Joining body and method for joining the same, and microfluidic device, and method for manufacturing the same
Ionizing radiation-based bonding of silicone and glass in microfluidic devices addresses temporary bonding issues, enhancing alignment precision and manufacturing yield, resulting in hydrophilic, gas-impermeable devices suitable for multi-stage structures.
Patent Information
- Application Number
- JP2024120295
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-03-25
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-02-19
AI Technical Summary
Existing bonding methods for silicone and glass in microfluidic devices are temporary, require immediate contact after surface modification, lack gas barrier properties, and are difficult to align accurately, leading to low manufacturing yield and unsuitable for multi-stage devices.
The method involves irradiating contact points between silicone and glass or silicone molded bodies with ionizing radiation, such as electron beams or gamma rays, to form covalent bonds at the interface, changing the surface properties from hydrophobic to hydrophilic and adding gas barrier properties, while allowing for precise alignment and multiple-stage stacking.
This method enables stable, strong bonding, reduces water contact angle, suppresses sample sorption, and facilitates mass production of microfluidic devices with hydrophilic and gas-impermeable channels, maintaining flatness and preventing voids.
Smart Images

Figure 2024156750000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for bonding a polyorganosiloxane (hereinafter also referred to as silicone) molded body and a silicone or glass molded body by irradiating ionizing radiation, and to a microfluidic device in which a silicone molded sheet and a silicone or glass molded sheet are laminated and bonded by ionizing radiation with a microchannel formed between them, and a method for manufacturing the same. [Background technology]
[0002] Silicone, whose main component is polyorganosiloxane, is a material with excellent processability and properties such as heat resistance, insulating properties, weather resistance, low toxicity, and transparency. It is a resin material used in a wide variety of fields, including electrical and electronic parts, transportation machinery, building materials, daily necessities, and medical products. As a result, there is a demand for the development of processing techniques for silicone molded bodies (hereafter, for the sake of convenience, simply referred to as silicone) and techniques for bonding between silicones or between silicone and glass.
[0003] Silicone itself has a certain degree of self-adhesiveness, but as a method for stronger bonding, a bonding method is known in which the surfaces of the silicone to be bonded are activated by irradiating them with atmospheric pressure plasma or excimer UV, and then the activated surfaces are bonded together to bond them, as disclosed in Patent Documents 1 and 2. However, since surface modification by irradiation with atmospheric pressure plasma or the like is temporary and short-lived, there is a restriction that the silicones must be bonded together immediately after surface modification.
[0004] Regarding the problem that the surface modification is temporary, the inventors of the present application have developed a new silicone processing method in which the surface of silicone is irradiated with an electron beam with an absorbed dose of 2 MGy or more to form recesses, and the recesses have a surface layer thickness of 1 μm or more, and the hydrophilicity is stable for a long period of time compared to the above surface modification (Non-Patent Document 1).
[0005] In recent years, there has been an increasing demand for microfluidic devices used in the fields of regenerative medicine, drug discovery, and diagnosis for applications such as mixing, reacting, synthesizing, extracting, and analyzing samples, and silicone is commonly used as a substrate for microfluidic devices because it has excellent biocompatibility, chemical resistance, low autofluorescence, optical transparency, and releasability, and is inexpensive and disposable compared to glass. A typical microfluidic device is formed by laminating a cover sheet made of silicone or glass that covers the microchannels on a substrate sheet made of silicone with fine microchannels of about 500 nm to 1 mm in width recessed on the surface, and bonding the laminated surfaces of the substrate sheet and cover sheet facing each other to integrate the two laminated sheets.
[0006] When using an existing bonding method that uses an adhesive to bond a base sheet and a cover sheet, there is a concern that the adhesive components (e.g., organic solvent) will leak from the bonding surface into the microchannel and affect the sample injected into the microchannel, so conventionally, as shown in Patent Documents 1 and 2, when laminating a base sheet and a cover sheet, the opposing lamination surfaces are irradiated with atmospheric pressure plasma or excimer UV to modify the surface of the lamination surfaces, and then the two lamination surfaces are closely attached to each other and left for a certain period of time to bond them, as shown in Patent Document 1 and Patent Document 2. It is also known in Patent Document 3 that the laminated surfaces of the base sheet and cover sheet made of silicone are irradiated with an electron beam to modify the surface of the lamination surfaces and bond them.
[0007] Patent Document 4 describes a photobonding method in which a glass substrate is placed on a silicone base, the surface of the glass substrate is irradiated with vacuum ultraviolet light, and an oxide film of 10 nm or less is formed on the laminated surface of the silicone base facing the glass substrate, and the silicone base and the glass substrate are bonded via the oxide film. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2004-154898 A [Patent Document 2] Patent No. 3714338 [Patent Document 3] JP 2014-21081 A [Patent Document 4] JP 2004-331731 A [Non-Patent Document 1] TGOyama et al.,Applied Physics Letters,112,213704(2018) Summary of the Invention [Problem to be solved by the invention]
[0009] The bonding methods disclosed in Patent Documents 1 to 3 are techniques for bonding silicones by modifying the surface of the silicone in a range of several tens of nm deep from the surface, but it is difficult to modify the deeper parts of the silicone.
[0010] Furthermore, in bonding by the above-mentioned surface modification treatment, the bonding surfaces of the silicone to be bonded are irradiated in advance with atmospheric pressure plasma or excimer UV, so it is necessary to separate the silicone to be bonded. Furthermore, because the surface modification is temporary, there is a constraint in the bonding process that the bonding surfaces must be quickly brought into close contact after the surface modification treatment.
[0011] Even in the manufacturing methods described in Patent Documents 1 to 3, in which the laminated surfaces of a silicone base sheet and a cover sheet are surface-modified, the base sheet and the cover sheet are bonded together, and a microfluidic device is formed in which the base sheet and the cover sheet are laminated together, a complicated manufacturing process is required in which the laminated surfaces are surface-modified by plasma irradiation or vacuum ultraviolet irradiation, the base sheet and the cover sheet are relatively positioned (aligned), the surface-modified laminated surfaces are brought into close contact, and the close contact state is maintained for a predetermined time. In addition, the alignment work between the base sheet in which the microchannel is recessed and the cover sheet covering the microchannel requires high accuracy, and once the laminated surfaces are brought into close contact, they cannot be reattached, resulting in a low manufacturing yield.
[0012] According to the photobonding method described in Patent Document 4, a glass cover sheet is laminated on a silicone base sheet, and the surface of the glass cover sheet is irradiated with vacuum ultraviolet light to bond the base sheet and cover sheet together. However, the cover sheet must be made of glass that transmits vacuum ultraviolet light, and the base sheet and cover sheet are bonded together via an oxide film that is formed on the surface of the silicone base sheet by irradiation with vacuum ultraviolet light, which can result in problems such as uneven bonding and insufficient bonding strength.
[0013] There is also a demand for microfluidic devices in which multiple base sheets, each with a recessed microchannel, are stacked in multiple stages and a sample is injected into each of the multiple microchannels formed between the stacked surfaces of the multiple stages, enabling high-speed parallel processing, and for microfluidic devices in which communication holes are drilled in each of the base sheets stacked in multiple stages to connect the microchannels formed on both sides of the base sheets, forming a three-dimensional microchannel. However, it is extremely difficult to manufacture these multi-stage microfluidic devices using the bonding methods described in Patent Documents 1 to 3, which require high-precision positioning and adhesion of each of the stacked base sheets and cover sheets, or the photobonding method described in Patent Document 4, which involves irradiating vacuum ultraviolet light.
[0014] Furthermore, as mentioned above, silicone is suitable as a material for microfluidic devices, but because it has a porous structure with countless micropores of about 2-3 μm, it lacks gas barrier properties and sorbs low molecular weight compounds (sorption, absorption into solid polymers). Therefore, when an aqueous solution of a sample is injected into a microchannel surrounded by silicone, the concentration drops significantly, and it was thought to be unsuitable as a material for microfluidic devices for culturing and analyzing water-soluble samples.
