Power storage module and power storage element
By using a thick spacer and solid graphite in power storage modules, the issues of electrode misalignment and deformation are mitigated, ensuring high output retention rates despite repeated charging and discharging.
Patent Information
- Application Number
- JP2023071065
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
In power storage modules, gaps between the electrode body and the container can lead to uneven spacing between positive and negative electrodes, misalignment, and reduced charging and discharging performance, as well as deformation of the container under load, especially when using graphite as the negative electrode active material.
Incorporating a relatively thick spacer between the electrode body and the container, with a ratio of the spacer's total thickness to the container's inner dimension of 0.5% or more, and using solid graphite as the negative electrode active material to minimize expansion and contraction during charging and discharging.
This configuration maintains high output retention rates after charge/discharge cycles by reducing the impact of electrode expansion and contraction, thereby minimizing output decrease.
Smart Images

Figure 2024156526000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an energy storage module and an energy storage element. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. Non-aqueous electrolyte secondary batteries generally have a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring charge-transporting ions between the electrodes. As storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and electric double layer capacitors, and storage elements using aqueous electrolyte solutions are also widely used. In addition, storage elements may be used in the form of storage modules formed by assembling a plurality of storage elements.
[0003] In the electrode body of the energy storage element in which the positive and negative electrodes are wound or stacked, even if they are manufactured in the same process, there is some variation in thickness. Therefore, in the case of an energy storage module including a plurality of energy storage elements, in some energy storage elements, a gap may be formed between the electrode body and the container that houses the electrode body in the thickness direction of the electrode body. If there is a gap between the electrode body and the container, the interval between the positive and negative electrodes constituting the electrode body may become uneven, or the electrode body itself may be misaligned, and thus the charge / discharge performance may not be fully exhibited. In addition, if there is a gap between the electrode body and the container, the container is likely to deform when a load is applied to the energy storage element to restrain it, and the desired load may not be applied. Therefore, in some energy storage elements in which there is a gap between the electrode body and the container, a spacer (also called a gap filling member, etc.) is disposed to fill the gap (see Patent Document 1).
[0004] Moreover, carbon materials such as graphite are widely used as negative electrode active materials for electricity storage elements (see Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-48966 A [Patent Document 2] JP 2005-222933 A Summary of the Invention [Problem to be solved by the invention]
[0006] For example, when an electrode body that is relatively thin compared to the size of the container in the thickness direction of the electrode body is housed in a container, it is necessary to make the total thickness of the spacers relatively thick by disposing a thick spacer or disposing a large number of spacers between the electrode body and the container. However, in an energy storage element in which graphite is used as the negative electrode active material, if the total thickness of the spacer disposed between the electrode body and the container is relatively thick, output reduction due to repeated charging and discharging is likely to occur.
[0007] The present invention has been made based on the above-mentioned circumstances, and its object is to provide an energy storage module including an energy storage element in which a relatively thick spacer is arranged between an electrode body and a container, and which has a high output retention rate after charge-discharge cycles, and an energy storage element in which a relatively thick spacer is arranged between an electrode body and a container, and which has a high output retention rate after charge-discharge cycles. [Means for solving the problem]
[0008] An energy storage module according to one aspect of the present invention comprises a plurality of energy storage elements, each of which comprises an electrode body having a positive electrode and a negative electrode, and a container that houses the electrode body, and the plurality of energy storage elements further comprise a spacer arranged between the electrode body and the container, and include a first energy storage element in which a ratio of a total thickness of the spacer to an inner dimension of the container is 0.5% or more, and a second energy storage element that does not comprise a spacer and is arranged between the electrode body and the container, and the negative electrode comprises solid graphite.
[0009] Another aspect of the present invention provides an energy storage element comprising an electrode body having a positive electrode and a negative electrode, a container for housing the electrode body, and a spacer disposed between the electrode body and the container, wherein a ratio of a total thickness of the spacer to an inner dimension of the container is 0.5% or more, and the negative electrode contains solid graphite. Effect of the Invention
[0010] According to one aspect of the present invention, it is possible to provide a storage module including a storage element in which a relatively thick spacer is arranged between an electrode body and a container, the storage module having a high output maintenance rate after charge / discharge cycles. According to another aspect of the present invention, it is possible to provide an energy storage element in which a relatively thick spacer is disposed between an electrode assembly and a container, and which has a high output maintenance rate after charge / discharge cycles. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram showing an embodiment of an electricity storage module. [Diagram 2] FIG. 2 is a transparent perspective view showing one embodiment of an energy storage element provided in the energy storage module. [Diagram 3] FIG. 3 is a schematic cross-sectional view taken along the line II in FIG. 2 when the energy storage element is a first energy storage element. [Figure 4] FIG. 4 is a schematic cross-sectional view taken along the line II in FIG. 2 when the energy storage element is a second energy storage element. [Diagram 5] FIG. 5 is a graph showing the relationship between the ratio of the total thickness of the spacer to the inner dimension of the container of the energy storage element and the output maintenance rate in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] First, an overview of the energy storage module and the energy storage element disclosed in this specification will be described.
[0013] [1] An energy storage module according to one aspect of the present invention comprises a plurality of energy storage elements, each of which comprises an electrode body having a positive electrode and a negative electrode, and a container that houses the electrode body, and the plurality of energy storage elements further comprise a spacer that is arranged between the electrode body and the container, and include a first energy storage element in which a ratio of a total thickness of the spacer to an inner dimension of the container is 0.5% or more, and a second energy storage element that does not comprise a spacer and is arranged between the electrode body and the container, and the negative electrode comprises solid graphite.
[0014] The storage module described in [1] above is a storage module including storage elements in which a relatively thick spacer is disposed between the electrode body and the container, and has a high output retention rate after charge / discharge cycles. The reason why such an effect occurs is unclear, but the following reason is presumed. As described above, in some storage elements of a storage module including a plurality of storage elements, even if they are manufactured in the same process, there may be some variation in thickness, and for example, the electrode body may become thinner than the designed thickness due to being strongly wound, stacked, or pressed. For such storage elements, a spacer is disposed to fill the gap between the electrode body and the container and to fix the electrode body in the container. In the case of a storage module including storage elements in which a relatively thick spacer is disposed, the load on the electrode body increases particularly greatly due to the expansion of the electrode body accompanying the charge / discharge cycle. If the load on the electrode body is large, the electrolyte is likely to flow out of the electrode body from inside the electrode body due to the expansion and contraction of the active material accompanying charge / discharge, and the output is likely to decrease with repeated charge / discharge. On the other hand, solid graphite is a negative electrode active material that has a small change in volume due to expansion and contraction during charging and discharging. Therefore, by using solid graphite as the negative electrode active material, the change in expansion and contraction of the negative electrode due to charging and discharging is suppressed, and even in a storage element in which a relatively thick spacer is disposed between the electrode body and the container, the output reduction due to repeated charging and discharging is suppressed. For these reasons, it is presumed that the output retention rate after the charge and discharge cycle is increased in the storage module described in [1] above.
[0015] The "inner dimension" of the container refers to the inner dimension in the thickness direction of the electrode body. If this inner dimension is not constant, the value of the smallest part is used. The thickness direction of the electrode body refers to the direction perpendicular to the widest plane of the electrode body.
[0016] "Total thickness of the spacer" refers to the sum of the thicknesses of the spacers disposed between the electrode assembly and the container in the thickness direction of the electrode assembly. The total thickness of the spacer is the average value of measurements taken at any five points.
