Polylactic acid-based fiber

Incorporating a β-methyl-δ-valerolactone polymer into polylactic acid fibers addresses brittleness and flexibility issues, enhancing mechanical properties and maintaining strength.

JP2024157077AInactive Publication Date: 2024-11-07KURARAY CO LTD

Patent Information

Application Number
JP2023071181
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polylactic acid fibers are brittle and have inferior flexibility and heat resistance, making them unsuitable for many applications due to the inhibition of crystallization by low molecular weight additives that improve flexibility.

Method used

Incorporating a β-methyl-δ-valerolactone polymer into polylactic acid fibers, which enhances flexibility while maintaining tensile strength by improving crystallization rate and impact resistance.

Benefits of technology

The resulting polylactic acid fibers exhibit improved flexibility and tensile strength, maintaining fiber integrity and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157077000001
    Figure 2024157077000001
  • Figure 2024157077000002
    Figure 2024157077000002
  • Figure 2024157077000003
    Figure 2024157077000003
Patent Text Reader

Abstract

To provide a polylactic acid-based fiber with superior flexibility while maintaining fiber strength.SOLUTION: A polylactic acid-based fiber contains a β-methyl-δ-valerolactone-based polymer and a polylactic acid-based resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polylactic acid fibers. [Background technology]

[0002] From the viewpoint of global environmental conservation, there is a demand in a wide range of fields for reducing the environmental impact of plastic materials used in products. In order to reduce the environmental impact, there has been active development of plastic materials using polylactic acid, which is one of the "biodegradable plastics". However, molded bodies and fibers made of polylactic acid tend to be more brittle than petroleum-based plastics, and have inferior flexibility and heat resistance, and are also easily hydrolyzed, so that their use as resin materials and various fiber products has been restricted.

[0003] In order to impart flexibility to polylactic acid fibers having properties such as hardness and brittleness, for example, Patent Document 1 (JP Patent Publication No. 2013-11033 A) describes that by adding polyglycerin fatty acid ester or polyglycerin condensed hydroxy fatty acid ester to polylactic acid fibers, a polylactic acid fiber having flexibility imparted to polylactic acid can be obtained by adding a small amount of polyglycerin without impairing heat resistance. Also, Patent Document 2 (JP Patent Publication No. 2010-84261 A) discloses that by adding a glycerin derivative having an average polymerization degree of 1 to 12 to polylactic acid fibers, the glycerin derivative contained inside the fibers imparts flexibility to the fibers, absorbs external impacts, and suppresses the occurrence and propagation of cracks, thereby improving wear resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-11033 A [Patent Document 2] JP 2010-84261 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when a low molecular weight additive is used as in Patent Documents 1 and 2, it has good dispersibility in polylactic acid, exerts a sufficient plasticizing effect, and can impart flexibility. However, in the case of polylactic acid, which has a slow crystallization rate, the additive inhibits the crystallization of polylactic acid, so that the strength of the fiber decreases depending on the amount added.

[0006] Therefore, in view of the above-mentioned current problems, an object of the present invention is to provide a polylactic acid fiber that has excellent flexibility while maintaining tensile strength. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have completed the present invention. That is, the present invention includes the following preferred embodiments. <1> A polylactic acid fiber comprising a β-methyl-δ-valerolactone polymer and a polylactic acid resin. <2> The β-methyl-δ-valerolactone polymer is represented by the following general formula (I): <1> The polylactic acid fiber according to claim 1. [ka] [In general formula (I), R 1 represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom of a linear alkyl group having 1 to 20 carbon atoms is substituted with a group represented by the following formula (X), or an oxygen-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the following formula (X). In the following formula (X), the bond represented by * bonds to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms. [ka] R 2 represents a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. n is an integer from 8 to 1,000, and m is an integer from 8 to 1,000. R 2 When a plurality of and m are present, they may be the same or different.] <3> The number average molecular weight of the β-methyl-δ-valerolactone polymer is 1,000 or more and 100,000 or less. <1> or <2> The polylactic acid fiber according to claim 1. <4> A long-period structure of 10.0 nm or more is observed in small-angle X-ray scattering measurement. <1> ~ <3> 10. The polylactic acid fiber according to claim 9, Effect of the Invention

