parts by weight, or 5.5 parts by weight or more, based on 100 parts by weight of the acrylic polymer.

[0082] In the case of using a carboxyl group-containing monomer (e.g., (meth)acrylic acid) and an epoxy-based crosslinking agent, the ratio (WB / WA) (weight basis) of the amount of the epoxy-based crosslinking agent WB to the amount of the carboxyl group-containing monomer (the total amount when two or more kinds of carboxyl group-containing monomers are used) WA is not particularly limited, but from the viewpoint of increasing the cohesive strength of the adhesive, it is preferably 0.7 or more, more preferably 0.8 or more, even more preferably 0.9 or more (e.g., 1.0 or more), and particularly preferably 1.1 or more. In addition, the above ratio (WB / WA) is usually 3.0 or less, may be 2.0 or less, may be 1.8 or less, may be 1.6 or less, may be 1.4 or less, or may be 1.3 or less.

[0083] As the isocyanate crosslinking agent, a polyisocyanate crosslinking agent having two or more isocyanate groups per molecule is preferably used. The number of isocyanate groups per molecule of the polyisocyanate crosslinking agent is preferably 2 to 10, for example, 2 to 4, typically 2 or 3. Examples of the polyisocyanate crosslinking agent include aromatic polyisocyanates such as tolylene diisocyanate and xylylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate; and aliphatic polyisocyanates such as hexamethylene diisocyanate. More specifically, for example, lower aliphatic polyisocyanates such as butylene diisocyanate, pentamethylene diisocyanate, and hexamethylene diisocyanate; alicyclic polyisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, and polymethylene polyphenyl diisocyanate; trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name "Coronate L"), trimethylolpropane / hexyl diisocyanate, and trimethylolpropane / hexyl diisocyanate; Examples of the isocyanate adduct include isocyanate adducts such as a trimer adduct of samethylene diisocyanate (manufactured by Tosoh, trade name "Coronate HL"), an isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh, trade name "Coronate HX"), and an isocyanurate of pentamethylene diisocyanate (manufactured by Mitsui Chemicals, trade name "Stabio D-370N"); polyisocyanates such as polyether polyisocyanate and polyester polyisocyanate; adducts of these polyisocyanates and polyols; and polyisocyanates obtained by multifunctionalizing these polyisocyanates with isocyanurate bonds, biuret bonds, allophanate bonds, etc. For example, in applications where transparency is required for the adhesive, it is preferable to use aliphatic diisocyanates such as pentamethylene diisocyanate and hexamethylene diisocyanate, and isocyanurates of such aliphatic diisocyanates.

[0084] The adhesive composition disclosed herein may contain a catalyst. By using a catalyst, the curing reaction of the adhesive composition (typically, the crosslinking reaction of the crosslinking agent described above) can be efficiently promoted, and stable adhesion can be easily achieved from an early stage after the preparation of the adhesive sheet. The catalyst is also called a crosslinking catalyst. Examples of the catalyst include tin (Sn)-containing compounds (tin-based catalysts), zirconium (Zr)-containing compounds (zirconium-based catalysts), titanium (Ti)-containing compounds (titanium-based catalysts), iron (Fe)-containing compounds (iron-based catalysts), aluminum (Al)-containing compounds (aluminum-based catalysts), zinc (Zn)-containing compounds (zinc-based catalysts), and bismuth (Bi)-containing compounds (bismuth-based catalysts). These are typically organic compounds having a metal in the active center, and are also called organometallic catalysts. The catalyst can be used alone or in combination of two or more types. The technology disclosed herein can be suitably implemented even in an embodiment that does not include a catalyst.

[0085] The above-mentioned adhesive composition may contain various additives known in the art, if necessary. Examples of such additives include surface lubricants, leveling agents, tackifier resins, plasticizers, softeners, fillers, colorants (pigments, dyes, etc.), antistatic agents, antioxidants, preservatives, light stabilizers, ultraviolet absorbers, polymerization inhibitors, silane coupling agents, etc. The content of these optional additives may be appropriately set according to the intended use. The amount of the optional additives used is, for example, less than 10 parts by weight, and is suitably about 3 parts by weight or less (for example, about 1 part by weight or less) relative to 100 parts by weight of the acrylic polymer.

[0086] (Method of forming pressure-sensitive adhesive layer) The form of the adhesive composition used to form the adhesive layer is not particularly limited, and an aqueous adhesive composition, a solvent-based adhesive composition, or the like is preferred. Here, the aqueous adhesive composition refers to an adhesive composition in a form containing an adhesive (adhesive layer forming component) in a solvent (aqueous solvent) mainly composed of water, and is a concept that includes an aqueous dispersion-type adhesive composition in which an adhesive is dispersed in water, and a water-soluble adhesive composition in which an adhesive is dissolved in water. In addition, the solvent-based adhesive composition refers to an adhesive composition in a form containing an adhesive in an organic solvent. As the organic solvent contained in the solvent-based adhesive composition, one or more organic solvents (toluene, ethyl acetate, etc.) that can be used in the above-mentioned solution polymerization can be used without particular limitation. The technology disclosed herein can be preferably implemented in an embodiment having an adhesive layer formed from a solvent-based adhesive composition from the viewpoint of adhesion properties, etc. In an embodiment having a solvent-based adhesive layer formed from a solvent-based adhesive composition, the effect of the technology disclosed herein is preferably realized.

