Electro-deposition liquid, and method for manufacturing insulation film
Patent Information
- Application Number
- JP2024017133
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-02-07
- Publication Date
- 2024-11-06
AI Technical Summary
【0019】 本発明によれば、電着膜を焼き付ける際に微細なクラックが発生することを抑制でき、絶縁性に優れた絶縁皮膜を形成可能な電着液、および、この電着液を用いた絶縁皮膜の製造方法を提供することができる。
Smart Images

Figure 2024156601000003 
Figure 2024156601000001 
Figure 2024156601000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrodeposition solution used when electrodepositing an electrodeposition film on a conductive substrate by anionic electrodeposition, and a method for producing an insulating film. [Background technology]
[0002] 2. Description of the Related Art Insulated conductors, which are made by covering a conductive base material with an insulating coating made of insulating resin, are widely used as conductive materials and heat sink materials for various electrical devices that require insulation. Various resins are used as constituent materials for the insulating coating. For example, Patent Document 1 discloses one that uses a polyimide resin such as polyamideimide resin, and Patent Document 2 proposes one that uses a mixed resin of a polyimide resin and a fluorine-based resin.
[0003] Electrodeposition is known as a method for forming an insulating film made of such an insulating resin on the surface of a conductive substrate. The electrodeposition method is a method in which a substrate on which an insulating film is to be formed and a counter electrode are immersed in an electrodeposition solution in which the material for the insulating film is dispersed, and a voltage is applied between the substrate and the counter electrode to form an electrodeposition film by depositing the material for the insulating film on the surface of the substrate.The formed electrodeposition film is then heated to bake the electrodeposition film onto the substrate, thereby forming the insulating film.
[0004] In addition, the electrodeposition method includes an anionic electrodeposition method in which a voltage is applied to the substrate as the anode to form an insulating coating on the substrate surface, and a cationic electrodeposition method in which a voltage is applied to the substrate as the cathode to form an insulating coating on the substrate surface. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-115120 A [Patent Document 2] JP 2018-070663 A Summary of the Invention [Problem to be solved by the invention]
[0006] Incidentally, the anionic electrodeposition solution used in the anionic electrodeposition method contains solid components including the above-mentioned resin, water, an organic solvent, and a neutralizing agent. When a voltage is applied, the pH decreases near the surface of the anode (substrate), and the solid components are precipitated on the surface of the anode (substrate), forming an electrodeposition film. Here, when the electrodeposited film formed on the surface of the anode is baked, there is a risk that fine cracks will occur, making it impossible to ensure the insulating properties of the insulating film.
[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide an electrodeposition liquid that can suppress the occurrence of fine cracks when baking an electrodeposition film and can form an insulating film with excellent insulating properties, and a method for manufacturing an insulating film using this electrodeposition liquid. [Means for solving the problem]
[0008] In order to solve the above problems, the inventors conducted extensive research and found that the fine cracks that occur when baking an electrodeposited film are caused by an insufficient amount of organic solvent contained in the electrodeposited film, but that the insufficient amount of organic solvent contained in the electrodeposited film can be eliminated by adding an appropriate amount of organic acid to the electrodeposition solution. Therefore, it was discovered that by adding an appropriate amount of organic acid to the electrodeposition solution, the amount of organic solvent contained in the electrodeposition film is optimized when the solid components are precipitated on the surface of the anode (substrate), making it possible to suppress the occurrence of fine cracks that occur during baking.
[0009] The present invention has been made based on the above-mentioned findings, and the electrodeposition liquid of aspect 1 of the present invention is an electrodeposition liquid for electrodepositing an electrodeposition film on a conductive substrate by anionic electrodeposition, and is characterized by containing water, an organic solvent, a solid component containing at least a polyimide-based resin, a neutralizing agent, and an organic acid.
[0010] According to the electrodeposition solution of the first aspect of the present invention, since the solution contains an organic acid, it is possible to adjust the amount of organic solvent contained in the electrodeposition film by the pH buffering effect of the organic acid and the effect of affecting the compatibility between the resin and the organic solvent. That is, it is possible to suppress a sudden drop in pH near the surface of the anode (substrate) and to allow the electrodeposition film to contain a sufficient amount of organic solvent. This makes it possible to suppress the occurrence of fine cracks when the electrodeposition film is baked, and to form an insulating film with high insulating properties.
