Rubber composition for tires
A tire rubber composition with silica, thermoplastic resin, and ester plasticizer addresses performance and compatibility issues in natural rubber-based treads, enhancing wet performance, rolling resistance, and chipping resistance while promoting sustainability.
Patent Information
- Application Number
- JP2023071251
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional tire rubber compositions for passenger car treads face challenges in maintaining wet performance, low rolling resistance, chipping resistance, and processability when transitioning from styrene-butadiene rubber to natural rubber, which can result in insufficient performance and compatibility issues.
A rubber composition for tires comprising 50-150 parts by mass of silica, 16 parts by mass of thermoplastic resin, and an ester plasticizer, primarily composed of isoprene rubber, which improves compatibility and viscoelastic behavior, enhancing wet performance, low rolling resistance, and chipping resistance.
The composition achieves a balanced improvement in wet performance, low rolling resistance, and chipping resistance while maintaining processability, with a high proportion of renewable and recycled materials, reducing environmental impact.
Smart Images

Figure 2024157114000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for tires intended to be used primarily in the tread portion of passenger vehicle tires. [Background technology]
[0002] Conventionally, rubber compositions for tires used in the tread portion of passenger car tires have been formulated mainly with styrene-butadiene rubber (SBR). However, in recent years, from the viewpoint of environmental protection, the adoption of compositions mainly with natural rubber (NR) has been considered (see, for example, Patent Document 1). That is, although it is difficult to use the conventionally used styrene-butadiene rubber (synthetic rubber) as recycled rubber, by replacing it with natural rubber, which is a renewable material, it is possible to increase the ratio of renewable and recycled raw materials in the tire (rubber composition) and reduce the environmental load.
[0003] However, simply replacing styrene-butadiene rubber with natural rubber may not provide the performance required for the tread portion of passenger car tires, and may also result in insufficient processability. For example, natural rubber tends to have a lower glass transition temperature than styrene-butadiene rubber, and has different compatibility with other polymers and compounding agents, so switching to a rubber composition mainly made of natural rubber has the problem of affecting the wet performance, low rolling resistance, chipping resistance, and other performance and processability required for tread rubber. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6092986 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a rubber composition for tires which maintains and improves wet performance, low rolling resistance, chipping resistance and processability, and which achieves a good balance between these performances to a high degree. [Means for solving the problem]
[0006] The rubber composition for tires of the present invention, which achieves the above-mentioned objective, is characterized in that it contains 100 parts by mass of diene-based rubber containing 50% by mass or more of isoprene-based rubber, 50 parts by mass or more and 150 parts by mass or less of silica, 16 parts by mass or more and 200 parts by mass or less of thermoplastic resin, and 10 parts by mass or less of an ester-based plasticizer. Effect of the Invention
[0007] The rubber composition for tires of the present invention is a compound in which a diene rubber mainly composed of an isoprene rubber is blended with a thermoplastic resin and an ester plasticizer, and therefore the compatibility between the isoprene rubber and the thermoplastic resin is improved, and the viscoelastic behavior is improved, so that wet performance, low rolling resistance, chipping resistance, and processability can be maintained and improved at levels higher than those of the past. In particular, the blending of the ester plasticizer improves the compatibility between the isoprene rubber and the thermoplastic resin, and the balance between wet performance, low rolling resistance, and chipping resistance can be improved.
[0008] The isoprene-based rubber is preferably a natural rubber, and all of the diene-based rubbers are preferably isoprene-based rubbers.
[0009] The ester-based plasticizer is preferably at least one selected from the group consisting of an aliphatic dibasic acid ester, a phosphate ester, a phthalate ester, and a trimellitate ester.