[0017] The "solid" in solid graphite means that the inside of the graphite particle is filled and there are substantially no voids. More specifically, "solid" means that in the cross section of the particle observed in an SEM image obtained using a scanning electron microscope (SEM), the area ratio of voids within the particle to the entire particle area (porosity) is 2% or less. The "area ratio of voids within a particle to the area of the entire particle (porosity)" of a graphite particle can be determined by the following procedure. (1) Preparation of the measurement sample The negative electrode to be measured is fixed with a thermosetting resin. The cross section of the negative electrode fixed with the resin is exposed by ion milling to prepare a measurement sample. The negative electrode to be measured is prepared by the following procedure. If a negative electrode before assembly of the storage element can be prepared, it is used as it is. When preparing from an assembled storage element, the storage element is first discharged at a constant current of 0.1C to the discharge end voltage during normal use to be in a discharged state. The storage element in this discharged state is disassembled, the negative electrode is taken out, and the components (electrolyte, etc.) attached to the negative electrode are thoroughly washed with dimethyl carbonate, and then dried under reduced pressure at room temperature for 24 hours. The work from disassembling the storage element to preparing the negative electrode to be measured is performed in a dry air atmosphere with a dew point of -40°C or less. Here, normal use refers to the use of the storage element by adopting the charge and discharge conditions recommended or specified for the storage element. (2) Acquiring SEM images To obtain SEM images, a JSM-7001F (manufactured by JEOL Ltd.) SEM is used. SEM images are obtained by observing secondary electron images. The acceleration voltage is 15 kV. The observation magnification is set so that 3 to 15 graphite particles appear in one field of view. The obtained SEM image is saved as an image file. Other conditions such as spot diameter, working distance, irradiation current, brightness, and focus are appropriately set so that the contours of the graphite particles are clearly visible. (3) Cutting out the outline of the graphite particles The image cutting function of the image editing software Adobe Photoshop Elements 11 is used to cut out the outlines of the graphite particles from the acquired SEM image. This cutting out of the outlines is performed by using the quick selection tool to select the area outside the outlines of the graphite particles, and then editing everything except the graphite particles to a black background. If the outlines of less than three graphite particles could be cut out at this time, another SEM image is acquired and the process is repeated until the outlines of three or more graphite particles can be cut out. (4) Binarization The image of the first graphite particle among the cut-out graphite particles is binarized using the image analysis software PopImaging 6.00, with a threshold value set to a concentration 20% lower than the concentration at which the intensity is at its maximum. The area of the higher concentration side is calculated through the binarization process, and this is taken as the "area S1 of the voids within the particle." Next, the image of the first graphite particle is binarized with a concentration of 10% as a threshold value. The binarization process determines the outer edge of the graphite particle, and the area inside the outer edge is calculated to obtain the "area of the entire particle, S0." Using the calculated S1 and S0, the ratio of S1 to S0 (S1 / S0) is calculated to calculate the "area ratio R1 of the voids within the particle to the area of the entire particle" for the first graphite particle. The above binarization process is also performed on the images of the second and subsequent graphite particles among the cut-out graphite particles, and the areas S1 and S0 are calculated. Based on the calculated areas S1 and S0, the area ratios R2, R3, ... of the voids in each graphite particle are calculated. (5) Determination of void area ratio (void ratio) The "area ratio of voids within a particle to the entire area of the particle (porosity)" is determined by calculating the average value of all void area ratios R1, R2, R3, ... calculated by the binarization process. Note that instead of the scanning electron microscope used in "obtaining SEM images," the image editing software used in "cutting out the contours of graphite particles," and the image analysis software used in "binarization processing," devices and software capable of equivalent measurements, image editing, and image analysis may be used.
[0018] "Graphite" refers to a material that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Here, the "discharged state" of the carbon material means a state in which the carbon material, which is a negative electrode active material, is discharged so that lithium ions that can be absorbed and released during charging and discharging are sufficiently released. For example, in a half cell using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic Li as a counter electrode, it is a state in which the open circuit voltage is 0.7 V or more.
[0019] [2] In the electricity storage module described in [1] above, the electrode body may be a wound electrode body having a flat portion, and the flat portion may not have a gap in the central portion.
[0020] In the case of the storage module described in [2] above, the electrode body is sufficiently fixed by spacers or the like, so that the charge / discharge performance tends to be improved. On the other hand, when the electrode body is sufficiently fixed by spacers or the like in this way, the load on the electrode body is generally increased with the charge / discharge cycle, and the electrolyte is likely to flow out of the electrode body due to the expansion of the negative electrode or the like, so that the output is likely to decrease with repeated charge / discharge. For this reason, in the case of the storage module described in [2] above in which one aspect of the present invention is applied to a storage module using a storage element that does not have a void in the central part of the flat part of the electrode body, the effect of increasing the output maintenance rate after the charge / discharge cycle is particularly remarkable.
[0021] [3] In the electricity storage module according to the above [1] or [2], the spacer may be a non-porous material.
[0022] A non-porous material is generally more difficult to compress than a porous material, and is therefore useful as a spacer member for fixing an electrode body in a container. On the other hand, when such a non-porous material that is difficult to compress is used as a spacer, the expansion of the electrode body, etc. is generally not easily counteracted by the compression of the spacer, and therefore output is likely to decrease with repeated charging and discharging. For this reason, in the case of the storage module described in the above [3] in which one aspect of the present invention is applied to a storage module using a storage element in which the spacer is a non-porous material, the effect of increasing the output retention rate after charging and discharging cycles is particularly remarkable.
[0023] "Non-porous member" refers to a member that is not a porous member (a material having many fine pores). A non-porous member may be a member with a porosity of 10% or less, or may be a member with a porosity of 5% or less, 1% or less, or 0.1% or less. The porosity refers to a value calculated from the true density of a member calculated from the true density of each component constituting the member and the apparent density of the member using the following formula. The apparent density of a member refers to the value obtained by dividing the mass of the member by the apparent volume of the member. The apparent volume refers to the volume including voids, and when the member is in the form of a film, it can be calculated as the product of the average thickness and the area. The average thickness is the average value of thicknesses measured at any five points. Porosity (%) = 100 - (apparent density / true density) x 100
[0024] [4] In the energy storage module according to any one of [1] to [3] above, the plurality of energy storage elements may be constrained so as to maintain a constant thickness.
[0025] When a plurality of electric storage elements are constrained to maintain a constant thickness, good charge / discharge performance tends to be exhibited due to the maintenance of electrical contact between active material particles, etc. On the other hand, when a plurality of electric storage elements are constrained to maintain a constant thickness, the expansion of the electrode body accompanying repeated charging and discharging is suppressed, so that the load on the electrode body is likely to increase and the output is likely to decrease. For this reason, in the case of the electric storage module described in the above [4] in which one aspect of the present invention is applied to an electric storage module in which a plurality of electric storage elements are constrained to maintain a constant thickness, the effect of increasing the output retention rate after charge / discharge cycles is particularly remarkable.
[0026] [5] The power storage module according to any one of [1] to [4] above may be for use in a hybrid electric vehicle.
[0027] The power storage module according to any one of the above items [1] to [4] has a high output retention rate after charge / discharge cycles, and therefore the power storage module according to the above item [5] is particularly suitable for use in hybrid electric vehicles.
[0028] [6] Another aspect of the present invention provides an energy storage element comprising an electrode body having a positive electrode and a negative electrode, a container for housing the electrode body, and a spacer disposed between the electrode body and the container, wherein a ratio of a total thickness of the spacer to an inner dimension of the container is 0.5% or more, and the negative electrode contains solid graphite.
