Hmpe fiber with improved bending fatigue performance
Multifilament ropes with controlled fiber orientation and specific properties address the durability and bending fatigue issues of existing synthetic ropes, enhancing their performance in heavy lifting applications.
Patent Information
- Application Number
- JP2024128678
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-10-29
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2039-11-04
AI Technical Summary
Existing high-strength synthetic ropes, particularly those made from ultra-high molecular weight polyethylene fibers, face limitations in long-term durability and bending fatigue resistance, especially in industrial heavy lifting applications.
The development of multifilament elongated bodies, such as ropes, using ultra-high molecular weight polyolefin fibers with specific properties including intrinsic viscosity, denier per filament, and toughness, achieved through controlled fiber orientation and processing techniques to enhance bending fatigue resistance.
The resulting ropes exhibit significantly improved bending fatigue resistance and durability, meeting the demands of heavy lifting applications by maintaining structural integrity under repeated bending stress.
Smart Images

Figure 2024156885000001_ABST
Abstract
Description
[Technical field]
[0001] The technology relates to improvements in ropes, and in particular to high tenacity synthetic ropes having improved durability and flexural fatigue performance. [Background technology]
[0002] Synthetic fiber ropes have been used in a variety of applications, including various marine applications. One type of rope with excellent properties is that made from high modulus polyolefin fibers and / or yarns. High tenacity polyolefin fibers, such as SPECTRA® extended chain polyethylene fiber from Honeywell International Inc., are known to be particularly useful in marine applications due to their high strength (15 times stronger than steel by weight), light weight (light enough to float (0.97 g / cc specific gravity)), hydrophobicity, corrosion resistance, excellent resistance to fungal growth, excellent abrasion resistance, excellent flex and flex fatigue performance, low coefficient of friction, and very good resistance to ultraviolet radiation, making them very durable in long term marine applications.
[0003] Fibers formed from ultra-high molecular weight polyethylene (UHMW PE) are known to have excellent tensile properties, such as toughness, tensile modulus, and energy to break, especially with respect to high strength. The term "toughness" refers to the tensile stress expressed as force (grams) per unit linear density (denier) of an unstressed sample as measured by ASTM D2256. The term "initial tensile modulus" refers to the ratio of the change in toughness expressed in grams-force per denier (g / d) to the change in strain expressed as a percentage of the original fiber / tape length (in / in), and as used herein, the terms "initial tensile modulus", "tensile modulus", and "modulus" refer to the modulus of elasticity as measured by ASTM 2256 for a fiber.
[0004] Such high tenacity fibers are typically made by a "gel spinning" process, also known as "solution spinning." In this type of process, a solution of ultra-high molecular weight polyethylene (UHMW PE) and a solvent is formed, followed by extrusion of the solution through a multi-hole spinneret (e.g., with 10-3000 spin holes) to form solution filaments (one filament per spin hole), cooling the solution filaments to gel filaments, and extracting the solvent to form dry filaments. These dry filaments are collected into bundles referred to in the art as "fibers" or "yarns." The fibers / yarns are then stretched (drawn) to their maximum extension limit to increase tenacity.
[0005] The preparation of high strength polyethylene filament and / or multifilament fibers / yarns is described, for example, in U.S. Pat. Nos. 4,413,110, 4,536,536, 4,551,296, 4,663,101, 5,006,390, 5,032,338, 5,578,374, 5,736,244, 5,741,451, 5,958,582, 5,972,498, 6,448, and 6,512,712. Nos. 6,359, 6,746,975, 6,969,553, 7,078,099, 7,344,668, 8,444,898, 8,506,864, 8,747,715, 8,889,049, 9,169,581, 9,365,953, and 9,556,537, all of which are incorporated herein by reference to the extent consistent therewith. Each of these patents teaches incremental improvements in UHMW PE processing technology and describes significant obstacles in improving the tensile properties of UHMW PE fibers. For example, UHMW PE fibers can be stretched only to a certain extent without breaking by drawing the fibers, although the toughness and tensile modulus of the fibers can be increased. The maximum amount that a fiber can be stretched, Thus, the maximum tenacity that can be achieved for a particular fiber type depends on several factors, including both improved raw materials and processing capabilities.
[0006] To increase fiber tenacity, polyethylene solutions and their precursors (i.e., the polymers and solvents that form the solutions) must have certain properties, such as high intrinsic viscosity ("IV"), and must be made in a specific manner. For example, U.S. Pat. No. 8,444,898 teaches a process for producing high tenacity fibers by a special process that limits the time that the fiber-forming polymer / solvent mixture is exposed to extreme processing conditions inside the extruder that degrade the polymer. This process is distinct from other processes that require longer residence times in the extruder, which reduces the maximum achievable fiber tenacity due to the associated polymer degradation in the extruder. U.S. Pat. No. 8,747,715 teaches a process for producing high tenacity polyethylene yarns, in which the fibers are highly oriented to form a product with a tenacity of greater than about 45 g / d and a tensile modulus of greater than about 1400 g / d. This process requires a step to maintain the intrinsic viscosity of the polymer so that fibers with a fiber IV of greater than about 19 dl / g and a tenacity of greater than about 45 g / dg are fabricated. These are just two examples that illustrate the significant scientific and technological efforts that are leading to improvements, even if only incrementally, in the tensile properties of polyethylene fibers.
[0007] Ropes made from high strength polyethylene fibers are known and have been used, for example, in applications requiring good flexural fatigue resistance. See, for example, U.S. Patent Application Publication Nos. 2007 / 0202328 and 2007 / 0202331, both of which are commonly owned by Honeywell International Inc., and which teach ropes that have good flexural fatigue performance when repeatedly bent over sheaves, pulleys, or posts in marine applications. Despite the existing high performance of such ropes, there is a continuing need for products with improved properties and performance. Specifically, there is a continuing need in the art for synthetic ropes that exhibit greater long-term durability when so repeatedly bent over sheaves, especially when used in industrial heavy lifting applications, and there is a need to improve the fatigue life of high performance synthetic ropes. In particular, there is a need to improve the cyclic bend over sheave (CBOS) performance of ropes made from high performance polyolefin fibers and yarns. The present technology provides a method for improving the cyclic bend over sheave (CBOS) performance of ropes made from high performance polyolefin fibers and yarns. This provides a solution to this need in the art.
[0008] In this regard, fiber orientation during the fiber manufacturing process, as conventionally known in the art, is known to increase the toughness of the fiber by exposing the fiber to heat and tension under carefully controlled conditions. In addition to increasing the toughness of the fiber, fiber orientation (i.e., stretching; drawing) also makes the fiber thinner. In a single multifilament fiber containing a combination of smaller filaments, the fiber orientation correspondingly thins each of the individual component filaments forming the fiber. In the textile field, a common measure of fiber / yarn fineness is "denier", a unit of linear density equal to the mass (grams) per 9000 meters of fiber / yarn. In addition to reducing the fiber denier, reducing the denier of the filaments forming the fiber makes the fiber more susceptible to breakage. This reduction in fiber / filament denier also makes the fiber more susceptible to bending fatigue, which is a common problem in applications where elongated bodies such as ropes formed from the fiber typically pass through one or more sheaves. Thus, in the context of the present disclosure, each of the fiber tenacity, fiber denier, and denier per filament are particularly important properties since the fiber is intended for use in the fabrication of ropes for heavy lifting applications, an application that requires substantial fiber strength, resistance to axial breakage, and the ability to withstand bending over time without breakage.
[0009] Such fine particles are useful in applications requiring particularly excellent strength properties and bending fatigue resistance. To produce the elongated bodies, it is necessary to incorporate fibers into the elongated bodies that have a balance of physical properties not currently available in known fibers. Specifically, to achieve the objectives of the present disclosure, a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g as measured in decalin at 135° C. is required. f ), one or more ultra-high molecular weight polyolefin fibers having a combination of a tenacity of at least 32 g / denier, a denier greater than 800, and a denier per filament greater than 2.0, preferably the denier per filament of the filament is greater than the IV of the filament. f is at least 75.0, preferably at least 75.0 to 110.0, and IV fto denier per filament ratios have been found to be from 4.0:1 to 8.0:1. This is accomplished by modifying known fiber / filament manufacturing techniques to fabricate elongated bodies incorporating one or more fibers having these properties and improving the fiber / filament quality. Summary of the Invention
[0010] The present disclosure provides multifilament strips, such as ropes, formed from fibers having an exceptional relationship of intrinsic viscosity, denier per filament, and tenacity, which unexpectedly achieves enhanced flexural fatigue resistance of the strips, fulfilling a need in the art.