[0015] Furthermore, polydimethylsiloxane (hereinafter referred to as PDMS), a typical silicone, is hydrophobic with a contact angle of 105 degrees, so there was a risk that liquid samples would stagnate due to surface tension within the minute microchannels of microfluidic devices.
[0016] The present invention has been made in consideration of the above-mentioned conventional problems, and has an object to provide a method for joining a joined body (a silicone joined body) that firmly joins a silicone molded body and another silicone or glass molded body simultaneously at multiple contact points between the two molded bodies.
[0017] Another object of the present invention is to provide a method for bonding silicone molded articles that changes the physical properties of silicone molded articles within a certain range.
[0018] Another object of the present invention is to provide a microfluidic device and a method for manufacturing the same, which can firmly bond the laminated surfaces of a pair of silicone molded sheets, in which a microchannel is formed between the laminated surfaces, after alignment, thereby laminated the pair of molded sheets together.
[0019] Another object of the present invention is to provide a microfluidic device and a manufacturing method thereof, in which a microchannel is formed between each laminated surface, and multiple silicone molded sheets that are laminated in multiple stages can be aligned together, and then the laminated surfaces can be firmly bonded together to integrally stack multiple molded sheets in multiple stages.
[0020] Another object of the present invention is to provide a microfluidic device and a method for manufacturing the same, which add gas barrier properties to the silicone molded sheet that forms the microchannel and suppresses sorption of samples injected into the microchannel.
[0021] Another object of the present invention is to provide a microfluidic device and a method for manufacturing the same, in which the silicone molded sheet that forms the microchannel is changed from hydrophobic to hydrophilic, thereby not impeding the flow of samples within the microchannel. [Means for solving the problem]
[0022] In order to achieve the above-mentioned object, the method for joining a joined body according to claim 1 is a method for joining a joined body in which one or more first molded bodies mainly composed of polyorganosiloxane and one or more second molded bodies mainly composed of polyorganosiloxane or glass are simultaneously joined together, The method is characterized in that, while the first molded body and the second molded body are in contact with each other, one or more contact points where they are in contact are irradiated with ionizing radiation consisting of any one of electron beams, gamma rays, and X-rays, and the siloxane main chains of the first molded body and the siloxane main chains of the second molded body are covalently bonded at the interface of the contact points by ionizing radiation crosslinking caused by the ionizing radiation.
[0023] At the contact points present within the range through which ionizing radiation penetrates, the siloxane main chains of the first and second molded bodies at the interface at the contact points are covalently bonded together by ionizing radiation crosslinking, resulting in a strong bond.
[0024] The method for bonding a bonded body according to claim 2 is characterized in that the ionizing radiation is either an electron beam or a gamma ray, and the absorbed dose of the ionizing radiation at the contact point is 860 kGy or more.
[0025] The bond strength at the contact point between the first and second compacts depends on the absorbed dose of ionizing radiation at the contact point, and when the absorbed dose of ionizing radiation is 860 kGy or more, a strong bond is formed at the contact point.
[0026] The method for bonding a bonded body according to claim 3 is characterized in that the ionizing radiation is an electron beam, and the accelerating voltage of the electron beam is 500 keV or more.
[0027] The higher the acceleration voltage, the deeper the ionizing radiation can penetrate through the first and second molded bodies along the direction of incidence of the ionizing radiation. By using an electron beam with an acceleration voltage of 500 keV or more, a thick material can be used as the first or second molded body that constitutes the silicone bonded body.
[0028] The microfluidic device described in claim 4 comprises a first molding sheet and a second molding sheet laminated on the first molding sheet, and the first lamination surface of the first molding sheet and the second lamination surface of the second molding sheet, which are in contact with each other in the lamination direction, are joined with a microchannel formed therebetween, and the first molding sheet and the second molding sheet are laminated together, wherein the first molding sheet is formed of polyorganosiloxane, and the second molding sheet is formed of polyorganosiloxane, glass, or an organic resin having a siloxane coating formed on the second lamination surface, and the first lamination surface and the second lamination surface, which are in contact with each other in the lamination direction, are bonded together by ionizing radiation consisting of any one of electron beams, gamma rays, and X-rays that penetrates the first lamination surface and the second lamination surface, so that the siloxane main chains of the first lamination surface and the siloxane main chains of the second lamination surface are covalently bonded by ionizing radiation crosslinking caused by the ionizing radiation, and the first molding sheet and the second molding sheet are laminated together.
[0029] At the interface between a first laminated surface formed from polyorganosiloxane and a second laminated surface on which a coating of polyorganosiloxane, glass or siloxane is formed, which are opposed in the lamination direction, the siloxane main chains of the first laminated surface and the second laminated surface are covalently bonded by ionizing radiation crosslinking, thereby forming a strong bond.
[0030] The first molded sheet, in which a microchannel is formed between the first and second laminated surfaces, is penetrated by ionizing radiation, and hydrophobic CH 3 The side chains (e.g., methyl groups) disappear when exposed to ionizing radiation, and the hydrophilic siloxane main chain with high binding energy appears. As a result, the microchannels are formed in the first molding sheet, which has changed from hydrophobic to hydrophilic.
[0031] Similarly, when ionizing radiation penetrates the first molded sheet having the microchannel formed between the first and second laminated surfaces, the irregular flexible siloxane main chains are bound by covalent bonds with adjacent siloxane main chains at many points, and the first molded sheet changes to have gas barrier properties. As a result, the microchannel is formed in the first molded sheet having gas barrier properties.
[0032] The microfluidic device described in claim 5 is characterized in that a stress relaxation portion consisting of a groove or a slit communicating with the side surfaces of the first molded sheet and the second molded sheet which are laminated together is formed on at least one of the first and second laminated surfaces excluding the portion where a microchannel is formed.
[0033] The stress relaxation portion formed on at least one of the first and second laminated surfaces absorbs distortion caused by the penetration of ionizing radiation into the first molded sheet or the second molded sheet, so that even when the first and second laminated surfaces are joined, the first and second molded sheets, which are laminated together, do not bend due to uneven distortion.
[0034] When ionizing radiation penetrates the first and second laminated surfaces, gas is generated at the interface between the first and second laminated surfaces and is released to the outside from the sides of the first and second molded sheets, which are laminated together, through the stress relief section.
[0035] The microfluidic device according to claim 6 is characterized in that the ionizing radiation is an electron beam.
[0036] The first and second lamination surfaces are bonded together using an electron beam, which has high directionality and allows easy control of irradiation timing.
[0037] The method for producing a microfluidic device according to claim 7 includes laminating a first molded sheet and a second molded sheet, and bonding the first and second laminated surfaces excluding a portion where the microchannel is formed, in a state where a first laminated surface of the first molded sheet and a second laminated surface of the second molded sheet opposed to each other in a lamination direction are formed with a microchannel. The first molded sheet is made of polyorganosiloxane, and the second molded sheet is made of polyorganosiloxane, glass, or an organic resin having a siloxane coating formed on the second laminated surface. the first and second molded sheets are laminated together, the laminated first and second molded sheets are positioned relative to one another, and the first and / or second molded sheets laminated after being positioned relative to one another are irradiated with ionizing radiation consisting of any one of electron beams, gamma rays, and X-rays, so that at a contact surface where the first and second laminated surfaces come into contact with each other, the siloxane main chains of the first and second laminated surfaces are covalently bonded to each other by ionizing radiation crosslinking caused by the ionizing radiation, thereby joining the first and second laminated surfaces except for the portion where the microchannel is formed.