[0029] The energy storage element described in [6] above is an energy storage element in which a relatively thick spacer is disposed between the electrode body and the container, and has a high output retention rate after charge / discharge cycles. The reason why such an effect occurs is unclear, but it is presumed to be for the same reason as the energy storage module described in [1] above has a high output after charge / discharge cycles.
[0030] An energy storage module, an energy storage element, a method for manufacturing an energy storage element according to an embodiment of the present invention, and other embodiments will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.
[0031] <Energy storage module> An electric storage module according to an embodiment of the present invention includes a plurality of electric storage elements. Hereinafter, an electric storage module according to an embodiment of the present invention will be described with reference to FIG. 1 and the like. An electric storage module 200 according to an embodiment of the present invention shown in FIG. 1 includes a plurality of electric storage elements 100. In the electric storage module 200 of this embodiment, a plurality of electrically connected electric storage elements 100 are assembled and are constrained so that each electric storage element 100 is maintained at a constant thickness (for example, the plurality of electric storage elements 100 are arranged in a predetermined direction and the total thickness of the arranged electric storage elements in the arrangement direction is maintained at a constant thickness). The plurality of electric storage elements 100 are accommodated in a housing 22 in a state of being arranged via a partition member 21. The electric storage elements 100 are electrically connected to each other by a bus bar (not shown). In the electric storage module 200, a flat plate 24 presses each electric storage element 100 in the housing 22 via the partition member 21 by rotation of a nut 23. That is, in the energy storage module 200, the pressing member or the restraining member is configured by the housing 22, the nut 23, and the flat plate 24. The pressing member or the restraining member presses (compresses) the container of the energy storage element 100, and the energy storage element 100 is in a restrained state so as to maintain a constant thickness.
[0032] In addition, as an energy storage module according to another embodiment of the present invention, a plurality of energy storage elements may be arranged in an unconstrained state. Furthermore, a plurality of energy storage elements may be constrained by a configuration other than that shown in FIG. 1. The energy storage elements may not be pressed as long as they are constrained so that the thickness of the energy storage elements is limited. Furthermore, a plurality of energy storage elements may not be pressed as a whole, and some of the energy storage elements may be pressed and some of the energy storage elements may be constrained. In this way, the energy storage module may include a constraining member or a pressing member that constrains the plurality of energy storage elements. Furthermore, the energy storage module may be used as an energy storage device in which a plurality of energy storage modules are assembled. The energy storage module or the energy storage device may include a state monitoring device that monitors the state of one or more energy storage elements.
[0033] (Electricity storage element) The following describes the energy storage elements 100 included in the energy storage module 200. The energy storage elements 100 included in the energy storage module 200 have substantially the same shape. Generally, the only substantial difference between the energy storage elements 100 is the presence or absence of a spacer, which will be described later, and the total thickness of the spacer.
[0034] The energy storage element 100 shown in FIG. 2 includes an electrode body 1, an electrolyte (not shown), and a container 3 that accommodates them. Note that FIG. 2 and other figures do not limit the orientation of the energy storage element 100 when it is used. The energy storage element 100 is a secondary battery, which is an example of an energy storage element. This secondary battery may be a non-aqueous electrolyte secondary battery. The electrode body 1 is a wound electrode body including a positive electrode, a negative electrode, and a separator. At least a part of the electrolyte is present in a state of being impregnated in the electrode body 1 (positive electrode, negative electrode, and separator). The energy storage element 100 further includes a positive electrode connection member 4, a positive electrode external terminal 5, a negative electrode connection member 6, and a negative electrode external terminal 7. The positive electrode of the electrode body 1 is electrically connected to the positive electrode external terminal 5 via the positive electrode connection member 4. The negative electrode of the electrode body 1 is electrically connected to the negative electrode external terminal 7 via the negative electrode connection member 6.
[0035] The multiple energy storage elements 100 included in the energy storage module 200 include those that further include a spacer 2 disposed between the electrode body 1 and the container 3, and those that do not include such a spacer 2. Note that FIG. 2 illustrates the energy storage elements 100 that include the spacer 2. An energy storage element 100 that includes the spacer 2 and in which the ratio of the total thickness of the spacer 2 to the inner dimension of the container 3 is 0.5% or more is defined as a first energy storage element 101 (see FIG. 3). An energy storage element 100 that does not include the spacer 2 is defined as a second energy storage element 102 (see FIG. 4). The multiple energy storage elements 100 included in the energy storage module 200 include a first energy storage element 101 and a second energy storage element 102. Of the multiple energy storage elements 100 included in the energy storage module 200, there may be only one first energy storage element 101, or there may be multiple first energy storage elements 101. Among the multiple energy storage elements 100 included in the energy storage module 200, there may be only one second energy storage element 101, or there may be multiple second energy storage elements 101. The multiple energy storage elements 100 included in the energy storage module 200 may also include a third energy storage element that does not fall under either the first energy storage element 101 or the second energy storage element 102. An example of the third energy storage element is a energy storage element that includes a spacer 2, and in which the ratio of the total thickness of the spacer 2 to the inner dimension of the container 3 is less than 0.5%.
[0036] (First storage element) A first electricity storage element 101 shown in FIG. 3 includes an electrode assembly 1, an electrolyte (not shown), a container 3 that houses the electrode assembly 1 and the electrolyte, and a spacer 2 disposed between the electrode assembly 1 and the container 3.
[0037] (electrode body) The electrode assembly 1 has a positive electrode, a negative electrode, and a separator, and the positive electrode and the negative electrode are stacked with the separator interposed between them. The electrode assembly 1 is a flat wound electrode assembly in which a strip-shaped positive electrode and a strip-shaped negative electrode are stacked with the strip-shaped separator interposed between them and wound.
[0038] The electrode body 1 is flat and has a flat portion 8 where the positive electrode, the negative electrode, and the separator are stacked substantially in parallel, and two curved portions 9a, 9b where the positive electrode, the negative electrode, and the separator are stacked in a curved state. The curved portions 9a, 9b may be called curved portions, R portions, etc. The two curved portions 9a, 9b are positioned so as to face each other. The positive electrode, the negative electrode, and the separator that constitute the electrode body 1 will be described in detail later.
[0039] In this embodiment, the electrode body 1 has no voids in the central portion 10 of the flat portion 8 (the portion surrounded by a thin two-dot chain line in FIG. 3). The central portion 10 of the flat portion 8 may be a region that passes through the winding axis P and is along the width direction (Z direction) of the flat portion 8 of the electrode body 1 when viewed in the winding axis P direction (X direction) of the electrode body 1. The central portion 10 of the flat portion 8 may be the innermost peripheral portion of the flat portion 8 of the electrode body 1. For example, when the electrode body 1 is sufficiently fixed by the spacer 2 and the container 3 and is sufficiently pressed from both sides in the thickness direction (Y direction), no voids exist in the central portion 10 of the flat portion 8. In such a case, the energy storage element 101 can exhibit particularly good charge / discharge performance, etc. The presence or absence of voids in the electrode body 1 can be confirmed, for example, by an X-ray computed tomography (CT) image based on a cross section (state of FIG. 3) viewed in the winding axis P direction (X direction).
[0040] In all the energy storage elements 100 provided in the energy storage module 200, it is preferable that the electrode body 1 is a wound type electrode body having a flat portion 8 and has no gap in the central portion 10 of the flat portion 8. In other words, in all the energy storage elements 100 provided in the energy storage module 200, it is preferable that a spacer 2 of an appropriate thickness is or is not arranged for each energy storage element 100 so that no gap is formed in the central portion 10 of the flat portion 8 of the electrode body 1.