[0011] In particular, the present disclosure provides an elongated body including a plurality of fibers, at least one of the fibers having a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g when measured in decalin at 135° C. f ), wherein at least one multifilament ultra-high molecular weight polyolefin fiber has a tenacity of at least 32 g / denier, a denier greater than 800, and a denier per filament greater than 2.0.
[0012] Also, there is provided an elongated body including at least one multifilament fiber including an ultra-high molecular weight polyolefin fiber formed from a plurality of ultra-high molecular weight polyolefin filaments, wherein the ultra-high molecular weight polyolefin filament has a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g when measured in decalin at 135°C. f ), the multifilament ultra-high molecular weight polyolefin fiber having a denier greater than 800, each filament of the multifilament ultra-high molecular weight polyolefin fiber having a denier of at least 2.0, and the denier per filament of the filament is greater than or equal to the IV of the filament. f The elongated body is provided with a product of 75.0 to 110.0.
[0013] There is also provided a method of making an elongated body, comprising the steps of: a) providing a plurality of fibers, at least one of the fibers having a filament intrinsic viscosity (IV) of from 15 dl / g to about 45 dl / g as measured in decalin at 135° C. f ), wherein at least one multifilament ultra high molecular weight polyolefin fiber has a tenacity less than 32 g / denier, a denier greater than 800, and a denier per filament greater than 2.0; b) stretching each multifilament fiber to increase the tenacity of the fiber to at least 32 g / denier, wherein the denier per filament remains greater than 2.0; c) optionally coating at least a portion of each fiber with either a thermoplastic resin or an oil; d) twisting, entangling, or braiding the fibers to form an elongated structure; e) optionally heating and stretching the strip structure to heat set the fibers of the strip. [Brief description of the drawings]
[0014] [Figure 1] 1 illustrates an exemplary post-draw process in which the fiber is drawn unidirectionally through multiple horizontally adjacent ovens. [Diagram 2] 1 illustrates an exemplary post-draw process in which the fiber is drawn by passing it through a single oven in multiple directions. [Diagram 3] 1 is a graph plotting fiber tenacity versus Cogswell extensional viscosity of a 10 wt % solution of UHMW PE polymer in mineral oil at 250° C. for fibers spun from a solution of UHMW PE polymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] As used herein, a "fiber" is an elongated strand of material, such as a strand of polymeric material, whose length dimension is much greater than its transverse dimensions of width and thickness. Fibers are preferably long, continuous strands, rather than short sections of strands referred to in the art as "staple" or "staple fibers." As used herein, the term "elongated" has its ordinary and customary meaning of having a shape that is much longer than it is wide. In the context of this disclosure, an "elongated body" may be a strand that includes a single fiber or includes multiple composite fibers, which may be combined, for example, by twisting, intertwining, braiding, or a combination thereof. An example of an elongated body that includes multiple fibers combined by twisting, intertwining, braiding, or a combination thereof is a rope, such as a braided rope.
[0016] The cross-section of a fiber for use in this disclosure may vary widely, and the fiber may be circular, flat, or elliptical in cross-section. Thus, the term "fiber" includes filaments, ribbons, strips having regular or irregular cross-sections, and the like, although it is preferred that the fiber has a substantially circular cross-section. A "strand" by conventional definition is a single, thin length such as a thread or fiber. A single continuous filament fiber may be formed from only one filament, or may be formed from multiple filaments. Fibers formed from only one filament are referred to herein as either "single filament" fibers, or "monofilament" fibers, and fibers formed from multiple filaments are referred to herein as "multifilament" fibers. Multifilament fibers, as defined herein, preferably contain from 2 to about 3000 filaments, more preferably from 2 to 1000 filaments, even more preferably from 30 to 500 filaments, even more preferably from 40 to 500 filaments, even more preferably from about 40 filaments to about 360 filaments, and most preferably from about 120 to about 240 filaments. Multifilament fibers are also often referred to in the art as filament bundles or bundles of filaments. A group of bundled fibers may also be referred to as a fiber bundle or bundle of fibers. The definition of multifilament fibers herein also encompasses pseudo-monofilament fibers, a term of art that describes multifilament fibers that are at least partially fused together and may appear to be monofilament fibers. As used herein, the term "yarn" is defined as a single continuous strand of multiple fibers or filaments, a term that is often used interchangeably with multifilament fiber.
[0017] A strip comprising, consisting of, or consisting essentially of one or more polyolefin fibers or a combination of polyolefin fibers and non-polyolefin fibers, wherein at least one of the polyolefin fibers forming the strip has a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g when measured in decalin at 135° C.f and at least one of the multifilament ultra-high molecular weight polyolefin fibers has a tenacity of at least 32 g / denier, a denier of greater than 800, and a denier per filament of greater than 2.0. Provided herein is an elongated body having a neal.
[0018] It is generally known that gel / solution spinning of ultra-high molecular weight polyolefins (UHMW PO), particularly ultra-high molecular weight polyethylene (UHMW PE), produces very high performance filaments and fibers with excellent tensile properties. In general, the "gel spinning" process involves forming a solution of spinning solvent and polymer (such as UHMW PE) and passing the solution through a spinneret to form a plurality of solution filaments that are collected to form a fiber (or yarn). These solution filaments are then cooled to form gel filaments. The spinning solvent must then be removed from the gel filaments to form an essentially dry multifilament fiber, which is then oriented (i.e., stretched or drawn) to enhance its tensile properties. It is also known to orient filaments at the solution and gel stages to enhance fiber properties. Generally, higher fiber tensile properties are obtained from polyethylenes with higher intrinsic viscosity. The intrinsic viscosity of a polymer is a measure of the molecular weight of the polymer. It is known that in most solution / gel spinning processes used to form high strength fibers, the polymer undergoes some degradation as it is mixed with the solvent in the extruder and converted into a solution. This degradation results in a slight decrease in molecular weight, and therefore intrinsic viscosity. Thus, in a typical UHMW PE filament / fiber fabrication process, the initial intrinsic viscosity (IV0) of the raw polymer material being spun to form the filament / fiber is IV f which in turn affects the maximum achievable tenacity of fibers formed therefrom.
[0019] Some methods, such as those of U.S. Patent Nos. 7,638,191 and 7,736,561, teach certain processing advantages of intentionally lowering the intrinsic viscosity, while others, such as those of U.S. Patent Nos. 8,444,898, 8,506,864, 8,747,715, 8,889,049, 9,169,581, 9,365,953, and 9,556,537, teach certain benefits of maximizing molecular weight and intrinsic viscosity. Nos. 8,747,715, 9,365,953, and 9,556,537 specifically teach how to make very high tenacity fibers, i.e., fibers having a tenacity of at least 45 g / d, by processing UHMW PE powder feedstock with a very high IV0 of at least 30 dl / g. Nos. 8,444,898 and 8,506,864 teach that molecular weight degradation is minimized by minimizing the time that the UHMW PE polymer feedstock is mixed with the spinning solvent in the extruder. In this regard, the initial steps of a conventional UHMW PE solution / gel spinning process involve (1) processing UHMW PE powder and spin solvent in either an extruder or a combination of an extruder and a heated vessel to form a solution of polymer and spin solvent, (2) passing the solution through a spinneret (as described above) to form a solution fiber comprising a plurality of solution filaments, (3) cooling the solution fiber to form a gel fiber, (4) removing the spin solvent by either extraction or evaporation to form an essentially dry solid fiber, and then (5) stretching at least one of the solution, gel, and dry yarns to form the final multifilament fiber product.
[0020] For purposes of this disclosure, it is understood that the final fiber product has a filament / fiber intrinsic viscosity (IV) of at least 15 dl / g, preferably from 15 dl / g to about 45 dl / g (measured in decalin at 135° C. according to the technique of ASTM D1601). fIt has been found that desirable fiber properties are achieved when the fibers of the present disclosure have an IV of 100 or less when measured in decalin at 135° C. Thus, the fibers of the present disclosure can be fabricated from any conventionally known solution or gel spinning process, provided that the process has an IV of 100 or less when measured in decalin at 135° C. f is at least 15 dl / g, more specifically, IV f The method is improved to minimize the degradation of polymer molecular weight during the fabrication of multifilament ultra-high molecular weight polyolefin fibers, so that the molecular weight of the multifilament ultra-high molecular weight polyolefin fibers is between 15 dl / g and about 45 dl / g. In a preferred embodiment, the filament / fiber fabrication methods of U.S. Patent Nos. 8,444,898, 8,506,864, 8,747,715, 8,889,049, 9,169,581, 9,365,953, and 9,556,537 are most effective in achieving this objective and are therefore most preferred for fabricating the UHMW PE fibers of the present disclosure.