[0038] By irradiating the first molded sheet and / or the second molded sheet which are stacked in relative position with respect to one another with ionizing radiation, at the interface between the first laminated surface formed from polyorganosiloxane which faces the stacking direction and the second laminated surface on which a coating of polyorganosiloxane, glass or siloxane is formed, the siloxane main chains of the first laminated surface and the second laminated surface are covalently bonded by ionizing radiation crosslinking, resulting in a strong bond.
[0039] By irradiating the first molded sheet and / or the second molded sheet formed from polyorganosiloxane with ionizing radiation, hydrophobic CH 3 The side chains (e.g., methyl groups) disappear when exposed to ionizing radiation, and a hydrophilic siloxane main chain with high binding energy appears. As a result, the microchannel is formed in the first molded sheet and / or the second molded sheet, which have changed from hydrophobic to hydrophilic.
[0040] Similarly, by irradiating the first molded sheet and / or the second molded sheet formed from polyorganosiloxane with ionizing radiation, the siloxane main chains having an irregular flexible structure are bound by covalent bonds with adjacent siloxane main chains at many points and are changed to have gas barrier properties. As a result, the microchannels are formed in the first molded sheet and / or the second molded sheet having gas barrier properties.
[0041] The method for manufacturing a microfluidic device described in claim 8 is characterized in that one or more of the first molded sheets and one or more of the second molded sheets are stacked alternately in multiple layers, all of the first molded sheets and all of the second molded sheets adjacent to each other in the stacking direction are positioned relative to each other, the first molded sheets and / or the second molded sheets stacked in multiple layers after being positioned relative to each other are irradiated with the ionizing radiation, and all of the first stacked surfaces and the second stacked surfaces except for the portions where microchannels are formed are simultaneously bonded.
[0042] After the first and second molded sheets, which are alternately stacked in multiple stages, are positioned relative to one another, the first and second molded sheets, which are stacked in multiple stages, are simultaneously and firmly joined together.
[0043] All of the first molded sheets and / or second molded sheets formed from polyorganosiloxane are simultaneously changed from hydrophobic to hydrophilic in a single step of exposure to ionizing radiation, and are endowed with gas barrier properties.
[0044] The manufacturing method of a microfluidic device described in claim 9 is characterized in that all of the first molded sheets and the second molded sheets adjacent to each other in the stacking direction are positioned relative to each other so that through holes penetrating the first molded sheet and / or the second molded sheet in the stacking direction are connected to a microflow path formed between the first stacking surface and the second stacking surface.
[0045] All of the first and second molded sheets that are adjacent in the stacking direction are positioned relative to one another so that the through holes that penetrate the first and / or second molded sheets in the stacking direction are connected to a microchannel, and then the first and second molded sheets stacked in multiple layers are firmly bonded together at the same time.
[0046] The method for manufacturing a microfluidic device described in claim 10 is characterized in that a stress relaxation portion consisting of a groove or a slit communicating with the side surfaces of the first molded sheet and the second molded sheet which are integrated by joining the first laminated surface and the second laminated surface is formed on at least one of the first laminated surface and the second laminated surface excluding the portion where the microchannel is formed.
[0047] The stress relaxation portion formed on at least one of the first and second lamination surfaces absorbs the distortion caused by the penetration of ionizing radiation into the first or second molded sheet, so that even if the first and second molded sheets are stacked in multiple layers and the bending displacement accumulates, the entire stack will not bend or warp significantly.
[0048] When a first molding sheet and / or a second molding sheet formed from polyorganosiloxane is irradiated with ionizing radiation, gas generated inside the first molding sheet and / or the second molding sheet is released to the outside from the side of the first molding sheet and the second molding sheet which are joined together through a stress relief portion consisting of a groove or a slit.
[0049] The method for manufacturing a microfluidic device according to an eleventh aspect of the present invention is characterized in that the microchannel and the recessed groove have the same depth from the first stacking surface and the same depth from the second stacking surface.
[0050] A mold having protrusions of the same height for forming the microchannels and recessed grooves can be easily obtained by resist etching using photolithography technology or electroforming.
[0051] The method for manufacturing a microfluidic device described in claim 12 is characterized in that the entire surface of the first molded sheet and / or the second molded sheet including the portion where the microchannel is formed is irradiated with ionizing radiation along the stacking direction.
[0052] Since the entire surface of the first molded sheet and / or the second molded sheet including the portion where the microchannel is formed is irradiated with ionizing radiation, the inner surface of the microchannel formed from polyorganosiloxane becomes hydrophilic and has gas barrier properties.
[0053] The method for producing a microfluidic device according to claim 13 is characterized in that the ionizing radiation is an electron beam.
[0054] All of the first and second lamination surfaces are bonded together using an electron beam, which has high directivity and allows easy control of the irradiation timing. Effect of the Invention
[0055] According to the invention of claim 1, one or more contact points where the first molded body or the second molded body are in contact can be firmly joined simultaneously.
[0056] In addition, the water contact angle can be reduced in the range from the surface to the contact point of the first molded article or the second molded article mainly composed of polyorganosiloxane.
[0057] According to the invention of claim 4, the first molding sheet and the second molding sheet are bonded in a stacked state by irradiation with ionizing radiation, so that the first molding sheet and the second molding sheet can be aligned before the bonding process.
[0058] The first and second molded sheets, which have a microchannel formed between their laminated surfaces, can be changed from hydrophobic to hydrophilic, so that an aqueous solution sample injected into the microchannel does not become stagnant within the microchannel due to surface tension.
[0059] In addition, the first and second molded sheets, which have a microchannel formed between their laminated surfaces, have gas barrier properties, and even if silicone is used as a material for the microfluidic device, sorption of samples such as low molecular weight compounds injected into the microchannel can be suppressed.
[0060] According to the invention of claim 5, even when joined by ionizing radiation that penetrates the first and second laminated surfaces, the first and second molded sheets laminated together maintain their flatness without bending due to uneven distortion.
[0061] Furthermore, even if ionizing radiation passes through the first and second lamination surfaces, gas does not remain at the interface between the first and second lamination surfaces, and the generation of voids at the interface due to residual gas can be suppressed.
[0062] According to the invention of claim 6, the first and second stacking surfaces are joined by an electron beam, which has high directionality and whose irradiation timing is easy to control, thereby facilitating mass production of microfluidic devices in which the first and second molding sheets are stacked together.
[0063] According to the invention of claim 7, after the stacked first and second molding sheets are positioned relative to each other, the first and / or second molding sheets are irradiated with ionizing radiation and bonded to each other, so that the relative positioning of the first and second molding sheets can be repeatedly performed before bonding.
[0064] The first molded sheet and / or the second molded sheet, in which a microchannel is formed between the laminated surfaces, can be changed from hydrophobic to hydrophilic, so that a liquid sample injected into the microchannel does not stagnate within the microchannel due to surface tension.
[0065] Furthermore, since gas barrier properties can be imparted to the first molded sheet and / or the second molded sheet having a microchannel formed between the laminated surfaces, even if silicone is used as a material for the microfluidic device, sorption of samples such as low molecular weight compounds injected into the microchannel can be suppressed.
[0066] According to the invention of claim 8, all of the first and second molded sheets stacked alternately in multiple layers can be positioned relative to one another with microchannels formed therebetween, and then all of the first and second molded sheets adjacent to one another in the stacking direction can be firmly bonded simultaneously, making it possible to easily manufacture a microfluidic device in which a large number of microchannels are formed in parallel or in which microchannels are formed in a three-dimensional shape.
[0067] All of the microchannels formed between the first and second stacking surfaces can be formed in the first molded sheet and / or the second molded sheet which are made of polyorganosiloxane and have been rendered hydrophilic.
[0068] Furthermore, even if the first molded sheet and / or the second molded sheet in which a microchannel is formed between the laminated surfaces is a molded sheet formed from polyorganosiloxane, gas barrier properties can be imparted to the molded sheet.
