Speaker diaphragm and speaker
The speaker diaphragm with carbon fibers of 20 mm or more, randomly oriented in a resin matrix, addresses the need for improved sound pressure in high frequencies by optimizing carbon fiber content and resin composition, achieving a superior balance of propagation velocity and internal loss.
Patent Information
- Application Number
- JP2023071155
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing speaker diaphragms with carbon fiber and resin balance propagation velocity and internal loss but require improvement in sound pressure in the high frequency range.
A speaker diaphragm composed of carbon fibers with an average length of 20 mm or more, randomly oriented in a resin matrix, with a carbon fiber content of 15% to 85% by mass, using resins like polypropylene or polyamide with aliphatic structural units, and a thickness of 0.1 mm to 2.0 mm, enhances sound pressure in the high frequency range.
The diaphragm achieves an excellent balance between propagation velocity and internal loss while significantly increasing sound pressure in the high frequency range.
Smart Images

Figure 2024156571000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a speaker diaphragm and a speaker. [Background technology]
[0002] Factors affecting the sound quality of speakers of audio equipment include the propagation speed (speed of vibrations traveling through the diaphragm) and internal loss (ease of vibration containment) of the diaphragm used in the speaker. Specifically, the higher the propagation speed of the diaphragm, the better, and the higher the internal loss, the better. However, the propagation speed and internal loss values of the diaphragm are generally in an inverse relationship. For example, metal diaphragms tend to have high propagation speeds but low internal losses. On the other hand, paper or resin diaphragms tend to have high internal losses but low propagation speeds. In view of this, a speaker diaphragm containing carbon fiber and resin has been proposed as a speaker diaphragm that has an excellent balance between the propagation speed and the internal loss (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-45715 Summary of the Invention [Problem to be solved by the invention]
[0004] As a result of the inventors' investigations, it was found that a speaker diaphragm containing carbon fiber and resin has an excellent balance between propagation speed and internal loss, but there is room for improvement in terms of sound pressure in the high-frequency range. In view of the above circumstances, an object of an embodiment of the present disclosure is to provide a speaker diaphragm that has an excellent balance between propagation speed and internal loss and has high sound pressure in the high-frequency range, and a speaker that includes this speaker diaphragm. [Means for solving the problem]
[0005] Specific means for solving the above problems include the following aspects. <1> A speaker diaphragm comprising carbon fibers and a resin, the carbon fibers having an average length of 20 mm or more. <2> The carbon fibers are randomly oriented in the resin. <1> 2. The speaker diaphragm according to claim 1 . <3> The carbon fiber content is 15% by mass to 85% by mass of the entire diaphragm. <1> or <2> 2. The speaker diaphragm according to claim 1 . <4> The resin includes polypropylene or polyamide containing an aliphatic structural unit having 10 to 12 carbon atoms. <1> ~ <3> 13. A speaker diaphragm according to any one of claims 1 to 12. <5> The thickness is 0.1mm~2.0mm. <1> ~ <4> 13. A speaker diaphragm according to any one of claims 1 to 12. <6> <1> ~ <5> A speaker comprising the speaker diaphragm according to any one of claims 1 to 5. Effect of the Invention
[0006] According to an embodiment of the present disclosure, there is provided a speaker diaphragm that has an excellent balance between propagation speed and internal loss and has high sound pressure in the high-pitched range, and a speaker including this speaker diaphragm. [Brief description of the drawings]
[0007] [Figure 1A] FIG. 1 is a cross-sectional view illustrating an example of a configuration of a speaker diaphragm. [Figure 1B] FIG. 1 is a plan view illustrating an example of a configuration of a speaker diaphragm. [Diagram 2] 1 is a graph showing the measurement results of the propagation velocity and the internal hearing loss of the speaker diaphragm produced in the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments of the present disclosure, and do not limit the scope of the invention. The mechanism of action described in this disclosure includes assumptions, and the correctness or incorrectness of such assumptions does not limit the scope of the invention.
[0009] In the present disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the lower limit and upper limit, respectively.
[0010] In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.
[0011] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified.
[0012] <Speaker diaphragms> The speaker diaphragm of the present disclosure contains carbon fibers and a resin, and the carbon fibers have an average length of 20 mm or more.