[0011] The electrodeposition solution of the second aspect of the present invention is characterized in that, in the electrodeposition solution of the first aspect of the present invention, the organic acid contains any one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid. Hydroxypropionic acid and hydroxybutyric acid are effective regardless of the position of the functional group, so that even positional isomers are effective. According to the electrodeposition liquid of the second aspect of the present invention, since it contains the above-mentioned organic acid, it is possible to reliably suppress a sudden drop in pH near the surface of the anode (substrate), and it is possible to allow the electrodeposition film to contain a sufficient amount of organic solvent, and therefore it is possible to sufficiently suppress the occurrence of cracks when the electrodeposition film is baked.
[0012] The electrodeposition solution of the third aspect of the present invention is characterized in that in the electrodeposition solution of the first or second aspect of the present invention, the organic acid is two or more selected from the group consisting of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid. According to the electrodeposition liquid of the third aspect of the present invention, since it contains two or more of the above-mentioned organic acids, it is possible to more effectively suppress a sudden drop in pH near the surface of the anode (substrate), and it is possible to sufficiently impregnate the organic solvent in the electrodeposition film, and therefore it is possible to sufficiently suppress the occurrence of cracks when the electrodeposition film is baked.
[0013] The electrodeposition solution of a fourth aspect of the present invention is the electrodeposition solution of any one of the first to third aspects of the present invention, characterized in that the organic acid contains a hydroxy acid. According to the electrodeposition solution of the fourth aspect of the present invention, the organic acid contains a hydroxy acid, so that a sudden drop in pH near the surface of the anode (substrate) can be more effectively suppressed, and the electrodeposition film can be sufficiently impregnated with the organic solvent, so that the occurrence of cracks when the electrodeposition film is baked can be sufficiently suppressed.
[0014] The electrodeposition solution of the fifth aspect of the present invention is characterized in that, in the electrodeposition solution of any one of the first to fourth aspects of the present invention, the concentration of the organic acid is within the range of 5 mg / L or more and 500 mg / L or less. According to the electrodeposition solution of the fifth aspect of the present invention, the concentration of the organic acid is within the range of 5 mg / L or more and 500 mg / L or less, so that an appropriate pH buffering effect can be exerted, and the occurrence of cracks during baking of the electrodeposition film can be sufficiently suppressed, and the electrodeposition film can be stably formed.
[0015] The electrodeposition solution of the sixth aspect of the present invention is characterized in that, in the electrodeposition solution of any one of the first to fifth aspects of the present invention, the ratio A / B of the concentration A mg / L of the neutralizing agent to the concentration b mg / L of the organic acid is in the range of 5 or more and 500 or less. According to the electrodeposition solution of the sixth aspect of the present invention, the ratio A / B of the concentration A mg / L of the neutralizing agent to the concentration b mg / L of the organic acid is within the range of 5 to 500, so that the action of the organic acid can suppress the occurrence of fine cracks during baking without inhibiting the action of the neutralizing agent.
[0016] The electrodeposition liquid of a seventh aspect of the present invention is the electrodeposition liquid of any one of the first to sixth aspects of the present invention, characterized in that the solid components further contain a fluororesin. According to the electrodeposition solution of the seventh aspect of the present invention, since the solid components contain a fluororesin together with a polyimide resin, it is possible to form an insulating film having particularly excellent insulating and dielectric properties. In addition, since it is more difficult to suppress cracking in an electrodeposition film containing a fluororesin than in the case of a polyimide resin alone, the addition of an organic acid is effective.
[0017] The method for producing an insulating coating according to aspect 8 of the present invention is a method for producing an insulating coating on a surface of a substrate, and is characterized by comprising an electrodeposition film formation step of immersing the substrate and a counter electrode in the electrodeposition solution according to any one of aspects 1 to 7 of the present invention, applying a voltage between the anode and the cathode, using the substrate as an anode and the counter electrode as a cathode, to form an electrodeposition film on the substrate, and a baking step of baking the electrodeposition film.