[0021] To form such fibers, steps must be taken to maintain the intrinsic viscosity (IV0) of the UHMW PE polymer (as measured in decalin at 135°C according to ASTM D1601 technique; in dl / g). As described in U.S. Pat. No. 9,169,581, effective steps include, for example, sparging the spinning solvent with nitrogen before mixing with the UHMW PE polymer, or sparging the polymer-solvent mixture and / or polymer-solvent solution with nitrogen gas, thereby reducing or completely eliminating the presence of oxygen, which is known to cause shear-induced chain scission. Nitrogen sparging, especially at temperatures below 290°C, promotes long chain branching rather than chain scission, thus preserving IV0. Nitrogen sparging refers to blowing nitrogen into the solvent / mixture / solution, preferably continuously, such as by continuously blowing nitrogen into a slurry tank that contains the solvent-polymer slurry that is added to the extruder for mixing. Nitrogen sparging in the slurry tank may be performed at a rate of, for example, about 2.4 liters / minute to about 23.6 liters / minute. However, any conventional sparging technique may be used. Other means of reducing or eliminating the presence of oxygen from the polymer-solvent mixture and / or solution during polymer processing, such as the incorporation of an antioxidant into the polymer-solvent mixture and / or solution, should be similarly effective. The use of antioxidants is taught in U.S. Patent No. 7,736,561, commonly owned by Honeywell International Inc. In this embodiment, the concentration of the antioxidant should be sufficient to minimize the effects of adventitious oxygen, but not so high that it reacts with the polymer. The weight ratio of antioxidant to solvent is preferably about 10 parts per million to about 1000 parts per million. Most preferably, the weight ratio of antioxidant to solvent is about 10 parts per million to about 100 parts per million. Useful antioxidants include, non-exclusively, hindered phenols, aromatic phosphites, amines, and mixtures thereof.Preferred antioxidants include 2,6-di-tert-butyl-4-methyl-phenol, tetrakis[methylene(3,5-di-tert-butylhydroxyhydrocinnamate)]methane, tris(2,4-di-tert-butylphenyl)phosphite, octadecyl 3,5-di-tert-butyl-4-hydroxyhydrocinnamate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,5,7,8-tetramethyl-2(4',8',12'-trimethyltridecyl)chroman-6-ol, and mixtures thereof. More preferably, the antioxidant is 2,5,7,8-tetramethyl-2(4',8',12'-trimethyltridecyl)chroman-6-ol, commonly known as vitamin E or α-tocopherol. Optionally, other additives such as processing aids, stabilizers, etc. may be added to the polymer and solvent mixture, as may be desirable to maintain polymer molecular weight and IV0.
[0022] It is also possible to control polymer degradation during the early stages of a conventional gel spinning process (i.e., (1) forming a slurry, (2) heating the slurry to melt the polymer and form a liquid mixture under conditions of intense discrete and dispersive mixing, thereby reducing the domain size of the molten polymer and solvent in the mixture to microscopic dimensions, and (3) allowing time sufficient for the solvent to diffuse into the polymer and the polymer to diffuse into the solvent to form a solution) by controlling the harshness of the environment in which the polymer is processed. For example, to minimize polymer degradation resulting from high heat and the amount of shear on the polymer, which is detrimental to the polymer molecular weight, it is necessary to minimize the residence time of the polymer in the extruder, as described in U.S. Pat. No. 8,444,898. Thus, it is necessary to minimize the residence time of the polymer in the extruder, as described in U.S. Pat. No. 8,444,898, outside the extruder (e.g., It is desirable to begin forming the polymer-solvent liquid mixture by heating the slurry tank (inside the slurry tank) to allow some melt to form in a milder environment. This in turn reduces the polymer residence time in the extruder, thereby reducing thermal and shear degradation of the polymer.
[0023] In addition to increasing the residence time of the polymer in the slurry tank, preferably in a heated slurry tank, lowering the temperature of the extruder helps to produce a solution in a milder environment. For example, the temperature at which the liquid mixture of molten UHMW PE polymer and spinning solvent is formed in the extruder is typically about 140°C to about 320°C. In order to minimize polymer degradation, it is necessary to use a lower temperature in this range. As is known from commonly owned U.S. Pat. No. 8,444,898, the residence time of the mixture in the extruder can also be limited by quickly passing the polymer-solvent mixture from the extruder into a heated vessel (e.g., a heated pipe with or without a static mixer), where the remaining time required for the solvent and polymer to completely diffuse into each other and form a uniform, homogeneous solution is provided. In this regard, operating conditions that can promote the formation of a homogeneous solution include, for example, (1) elevating the temperature of a liquid mixture of UHMW PE and spin solvent to a temperature near or above the melting temperature of UHMW PE, and (2) maintaining the liquid mixture at the elevated temperature for a sufficient time for the spin solvent to diffuse into the UHMW PE and for the UHMW PE to diffuse into the spin solvent. Preferably, the majority of the time required to convert the polymer-solvent slurry to a liquid mixture and then to a homogeneous solution is spent in a heated vessel, and preferably the average residence time of the polymer-solvent mixture in an extruder is about 1.5 minutes or less, more preferably about 1.2 minutes or less, and most preferably about 1.0 minute or less. Heated vessels such as extruders are typically maintained at a temperature of about 140° C. to about 320° C., but without active mixing. The residence time of the liquid mixture in the heated vessel can be from about 2 minutes to about 120 minutes, preferably from about 6 minutes to about 60 minutes, until a solution is formed. Variations of this procedure may also be suitably used. For example, the arrangement and use of the heated vessel and extruder may be reversed, in which case a liquid mixture of UHMW PE and spinning solvent is first formed in the heated vessel and then passed through the extruder to form a solution.
[0024] Further opportunities exist for preserving intrinsic viscosity during post-solution processing. For example, upon exiting the spinneret, the polymer solution passes through a gas space into a liquid quench bath (e.g., water, ethylene glycol, ethanol, isopropanol, preferably maintained at about -35°C to about 35°C) to form gel filaments. If the space contains oxygen, such as when the space is filled with air, the solution filaments are susceptible to oxidation as they pass through this space, minimizing polymer degradation and preserving the IV of the fiber. f To maximize the yield, it may be desirable to fill the gas space with another inert gas, such as nitrogen or argon, to prevent any oxidation. Limiting the length of the gas space also minimizes the possibility of oxidation, especially if filling the gap with an inert gas is not practical. The length of the gas space between the spinneret and the surface of the liquid quench bath is preferably about 0.3 cm to about 10 cm, more preferably about 0.4 cm to about 5 cm. If the residence time of the solution filaments in the gas space is less than about 1 second, the gas space may be filled with air, otherwise it is most preferred to fill the space with an inert gas.
[0025] High IV0 and IV f This can also be achieved by improving the quality of the polymer raw material. For example, it is known that the particle size and particle size distribution of particulate UHMW PE polymer can affect the degree to which the UHMW PE polymer dissolves in the spinning solvent during formation of the gel spun solution, which can affect the ultimate tensile strength capabilities of the fiber. It is desirable for the UHMW PE polymer to dissolve completely in the solution, and therefore it is desirable to produce fiber from UHMW PE polymer having an average particle size of about 100 μm to about 400 μm, most preferably about 100 μm to about 200 μm. Preferably, the fibers are spun and the particles also have a weight average molecular weight of about 300,000 to about 7,000,000, more preferably about 700,000 to about 5,000,000, as described in U.S. Pat. No. 9,169,581. Preferably, the UHMW PE of the present disclosure has a ratio of weight average molecular weight to number average molecular weight (M w / Mn ) is 4 or less, and more preferably M w / M n The ratio is preferably 3 or less, and more preferably M w / M n The ratio is preferably 2 or less, and more preferably M w / M n The ratio is about 1.