[0010] The thermoplastic resin is preferably at least one selected from the group consisting of C5 petroleum resins, C9 petroleum resins, C5 / C9 petroleum resins, dicyclopentadiene resins, C5 / dicyclopentadiene resins, C9 / dicyclopentadiene resins, terpene resins, aromatic modified terpene resins, rosin resins, and hydrogenated resins thereof. The thermoplastic resin is preferably composed of aliphatic monomer-derived units and / or aromatic monomer-derived units, and has an aromatic proton content of 30% or less. [Brief description of the drawings]
[0011] [Figure 1] 1 is a meridian cross-sectional view showing an example of a pneumatic tire using the rubber composition for tires of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The configuration of the present invention will be described in detail below with reference to the accompanying drawings. As illustrated in FIG. 1, a pneumatic tire using the rubber composition for tires of the present invention includes a tread portion 1, a pair of sidewall portions 2 arranged on both sides of the tread portion 1, and a pair of bead portions 3 arranged on the tire radially inward side of the sidewall portions 2. In FIG. 1, the symbol CL indicates the tire equator. Although not depicted in FIG. 1 because it is a meridian cross section, the tread portion 1, the sidewall portions 2, and the bead portions 3 each extend in the tire circumferential direction to form an annular shape, thereby forming a toroidal basic structure of a pneumatic tire. The following description using FIG. 1 is basically based on the meridian cross section shown in the figure, but each tire component extends in the tire circumferential direction to form an annular shape.
[0013] A carcass layer 4 is installed between a pair of left and right bead portions 3. This carcass layer 4 includes a plurality of reinforcing cords extending in the tire radial direction, and is folded back from the vehicle inner side to the vehicle outer side around a bead core 5 arranged in each bead portion 3. A bead filler 6 is arranged on the outer periphery of the bead core 5, and this bead filler 6 is wrapped by the main body and the folded back part of the carcass layer 4. Meanwhile, a plurality of belt layers 7 (two layers in FIG. 1) are embedded on the outer periphery side of the carcass layer 4 in the tread portion 1. Each belt layer 7 includes a plurality of reinforcing cords inclined with respect to the tire circumferential direction, and the reinforcing cords are arranged so as to cross each other between the layers. In these belt layers 7, the inclination angle of the reinforcing cords with respect to the tire circumferential direction is set to, for example, a range of 10° to 40°. Furthermore, a belt reinforcing layer 8 (two layers, a full cover 8a that covers the entire width of the belt layer 7 and an edge cover 8b that locally covers the end portion of the belt layer 7) is provided on the outer periphery side of the belt layer 7. The belt reinforcing layer 8 includes organic fiber cords oriented in the tire circumferential direction. In the belt reinforcing layer 8, the organic fiber cords are set at an angle of, for example, 0° to 5° with respect to the tire circumferential direction.
[0014] A tread rubber layer 10 is disposed on the outer peripheral side of the carcass layer 4 in the tread portion 1, and this tread rubber layer 10 has a structure in which two types of rubber layers with different physical properties (a cap tread 11 constituting the tread surface of the tread portion 1 and an undertread 12 disposed on its inner peripheral side) are laminated in the tire radial direction. The rubber composition for tires of the present invention is mainly used for the cap tread 11 of such tires.
[0015] The tire in which the rubber composition for tires of the present invention is used is preferably a pneumatic tire (a tire filled with air, an inert gas such as nitrogen, or other gases) as described above, but may be a non-pneumatic tire. Even in the case of a non-pneumatic tire, the rubber composition for tires of the present invention is used in the portion that comes into contact with the road surface (the portion corresponding to the cap tread 11 that constitutes the tread surface of the tread portion 1 in a pneumatic tire).
[0016] In the rubber composition for tires of the present invention, the rubber component is a diene rubber, and necessarily contains an isoprene rubber. The amount of the isoprene rubber is 50% by mass or more, preferably 70 to 100% by mass, and more preferably 85 to 100% by mass, based on 100% by mass of the diene rubber. All of the diene rubber may be isoprene rubber. Examples of the isoprene rubber include various natural rubbers and various synthetic polyisoprene rubbers. Among these isoprene rubbers, natural rubber is particularly suitable. By using isoprene rubber as the majority of the diene rubber in this way, it is possible to reduce the environmental load. That is, in the case of natural rubber, since no synthetic rubber derived from petroleum is used, the dependency on petroleum can be reduced and the environmental load can be reduced. In addition, compared to a rubber composition mainly composed of conventional synthetic rubber (e.g., styrene butadiene rubber), a rubber composition mainly composed of natural rubber is easy to use as regenerated rubber after disposal, so that the environmental load can also be reduced from the viewpoint of recyclability. Meanwhile, in recent years, technology has been developed to produce isoprene from sugars derived from biomass (biological resources), and by using synthetic polyisoprene rubber obtained by polymerizing such isoprene, it is possible to reduce dependence on petroleum and reduce the burden on the environment.