[0041] (Spacer) The spacer 2 is disposed between the electrode assembly 1 and the container 3. The spacer 2 is a member that fills the gap between the electrode assembly 1 and the container 3 and fixes the electrode assembly 1 within the container 3. It is sufficient that the spacer 2 is disposed between the electrode assembly 1 and the container 3 at least in the thickness direction (Y direction) of the electrode assembly 1.
[0042] In this embodiment, as shown in FIG. 3, the spacer 2 is disposed on both sides of the flat portion 8 of the electrode body 1. In this embodiment, the spacer 2 is disposed so that the thickness of each of the spacer 2 on one side and the other side of the flat portion of the flat wound electrode body is 1 / 2 of the total thickness. The two spacers 2 may each be a plate-shaped insulating sheet. The number of insulating sheets constituting the spacer 2 is not limited to this embodiment. When the gap between the electrode body 1 and the container 3 is large, multiple insulating sheets may be stacked and disposed as the spacer 2, or a single thick insulating sheet may be disposed as the spacer 2. The two spacers 2 may be made of the same material or different materials. The multiple insulating sheets may be made of the same material or different materials.
[0043] When one or two or more insulating sheets are used as the spacer 2, the thickness of each insulating sheet may be, for example, 0.01 mm to 3 mm, 0.02 mm to 2 mm, or 0.03 mm to 1 mm. Two or more insulating sheets may have the same thickness or different thicknesses.
[0044] The material constituting the spacer 2 is not particularly limited, and an electrically insulating material such as a resin, paper, or an inorganic material can be suitably used, with a resin being preferred. Examples of the resin constituting the spacer 2 include polyolefins such as polyethylene and polypropylene, polyimides, and aramids, with polyolefins being preferred, and polypropylene being more preferred. The resin spacer 2 may contain components other than the resin, such as inorganic particles.
[0045] The spacer 2 may be a porous material or a non-porous material, but is preferably a non-porous material. A non-porous material is particularly useful as the spacer 2 that fixes the electrode body 1 inside the container 3. Furthermore, when one embodiment of the present invention is applied to an energy storage module 200 including an energy storage element 100 in which the spacer 2 is a non-porous material, the effect of increasing the output maintenance rate after charge / discharge cycles is particularly remarkable. The spacer 2 may be composed of a porous material and a non-porous material.
[0046] The lower limit of the ratio ((B1+B2) / A) of the total thickness (B1+B2) of the spacer 2 to the inner dimension A of the container 3 is 0.5%, and may be 0.6%, 0.8%, 1.0%, 1.2%, or 1.5%. In some embodiments, the lower limit of the ratio ((B1+B2) / A) may be 1.8%, 2.2%, or 2.5%. As shown in FIG. 3, B1 indicates the thickness of the spacer 2 located on one surface side of the electrode body 1, and B2 indicates the thickness of the spacer 2 located on the other surface side of the electrode body 1. The energy storage element 100 has a high output retention rate after charge / discharge cycles, even though the ratio of the total thickness of the spacer 2 to the inner dimension of the container 3 is equal to or greater than the lower limit. On the other hand, the upper limit of the ratio ((B1+B2) / A) of the total thickness (B1+B2) of the spacer 2 to the inner dimension A of the container 3 may be, for example, 10%, 8%, 5%, 4% or 3%. When the ratio is equal to or less than the upper limit, the energy density of the energy storage element 100 can be increased. The ratio of the total thickness of the spacer 2 to the inner dimension of the container 3 can be equal to or more than any of the lower limits and equal to or less than any of the upper limits. This ratio is usually determined in a range in which no gap is generated between the electrode body 1 and the container 3 according to the thickness C of the electrode body 1 and the inner dimension A of the container 3. Usually, the thinner the thickness C of the electrode body 1 is, the higher the ratio ((B1+B2) / A). In addition, this ratio can be adjusted by changing the number of spacers 2 (insulating sheets, etc.) to be arranged, the thickness of one spacer 2 (insulating sheet, etc.) itself, etc. Although not particularly limited, the total thickness (B1+B2) of the spacer 2 is generally 0.06 mm or more and 3 mm or less (e.g., 1 mm or less, typically 0.5 mm or less), for example, 0.1 mm or more and 0.4 mm or less. The inner dimension A of the container 3 is generally 5 mm or more and 100 mm or less (e.g., 60 mm or less), for example, 10 mm or more and 30 mm or less (e.g., 15 mm or less). In the energy storage module 200 using the spacer 2 having such a total thickness (B1+B2) and the container 3 having the inner dimension A, the above-mentioned effects can be better exhibited.
[0047] (container) The container 3 is a sealed container that houses the electrode assembly 1 together with the spacer 2 and seals an electrolyte therein. The material of the container 3 is not particularly limited as long as it has the sealability to seal in the electrolyte and the strength to protect the electrode assembly 1, and may be, for example, a resin or a metal.
[0048] In this embodiment, the container 3 is a rectangular container. Usually, the outer surface of the flat portion 8 of the electrode body 1 is in contact with the inner surface of the container 3 via the spacer 2. Note that other members than the spacer 2 may be disposed between the electrode body 1 and the container 3. For example, the electrode body 1 may be housed in the container 3 in a state where it is wrapped in an insulating bag or insulating case formed from an insulating film. In such a case, an insulating film forming the insulating bag or insulating case is interposed between the electrode body 1 and the container 3 together with the spacer 2. When the electrode body 1 is wrapped in an insulating bag or insulating case, usually, the electrode body 1 is wrapped in an insulating bag or insulating case in all the energy storage elements 100 provided in the energy storage module 200. Such an insulating bag or insulating case does not fall under the spacer 2.
[0049] (positive electrode) The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.
[0050] The positive electrode substrate is conductive. Whether or not it has "conductivity" is determined by the volume resistivity being 10 or less, as measured in accordance with JIS-H-0505 (1975). -2The threshold value is Ω·cm. The material of the positive electrode substrate is a metal such as aluminum, titanium, tantalum, stainless steel, or an alloy thereof. Among these, aluminum or an aluminum alloy is preferred from the viewpoints of potential resistance, high conductivity, and cost. The positive electrode substrate may be a foil, a vapor deposition film, a mesh, a porous material, etc., and a foil is preferred from the viewpoint of cost. Therefore, aluminum foil or an aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or an aluminum alloy include A1085, A3003, A1N30, etc., as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).
[0051] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, further preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate and to increase the energy density per volume of the energy storage element and the energy storage module.
[0052] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.
[0053] The positive electrode active material layer contains a positive electrode active material and, as necessary, optional components such as a conductive agent, a binder, a thickener, and a filler.
[0054] The positive electrode active material can be appropriately selected from known positive electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the positive electrode active material for a lithium ion secondary battery. Examples of the positive electrode active material include lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, lithium transition metal composite oxides having a spinel type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. Examples of the lithium transition metal composite oxides having an α-NaFeO2 type crystal structure include Li[Li x Ni (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Co (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2(0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β). Lithium transition metal composite oxides with spinel crystal structure include Li x Mn2O4, Li x Ni γ Mn (2-γ)O4, etc. Examples of polyanion compounds include LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more may be mixed and used.
[0055] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. In addition, when a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. The "average particle size" means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).
[0056] In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both dry and wet methods.
[0057] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% by mass to 99% by mass, more preferably 70% by mass to 98% by mass, and even more preferably 80% by mass to 95% by mass. By setting the content of the positive electrode active material in the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.