[0087] The formation of the adhesive (layer) from the adhesive composition can be carried out by a conventionally known method. For example, in the case of a substrate-less double-sided adhesive sheet, an adhesive composition is applied to a surface (release surface) having releasability, and then the adhesive composition is cured to form an adhesive layer (a layer made of an adhesive) on the surface, thereby forming an adhesive sheet. In addition, in the case of an adhesive sheet with a substrate, a method (direct method) in which an adhesive composition is directly applied (typically coated) to the substrate and cured to form an adhesive layer can be preferably adopted. In addition, a method (transfer method) in which an adhesive composition is applied to a surface (release surface) having releasability and cured to form an adhesive layer on the surface, and the adhesive layer is transferred to a substrate may be adopted. As the release surface, the surface of a release sheet, the back surface of a substrate treated for release, etc. may be used. In addition, the adhesive composition can be cured by subjecting the adhesive composition to a curing treatment such as drying, crosslinking, polymerization, cooling, etc. Two or more types of curing treatments may be carried out simultaneously or stepwise.

[0088] The pressure-sensitive adhesive composition can be applied using a known or commonly used coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a die coater, a bar coater, a knife coater, a spray coater, etc. Alternatively, the pressure-sensitive adhesive composition may be applied by impregnation, a curtain coating method, or the like. From the viewpoints of promoting the crosslinking reaction, improving production efficiency, etc., the pressure-sensitive adhesive composition is preferably dried under heating. The drying temperature can be, for example, about 40 to 150° C., and is usually preferably about 60 to 130° C. After drying the pressure-sensitive adhesive composition, aging may be further performed for the purpose of adjusting the component migration in the pressure-sensitive adhesive layer, advancing the crosslinking reaction, and relaxing distortion that may exist in the substrate or pressure-sensitive adhesive layer, etc.

[0089] (Thickness) Although not particularly limited, the thickness of the adhesive layer is, for example, about 1 μm or more, preferably about 2 μm or more (for example, about 3 μm or more), and may be 4 μm or more. The thickness can be, for example, about 100 μm or less, and is preferably about 50 μm or less (for example, about 30 μm or less), preferably about 25 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, may be 10 μm or less, or may be 8 μm or less. The adhesive layer having the above thickness is suitable as an adhesive layer for surface protection film applications.

[0090] (Gel fraction) Although not particularly limited, the gel fraction of the adhesive layer is preferably 70% or more. An adhesive having a gel fraction of 70% or more is unlikely to undergo deformation or damage such as dents due to external forces during, for example, production, and is unlikely to undergo changes in appearance. Such an adhesive is likely to become an adhesive sheet having a smooth surface, and is preferable because it enables high-precision inspection when, for example, forming a transparent adhesive sheet and inspecting an adherend through the adhesive sheet. In addition, by setting the gel fraction high, an adhesive having excellent removability is likely to be formed. From this viewpoint, the gel fraction is more preferably more than 80%, and may be more than 85% (e.g., 90% or more), may be 92% or more, or may be 94% or more (e.g., 95% or more). The gel fraction may be 100%, but from the viewpoint of adhesion to an adherend, it may be, for example, less than 99% or less than 95% (e.g., 94% or less).

[0091] The gel fraction of the adhesive layer is measured by the following method. W1g is taken from the adhesive layer and wrapped in a porous PTFE (polytetrafluoroethylene) sheet to prepare a sample. The sample is placed in a glass bottle, immersed in an ethyl acetate solution, and left to stand for 7 days, after which the sample is taken out and dried at 130°C for 2 hours. The dried sample is weighed, and the weight of the porous PTFE sheet is subtracted from it to determine the weight of the adhesive after drying, W2g. W1 and W2 are substituted into the following formula to calculate the gel fraction [%]. Gel fraction [%] = (W2 / W1) × 100 As the porous PTFE sheet, "TEMISH" (trade name) manufactured by Nitto Denko Corporation or an equivalent product can be used. The same applies to the examples described below.

[0092] (Biomass carbon ratio) In some embodiments, the pressure-sensitive adhesive layer contains a biomass-derived material, and the biomass carbon ratio thereof may be a predetermined value or more. The biomass carbon ratio of the pressure-sensitive adhesive layer is, for example, 1% or more, and may be 10% or more, preferably 30% or more, and more preferably 50% or more. A high biomass carbon ratio of the pressure-sensitive adhesive means that the amount of fossil resource-based materials, such as petroleum, used is small. In this respect, the higher the biomass carbon ratio of the pressure-sensitive adhesive, the more preferable it is. For example, the biomass carbon ratio of the pressure-sensitive adhesive layer may be 55% or more, 60% or more, 70% or more, 75% or more, 80% or more, or more than 80%. The upper limit of the biomass carbon ratio is 100% by definition, and may be 99% or less, and from the viewpoint of material availability, it may be 95% or less, or 90% or less. From the viewpoint of easily exerting good adhesive performance, in some embodiments, the biomass carbon ratio of the pressure-sensitive adhesive layer may be, for example, 90% or less, 85% or less, or 80% or less.

[0093] (base material) The material of the support substrate used as the support of the adhesive sheet disclosed herein is not particularly limited, and for example, a resin film can be preferably used. The resin film can be a resin material formed into a film shape from various resin materials. The resin material is preferably one that can form a resin film excellent in one or more of the following properties: transparency, mechanical strength, thermal stability, moisture shielding property, isotropy, etc. For example, a resin film made of a resin material containing polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate; celluloses such as diacetyl cellulose and triacetyl cellulose; polycarbonates; acrylic polymers such as polymethyl methacrylate; etc. as the main component (i.e., a component contained in more than 50% by weight) can be preferably used as the substrate. Other examples of the resin material constituting the resin film include those mainly composed of styrene-based polymers such as polystyrene and acrylonitrile-styrene copolymers; polyolefins such as polyethylene, polypropylene, polyolefins having a cyclic or norbornene structure, ethylene-propylene copolymers, etc.; polyvinyl chlorides; polyamides such as nylon 6, nylon 6,6, and aromatic polyamides; etc. Alternatively, a resin film composed of a resin material mainly composed of polyimides, polysulfones, polyethersulfones, polyetheretherketones, polyphenylene sulfides, fluorine-based resins, polyvinyl alcohols, polyvinyl acetates, polyvinylidene chlorides, polyvinyl butyrals, polyarylates, polyoxymethylenes, epoxy resins, etc. may be used as the substrate. The resin material constituting the resin film may be a blend of two or more of these.