[0017] The rubber composition for tires of the present invention may contain other diene rubbers in addition to the above-mentioned isoprene rubber. As the other diene rubber, rubbers that can be generally used in rubber compositions for tires can be used. For example, butadiene rubber, styrene butadiene rubber, etc. can be exemplified. These other diene rubbers can be used alone or as any blend. However, even when other diene rubbers are blended, the blending amount is 50% by mass or less, preferably 20% by mass or less, and more preferably 15% by mass or less, based on 100% by mass of the diene rubber. That is, when the ratio of other diene rubbers (especially synthetic rubbers) is high, the ratio of renewable raw materials and recycled raw materials is low, and the effect of reducing environmental load is not sufficiently obtained. Specifically, when the blending amount of other diene rubbers exceeds 50% by mass (that is, when the blending amount of isoprene rubber is less than 50% by mass), the ratio of isoprene rubber that contributes to reducing environmental load is reduced, and the effect of reducing environmental load is not sufficiently obtained.
[0018] Rubber compositions for tires always contain a thermoplastic resin. By compounding a relatively large amount of a specific thermoplastic resin having good compatibility with a diene rubber containing 50% by mass or more of isoprene rubber, it is possible to improve the tensile strength at break and tan δ at 0°C to the same level or higher as a rubber composition mainly composed of styrene-butadiene rubber, and further, the processability is good. When used in the tread portion of a tire, it is possible to improve wet performance, low rolling resistance, and chipping resistance.
[0019] The thermoplastic resin is preferably composed of aliphatic monomer-derived units and / or aromatic monomer-derived units. That is, it may be composed of only aliphatic monomer-derived units, only aromatic monomer-derived units, or both aliphatic monomer-derived units and aromatic monomer-derived units. Examples of the aliphatic monomer-derived units include monomer-derived units whose monomer is an aliphatic compound or an alicyclic compound. The aliphatic compound may be either linear or branched, and may be either saturated or unsaturated. The alicyclic compound is a compound composed of a ring that does not have aromaticity, and may be either saturated or unsaturated. In addition, the alicyclic compound may have any aliphatic compound bonded to its side chain. Examples of the aromatic monomer-derived units include monomer-derived units whose monomer is a compound (aromatic compound) having an aromatic ring. The aromatic compound may have any aliphatic compound or alicyclic compound bonded to it.
[0020] Examples of thermoplastic resins include petroleum-based resins, aromatic resins, etc. Examples of petroleum-based resins include C5 petroleum resins (aliphatic petroleum resins polymerized from fractions such as isoprene, 1,3-pentadiene, cyclopentadiene, methylbutene, and pentene), C9 petroleum resins (aromatic petroleum resins polymerized from fractions such as α-methylstyrene, o-vinyltoluene, m-vinyltoluene, and p-vinyltoluene), C5 / C9 resins, dicyclopentadiene resins (DCPD resins), and C9 / dicyclopentadiene resins. Examples of the resins include hydrogenated C5 petroleum resins, hydrogenated C9 petroleum resins, hydrogenated C5 / C9 petroleum resins, hydrogenated dicyclopentadiene resins (hydrogenated DCPD resins), hydrogenated C5 / dicyclopentadiene resins (C5 / hydrogenated DCPD resins), and hydrogenated C9 / dicyclopentadiene resins (C9 / hydrogenated DCPD resins). Examples of aromatic resins include coumarone resins, phenolic resins, alkylphenolic resins, terpene resins, aromatic modified terpene resins, rosin resins, novolac resins, resol resins, and aromatic indene copolymers. These resins can be used alone or as a blend of multiple resins. The above-mentioned C9 petroleum resins are also classified as aromatic resins.
[0021] The thermoplastic resin is preferably at least one selected from the group consisting of C5 petroleum resins, C9 petroleum resins, C5 / C9 petroleum resins, dicyclopentadiene resins, C5 / dicyclopentadiene resins, C9 / dicyclopentadiene resins, terpene resins, aromatic modified terpene resins, rosin resins, and hydrogenated resins thereof.