[0058] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, and the like. Examples of carbonaceous materials include graphite, non-graphitic carbon, graphene-based carbon, and the like. Examples of non-graphitic carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, and the like. Examples of carbon black include furnace black, acetylene black, ketjen black, and the like. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, and the like. Examples of the conductive agent include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. These materials may also be used in combination. For example, a material in which carbon black and CNT are combined may be used. Among these, carbon black is preferable from the viewpoint of electronic conductivity and coatability, and acetylene black is preferable among them.
[0059] The content of the conductive agent in the positive electrode active material layer is preferably from 1 mass % to 10 mass %, and more preferably from 3 mass % to 9 mass %. By setting the content of the conductive agent in the above range, the energy density of the energy storage element and the energy storage module can be increased.
[0060] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.
[0061] The content of the binder in the positive electrode active material layer is preferably from 1% by mass to 10% by mass, more preferably from 2% by mass to 9% by mass. By setting the content of the binder in the above range, the positive electrode active material can be stably held.
[0062] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. When the thickener has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like. When the positive electrode active material layer contains a thickener, the content of the thickener in the positive electrode active material layer may be, for example, 0.1% by mass or more and 10% by mass or less. The content of the thickener in the positive electrode active material layer may be 5% by mass or less, 1% by mass or less, or 0% by mass.
[0063] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof. When the positive electrode active material layer contains a filler, the content of the filler in the positive electrode active material layer can be, for example, 0.1% by mass or more and 10% by mass or less. The content of the filler in the positive electrode active material layer may be 5% by mass or less, 1% by mass or less, or 0% by mass.
[0064] The positive electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.
[0065] The porosity of the positive electrode active material layer is preferably 30% to 50%, more preferably 35% to 45%. By having the porosity of the positive electrode active material layer in the above range, it is possible to exhibit good charge / discharge performance, etc. The porosity of the positive electrode active material layer can be adjusted by the particle size of the positive electrode active material, the presence or absence of pressing during the preparation of the positive electrode, and the strength of the pressing, etc.
[0066] The mass per unit area of the positive electrode active material layer is 4 mg / cm 2 More than 12mg / cm 2 Less than 5 mg / cm is preferred. 2 More than 8mg / cm 2 The following is more preferable. In a storage element having a positive electrode in which the mass per unit area of the positive electrode active material layer is within the above range, the above-mentioned effect can be better exhibited. The "mass per unit area of the positive electrode active material layer" refers to the mass per unit area of one positive electrode active material layer. For example, when a positive electrode has a positive electrode substrate and a positive electrode active material layer is provided on each of both sides of the positive electrode substrate, the "mass per unit area of the positive electrode active material layer" is the mass per unit area of the positive electrode active material layer on one side.
[0067] The positive electrode can be produced, for example, by applying a positive electrode mixture paste directly or via an intermediate layer to a positive electrode substrate and drying it. After drying, pressing or the like may be performed as necessary. The positive electrode mixture paste contains each component constituting the positive electrode active material layer, including a positive electrode active material and optional components such as a conductive agent and a binder. The positive electrode mixture paste usually further contains a dispersion medium.
[0068] (Negative electrode) The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode.
[0069] The negative electrode substrate has electrical conductivity. Metals such as copper, nickel, stainless steel, and nickel-plated steel, or alloys thereof, and carbonaceous materials are used as the material of the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foils, vapor deposition films, meshes, and porous materials, and foils are preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.
[0070] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the energy storage element and the energy storage module.
[0071] The negative electrode active material layer contains solid graphite. The negative electrode active material layer contains optional components such as other negative electrode active materials other than solid graphite, conductive agents, binders, thickeners, and fillers, as necessary. The optional components such as conductive agents, binders, thickeners, and fillers can be selected from the materials exemplified for the positive electrode above.
[0072] The negative electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the solid graphite, other negative electrode active materials, conductive agents, binders, thickeners, and fillers.
[0073] Solid graphite is a component that functions as a negative electrode active material. The upper limit of the porosity of the solid graphite contained in the negative electrode active material layer is 2%, preferably 1%, and more preferably 0.5%. By making the porosity of the graphite particles equal to or less than the above upper limit, the expansion of the solid graphite during charging and discharging is suppressed, and the outflow of electrolyte from the electrode body due to the expansion of the negative electrode active material layer is suppressed, so that the output retention rate after the charge and discharge cycles can be increased. The lower limit of the porosity of the solid graphite may be 0%, 0.01%, or 0.05%. The porosity of the solid graphite may be equal to or more than any of the above lower limits and equal to or less than any of the above upper limits.
[0074] Solid graphite can be obtained by subjecting conventional graphite to compression treatment or the like.
[0075] The solid graphite may be natural graphite or artificial graphite, but is preferably natural graphite. When the solid graphite is natural graphite, the initial resistance of the energy storage element can be reduced and the output retention rate after charge / discharge cycles can be further increased.
[0076] Natural graphite is a general term for graphite extracted from natural resources. Solid graphite made of natural graphite may be spherical natural graphite particles obtained by spheroidizing flake natural graphite or the like. Natural graphite may have four peaks at a diffraction angle 2θ in the range of 40° to 50° in an X-ray diffraction pattern using CuKα radiation measured before charging and discharging or in a discharged state. These four peaks are considered to be two peaks derived from a hexagonal crystal structure and two peaks derived from a rhombohedral crystal structure. In the case of artificial graphite, it is generally considered that only two peaks derived from a hexagonal crystal structure appear. In the X-ray diffraction pattern, the ratio of the peak intensity derived from the (012) plane to the peak intensity derived from the (100) plane ((012) / (100)) is preferably 0.3 or more, more preferably 0.4 or more. The above peak intensity ratio ((012) / (100)) is preferably 0.6 or less. Here, the (100) plane originates from a hexagonal crystal structure, and the (012) plane originates from a rhombohedral crystal structure.
[0077] The average particle size of the solid graphite is preferably 1 μm or more and 25 μm or less, more preferably 4 μm or more and 20 μm or less, and even more preferably 5 μm or more and 15 μm or less. By having the average particle size of the solid graphite in the above range, it is possible to further increase the output maintenance rate after charge and discharge cycles. In order to obtain solid graphite with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverization method and the classification method can be selected, for example, from the methods exemplified for the above positive electrode active material.
[0078] The content of solid graphite in the negative electrode active material layer is preferably 60% by mass or more and 99% by mass or less, more preferably 90% by mass or more and 98% by mass or less, and in some cases is even more preferably 95% by mass or more, 97% by mass or more, or 98% by mass or more. By setting the content of solid graphite in the above range, it is possible to achieve both high energy density and manufacturability of the negative electrode active material layer, and to further increase the output retention rate after charge / discharge cycles.
[0079] The negative electrode active material layer may contain a negative electrode active material other than solid graphite. As the other negative electrode active material, graphite other than solid graphite (hollow graphite) and other various conventionally known negative electrode active materials can be used. Note that the hollow graphite, which is graphite other than solid graphite, is graphite having the above-mentioned porosity of more than 2%. However, the content of solid graphite in all the negative electrode active materials contained in the negative electrode active material layer is preferably 90% by mass or more, more preferably 99% by mass or more, and may be substantially 100% by mass. The negative electrode active material layer may contain graphite, and all the graphite contained in the negative electrode active material layer may be solid graphite.