[0069] According to the invention of claim 9, after all of the first and second molded sheets stacked in multiple alternating stages are positioned relative to one another so that the through holes passing through the first and / or second molded sheets in the stacking direction are connected to the microchannel, all of the first and second molded sheets adjacent in the stacking direction can be firmly bonded together at the same time, making it possible to easily manufacture a microfluidic device in which a microchannel is formed in a three-dimensional shape.
[0070] According to the invention of claim 10, in the step of irradiating the first and / or second molded sheets stacked in multiple stages with ionizing radiation and bonding the first and second laminated surfaces, even if distortion occurs in a part of the bonding surface, the distortion does not extend beyond the stress relaxation part formed on the bonding surface, and each of the first and second molded sheets to be bonded can be maintained flat. Therefore, even if the first and second molded sheets are alternately and integrally stacked in multiple stages, the microchannels formed between the first and second laminated surfaces do not become partially inclined or have a change in inner diameter, and the entire stacked multistage structure does not bend or warp significantly.
[0071] When the first and / or second molded sheets stacked in multiple layers are irradiated with ionizing radiation, even if gas is generated inside the first and / or second molded sheets formed from polyorganosiloxane, the gas is released to the outside through the fine pores in the polyorganosiloxane and the stress relaxation parts formed on the bonding surfaces, thereby suppressing voids that would occur in the first and second molded sheets due to residual gas.
[0072] According to the invention of claim 11, the microchannel and the grooves of the stress relaxation portion can be formed by an electroforming mold capable of high-precision forming or a resist etching mold by photolithography technology.
[0073] According to the invention of claim 12, the inner surface of the microchannel becomes hydrophilic, so that an aqueous solution sample injected into the microchannel does not stagnate within the microchannel, and sorption of a sample such as a low molecular weight compound injected into the microchannel can be suppressed.
[0074] In addition, since ionizing radiation penetrates all the microchannels, the insides of the microchannels are sterilized.
[0075] According to the invention of claim 13, all of the first and second stacking surfaces are bonded by an electron beam, which has high directionality and makes it easy to control the irradiation timing, thereby facilitating mass production of microfluidic devices in which the first and second molding sheets are stacked together. [Brief description of the drawings]
[0076] [Figure 1] FIG. 1 shows a manufacturing process for a silicone bonded body 1 in accordance with a first embodiment of the present invention, in which (a) is a temporarily fastened body 1′, (b) is a step of irradiating the temporarily fastened body 1′ with ionizing radiation, and (c) is a side view of the silicone bonded body 1 in which a first molded body 2 and a second molded body 3 have been bonded together by irradiating with ionizing radiation. [Diagram 2] FIG. 13 is an explanatory diagram illustrating a method for comparing the bonding strength of two PDMS films 5A and 5B bonded by irradiating them with gamma rays. [Diagram 3]1 is a graph showing a bondable range when a bonded body is obtained by irradiating PDMS with electron beams having different accelerating voltages. [Figure 4] The photograph was taken from the flat side of a silicone bonded assembly in which ten PDMS films were bonded together by irradiation with an electron beam. [Diagram 5] 5 is a photograph of the silicone bonded body of FIG. 4 taken from the side. [Figure 6] FIG. 11 is an exploded perspective view of a microfluidic device 10 according to a second embodiment. [Figure 7] FIG. 1 is a longitudinal cross-sectional view of a microfluidic device 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0077] A silicone bonded body 1 according to a first embodiment of the present invention and a method for manufacturing the silicone bonded body 1 will be described below with reference to Fig. 1. In Fig. 1, the bonded body 1 is composed of three first molded bodies 2 (2a, 2b, 2c) and three second molded bodies 3 (3a, 3b, 3c), which are bonded to each other at contact regions 4a to 4h by covalent bonds, which will be described later.
[0078] <Method of Manufacturing Silicone Bonded Body> The method for producing the silicone bonded body 1 includes a step of irradiating ionizing radiation to a contact point where one or more first molded bodies 2 and one or more second molded bodies 3 are in contact with each other. The ionizing radiation irradiation step includes irradiating the first molded body 2 and the second molded body 3 in a state where they are in contact with each other with ionizing radiation. In other words, the method includes a step of irradiating a temporarily joined body in which the first molded body 2 and the second molded body 3 are in contact with each other with ionizing radiation. By the irradiation of ionizing radiation, the first molded body 2 and the second molded body 3 are bonded to each other at the contact point where they are in contact with each other.
[0079] 1(a) shows the temporarily fixed body before being irradiated with ionizing radiation. As shown in the figure, the first molded body 2 and the second molded body 3 are temporarily held to maintain contact at all of the contact areas 4a to 4h where they are in contact with each other, forming a temporarily fixed body 1'. The temporarily fixed body 1' may maintain the contact state of each molded body with a jig (not shown) or may maintain the contact state of each molded body by utilizing the self-adhesive properties of silicone.
[0080] The first molded body 2 may contain other substances as long as it is mainly composed of polyorganosiloxane. Here, the main component refers to a polyorganosiloxane content of 50 mass% or more. It preferably contains 80 mass% or more, more preferably 90 mass% or more, and even more preferably 98 mass% or more of polyorganosiloxane. For example, it may be formed of an organic resin such as cycloolefin polymer (COP) with a siloxane film formed on the lamination surface with another molded body. Furthermore, the main component of polyorganosiloxane includes one that is substantially composed of polyorganosiloxane.
[0081] The second molded body 3 is mainly composed of polyorganosiloxane or SiO 2 It is made of glass whose main component is SiO 2 The main component of glass is SiO 2 The content of SiO is 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and further preferably 98% by mass or more. 2 Includes.
[0082] Here, the polyorganosiloxane includes polydimethylsiloxane (PDMS). Hereinafter, the bonded body and the method for producing the bonded body will be described using an example in which the polyorganosiloxane is PDMS. In the embodiment shown in FIG. 1(a), a first molded body 2 and a second molded body 3 are both made of polyorganosiloxane and each is formed into a desired shape.
[0083] In this first embodiment, the first molded body 2a, 2b, 2c and the second molded body 3a, 3b, 3c may have any shape such as a film shape or a sphere shape, and each contact area 4a-4h or each inside may have a hollow portion, or a recess or a protrusion may be formed. In addition, the first molded body 2 and the second molded body 3 may have a positioning mechanism for facilitating contact at a desired position.
[0084] Next, the temporary fastener 1' is irradiated with ionizing radiation. The irradiation of ionizing radiation bonds the first compact 2 and the second compact 3 at contact points or contact areas present within a range of a depth D through which the ionizing radiation penetrates. In the embodiment shown in Fig. 1(b), ionizing radiation is irradiated vertically from above downward, bonding contact areas 4a to 4h of the temporary fastener 1'.
[0085] In the present embodiment, the ionizing radiation may be any known type, such as an electron beam, gamma rays, or X-rays. One or more types of such ionizing radiation may be irradiated in combination.
[0086] When the ionizing radiation is an electron beam, the depth D of penetration of the electron beam into the temporary fastener 1' varies depending on the acceleration voltage of the electron beam, and the higher the acceleration voltage, the longer D becomes. For example, when PDMS with a density of 0.965 g / cm3 is irradiated from one direction with an electron beam of 500 keV, D is approximately 1.5 mm, and if there is a hollow area in between, D becomes even longer. Therefore, when the length from the surface of the first molded body 2a of the temporary fastener 1' made of PDMS to the contact area 4d along the incident direction of the ionizing radiation is 1.5 mm, an electron beam with an acceleration voltage of 500 keV is irradiated.
[0087] When the ionizing radiation is gamma rays from cobalt 60, the depth D to which the gamma rays penetrate into the temporary fixing body 1' made of PDMS is about 300 mm, and if there is a hollow region therebetween, D becomes even longer.
