Photosensitive composition and use thereof
The photosensitive composition with conductive particles and silicone resin addresses the issue of cracking and resistance in conductive films during high-temperature firing, ensuring stable and low-resistance conductor films.
Patent Information
- Application Number
- JP2024133757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conductive films experience increased volume and risk of cracking during high-temperature firing, leading to decreased conductivity and performance issues.
A photosensitive composition containing conductive particles, a photopolymerizable compound, and a silicone resin with specific formula (I) is used, with the silicone resin present at 0.05% to 1.0% of the total weight of conductive particles, to suppress reverse expansion and reduce resistance.
The composition effectively prevents cracking and reduces resistance in conductive films during high-temperature firing, enabling stable formation of thin, high-quality conductor films.
Smart Images

Figure 2024156966000008 
Figure 2024156966000009 
Figure 2024156966000010
Abstract
Description
[Technical field]
[0001] The present disclosure relates to photosensitive compositions and their uses. [Background technology]
[0002] For example, electronic materials such as multilayer chip inductors include a circuit board in which a conductor film (wiring conductor) of a predetermined pattern is formed on a substrate. For example, Patent Document 1 discloses a conductive composition containing a partial hydrolysis condensate of tetraalkoxysilane from the viewpoint of obtaining a conductor film with high heat resistance.
[0003] On the other hand, in recent years, there has been a demand for further thinning of the conductor film, and a method (typically a photolithography method) of producing a conductor film by utilizing a photochemical action using a composition containing a photopolymerizable compound and conductive particles (hereinafter referred to as a "photosensitive composition") is preferably used. In this method, a photosensitive composition prepared in advance is first applied to a substrate and dried. Next, the applied composition is exposed to light and cured (reacted). At this time, a wiring circuit of a desired pattern can be drawn by controlling the exposed area using a photomask or the like. Thereafter, the uncured part shielded by the photomask is removed by washing with a developer. Finally, the substrate is baked at a predetermined temperature to produce (baked) the cured part, i.e., a patterned photocured film, on the surface of the substrate. According to this method, a conductor film of a fine pattern can be produced relatively easily on the substrate. For example, Patent Document 2 discloses a photosensitive composition suitable for such an application. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4965232 [Patent Document 2] Patent No. 4660991 Summary of the Invention [Problem to be solved by the invention]
[0005] Meanwhile, according to the study by the present inventors, for example, when the photosensitive composition as described above is fired at a high temperature (for example, about 800°C to 900°C), it has been found that the higher the firing temperature, the larger the volume of the resulting conductor film (hereinafter, such a phenomenon is also simply referred to as "inverted expansion"). In such a case, the conductivity of the conductor film may decrease, or cracks may occur in the conductor film during firing, which is undesirable from the viewpoint of the performance of electronic materials. In addition, there is a demand for further reducing the resistance of such conductor films.
[0006] The present disclosure has been made in view of the above circumstances, and a main object of the present disclosure is to provide a photosensitive composition that can suitably suppress inversion expansion of a conductor film, for example, during high-temperature firing, and can suitably realize low resistance of the conductor film and prevention of cracks. Another object is to provide such a conductor film and an electronic material including the conductor film. [Means for solving the problem]
[0007] In order to achieve this object, the present disclosure provides a photosensitive composition comprising conductive particles, a photopolymerizable compound, and a silicone resin, the silicone resin being represented by the following formula (I): [ka] (R in formula I 1 ~R 6 are each independently an alkyl group, a phenyl group, a polyether group, an aralkyl group, a fluoroalkyl group, a fatty acid ester group, or a group into which a fatty acid amide group has been inserted. Also, m and n are each independently an integer of 0 or more. and the silicone resin is contained in an amount of 0.05% to 1.0% when the total weight of the conductive particles is taken as 100%. Although details will be described later, a photosensitive composition containing the silicone resin represented by the above formula (I) within the above range can suitably suppress inversion expansion of a conductive film during high-temperature firing, for example, and can suitably realize low resistance of the conductive film and prevention of cracks.
[0008] In addition, suitable examples of the silicone resin include polydimethylsiloxane, poly(methylphenylsiloxane), and side-chain polyether-modified polysiloxane. In the embodiment in which these types of silicone resins are used as the silicone resin, the above-mentioned effects can be more suitably obtained.
[0009] In a preferred embodiment of the photosensitive composition disclosed herein, the weight average molecular weight of the silicone resin is 1,000 to 100,000. In an embodiment in which a silicone resin having a weight average molecular weight within the above range is used as the silicone resin, the above-mentioned effects can be more suitably obtained.
[0010] In a preferred embodiment of the photosensitive composition disclosed herein, the conductive particles have an average particle size of 1 μm to 5 μm. In an embodiment using conductive particles having an average particle size of 1 μm to 5 μm, in addition to the above-mentioned effects, thinning of the conductor film can be more suitably achieved.
[0011] In a preferred embodiment of the photosensitive composition disclosed herein, the conductive particles have a lightness L* of at least 50 in the L*a*b color system based on JIS Z 8781. In an embodiment containing conductive particles having a lightness L* of at least 50, the irradiated light can stably reach deep inside the conductive film before curing, so that the conductive film can be formed more stably.
[0012] The photosensitive compositions disclosed herein can be used, for example, to form electrodes on ceramic green sheets.
[0013] The photosensitive composition disclosed herein can be used to form fine lines with a line width of, for example, 30 μm or less.
[0014] From another aspect, there is provided a conductor film made of a sintered body of any of the photosensitive compositions disclosed herein. Furthermore, there is provided an electronic material having a conductor film made of a sintered body of any of the photosensitive compositions disclosed herein. Such an electronic material can be said to be a high-quality electronic material because it has a conductor film in which inversion expansion during high-temperature sintering is suitably suppressed and low resistance is suitably achieved, for example. [Brief description of the drawings]
[0015] [Figure 1] 1 is a cross-sectional view showing a schematic structure of an electronic material (multilayer chip inductor) according to one embodiment. [Diagram 2] 11A to 11C are explanatory views for explaining a method for manufacturing an electronic material (multilayer chip inductor) according to another embodiment. [Diagram 3] 13 is an SEM image showing the electrode surface at the time of firing at 900° C. according to Example 14 of the Test Example. [Figure 4] 1 is a SEM image showing an electrode surface at the time of firing at 900° C. according to Example 3 of the Test Example. [Diagram 5] 1 is a SEM image showing the electrode surface at the time of firing at 900° C. according to Example 4 of the Test Example. [Figure 6] 1 is a SEM image showing an electrode surface at the time of firing at 900° C. according to Example 6 of the Test Example. [Figure 7] 1 is a SEM image showing an electrode surface at the time of firing at 900° C. according to Example 8 of the Test Example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] A preferred embodiment of the present disclosure will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the present disclosure can be understood as design matters for a person skilled in the art based on the conventional technology in the field. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The following embodiments are not intended to limit the technology disclosed herein to such embodiments. In the following drawings, dimensional relationships (length, width, thickness, etc.) do not reflect actual dimensional relationships, and do not limit the present disclosure unless otherwise specified. In this specification and claims, when a certain numerical range is described as A to B (A and B are arbitrary numerical values), it means A or more and B or less. Therefore, it includes the case where it is greater than A and less than B.
[0017] In addition, when the term "conductive particles" is used, it means a group of many fine particles (i.e., particles), except when referring to a single particle. In Japanese, it is unclear whether to use the singular or plural form, so the above definition is used to clarify the meaning of "conductive particles." In addition, in this specification, the term "paste" is a concept that includes a slurry-like composition and an ink-like composition.