[0080] The content of graphite in all the negative electrode active materials contained in the negative electrode active material layer is preferably 90% by mass or more, more preferably 99% by mass or more, and may be substantially 100% by mass. When one embodiment of the present invention is applied to an electric storage element in which graphite is mainly used as the negative electrode active material, the effect of increasing the output maintenance rate after charge / discharge cycles is particularly remarkable. The content of solid graphite in all the graphite (solid graphite and hollow graphite) contained in the negative electrode active material layer is preferably 90% by mass or more, more preferably 99% by mass or more, and may be substantially 100% by mass. In other words, it is preferable that the negative electrode active material layer contains graphite, and the porosity of the graphite contained in the negative electrode active material layer is 2% or less.
[0081] When the negative electrode active material layer contains a conductive agent, the content of the conductive agent in the negative electrode active material layer may be, for example, 1% by mass or more and 10% by mass or less. The content of the conductive agent in the negative electrode active material layer is preferably 5% by mass or less, and may be more preferably 2% by mass or less, 1% by mass or less, 0.1% by mass or less, or 0% by mass or less. When the content of the conductive agent in the negative electrode active material layer is small or no conductive agent is contained, the content of the negative electrode active material such as solid graphite can be increased, and the energy density can be increased. Note that the graphite in the negative electrode active material layer does not correspond to the conductive agent in the negative electrode active material layer.
[0082] The content of the binder in the negative electrode active material layer is preferably 0.1% by mass to 10% by mass, more preferably 1% by mass to 5% by mass. By setting the content of the binder in the above range, the solid graphite and the like can be stably maintained.
[0083] The content of the thickener in the negative electrode active material layer is preferably 0.1% by mass or more and 5% by mass or less.
[0084] When the negative electrode active material layer contains a filler, the content of the filler in the negative electrode active material layer can be, for example, 0.1% by mass or more and 10% by mass or less. The content of the filler in the negative electrode active material layer can be 5% by mass or less, 1% by mass or less, or 0% by mass. When the content of the filler in the negative electrode active material layer is small or no filler is contained, the content of the negative electrode active material such as solid graphite can be increased, and the energy density can be increased.
[0085] The porosity of the negative electrode active material layer is preferably 30% or more and 55% or less, more preferably 35% or more and 45% or less. By setting the porosity of the negative electrode active material layer to the above upper limit or less, the energy density is increased. On the other hand, the lower the porosity of the negative electrode active material layer, the easier it is for the negative electrode active material layer to expand during charging and discharging. In contrast, in the energy storage element provided in the energy storage module according to one embodiment of the present invention, solid graphite is used, so that even if the porosity of the negative electrode active material layer is relatively low, the expansion of the negative electrode active material layer during charging and discharging is small, and the output maintenance rate after charging and discharging cycles can be increased. The porosity of the negative electrode active material layer can be adjusted by the particle size of solid graphite, the presence or absence of pressing during the preparation of the negative electrode, and the strength, etc.
[0086] The mass per unit area of the negative electrode active material layer is 2.5 mg / cm 2 More than 6mg / cm 2 Less than 3 mg / cm is preferred. 2 More than 5mg / cm 2 The following is more preferable. In a storage element having a negative electrode in which the mass per unit area of the negative electrode active material layer is within the above range, the above-mentioned effect can be better exhibited. The "mass per unit area of the negative electrode active material layer" refers to the mass per unit area of one negative electrode active material layer. For example, when a negative electrode has a negative electrode substrate and a negative electrode active material layer is provided on each of both sides of the negative electrode substrate, the "mass per unit area of the negative electrode active material layer" is the mass per unit area of the negative electrode active material layer on one side.
[0087] The negative electrode can be produced, for example, by applying the negative electrode mixture paste directly or via an intermediate layer to the negative electrode substrate and drying it. After drying, pressing or the like may be performed as necessary. The negative electrode mixture paste contains solid graphite and each component constituting the negative electrode active material layer, such as an optional conductive agent and binder. The negative electrode mixture paste usually further contains a dispersion medium.
[0088] (Separator) The separator can be appropriately selected from known separators. For example, a separator consisting of only a substrate layer, a separator in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer, etc. can be used as the separator. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, a porous resin film is preferable from the viewpoint of strength, and a nonwoven fabric is preferable from the viewpoint of electrolyte retention. As the material of the substrate layer of the separator, polyolefins such as polyethylene and polypropylene are preferable from the viewpoint of shutdown function, and polyimide and aramid are preferable from the viewpoint of oxidation decomposition resistance. A material obtained by combining these resins may be used as the substrate layer of the separator.
[0089] The heat-resistant particles contained in the heat-resistant layer preferably have a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably have a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials with a mass loss of a predetermined amount or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ion crystals such as calcium fluoride, barium fluoride, and barium titanate; covalent crystals such as silicon and diamond; mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the energy storage element.
[0090] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.
[0091] As the separator, a polymer gel composed of a polymer and an electrolyte may be used. Examples of the polymer include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of the polymer gel has an effect of suppressing leakage. As the separator, the above-mentioned porous resin film or nonwoven fabric may be used in combination with the polymer gel.
[0092] (electrolyte) The electrolyte can be appropriately selected from known electrolytes. The electrolyte may be an electrolytic solution. The electrolyte may be a non-aqueous electrolyte or a non-aqueous electrolytic solution. The non-aqueous electrolytic solution includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.
[0093] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of the non-aqueous solvent include cyclic carbonates, chain carbonates, carboxylates, phosphates, sulfonates, ethers, amides, and nitriles. As the non-aqueous solvent, those in which some of the hydrogen atoms contained in these compounds are replaced with halogen atoms may be used.
[0094] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among these, EC is preferred.
[0095] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferable.
[0096] As the non-aqueous solvent, it is preferable to use a cyclic carbonate or a chain carbonate, and it is more preferable to use a combination of a cyclic carbonate and a chain carbonate. By using a cyclic carbonate, it is possible to promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. By using a chain carbonate, it is possible to keep the viscosity of the non-aqueous electrolyte low. When using a cyclic carbonate and a chain carbonate in combination, it is preferable that the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is, for example, in the range of 5:95 to 50:50.
[0097] The electrolyte salt can be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, onium salts, etc. Among these, lithium salts are preferred.
[0098] Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP), and lithium salts having a halogenated hydrocarbon group such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3. Among these, inorganic lithium salts are preferred, and LiPF6 is more preferred.
[0099] The electrolyte salt content in the non-aqueous electrolyte is 0.1 mol / dm at 20°C and 1 atmosphere. 3 More than 2.5mol / dm 3 It is preferable that the value is 0.3 mol / dm or less. 3 More than 2.0mol / dm 3 More preferably, it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3 More preferably, it is 0.7 mol / dm or less. 3More than 1.5mol / dm 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the nonaqueous electrolyte can be increased.
[0100] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additives include aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, and cyclohexanedicarboxylic anhydride; ethyl sulfite; Examples of the additives include propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, and tetrakistrimethylsilyl titanate. These additives may be used alone or in combination of two or more.
[0101] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and to further improve safety.
[0102] The electrolyte may be a solid electrolyte, or a non-aqueous electrolyte and a solid electrolyte may be used in combination.
[0103] The solid electrolyte can be selected from any material that has ionic conductivity such as lithium, sodium, calcium, etc., and is solid at room temperature (e.g., 15° C. to 25° C.). Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.
[0104] As the sulfide solid electrolyte, in the case of a lithium ion secondary battery, for example, Li2S-P2S5, LiI-Li2S-P2S5, Li 10 Ge-P2S 12 etc.