[0088] Any number of contact points or contact areas 4 can be bonded at one time by irradiation with ionizing radiation as long as they are within the range of ionizing radiation penetration D. For example, in the case where five film-like silicone molded bodies or glass molded bodies each having a thickness of 100 μm are stacked, all of the molded bodies can be bonded at once by irradiating them with ionizing radiation that penetrates to a depth of 500 μm or more from the surface.
[0089] The irradiation conditions of the ionizing radiation are not particularly limited, but for example, when an electron beam is used, it is preferably 10 keV or more, more preferably 30 keV or more, and even more preferably 500 keV or more. The acceleration voltage may be appropriately set according to the thickness of the objects to be joined. As described above, the higher the acceleration voltage of the electron beam, the greater the penetration depth D of the electron beam. The upper limit of the acceleration voltage of the electron beam is not particularly limited, but it may be set to, for example, 10 MeV or less, for example, 5 MeV or less.
[0090] Also, the absorbed dose of ionizing radiation (e.g., electron beam or gamma ray) in each of the contact regions 4a-4h is preferably 200 kGy or more, more preferably 500 kGy or more, and even more preferably 860 kGy or more, so as to firmly bond each of the contact regions 4a-4h. The greater the absorbed dose, the more covalent bonds are formed, as described below. However, if the absorbed dose is too large, the mechanical strength of the first or second molded body decreases, so it is preferably 40 MGy or less, and more preferably 20 MGy or less, for example.
[0091] Furthermore, the size of the irradiation spot of the ionizing radiation may be any size as long as the joining contact point or contact area 4 is included in the range through which the ionizing radiation passes, and may be either fixed irradiation in which the irradiation spot does not move, or scanning irradiation in which the irradiation spot moves.
[0092] The irradiation of ionizing radiation may be performed once or in a combination of multiple steps, and the bonded body (temporarily bonded body) may be irradiated with ionizing radiation from one direction or the irradiation direction may be changed. Furthermore, the bonding of each of the contact regions 4a to 4h may be performed by combining the above-mentioned irradiation of ionizing radiation with an existing bonding method using an adhesive or surface modification of the contact surface by plasma treatment or the like.
[0093] When the temporary fixing body 1' is irradiated with ionizing radiation, the ionizing radiation penetrates the first molded bodies 2a, 2b, and 2c made of polyorganosiloxane (e.g., PDMS) and the second molded bodies 3a, 3b, and 3c, as shown by the dashed lines in FIG. 1(b). Polyorganosiloxane (e.g., PDMS) is exposed to the ionizing radiation and becomes CH 3 Side chains such as (methyl groups) are cut off and disperse as gas. Therefore, between the siloxane main chains, (1 set) [ka] (2 sets) [ka] (3 types) [ka] (In formula 1, formula 2, and formula 3, R represents an organic group and may be the same or different from each other) and are bonded by a covalent bond through a siloxane bond (-Si-O-Si-) shown in any one of the structural formulas.
[0094] In the above formulas 1, 2, and 3, R is not particularly limited as long as it is an organic group, for example, an alkyl group (e.g., methyl, ethyl, propyl, or butyl), an aryl group (e.g., phenyl or naphthyl), or a hydrogen atom, and is preferably a methyl group.
[0095] The ionizing radiation also penetrates each of the contact areas 4a to 4h (i.e., contact points) where the first molded bodies 2a, 2b, and 2c come into contact with the second molded bodies 3a, 3b, and 3c. The polyorganosiloxane (e.g., PDMS) facing these contact areas 4a to 4h is similarly subjected to the ionizing radiation and is converted into CH 3 Side chains such as methyl groups are cleaved, and at the interface of each contact region 4a to 4h, the PDMS having a (-Si-O-) group and the PDMS or glass are covalently bonded via a siloxane bond consisting of (-Si-O-Si-) having the structure shown in formulas (1) to (3).
[0096] That is, along the incident direction of the ionizing radiation (vertical direction), the first molded bodies 2a, 2b, 2c and the second molded bodies 3a, 3b, 3c that are in contact with each other are simultaneously and firmly bonded to each other at all contact regions 4a-4h (i.e., contact points) within the range of depth D through which the ionizing radiation penetrates from the surface of the temporary fixing body 1' (the surface of the first molded body 2a or the surface of the second molded body 3a), thereby obtaining an integral silicone bonded body 1 as shown in Figure 1(c).
[0097] In addition, when the first molded body 2a, 2b, 2c or the second molded body 3a, 3b, 3c is mainly composed of polyorganosiloxane (e.g., PDMS), the polyorganosiloxane (e.g., PDMS) constituting the first molded body and the second molded body within the range where the ionizing radiation penetrates along the incident direction of the ionizing radiation (the range from the ionizing radiation irradiated surface to a depth D) is subjected to ionizing radiation and covalently bonds between the siloxane main chains with siloxane bonds consisting of (-Si-O-Si-) having the structures shown in formulas (1) to (3). That is, covalent bonds having the structures shown in formulas (1) to (3) are formed at the junction between the first molded body and the second molded body present within the range where the ionizing radiation penetrates and in a region 500 nm or more away from the junction of the first molded body or the second molded body.
[0098] When the first molded body or the second molded body mainly made of polyorganosiloxane (e.g., PDMS) is irradiated with the ionizing radiation, hydrophobic CH 3Side chains such as (methyl group) are exposed to ionizing radiation and disappear, revealing the hydrophilic siloxane main chain. As a result, the contact angle of the molded body with water decreases in the range from the surface (irradiated surface) of the molded body mainly composed of polyorganosiloxane to the contact point. That is, the water contact angle can be reduced in the range from the surface of the first molded body or the second molded body mainly composed of polyorganosiloxane to the point where the ionizing radiation penetrates. For example, when the first molded body or the second molded body is mainly composed of PDMS, the water contact angle before irradiation with ionizing radiation is about 105 degrees, but after irradiation with ionizing radiation, the water contact angle can be reduced to 100 degrees or less, preferably 90 degrees or less, more preferably 80 degrees or less.
[0099] In addition, when the first or second molded body mainly made of polyorganosiloxane (e.g., PDMS) is irradiated with the ionizing radiation, covalent bonds having the structures shown in the formulae (1) to (3) above are formed in the ionizing radiation transmission range of the molded body. That is, in the range from the surface (irradiated surface of ionizing radiation) of the molded body mainly made of polyorganosiloxane to the transmission of ionizing radiation, the siloxane main chains having an irregular flexible structure are bound by covalent bonds with adjacent siloxane main chains at many points and change to have gas barrier properties. For example, compared to the gas barrier property before the irradiation of ionizing radiation, the gas permeability is reduced to 90% or less, preferably 80% or less, and more preferably 70% or less. In other words, the ionizing radiation transmission region of the bonded body has a lower gas permeability than the ionizing radiation non-transmission region, and the gas permeability of the ionizing radiation transmission region is preferably 90% or less of the ionizing radiation non-transmission region, more preferably 80% or less, and more preferably 70% or less.
[0100] The gas barrier properties (gas permeability) of the bonded structure can be evaluated using oxygen permeability and / or water vapor permeability as indicators. Oxygen permeability can be evaluated in accordance with JIS K7126-1 Appendix 2, and water vapor permeability can be evaluated in accordance with JIS K7129-1 Method A.
[0101] Whether the structures of the first molded bodies 2a, 2b, 2c and the second molded bodies 3a, 3b, 3c have changed to the above structures can be confirmed by X-ray photoelectron spectroscopy or Fourier transform infrared spectroscopy, since the amount of carbon or structures containing carbon (such as methyl groups) is reduced by 3% or more compared to before irradiation with ionizing radiation.
[0102] Silicone Bonded Body The silicone bonded body 1 disclosed in this specification is a bonded body in which one or more first molded bodies mainly composed of polyorganosiloxane are bonded to one or more second molded bodies mainly composed of polyorganosiloxane or glass, and the first molded bodies and the second molded bodies are bonded at one or more bonding points. The first molded body and the second molded body may be appropriately selected from those described in the manufacturing method of the silicone bonded body 1. A detailed description thereof will be omitted here.