[0018] The method for producing an insulating coating according to aspect 8 of the present invention includes an electrodeposition film formation step of forming an electrodeposition film using the electrodeposition liquid according to any one of aspects 1 to 7 of the present invention, and a baking step of baking the electrodeposition film. This makes it possible to suppress the occurrence of fine cracks in the electrodeposition film during the baking step, and thus makes it possible to stably produce an insulating coating with excellent insulating properties. Effect of the Invention
[0019] According to the present invention, it is possible to provide an electrodeposition liquid capable of suppressing the occurrence of fine cracks when baking an electrodeposition film and forming an insulating coating with excellent insulating properties, and a method for producing an insulating coating using this electrodeposition liquid. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a flow diagram showing a method for producing an insulating coating using an electrodeposition liquid according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] An electrodeposition liquid and a method for producing an insulating film according to one embodiment of the present invention will be described below. The electrodeposition liquid of this embodiment is used when forming an electrodeposition film that serves as a precursor of an insulating film on the surface of a conductive substrate. In this embodiment, the substrate is used as an anode and a voltage is applied to form an insulating film on the surface of the substrate, which is the anode, in an anionic electrodeposition method.
[0022] The electrodeposition liquid of this embodiment contains water, an organic solvent, a solid component, a neutralizing agent, and an organic acid. As described above, the electrodeposition solution of the present embodiment is used in an anionic electrodeposition method, and therefore contains an amine as a neutralizing agent.
[0023] In this embodiment, the solid component contains at least a polyimide resin, and preferably contains two types of resin, a polyimide resin and a fluorine-based resin. In this embodiment, examples of the polyimide resin include polyamideimide, polyetherimide, polyimide, etc. Examples of the fluorine resin include polytetrafluoroethylene, perfluoroalkoxyalkane, etc.
[0024] The solid component may have an average particle size of 50 nm or more and 500 nm or less, more preferably 50 nm or more and 450 nm or less, and even more preferably 50 nm or more and 300 nm or less, and the standard deviation of the particle size of the solid component may be 250 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.
[0025] The polyimide resin and the fluorine resin, which are solid components, are dispersed in the water and the organic solvent. Examples of the organic solvent include N,N-dimethylacetamide, propylene carbonate, dimethylsulfoxide, N,N-dimethylformamide, 4-butyrolactone, N-methyl-2-pyrrolidone, and N-methyl-2-pyrrolidone.
[0026] The water content in the electrodeposition solution is preferably 15% by mass or more, more preferably 50% by mass or more, while the water content in the electrodeposition solution is preferably 85% by mass or less, more preferably 75% by mass or less. Furthermore, the content of the organic solvent in the electrodeposition solution is preferably 15% by mass or more, more preferably 50% by mass or more, while the content of the organic solvent in the electrodeposition solution is preferably 85% by mass or less, more preferably 75% by mass or less.
[0027] The organic acid has a pH buffering effect and an effect of influencing the compatibility between the resin, which is a solid component, and the organic solvent. By adjusting the material and content of this organic acid, it is possible to control the amount of the organic solvent contained in the electrodeposition film. Here, the organic acid preferably includes any one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, and more preferably includes two or more selected from these. In addition, the organic acid preferably contains a hydroxy acid. Examples of the hydroxy acid include glycolic acid, hydroxypropionic acid, hydroxybutyric acid, tartronic acid, glyceric acid, etc. Note that since hydroxypropionic acid and hydroxybutyric acid exert their effects regardless of the position of the functional group, even positional isomers will produce the effect.
[0028] In this embodiment, the concentration of the organic acid in the electrodeposition solution is preferably in the range of 5 mg / L or more and 500 mg / L or less. By setting the concentration of the organic acid to 5 mg / L or more, the pH buffer effect can be fully achieved, the organic solvent can be appropriately incorporated into the electrodeposition film, and the occurrence of fine cracks during baking can be appropriately suppressed. On the other hand, by setting the concentration of the organic acid to 500 mg / L or less, swelling and a decrease in Coulomb efficiency due to an excessive amount of organic solvent being incorporated into the electrodeposition film can be prevented, and the electrodeposition film can be efficiently formed. The concentration of the organic acid in the electrodeposition solution is more preferably 10 mg / L or more, and even more preferably 20 mg / L or more. The concentration of the organic acid in the electrodeposition solution is more preferably 100 mg / L or less, and even more preferably 50 mg / L or less.