[0105] (Second storage element) The second electricity storage element 102 shown in FIG. 4 includes an electrode assembly 1, an electrolyte (not shown), and a container 3 that accommodates the electrode assembly 1 and the electrolyte.
[0106] The second energy storage element 102 is the same as the first energy storage element 101 in Fig. 3 except that it does not include the spacer 2 disposed between the electrode body 1 and the container 3. Therefore, the components constituting the second energy storage element 102 in Fig. 4 are denoted by the same reference numerals as those of the first energy storage element 101 in Fig. 3, and detailed description thereof will be omitted.
[0107] In the second electricity storage element 102, there is substantially no gap between the electrode body 1 and the container 3, and the spacer 2 is not disposed. Normally, the electrode body 1 is designed so that there is substantially no gap between the electrode body 1 and the container 3, and therefore if the electrode body 1 is manufactured as designed, the spacer 2 is not disposed. However, when the electrode body 1 is manufactured, for example, by tightly winding, laminating, or pressing, the electrode body 1 becomes thinner than the designed thickness, and in such a case, the spacer 2 is disposed.
[0108] That is, the multiple energy storage elements 100 included in the energy storage module 200 include a second energy storage element 102 in which the electrode body 1 is manufactured to have a thickness substantially as designed, and a first energy storage element in which the electrode body 1 is manufactured to be thinner than designed and a spacer 2 is disposed between the electrode body 1 and the container 3 at a ratio of the total thickness of 0.5% or more to the inner dimension of the container 3. In addition, in the case of an energy storage element in which a relatively thick spacer is disposed, output reduction due to repeated charging and discharging is usually likely to occur. In contrast, since each of the energy storage elements 100 included in the energy storage module 200 uses solid graphite as the negative electrode active material, output reduction due to repeated charging and discharging is unlikely to occur even in the energy storage element (first energy storage element 101) in which a relatively thick spacer is disposed. In this way, the energy storage module 200 has a high output maintenance rate after charge and discharge cycles, even though it is a storage module including an energy storage element 100 (first energy storage element 101) in which a relatively thick spacer 2 is disposed between the electrode body 1 and the container 3.
[0109] In addition, in the energy storage module 200 according to the embodiment of FIG. 1, as described above, the multiple energy storage elements 100 are arranged in a predetermined direction, and the multiple energy storage elements 100 are constrained so that the total thickness of the multiple energy storage elements 100 in the arrangement direction is maintained at a constant thickness. When the multiple energy storage elements 100 are constrained so that the total thickness is maintained at a constant thickness, good charge / discharge performance tends to be exhibited due to the maintenance of electrical contact between active material particles, etc. In addition, when an embodiment of the present invention is applied to an energy storage module in which the energy storage elements 100 are constrained, the effect of excellent output performance after charge / discharge cycles is particularly remarkable. For example, the thickness of the energy storage elements 100 in the thickness direction (Y direction in FIGS. 2 to 4) may be constrained so that the thickness is maintained at a constant thickness.
[0110] The storage module of the present embodiment can be particularly suitably applied to storage modules used in a manner in which charging and discharging at high output are repeated. This is because such storage modules are prone to a drop in output due to repeated charging and discharging, and a high output maintenance rate is particularly important. Specifically, the storage module of the present embodiment can be suitably used as a power source for automobiles such as electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), and is particularly suitable for use in HEVs. In addition, the storage module of the present embodiment may be used as a power source for electronic devices such as personal computers and communication terminals, or a power source for power storage. It can also be used as a storage device in which a plurality of storage modules are further assembled.
[0111] <Electricity storage element> An energy storage element according to one embodiment of the present invention comprises an electrode body having a positive electrode and a negative electrode, a container for housing the electrode body, and a spacer disposed between the electrode body and the container, wherein a ratio of a total thickness of the spacer to an inner dimension of the container is 0.5% or more, and the negative electrode contains solid graphite.
[0112] The energy storage element according to one embodiment of the present invention is an energy storage element in which a relatively thick spacer is disposed between the electrode body and the container, and has a high output retention rate after charge / discharge cycles. A specific example of the energy storage element is the first energy storage element 101 included in the energy storage module 200 according to one embodiment of the present invention.
[0113] <Method of manufacturing the energy storage element> The method for producing the energy storage element of the present embodiment can be appropriately selected from known methods. The method for producing the energy storage element of the present embodiment includes, for example, preparing an electrode body, preparing a spacer, preparing an electrolyte, and housing the electrode body, the spacer, and the electrolyte in a container. The preparation of the electrode body includes preparing a positive electrode and a negative electrode, and forming the electrode body by stacking or rolling the positive electrode and the negative electrode with a separator interposed therebetween.
[0114] The method of housing the electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte is used as the electrolyte, the non-aqueous electrolyte may be injected through an injection port formed in the container, and then the injection port may be sealed.
[0115] <Other embodiments> The energy storage module and energy storage element of the present invention are not limited to the above-described embodiments, and various modifications may be made without departing from the scope of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and part of the configuration of one embodiment may be replaced with the configuration of another embodiment or a well-known technique. Furthermore, part of the configuration of one embodiment may be deleted. Also, a well-known technique may be added to the configuration of one embodiment.
[0116] In the above embodiment, the case where the storage element is used as a chargeable and dischargeable non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) has been described, but the storage element may be of any type, shape, size, capacity, etc. The present invention can also be applied to various secondary batteries, capacitors such as electric double layer capacitors and lithium ion capacitors, storage elements using an aqueous electrolyte solution as the electrolyte, and the like.
[0117] In the above embodiment, the electrode body in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode body may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode. In addition, in the above embodiment, the description has been centered on the case in which the energy storage element includes a wound type electrode body, but the shape of the electrode body included in the energy storage element is arbitrary. The present invention can also be applied to an energy storage element including a stacked type electrode body in which multiple positive electrodes and multiple negative electrodes are stacked with a separator interposed therebetween.
[0118] The arrangement of the spacers is not limited to the above embodiment. The spacers may be provided only on one side of the flat part of the flat wound electrode body. Spacers of different thicknesses or numbers may be arranged on one side and the other side of the flat part of the flat wound electrode body. However, as in the above embodiment, it is preferable that the spacers are arranged so that the thickness of each of the spacers is 1 / 2 of the total thickness on one side and the other side of the flat part of the flat wound electrode body, respectively, in order to apply a load evenly to the electrode body from both sides. EXAMPLES
[0119] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0120] [Example 1] Positive electrode active material LiNi 1 / 3 Co 1 / 3 Mn 1 / 3A positive electrode mixture paste was prepared using O2, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium. The mass ratio of the positive electrode active material, AB, and PVDF was 93:3.5:3.5 (solid content conversion). The positive electrode mixture paste was applied to both sides of an aluminum foil as a positive electrode substrate, and dried. Then, a roll press was performed to obtain a positive electrode. The mass per unit area of the positive electrode active material layer in the obtained positive electrode (one side) was 6 mg / cm. 2 It was.
[0121] (Preparation of negative electrode) A negative electrode mixture paste was prepared using solid graphite (void ratio 0.49%, average particle size 8 μm) as the negative electrode active material, styrene-butadiene rubber (SBR) as the binder, carboxymethyl cellulose (CMC) as the thickener, and water as the dispersion medium. The solid graphite was produced by consolidating natural graphite. The mass ratio of the negative electrode active material, SBR, and CMC was 98:1:1 (solid content conversion). The negative electrode mixture paste was applied to both sides of copper foil as the negative electrode substrate and dried. Then, roll pressing was performed to obtain a negative electrode. The porosity of the negative electrode active material layer in the obtained negative electrode was 45%, and the mass per unit area (one side) was 4 mg / cm. 2 It was.