[0008] The present invention can provide a polylactic acid fiber that is excellent in flexibility while maintaining fiber strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following is a description based on an example of an embodiment of the present invention. However, the embodiment shown below is an example for embodying the technical idea of ​​the present invention, and the present invention is not limited to the following description. In addition, although preferred forms of the embodiment are shown in this specification, a combination of two or more of each preferred form is also a preferred form. When there are several numerical ranges for matters shown in numerical ranges, the lower limit value and the upper limit value can be selectively combined to form a preferred form. In this specification, when a numerical range is stated as "XX to YY", it means "not less than XX and not more than YY".

[0010] [Polylactic acid resin] In this embodiment, the polylactic acid fiber contains a polylactic acid resin. Examples of the polylactic acid resin used in this embodiment include at least one selected from the group consisting of homopolymers of L-lactic acid, homopolymers of D-lactic acid, copolymers of L-lactic acid and D-lactic acid, homopolymers of DL-lactic acid, copolymers of DL-lactic acid and L-lactic acid, copolymers of DL-lactic acid and D-lactic acid, and polymers of lactide, which is a cyclic dimer of lactic acid. The polylactic acid resin may preferably have a content of L-lactic acid or D-lactic acid of 95% or more, more preferably 98% or more, and even more preferably 99% or more. By making it 95% or more, the crystallinity is high, the operability is good, and the fiber strength is good.

[0011] The polylactic acid resin may be a commercially available product, such as the "INGEO" series manufactured by Nature Works, the "Luminy" series manufactured by TOTALCORBION PLA, the "Revode" series manufactured by ZhejiangHisun Biomaterials Co., Ltd., and the "SUPLA" series manufactured by SUPLA Material Technology Co., Ltd.

[0012] The weight average molecular weight of the polylactic acid resin is preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 150,000 or more, from the viewpoint of melt spinnability. Also, from the viewpoint of compatibility with β-methyl-δ-valerolactone polymer, it is preferably 600,000 or less, more preferably 550,000 or less, and even more preferably 500,000 or less. That is, the weight average molecular weight of the polylactic acid resin is preferably 50,000 or more and 600,000 or less. The weight average molecular weight of the polylactic acid resin can be determined in terms of standard polystyrene by gel permeation chromatography (GPC) measurement. Also, when a commercially available product is used, the catalog value may be adopted.

[0013] [β-Methyl-δ-valerolactone polymer] In this embodiment, the polylactic acid fiber includes a β-methyl-δ-valerolactone polymer. The β-methyl-δ-valerolactone polymer (hereinafter, sometimes simply referred to as "polymer") used in this embodiment is preferably a polymer represented by the following general formula (I). The following polymer has a structure represented by general formula (I) and serves as an excellent modifier for polylactic acid resins. The following polymer is a polymer obtained by ring-opening polymerization of β-methyl-δ-valerolactone, and at least one hydroxyl group at the molecular end is modified to another functional group, resulting in a polymer in which the decrease in thermal decomposition is suppressed. TIFF2024157077000003.tif27150

[0014] In addition, the polymer is expected to be able to improve the tensile elongation at break of the polylactic acid fiber depending on the structure and number of the molecular terminals, and also to exhibit a good balance of properties such as improved crystallization rate, improved impact resistance, improved hydrolysis resistance, other functions, and ease of handling. Furthermore, since the raw material of the polymer is β-methyl-δ-valerolactone, the polylactic acid fiber of this embodiment is expected to have good biodegradability.

[0015] In general formula (I), R 1 represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. In the case of the above "branched alkyl group", the number of carbon atoms is 3 to 20, and in the case of the above "branched alkenyl group", the number of carbon atoms is 3 to 20.