[0094] In this specification, the term "resin film" refers to a resin film that has a non-porous structure and typically does not substantially contain air bubbles (void-free). Therefore, the resin film is a concept that is distinct from foam films, nonwoven fabrics, and woven fabrics.

[0095] Other examples of the substrate include foam sheets made of foams such as polyurethane foam, polyethylene foam, and polychloroprene foam; woven and nonwoven fabrics made by single or mixed spinning of various fibrous materials (natural fibers such as hemp and cotton, synthetic fibers such as polyester and vinylon, and semi-synthetic fibers such as acetate); papers such as Japanese paper, fine paper, craft paper, and crepe paper; metal foils such as aluminum foil and copper foil; and glass. Substrates having a composite structure of these may also be used. Examples of substrates having such a composite structure include substrates having a structure in which metal foil and the above-mentioned plastic film are laminated, and plastic sheets reinforced with inorganic fibers such as glass cloth.

[0096] The substrate may be formed from a material derived from biomass or a material derived from non-biomass. From the viewpoint of producing a PSA sheet that takes into consideration the reduction of dependency on fossil resource-based materials, a substrate material derived from biomass (typically a resin film) is preferably used.

[0097] The substrate may be formed using a recyclable material or a recycled material (also called a recycled material). A resin film is preferably used as such a recycled material. Since a resin film (for example, a polyester film such as a PET film) is recyclable, it is possible to continuously reproduce the resin film after use, regardless of whether or not a plant-derived material is used, and the environmental load can be reduced by reusing the resin film after use. Such a recyclable resin film or recycled resin film is also called a recycled film. The recycled material (for example, a recycled film) may be formed from a biomass-derived material or a non-biomass-derived material.

[0098] In some preferred embodiments, the substrate is a resin film (polyester resin film) formed from a resin (polyester resin) containing polyester as the main component (a component contained in an amount of more than 50% by weight). For example, a resin film in which the polyester is mainly PET (PET film), a resin film in which the polyester is mainly PEN (PEN film), etc. can be preferably used.

[0099] The substrate may have a single layer structure or a multilayer structure. Therefore, the resin film that can be used as the substrate may also have a single layer structure or a multilayer structure of two or more layers (for example, a three-layer structure). A resin film with a single layer structure can be preferably used as the substrate.

[0100] The above-mentioned substrate (typically a resin film) may contain various additives such as antioxidants, ultraviolet absorbers, antistatic components, plasticizers, colorants (pigments, dyes, etc.) as necessary.

[0101] The adhesive layer side surface of the substrate may be subjected to a surface treatment such as chromate treatment, ozone exposure, flame exposure, high-voltage shock exposure, ionizing radiation treatment, etc. Such a surface treatment may be, for example, a treatment for enhancing adhesion between the substrate and the adhesive layer. In some embodiments, the adhesive layer side surface of the substrate may be subjected to a primer treatment. From the viewpoint of adhesion with the silicone-based adhesive, a silicone primer treatment is preferred. In some embodiments, the back surface of the substrate may be subjected to a hard coat treatment. This improves the scratch resistance of the back surface of the substrate, and when the adhesive sheet is used as a protective sheet, it may exhibit better protective performance. In other embodiments, the substrate may be subjected to an antistatic treatment from the viewpoint of suppressing the generation of static electricity. The substrate may also be subjected to various treatments such as antifouling, antifingerprinting, antiglare, and antireflection.

[0102] The thickness of the substrate can be appropriately selected in consideration of the application, purpose, and usage form of the pressure-sensitive adhesive sheet. From the viewpoint of workability such as strength and handling, a substrate having a thickness of about 10 μm or more is suitable, and the thickness is preferably about 20 μm or more, and more preferably about 30 μm or more (e.g., 35 μm or more). From the viewpoint of cost, the thickness of the substrate is suitable to be about 200 μm or less, preferably about 150 μm or less, more preferably about 100 μm or less, and even more preferably about 75 μm or less (e.g., 50 μm or less). Substrates having the above thickness are suitable as substrates for protective films, for example.

[0103] (Adhesive sheet characteristics) The adhesive strength of the adhesive sheet is not limited to a specific range, since it can be appropriately set according to the purpose of use and the application site. In some embodiments, the adhesive sheet preferably has an adhesive strength of 2.0 N / 25 mm or less to an optical member (e.g., a polarizing plate) measured under conditions of 23° C., 50% RH, peel angle of 180°, and tensile speed of 0.3 m / min. An adhesive sheet satisfying this characteristic has a low peel strength (adhesive strength) when peeled from an adherend, which is an object to be protected, and is therefore easy to peel. From the viewpoint of peeling workability, the adhesive strength is more preferably 1.0 N / 25 mm or less, even more preferably 0.5 N / 25 mm or less, and particularly preferably 0.1 N / 25 mm or less (e.g., less than 0.1 N / 25 mm). From the viewpoint of adhesion to the adherend and protection of the adherend, the adhesive strength is suitably 0.01 N / 25 mm or more, may be 0.03 N / 25 mm or more, or may be 0.05 N / 25 mm or more. Specifically, the adhesive strength is measured by the method described in the Examples below.

[0104] The adhesive sheet disclosed herein has reduced staining properties on the adherend. The staining properties of the adhesive sheet can be evaluated by analyzing the presence or absence of adhesion on the adherend surface after peeling and removal in a test in which the adhesive sheet is attached to the adherend and left to stand for a predetermined time, and then peeled and removed from the adherend, using various methods. The method for analyzing the adherend surface can be, for example, an optical method.