[0022] The thermoplastic resin is composed of aliphatic monomer-derived units and / or aromatic monomer-derived units, and the aromatic proton content is 30% or less, preferably 0% to 30%, more preferably 2% to 20%, and even more preferably 5% to 15%. If the aromatic proton content exceeds 30%, the compatibility with isoprene-based rubber (natural rubber) deteriorates, and sufficient tensile strength at break cannot be obtained. The aromatic proton content of the thermoplastic resin can be adjusted by the ratio of the aliphatic monomer-derived units and the aromatic monomer-derived units or by hydrogenating the thermoplastic resin. In this specification, the aromatic proton content of the thermoplastic resin is the ratio of the aromatic proton content to the total of the aromatic proton content and the aliphatic proton content contained in the thermoplastic resin, 1 It can be determined from the results of H-NMR spectroscopy.
[0023] The softening point of the thermoplastic resin is 80°C or higher and 160°C or lower, preferably 85°C to 145°C, and more preferably 90°C to 130°C. If the softening point of the thermoplastic resin is lower than 80°C, the effect of improving wet performance cannot be sufficiently obtained. If the softening point of the thermoplastic resin is higher than 160°C, the compatibility with the isoprene-based rubber decreases. In this specification, the softening point of the thermoplastic resin can be measured in accordance with JIS K6220-1 (ring and ball method).
[0024] The rubber composition for tires may contain other thermoplastic resins different from the above-mentioned thermoplastic resins that satisfy the requirements for aromatic proton content and softening point. The other thermoplastic resins different from the above-mentioned thermoplastic resins refer to thermoplastic resins that differ from each other in properties such as aromatic proton content, softening point, and average molecular weight, and / or thermoplastic resins that differ in the type, content ratio, and presence or absence of hydrogenation of aliphatic monomer-derived units and / or aromatic monomer-derived units. The number of other thermoplastic resins may be one or more. When the other thermoplastic resin is contained, it is preferable that the weighted average of the aromatic proton content of the thermoplastic resin and the aromatic proton content of the other thermoplastic resin is 30% or less. That is, when the aromatic proton contents of the thermoplastic resin and the other thermoplastic resin are H1% and H2%, and the respective contents are m1% by mass and m2% by mass, the weighted average Hav of the aromatic proton contents calculated by the following calculation formula is 30% or less. Hav = (H1 × m1 + H1 × m1) / (m1 + m2) When three or more thermoplastic resins are used, the weighted average value can be calculated in the same manner. The weighted average Hav of the aromatic proton content is preferably 0% to 30%, more preferably 2% to 20%, and further preferably 5% to 15%.
[0025] The thermoplastic resin is blended in an amount of 16 parts by mass or more and 200 parts by mass or less, preferably 25 parts by mass or more and 180 parts by mass or less, more preferably more than 50 parts by mass or less and 150 parts by mass or less, and even more preferably 55 parts by mass or more and 120 parts by mass or less, per 100 parts by mass of diene rubber. When the thermoplastic resin is blended in an amount of 16 parts by mass or more, the tensile strength at break and tan δ at 0°C of the rubber composition can be improved, and the chipping resistance and wet performance of the pneumatic tire can be improved. When the thermoplastic resin exceeds 200 parts by mass, the low rolling resistance is deteriorated.
[0026] The rubber composition for tires is compounded with an ester-based plasticizer together with the isoprene-based rubber and the thermoplastic resin. The coexistence of the ester-based plasticizer can further increase the affinity between the isoprene-based rubber and the thermoplastic resin, which is advantageous for improving wet performance, low rolling resistance, and chipping resistance. Furthermore, the viscosity of the rubber composition can be reduced to improve processability. In contrast, ether-based plasticizers such as oil, polyethylene glycol, and polypropylene glycol can contribute to improving processability as a processing aid, but do not affect the affinity between the isoprene-based rubber and the thermoplastic resin, unlike the ester-based plasticizers.
[0027] The ester plasticizer is preferably blended in an amount of 10 parts by mass or less, preferably 1 to 8 parts by mass, more preferably 2 to 6 parts by mass, per 100 parts by mass of diene rubber. If the amount of the ester plasticizer exceeds 10 parts by mass, wet performance and low rolling resistance are reduced.