[0018] ≪Photosensitive composition≫ The photosensitive composition disclosed herein includes conductive particles, a photopolymerizable compound, and a silicone resin. The silicone resin is represented by the following formula (I): [ka] (R in formula I 1 ~R 6 are each independently a group having an alkyl group, a phenyl group, a polyether group, an aralkyl group, a fluoroalkyl group, a fatty acid ester group, or a fatty acid amide group inserted therein. m and n are each independently an integer of 0 or more.) The silicone resin is contained in an amount of 0.05% to 1.0% when the total weight of the conductive particles is taken as 100%.
[0019] As a result of intensive research by the present inventors, it was found that the silicone resin functions as a sintering aid for the conductive particles when the conductive particles sinter and grow together during high-temperature firing at, for example, 800°C to 900°C. In addition, when a silicone resin having low compatibility (in other words, low reactivity) with resins such as the photopolymerizable resins listed above is used, the silicone resin functions favorably as a sintering aid for the conductive particles because the contact opportunity with the conductive particles increases. Furthermore, as a result of further examining various blending ratios of the conductive particles and the silicone resin, it was found that the silicone resin is preferably contained at a ratio of 0.05% to 1.0% when the total weight of the conductive particles is taken as 100% from the viewpoint of favorably obtaining the above-mentioned effects. That is, it was found that a photosensitive composition containing the silicone resin represented by the above formula (I) within the above range can favorably realize low resistance and prevention of cracks in the obtained conductor film because the conductive particles are sintered together in a dense state with few voids during high-temperature firing. In addition, it was also found that, with this configuration, as the firing temperature increases, sintering and grain growth between conductive particles progresses, so that the inversion expansion of the resulting conductor film is suitably suppressed. Note that the above explanation is the inventor's consideration based on experimental results, and the technology disclosed herein should not be interpreted as being limited to the above mechanism. Each component will be described in detail below.
[0020] <Conductive particles> The photosensitive composition disclosed herein contains conductive particles. The conductive particles are materials for mainly forming layers with high electrical conductivity (hereinafter simply referred to as "conductivity") such as electrodes, conductors, and conductive films in electronic materials. The type of conductive particles is not particularly limited, and one or more types of conductive particles may be used in appropriate combination from among conventionally known conductive particles. Examples of the types of conductive particles include simple noble metals such as silver (Ag), platinum (Pt), gold (Au), palladium (Pd), rhodium (Rh), iridium (Ir), ruthenium (Ru), and osmium (Os), simple base metals such as nickel (Ni), aluminum (Al), copper (Cu), tungsten (W), and molybdenum (Mo), carbonaceous materials such as carbon black, and mixtures and alloys thereof. Among these, silver (silver particles) can be preferably used from the viewpoint of suitably obtaining an electronic material having a dense and low-resistance conductive film. Examples of the alloy include silver-palladium (Ag-Pd) alloy, silver-platinum (Ag-Pt) alloy, and silver-copper (Ag-Cu) alloy. Core-shell particles, in which the core is made of the above-mentioned metal and the core is covered by a shell, can also be used. The conductive particles described above can be, for example, commercially available ones.
[0021] The average particle diameter of the conductive particles is not particularly limited as long as the effect of the technique disclosed herein can be obtained. The lower limit of the average particle diameter of the conductive particles is, for example, 0.1 μm or more, and from the viewpoint of suitably suppressing aggregation between the conductive particles, it is preferably 0.5 μm or more, and more preferably 1 μm or more. The upper limit of the average particle diameter of the conductive particles is, for example, 10 μm or less, and from the viewpoint of suitably realizing thinning of the conductor film, it is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 2 μm or less. The average particle diameter of the conductive particles is preferably, for example, within the range of 1 μm to 5 μm. The "average particle diameter" of the conductive particles means a particle diameter (D50 particle diameter) corresponding to 50% of the cumulative value from the small particle diameter side in the volume-based particle size distribution based on the laser diffraction and scattering method. Such a measurement can be performed, for example, using a commercially available device, Microtrack MT3000II manufactured by Microtrack Bell Co., Ltd.
[0022] Although not particularly limited, the entire conductive particles may have a lightness L* of 50 or more in the L*a*b* color system based on JIS Z 8781:2013. This allows the irradiated light to reach the deep part of the conductive film before curing stably, and a thick conductive film, for example, a film thickness of 5 μm or more, or even 10 μm or more, can be stably realized. From the above viewpoint, the lightness L* of the conductive particles may be approximately 55 or more, for example, 60 or more. The lightness L* can be adjusted, for example, by the type and average particle diameter of the conductive particles. The lightness L* can be measured, for example, by a spectrophotometer conforming to JIS Z 8722:2009.
[0023] Although not particularly limited, the ratio of the conductive particles in the entire photosensitive composition (in other words, the ratio of the conductive particles when the entire photosensitive composition is taken as 100% by weight) is preferably about 50% by weight or more, typically 60 to 95% by weight, for example 70 to 90% by weight. By satisfying the above range, a conductive film excellent in density and electrical conductivity can be formed. In addition, the handleability of the photosensitive composition and the workability when forming the conductive film can be improved.
[0024] <Photopolymerization compound> The photosensitive composition disclosed herein includes a photopolymerizable compound. The photopolymerizable compound is a photocurable component that undergoes a polymerization reaction, a crosslinking reaction, or the like, and hardens due to an active species generated by decomposition of a photopolymerization initiator, which will be described later. The polymerization reaction may be, for example, addition polymerization or ring-opening polymerization. The photopolymerizable compound is not particularly limited, and one or more types may be appropriately selected from conventionally known compounds according to, for example, the purpose and the type of substrate. The photopolymerizable compound typically has one or more unsaturated bonds and / or cyclic structures. Suitable examples of the photopolymerizable compound include radically polymerizable compounds having one or more ethylenically unsaturated bonds, such as (meth)acryloyl groups and vinyl groups, and cationic polymerizable compounds having a cyclic structure, such as epoxy groups. In this specification and claims, the term "photopolymerizable compound" includes photopolymerizable polymers, photopolymerizable oligomers, and photopolymerizable monomers.
[0025] The photosensitive composition disclosed herein may contain a photopolymerizable polymer as a photopolymerizable compound. Compared with monomers and oligomers, photopolymerizable polymers can be cured with a relatively small amount of exposure. Therefore, it is possible to stably cure deep parts of the exposed part (parts close to the substrate). Therefore, by containing a photopolymerizable polymer, the adhesion between the substrate and the conductive film is increased, and defects such as peeling and disconnection of the conductive film can be suitably suppressed. In addition, the water resistance and durability of the conductive film can be improved. In addition, when the photopolymerizable compound contains a photopolymerizable polymer, the adhesion (tackiness) to the substrate is increased, and the removability of the unexposed part in the development process is reduced. The weight average molecular weight of the photopolymerizable polymer is generally larger than 5,000, typically 10,000 or more, for example 15,000 or more, 20,000 or more, and may be generally 100,000 or less, for example 50,000 or less. It is preferable that the photopolymerizable compound further contains at least one of a photopolymerizable monomer and a photopolymerizable oligomer in addition to the photopolymerizable polymer. Although not particularly limited, the weight average molecular weight of the photopolymerizable monomer can be, for example, less than about 500, and the weight average molecular weight of the photopolymerizable oligomer can be, for example, about 500 to 5000. In this specification and claims, the "weight average molecular weight" refers to the weight-based average molecular weight measured by gel permeation chromatography (GPC) and converted using a standard polystyrene calibration curve.