[0013] The speaker diaphragm (hereinafter, simply referred to as the diaphragm) of the present disclosure has an excellent balance between the propagation velocity and the internal loss. This is believed to be because the diaphragm contains resin, which provides high internal loss, and contains carbon fiber, which provides high propagation velocity. Furthermore, the diaphragm of the present disclosure has a higher sound pressure in the high-pitched range than existing diaphragms containing carbon fiber and resin. The reason for this is not necessarily clear, but it is thought that, for example, the length of the carbon fiber contained in the diaphragm of the present disclosure is longer than that of the carbon fiber contained in existing diaphragms, thereby increasing rigidity while suppressing an increase in the amount of carbon fiber contained in the diaphragm.
[0014] (Carbon Fiber) The carbon fibers contained in the diaphragm have an average length of 20 mm or more. In the present disclosure, the average length of the carbon fibers is the arithmetic mean value of the lengths of the individual carbon fibers contained in the diaphragm. From the viewpoint of increasing the sound pressure in the high-pitched range, the average length of the carbon fibers contained in the diaphragm is preferably 30 mm or more, more preferably 40 mm or more, and even more preferably 60 mm or more. The upper limit of the average length of the carbon fibers contained in the diaphragm is not particularly limited. From the viewpoint of facilitating dispersion of the carbon fibers, the average length of the carbon fibers is preferably 150 mm or less, more preferably 120 mm or less, and even more preferably 100 mm or less.
[0015] From the viewpoint of increasing the sound pressure in the treble range, the proportion of carbon fibers satisfying the formula: Y×0.8≦X is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more of the total carbon fibers contained in the diaphragm, where X is the individual length of the carbon fibers and Y is the average length of the carbon fibers.
[0016] There is no particular limitation on the thickness of the carbon fibers contained in the diaphragm. For example, the thickness of the carbon fibers may be selected from the range of 3 μm to 15 μm.
[0017] The carbon fibers contained in the diaphragm may be randomly or non-randomly oriented (eg, oriented along a particular direction). From the viewpoint of making the characteristics of the diaphragm uniform, it is preferable that the carbon fibers contained in the diaphragm are randomly oriented. In the present disclosure, the orientation state of the carbon fibers is determined by observing the diaphragm from a direction perpendicular to the main surface of the diaphragm. The carbon fibers contained in the diaphragm may or may not be bent.
[0018] Examples of carbon fibers include carbon fibers made from resins such as polyacrylonitrile (PAN) and carbon fibers made from pitch, and are not particularly limited.
[0019] The content of carbon fibers in the diaphragm is not particularly limited and can be selected according to the desired characteristics. From the standpoint of ensuring the rigidity of the diaphragm, the carbon fiber content of the entire diaphragm is preferably 15 mass % or more, more preferably 25 mass % or more, and even more preferably 35 mass % or more. From the viewpoint of reducing the weight of the diaphragm, the carbon fiber content is preferably 85 mass % or less of the entire diaphragm, more preferably 75 mass % or less, and even more preferably 65 mass % or less.
[0020] (resin) The type of resin contained in the diaphragm is not particularly limited and can be selected according to the desired characteristics of the diaphragm, etc. Specific examples of the resin contained in the diaphragm include thermoplastic resins such as polypropylene, polyethylene, polyamide, polyvinyl chloride, polycarbonate, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polystyrene, polyimide, polyurethane, polyphenylene sulfide, and poly(meth)acrylate, and thermosetting resins such as epoxy resin, phenol resin, melamine resin, urea resin, unsaturated polyester resin, and silicone resin. The diaphragm may contain only one type of resin or two or more types of resin. The resin contained in the diaphragm may be a resin whose raw materials are partly or entirely derived from plants (biomass plastic).
[0021] From the viewpoint of the balance of the properties of the diaphragm and moldability, the resin contained in the diaphragm preferably contains at least one selected from polypropylene, polyethylene, and polyamide. Examples of polyamide include polyamides containing aliphatic structural units, aromatic polyamides containing only aromatic structural units, and polyamides containing aliphatic structural units and aromatic structural units. Among these, polyamides containing only aliphatic structural units or polyamides containing aliphatic structural units and aromatic structural units are preferred. The carbon number of the aliphatic structural units contained in the polyamide can be selected from 6 to 12, and is preferably 10 to 12.