[0016] In addition, in the general formula (I), R 1represents, in addition to the above-mentioned substituents, an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom in a linear alkyl group having 1 to 20 carbon atoms is substituted with a group represented by the following formula (X), or an oxygen-atom-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the following formula (X). In the following formula (X), the bond represented by * bonds to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms. TIFF2024157077000004.tif25154

[0017] In the general formula (I), n represents the average number of repetitions and is an integer of 8 to 1,000, preferably 8 to 800, more preferably 10 to 600, even more preferably 10 to 500, and even more preferably 10 to 300. When n is an integer of 8 or more, a more excellent modifying effect can be obtained. Also, when n is an integer of 1,000 or less, good compatibility with polylactic acid resins can be achieved.

[0018] R in the above formula (X) 2 is R 2 The linear alkyl group having 1 to 20 carbon atoms bonded to the above formula (X) can be exemplified by the same groups exemplified as the "linear alkyl group having 1 to 20 carbon atoms" described above. The linear alkyl group having 1 to 20 carbon atoms bonded to the above formula (X) is preferably a linear alkyl group having 1 to 15 carbon atoms, more preferably a linear alkyl group having 1 to 10 carbon atoms, even more preferably a linear alkyl group having 2 to 10 carbon atoms, and even more preferably a linear alkyl group having 2 to 5 carbon atoms.

[0019] Examples of the branched alkyl group having 3 to 20 carbon atoms bonded to the above formula (X) include the same groups exemplified as the above-mentioned "branched alkyl group having 3 to 20 carbon atoms". The branched alkyl group having 3 to 20 carbon atoms bonded to the above formula (X) is preferably a branched alkyl group having 3 to 15 carbon atoms, more preferably a branched alkyl group having 3 to 10 carbon atoms, still more preferably a branched alkyl group having 3 to 6 carbon atoms, and may be a branched alkyl group having 3 to 5 carbon atoms. Alternatively, it may be an oxygen atom-containing hydrocarbon group in which one hydrogen atom bonded to all terminal carbon atoms of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the above formula (X).

[0020] In the above formula (X), m represents the average number of repetitions and is an integer of 8 to 1,000, preferably 8 to 800, more preferably 10 to 500, and further preferably 10 to 300, and may be 10 to 100, 10 to 80, or 10 to 60. When m is an integer of 8 or more, a more excellent modifying effect can be obtained. Also, when m is an integer of 1,000 or less, good compatibility with polylactic acid resins can be achieved. In addition, R 1 In the case where a plurality of groups represented by the above formula (X) are present, they may be the same or different from each other. 2 and m may be present multiple times. 2 When a plurality of is present, they may be the same or different from each other. When a plurality of m is present, they may be the same or different from each other.

[0021] (Number average molecular weight (Mn)) From the viewpoint of obtaining a more excellent softening effect, the number average molecular weight of the polymer is preferably 1,000 or more, more preferably 1,500 or more, and even more preferably 2,000 or more. From the viewpoint of compatibility with polylactic acid resins, the number average molecular weight of the polymer is preferably 100,000 or less, more preferably 80,000 or less, and even more preferably 50,000 or less. That is, the number average molecular weight of the polymer is preferably 1,000 or more and 100,000 or less. In this specification, the number average molecular weight of the β-methyl-δ-valerolactone polymer is a number average molecular weight calculated as a standard polystyrene by gel permeation chromatography (GPC). The detailed measurement method can be according to the method described in the Examples.

[0022] (Weight average molecular weight (Mw)) The weight average molecular weight of the polymer is preferably 1,500 or more and 200,000 or less. If the weight average molecular weight is 1,500 or more, it is easy to exhibit a more excellent softening effect. If the weight average molecular weight is 200,000 or less, it is easy to be compatible with polylactic acid resins. The weight average molecular weight of the polymer is more preferably 2,200 or more, and even more preferably 3,000 or more. In addition, the number average molecular weight of the polymer is more preferably 160,000 or less, even more preferably 125,000 or less, and even more preferably 100,000 or less. In this specification, the weight average molecular weight of the β-methyl-δ-valerolactone polymer is a weight average molecular weight calculated based on standard polystyrene by gel permeation chromatography (GPC). The detailed measurement method can be according to the method described in the Examples.