[0105] Specifically, the staining property of the adherend is evaluated by attaching the pressure-sensitive adhesive sheet to the surface of an optical component (e.g., a polarizing plate), leaving it to stand for 24 hours in an environment of 23°C and 50% RH, and then peeling and removing the attached pressure-sensitive adhesive sheet from the optical component. initial and the reflected chromaticity b* of the optical component after peeling after Each was measured using a spectrophotometer, and the reflection chromaticity b* initial and reflected chromaticity b* after The reflectance can be evaluated by calculating the reflection chromaticity change |Δb*|, which is the absolute value of the difference between the reflectance and the reflectance. The smaller the reflectance chromaticity change |Δb*|, the lower the staining tendency of the adhesive to the adherend, and the larger the reflectance chromaticity change |Δb*|, the higher the staining tendency of the adhesive to the adherend. More specifically, the reflectance chromaticity change |Δb*| is measured by the method described in the Examples below. In some embodiments, the reflectance chromaticity change |Δb*| is preferably 3.5 or less, more preferably 3.0 or less, even more preferably 2.0 or less, and particularly preferably 1.0 or less. The reflectance chromaticity change |Δb*| is, in principle, 0 or more.

[0106] In addition, the adhesive sheet disclosed herein suppresses zipping during high-speed peeling. Zipping evaluation of the adhesive sheet can be performed, for example, by attaching the adhesive sheet to the surface of an optical member (e.g., a polarizing plate), and performing a tensile test at a peeling angle of 180° and a tensile speed of 30 m / min under an environment of 23°C and 50% RH, by an examiner checking whether or not peeling noise occurs. Specifically, it is evaluated by the method described in the examples below.

[0107] In some embodiments, the pressure-sensitive adhesive sheet preferably has a transparency of about 50% or more in total light transmittance. A transparent pressure-sensitive adhesive sheet having a total light transmittance of 80% or more (e.g., 85% or more) is more preferable. The upper limit of the total light transmittance may be about 99% or less (e.g., 95% or less) in applications requiring transparency. A pressure-sensitive adhesive sheet having such transparency is preferable because it enables high-precision inspection, for example, when inspecting an adherend through the pressure-sensitive adhesive sheet. Such a pressure-sensitive adhesive sheet is suitable as an optical surface protection film. The value of the total light transmittance can be a value measured in accordance with JIS K 7361-1.

[0108] <Applications of adhesive sheets> The adhesive sheet having the adhesive layer formed from the adhesive composition disclosed herein can be used for various applications. The adhesive disclosed herein has low contamination, suppresses zipping, and has light peelability and excellent peeling workability when peeled off again, so that, for example, it is suitable as a surface protection film that is usually peeled off (re-peeled off) from the object to be protected after being attached to the object to be protected and achieving its protection purpose. The object to be protected by the surface protection film is not particularly limited, and it can be used as a surface protection film for various products, parts, etc. For example, the surface protection film is particularly suitable as a surface protection film that protects the surface of optical components (for example, optical components used as components of liquid crystal display panels such as polarizing plates and wave plates) during processing or transportation of the optical components. More specifically, the surface protection film is suitable for applications in which the optical components used as components of liquid crystal display panels, plasma display panels (PDPs), organic electroluminescence (EL) displays, etc. are protected during production, transportation, etc. In particular, it is useful as a surface protection film applied to optical components such as polarizing plates (polarizing films, for example, reflective polarizing films) for liquid crystal display panels, wave plates, retardation plates, optical compensation films, brightness enhancement films, light diffusion sheets, and reflective sheets.

[0109] In addition, in some embodiments, the PSA composition disclosed herein may contain an acrylic polymer with a high biomass carbon ratio, and therefore can be used as a substitute for a conventional acrylic PSA in various applications in which the acrylic PSA is used (i.e., an acrylic PSA with a low biomass carbon ratio), thereby contributing to reducing dependency on fossil resource-based materials. The PSA sheet disclosed herein can typically be preferably used as a PSA sheet (surface protection film) with reduced dependency on fossil resource-based materials.

[0110] <Optical component with adhesive sheet> According to the technology disclosed herein, an optical member with a pressure-sensitive adhesive sheet is provided. The optical member with a pressure-sensitive adhesive sheet disclosed herein includes a pressure-sensitive adhesive sheet and an optical member. Any of the pressure-sensitive adhesive sheets disclosed herein can be used as the pressure-sensitive adhesive sheet. The optical member with a pressure-sensitive adhesive sheet is a laminate formed by laminating the pressure-sensitive adhesive sheet on at least one surface of an optical member.

[0111] The optical member in the optical member with the adhesive sheet can be the same as that described as the optical member as the adherend used to measure the shear force of the adhesive layer described above. The overlapping description of the optical member will be omitted. A preferred example of the optical member as a component of the optical member with the adhesive sheet is a polarizing plate. The polarizing plate generally has a configuration in which a polarizing film is sandwiched between two triacetyl cellulose (TAC) films. Of the two TAC films, at least the TAC film arranged on the side to which the adhesive sheet is attached is preferably protected on its surface (attached surface) with a hard coat layer. The hard coat layer is preferably made of a urethane acrylate-based material. In addition, the polarizing plate is preferably configured such that an anti-reflection layer is further provided on the hard coat layer. The optical member with the adhesive sheet disclosed herein typically has a configuration in which an adhesive sheet is attached to the anti-reflection layer that constitutes the surface of the polarizing plate. The configuration of the main body part other than the surface of the polarizing plate may be a normal configuration for functioning as a polarizing plate, and since it is not closely related to the present invention, a description thereof will be omitted.