[0103] The silicone bonded body 1 is formed by bonding a first molded body and a second molded body at the interface between the two bodies via siloxane bonds (-Si-O-Si-) having structures represented by formulas (1) to (3).
[0104] In the silicone bonded body 1, in a region of a molded body mainly composed of polyorganosiloxane, through which ionizing radiation has penetrated during the manufacturing process of the bonded body, the siloxane main chain of the polyorganosiloxane is bonded by a siloxane bond having the structure (-Si-O-Si-) shown in the above formulas (1) to (3). In other words, in at least one of the first molded body or the second molded body, the siloxane main chains are bonded by a siloxane bond having the structure (-Si-O-Si-) shown in the formulas (1) to (3) at a depth of 500 nm or more from the bonding point. The depth at which the siloxane bonds formed inside the first molded body or the second molded body can be confirmed depends on the thickness of the molded body, but can be confirmed in a region at least 500 nm or more, preferably 800 nm or more, and more preferably 1000 nm or more away from the bonding point.
[0105] The presence of the siloxane bond consisting of (-Si-O-Si-) in the structures represented by formulas (1) to (3) can be confirmed by the above structural change using an X-ray photoelectron spectrometer or Fourier transform infrared spectroscopy.
[0106] In addition, in the above structure, the hydrophobic CH 3 The side chains (such as methyl groups) are scattered by the ionizing radiation, and the hydrophilic siloxane main chain is revealed, so that the contact angle with water of the first molded bodies 2a, 2b, 2c and the second molded bodies 3a, 3b, 3c through which the ionizing radiation has penetrated also decreases.
[0107] In addition, the main chains of the siloxane having an irregular flexible structure of PDMS in the first molded bodies 2a, 2b, 2c and the second molded bodies 3a, 3b, 3c are bound by covalent bonds with adjacent main chains of siloxane at many points, changing to have gas barrier properties, and the gas permeability is suppressed by 3% or more compared to before the irradiation of ionizing radiation. The change in gas permeability can be evaluated by measuring the amount of oxygen or water vapor that permeates the test piece with a pressure sensor, gas chromatograph, etc.
[0108] Furthermore, the first molded bodies 2a, 2b, and 2c and the second molded bodies 3a, 3b, and 3c through which ionizing radiation has penetrated shrink depending on the absorbed dose of ionizing radiation, and the compressive elastic modulus increases by 5% or more compared to that before the irradiation of ionizing radiation. For example, by appropriately setting the absorbed dose of ionizing radiation, a bonded body can be obtained in which the elastic modulus has increased by preferably 8% or more, more preferably 10% or more compared to that before the irradiation of ionizing radiation. In other words, the ionizing radiation transmitting region of the bonded body has an elastic modulus increased by 5% or more compared to the ionizing radiation non-transmitting region, and a bonded body can be obtained in which the elastic modulus of the ionizing radiation transmitting region is increased by preferably 8% or more, more preferably 10% or more compared to that of the ionizing radiation non-transmitting region. The upper limit of the elastic modulus is not particularly limited, but if the elastic modulus is too high, the mechanical strength tends to decrease. For this reason, for example, the elastic modulus is preferably 50 MPa or less. The change in the elastic modulus can be confirmed by a scanning probe microscope or a compression test.
[0109] Example 1 (Joining between PDMS films by gamma rays) Two PDMS films 5A and 5B, each 1 mm thick, 1.5 cm wide, and 2 cm long, were placed horizontally with a 1 cm overlap, and were irradiated with gamma rays (cobalt-60) at four different absorbed doses of 700 kGy, 860 kGy, 1000 kGy, and 1640 kGy.Then, as shown in Figure 2, the two PDMS films 5A and 5B were pulled in opposite longitudinal directions as indicated by the arrows, and the bonding strength between the PDMS films 5A and 5B was compared.
[0110] As a result, as shown in Table 1, when the absorbed dose was 700 kGy or less, peeling occurred before material destruction occurred. When the absorbed dose was 860 kGy or more, the PDMS films 5A and 5B were firmly bonded to each other to such an extent that material destruction occurred before peeling occurred.
[0111] [Table 1]
[0112] Example 2 (Electron beam bonding between molded sheets constituting a multi-stage microfluidic device) A molded sheet made of 11 PDMS sheets, each of which had a microchannel formed between each layer, was irradiated with an electron beam in the stacking direction to confirm the bonding state between the 11 molded sheets.
[0113] The molded sheets are 0.5 mm thick PDMS sheets with microchannels microfabricated on the lamination surface, and the total thickness of the 11 molded sheets stacked and temporarily fixed is 5.5 mm. The acceleration voltage and irradiation energy (absorbed dose) of the electron beam for bonding the 11 molded sheets together are selected from the results of simulation. For example, Figure 3 shows the depth to which the electron beam penetrates when PDMS is irradiated with electron beams of different acceleration voltages, that is, the bondable range (D), calculated using a Monte Carlo simulation code. It shows that the bondable range D expands depending on the acceleration voltage.
[0114] Based on the results of this simulation, a stack of 11 0.5 mm-thick PDMS molded sheets was temporarily bonded together and irradiated with an electron beam at an accelerating voltage of 2 MeV until the average absorbed dose of the stack reached 2.2 MGy. As a result, a microfluidic device was obtained in which the 11 PDMS molded sheets were completely bonded together.
[0115] Example 3 (Joining of PDMS films by electron beam) Ten square PDMS films, each 0.5 mm thick and 20 mm long on each side, were temporarily laminated and irradiated with an electron beam at an accelerating voltage of 2 MeV until the average absorbed dose of the laminate reached 2 MGy.
[0116] As a result, a silicone bonded structure was obtained in which ten PDMS films were completely bonded between their respective laminated surfaces, as shown in Figures 4 and 5. This silicone bonded structure maintains high transparency, as shown in Figure 4.
[0117] Example 4 (Gas permeability evaluation) A PDMS sheet measuring 1 mm thick and 15 cm square was irradiated with a 1 MeV electron beam at approximately 2.2 MGy, and the oxygen permeability and water vapor permeability were compared with that of an unirradiated PDMS sheet. The oxygen permeability was evaluated in accordance with JIS K7126-1 Appendix 2, and the water vapor permeability was evaluated in accordance with JIS K7129-1 Method A. As shown in Table 2 below, the oxygen permeability and water vapor permeability of PDMS both decreased after irradiation, indicating that the present invention reduces gas permeability and improves gas barrier properties.
[0118] [Table 2]
[0119] Example 5 (Hardness rating) A sample consisting of three 500μm thick, 10mm x 20mm PDMS films was irradiated with 1.6MGy of gamma rays (cobalt 60) and bonded. The compressive modulus of the sample before and after irradiation, i.e. before and after bonding, was evaluated using a creep meter (RE2-3305B, Yamaden) under a load of 20N, and it was found that the Young's modulus, which was about 3MPa before irradiation, increased to about 5.5MPa after irradiation. This result shows that the compressive modulus of PDMS increases according to the present invention.
[0120] Next, a microfluidic device 10 according to a second embodiment of the present invention and a method for manufacturing the same will be described with reference to Figures 6 and 7. This microfluidic device 10 is configured by alternately laminating two cover sheets 11a, 11b and two base sheets 12a, 12b in four stages, and is used for injecting a trace amount of sample such as an organic compound or a biological sample into a microchannel 15 formed between a lamination surface 13 of the cover sheet 11 and a lamination surface 14 of the base sheet 12, which face each other in the lamination direction, and mixing, reacting, synthesizing, extracting, separating, or analyzing the sample injected into the microchannel 15.