[0023] (Molecular weight distribution (Mw / Mn)) The molecular weight distribution (Mw / Mn) of the β-methyl-δ-valerolactone polymer is preferably 1.0 to 3.0, more preferably 1.1 to 2.0, and further preferably 1.2 to 1.8. All "molecular weight distributions" described in this specification are values ​​calculated from the number average molecular weight and weight average molecular weight in terms of standard polystyrene measured by gel permeation chromatography (GPC). The detailed method for measuring the number average molecular weight and weight average molecular weight can be according to the method described in the Examples.

[0024] (viscosity) In this specification, the term "viscosity" refers to the viscosity of a polymer measured with an E-type viscometer. The measurement temperature can be optimized according to the molecular weight, etc. From the viewpoint of exhibiting a more excellent softening effect, the viscosity of the polymer is preferably 400 mPa·s or more at 80°C, and more preferably 1,000 mPa·s or more at 80°C. In addition, from the viewpoint of compatibility with polylactic acid resins and fluidity in a liquid feeder, the viscosity is preferably 200,000 mPa·s or less at 80°C, and more preferably 150,000 mPa·s or less at 80°C. That is, the viscosity of the polymer is preferably 400 mPa·s or more and 200,000 mPa·s or less at a measurement temperature of 80°C. When the polymer is measured with an E-type viscometer, the measurement temperature can be set according to the molecular weight, etc. In another preferred embodiment, the polymer has a viscosity of, for example, preferably 3,500 to 150,000 mPa·s, more preferably 4,000 to 150,000 mPa·s at 30°C. In another preferred embodiment, the polymer has a viscosity of, for example, preferably 650 to 150,000 mPa·s, more preferably 800 to 150,000 mPa·s at 60°C.

[0025] (Polymer manufacturing method) The method for producing the β-methyl-δ-valerolactone polymer is not particularly limited. On the other hand, from the viewpoint of productivity and simplicity, or when producing a high molecular weight polymer, it is preferable to adopt a production method including a step of adding a terminal modifying agent to a reaction solution obtained by reacting β-methyl-δ-valerolactone with an alcohol compound or water and a base catalyst to perform a terminal modification reaction (hereinafter also referred to as a "reaction step"). The above production method is characterized in that a terminal modifier is added directly to a reaction solution obtained by reacting β-methyl-δ-valerolactone with an alcohol compound or water and a base catalyst. That is, after ring-opening polymerization of β-methyl-δ-valerolactone, the terminals of the ring-opened polymer can be modified by adding a terminal modifier to the reactor in which the ring-opening polymerization was carried out, without taking out the ring-opened polymer once. Since the reaction process involves ring-opening polymerization reaction and terminal modification reaction in one pot, the above production method can be said to be a simplified process. The method for producing the polymer is not limited to the above-mentioned method.

[0026] (β-methyl-δ-valerolactone) The β-methyl-δ-valerolactone used in the production of the polymer may be one produced by a known method, for example, 2-hydroxy-4-methyltetrahydropyran or the like may be used as a raw material to produce the polymer by a known method (JP-B-6-53691, etc.). In addition, β-methyl-δ-valerolactone may be a commercially available product, and may be of petrochemical or biological origin.

[0027] The polylactic acid fiber of this embodiment contains the polylactic acid resin and the β-methyl-δ-valerolactone polymer, and the β-methyl-δ-valerolactone polymer is preferably contained in an amount of 0.1 to 10 parts by mass, more preferably 0.5 parts by mass or more, even more preferably 1.0 part by mass or more, and more preferably 8.0 parts by mass or less, per 100 parts by mass of the polylactic acid resin.

[0028] (Polylactic acid fiber) The polylactic acid fiber of this embodiment preferably has a single fiber fineness of 0.1 to 100 dtex, more preferably 0.1 to 30 dtex, and even more preferably 0.1 to 20 dtex. The method for obtaining the fiber used in this embodiment is not particularly limited, and a direct spinning method or a splitting method can be used. The direct spinning method is preferred as a method for obtaining fibers with a single fiber fineness of 0.5 to 100 dtex, and the splitting method is preferred as a method for obtaining fibers with a single fiber fineness of 0.3 to 1 dtex.