[0122] (electrolyte) A 1.2 mol / dm 3 LiPF6 was dissolved in the electrolyte at a concentration of 0.01g / L to obtain an electrolyte.
[0123] (Separator) The separator used was a microporous polyolefin film.
[0124] (Spacer) A non-porous polypropylene sheet (insulating sheet) was used as the spacer.
[0125] (Assembly of energy storage elements) A flat wound electrode body was obtained using the positive electrode, negative electrode, and separator. A spacer was placed on each side of the flat part of the electrode body, and the electrode body was housed in a container (inner dimension 11.60 mm) together with the spacer, and an electrolyte was poured and sealed to obtain an energy storage element of Example 1. The energy storage element was in a state where the container of the energy storage element was restrained by a restraining member and the container was maintained at a constant thickness. The total thickness of the spacer in the thickness direction of the electrode body was 0.10 mm. The ratio of the total thickness of the spacer to the inner dimension of the container was 0.9%.
[0126] [Examples 2 to 3, Comparative Examples 1 to 5, Reference Examples 1 and 2] The type of negative electrode active material was as shown in Table 1. In addition, the strength of the roll press during negative electrode preparation was changed to produce electrode bodies with different thicknesses, and the total thickness of the spacer was set as shown in Table 1 so that the sum of the total thickness of the spacer and the thickness of the electrode body was the same. Except for these points, the energy storage elements of Examples 2 to 3, Comparative Examples 1 to 5, and Reference Examples 1 and 2 were obtained in the same manner as in Example 1. The total thickness of the spacer was adjusted by changing the number of spacers (non-porous sheets) to be arranged. In each of the energy storage elements of the Examples, Comparative Examples, and Reference Examples, no voids were present in the center of the flat part of the electrode body. In addition, the "hollow graphite" in Table 1 is natural graphite with a porosity of 4.44% and an average particle size of 8 μm.
[0127] [evaluation] (1)Initial charge / discharge The obtained storage elements were initially charged and discharged under the following conditions. At 25°C, the elements were charged at a constant current of 1.0C up to 4.10V. Then, the elements were charged at a constant voltage of 4.10V. The charging was terminated when the total charging time reached 3 hours. Then, a rest period of 10 minutes was provided. The elements were discharged at a constant current of 1.0C up to a discharge end voltage of 2.50V. The amount of electricity discharged at this time was taken as the initial discharge capacity. (2) Initial output Each storage element after the above initial charge and discharge was charged at a constant current of 1.0 C at 25° C. with an amount of electricity of 50% of the initial discharge capacity, and the SOC (state of charge) was set to 50%. Then, the element was discharged for 30 seconds at a current of 0.2 C, 0.5 C, or 1.0 C. After each discharge, the element was charged at a constant current of 1.0 C to set the SOC to 50%. The relationship between the current and the voltage 10 seconds after the start of discharge in each discharge was plotted, and the DC resistance was calculated from the slope of the straight line obtained from the plot of the three points. The output 10 seconds after the start of discharge was calculated from the obtained DC resistance, and was taken as the initial output. (3) Charge / discharge cycle test Next, each storage element was discharged at a constant current of 1.0 C at 25° C. to an SOC of 20%. After storage in a thermostatic chamber at 60° C. for 4 hours, it was charged at a constant current of 4.0 C at 60° C. to a voltage equivalent to an SOC of 80%, and then discharged at a constant current of 4.0 C to a voltage equivalent to an SOC of 20%. The above charge and discharge cycle was repeated for 500 hours without a rest period after the above charge and discharge. (4) Output after charge / discharge cycle test Thereafter, the output after the charge-discharge cycle test was calculated using the same procedure as that for calculating the initial output. For each storage element, the percentage of the output after the charge-discharge cycle test relative to the initial output was calculated, and this was taken as the output maintenance rate. The results are shown in Table 1 and FIG. 5.
[0128] [Table 1]
[0129] As shown in Table 1 and FIG. 5, in the energy storage elements of Comparative Examples 1 to 5 in which hollow graphite was used as the negative electrode active material, the output retention rate after the charge-discharge cycles decreased as the ratio of the total thickness of the spacer to the inner dimensions of the container increased, and the decrease was particularly noticeable when the ratio was 0.5% or more. In contrast, in the energy storage elements of Reference Examples 1 and 2 and Examples 1 to 3 in which solid graphite was used as the negative electrode active material, the output retention rate after the charge-discharge cycles hardly decreased even when the ratio of the total thickness of the spacer to the inner dimensions of the container increased. In particular, in the energy storage elements of Examples 1 to 3 in which the ratio was 0.5% or more, the ratio of the output retention rate to that in the case in which hollow graphite was used (for example, the ratio of the output retention rate of the energy storage element of Example 1 to the output retention rate of the energy storage element of Comparative Example 3 in which the ratios were both 0.9%) exceeded 110%, and a high improvement effect due to the use of solid graphite was confirmed. Thus, it was confirmed that each of the energy storage elements of Examples 1 to 3 is an energy storage element in which a relatively thick spacer is disposed between the electrode body and the container, and has an effect of having a high output maintenance rate after charge / discharge cycles. Furthermore, from this result, it is also clear that an energy storage module including a plurality of energy storage elements including any of the energy storage elements of Examples 1 to 3 as a first energy storage element and the energy storage element of Reference Example 1 as a second energy storage element also has a high output maintenance rate after charge / discharge cycles. [Industrial Applicability]
[0130] The present invention can be applied to power storage elements and power storage modules used as power sources for electronic devices such as personal computers and communication terminals, and automobiles. [Explanation of symbols]
[0131] 100 Energy storage element 101 First storage element 102 Second storage element 1 Electrode body 2 Spacers 3 containers 4 Positive electrode connection material 5 Positive external terminal 6 Negative electrode connecting member 7 Negative external terminal 8 Flat area 9a, 9b Curved section 10 Central part of flat area 21 Partitioning material 22 Case 23 Nut 24 flat plate 200 Energy Storage Module P winding shaft
Claims
1. A plurality of storage elements are provided, Each of the plurality of storage elements is An electrode assembly having a positive electrode and a negative electrode, and A container for accommodating the electrode assembly Equipped with The plurality of storage elements include a first storage element further including a spacer disposed between the electrode body and the container, the ratio of a total thickness of the spacer to an inner dimension of the container being 0.5% or more; a second storage element that does not include a spacer and is disposed between the electrode body and the container; Including, The negative electrode of the energy storage module comprises solid graphite.
2. The electric storage module according to claim 1 , wherein the electrode body is a wound electrode body having a flat portion, and the flat portion has no gap in a central portion thereof.
3. The electricity storage module according to claim 1 or 2, wherein the spacer is a non-porous material.
4. 3. The energy storage module according to claim 1, wherein the plurality of energy storage elements are constrained so as to maintain a constant thickness.
5. 3. The electricity storage module according to claim 1 or 2, which is for use in a hybrid electric vehicle.
6. An electrode assembly having a positive electrode and a negative electrode; A container for housing the electrode assembly; and A spacer disposed between the electrode assembly and the container. Equipped with The ratio of the total thickness of the spacer to the inner dimension of the container is 0.5% or more; The negative electrode of the energy storage element comprises solid graphite.
Citation Information
Patent Citations
Negative pole material for lithium battery, and lithium battery
JP2005222933A
Battery, and manufacturing method thereof
JP2009048966A