[0026] The UHMW PE itself may contain small amounts, generally less than about 5% by weight, preferably less than about 3% by weight, of additives such as antioxidants, heat stabilizers, colorants, flow promoters, solvents, etc. U.S. Patents 8,747,715, 8,889,049, 9,365,953, and 9,556,537 further recognize the importance of a property known as the Cogswell extensional viscosity (λ) of UHMW PE polymer raw materials and its effect on fiber processability and fiber tensile properties, stating that a 10 wt. % solution of UHMW PE polymer in mineral oil at 250° C. has a viscosity of λ≧5,917(IV): 0.8 (where IV refers to IV0).
[0027] Preferred spinning solvents that can be used in forming solution / gel spun fibers from the UHMW PE polymer include hydrocarbons having a boiling point above 100° C. at atmospheric pressure, and preferred spinning solvents can be selected from the group consisting of aliphatic, cycloaliphatic, and aromatic hydrocarbons, and halogenated hydrocarbons such as dichlorobenzene, and mixtures thereof. In some examples, the spinning solvent can have a boiling point of at least about 180° C. at atmospheric pressure. In such examples, the spinning solvent can be selected from the group consisting of halogenated hydrocarbons, mineral oil, decalin, tetralin, naphthalene, xylene, toluene, dodecane, undecane, decane, nonane, octene, cis-decahydronaphthalene, trans-decahydronaphthalene, low molecular weight polyethylene wax, and mixtures thereof. Preferably, the solvent is selected from the group consisting of cis-decahydronaphthalene, trans-decahydronaphthalene, decalin, mineral oil, and mixtures thereof. The most preferred spinning solvent is mineral oil, such as HYDROBRITE® 55O PO white mineral oil, commercially available from Sonneborn, LLC (Mahwah, NJ). HYDROBRITE® 55O PO mineral oil is comprised of about 67.5% paraffinic carbon to about 72.0% paraffinic carbon and about 28.0% to about 32.5% naphthenic carbon, calculated according to ASTM D3238. The slurry, liquid mixture, and solution formed according to the preferred gel / solution spinning process each contain UHMW PE in an amount of about 1% to about 50% by weight of the solution, preferably about 1% to about 30% by weight of the solution, more preferably about 2% to about 20% by weight of the solution, and even more preferably about 3% to about 10% by weight of the solution.
[0028] U.S. Patents 8,444,898 and 8,506,864 teach additional steps that may be taken to minimize the drop in intrinsic viscosity during the fiber spinning process, specifically by first forming a slurry from UHMW PE powder and solvent in an extruder, followed by spinning at a rate of at least 2.0 D / min. 2They teach that polymer degradation can be minimized by processing the slurry through an extruder at an extrusion rate of 100 g / min (g / min; D is the extruder screw diameter in centimeters) to form a liquid mixture, which is then converted to a solution in a heated vessel rather than in an extruder, such that the heated vessel exerts very little, if any, shear stress on the mixture.
[0029] Thus, consistent with the objectives of the present disclosure, at least one or all of the fibers forming the elongated body of the present disclosure have a viscosity in decalin at 135° C. of at least about 21 dl / g, or greater than about 21 dl / g, more preferably from about 21 dl / g to about 100 dl / g, even more preferably from about 30 dl / g to about 100 dl / g, even more preferably from about 35 dl / g to about 100 dl / g, and even more preferably from about 40 dl / g to about 100 dl / g. More preferably, the polymer should be made from a UHMW polyethylene polymer having an intrinsic viscosity of about 40 dl / g to about 100 dl / g, even more preferably about 45 dl / g to about 100 dl / g, and even more preferably about 50 dl / g to about 100 dl / g, all intrinsic viscosity values specified throughout this specification are measured in decalin at 135° C. A high initial IV0 of at least about 21 dl / g should be achieved while allowing for some IV drop, and a high IV0 of 15 dl / g or more should be achieved. f Typically, the IV is from 15 dl / g to about 45 dl / g, or from 30 dl / g to about 45 dl / g, or from 35 dl / g to about 45 dl / g, or from 40 dl / g to about 45 dl / g. f This ensures the production of fibers having
[0030] In addition to describing effective methods for making UHMW PE fibers with an IVf of 15 dl / g or more, many of the above-incorporated US patents also teach methods for drawing fibers during the spinning process. US Patents 8,444,898, 8,506,864, 8,747,715, 8,889,049, 9,365,953, and 9,556,537 specifically teach methods for drawing fibers during the spinning process, as well as post-spinning drawing operations that further increase the toughness of the fibers. Each of these methods of drawing fibers is effective in enhancing the toughness of the fibers, but when the fibers are drawn, the denier and denier per filament (i.e., the denier of each individual filament that forms the multifilament fiber (i.e., the fiber / bundle)) are reduced, making the fibers more susceptible to breakage. Thus, while the spinning and drawing methods described in the above patents may be usefully employed to make one or more UHMW PE fibers of the present disclosure, it is necessary to limit the degree of drawing to ensure a filament denier greater than 2.0 and a total fiber denier greater than 800, preferably at least 1000, and most preferably 1600 or greater, while also achieving a high fiber tenacity of at least 32 g / d.
[0031] This, while limiting the extent of post-drawing operations for such high molecular weight fibers (although drawing of solution and gel fibers may be similarly limited), is achievable when the intrinsic viscosity of the polymer (a measure of polymer molecular weight) is greater than 15 dl / g as the raw material and maintained at greater than 15 dl / g during and after the fiber spinning process. For example, U.S. Patent No. 9,365,953 describes a UHMW PE fiber having a tenacity of at least about 45 g / denier, comprising: a) feeding a slurry containing UHMW PE polymer (supplied as a powder) and a spinning solvent to an extruder to produce a liquid mixture, the UHMW PE polymer having an intrinsic viscosity of at least about 30 dl / g in decalin at 135° C.; a) passing the PE polymer and spin solvent into an extruder to form both a slurry and a liquid mixture within the extruder; b) passing the liquid mixture through a heated vessel to form a homogenous solution of the UHMW PE polymer and the spin solvent; c) feeding the solution from the heated vessel to a spinneret to form a solution fiber; d) drawing the solution fiber exiting the spinneret at a draw ratio of about 1.1:1 to about 30:1 to form a drawn solution fiber; and e) drawing the drawn solution fiber through the UHMW PE polymer. f) drawing the gel fiber in one or more stages at a first draw ratio DR1 of about 1.1:1 to about 30:1; g) drawing the gel fiber at a second draw ratio DR2; h) removing spinning solvent from the gel fiber in a solvent removal unit to form a dry fiber; i) drawing the dry fiber in at least one stage at a third draw ratio DR3 to form a partially oriented fiber; j) passing the partially oriented fiber to a post-drawing operation; and k) drawing the partially oriented fiber in the post-drawing operation at a post-drawing temperature to a fourth draw ratio DR4 of about 1.8:1 to about 15:1 to form a highly oriented fiber product having a tenacity of at least about 45 g / denier.
[0032] Thus, the fibers of U.S. Pat. No. 9,365,953 are subjected to multiple drawing steps. The term "draw ratio" refers to the ratio of the speeds of the draw rolls used during the orientation process. First, the solution fiber flowing out of the spinneret is drawn at a draw ratio of about 1.1:1 to about 30:1. Next, the solidified gel fiber is drawn at two draw ratios, DR1, which is about 1.1:1 to about 30:1, and DR2, which is about 1.5:1 to about 3.5:1. The dried fiber is then drawn at a draw ratio (DR3) of about 1.10:1 to about 3.00:1, and then the dried fiber is subjected to an offline post-draw operation in which the fiber is drawn at a draw ratio (DR4) of about 1.8:1 to about 15:1 to increase the fiber tenacity to 45 g / denier. Each of these drawing steps gradually increases the fiber tenacity while decreasing the fiber denier, so the drawing profile can be customized to limit the increase in tenacity and the decrease in denier in the same way. For example, US Patent No. 9,365,953 indicates that the combined stretch of gel and dry fibers, which can be determined by multiplying DR1, DR2, and DR3 (written as DR1 x DR2 x DR3:1 or (DR1)(DR2)(DR3):1), should be at least about 5:1, more preferably at least about 10:1, and most preferably at least 12:1. In embodiments following a similar stretching process according to US Patent No. 9,365,953, but with limited stretching of solution and gel fibers, the value of DR1 x DR2 x DR3:1 (or (DR1)(DR2)(DR3):1) can be from 1.1:1 to less than 5:1, or from 1.1:1 to 4:1, or from 1.1:1 to 3:1, or from 2:1 to 4:1.