[0028] Examples of ester-based plasticizers include organic acid esters such as carboxylates, which are made of organic acids such as carboxyl groups and alcohols such as monohydric alcohols, polyhydric alcohols, and phenols, phosphoric acid esters made of phosphoric acid and alcohols, and sulfonic acid esters having amide groups. Of these, carboxylates and phosphoric acid esters are preferred.
[0029] Examples of carboxylic acids constituting the ester-based plasticizer include aliphatic monocarboxylic acids, aliphatic dicarboxylic acids (aliphatic dibasic acids), aliphatic tricarboxylic acids, aromatic monocarboxylic acids, aromatic dicarboxylic acids, aromatic tricarboxylic acids, etc. The number of carbon atoms in the carboxylic acid is preferably 1 to 20, more preferably 3 to 12, and may have a carbon-carbon double bond. The hydrocarbon constituting the carboxylic acid may be linear, branched, alicyclic, or aromatic.
[0030] The alcohols constituting the ester-based plasticizer are preferably monohydric alcohols, and the number of carbon atoms therein is preferably 1 to 20, more preferably 3 to 12. The hydrocarbon group of the monohydric alcohol may be linear, branched, or alicyclic.
[0031] Examples of the carboxylic acid ester include monoesters, diesters, triesters, and mixtures thereof.Specific examples of the carboxylic acid monoester include oleic acid esters such as octyl oleate and nonyl oleate, stearic acid esters, linoleic acid esters, linolenic acid esters, and ricinoleic acid esters.Examples of the carboxylic acid diester include aliphatic dibasic acid esters and phthalic acid esters.Examples of the carboxylic acid triester include trimellitic acid esters such as tris(2-ethylhexyl) trimellitate.
[0032] Examples of aliphatic dibasic acid esters include malonic acid esters, malic acid esters, fumaric acid esters, and succinic acid esters; adipic acid esters such as dibutyl adipate, diisobutyl adipate, bis(2-ethylhexyl) adipate, diisooctyl adipate, dioctyl adipate, diisononyl adipate, and diisodecyl adipate; and sebacate esters such as dibutyl sebacate, bis(2-ethylhexyl) sebacate, and diisooctyl sebacate.
[0033] Examples of phthalic acid esters include phthalic acid esters such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, bis(-2-ethylhexyl) phthalate, dioctyl phthalate, diisodecyl phthalate, and diisononyl phthalate, isophthalic acid esters, and tetrahydrophthalic acid esters.
[0034] Examples of phosphate esters include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tris(2-ethylhexyl) phosphate, trioctyl phosphate, dioctyl phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, tritolyl phosphate, cresyl diphenyl phosphate, isodecyl diphenyl phosphate, and 2-ethylhexyl diphenyl phosphate.
[0035] Examples of the sulfonic acid ester include N-butylbenzenesulfonamide, toluenesulfonamide, N-ethyl-toluenesulfonamide, and N-cycloalkyl-p-toluenesulfonamide.
[0036] Among the above-mentioned ester-based plasticizers, aliphatic dibasic acid esters, phosphate esters, phthalate esters, and trimellitate esters are more preferable.
[0037] The rubber composition for tires improves wet performance and low rolling resistance by compounding silica. The compounding amount of silica is 50 parts by mass or more and 150 parts by mass or less, preferably 60 parts by mass or more and 135 parts by mass or less, more preferably 70 parts by mass or more and 120 parts by mass or less, per 100 parts by mass of diene rubber. If the silica is less than 50 parts by mass, the effect of improving wet performance cannot be obtained sufficiently. If the silica is more than 150 parts by mass, dispersibility is deteriorated and rolling resistance is rather increased.
[0038] As the silica, silica that is usually used in rubber compositions for tires, such as wet-process silica, dry-process silica, or surface-treated silica, can be used. Silica can be appropriately selected from commercially available products and used. Silica obtained by a normal manufacturing method can also be used.
[0039] The rubber composition for tires may contain fillers other than silica. Examples of the other fillers include materials that are generally used in rubber compositions for tires, such as carbon black, clay, talc, calcium carbonate, mica, and aluminum hydroxide. In particular, it is preferable to use carbon black in combination. The use of carbon black in combination can improve abrasion resistance. When carbon black is used in combination, the amount of carbon black is not particularly limited, but can be set to, for example, 5 to 20 parts by mass with respect to 100 parts by mass of the diene rubber.