[0029] The total fineness of the polylactic acid fiber of this embodiment is not particularly limited, but is preferably 50 to 10,000 dtex, more preferably 80 to 5,000 dtex, even more preferably 100 to 2,000 dtex, and particularly preferably 200 to 1,000 dtex. The number of filaments is not particularly limited, but is preferably 2 to 1,000, and more preferably 5 to 500.

[0030] The polylactic acid fiber of this embodiment preferably has a melting point of 150°C or higher, more preferably 160°C or higher, and even more preferably 170°C or higher. Within the above range, a fiber with sufficient strength can be obtained. Furthermore, it is known that the melting point of polylactic acid varies depending on the ratio of D / L optical isomers, but if the melting point is 150°C or higher, a fiber with excellent crystallinity and sufficient strength can be obtained.

[0031] The polylactic acid fiber of this embodiment preferably has a tensile strength of 1.0 cN / dtex or more. More preferably, it is 2.0 cN / dtex or more, and even more preferably, it is 3.0 cN / dtex or more. There is no particular upper limit, but it may be 6.0 cN / dtex or less, 5.0 cN / dtex or less, or 4.5 cN / dtex or less. The elongation is preferably 10% or more. It is more preferably 15% or more, and even more preferably 20% or more. There is no particular upper limit, but it may be 500% or less, 400% or less, or 300% or less.

[0032] The polylactic acid fiber of this embodiment preferably has an elastic modulus of 5 cN / dtex or more, more preferably 10 cN / dtex or more, and although there is no particular upper limit, it may be 100 cN / dtex or less, or 80 cN / dtex or less.

[0033] The polylactic acid fiber of this embodiment preferably has a snag strength of 1.0 cN / dtex or more, more preferably 1.5 cN / dtex or more, and even more preferably 2.0 cN / dtex or more. There is no particular upper limit, but it may be 5.0 cN / dtex or less, or 4.0 cN / dtex or less. The knot strength is preferably 1.0 cN / dtex or more, more preferably 1.5 cN / dtex or more, and even more preferably 2.0 cN / dtex or more. There is no particular upper limit, but it may be 5.0 cN / dtex or less, or 4.0 cN / dtex or less.

[0034] In the polylactic acid fiber of this embodiment, the crystallite size-1 is preferably 1.0 nm or more using a diffraction peak observed in the meridian direction 2θ=16.5° in wide-angle X-ray measurement. If it is within this range, a polylactic acid fiber having excellent mechanical properties can be obtained. More preferably, it is 3.0 nm or more, and even more preferably, it is 5.0 nm or more. There is no particular limit to the upper limit, but it may be 20.0 nm or less, 17.0 nm or less, or 10.0 nm or less. In addition, it is preferable that the crystallite size-2 is 1.0 nm or more using a diffraction peak observed in the vicinity of 2θ=31°. If it is within this range, a polylactic acid fiber having excellent mechanical properties can be obtained. More preferably, it is 3.0 nm or more, and even more preferably, it is 5.0 nm or more. There is no particular limit to the upper limit, but it may be 20.0 nm or less, 17.0 nm or less, or 10.0 nm or less.

[0035] In the polylactic acid fiber of this embodiment, it is preferable that a long-period structure of 10.0 nm or more is observed in small-angle X-ray scattering measurement. More preferably, it is 12.0 nm or more, and even more preferably, it is 14.0 nm or more. There is no particular limit to the upper limit, but 20.0 nm or less is preferable. When a plasticizer consisting of a low molecular weight component is added to impart flexibility to polylactic acid, as in Patent Document 1 (JP Patent Publication 2013-11033 A), for example, a plasticizing effect is exerted on polylactic acid, and polylactic acid becomes soft. However, since the inhibition of crystallization due to the plasticizing effect also occurs at the same time, the crystallization size decreases as described above. On the other hand, the β-methyl-δ-valerolactone polymer of this embodiment is a liquid polymer at room temperature, and when this is added to polylactic acid, the β-methyl-δ-valerolactone polymer is localized in the amorphous part of polylactic acid and reduces the density of the amorphous part, so that the polylactic acid can be softened. Furthermore, even when β-methyl-δ-valerolactone-based polymers are added, the crystallization size of polylactic acid does not decrease, so a density difference occurs between the crystalline and amorphous components in the polylactic acid, and a long-period structure is observed in small-angle X-ray scattering measurements due to this density difference.