[0026] In a preferred embodiment, the photopolymerizable compound contains a (meth)acrylate having a (meth)acryloyl group. For example, the photopolymerizable compound may contain a (meth)acrylate polymer as the photopolymerizable polymer, may contain a (meth)acrylate monomer as the photopolymerizable monomer, or may contain a (meth)acrylate oligomer as the photopolymerizable oligomer. When the photopolymerizable compound contains a (meth)acrylate, the flexibility of the conductor film and its conformity to the substrate can be improved. As a result, the occurrence of defects such as peeling and disconnection can be better suppressed. As a preferred example of the (meth)acrylate polymer, there can be mentioned a homopolymer of an alkyl (meth)acrylate, or a copolymer containing an alkyl (meth)acrylate as a main monomer and a sub-monomer having copolymerizability with the main monomer. In this specification, "(meth)acryloyl" includes "methacryloyl" and "acryloyl", and "(meth)acrylate" includes "methacrylate" and "acrylate".
[0027] In another preferred embodiment, the photopolymerizable compound contains a photopolymerizable compound (a urethane bond-containing compound) having a urethane bond (-NH-C(=O)-O-). For example, the photopolymerizable compound may contain a urethane bond-containing polymer having a urethane bond as the photopolymerizable polymer, may contain a urethane bond-containing monomer having a urethane bond as the photopolymerizable monomer, or may contain a urethane bond-containing oligomer having a urethane bond as the photopolymerizable oligomer. When the photopolymerizable compound contains a urethane bond-containing compound, the etching resistance of the exposed portion can be improved and a conductive film having even better flexibility and stretchability can be realized. Therefore, the adhesion between the substrate and the conductive film can be improved, and the occurrence of defects such as peeling and disconnection can be suppressed to a high level. Preferred examples of the urethane bond-containing compound include urethane-modified (meth)acrylate, urethane-modified epoxy, and polyfunctional urethane (meth)acrylate. In addition, as the (meth)acrylate-containing compound and the urethane bond-containing compound as described above, commercially available compounds can be used without any particular restrictions.
[0028] Although not particularly limited, when the photopolymerizable compound contains a photopolymerizable polymer, the ratio of the photopolymerizable polymer in the entire photopolymerizable compound may be approximately 10% by weight or more, typically 20% by weight or more, for example 30% by weight or more, and approximately 90% by weight or less, typically 80% by weight or less, for example 70% by weight or less, on a weight basis. When the above range is satisfied, the effect of the technology disclosed herein is exerted at a high level. Furthermore, although not particularly limited, when the photopolymerizable compound contains at least one of a photopolymerizable monomer and a photopolymerizable oligomer, the ratio of the photopolymerizable monomer and / or the photopolymerizable oligomer in the entire photopolymerizable compound may be approximately 10% by weight or more, typically 20% by weight or more, for example 50% by weight or more, and approximately 90% by weight or less, typically 80% by weight or less, for example 70% by weight or less, on a weight basis.
[0029] Although not particularly limited, the ratio of the photopolymerizable compound in the entire photosensitive composition may be about 0.1 to 20% by weight, typically 0.5 to 10% by weight, for example, 1 to 5% by weight. Although not particularly limited, the content ratio of the photopolymerizable compound may be about 0.1 to 20 parts by weight, for example, 0.5 to 10 parts by weight, relative to 100 parts by weight of the conductive particles. By satisfying the above range, the photocurability of the photosensitive composition is suitably exhibited, and a conductive film can be formed stably at a high level.
[0030] <Silicone resin> The photosensitive composition disclosed herein contains a silicone resin represented by the following formula (I): 1 ~R 6 are independent of each other and each represents a group having an alkyl group, a phenyl group, a polyether group, an aralkyl group, a fluoroalkyl group, a fatty acid ester group, or a fatty acid amide group inserted therein. m and n each represent an integer of 0 or more, independent of each other. The photosensitive composition disclosed herein may contain one or more silicone resins represented by the following formula (I). As the silicone resin, one having a main skeleton based on a siloxane bond (Si-O-Si) can be preferably used.
[0031] [ka]
[0032] Here, the alkyl group may be linear or branched. Although not particularly limited, the number of carbon atoms in the alkyl group is, for example, 1 to 12, preferably 1 to 6, and more preferably 1 to 3. In addition, although not particularly limited, a polyether group (typically, -R(C2H4O) a (C3H6O) bR'. a and b are integers of 0 or more, each being independent of the other. In the formula (a), a+b may be, for example, 1≦a+b≦80, 2≦a+b≦70, 3≦a+b≦60, or 5≦a+b≦50. The carbon number of R and R' may be, for example, 1 to 12, or 1 to 6 or 1 to 3. The carbon numbers of R and R' may be the same or different. Although not particularly limited, in a fatty acid ester group (typically represented as -OCOR), the carbon number of R may be, for example, 1 to 12, or 1 to 6 or 1 to 3. Although not particularly limited, in a fatty acid amide group (typically represented as -RNHCOR'), the carbon number of R and R' may be, for example, 1 to 12, or 1 to 6 or 1 to 3. The carbon numbers of R and R' may be the same or different. In the formula (b), a and b are integers of 0 or more, each being independent of the other ... 1 ~R 6 The combination may be, for example, a combination of a polyether group, an alkyl group, and an aralkyl group, or a combination of an alkyl group and an aralkyl group.
[0033] Examples of the silicone resin include polydimethylsiloxane; poly(methylphenylsiloxane) (specifically, R 1 ,R 3 ,R 5 ,R 6 is a methyl group, R 2 ,R 4 is a phenyl group), poly(dimethylsiloxane-co-diphenylsiloxane) (more specifically, 1 ,R 2 ,R 5 ,R 6 is a methyl group, R 3 ,R 4 is a phenyl group), poly(dimethylsiloxane-co-methylphenylsiloxane) (more specifically, 1 ,R 2 ,R 3 ,R 5 ,R 6 is a methyl group, R 4side-chain phenyl-modified polysiloxanes such as polysiloxanes in which R in the above formula (I) is a phenyl group; side-chain polyether-modified polysiloxanes such as polysiloxanes in which R in the above formula (I) is a phenyl group; 5 ,R 6 is a methyl group, R 1 ,R 2 ,R 3 and R 4 at least one of R in the above formula (I) is substituted with a polyether group), 5 ,R 6 is a methyl group, R 1 ,R 2 ,R 3 and R 4 at least one of R in the above formula (I) is substituted with a fluoroalkyl group), 5 ,R 6 is a methyl group, R 1 ,R 2 ,R 3 and R 4 at least one of R in the above formula (I) is substituted with a fatty acid ester group), side-chain fatty acid amide-modified polysiloxane, etc. 5 ,R 6 is a methyl group, R 1 ,R 2 ,R 3 and R 4 at least one of R 1 ,R 2 ,R 3 ,R 4 is a methyl group, R 5 and R 6 or the like is substituted with a polyether group. The non-substituted end may be, for example, a substituent other than a polyether group among the above-listed substituents.); or a siloxane modified with polyether at both ends (more specifically, 1 ,R 2 ,R 3 ,R 4 is a methyl group, R 5and R 6 substituted with a polyether group). Among them, from the viewpoint of more suitably realizing the suppression of the inversion expansion and the reduction of the resistance of the conductor film, polydimethylsiloxane, poly(methylphenylsiloxane), and side chain polyether modified polysiloxane can be preferably used. As described above, m and n in the above formula (I) represent integers that are independent of each other and are 0 or more. m and n may be the same or different from each other. Although not particularly limited, m+m may be, for example, 1≦m+n≦2000, 1≦m+n≦1500, or 1≦m+n≦1000. As the above silicone resin, for example, one that is not photocurable can be more preferably used. As the above silicone resin, commercially available ones can be used without any particular restrictions. As the silicone resin, for example, one manufactured by Shin-Etsu Chemical Co., Ltd., Dow-Toray Co., Ltd., BYK-Chemie, and Asahi Kasei Corporation can be used.