[0033] In a preferred embodiment of the present disclosure, the UHMW PE fibers useful herein are produced according to the method of U.S. Patent No. 9,365,953, but the post-drawing of the fibers is limited to maintain a filament denier greater than 2.0, a total fiber denier greater than 800, preferably at least 1000, preferably 1600 or greater, and a fiber tenacity of at least 32 g / d, preferably from 35 g / d to 45 g / d. This can be accomplished, for example, by conducting a post-drawing operation according to the process disclosed in U.S. Patent No. 9,365,953, but with a post-drawing draw ratio (DR4) of from about 1.1:1 to about 4.5:1, or from about 2.0:1 to about 3.5:1, or from about 2.5:1 to about 2.7:1. Alternatively, the post-draw may be carried out at a draw ratio of about 1.1:1 to 1.7:1, or about 1.1:1 to 1.6:1, or 1.1:1 to 1.5:1, or about 1.1:1 to about 1.4:1, or 1.1:1 to 1.3:1, or 1.1:1 to 1.2:1. Any of these post-draw draw ratio ranges may be limited such that DR1, DR2, and DR3, as defined in U.S. Pat. No. 9,365,953, have a DR1 x DR2 x DR3:1 ratio (or (DR1)(DR2)(DR3):1 ratio) of from 1.1:1 to less than 5:1, or from 1.1:1 to 4:1, or from 1.1:1 to 3:1, or from 2:1 to 4:1, such that after drawing / stretching of all fibers is complete, such fibers (multifilament fibers) have a denier per filament (dpf) in the range of from about 2.0 dpf to about 7.0 dpf, more preferably from about 2.3 dpf to about 6.0 dpf, more preferably from about 2.5 dpf to about 5.0 dpf, and most preferably from about 3.0 dpf to about 5.0 dpf, and a filament intrinsic viscosity (IV) of from 15 dl / g to about 45 dl / g as measured in decalin at 135° C. f), and a tenacity of at least 32 g / denier; according to a preferred embodiment of the present disclosure, the strip / rope of the present disclosure comprises at least one multifilament polyolefin fiber having all of the above properties, also having a denier of greater than 800, i.e., the at least one multifilament polyolefin fiber is fabricated to include at least enough component filaments such that the combined deniers of all the component filaments forming the fiber have a denier of greater than 800. Fibers formed from filaments having deniers within these ranges, and the other above properties of intrinsic viscosity and tenacity, are stretched to a degree significantly less than their maximum drawability, the fibers having an elongation to break of about 4.0% or less, typically about 3.0% to 4.0%, as measured according to the test method of ASTM D638.
[0034] In this regard, methods for drawing fibers are conventionally known in the art and are described in US Pat. Any suitable method may be used, including those of Patents 6,969,553, 7,370,395, 7,344,668, 8,747,715, 9,365,953, and 9,556,537, each of which is incorporated herein by reference to the extent consistent therewith. Generally, post-drawing of dry fibers is accomplished in at least one step by passing the continuous fibers through a heated environment provided by a heating device, such as a forced air convection oven, at a post-drawing temperature of about 125°C to about 160°C. Drawing may be performed in one or more passes through the oven, and drawing is initiated once the fiber reaches the desired temperature within the ranges described above. Exemplary post-drawing devices are shown in Figures 1 and 2. As shown in FIG. 1, the post-drawing process 200 is performed by passing a continuous fiber 208 through a heating device 202 having a first set of rolls 204 external to the heating device 202 and a second set of rolls 206 external to the heating device 202. The fiber 208 may be fed from a source and passed through the first set of rolls 204. The first set of rolls 204 may be driven rolls that are operated to rotate at a desired speed to provide the fiber to the heating device 202 at a desired feed rate of V1 meters / min. The first set of rolls 204 may include a plurality of individual rolls 210. In one example, the first few individual rolls 210 are unheated and the remaining individual rolls 210 are heated to preheat the fiber 208 before entering the heating device 202. The first set of rolls 204 includes a total of seven individual rolls 210 as shown in FIG. 1, although the number of individual rolls 210 may be more or less depending on the desired configuration.
[0035] As shown in the figure, the fiber 208 may be fed into a heating device 202 that includes one or more ovens. As shown, the one or more ovens may be adjacent horizontal ovens. Each oven is preferably a forced convection air oven. Because it is desirable to have effective heat transfer between the fiber 208 and the air within the oven, air circulation within each oven is preferably turbulent, and the time-averaged air velocity within each oven in the vicinity of the fiber 208 is preferably from about 1 meter / minute to about 200 meters / minute. In the illustrated example, six adjacent horizontal ovens 212, 214, 216, 218, 220, and 222 are shown, although any suitable number of ovens may be utilized. The heating device may be of any suitable fiber path length, and each oven may have any suitable length to provide the desired fiber path length. For example, each oven may be from about 10 feet to about 16 feet (3.05 meters to 4.88 meters) in length. The temperature and velocity of the fiber 208 passing through the heating device 202 may be varied as desired. The path of the fiber 208 in the heating device 202 may be approximately linear, and the tenacity profile of the fiber 208 during the post-drawing process may be adjusted by adjusting the speed of the various rolls or by adjusting the temperature profile of the heating device 202. Preferably, the tension of the fiber 208 in the heating device 202 is approximately constant or increases through the heating device 202. The heated fiber 224 may exit the final oven 222 and then pass through a second set of rolls 206 to form a final fiber product 226. The second set of rolls 206 may be driven rolls that are operated to rotate at a desired speed to remove the heated fiber 222 from the heating device 202 at a desired exit speed of V2 meters / min. The second set of rolls 206 may include multiple individual rolls 228. The second set of rolls 206 includes a total of seven individual rolls 228 as shown in FIG. 1, although the number of individual rolls 228 may be more or less depending on the desired configuration.Additionally, the number of individual rolls 228 in the second set of rolls 206 may be the same as or different from the number of individual rolls 210 in the first set of rolls 204. Preferably, the second set of rolls 206 may be cooled such that the final textile product 226 is cooled to a temperature of at least about 90° C. under tension to retain its orientation and configuration.
[0036] An alternative heating device 300 is shown in FIG. 2. As shown, the heating device 300 includes a single The heating apparatus 300 may include one or more ovens, such as a bun 304. Each oven is preferably a forced convection air oven having the same conditions as the oven of FIG. 1. The ovens 304 may have any suitable length, and in one example may be about 10 feet to about 20 feet (3.05 to 6.10 meters) long. The ovens 304 may include one or more intermediate rolls 302 that can redirect the fiber 208 passing through the oven 304 to increase the travel path of the fiber 208 through the heating apparatus 300. Each of the one or more intermediate rolls 302 may be a fixed roll that does not rotate, a driven roll that rotates at a predetermined speed, or an idler roll that can rotate freely as the fiber 208 passes through it. In addition, each of the one or more intermediate rolls 302 may be located inside the oven 304 as shown, or the one or more intermediate rolls 302 may be located outside the oven 304. Utilizing one or more intermediate rolls 302 increases the effective length of the heating apparatus 300. Any suitable number of intermediate rolls can be utilized to provide the desired total yarn path length. The final textile product 306 then exits the oven, or the textile product 306 may be further drawn with additional external rolls similar to those illustrated in Figure 1. In either embodiment, the variable speed of the first set of rolls (e.g., speed of the feed rolls, V1 (meters / min)) and the variable speed of the second set of rolls (e.g., speed of the exit rolls, V2 (meters / min)) determine the draw ratios at each stage of the drawing process (e.g., solution fiber draws, DR1, DR2, DR3, and DR4), which reduces the denier of each filament of the drawn fiber.
[0037] By fabricating fibers from high IV0 UHMW PE polymers and taking steps to maintain the polymer intrinsic viscosity during the spinning process as described above, such as sparging the solvent, solvent-UHMWPE polymer mixture, and / or solvent-UHMWPE polymer solution with nitrogen, drawing of the fibers according to any of the above conditions can be limited to maintain a filament denier of at least 2.0 while also achieving a fiber tenacity of 32 g / denier to 45 g / d. Such fibers have a preferred post-draw denier per filament (dpf) in the range of about 2.0 dpf to about 7.0 dpf, more preferably about 2.3 dpf to about 6.0 dpf, more preferably about 2.5 dpf to about 5.0 dpf, and most preferably about 3.0 dpf to about 5.0 dpf. Fibers formed from filaments having deniers within these ranges are maximally elongated to have an elongation at break of about 4.0% or less, typically about 3.0% to 4.0%, according to the test method of ASTM D638.