[0036] The polylactic acid fiber of this embodiment can be spun by a conventional melt spinning method, and can be produced by any of the following methods: a method of melt spinning at low or medium speed followed by drawing, a direct spinning-drawing method at high speed, and a method of spinning followed by drawing and false twisting simultaneously or successively.

[0037] More specifically, the polylactic acid resin is melted in a melt extruder, the molten polymer flow is introduced into a spinning head, metered by a gear pump, discharged from a spinning nozzle of a desired shape, and stretched as necessary, and then wound up, to produce the fiber of this embodiment. The melting temperature during spinning is appropriately adjusted depending on the melting point of the polylactic acid resin, and is usually preferably about 150 to 300°C. The thread discharged from the spinning nozzle may be wound up at high speed without being stretched, or may be stretched as necessary. The stretching operation may be performed at a temperature of 0.55 to 0.9 times the breaking elongation (HDmax) at a temperature equal to or higher than the glass transition point. If the stretching is less than 0.55 times the breaking elongation, it is difficult to stably obtain a fiber having sufficient strength, and if the stretching is more than 0.9 times the breaking elongation, thread breakage and fluff are likely to occur.

[0038] The stretching process may be performed by winding the fiber once after it is discharged from the spinning nozzle, or by spinning followed by stretching, either of which may be used in this embodiment. The stretching method may be a one-stage stretching method or a multi-stage stretching method of two or more stages. The take-up speed may vary depending on whether the fiber is once wound up and then stretched, whether it is spun and stretched in a single step of direct spinning and then wound up, or whether it is wound up at a high speed without stretching, but it can be taken up in the range of about 500 to 6000 m / min. If it is less than 500 m / min, the productivity is poor, and if it is an ultra-high speed exceeding 6000 m / min, fiber breakage is likely to occur. The fiber cross-sectional shape of this embodiment is not particularly limited, and it can be made into a perfect circle, hollow, or irregular cross section by using a normal melt spinning technique and depending on the shape of the nozzle. A perfect circle is preferable from the viewpoint of process passability in fiberization and weaving.

[0039] Furthermore, after drawing, it is preferable to heat set the fiber at a temperature equal to or lower than the melting point of the fiber in order to suppress shrinkage of the fiber. By heat setting the fiber at a temperature equal to or higher than the final drawing temperature and equal to or lower than the melting point of the fiber, crystallization of the fiber is promoted, so that a fiber with higher strength and lower heat shrinkage can be obtained. EXAMPLES

[0040] The present invention will now be described in detail with reference to examples. In the examples, various properties were measured and evaluated by the following methods.

[0041] (Number average molecular weight and weight average molecular weight) The number average molecular weight (Mn) and weight average molecular weight (Mw) were determined as standard polystyrene equivalent molecular weights by gel permeation chromatography (GPC). The specific measurement method is as follows.