[0034] The weight average molecular weight of the silicone resin is not particularly limited as long as the effect of the technology disclosed herein is exhibited. The lower limit of the weight average molecular weight of the silicone resin is, for example, 500 or more, and from the viewpoint of suitably realizing the suppression of inversion expansion and low resistance of the conductor film, it is preferably 1000 or more, and may be 5000 or more. The upper limit of the weight average molecular weight of the silicone resin is, for example, 200,000 or less, and from the viewpoint of suitably obtaining the above-mentioned effects, it is preferably 100,000 or less, and may be, for example, 90,000 or less (less than 90,000), 50,000 or less, or 10,000 or less. The weight average molecular weight of the silicone resin is preferably, for example, within a range of 1,000 to 100,000. In addition to the above effects, from the viewpoint of resolution, it is preferably, for example, within a range of 1,000 to 10,000. In addition, from the viewpoint of increasing compatibility with the conductive particles and functioning suitably as a sintering aid for the conductive particles, the silicone resin is preferably liquid or oily, for example, at room temperature (about 20±5° C.) and at 1 atmospheric pressure. The silicone resin is preferably a liquid or oily composition that is uniformly dispersed or dissolved in the photosensitive composition.When the silicone resin is liquid or oily, it is preferred because it is easily compatible with conductive particles.In addition, among silicone resins, for example, those that are mainly composed of a straight chain structure with 2000 or less siloxane bonds are preferably used because they are oily.
[0035] In the photosensitive composition disclosed herein, the silicone resin is contained in an amount of 0.05% to 1.0% when the total weight of the conductive particles is taken as 100%. By containing the silicone resin within the above range, it is possible to preferably suppress the inversion expansion of the obtained conductor film and reduce the resistance. In addition, from the viewpoint of more preferably obtaining the above-mentioned effects, the silicone resin may be in the range of 0.1% to 1.0% when the total weight of the conductive particles is taken as 100%, more preferably in the range of 0.15% to 1.0%, more preferably in the range of 0.15% to 0.8%, and even more preferably in the range of 0.15% to 0.6% when the total weight of the conductive particles is taken as 100%. In addition to the above-mentioned effects, from the viewpoint of preferably obtaining resolution, the silicone resin is preferably in the range of 0.05% to 0.8% when the total weight of the conductive particles is taken as 100%.
[0036] <Organic binder> The photosensitive composition disclosed herein may contain an organic binder in addition to the above components. The organic binder is a component that enhances the adhesion between the substrate and the film-like body (uncured material) before photocuring. As the organic binder, one or more types can be appropriately selected and used from conventionally known ones depending on, for example, the type of substrate and the type of photopolymerizable compound. As the organic binder, one that can be easily removed with an aqueous developer in the development process is preferable. For example, when an alkaline aqueous developer is used in the development process, an alkali-soluble resin or the like can be preferably used. This makes it easier to remove the unexposed part in the development process.
[0037] The alkali-soluble resin may have a structural portion with high alkali solubility, for example, an acidic group (acidic functional group) such as a phenolic hydroxyl group, a carboxyl group, a sulfo group, a phosphono group, or a boronic acid group. Among them, a carboxyl group is preferable. The acidic group is a substituent that has a dissociable proton and shows acidity in water. The acidic group may be partially esterified. The acidic group may be bonded to a carbon atom in the main chain (a carbon chain with the maximum number of carbon atoms; the same applies below) of the alkali-soluble resin, or may be bonded to a carbon atom in a side chain (a carbon chain branched from the main chain; the same applies below). By including a structural portion with high alkali solubility, the unexposed portion can be more quickly and easily removed without leaving any residue with an alkaline aqueous developer.
[0038] In a preferred embodiment, the alkali-soluble resin has an acid value. The acid value of the alkali-soluble resin is, for example, 10 mgKOH / g or more, preferably 20 mgKOH / g or more, more preferably 25 mgKOH / g or more, for example 30 mgKOH / g or more, and is typically smaller than the (meth)acrylic photocurable resin described later, and is approximately 150 mgKOH / g or less, preferably 100 mgKOH / g or less, for example 50 mgKOH / g or less. It is more preferable that the acid value of the entire organic binder is in the above range. In other words, it is preferable that the entire organic binder exhibits a predetermined acidity. When the acid value is a predetermined value or more, the removability of the unexposed part in the development process is enhanced, and the developability can be improved. In addition, when the acid value is a predetermined value or less, the solubility in the aqueous developer is suppressed, and peeling and disconnection of the exposed part in the development process can be suppressed better. Therefore, the effect of the technology disclosed herein can be exhibited at a higher level. In this specification, the term "acid value" refers to the amount (mg) of potassium hydroxide (KOH) required to neutralize the free fatty acids contained in a unit sample (1 g), expressed in mgKOH / g.
[0039] Suitable examples of the organic binder include cellulose-based resins such as methyl cellulose, ethyl cellulose, carboxymethyl cellulose, and hydroxymethyl cellulose, (meth)acrylic resins, phenolic resins, alkyd resins, polyvinyl alcohol, and polyvinyl butyral. Among them, cellulose-based resins and acrylic resins can be preferably used from the viewpoint of easy removal in the development process. As described above, these resins preferably have an acidic group, and the acid value is preferably within the above range. In addition, the weight average molecular weight of the organic binder is not particularly limited as long as the effect of the technology disclosed herein is exhibited, but is generally 5,000 to 500,000, and can be within the range of, for example, 7,000 to 200,000 or 10,000 to 150,000. In addition, as the organic binder as described above, commercially available ones can be used without any particular limitation.
[0040] When the photosensitive composition contains an organic binder, the proportion of the organic binder in the entire photosensitive composition is not particularly limited, but may be approximately 0.1 to 20% by weight, typically 0.5 to 10% by weight, for example 1 to 5% by weight.
[0041] <Dispersion medium> The photosensitive composition disclosed herein may contain, in addition to the above components, a dispersion medium (e.g., an organic dispersion medium) for dispersing these components. The dispersion medium is a component that imparts appropriate viscosity and fluidity to the photosensitive composition, thereby improving the handleability of the photosensitive composition and improving the workability when forming a conductor film. From the viewpoint of improving the workability when forming a conductor film, it is preferable that the photosensitive composition is prepared in a paste form using the dispersion medium. As the dispersion medium, one or more types can be appropriately selected and used from conventionally known ones depending on, for example, the type of photopolymerizable compound.
[0042] Suitable examples of the dispersion medium include alcohol-based solvents such as terpineol, dihydroterpineol, texanol, 3-methyl-3-methoxybutanol, and benzyl alcohol; glycol-based solvents such as ethylene glycol, propylene glycol, and diethylene glycol; ether-based solvents such as dipropylene glycol methyl ether, methyl cellosolve (ethylene glycol monomethyl ether), cellosolve (ethylene glycol monoethyl ether), ethylene glycol monobutyl ether, and butyl carbitol (diethylene glycol monobutyl ether); ester-based solvents such as diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, dipropylene glycol methyl ether acetate, butyl glycol acetate, butyl diglycol acetate, butyl cellosolve acetate, butyl carbitol acetate (diethylene glycol monobutyl ether acetate), and isobornyl acetate; hydrocarbon-based solvents such as toluene, xylene, naphtha, and petroleum-based hydrocarbons; and mineral spirits. As the dispersion medium as described above, commercially available ones can be used without any particular limitation.