[0022] If desired, the diaphragm may contain materials other than carbon fiber and resin. Materials other than carbon fiber and resin include glass fiber, inorganic filler, and the like. When the diaphragm contains materials other than carbon fiber and resin, the total amount of carbon fiber and resin is preferably 80 mass% or more of the entire diaphragm, more preferably 90 mass% or more, and even more preferably 95 mass% or more.
[0023] The thickness of the diaphragm is not particularly limited and can be selected according to the desired characteristics. From the standpoint of ensuring the rigidity of the diaphragm, the thickness of the diaphragm is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. From the standpoint of reducing the weight of the diaphragm, the thickness of the diaphragm is preferably 2.0 mm or less, more preferably 1.0 mm or less, and even more preferably 0.5 mm or less.
[0024] The shape and size of the diaphragm are not particularly limited and can be selected according to the desired characteristics. Fig. 1A is a cross-sectional view showing an example of the shape of a diaphragm, and Fig. 1B is a plan view of the diaphragm shown in Fig. 1A. The diaphragm 1 shown in Fig. 1A and Fig. 1B is cylindrical and has an opening A on the speaker body side and an opening B on the opposite side to the speaker body side. There is no particular limitation on the diameter of the opening A and the opening B. For example, each of them can be selected within the range of 10 mm to 300 mm. There is no particular limitation on the height H of the diaphragm 1. For example, it can be selected from the range of 1 cm to 10 cm. The side surface S of the diaphragm 1 may be flat as shown in Fig. 1, or may not be flat. For example, the side surface S may be curved inwardly in a convex shape. The shape of the diaphragm is not limited to the three-dimensional shape shown in FIG. 1, but may be planar.
[0025] The diaphragm of the present disclosure may be made of only a main body containing carbon fiber and resin, or may further include a member different from the main body. For example, the diaphragm may have a functional layer on one or both sides of the main body containing carbon fiber and resin. The function of the functional layer is not particularly limited, and may include a dustproof function, a waterproof function, a flame retardant function, etc.
[0026] The diaphragm of the present disclosure can be produced, for example, by producing a sheet-like material containing carbon fiber and resin, and then processing this sheet-like material. The method for producing a sheet-like material containing carbon fibers and a resin is not particularly limited, and any known method can be used.
[0027] The propagation velocity of the diaphragm is preferably 3,000 m / s to 5,200 m / s. In the present disclosure, the propagation velocity of the diaphragm is a value measured by the vibrating reed method.
[0028] The internal loss of the diaphragm is preferably 0.005 to 0.032. In the present disclosure, the internal loss of the diaphragm is a value measured by a vibrating reed method.
[0029] The density of the diaphragm is 1.0g / cm 3 ~1.3g / cm 3 It is preferable that:
[0030] <Speaker> A speaker according to the present disclosure includes the speaker diaphragm according to the present disclosure described above. The uses of the speaker of the present disclosure are not particularly limited, and the speaker can be applied to audio equipment, car audio, microphones, smartphones, personal computers, and the like. EXAMPLES
[0031] Hereinafter, the embodiments of the present disclosure will be specifically described with reference to examples, but the present disclosure is not limited to these examples. In the following examples, sound pressure was measured according to the method specified in JIS C 5532:2014.
[0032] (1) Study on the average length of carbon fibers A sheet (130 g / m) in which the carbon fibers are randomly oriented in the resin was prepared using 40 parts by mass of carbon fibers (thickness 7 μm) having an average length shown in Table 1 and 60 parts by mass of resin (biomass nylon obtained from metaxylylenediamine and sebacic acid, hereinafter referred to as MXD10). 2 ) was produced by the carding method. The produced sheet was hot pressed using a mold to obtain a diaphragm with a thickness of 0.2 mm. The size of the diaphragm was 21.15 mm in diameter at the opening on the speaker body side, 114 mm in diameter at the opening on the opposite side to the speaker body, and 24.7 mm in height. Sound pressure was measured using the produced diaphragm. The results are shown in Table 1.
[0033] [Table 1]
[0034] As shown in Table 1, the diaphragms of Examples 1 to 3, in which the average carbon fiber length was 25 mm, 50 mm, or 70 mm, had higher sound pressure in at least one of the ranges of 5 kHz to 10 kHz and 10 kHz to 20 kHz compared to the diaphragm of Comparative Example 1, in which the average carbon fiber length was 12.5 mm.