[0042] <For amounts less than Mn15,000> Samples with Mn less than 15,000 were measured as follows to determine Mn and Mw. Tetrahydrofuran (THF) solution was used as the eluent. 10 mg of the sample was weighed out in terms of resin and dissolved in 1 mL of the eluent. The solution was passed through a 0.2 μm membrane filter to prepare a measurement sample. The measurement conditions were as follows. (Measurement conditions) Equipment: HLC-EcoSEC8320GPC (Tosoh Corporation) Column: KF-803, KF-802.5, and KF-802 (manufactured by Showa Denko KK) were connected in series. Eluent: Tetrahydrofuran Flow rate: 0.9mL / min Sample injection volume: 30 μL Column temperature: 40℃ Standard polystyrene: Tosoh Corporation's PSt Oligomer Kit (molecular weight 589 to 98,900) was used and approximated by a third-order equation. Detector: RI detector

[0043] <For Mn15,000 or more> Samples with Mn of 15,000 or more were measured as follows to determine Mn and Mw. Tetrahydrofuran (THF) solution was used as the eluent. 1.0 mg of the sample was weighed out in terms of resin and dissolved in 1 mL of the eluent. The solution was passed through a 0.2 μm membrane filter to prepare a measurement sample. The measurement conditions were as follows. (Measurement conditions) Equipment: HLC-8220GPC (Tosoh Corporation) Column: Two TSK-gel SuperMultiporeHZ-M columns (manufactured by Tosoh Corporation) were connected in series. Eluent: Tetrahydrofuran Flow rate: 0.35mL / min Sample injection volume: 10 μL Column temperature: 40℃ Standard polystyrene: Polystyrene molecular weight standards (molecular weight 580 to 1,214,000) manufactured by GL Sciences Inc. were used and approximated by a cubic equation. Detector: RI detector

[0044] (fineness, tensile strength) Measurement was performed in accordance with JIS L 1013.

[0045] (Hook strength) The hook strength was measured in accordance with JIS L 1013, and calculated by dividing the hook strength by twice the fineness.

[0046] (Nodule strength) The knot strength was measured in accordance with JIS L 1013, and the knot strength was divided by the fineness to calculate the knot strength.

[0047] (Measurement of crystallite size and long-period structure) Wide-angle X-ray measurement Measurement equipment: Bruker D8 DISCOVER IμS Detector: 2D PSPC・VANTEC-500 Measurement conditions: current = 1mA, voltage = 50kV, camera distance = 10cm, collimator diameter = long 0.5mm, exposure time = 10min, 2θ axis = 20°, θ axis = 10°, χ axis = 90° (equator) - 0° (meridian) The sample was a bundle of four pieces. The angle of the chi-axis was changed so that the equator line was vertical and the meridian line was horizontal. Next, the crystallite size-1 and crystallite size-2 were estimated using the diffraction peaks observed in the meridian direction 2θ=16.5° and 31° obtained by the above method. Specifically, they were calculated from the peak position (2θ) and half-width using the Scherrer formula.

[0048] Small angle X-ray measurement Measurement equipment: Rigaku NANOPIX Detector: Semiconductor 2D detector HyPix-6000 Measurement conditions: current = 30 mA, voltage = 40 kV, incident optical system = 2PHF, beam stopper diameter = 4 mm, camera position = 1300.87 mm, exposure time = 10 minutes, sample was a bundle of 8 pieces. Next, calculation was performed using Black's formula from the peak top position of the small angle profile obtained by the above method.

[0049] (Production of β-methyl-δ-valerolactone polymers) A 500 mL glass 4-neck flask was purged with nitrogen, and 7.9 g (90 mmol) of isoamyl alcohol and 231 g (2,025 mmol) of β-methyl-δ-valerolactone were added and heated to 60° C. 0.84 mL of n-butyllithium (1.6 M hexane solution) was added and stirred at 60° C. for 60 minutes. Next, 11.0 g (108 mmol) of acetic anhydride and 0.55 g (4.5 mmol) of 4-dimethylaminopyridine dissolved in 5.5 g of β-methyl-δ-valerolactone were placed in the above-mentioned four-necked glass flask, and the mixture was stirred at 60° C. for 60 minutes to obtain a reaction solution containing a polymer. The reaction solution containing the obtained polymer was extracted with toluene and water, and purified by distillation to obtain 155 g (0.04 mmol) of a polymer. The obtained β-methyl-δ-valerolactone-based polymer is represented by the above-mentioned general formula (I), and R 1 =(CH 3 ) 2 CHCH 2 CH 2 , R 2 =CH 3, n = 25. The resulting β-methyl-δ-valerolactone polymer had a number average molecular weight of 4,000 and a weight average molecular weight of 6,000.