[0043] Among these, from the viewpoint of improving the storage stability of the photosensitive composition and the handleability during the formation of the conductive film, organic solvents having a boiling point of 150° C. or higher, and more preferably 170° C. or higher, are preferred. As another preferred example, from the viewpoint of keeping the drying temperature low after printing the conductive film, organic solvents having a boiling point of 250° C. or lower, and more preferably 220° C. or lower, are preferred. This can improve productivity and reduce production costs.
[0044] When the photosensitive composition contains a dispersion medium, the ratio of the dispersion medium to the entire photosensitive composition may be about 1 to 50% by weight, typically 3 to 30% by weight, for example 5 to 20% by weight, although it is not particularly limited. When the photosensitive composition is prepared in a paste form containing a dispersion medium, the viscosity of the paste is not particularly limited, but is preferably about 10 to 100 mPa·s (for example, about 20 to 70 Pa·s). Such a viscosity can be measured, for example, by a commercially available viscometer.
[0045] <Photopolymerization initiator> The photosensitive composition disclosed herein may contain a photopolymerization initiator in addition to the above components. As the photopolymerization initiator, one or more types can be appropriately selected from conventionally known ones depending on the type of photosensitive resin, etc., and used. The photopolymerization initiator is a component that decomposes when irradiated with active energy rays such as visible light, ultraviolet light, and electron beams, generates active species such as radicals and cations, and initiates the reaction of the photopolymerizable compound. Suitable examples include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,4-diethylthioxanthone, benzophenone, and the like. As the photopolymerization initiator as described above, commercially available ones can be used without any particular restrictions.
[0046] Although not particularly limited, the ratio of the photopolymerization initiator in the entire photosensitive composition is preferably about 0.01 to 5% by weight, typically 0.1 to 4% by weight, for example, 0.2 to 3% by weight or 0.3 to 2% by weight, which allows the photocuring property of the photosensitive composition to be suitably exhibited, and allows the conductive film to be formed more stably.
[0047] <Other added ingredients> The photosensitive composition disclosed herein may further contain various additive components as necessary in addition to the above components, so long as the effect of the technology disclosed herein is not significantly impaired. As the additive components, one or more of conventionally known ones may be appropriately selected and used. Examples of the additive components include inorganic fillers such as silica (SiO2) and alumina (Al2O3), glass particles, photosensitizers, polymerization inhibitors, radical scavengers, antioxidants, ultraviolet absorbers, dispersants (e.g., anionic dispersants, cationic dispersants, nonionic dispersants, etc.), plasticizers, surfactants, leveling agents, thickeners, defoamers, gelling inhibitors, stabilizers, preservatives, pigments, etc. Although not particularly limited, the ratio of the additive components to the entire photosensitive composition is generally 5% by weight or less, typically 3% by weight or less, for example 2% by weight or less, and preferably 1% by weight or less.
[0048] The photosensitive composition disclosed herein can be used, for example, to form an electrode on a ceramic green sheet (see <<Uses of the Photosensitive Composition>> described later). One example of such a ceramic green sheet is a ceramic green sheet made of borosilicate glass. In addition, such a ceramic sheet may contain ceramic particles such as alumina or silica as appropriate from the viewpoint of improving heat resistance, etc.
[0049] The photosensitive composition disclosed herein can be used to form fine lines with a line width (in other words, line L) of 30 μm or less. Furthermore, a conductive film with a space S of 30 μm or less can be formed. In this case, the film thickness is not particularly limited, but is generally 10 μm or less, and preferably 8 μm or less.
[0050] In addition, according to the photosensitive composition disclosed herein, the difference BA (%) between the disk shrinkage A (%) when fired at 800°C and the disk shrinkage B (%) when fired at 900°C can be adjusted to BA≧-0.5. Here, the "disk shrinkage" is a parameter indicating the shrinkage of the conductor film, and is a value that can be calculated, for example, by the method described in the test example described later. Here, the volume of the conductor film made of the photosensitive composition can be equal to or reduced as the temperature increases from room temperature (for example, about 25°C) to a certain temperature (for example, about 800°C) due to resin burnout and sintering of the photosensitive composition. On the other hand, in a photosensitive composition having a relatively high resin content of 5% by weight or more, or even 7% by weight or more, the volume of the conductor film when fired at about 900°C may be larger than the volume of the conductor film when fired at about 800°C (i.e., the shrinkage rate may be smaller). This is undesirable because it may cause the conductivity of the conductive film to decrease, or may cause a shrinkage difference between the conductive film and the substrate (e.g., green sheet) which tends to shrink as the firing temperature increases, resulting in peeling of the conductive film from the substrate or cracking. In contrast, the photosensitive composition disclosed herein can suitably suppress such inverted expansion, and thus can solve the above-mentioned problems. The more positive the BA, the higher the firing temperature, and it is preferable that BA>0, and more preferably BA≧0.5 (e.g., BA>0.5). The upper limit of the BA is not particularly limited as long as the effect of the technology disclosed herein can be obtained, but may be, for example, BA≦20, or BA≦10.
[0051] <Uses of the photosensitive composition> According to the photosensitive composition disclosed herein, a fine-line conductor film can be stably formed. Therefore, the photosensitive composition disclosed herein can be suitably used for forming a conductive film in various electronic materials such as inductance parts, capacitor parts, and multilayer circuit boards. In other words, the present disclosure can provide a conductor film made of a sintered body of the photosensitive composition disclosed herein, or an electronic material having a conductor film made of a sintered body of the photosensitive composition disclosed herein. Such an electronic material can be said to be a high-quality electronic material, since it has a conductor film in which, for example, inversion expansion during high-temperature sintering is suitably suppressed and low resistance is suitably realized.
[0052] The electronic material may be of various mounting forms, such as a surface mount type or a through-hole mount type. The electronic material may be of a laminated type, a wire-wound type, or a thin-film type. Typical examples of inductance components include high-frequency filters, common mode filters, inductors (coils) for high-frequency circuits, inductors (coils) for general circuits, high-frequency filters, choke coils, transformers, and the like.
[0053] An example of an electronic material is a ceramic electronic material. In this specification, the term "ceramic electronic material" refers to electronic materials made of ceramic materials in general, including electronic materials having an amorphous ceramic substrate (glass ceramic substrate) or a crystalline (i.e., non-glass) ceramic substrate in general. Typical examples of ceramic electronic materials include high-frequency filters having a ceramic substrate, ceramic inductors (coils), ceramic capacitors, low-temperature co-fired ceramic substrates (LTCC substrates), and high-temperature co-fired ceramic substrates (HTCC substrates). The ceramic material is not particularly limited, and examples thereof include materials composed of the components listed as the ceramic components above.
[0054] Fig. 1 is a cross-sectional view showing a schematic structure of a multilayer chip inductor 1. Note that the dimensional relationships (length, width, thickness, etc.) in Fig. 1 do not necessarily reflect the actual dimensional relationships. Also, the symbols X and Y in the drawing represent the left-right direction and the up-down direction, respectively. However, these are merely directions for the convenience of explanation.
[0055] The laminated chip inductor 1 includes a main body 10 and external electrodes 20 provided on both side surfaces in the left-right direction X of the main body 10. The laminated chip inductor 1 has a size of, for example, 0603 (0.6 mm×0.3 mm), 0806 shape (0.8 mm×0.6 mm), 1608 shape (1.6 mm×0.8 mm), 2520 shape (2.5 mm×2.0 mm), etc.