[0038] Once suitable fibers are fabricated, they may be formed into ropes or other multi-filament structures according to conventional methods in the art, where multiple fibers are combined, for example, by twisting, braiding, entangling, or a combination of these techniques, or by other conventionally known techniques for bonding multiple fibers. In this regard, the ropes of the present disclosure may be of any suitable construction, such as braided ropes, twisted ropes, wire-lay ropes, parallel core ropes, etc. In one embodiment of the present disclosure, the strip consists of or consists essentially of braided, twisted, or entangled polyolefin fibers, or more preferably braided, twisted, or entangled polyethylene fibers. In another embodiment, one or more core fibers may be further incorporated to form the strip, with the braid surrounding the core fibers as a sheath.
[0039] Core-sheath braided structures are well known in the art for both rope applications. Suitable core fibers include, non-exclusively, any stretchable synthetic, recycled or metal fibers, and may optionally include ceramic or glass fibers. Particularly suitable core fibers are stretchable thermoplastic fibers, including polyolefin fibers, polyester fibers, and fluoroplastic fibers. In forming the core-sheath rope structures herein, Herzog Maschinenfabrik The braiding may be performed using conventional equipment, such as a braiding machine available from GE Healthcare GmbH (Oldenberg, Germany), and may involve plaiting or other braiding structures, as well as the core "fibers." The braid may be formed around the core using any conventional method known in the art, such as a double braid technique, where the core is itself a braided structure. In this embodiment, preferably between 2 and 100 separate fibers for small diameter ropes, or thousands of separate fibers, e.g., 5000 to 6000 or more separate fibers, for large diameter ropes, are incorporated into the braided sheath structure.
[0040] In the core-sheath structure, the braided fibers and the core are optionally fused. Fusing the braided fibers with the core is typically accomplished by applying heat and tension, and optionally applying a solvent or plasticizing material before exposure to heat and tension, as described in U.S. Patent Nos. 5,540,990, 5,749,214, and 6,148,597, the disclosures of which are incorporated herein by reference to the extent consistent therewith. As described in these patents, the braid is subjected to elongation at an elevated temperature within the melting point range of the filament polymer material for a time sufficient to soften the filaments and at least partially fuse the contact surfaces of the individual filaments forming the fiber into a line with monofilament-like characteristics.
[0041] Fusing can also be achieved by bonding, for example, at least partially coating the sheath and / or core fibers with a thermoplastic resin or other polymer binder material having adhesive properties. Suitable thermoplastic resins non-exclusively include polyolefin resins, such as polyolefin waxes, low density polyethylene, linear low density polyethylene, polyolefin copolymers, ethylene copolymers, such as ethylene-acrylic acid copolymers, ethylene-ethyl acrylate copolymers, ethylene-vinyl acetate copolymers, polyisoprene-polystyrene block copolymers (such as KRATON® D1107 available from Kraton Polymers, Houston, TX), polyurethanes, polyvinylidene fluoride, polychlorotetrafluoroethylene (PCTFE), and copolymers and blends of one or more of the foregoing. Suitable polyolefin waxes non-exclusively include ACumist® micronized polyolefin wax available from Honeywell International Inc., Morristown, NJ. The most preferred thermoplastic resins are materials that have a melting point lower than the particular polyolefin fiber utilized and are stretchable, most preferably polyolefin resins. The braid sheath fibers may also be thermally bonded to each other and / or to the core fiber without an adhesive coating. The thermal bonding conditions depend on the type of fiber. The fibers may also be pre-coated with an oil, such as mineral oil, paraffin oil, or vegetable oil, prior to fusing, as conventionally known in the art, for example, as described in U.S. Pat. Nos. 5,540,990, 5,749,214, and 6,148,597. As described in the above patents, the mineral oil acts as a plasticizer, improving the efficiency of the fusing process and allowing it to be carried out at lower temperatures. The fibers may be coated with the oil or thermoplastic resin using any conventional method, such as dipping, spraying, or otherwise passing the fibers through a bath of the coating material.
[0042] When the sheath and / or core fibers are coated with a resin or other polymeric binder material having adhesive properties to bind the fibers together, only a small amount of resin / binder is required. In this regard, the amount of resin / binder applied is typically 5% or less by weight based on the total weight of the fibers + resin / binder, such that the fibers comprise at least 95% by weight of coated fibers based on the total weight of the fibers + resin / binder. Thus, the elongated body comprises at least 95% by weight of the constituent fibers. In more preferred embodiments, the elongated body comprises at least about 96% by weight of fibers, even more preferably 97% by weight of fibers, even more preferably 98% by weight of fibers, even more preferably 99% by weight of fibers. Most preferably, the elongated body is completely resin-free, i.e., not coated with any binding resin / binder, and consists essentially of fibers / filaments or Or consisting of:
[0043] In the most preferred embodiment herein, the elongate body consists of or essentially consists of a braid without incorporating a core fiber, so that the braid is essentially a braided rope of any diameter that does not contain any unbraided fibers or strands. The braid is preferably circular, has a circular, annular, or elliptical cross section rather than flat, and can be formed using any conventionally known braiding technique as determined by one skilled in the art, such as plating, single braid, solid braid, or hollow braid techniques. These braids, which do not have a core fiber, are made with conventional braiding equipment and methods. Suitable braiding devices are commercially available, for example, from Herzog Maschinenfabrik GmbH (Oldenberg, Germany). For example, in forming the braided rope, a conventional braiding machine with multiple bobbins can be used. As known in the art, as the bobbins move around, the fibers thread over and under each other and are eventually collected on a take-up reel. The details of the braiding machine and the formation of the rope therefrom are known in the art and will not be disclosed in detail herein.
[0044] Preferably, the braid is formed from a plurality of fibers, and at least one of the fibers has a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g when measured in decalin at 135°C. f A braided body comprising multifilament ultra high molecular weight polyolefin fibers having a tenacity of at least 32 g / denier, a denier greater than 800, and a denier per filament greater than 2.0 incorporates 2-100 separate fibers, more preferably 3-40, even more preferably 3-20 separate fibers, and even more preferably 3-15 separate fibers. However, as noted above, depending on the desired diameter of the rope, more than 100 separate fibers may be incorporated, potentially including several thousand separate fibers, for example about 5000-6000 or more separate fibers, depending on the denier per fiber and the desired end use. The fiber diameter can be calculated from the denier of the fiber using the following formula:
[0045]
number
[0046] where density is grams per cubic centimeter (g / cm 3) (g / cc) and diameter in mm. Ultra-high molecular weight polyethylene has a density of 0.97 g / cc, but as known to those skilled in the art, at very high molecular weights, this can increase to about 0.98 g / cc to about 0.995 g / cc. Generally, a lower fiber denier corresponds to a smaller fiber diameter. In a preferred embodiment herein, the at least one multifilament fiber forming the elongated body (e.g., braided rope) has a denier of about 800 to about 5000 denier, more preferably about 800 to about 4000 denier, even more preferably about 800 to about 3000 denier, even more preferably about 800 to about 1600 denier, even more preferably about 900 denier or more, even more preferably 900 to about 3000 denier, even more preferably about 900 to about 1600 denier, even more preferably about 1000 denier or more, even more preferably about 1000 to about 1600.