[0050] Example 1 0.5 parts by mass of the β-methyl-δ-valerolactone polymer synthesized by the above method was added to 100 parts by mass of polylactic acid resin (TOTAL CORBION PLA's "L-130" L-isomer purity >99%), and melt extruded while kneading in a twin-screw extruder. The mixture was discharged from a 0.2 mmΦ×50 hole round hole nozzle at a spinning temperature of 240°C, the ratio of the discharge speed to the winding speed (draft) was adjusted to 47, and the winding speed was within the range of 1000 m / min. The single yarn fineness of the obtained raw yarn was 6.6 dtex. Next, it was drawn at a draw ratio of 3.71 times by dry heat drawing at 100°C in one furnace to obtain a drawn yarn of 100 dtex / 50 filaments. The obtained drawn yarn was evaluated, and the results are shown in Table 1. The flexibility was evaluated using the hook strength and knot strength, which are indicators of the fragility of the fiber. The resulting polylactic acid fiber had a tensile strength of 3.60 cN / dtex, a hook strength of 2.70 cN / dtex, and a knot strength of 2.30 cN / dtex.

[0051] (Examples 2 to 3) Polylactic acid fibers were obtained in the same manner as in Example 1, except that the addition ratio of the β-methyl-δ-valerolactone polymer and the draw ratio were changed as shown in Table 1. The results are shown in Table 1.

[0052] (Reference example 1) Polylactic acid fibers were obtained in the same manner as in Example 1, except that no β-methyl-δ-valerolactone polymer was added and the draw ratio was changed as shown in Table 1. The results are shown in Table 1.

[0053] [Table 1]

[0054] From Table 1, it can be seen that the polylactic acid fibers containing the β-methyl-δ-valerolactone polymers of Examples 1 to 3 have improved flexibility by improving the loop strength and knot strength while suppressing the decrease in tensile strength compared to the polylactic acid fiber of Reference Example 1. [Industrial Applicability]

[0055] The polylactic acid-based fiber of the present invention has excellent flexibility while maintaining fiber strength, and therefore can be used extremely effectively in many applications, including industrial materials, agricultural materials, apparel, and the aircraft, automobile, and ship fields.

Claims

1. A polylactic acid fiber comprising a β-methyl-δ-valerolactone polymer and a polylactic acid resin.

2. 2. The polylactic acid fiber according to claim 1, wherein the β-methyl-δ-valerolactone polymer is represented by the following general formula (I): [Formula 1] [In general formula (I), R 1 represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, an arylalkyl group having 7 to 12 carbon atoms, an oxygen-containing hydrocarbon group in which one hydrogen atom bonded to a terminal carbon atom of a linear alkyl group having 1 to 20 carbon atoms is substituted with a group represented by the following formula (X), or an oxygen-containing hydrocarbon group in which one hydrogen atom bonded to at least one terminal carbon atom of a branched alkyl group having 3 to 20 carbon atoms is substituted with a group represented by the following formula (X). In the following formula (X), the bond represented by * bonds to the linear alkyl group having 1 to 20 carbon atoms or the branched alkyl group having 3 to 20 carbon atoms. [Case 2] R 2 represents a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an arylalkyl group having 7 to 12 carbon atoms. n is an integer from 8 to 1,000, and m is an integer from 8 to 1,000. R 2 When a plurality of and m are present, they may be the same or different from each other.

3. 3. The polylactic acid fiber according to claim 1, wherein the number average molecular weight of the β-methyl-δ-valerolactone polymer is 1,000 or more and 100,000 or less.

4. 3. The polylactic acid fiber according to claim 1, in which a long-period structure of 10.0 nm or more is observed in small-angle X-ray scattering measurement.

Citation Information

Patent Citations

  • Biodegradable fiber

    JP2010084261A

  • Polylactic acid fiber

    JP2013011033A

Cited By

  • Nonwoven fabric and method for producing same

    WO2026048821A1