[0121] 7, the third cover sheet 11b from the top also serves as a base sheet having recesses 15a recessed into its upper layer surface 13a facing the base sheet 12a above it, forming microchannels 15, and the second base sheet 12a from the top also serves as a cover sheet covering the recesses 15a recessed into the upper layer surface 13a of the cover sheet 11b. As a result, the microchannels 15 divided into three stages are formed in parallel between the respective layer surfaces 13, 14 of the cover sheets 11 and base sheets 12 stacked in four stages.
[0122] As the material of the microfluidic device 10, silicone (PDMS) has excellent biocompatibility, chemical resistance, low autofluorescence, optical transparency, and mold releasability, and is inexpensive and disposable compared to glass, so here, both the cover sheet 11 and the base sheet 12 are formed from PDMS, a type of polyorganosiloxane, but they may also be formed from an organic resin such as cycloolefin polymer (COP) with a siloxane coating formed on the lamination surfaces 13, 14. In addition, if neither the cover sheet 11 nor the base sheet 12, whose lamination surfaces 13, 14 face each other in the lamination direction, are formed from glass, one of the cover sheet 11 and the base sheet 12 may be formed from glass containing SiO2 as the main component.
[0123] The cover sheet 11 and the base sheet 12 are each formed into a flat plate with a thickness of 1.5 mm by injection molding using an electroforming mold, using PDMS as the molding material, and the surfaces (upper layered surfaces 13a, 14a) of the second to fourth layers of cover sheet 11b and base sheets 12a, 12b are formed with recesses 15a that form microchannels 15 with a width and depth of 500 nm to 1 mm, and numerous grooves 16 that serve as stress relief sections with the same depth as the recesses 15a.
[0124] The length, shape and number of recesses 15a forming microchannels 15 are arbitrarily designed according to the application of microfluidic device 10, and one end of recess 15a is cylindrical with an inner diameter longer than the width of recess 15a as shown in Fig. 6 in order to connect microchannel 15 to injection hole 18 and discharge hole 19 described later. Microchannels 15 formed in parallel in three stages between lamination surfaces 13, 14 of cover sheet 11 and base sheet 12 communicate with each other via through-holes 17 penetrating through second to fourth stages of cover sheet 11b and base sheets 12a, 12b, respectively.
[0125] Furthermore, the numerous grooves 16 that serve as stress relaxation sections are formed in a lattice pattern, with numerous grooves 16 extending in two perpendicular directions, intersecting with each other and evenly formed on the entire upper layer surface 13a of the cover sheet 11b and the upper layer surfaces 14a of the base sheets 12a and 12b, excluding the areas where the recesses 15a that form the microchannels 15 are formed. The grooves 16 are formed continuously up to the end faces of the cover sheet 11b and the base sheets 12a and 12b, and therefore communicate with the outside at the side of the microfluidic device 10 in which the cover sheets 11a, 11b and the base sheets 12a, 12b are alternately layered in four stages.
[0126] According to this embodiment, the recesses 15a forming the microchannels 15 recessed into the surfaces (upper layer surfaces 13a, 14a) of the cover sheet 11b and the base sheets 12a, 12b and the grooves 16 serving as stress relief sections are made to be the same depth, so that the recesses 15a and the grooves 16 forming the fine microchannels 15 can be formed by injection molding using an electroforming mold that can be molded with high precision.
[0127] The top cover sheet 11a is provided with an injection hole 18 for injecting a sample into the microchannel 15 and a discharge hole 19 for discharging the sample from the microchannel 15 at positions communicating with the microchannel 15 formed between the top cover sheet 11a and the base sheet 12a of the second layer.
[0128] As described above, both the base sheet 12 and the cover sheet 11 are molded by injection molding. However, if they can be molded using a mold to enable mass production, they can be molded by various molding methods such as transfer molding and compression molding as appropriate depending on the flow rate, type of PDMS, and shape of the base sheet 12 and cover sheet 11.
[0129] The two cover sheets 11a, 11b and the two base sheets 12a, 12b constructed as described above are bonded together by irradiating an electron beam between each of the stacking surfaces 13, 14 facing each other in the stacking direction, as shown in Figure 7, to form a microfluidic device 10 in which microchannels 15 are formed in parallel in three stages between each of the stacking surfaces 13, 14.
[0130] The following describes a method for manufacturing the microfluidic device 10. First, the two cover sheets 11a, 11b and the two base sheets 12a, 12b molded by injection molding as described above are stacked in order from the bottommost base sheet 12b to the topmost cover sheet 11a while positioning the top sheets relative to the bottom sheets. That is, the lower lamination surface 13b of the cover sheet 11b is bonded to the upper lamination surface 14a of the base sheet 12b so that the through-hole 17 drilled in the third-layer cover sheet 11b coincides with the recess 15a forming the microchannel recessed in the upper lamination surface 14a of the fourth-layer base sheet 12b, and then the lower lamination surface 14b of the base sheet 12a is bonded to the upper lamination surface 13a of the cover sheet 11b so that the through-hole 17 drilled in the second-layer base sheet 12a coincides with the recess 15a forming the microchannel recessed in the upper lamination surface 13a of the cover sheet 11b, and then the lower lamination surface 13b of the cover sheet 11a is bonded to the upper lamination surface 14a of the base sheet 12a so that the injection hole 18 and the discharge hole 19 drilled in the first-layer cover sheet 11a coincide with each end of the cylindrical recess 15a forming the microchannel recessed in the upper lamination surface 14a of the second-layer base sheet 12a.
[0131] In the above alignment step, in which the upper and lower lamination surfaces 13, 14 facing each other in the lamination direction are bonded together while the cover sheet 11 and the base sheet 12 are positioned relative to each other, the lamination surfaces 13, 14 are not joined together, so they can be peeled off and reattached many times until they are positioned accurately. In addition, since PDMS has a certain degree of self-adhesiveness, the two cover sheets 11a, 11b and the two base sheets 12a, 12b that are positioned relative to each other and stacked alternately can be temporarily held in a stacked state without using a specific jig or the like.
[0132] Next, the laminate consisting of the four sheets 11a, 11b, 12a, and 12b is irradiated with ionizing radiation to simultaneously bond the laminate surfaces 13 of all cover sheets 11 and the laminate surfaces 14 of the base sheet 12 that face each other in the stacking direction. Since the thickness of the laminate consisting of four stacked PDMS sheets is 6 mm, the simulation results shown in Figure 3 are referenced and an electron beam with an accelerating voltage of 2 MeV is irradiated.
[0133] The electron beam is applied evenly to the entire plane of the uppermost cover sheet 11a along the stacking direction (vertical direction) of the laminate, thereby simultaneously firmly bonding the stacking surfaces 13 of all cover sheets 11 and the stacking surfaces 14 of the base sheets 12 that face each other in the stacking direction, thereby producing a microfluidic device 10 in which two cover sheets 11a, 11b and two base sheets 12a, 12b are stacked together alternately.
[0134] As shown by the dashed line in FIG. 7, in this microfluidic device 10, upper and lower microchannels 15 communicate with each other via through-holes 17, so that a desired microchannel 15 can be designed in a three-dimensional shape.
[0135] In the step of irradiating the electron beam, the electron beam penetrates the entire area of the two cover sheets 11a, 11b and the two base sheets 12a, 12b, including the area where the microchannel 15 is formed. Therefore, the contact angle of the inner wall surface of the microchannel 15 with water decreases, and the aqueous solution injected into the microchannel 15 does not stagnate within the microchannel 15 due to surface tension.
[0136] Similarly, in the step of irradiating the electron beam, the electron beam penetrates the entire area of the two cover sheets 11a, 11b and the two base sheets 12a, 12b including the area where the microchannel 15 is formed, and therefore the gas permeability of the cover sheets 11a, 11b and the two base sheets 12a, 12b made of PDMS decreases. As a result, sorption of the sample injected into the microchannel 15 into the cover sheets 11a, 11b and the base sheets 12a, 12b can be suppressed.