[0047] The overall denier of the strip / rope depends on the number of multifilament fibers combined to form the strip / rope, which generally depends on the end use requirements of the rope. The strip itself, incorporating at least two separate fibers, e.g., a core fiber, Braids having 3 to 12 separate fibers that do not have any fibers have preferred deniers of 1500 denier or more, more preferably greater than 2300 denier, even more preferably greater than 2300 to about 5000 denier, more preferably greater than 2500 denier, even more preferably greater than 2500 to about 5000 denier, more preferably greater than 3000 denier, even more preferably greater than 3000 to about 5000 denier. Due to the braid structure in which the fibers are inverted over one another at the intersections (i.e., picks), the braid denier is typically greater than the total denier of all the component fibers, since 9000 meters of braid incorporates more than 9000 meters of each individual fiber. In this regard, preferred ropes have a denier of at least 1500 denier, preferably 1500 to about 30,000 denier, more preferably about 1600 denier or more, more preferably about 1600 to about 26,000 denier, even more preferably about 8,000 to about 26,000. Most preferred ropes have from about 3 to about 50 individual fibers, preferably from about 10 to about 20 individual fibers, preferably each individual fiber having a denier greater than 800, preferably about 900 denier or greater, even more preferably about 1000 denier or greater, even more preferably about 1100 denier or greater, even more preferably about 1200 denier or greater, even more preferably about 1300 denier or greater, even more preferably about 1400 denier or greater, even more preferably about 1500 denier or greater, even more preferably about 1600 denier or greater, even more preferably about 1700 denier or greater, even more preferably about 1800 denier or greater, even more preferably about 1900 or greater, and even more preferably each individual fiber has a denier of about 2000 or greater, and at least 3 to about 20 individual fibers, more preferably about 3 to about 15, and most preferably about 5 to about 13 individual fibers are incorporated into the rope (e.g., braid). The fineness of the rope depends on the required breaking strength and / or other properties dictated by the desired end use.
[0048] Also, any range stated using specific minimum and maximum endpoints is intended to cover any range within those endpoints not expressly stated herein that is also within the scope of the invention.
[0049] Optionally, the fibers forming the single braid, solid braid, or hollow body may be fused together according to the above-mentioned techniques of U.S. Patent Nos. 5,540,990, 5,749,214, and 6,148,597, in which heat and tension are applied to fuse the individual fibers forming the braid together. When this option is implemented, the braid is optionally subjected to elongation at an elevated temperature within the melting point range of the filament polymer material sufficient to at least partially fuse the contact surfaces of the individual filaments forming the fiber into a line with monofilament-like characteristics. Useful conditions for the elongation / surface fusion process are the same as those listed above for core-sheath fibers. As described above for the core / sheath structure, the fibers forming the non-core / sheath braid may also be at least partially coated with either a thermoplastic resin or oil and then fused together as described above, and such coatings may be applied either before or after the fibers are twisted, entangled, or braided to form the braided / twisted / entangled structure. Suitable thermoplastic resins, waxes, and oils are the same as those described above. However, in the most preferred embodiment, the fibers forming the braid are not fused to one another, i.e., non-fused. This is in distinction to the methods of U.S. Patent Nos. 5,540,990, 5,749,214, and 6,148,597, which fuse the fibers to one another.
[0050] After the braid is formed, it may or may not be stretched. Stretching may be performed with or without heating the fibers / braid, but heating is preferred. As described herein, stretching the braid refers to stretching after the fibers are braided into a braid; even in a non-stretched braid, the component fibers forming the braid have already been stretched during the gel / solution spinning process described above prior to braiding. If it is desired to stretch the braid with heat but not fuse the component fibers of the braid, the braid may be stretched at a temperature below the melting point of the fibers. Fusion is avoided by heating to about 145°C. For example, when incorporating ultra-high molecular weight gel-spun polyethylene multifilament fibers in the braid, this temperature is preferably in the range of about 145°C to about 153°C, more preferably about 148°C to about 151°C. In this regard, it is noted that highly oriented ultra-high molecular weight polyethylene fibers generally have a higher melting point than bulk UHMW PE or lower molecular weight polyethylene. During this stretching without fusion process, the fibers are preferably held under tension, which is preferably continuously applied. Preferably, the stretching step without fusion is carried out with an overall stretch ratio of about 1.01 to about 3.0, more preferably about 1.1 to about 1.8, in one or more stages of stretching, preferably with the addition of heat.
[0051] The braids of the present disclosure have what is also known in the art as braid tightness. The braid may have any desired braid density. The angle that the braided components make with respect to the braid axis is referred to as the braid angle. The braid density may be adjusted using selected devices, as desired, to increase or decrease the braid angle along the length of the braid. In preferred embodiments, the braid has a braid angle of less than about 40°, or between about 5° and about 40°, more preferably the braid angle is 30° or less, or between about 5° and about 30°, and most preferably between about 15° and about 30°. Each of these ranges is specific to the braid density / tightness of the unstretched braid, i.e., the braid after braiding of the braid but before any optional additional stretching.
[0052] Multifilament fibers may optionally be twisted or air entangled prior to braiding. Various methods of twisting fibers are known in the art, and any method may be utilized. Useful twisting methods are described, for example, in U.S. Pat. Nos. 2,961,010, 3,434,275, 4,123,893, 4,819,458, and 7,127,879, the disclosures of which are incorporated herein by reference to the extent consistent herewith. In a preferred embodiment, the fibers are twisted to have an angle of 5° to about 40°, more preferably about 5° to about 30°, and most preferably about 15° to about 30° relative to the twisted bundle axis. A standard method for determining the twist in twisted fibers is ASTM D1423. Similarly, various methods of air entangling multifilament fibers are known in the art and are described, for example, in U.S. Patent Nos. 3,983,609, 4,125,922, and 4,188,692, the disclosures of which are incorporated herein by reference to the extent consistent therewith. In a preferred embodiment, the multifilament fibers are neither twisted nor air entangled, and the individual fibers themselves are preferably not braided prior to braiding a plurality of fibers together to form a braid.
[0053] Although the most preferred embodiment braided body includes only multifilament polyethylene fibers having a tenacity of at least 32 g / denier, the braided body may further include other polyolefin or polyethylene fibers having different tenacities, including, for example, any of the fibers disclosed in U.S. Pat. Nos. 4,411,854; 4,413,110; 4,422,993; 4,430,383; 4,436,689; 4,455,273; 4,536,536; 4,545,950; 4,551,296; 4,584,347; 4,663,101; 5,248,471; and 5,311,282. , No. 578,374, No. 5,736,244, No. 5,741,451, No. 5,972,498, No. 6,448,359, No. 6,969,553 , No. 7,078,097, No. 7,078,099, No. 7,081,297, No. 7,115,318, No. 7,344,668, No. 7,638, Nos. 191, 7,674,409, 7,736,561, 7,846,363, 8,070,998, 8,361,366, 8,444,898, 8,506,864, and 8,747,715, each of which is incorporated herein by reference to the extent consistent herewith. All polyolefin fiber types, including polypropylene fibers, high density polyethylene, and low density polyethylene fibers, may also be included as component fibers, such as aramid fibers, particularly para-aramid and meta-aramid fibers, polyamide fibers, polyester fibers, including polyethylene terephthalate and polyethylene naphthalate fibers, extended chain polyvinyl alcohol fibers, extended chain polyacrylonitrile fibers, polybenzoazole fibers, such as polybenzoxazole (PBO) and polybenzothiazole (PBT) fibers, polytetrafluoroethylene fibers, carbon fibers, graphite fibers, silicon carbide fibers, boron carbide fibers, glass fibers, recycled fibers, metal fibers, ceramic fibers, graphite fibers, liquid crystal copolyester fibers, and other rigid rod fibers, such as M5® fibers, as well as fibers formed from copolymers, block polymers, and blends of the above materials. However, not all of these fiber types are suitable for use in embodiments in which the braid is stretched.
[0054] It should also be understood that all references herein to the term "ultra-high" with respect to the molecular weight of the polyolefins or polyethylenes of the present disclosure are also not intended to be limiting at the maximum end of polymer viscosity and / or polymer molecular weight. The term "ultra-high" is only intended to limit at the minimum end of polymer intrinsic viscosity and / or polymer molecular weight to the extent that useful polymers within the scope of the present disclosure can be processed into fibers having the desired properties described herein. It should also be understood that the process described herein is most preferably applied to the processing of UHMW polyethylene, but is equally applicable to all other poly(α-olefins), i.e., UHMW PO polymers.
[0055] The elongated bodies of the present disclosure may be useful in a variety of end uses such as suspension lines, water ski ropes, climbing ropes, yacht ropes, parachute lines, fishing nets, mooring lines, hawsers, shoe laces, medical applications such as catheters or dental floss, high pressure tubing, ground cables, and harnesses, but are particularly useful in applications requiring improved cyclic bending over sheave (CBOS) fatigue resistance as described above, including marine applications such as lifting and mooring heavy loads from the ocean floor.