[0029] In this embodiment, it is preferable that the ratio A / B of the concentration A mg / L of the neutralizing agent to the concentration b mg / L of the organic acid is in the range of 5 to 500. Since the organic acid may cause an acid-base reaction with the neutralizing agent made of an amine compound and inhibit the neutralizing agent's function of ionizing the resin, it is preferable that the ratio A / B of the concentration A mg / L of the neutralizing agent to the concentration b mg / L of the organic acid is set within the above-mentioned range in order to ensure that each effect is exerted. If the ratio A / B is less than 5, the ionization effect of the neutralizing agent on the resin is impaired, and the stability of the liquid is impaired. If the ratio A / B exceeds 500, the organic acid does not exert the desired effect and cracks occur in the film. The ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L is more preferably 20 or more, and even more preferably 50 or more. The ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L is more preferably 400 or less, and even more preferably 200 or less.
[0030] Next, a method for producing an insulating film using the electrodeposition liquid according to this embodiment will be described with reference to FIG.
[0031] As shown in FIG. 1, the method for producing an insulating coating in this embodiment includes a surface pretreatment step S01, an electrodeposition film formation step S02, and a baking step S03.
[0032] (Surface pretreatment process S01) First, a substrate on which an electrodeposited film (insulating film) is to be formed is prepared. This substrate is conductive and is made of a metal material such as copper or a copper alloy, aluminum or an aluminum alloy, etc. Then, the oil and fat and oxide film adhering to the surface of the above-mentioned base material are removed using a surface treatment liquid such as an organic solvent or a surfactant.
[0033] (Electrodeposited film formation step S02) Next, the substrate and the counter electrode are immersed in the electrodeposition solution of this embodiment, and a voltage is applied between the anode (substrate) and the cathode (counter electrode) with the substrate as the anode and the counter electrode as the cathode. This reduces the pH of the electrodeposition solution around the substrate, and a solid component (in this embodiment, a mixture of polyimide resin and fluororesin) is precipitated on the surface of the substrate. This forms an electrodeposition film on the surface of the substrate. At this time, since an organic acid is added to the electrodeposition solution in this embodiment, the organic solvent is appropriately contained in the electrodeposition film due to the pH buffer effect of the organic acid.
[0034] The temperature of the electrodeposition liquid in the electrodeposition film forming step S02 is preferably adjusted to within a range of 5° C. or higher and 35° C. or lower. By keeping the liquid temperature at 5° C. or higher, it is possible to prevent water from being mixed into the electrodeposition liquid due to condensation. On the other hand, by keeping the liquid temperature at 35° C. or lower, the storage stability of the electrodeposition liquid is improved, and the electrodeposition film can be stably formed.
[0035] The voltage applied between the substrate (anode) and the counter electrode (cathode) in the electrodeposition film forming step S02 is preferably within the range of 10V or more and 600V or less. By setting the applied voltage to 10 V or more, the electrodeposition speed can be ensured and productivity can be improved. On the other hand, by setting the applied voltage to 600 V or less, the generation of many bubbles on the surface of the substrate can be suppressed, and the generation of many irregularities in the insulating coating due to the bursting of the bubbles in the subsequent baking step S03 can be suppressed.
[0036] (Baking process S03) In the baking step S03, the substrate on which the electrodeposited film containing the solid components (in this embodiment, a mixture of polyimide resin and fluororesin) obtained in the electrodeposited film forming step S02 is formed is dried, for example, within a temperature range of 200° C. or higher and lower than the melting point of the solid components to remove the residual electrodeposition liquid, and then the electrodeposited film is baked onto the substrate to form an insulating coating.
[0037] The baking temperature in the baking step S03 may be within a temperature range in which an electrodeposition film of a solid component (in this embodiment, a mixture of a polyimide resin and a fluororesin) is formed and an insulating coating is formed on the substrate, and may be within a range of, for example, 200° C. to 400° C. The baking time may be within a range of, for example, 0.5 minutes to 60 minutes.
[0038] Through the above-mentioned steps, an insulating film containing a solid component (in this embodiment, a mixture of polyimide resin and fluororesin) can be formed on a conductive base material, which suppresses the occurrence of fine cracks during baking and provides an insulating film with good insulating properties.
[0039] The electrodeposition liquid of the present embodiment configured as described above contains an organic acid. Due to the pH buffering effect of the organic acid and the effect of influencing the compatibility between the resin and the organic solvent, by adjusting the amount of organic solvent contained in the electrodeposition film, it is possible to suppress the occurrence of fine cracks when the electrodeposition film is baked, and to form an insulating coating with high insulating properties.