[0056] The main body 10 has a structure in which ceramic layers (dielectric layers) 12 and internal electrode layers 14 are integrated. The ceramic layers 12 are made of a ceramic material. In the vertical direction Y, the internal electrode layers 14 are disposed between the ceramic layers 12. The internal electrode layers 14 are formed using the above-mentioned photosensitive composition. The internal electrode layers 14 adjacent to each other in the vertical direction Y across the ceramic layer 12 are electrically connected through vias 16 provided in the ceramic layers 12. As a result, the internal electrode layers 14 are configured in a three-dimensional spiral shape (spiral shape). Both ends of the internal electrode layers 14 are connected to external electrodes 20, respectively.
[0057] Such a multilayer chip inductor 1 can be manufactured, for example, by the following procedure. First, a paste containing raw ceramic material, binder resin, and organic solvent is prepared and supplied onto a carrier sheet to form a ceramic green sheet. Next, the ceramic green sheet is rolled and then cut to a desired size to obtain a plurality of green sheets for forming ceramic layers. Next, via holes are appropriately formed at predetermined positions of the plurality of green sheets for forming ceramic layers using a punch or the like.
[0058] Next, the above-mentioned photosensitive composition is used to form a conductive film of a predetermined coil pattern at a predetermined position of a plurality of green sheets for forming a ceramic layer. As an example, a conductive film in an unfired state can be formed by a manufacturing method including the following steps: (Step S1: film-like body forming step) a step of forming a conductive film made of a dried body of the photosensitive composition by applying the photosensitive composition onto a green sheet for forming a ceramic layer and drying it; (Step S2: exposure step) a step of covering the conductive film with a photomask of a predetermined opening pattern, exposing the conductive film through the photomask, and partially photocuring the conductive film; (Step S3: development step) a step of etching the conductive film after photocuring to remove the unexposed parts;
[0059] In addition, when forming a conductive film using the photosensitive composition, a conventionally known method can be appropriately used. For example, in (step S1), the photosensitive composition can be applied by various printing methods such as screen printing, or by using a bar coater or the like. The photosensitive composition can be dried at a temperature below the boiling point of the photopolymerizable compound and the photopolymerization initiator, typically at 50 to 100°C. In (step S2), for exposure, an exposure machine that emits light in a wavelength range of, for example, 10 to 500 nm, such as an ultraviolet ray irradiation lamp such as a high-pressure mercury lamp, a metal halide lamp, or a xenon lamp, can be used. In (step S3), for etching, typically, an alkaline aqueous developer can be used. For example, an aqueous solution containing sodium hydroxide, sodium carbonate, or the like can be used. The concentration of the alkaline aqueous solution can be adjusted to, for example, 0.01 to 0.5% by weight.
[0060] Next, (Step S4: Firing step) a plurality of green sheets for forming ceramic layers, on which unfired conductive films are formed, are stacked and pressure-bonded. This produces a laminate of unfired ceramic green sheets. Then, the laminate is cut into a desired chip size. Next, the laminate cut into the chip size is fired, for example, at 600 to 950°C. This causes the ceramic green sheets to be integrally sintered to form a main body 10 including a ceramic layer 12 and an internal electrode layer 14 made of a fired body of a photosensitive composition. Then, a suitable paste for forming external electrodes is applied to both ends of the main body 10 and fired to form external electrodes 20. In this manner, the multilayer chip inductor 1 can be manufactured.
[0061] In addition, the photosensitive composition disclosed herein can be used, for example, in combination with a photosensitive glass composition to form an electrode, and further in manufacturing electronic materials. Here, Fig. 2 is an explanatory diagram for explaining the manufacture of a multilayer chip inductor having an electrode formed by combining such a photosensitive composition and a photosensitive glass composition. An example of a method for manufacturing such a multilayer chip inductor will be described below.
[0062] First, a paste containing a ceramic material, a binder resin, and an organic solvent is prepared, and then supplied onto a carrier sheet to form a ceramic green sheet.
[0063] Next, the above-mentioned photosensitive composition is used to form a cured film of a predetermined coil pattern at a predetermined position of the green sheet. As an example, the following steps are included: a first forming step of applying (printing) the photosensitive glass composition onto a green sheet as a substrate and drying to form a glass film body which is a dried body of the photosensitive glass composition; a first exposure step of covering the glass film body with a photomask having a predetermined pattern, exposing a part of the glass film body exposed from the opening, and forming a part of the glass film body into a cured glass film; a first development step of removing the uncured glass film body using a developer to form a cured glass film having a predetermined groove on the substrate; a second forming step of applying (printing) the photosensitive composition onto the groove of the formed cured glass film and drying to form a conductive film body which is a dried body of the photosensitive composition into the groove of the glass film body; a second exposure step of covering the conductive film body with a photomask having a predetermined pattern, exposing a part of the conductive film body exposed from the opening, and forming a part of the conductive film body into a cured conductive film; and a second development step of removing the uncured conductive film body using a developer. This makes it possible to form an unfired cured glass film on the surface of the substrate and a conductive cured film in the grooves of the cured glass film.
[0064] Here, the photosensitive glass composition is not particularly limited, and a conventionally known photosensitive glass composition that can be used when manufacturing electronic components can be used without any particular limitation. For example, the photosensitive composition may be a paste-like composition containing a glass powder, a photopolymerizable compound, a photopolymerization initiator, and an organic dispersion medium. As the glass powder, any material that can be used in this type of photosensitive glass composition can be used without any particular limitation. In addition, as the photopolymerizable compound, the photopolymerization initiator, and the organic dispersion medium, the same type as the above-mentioned photosensitive composition can be used without any particular limitation, so detailed explanations are omitted. In addition, the photosensitive glass composition may contain additional components other than the above-mentioned components. Such additional components are not particularly limited, and include polymerization inhibitors, radical scavengers, antioxidants, plasticizers, surfactants, leveling agents, dispersants, defoamers, gelling inhibitors, stabilizers, preservatives, and the like.
[0065] In addition, when forming the glass cured film and the conductive cured film using the photosensitive glass composition and the photosensitive composition, a conventionally known method can be appropriately used. For example, in the first forming step and the second forming step, the photosensitive glass composition and the photosensitive composition can be applied by various printing methods such as screen printing, or by using a bar coater. These compositions are typically dried at 40 to 100°C.
[0066] Next, the first exposure step and the second exposure step are performed by placing a photomask having slits of a predetermined pattern on the glass film and exposing a part of the glass film (or the conductive film) exposed through the slits. In this exposure process, an exposure machine that emits light rays (typically ultraviolet rays) in the wavelength range of, for example, 10 nm to 500 nm, such as an ultraviolet irradiation lamp such as a high-pressure mercury lamp, a metal halide lamp, or a xenon lamp, can be used. The exposure dose of the exposure machine is, for example, 100 mJ / cm. 2 ~3000mJ / cm 2 The conditions can be set as follows.
[0067] In the first and second developing steps, an alkaline aqueous developer can be used as the developer. Examples of the aqueous developer include an aqueous sodium hydroxide solution and an aqueous sodium carbonate solution. The alkali concentration of these developers is preferably adjusted to, for example, 0.01 to 0.5% by weight.