[0112] The structure of an optical member with an adhesive sheet according to an embodiment is shown in FIG. 2. In the embodiment shown in FIG. 2, the optical member is a polarizing plate 210. The optical member with an adhesive sheet 200 includes a sheet-like polarizing plate 210 having a first surface 210A and a second surface 210B, and an adhesive sheet 220 arranged on the first surface 210A side. Here, the polarizing plate 210 includes a polarizing plate main body 214 including a polarizer, and an antireflection layer 212 arranged on at least one surface of the polarizing plate main body 214, and the surface constituting the first surface 210A of the polarizing plate 210 is composed of the antireflection layer 212. The adhesive sheet 220 is configured as a single-sided adhesive sheet with a substrate, which includes a sheet-like supporting substrate (e.g., a resin film) 226 having a first surface 226A and a second surface 226B, and an adhesive layer 224 provided on the first surface 226A side. The adhesive layer 224 is fixedly provided on the first surface 226A side of the supporting substrate 226, i.e., without any intention of separating the adhesive layer 224 from the supporting substrate 226. The single-sided adhesive sheet 220 is laminated on the first surface 210A of the polarizing plate 210 via the adhesive layer 224.

[0113] The matters disclosed by this specification include the following: [1] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer contains an acrylic polymer, The acrylic polymer is a polymer of a monomer component including an alkyl (meth)acrylate (m1) having an alkyl group having 6 to 17 carbon atoms at an ester terminal, wherein the alkyl group having 6 to 17 carbon atoms is a linear alkyl group or a branched alkyl group having one carbon atom in the branch, The adhesive layer has an adhesive area of ​​1 cm 2 was attached to an optical component and pulled in the shear direction at a pulling speed of 0.06 mm / min in an environment of 23°C and 50% RH, resulting in a shear force of 17 N / cm 2 That's it, the adhesive sheet. [2] The pressure-sensitive adhesive sheet according to the above-mentioned [1], wherein the alkyl (meth)acrylate (m1) includes at least one selected from n-heptyl acrylate and n-octyl acrylate. [3] The pressure-sensitive adhesive sheet according to the above [1] or [2], wherein the monomer component further contains (meth)acrylic acid. [4] The pressure-sensitive adhesive sheet according to any one of the above [1] to [3], wherein the acrylic polymer has a glass transition temperature of −55° C. or lower, calculated based on the composition of the monomer components. [5] The pressure-sensitive adhesive sheet according to any one of the above [1] to [4], wherein the pressure-sensitive adhesive layer contains an epoxy-based crosslinking agent. [6] The pressure-sensitive adhesive sheet according to any one of the above [1] to [5], wherein the pressure-sensitive adhesive layer has a gel fraction of 70% or more. [7] The pressure-sensitive adhesive sheet (or optical surface protection film) according to any one of the above [1] to [6], which is used for protecting the surface of an optical member. [8] An optical member with an adhesive sheet (or an optical member with a surface protective film) configured by attaching the adhesive sheet according to any one of [1] to [7] above to at least one surface of an optical member. EXAMPLES

[0114] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples. In the following description, "%" and "parts" are by weight unless otherwise specified.

[0115] <Preparation of acrylic polymer> (Preparation example A1) In a flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet tube and a thermometer, 95 parts of n-heptyl acrylate (HpA) and 5 parts of acrylic acid (AA) as monomer components, and ethyl acetate (polymerization solvent) were charged to a solid concentration (polymerization concentration) of 35%, and 0.2 parts of azobisisobutyronitrile (AIBN) was further charged as a polymerization initiator. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 63°C and polymerization reaction was carried out for 7 hours to obtain a solution of acrylic polymer (A1). The weight average molecular weight (Mw) of the obtained acrylic polymer (A1) was 920,000. The Tg derived from the Fox formula of the acrylic polymer (A1) was -65.2°C. The above HpA is a compound synthesized using heptyl alcohol derived from biomass and having a heptyl group derived from biomass at the ester end.

[0116] (Preparation example A2) In a flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet tube and a thermometer, 95 parts of n-heptyl acrylate (HpA) and 5 parts of acrylic acid (AA) as monomer components, and ethyl acetate (polymerization solvent) were charged to a solid concentration of 30%, and 0.05 parts of AIBN were further added as a polymerization initiator. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 63°C and polymerization reaction was carried out for 3 hours to obtain a solution of acrylic polymer (A2). The Mw of the obtained acrylic polymer (A2) was 810,000. The Tg of the acrylic polymer (A2) calculated from the Fox formula was -65.2°C. The above HpA is a compound synthesized using heptyl alcohol derived from biomass and having a biomass-derived heptyl group at the ester end.

[0117] (Preparation example A3) In a flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet tube and a thermometer, 95 parts of n-heptyl acrylate (HpA) and 5 parts of acrylic acid (AA) as monomer components, and ethyl acetate (polymerization solvent) were charged to a solid concentration of 30%, and 0.05 parts of AIBN were further added as a polymerization initiator. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 63°C and polymerization reaction was carried out for 5 hours to obtain a solution of acrylic polymer (A3). The Mw of the obtained acrylic polymer (A3) was 920,000. The Tg of the acrylic polymer (A3) calculated from the Fox formula was -65.2°C. The above HpA is a compound synthesized using heptyl alcohol derived from biomass and having a biomass-derived heptyl group at the ester end.

[0118] (Preparation example A4) In a flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet tube and a thermometer, 95 parts of n-heptyl acrylate (HpA) and 5 parts of acrylic acid (AA) as monomer components, and ethyl acetate (polymerization solvent) were charged to a solid concentration of 30%, and 0.05 parts of AIBN were further added as a polymerization initiator. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 63°C and polymerization reaction was carried out for 7 hours to obtain a solution of acrylic polymer (A4). The Mw of the obtained acrylic polymer (A4) was 840,000. The Tg derived from the Fox formula of the acrylic polymer (A3) was -65.2°C. The above HpA is a compound synthesized using heptyl alcohol derived from biomass and having a biomass-derived heptyl group at the ester end.