[0040] In the electrodeposition solution of the present embodiment, when the organic acid contains any one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, a sudden drop in pH near the surface of the anode (substrate) can be reliably suppressed, and the occurrence of cracks when the electrodeposition film is baked can be sufficiently suppressed. Furthermore, when the acid contains two or more selected from formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, the rapid decrease in pH near the surface of the anode (substrate) can be more effectively suppressed, and the occurrence of cracks when the electrodeposition film is baked can be sufficiently suppressed. Furthermore, when the organic acid contains a hydroxy acid, a sudden drop in pH near the surface of the anode (substrate) can be more effectively suppressed, and the occurrence of cracks when the electrodeposition film is baked can be sufficiently suppressed.
[0041] In the electrodeposition solution of the present embodiment, when the concentration of the organic acid is 5 mg / L or more, the pH buffer effect of the organic acid can be ensured, and the occurrence of cracks during baking of the electrodeposition film can be sufficiently suppressed. On the other hand, when the concentration of the organic acid is 500 mg / L or less, the pH buffer effect is prevented from acting excessively, and the electrodeposition film can be efficiently formed without causing blistering.
[0042] In the electrodeposition solution of this embodiment, when the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L is within the range of 5 to 500, the content of the neutralizing agent is secured, and the occurrence of fine cracks during baking can be suppressed by the pH buffering effect of the organic acid without inhibiting the action of the neutralizing agent.
[0043] In the electrodeposition solution of the present embodiment, when the solid components contain a fluororesin together with a polyimide resin, an electrodeposition film made of a mixed resin of a polyimide resin and a fluororesin can be formed, making it possible to form an insulating coating having particularly excellent insulating properties.
[0044] The method for producing an insulating coating of the present embodiment includes an electrodeposition film formation step S02 in which a substrate and a counter electrode are immersed in the electrodeposition liquid of the present embodiment, and a voltage is applied between the substrate as the anode and the counter electrode as the cathode to form an electrodeposition film on the substrate, and a baking step S03 in which the electrodeposition film is baked. Therefore, it is possible to suppress the occurrence of fine cracks in the electrodeposition film in the baking step S03, and an insulating coating with excellent insulating properties can be stably produced.
[0045] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES
[0046] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.
[0047] As shown in Tables 1 and 2, water, an organic solvent, a solid component, a neutralizing agent, and an organic acid were prepared, and mixed in the mass ratios shown in Tables 1 and 2 to obtain electrodeposition solutions. Then, a rectangular bar of oxygen-free copper (1.47 mm x 2.94 mm x 25 cm in length) was prepared as a conductive substrate, and a cylindrical copper plate was prepared as a counter electrode. The substrate and the counter electrode were immersed in the above-mentioned electrodeposition solution, and an electrodeposition film was formed by setting the temperature of the electrodeposition solution to 20° C., the applied voltage to 500 V, and the holding time to 0.5 minutes. The electrodeposited film was then baked using a three-stage heating profile, in which the work temperature during baking was 140-170°C for 10 minutes, 240-260°C for 5 minutes, and 340-350°C for 90 seconds, followed by rapid cooling, to form an insulating coating.
[0048] The concentration of the organic acid contained in the electrodeposited film was evaluated as follows. The electrodeposition solution was diluted with ultrapure water, and then impurities were removed. The filtrate was passed through a membrane filter to prepare a solution for ion chromatography measurement. Next, the measurements were performed using an ion chromatograph Thermo Fisher Scientific ICS-5000+. Anion exchange columns Dionex IonPac AG15 and Dionex IonPac AS15 were used as the stationary phase of the ion chromatograph, potassium hydroxide aqueous solution was used as the eluent, Dionex ADRS 600 was used as the suppressor, and electrical conductivity was used as the detector.
[0049] The appearance of the insulating film thus formed was also observed, and the film was evaluated for cracks and blisters. Those with cracks that allowed the Cu in the substrate to be confirmed by visual observation were rated as "X", those with cracks that prevented the Cu in the substrate from being confirmed by visual observation were rated as "△", those with cracks that were not visible to the naked eye but were visible under a microscope were rated as "◯", and those with no cracks visible even under a microscope were rated as "◎". Furthermore, when blistering was observed in the insulating coating by visual observation, it was rated as "present", and when no blistering was observed, it was rated as "absent".