[0068] FIG. 2 is a schematic diagram showing a laminate 100 before firing. As shown in FIG. 2, by repeatedly carrying out the above-mentioned first forming step to second developing step, a laminate 100 having a plurality of layers (the first layer L1 to the fourth layer L4 in FIG. 2) including a cured glass film 21 having a precise groove and a conductive cured film 22 formed in the groove can be produced on a ceramic base material 50. In addition, in this laminate 100, the conductive cured films 22 of the first layer L1 to the fourth layer L4 are connected through vias 26. The vias 26 can be formed by, for example, forming a via hole in the cured glass film 21 forming the upper surface of the first layer L1 using a guide punching machine, exposing a part of the upper surface of the conductive cured film 22, filling the via hole with a photosensitive composition, and then drying and exposing the via hole.
[0069] By applying a paste for forming external electrodes to the laminate 100 and then performing a firing process, a laminated chip inductor having a precise conductive layer 24 is manufactured. The firing temperature (maximum temperature in the firing process) is preferably, for example, about 600 to 950°C. In the manufacture of such a laminated chip inductor, the photosensitive glass composition having the above-mentioned configuration is used to form the cured glass film 21, so that precise patterning with high rectangularity is possible. By applying a photosensitive composition to the cured glass film 21 to form the cured conductive film 22, the cured conductive film 22 having a fine pattern can be formed. Then, by firing these, an electronic component having a fine pattern with an L / S of 30 μm / 30 μm or less can be manufactured with high precision. That is, according to this manufacturing method, even if the electronic component has a fine pattern, undercutting in which the exposed part of the film-like body is removed in the above-mentioned development process can be suppressed, and a highly reliable electronic component can be manufactured. Furthermore, in the manufacture of such laminated chip inductors, the density of the electrode layer, which is the sintered body of the conductor cured film, and the dielectric layer, which is the sintered body of the glass cured film, during the sintering process is very important, and the effects of the technology disclosed herein are more pronounced.
[0070] Test examples relating to the present disclosure will be described below, but it is not intended that the present disclosure be limited to such test examples.
[0071] [Test example] In the following test examples, 18 types of photosensitive compositions were prepared as Examples 1 to 18, and the conductive films, which were fired products of each photosensitive composition, were evaluated. Note that the resolution evaluation described below was performed using conductive films in an unfired state.
[0072] <Preparation of photosensitive compositions according to each example> (Photosensitive composition according to Example 1) First, silver particles (average particle diameter (D50 particle diameter): 2 μm) were prepared as conductive particles. In addition, commercially available reactive polymers (urethane, weight average molecular weight: 9000) and reactive oligomers (urethane, weight average molecular weight: 2000) were prepared as photopolymerization compounds, and commercially available cellulose-based water-soluble resins and acrylic-based water-soluble resins were prepared as binder resins. In addition, commercially available polydimethylsiloxane (weight average molecular weight: 50,000) was prepared as silicone resin. A mixture of commercially available 2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone and 2,4-diethylthioxanthone was prepared as a photopolymerization initiator, with the weight average molecular weight being 300. The silver particles, photopolymerizable compound, binder resin, silicone resin, and photopolymerization initiator prepared above were dispersed in a mixed solvent of commercially available dipropylene glycol methyl ether acetate and dihydroterpineol as a solvent to prepare a photosensitive composition according to Example 1. The blending ratio (wt%) of each material was as shown in Table 1. The viscosity of the photosensitive composition was about 20 to 70 Pa s at 25°C and 100 rpm (measured using a Brookfield HB type viscometer, spindle: SC-4-14, small cup, and at a measurement temperature of 25°C).
[0073] (Photosensitive compositions according to Examples 2 to 7 and 15) Photosensitive compositions according to Examples 2 to 7 and 15 were prepared in the same manner as the photosensitive composition according to Example 1, except that the blending amount of silicone resin (polydimethylsiloxane) was as shown in Table 1.
[0074] (Photosensitive compositions according to Examples 8 to 10) Photosensitive compositions according to Examples 8 to 10 were prepared in the same manner as the photosensitive composition according to Example 4, except that the weight average molecular weight of the silicone resin (polydimethylsiloxane) was as shown in Table 1.
[0075] (Photosensitive compositions according to Examples 11, 12, 16 and 17) Photosensitive compositions according to Examples 11, 12, 16, and 17 were prepared in the same manner as the photosensitive composition according to Example 1, except that the type of silicone resin was as shown in Table 1. Note that the side-chain fatty acid-modified polysiloxane in Table 1 refers to the R 1 ,R 2 ,R 3 ,R 5 ,R 6 is a methyl group, R 4 The side-chain amine-modified polysiloxane means a polysiloxane in which R 1 ,R 2 ,R 3 ,R 5 ,R 6 is a methyl group, R 4 The polysiloxanes used herein are commercially available products.
[0076] (Photosensitive composition according to Example 13) A photosensitive composition according to Example 13 was prepared in the same manner as in the photosensitive composition according to Example 4, except that a silane coupling agent (trimethoxymethylsilane) was added instead of the silicone resin.
[0077] (Photosensitive composition according to Example 14) The photosensitive composition of Example 14 was prepared in the same manner as the photosensitive composition of Example 1, except that no silicone resin was added.
[0078] (Photosensitive composition according to Example 18) A photosensitive composition according to Example 18 was prepared in the same manner as in the photosensitive composition according to Example 4, except that silica (SiO2) was added instead of the silicone resin.
[0079] (Evaluation test) In this evaluation test, the photosensitive composition according to each example was used to evaluate the resolution, the shrinkage rate, and the resistance value. The procedures for each evaluation are described below.
[0080] (1) Resolution evaluation First, the photosensitive composition (Examples 1 to 18) was applied to a ceramic green sheet made of commercially available borosilicate glass and alumina in a size of 4 cm x 4 cm by screen printing (printing process). Next, this was dried at 60°C for 15 minutes to form a film-like body (solid film) on the green sheet (forming process). Next, a photomask having openings of a predetermined pattern was placed on the film-like body, and then the film was exposed to light at an illuminance of 50 mW / cm by an exposure machine. 2 , exposure amount 300mJ / cm 2 The exposed portion was cured (exposure step). At this time, the pattern of openings formed in the photomask was formed by linear openings formed in parallel at a predetermined interval. A photomask was used in which the ratio L / S (line / space) of the width of the openings (width of the cured film) to the width of the space between adjacent openings (space between the cured film) was set to 30 μm / 30 μm.
[0081] Next, a 0.1 wt% alkaline Na2CO3 aqueous solution (developer) was sprayed onto the surface of the ceramic green sheet until the time reached 1.1 times the break point (BP) (developing step). The BP was defined as the time until the unexposed film was removed by the 0.1 wt% alkaline developer and it was possible to visually confirm that the film had been removed. The ceramic green sheet after the unexposed film had been removed was washed with pure water and dried at room temperature. This resulted in a composite in which a cured film was formed on the ceramic green sheet with a wiring pattern of L / S=30μm / 30μm and a film thickness of 8μm.
[0082] The spacing of the wiring pattern of the cured film formed after the development step was visually observed with an optical microscope in a total of 20 fields of view. Then, it was confirmed whether or not any part of the film-like body that had not been removed remained (presence or absence of residue). The results are shown in the corresponding columns in Table 1. The evaluation criteria in this evaluation are as follows: "◎": No residue was found within 20 fields of view. "○": Residue was confirmed in one visual field. "△": Residues were observed in 2 to 4 visual fields. "X": Residues were confirmed in five or more fields of view.