[0119] (Preparation example A5) In a flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet tube and a thermometer, 95 parts of n-butyl acrylate (BA) and 5 parts of acrylic acid (AA) as monomer components, and ethyl acetate (polymerization solvent) were charged to a solid concentration of 30%, and 0.2 parts of AIBN were added as a polymerization initiator. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 63°C and polymerization reaction was carried out for 7 hours to obtain a solution of acrylic polymer (A5). The weight average molecular weight (Mw) of the obtained acrylic polymer (A5) was 630,000. The Tg of the acrylic polymer (A5) calculated by the Fox formula was -49.3°C.

[0120] (Preparation example A6) In a flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet tube and a thermometer, 95 parts of 2-ethylhexyl acrylate (2EHA) and 5 parts of acrylic acid (AA) as monomer components, and ethyl acetate (polymerization solvent) were charged to a solid concentration of 40%, and 0.2 parts of AIBN were added as a polymerization initiator. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 60°C to carry out a polymerization reaction for 4 hours, and then the mixture was aged at 70°C for 4 hours to obtain a solution of acrylic polymer (A6). The Mw of the obtained acrylic polymer (A6) was 630,000. The Tg of the acrylic polymer (A6) calculated by the Fox formula was -66.2°C.

[0121] (Preparation example A7) In a flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet tube and a thermometer, 95 parts of n-heptyl acrylate (HpA) and 5 parts of acrylic acid (AA) as monomer components, and ethyl acetate (polymerization solvent) were charged to a solid concentration of 30%, and 0.2 parts of AIBN were further added as a polymerization initiator. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 63°C and polymerization reaction was carried out for 7 hours to obtain a solution of acrylic polymer (A7). The Mw of the obtained acrylic polymer (A7) was 660,000. The Tg of the acrylic polymer (A7) calculated from the Fox formula was -65.2°C. The above HpA is a compound synthesized using heptyl alcohol derived from biomass and having a biomass-derived heptyl group at the ester end.

[0122] For each of the acrylic polymers (A1) to (A7) obtained in Preparation Examples A1 to A7, the weight fraction [%] of molecular weights of 100,000 or less was calculated by GPC measurement, and the results are shown in the corresponding columns in Table 1.

[0123] <Example 1> (Preparation of Pressure-Sensitive Adhesive Composition) The solution of the acrylic polymer (A1) obtained in Preparation Example A1 was diluted with ethyl acetate to a solid concentration of 22%, and 6 parts (solid content) of an epoxy crosslinking agent (B1) (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Tetrad C") was added to this solution per 100 parts solid content of the solution, followed by stirring to obtain an acrylic pressure-sensitive adhesive composition according to this example.

[0124] (Preparation of adhesive sheet) The acrylic adhesive composition immediately after blending was applied onto a polyethylene terephthalate (PET) film (thickness 38 μm) and the solvent was removed by drying at 130° C. for 1 minute to form an adhesive layer (thickness 5 μm). The surface of the adhesive layer was then covered with a release film and aged for 3 days in a temperature environment of 50° C. to obtain an adhesive sheet according to this example.

[0125] <Example 2> An adhesive composition was prepared in the same manner as in Example 1, except that the acrylic polymer used was changed to the acrylic polymer (A2) obtained in Preparation Example A2. This adhesive composition was used to obtain an adhesive sheet according to this example in the same manner as in Example 1.

[0126] <Example 3> An adhesive composition was prepared in the same manner as in Example 1, except that the acrylic polymer used was changed to the acrylic polymer (A3) obtained in Preparation Example A3. This adhesive composition was used to obtain an adhesive sheet according to this example in the same manner as in Example 1.

[0127] <Example 4> An adhesive composition was prepared in the same manner as in Example 1, except that the acrylic polymer used was changed to the acrylic polymer (A4) obtained in Preparation Example A4. This adhesive composition was used to obtain an adhesive sheet according to this example in the same manner as in Example 1.

[0128] <Comparative Example 1> An adhesive composition was prepared in the same manner as in Example 1, except that the acrylic polymer used was changed to the acrylic polymer (A5) obtained in Preparation Example A5. This adhesive composition was used to obtain an adhesive sheet according to this example in the same manner as in Example 1.

[0129] <Comparative Example 2> An adhesive composition was prepared in the same manner as in Example 1, except that the acrylic polymer used was changed to the acrylic polymer (A6) obtained in Preparation Example A6. This adhesive composition was used to obtain an adhesive sheet according to this example in the same manner as in Example 1.

[0130] <Comparative Example 3> An adhesive composition was prepared in the same manner as in Example 1, except that the acrylic polymer used was changed to the acrylic polymer (A7) obtained in Preparation Example A7. This adhesive composition was used to obtain an adhesive sheet according to this example in the same manner as in Example 1.

[0131] <Evaluation> (Gel fraction of adhesive layer) The gel fraction of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet of each example was measured by the method described above, and the resulting gel fractions are shown in the corresponding columns in Table 1.

[0132] (shear force measurement) As shown in FIG. 3, the adhesive sheet of each example was cut to a size of 10 mm wide and 50 mm long, and the release film was peeled off to prepare a shear force measurement sample (adhesive sheet) 340. In addition, an anti-reflection film 350 was prepared by the method described below. The anti-reflection film 350 was used after being cut to a size of 70 mm long and 100 mm wide. A portion A of 10 mm×10 mm at one end of the shear force measurement sample 340 was attached to the upper end center of the anti-reflection layer side surface of the anti-reflection film 350 in a direction such that the shear force measurement sample 340 protrudes from the anti-reflection film 350. Next, a portion B of 10 mm×10 mm at the other end of the shear force measurement sample 340 was clamped by a chuck 342, and the lower end center of the anti-reflection film 340 was clamped by a chuck 344. Under conditions of 23°C and 50% RH, the sample 340 for shear force measurement was pulled in the length direction (i.e., shear direction) using a universal tension and compression tester (manufactured by Shimadzu Corporation, product name "AUTOGRAPH AG-X plus") under conditions of an initial chuck distance of 60 mm and a pulling speed of 0.06 mm / min. The maximum stress measured until the pulling distance reached 2.0 mm was defined as the shear force (unit: N / cm 2 The shear forces obtained are shown in the corresponding columns in Table 1.