[0050] Furthermore, the relative dielectric constant of the insulating coating was measured as follows. A measurement sample was prepared by applying silver paste to the surface of the insulating film at two 10 mm points on the edges and at a 100 mm area in the center. The capacitance between the conductor and the silver paste in the center was measured using a Hioki IM3536 LCR meter, and the relative dielectric constant was calculated from the measured capacitance and the thickness of the film.
[0051] The electrodeposition solution was also evaluated for stability. When the electrodeposition solution was kept at 40°C for 5 days, the solution that showed separation or precipitation was rated as "△", and the solution that did not show separation or precipitation was rated as "◯".
[0052] [Table 1]
[0053] [Table 2]
[0054] In Comparative Examples 1 to 3, no organic acid was added to the electrodeposition solution, and cracks were generated in the insulating coating after baking, in which Cu of the substrate could be confirmed.
[0055] In contrast, in Examples 1 to 24 of the present invention, an organic acid was added to the electrodeposition solution, and no cracks that would reveal Cu in the substrate were formed in the insulating coating after baking. In addition, in Examples 3 to 24 of the present invention, the organic acid contained any one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid, and no cracks were observed with the naked eye.
[0056] In Examples 1 to 5, the organic acid concentration was less than 5 mg / L, and fine cracks were observed, but no cracks were observed that revealed the substrate, and there was no problem with insulation. In Examples 6 to 9, the organic acid concentration exceeded 500 mg / L, and therefore blisters occurred in the coating. In addition, in Examples 6, 8, 9, 15, and 16 of the present invention, the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L was less than 5, and separation and precipitation occurred in the electrodeposition solution when it was held at 40° C. for 5 days, and the stability of the electrodeposition solution was poor. In Examples 10 to 14 of the present invention, even though the organic acid concentration was 5 mg / L or more, the ratio A / B of the neutralizing agent concentration A mg / L to the organic acid concentration B mg / L exceeded 500, and therefore fine cracks occurred. Furthermore, in Examples 21 and 22 of the present invention, polyimide resin and fluororesin were contained as solid components, and the relative dielectric constant was sufficiently low, and the insulating properties were particularly excellent.
[0057] From the results of the above confirmation experiments, it was confirmed that the present invention can provide an electrodeposition liquid capable of suppressing the occurrence of fine cracks when baking an electrodeposition film and forming an insulating film with excellent insulating properties, as well as a method for manufacturing an insulating film using this electrodeposition liquid.
Claims
1. An electrodeposition solution for electrodepositing an electrodeposition film on a conductive substrate by anionic electrodeposition, comprising: The composition includes water, an organic solvent, a solid component, a neutralizing agent, and an organic acid, The electrodeposition solution, wherein the solid component contains at least a polyimide resin.
2. 2. The electrodeposition solution according to claim 1, wherein the organic acid contains any one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid.
3. 2. The electrodeposition solution according to claim 1, wherein the organic acid is two or more selected from the group consisting of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, glycolic acid, hydroxypropionic acid, and hydroxybutyric acid.
4. 2. The electrodeposition solution according to claim 1, wherein the organic acid includes a hydroxy acid.
5. 2. The electrodeposition solution according to claim 1, wherein the concentration of the organic acid is within a range of 5 mg / L to 500 mg / L.
6. 2. The electrodeposition solution according to claim 1, wherein a ratio A / B of a concentration A mg / L of said neutralizing agent to a concentration B mg / L of said organic acid is within a range of 5 to 500.
7. 2. The electrodeposition solution according to claim 1, wherein the solid component further contains a fluororesin.
8. A method for producing an insulating film for forming an insulating film on a surface of a substrate, comprising the steps of: an electrodeposition film forming step of immersing the substrate and a counter electrode in the electrodeposition solution according to any one of claims 1 to 7, using the substrate as an anode and the counter electrode as a cathode, and applying a voltage between the anode and the cathode to form an electrodeposition film on the substrate; and a baking step of baking the electrodeposition film.
Citation Information
Patent Citations
Electrodeposition liquid for forming water dispersion type insulation film
JP2017115120A