[0083] (2) Evaluation of disc shrinkage rate First, the photosensitive composition according to each example was applied onto a PET film to form a coating film. The application was performed using an applicator with a gap of 150 μm. The coating film was then dried at 150° C. for 1 hour. Next, the dried coating film was punched out with a die of φ15 mm to obtain a disk-shaped dried film. The dried film was then fired on a ceramic plate. The firing conditions were as follows: the temperature was raised to 400° C. in 8 hours, then held for 30 minutes, cooled to room temperature (about 25° C., the same below), heated to 800° C. (or 900° C.) at 10° C. / min, held for another 30 minutes, and then cooled to room temperature. The ratio of the diameter of the dried film before and after firing was calculated as the disk shrinkage rate. The results are shown in the corresponding columns of Table 1. In Table 1, the disk shrinkage rate at 800° C. is A (%), and the disk shrinkage rate at 900° C. is B (%). The evaluation criteria in this evaluation are as follows: "◎": The difference in disc shrinkage rate: BA (%) was more than 0.5. "◯": The difference in disc shrinkage rate: BA (%) was -0.5 or more and 0.5 or less. "X": The difference in disc shrinkage rate: BA (%) was less than -0.5.
[0084] (3) Evaluation of electrical resistivity First, the photosensitive composition according to each example was formed on an alumina substrate. The silver conductive film was formed by screen printing, and the screen pattern was 200 μm wide and 2 cm long. This was baked at 900° C. (held for 30 minutes) to form a silver line electrode. Next, the direct current resistance of each silver line electrode according to each example was measured based on a two-terminal measurement method, and the electrical resistivity was calculated from the cross-sectional area and length of the silver line electrode. A digital multimeter (SC-7401, manufactured by Iwasaki Electric Co., Ltd.) was used to measure the direct current resistance, and a laser microscope (VK-X1050, manufactured by Keyence Corporation) was used to measure the electrode cross-sectional area. The results are shown in the “Electrical resistivity” column in Table 1. The evaluation criteria in this evaluation are as follows. "◎": Electrical resistivity is 2.5×10 6 It was less than μΩcm. "○": Electrical resistivity is 2.5×10 6 μΩcm super 3.0×10 6 It was less than μΩcm. "×": Electrical resistivity is 3.0×10 6 It was more than μΩcm.
[0085] 3 to 7 are SEM images (magnification: 9000 times) showing the electrode surfaces of Examples 14, 3, 4, 6, and 8, respectively, after firing at 900° C.
[0086] [Table 1]
[0087] As shown in Table 1, in Examples 1 to 12, which are photosensitive compositions containing conductive particles (here, silver particles), a photopolymerizable compound, and a silicone resin, the silicone resin being represented by the above formula (I) and containing 0.05% to 1.0% of the silicone resin when the total weight of the conductive particles is 100%, it was confirmed that the inversion expansion of the conductive film during high-temperature firing (here, 800°C to 900°C) was suitably suppressed and the resistance of the conductive film was suitably reduced, compared with Example 13 in which a silane coupling agent was added, Example 14 in which no silicone resin was added, Example 16 and 17 in which a silicone resin other than the above formula (I) was added (in other words, a silicone resin highly reactive with resins such as photopolymerizable compounds and organic binders), Example 18 in which silica was added, and Example 15 in which the silicone resin represented by the above formula (I) was added outside the above range. Furthermore, as can be seen from Figures 3 to 7, in Example 14, in which silicone resin was not added, sintering of the silver particles did not progress sufficiently and there were large voids, whereas in Examples 3, 4, 6, and 8, sintering and grain growth of the silver particles progressed, resulting in higher conductivity of the conductor film (i.e., lower resistance).
[0088] As can be seen from the results of Examples 1 to 7, when the total weight of the conductive particles is taken as 100%, the silicone resin content of 0.15% to 0.6% can more suitably suppress the inversion expansion of the conductor film during high-temperature firing and reduce the resistance of the conductor film. As can be seen from the results of Examples 8 to 10, in addition to suppressing the inversion expansion of the conductor film during high-temperature firing and reducing the resistance of the conductor film, it is more preferable for the weight-average molecular weight of the silicone resin to be 1,000 to 10,000 in order to more suitably improve the resolution.
[0089] Although specific examples of the present disclosure have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.
[0090] As described above, specific aspects of the technology disclosed herein include those described in the following items. Item 1: A photosensitive composition comprising conductive particles, a photopolymerizable compound, and a silicone resin, the silicone resin being represented by the following formula (I): [ka] (R in formula I 1 ~R 6 are each independently an alkyl group, a phenyl group, a polyether group, an aralkyl group, a fluoroalkyl group, a fatty acid ester group, or a group into which a fatty acid amide group has been inserted. Also, m and n are each independently an integer of 0 or more. and the silicone resin is contained in an amount of 0.05% to 1.0% when the total weight of the conductive particles is taken as 100%. Item 2: The photosensitive composition according to item 1, wherein the silicone resin comprises at least one selected from the group consisting of polydimethylsiloxane, poly(methylphenylsiloxane), and side-chain polyether-modified polysiloxane. Item 3: The photosensitive composition according to item 1 or 2, wherein the silicone resin has a weight average molecular weight of 1,000 to 100,000. Item 4: The photosensitive composition according to any one of Items 1 to 3, wherein the conductive particles have an average particle size of 1 μm to 5 μm. Item 5: The photosensitive composition according to any one of Items 1 to 4, wherein the conductive particles have a lightness L* of 50 or more in the L*a*b color system based on JIS Z 8781. Item 6: The photosensitive composition according to any one of Items 1 to 5, which is used for forming an electrode on a ceramic green sheet. Item 7: The photosensitive composition according to any one of items 1 to 6, which is used for forming fine lines having a line width of 30 μm or less. Item 8: A conductive film comprising a fired product of the photosensitive composition according to any one of items 1 to 7. Item 9: An electronic material having a conductor film made of a sintered product of the photosensitive composition according to any one of items 1 to 7. [Explanation of symbols]
[0091] 1 Multilayer chip inductor 10 Main body 12 Ceramic layer 14 Internal electrode layer 16 Via 20 External electrode 21 Glass hardening film 22 Conductive hardened film 26 Via 50 Ceramic substrate 100 Laminate
Claims
1. A photosensitive composition comprising conductive particles, a photopolymerizable compound, and a silicone resin, The silicone resin has the following formula (I): 【Chemistry 1】 (R in formula I 1 ~R 6 are each independently an alkyl group, a phenyl group, a polyether group, an aralkyl group, a fluoroalkyl group, a fatty acid ester group, or a group into which a fatty acid amide group has been inserted. m and n are each independently an integer of 0 or more. It is expressed as The photosensitive composition contains the silicone resin in an amount of 0.05% to 1.0% when the total weight of the conductive particles is taken as 100%.
2. 2. The photosensitive composition according to claim 1, wherein the silicone resin comprises at least one selected from the group consisting of polydimethylsiloxane, poly(methylphenylsiloxane), and side-chain polyether-modified polysiloxane.
3. 3. The photosensitive composition according to claim 1, wherein the silicone resin has a weight average molecular weight of 1,000 to 100,000.
4. 3. The photosensitive composition according to claim 1, wherein the conductive particles have an average particle size of 1 μm to 5 μm.
5. 3. The photosensitive composition according to claim 1, wherein the conductive particles have a lightness L* of 50 or more in the L*a*b color system based on JIS Z 8781.
6. 3. The photosensitive composition according to claim 1, which is used to form an electrode on a ceramic green sheet.
7. 3. The photosensitive composition according to claim 1, which is used for forming fine lines having a line width of 30 μm or less.
8. A conductive film comprising a fired product of the photosensitive composition according to claim 1 or 2.
9. 3. An electronic material comprising a conductor film made of a sintered product of the photosensitive composition according to claim 1.
Citation Information
Patent Citations
JP1974065232A
Photosensitive conductive paste and electronic components
JP4660991B2