[0035] (2) Consideration of the thickness of the diaphragm A sheet (130 g / m) in which the carbon fibers are randomly oriented in the resin was prepared using 40 parts by mass of carbon fibers with an average length of 70 mm and a thickness of 7 μm and 60 parts by mass of resin (MXD10).2 ) was produced by carding. The produced sheet was hot pressed using a mold to obtain a diaphragm having a thickness of 0.2 mm or 0.5 mm in the same manner as in Example 1. The sound pressure was measured using the produced diaphragm. The results are shown in Table 2.
[0036] [Table 2]
[0037] As shown in Table 2, the diaphragm of Example 4, which had a thickness of 0.2 mm, had a higher sound pressure in the 5 kHz to 10 kHz range than the diaphragm of Example 5, which had a thickness of 0.5 mm, and the diaphragm of Example 5 had a higher sound pressure in the 10 kHz to 20 kHz range than the diaphragm of Example 4.
[0038] (3) Examination of carbon fiber content Carbon fibers with an average length of 70 mm and a thickness of 7 μm and resin (MXD10) were used so that the carbon fiber content was the value shown in Table 3, and a sheet (130 g / m) in which the carbon fibers were randomly oriented in the resin was prepared. 2 ) was produced by carding. The produced sheet was hot pressed using a mold to obtain a diaphragm having a thickness of 0.2 mm in the same manner as in Example 1. The sound pressure was measured using the produced diaphragm. The results are shown in Table 3.
[0039] [Table 3]
[0040] As shown in Table 3, the diaphragms of Examples 7 and 8, which had a carbon fiber content of 40% by mass or 60% by mass, had higher sound pressure in the ranges of 5 kHz to 10 kHz and 10 kHz to 20 kHz than the diaphragms of Examples 6 and 9, which had a carbon fiber content of 20% by mass or 80% by mass.
[0041] (4) Consideration of resin type A sheet (130 g / m) in which the carbon fibers are randomly oriented in the resin was prepared using 40 parts by mass of carbon fibers having an average length of 70 mm and a thickness of 7 μm and 60 parts by mass of the resin shown in Table 4. 2 ) was produced by carding. The produced sheet was hot pressed using a mold to obtain a diaphragm having a thickness of 0.2 mm in the same manner as in Example 1. The sound pressure was measured using the produced diaphragm. The results are shown in Table 4.
[0042] [Table 4]
[0043] In Table 4, PP means polypropylene, PA6 means polycaprolactam (nylon 6), and MXD10 means biomass nylon obtained from metaxylylenediamine and sebacic acid. As shown in Table 4, the diaphragms of Example 10, which used PP as the resin, and Example 12, which used MXD10 as the resin, had higher sound pressure in the ranges of 5 kHz to 10 kHz and 10 kHz to 20 kHz than the diaphragm of Example 11, which used PA6 as the resin.
[0044] (5) Measurement of propagation velocity and internal loss The diaphragms of Samples 1 to 7 were produced in the same manner as in Example 1 using the materials shown in Table 5. Diaphragms of the same size as Samples 1 to 7 were also produced, made of paper, polypropylene, or aluminum. The carbon fibers used to produce the diaphragms had an average length of 70 mm and a thickness of 7 μm. The density, Young's modulus, propagation velocity, and internal loss of the fabricated diaphragm were measured. The results are shown in Table 5 and Figure 2.
[0045] [Table 5]
[0046] As shown in Table 5 and FIG. 2, the diaphragms of Samples 1 to 7, which contained carbon fiber and resin, had a better balance between propagation velocity and internal loss than diaphragms made only of paper, polypropylene, or aluminum.
Claims
1. A speaker diaphragm comprising carbon fibers and a resin, the carbon fibers having an average length of 20 mm or more.
2. 2. The speaker diaphragm according to claim 1, wherein the carbon fibers are randomly oriented in the resin.
3. 2. The speaker diaphragm according to claim 1, wherein the carbon fiber content is 15% by mass to 85% by mass of the entire diaphragm.
4. 2. The speaker diaphragm according to claim 1, wherein the resin comprises polypropylene or polyamide containing an aliphatic structural unit having 10 to 12 carbon atoms.
5. 2. The speaker diaphragm according to claim 1, having a thickness of 0.1 mm to 2.0 mm.
6. A speaker comprising the speaker diaphragm according to any one of claims 1 to 5.
Citation Information
Patent Citations
Diaphragm for speaker, manufacturing method of diaphragm for speaker, and speaker
JP2022045715A