[0137] Furthermore, an electron beam passes through the microchannel 15 between the stacking surfaces 13 and 14 while being shielded from the outside, so that the inside of the microchannel 15 is sterilized before the sample is injected.
[0138] Furthermore, the cover sheets 11a, 11b and the two base sheets 12a, 12b shrink when an electron beam penetrates them, but the shrinkage distortion is absorbed in the stress relaxation section, the recessed grooves 16, so the cover sheets 11a, 11b and the two base sheets 12a, 12b can be maintained flat. As a result, even if the cover sheets 11 and the base sheets 12 are stacked in multiple layers, the entire microfluidic device 10 does not bend or flex significantly.
[0139] Furthermore, by passing an electron beam through the cover sheet 11 and the base sheet 12 made of PDMS, CH 3 Side chains such as (methyl groups) turn into gas and are generated within the cover sheet 11 and the base sheet 12, but this gas is released to the outside through the micropores in the PDMS and the grooves 16, which serve as stress relief sections, so there is no risk of voids being generated within the cover sheet 11 or base sheet 12, or on their laminated surfaces 13, 14.
[0140] In the second embodiment, the cover sheet 11 and the base sheet 12, which are alternately laminated, are bonded together by irradiation with an electron beam, but they may also be bonded together by irradiation with other ionizing radiation such as gamma rays or X-rays.
[0141] In addition, in the above embodiment, the cover sheet 11 and the base sheet 12, which are stacked in four layers, are bonded by irradiating them with ionizing radiation. However, the present invention can also be applied to a microfluidic device 10 in which the cover sheets 11 and the base sheet 12 are stacked in multiple layers, as long as ionizing radiation reaches between all of the bonded laminated surfaces of the temporarily bonded laminate.
[0142] Furthermore, the direction of irradiation with ionizing radiation is not limited to the vertical direction described above, and if there is no need to join the entire surfaces of the laminated surface 13 of the cover sheet 11 and the laminated surface 14 of the base sheet 12, an electron beam may be irradiated onto a portion of the surface of the temporarily held laminate. [Industrial Applicability]
[0143] The present invention is suitable for a silicone bonded body which is produced by bonding silicone molded bodies together at a plurality of locations. [Explanation of symbols]
[0144] 1 Silicone joint 2(2a, 2b, 2c) First molded body 3(3a, 3b, 3c) Second molded body 4a~4h contact area 10 Microfluidic Devices 11a, 11b Cover sheet (first molding sheet) 12a, 12b Base sheet (second molding sheet) 13 Lamination surface (first molding surface) 14 Laminated surface (second laminated surface) 15 Microchannel 16 Groove (stress relief section)
Claims
1. A method for simultaneously bonding one or more first molded bodies mainly composed of polyorganosiloxane and one or more second molded bodies mainly composed of polyorganosiloxane or glass, A bonding method characterized by irradiating one or more contact points where the first and second molded bodies are in contact with each other with ionizing radiation consisting of any one of electron beams, gamma rays, and X-rays, and covalently bonding the siloxane main chain of the first molded body and the siloxane main chain of the second molded body at the interface of the contact point by ionizing radiation crosslinking caused by the ionizing radiation.
2. 2. The bonding method according to claim 1, wherein the ionizing radiation is either an electron beam or a gamma ray, and an absorbed dose of the ionizing radiation at the contact point is 860 kGy or more.
3. 2. The bonding method according to claim 1, wherein the ionizing radiation is an electron beam, and an accelerating voltage of the electron beam is 500 keV or more.
4. A first molded sheet; A second molded sheet laminated on the first molded sheet, A microfluidic device in which a first lamination surface of the first molded sheet and a second lamination surface of the second molded sheet that are in contact with each other in a lamination direction are joined together with a microchannel formed therebetween, and the first molded sheet and the second molded sheet are laminated together, The first molded sheet is formed from polyorganosiloxane, The second molded sheet is formed from polyorganosiloxane, glass, or an organic resin having a siloxane coating formed on the second lamination surface, A microfluidic device characterized in that the first and second stacking surfaces, which are in contact in the stacking direction, are exposed to ionizing radiation consisting of any one of electron beams, gamma rays, and X-rays that penetrates the first and second stacking surfaces, and the siloxane main chains of the first and second stacking surfaces are covalently bonded to each other through ionizing radiation crosslinking caused by the ionizing radiation, thereby stacking the first and second molded sheets together.
5. The microfluidic device according to claim 4, characterized in that a stress relaxation portion consisting of a groove or a slit communicating with the side surfaces of the first molded sheet and the second molded sheet which are laminated together is formed on at least one of the first and second laminated surfaces excluding the portion where the microchannel is formed.
6. 6. The microfluidic device according to claim 4, wherein the ionizing radiation is an electron beam.
7. The first molded sheet and the second molded sheet are laminated together, A method for manufacturing a microfluidic device, comprising bonding the first lamination surface and the second lamination surface of the second molded sheet, the first lamination surface and the second lamination surface being bonded together except for a portion where the microchannel is formed, in a state where a microchannel is formed between the first lamination surface of the first molded sheet and the second lamination surface of the second molded sheet, the first lamination surface and the second lamination surface being bonded together except for a portion where the microchannel is formed, the method comprising the steps of: The first molded sheet made of polyorganosiloxane and the second molded sheet made of polyorganosiloxane, glass, or an organic resin having a siloxane coating formed on the second lamination surface are laminated together, The first molded sheet and the second molded sheet are positioned relative to each other, Irradiating the first molded sheet and / or the second molded sheet, which are stacked in relative position, with ionizing radiation consisting of any one of electron beams, gamma rays, and X-rays, and covalently bonding the siloxane main chain of the first stacking surface and the siloxane main chain of the second stacking surface at a contact surface where the first stacking surface and the second stacking surface are in contact with each other through ionizing radiation crosslinking by the ionizing radiation; A method for manufacturing a microfluidic device, comprising bonding the first and second stacking surfaces together except for a portion where the microchannel is to be formed.
8. One or more of the first molded sheets and one or more of the second molded sheets are alternately stacked in multiple stages, All of the first molded sheets and the second molded sheets adjacent to each other in the stacking direction are positioned relative to each other, Irradiating the first molded sheet and / or the second molded sheet, which are stacked in multiple stages while being positioned relative to one another, with the ionizing radiation; The method for producing a microfluidic device according to claim 7 , wherein the first and second stacking surfaces are simultaneously bonded to each other except for a portion where the microchannel is formed.
9. 9. A method for manufacturing a microfluidic device as described in claim 8, characterized in that all of the first molded sheets and the second molded sheets adjacent to each other in the stacking direction are positioned relative to each other so that through holes penetrating the first molded sheet and / or the second molded sheet in the stacking direction are connected to the microchannel formed between the first stacking surface and the second stacking surface.
10. 10. The method for manufacturing a microfluidic device according to claim 7, characterized in that a stress relaxation portion consisting of a groove or a slit communicating with the side surface of the first molded sheet and the second molded sheet which are integrated by joining the first laminated surface and the second laminated surface is formed on at least one of the first laminated surface and the second laminated surface excluding the portion where the microchannel is formed.
11. The method for manufacturing a microfluidic device according to claim 10 , wherein the microchannel and the recessed groove have the same depth from the first layering surface and the same depth from the second layering surface.
12. 10. The method for manufacturing a microfluidic device according to claim 7, wherein the entire surface of the first molded sheet and / or the second molded sheet including the portion where the microchannel is formed is irradiated with the ionizing radiation along the stacking direction.
13. 10. The method for producing a microfluidic device according to claim 7, wherein the ionizing radiation is an electron beam.
Citation Information
Patent Citations
Microchip and its manufacturing method
JP2004325153A
Method for bonding film base material
JP2011136492A
Modular microfluidic assembly block and system including the same
US20100258211A1
Three-dimensional microchemical chip
WO2015098720A1
Microchip manufacturing method
JP2004154898A