[0133] (Adhesive strength measurement) The adhesive sheet of each example was cut to a size of 25 mm wide and 100 mm long, and the release film was peeled off to expose the adhesive surface. The adhesive sheet was roll-pressed to the anti-reflection layer side surface of an anti-reflection film cut to a size of 70 mm wide and 100 mm long at a pressure of 0.25 MPa and a feed rate of 0.3 m / min to obtain a sample for measuring adhesive strength. The sample for measuring adhesive strength was left to stand for 30 minutes in an environment of 23°C and 50% RH, and then a tensile test was performed in the same environment using a high-speed peel tester (manufactured by Kyowa Interface Science Co., Ltd., product name "VPA-H200") at a peel angle of 180° and a tensile speed of 300 mm / min to measure the adhesive strength (unit: N / 25 mm). The obtained adhesive strength is shown in the corresponding column of Table 1.

[0134] (Reflected chromaticity change |Δb*|) A black acrylic plate (2.0 mm thick, manufactured by Mitsubishi Chemical Corporation) was attached to the back surface of the anti-reflection film (i.e., the surface opposite to the anti-reflection layer side) via a transparent acrylic adhesive having a thickness of about 20 μm. The reflection chromaticity b* of the surface on the anti-reflection layer side of this anti-reflection film with the black acrylic plate was initial was measured using a spectrophotometer (manufactured by Hitachi, Ltd., product name "U-4100"). Next, the release film was peeled off from the adhesive sheet of each example to expose the adhesive surface, and then the adhesive surface of the adhesive sheet was attached to the anti-reflection layer side surface of the anti-reflection film with the black acrylic plate, and left to stand for 24 hours in an environment of 23°C and 50% RH. Thereafter, the adhesive sheet attached to the anti-reflection film was peeled off and removed, and the reflective chromaticity b* of the surface of the anti-reflection film where the adhesive sheet was attached was measured. after The reflection chromaticity b* of the surface of the anti-reflection film before the adhesive sheet was attached was measured using the spectrophotometer. initial and the reflected chromaticity b* after peeling after The absolute value of the difference between these values ​​was calculated and taken as the reflected chromaticity change |Δb*|. The reflected chromaticity change |Δb*| obtained is shown in the corresponding column in Table 1.

[0135] (Evaluation of zipping during high speed peeling) The adhesive sheet of each example was cut to a size of 25 mm wide and 100 mm long, and the release film was peeled off to expose the adhesive surface. The adhesive sheet was roll-pressed to the anti-reflection layer side surface of an anti-reflection film cut to a size of 70 mm wide and 100 mm long at a pressure of 0.25 MPa and a feed rate of 0.3 m / min to prepare a sample for zipping evaluation. The sample for zipping evaluation was left to stand for 30 minutes in an environment of 23°C and 50% RH, and then in the same environment, a high-speed peel tester (manufactured by Kyowa Interface Science Co., Ltd., product name "VPA-H200") was used to perform a tensile test at a peel angle of 180° and a tensile speed of 30 m / min. The peeling sound was confirmed by the tester's ears. If no peeling sound was confirmed, the zipping evaluation was G (good), and if a peeling sound was confirmed, the zipping evaluation was P (bad). The results of the zipping evaluation during high-speed peeling are listed in the corresponding columns of Table 1.

[0136] (Anti-reflective film as an adherend) The antireflection film as the adherend used for evaluating the shear force, adhesive force, reflected chromaticity change |Δb*|, and zipping during high-speed peeling of the pressure-sensitive adhesive sheets according to the Examples and Comparative Examples of the present application was prepared by the following procedures (1) to (4). This antireflection film has the same structure as the surface treatment layer that constitutes the surface of a polarizing plate, so the results of the shear force, adhesive force, reflected chromaticity change |Δb*|, and zipping evaluation during high-speed peeling measured using the antireflection film as the adherend can be considered to be the same as the results of the shear force, adhesive force, reflected chromaticity change |Δb*|, and zipping evaluation during high-speed peeling measured using a polarizing plate, particularly a polarizing plate having a surface treatment layer such as an antireflection layer on its surface, as the adherend.

[0137] (1) Preparation of Coating Solution for Forming Hard Coat Layer A resin solution in which an ultraviolet-curable resin monomer or oligomer mainly composed of urethane acrylate is dissolved in butyl acetate (manufactured by DIC Corporation, product name "UNIDIC 17-806", solid content concentration 80%) was added with 5 parts of a photopolymerization initiator (manufactured by Ciba Japan Co., Ltd., product name "IRGACURE906") and 0.01 parts of a leveling agent (manufactured by DIC Corporation, product name "GRANDIC PC4100") per 100 parts of solid content of the resin solution. Then, butyl acetate was added to the resin solution so that the solid content concentration of the resin solution was 75%. Furthermore, cyclopentanone (hereinafter referred to as "CPN") was added to the resin solution so that the solid content concentration of the resin solution was 50%. In this way, a hard coat layer forming coating liquid for forming a hard coat layer was prepared.