[0056] CBOS resistance can be tested, for example, by bending a rope of the present disclosure about 180 degrees on a free-running sheave or pulley. The rope is placed under load and cycled on the sheave until the rope reaches failure. In an exemplary test, the rope is bent over a 38 mm diameter sheave / pulley with a D:d ratio (D=sheave / pulley diameter, d=rope diameter) of 20 at 56 cycles / min and a 156 kg load on the sheave / pulley (78 kg tension on each side of the rope). The number of cycles to failure is typically averaged and determined, for example, based on an average of 3-5 tests.
[0057] Filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g (measured in decalin at 135°C) f A multifilament elongated body (rope) comprising a plurality of multifilament ultra-high molecular weight polyolefin fibers having a tenacity of at least 32 g / denier, a denier of greater than 800, each of the filaments having a denier (dpf) of at least 2.0, and an IV f The ratio of (dl / g) to dpf (IV f Particularly good CBOS fatigue resistance has been achieved for multifilament strips (ropes) having a dpf of IV to 4.0:1, including all narrower ranges between the above endpoints, such as 4.1 to 7.5 and 4.2 to 7.0. f (dl / g) multiplied by the product (IV f It is most preferred that the "IV × dpf" is at least 75.0, and more preferably, the dpf plus IVf The product of these values I is at least 75.0 to 110.0, including all narrower ranges between the above endpoints, such as 80.0 to 105.0, or 85.0 to 100.0, or 88.0 to 95.0. The most preferred polyolefin fiber types have a fiber length of at least 100 mm and a fiber length of at least 150 mm. V f ×dpf and IV f In one exemplary embodiment, each multifilament fiber of the elongated body has a denier of about 1600 and contains 480 filaments (i.e., dpf 3.33), and the filaments have an IV of about 22.6 dl / g to about 26.5 dl / g. f Thus, in this exemplary embodiment, a multifilament elongate body is formed having an IV f ×dpf value is in the range of 75.3 to 88.2, IV f The / dpf value ranges from 6.79 to 7.96.
[0058] Also, at least one polyolefin fiber in the rope is IV f ×dpf (i.e., at least 75.0 to 110.0) and / or IV f :dpf ratio(IV f It is within the scope of this disclosure that a multifilament strip (rope) may include one or more highly oriented polyolefin multifilament fibers having a tenacity of 45 g / d or greater, e.g., 45 g / denier to about 60 g / denier, so long as the multifilament strip meets the above characteristics of dpf (i.e., 4.0:1 to 8.0:1), although the component fibers of such a multifilament fiber do not necessarily have a dpf of 2.0 or greater or a denier of 800 or greater.
[0059] The following non-limiting examples serve to illustrate preferred embodiments.
[0060] Example 1 The spinning solvent and UHMW PE polymer were mixed to form a slurry inside a slurry tank heated to 100°C. The UHMW PE polymer had an intrinsic viscosity IV0 of about 30 dl / g. A solution was formed from the slurry by heating to at least the melting point of the UHMW PE polymer. The polymer concentration in the slurry was about 7%. After forming a homogeneous spinning solution, the solution was spun through a 360-hole spinneret to form a multifilament solution fiber. The spinneret holes had a diameter of about 1 mm and a length / diameter (L / D) ratio of 15:1. The solution fiber was then passed through a 1.5 inch (3.8 cm) long air gap and placed in a water quench bath with a water temperature of about 10°C to form a gel fiber. The solution fiber was stretched in the 1.5 inch air gap with a draw ratio of about 1.5:1, and the gel yarn was cold stretched on a set of rolls with a draw ratio of 5.5:1 before entering a solvent removal device. In the solvent removal apparatus, the solvent was extracted with the extraction solvent and the gel fiber was stretched at a stretch ratio of about 1.4:1. Fiber IV of 20 dl / g f The resulting dry fibers having a tenacity of about 24.5 g / denier were then drawn through multiple roller sets to form a partially oriented fiber having a tenacity of about 24.5 g / denier. The partially oriented fiber was then drawn at about 150° C. in a 22 meter oven with a fiber feed speed of about 12 meters / min and an uptake speed of about 31 meters / min to form a highly oriented fiber having a tenacity of greater than about 32 g / d, the fiber having a denier of 1600 and a denier per filament (dpf) of 4.4, and an IV of the fiber. f remained at 20 dl / g.
[0061] Twelve of these highly oriented fibers were then braided together according to conventional braiding techniques to form a rope having a denier of approximately 20,000.
[0062] Example 2 and Comparative Examples 1 to 4 Five identical braided structures with a length:diameter (L:D) ratio of 10:1 were formed by braiding together 12 ultra-high molecular weight polyethylene fibers having the properties listed in Tables 1 and 2 below. No coating was applied to either the component fibers or the braid. The number of bending cycles to failure was determined by continuously cycling the braid at 56 bending cycles per minute on a 38 mm sheave with a load of 78 kg applied to each end of the sample.
[0063] [Table 1]
[0064] [Table 2]
[0065] As shown by the CBOS tests, braids formed from the novel fibers had substantially improved abrasion resistance and durability compared to other fiber types, especially those that did not meet the recited requirements for IV:dpf ratio and IV x dpf product values.
[0066] While the present disclosure has been particularly shown and described with reference to preferred embodiments, it will be readily understood by those skilled in the art that various changes and modifications may be made therein without departing from the spirit and scope of the present disclosure. It is intended that the claims be construed to cover the disclosed embodiments, their alternatives as described above, and all equivalents thereof.
Claims
1. 1. An elongated body comprising a plurality of fibers, at least one of the fibers having a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g as measured in decalin at 135° C. f ), wherein at least one multifilament ultra high molecular weight polyolefin fiber has a tenacity of at least 32 g / denier, a denier greater than 800, and a denier per filament greater than 2.
0.
2. All of the fibers forming the elongated body have an IV of 15 dl / g to about 45 dl / g as measured in decalin at 135° C. f 2. The elongated body of claim 1, comprising a multifilament ultra high molecular weight polyolefin fiber having a tenacity of at least 32 g / denier, a denier of 900 or greater, and a denier per filament greater than 2.
0.
3. The elongated body of claim 1 , wherein all of the fibers forming the elongated body are polyethylene fibers.
4. The elongated body of claim 1 , wherein the plurality of fibers are twisted together, braided together, or a combination thereof.
5. IV f 2. The elongated body of claim 1, wherein the ratio of fiber length to denier per filament is from 4.0:1 to 8.0:
1.
6. 1. An elongated body comprising at least one multifilament fiber comprising an ultra-high molecular weight polyolefin fiber formed from a plurality of ultra-high molecular weight polyolefin filaments, wherein the ultra-high molecular weight polyolefin fiber has a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g as measured in decalin at 135° C. f), the multifilament ultra-high molecular weight polyolefin fiber having a denier greater than 800, each filament of the multifilament ultra-high molecular weight polyolefin fiber having a denier of at least 2.0, and the denier per filament of the filament is greater than the IV of the filament. f A slender body having a product of 75.0 to 110.
0.
7. IV in denier per filament f The elongated body according to claim 6, wherein the product of said multiplication is between 85.0 and 110.
0.
8. IV f 7. The body of claim 6, wherein the ratio of fiber to denier per filament is from 4.0:1 to 8.0:
1.
9. IV f to denier per filament is from 4.0:1 to 8.0:1, and said denier per filament is f 7. The elongated body of claim 6, wherein the product of x, y, and z is at least 75.0, all of the fibers forming the elongated body have a denier of at least 900, the elongated body has a denier of at least 2300, and the plurality of multifilament fibers are combined in a twisted structure, a braided structure, or a combination thereof.
10. 1. A method of making an elongated body, comprising the steps of: a) providing a plurality of fibers, at least one of the fibers having a filament intrinsic viscosity (IV) of 15 dl / g to about 45 dl / g as measured in decalin at 135° C. f ), wherein at least one multifilament ultra-high molecular weight polyolefin fiber has a denier of 32 g / denier; providing a woven fiber having a tenacity of less than 1.0, a denier greater than 800, and a denier per filament greater than 2.0; b) stretching each multifilament fiber to increase the tenacity of said fiber to at least 32 g / denier, wherein said denier per filament remains greater than 2.0; c) optionally coating at least a portion of each fiber with either a thermoplastic resin or an oil; d) twisting, intertwining, or braiding the fibers to form a strip structure; e) optionally heating and stretching the strip structure to heat set the fibers of the strip.
Citation Information
Patent Citations
High-toughness, high-modulus UHMWPE fiber and method for manufacturing the same
JP2015508849A