[0138] (2) Preparation of coating solution for forming anti-reflection layer 100 parts of a polyfunctional acrylate mainly composed of pentaerythritol triacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., product name "Viscoat #300", solid content 100%), 100 parts of hollow nanosilica particles (manufactured by JGC Catalysts and Chemicals Co., Ltd., product name "Suluria 5320", solid content 20%, weight average particle diameter 75 nm), 12 parts of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KY-1203", solid content 20%), and 3 parts of a photopolymerization initiator (manufactured by BASF, product name "OMNIRAD907", solid content 100%) were mixed. A mixed solvent of TBA (tertiary butyl alcohol), MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 was added as a dilution solvent to the mixture so that the total solid content was 4%, and the mixture was stirred to prepare a coating liquid for forming an antireflection layer.

[0139] (3) Formation of hard coat layer The above hard coat layer-forming coating solution was applied onto a transparent TAC (triacetyl cellulose) film (manufactured by Fuji Film Corporation, product name "TD80UL", thickness 80 μm, refractive index 1.49) using a die coater so that the thickness of the coating film (hard coat layer) after curing would be 7.5 μm. The coating film was dried at 80° C. for 2 minutes. Thereafter, the coating film was irradiated with a high-pressure mercury lamp with an integrated light amount of 300 mJ / cm. 2 The resin monomer was polymerized by irradiating the triacetyl cellulose film with ultraviolet light of 1000 nm to form a hard coat layer on the triacetyl cellulose film.

[0140] (4) Formation of an anti-reflection layer The antireflection layer-forming coating liquid was applied onto the hard coat layer using a wire bar. The applied coating liquid was heated at 80°C for 1 minute and dried to form a coating film (antireflection layer). After drying, the coating film was irradiated with a high-pressure mercury lamp with an integrated light quantity of 300 mJ / cm. 2 The coating film was cured by irradiating it with ultraviolet light of 1000 nm to form an antireflection layer having a thickness of 0.1 μm. In this manner, an antireflection film having a structure of TAC film / hard coat layer / antireflection layer was produced.

[0141] The outline of each example and the evaluation results are shown in Table 1.

[0142] [Table 1]

[0143] As shown in Table 1, HpA (a linear alkyl group having 7 carbon atoms) was used as the monomer component of the acrylic polymer contained in the adhesive, and the shear force was 17 N / cm 2 It is clear that the pressure-sensitive adhesive sheets of Examples 1 to 4 have smaller reflected chromaticity changes |Δb*| and reduced staining properties compared to the pressure-sensitive adhesive sheet of Comparative Example 2, which used 2EHA as the monomer component of the acrylic polymer contained in the pressure-sensitive adhesive. Furthermore, it was confirmed that the pressure-sensitive adhesive sheets of Examples 1 to 4 exhibit lighter peelability than the pressure-sensitive adhesive sheet of Comparative Example 2.

[0144] In addition, Comparative Example 1, which used BA as a monomer component of the acrylic polymer contained in the adhesive, was rated P (poor) in the zipping evaluation during high-speed peeling. The occurrence of zipping can also be a cause of adhesive residue on the adherend.

[0145] In addition, HpA (a straight-chain alkyl group with seven carbon atoms) is used as the monomer component of the acrylic polymer contained in the adhesive, and the shear force is 17 N / cm 2 The pressure-sensitive adhesive sheets of Examples 1 to 4 described above use HpA as a monomer component of the acrylic polymer contained in the pressure-sensitive adhesive, and the shear force is 17 N / cm 2 It was confirmed that the reflected chromaticity change |Δb*| was smaller than that of the pressure-sensitive adhesive sheet of Comparative Example 3, which was less than |Δb*|, and that the staining of the adherend was further reduced.

[0146] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Explanation of symbols]

[0147] 100 Adhesive sheet with release liner 130 Adhesive Sheet 132 Supporting base material 132A Front page 132B Second side 134 Adhesive layer 134A Surface (adhesive surface) 136 Release Liner 200 Optical components with adhesive sheets 210 Polarizing plate 210A Front page 210B second side 212 Anti-reflection layer 214 Polarizing plate body 220 Adhesive Sheet 224 Adhesive layer 226 Supporting base material 226A Front page 226B Second side 340 Shear force measurement sample (adhesive sheet) 342, 344 Chuck 350 Anti-reflective film

Claims

1. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer contains an acrylic polymer, The acrylic polymer is a polymer of a monomer component including an alkyl(meth)acrylate (m1) having an alkyl group having 6 to 17 carbon atoms at an ester terminal, wherein the alkyl group having 6 to 17 carbon atoms is a linear alkyl group or a branched alkyl group having one carbon atom in the branch, The adhesive area of ​​the adhesive layer is 1 cm 2 was attached to an optical member, and pulled in the shear direction at a pulling speed of 0.06 mm / min under an environment of 23°C and 50% RH, resulting in a shear force of 17 N / cm 2 That's it, the adhesive sheet.

2. The pressure-sensitive adhesive sheet according to claim 1, wherein the alkyl (meth)acrylate (m1) comprises at least one selected from the group consisting of n-heptyl acrylate and n-octyl acrylate.

3. The pressure-sensitive adhesive sheet according to claim 1 , wherein the monomer component further comprises (meth)acrylic acid.

4. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the acrylic polymer has a glass transition temperature of −55° C. or lower, calculated based on the composition of the monomer components.

5. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer contains an epoxy-based crosslinking agent.

6. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer has a gel fraction of 70% or more.

7. The pressure-sensitive adhesive sheet according to claim 1 or 2, which is used for protecting the surface of an optical member.

8. 3. An optical member with a pressure-sensitive adhesive sheet, comprising an optical member having the pressure-sensitive adhesive sheet according to claim 1 or 2 attached to at least one surface of the optical member.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive for protective sheets

    JP4682299B2

  • Adhesive agent, adhesive tape, electrical appliance, onboard member, and securing method

    WO2021125247A1

  • Adhesive agent composition, adhesive tape, affixing method for electronic device component or in-vehicle component, and production method for electronic device component or in-vehicle component

    WO2021125278A1