[0040] In the rubber composition for tires, it is preferable to use a silane coupling agent in combination with the silica. By compounding the silane coupling agent, the dispersibility of the silica in the diene rubber can be improved. The type of silane coupling agent is not particularly limited as long as it can be used in a rubber composition containing silica, and examples of the silane coupling agent include sulfur-containing silane coupling agents such as bis-(3-triethoxysilylpropyl) tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, 3-trimethoxysilylpropyl benzothiazole tetrasulfide, γ-mercaptopropyl triethoxysilane, and 3-octanoylthiopropyl triethoxysilane. Among these, those having a tetrasulfide bond in the molecule can be preferably used. The compounding amount of the silane coupling agent is preferably less than 10% by mass, more preferably 6% to 9% by mass, based on the compounding amount of silica. If the amount of the silane coupling agent is 10% by mass or more of the amount of silica, the silane coupling agents will condense with each other, making it impossible to obtain the desired hardness and strength in the rubber composition.
[0041] Other compounding agents than those mentioned above can be added to the rubber composition of the present invention. Examples of other compounding agents include various compounding agents generally used in rubber compositions for tires, such as vulcanizing or crosslinking agents, vulcanization accelerators, antiaging agents, and liquid polymers. The compounding amounts of these compounding agents can be conventional general compounding amounts as long as they do not go against the object of the present invention. In addition, as the kneading machine, a normal rubber kneading machine, such as a Banbury mixer, a kneader, or a roll, can be used.
[0042] The rubber composition for tires is suitable for forming the tread portion of a tire, particularly the cap tread. A tire having a cap tread formed from the above-mentioned rubber composition has improved wet performance, low rolling resistance, and chipping resistance, and can achieve a good balance of these performances. In addition, the tire has excellent processability, and high quality tires can be stably produced.
[0043] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES
[0044] Rubber compositions for tires (Reference Example 1, Comparative Examples 1-8, Examples 1-12) were prepared having the common compounding agent recipe shown in Table 3 and the compositions shown in Tables 1-2. The manufacturing method thereof was to weigh out the compounding ingredients except for the vulcanization accelerator and sulfur, knead them in a 1.8 L internal Banbury mixer for 5 minutes, release the master batch, and cool at room temperature. Thereafter, the master batch was fed to a 1.8 L internal Banbury mixer, and the vulcanization accelerator and sulfur were added and mixed for 2 minutes to obtain each rubber composition for tires. The compounding amounts of the common compounding agents in Table 3 are parts by mass relative to 100 parts by mass of the diene rubber in Tables 1-2.
[0045] The Mooney viscosity of the obtained rubber composition for tires was measured by the following method. In addition, the rubber composition for tires was used to evaluate low rolling resistance, wet performance, and chipping resistance by the following methods.
[0046] Mooney Viscosity Mooney viscosity (ML) of rubber composition for tires 1+4 ) was measured in accordance with JIS K6300 using a Mooney viscometer with an L-type rotor under the conditions of a preheating time of 1 minute, a rotor rotation time of 4 minutes, a temperature of 100°C, and 2 rpm. The reciprocals of the obtained results were calculated and shown in the "Processability" column of Tables 1 and 2 as an index with Reference Example 1 being 100. A higher index indicates a lower Mooney viscosity and better processability.
[0047] Wet performance and low rolling resistance Each rubber composition for tires was used in a mold (inner dimensions: length 150 mm, width 150 mm, thickness 2 mm) of a predetermined shape, and vulcanized at 170°C for 10 minutes to prepare a vulcanized rubber test piece. Using this vulcanized rubber test piece, dynamic viscoelasticity was measured under conditions of initial strain 10%, amplitude ±2%, and frequency 20Hz using a viscoelasticity spectrometer manufactured by Toyo Seiki Seisakusho Co., Ltd., and tan δ was obtained at 0°C and 60°C. The results of tan δ at 0°C are shown in the "wet performance" column of Tables 1 to 2 as an index with the value of Reference Example 1 set to 100. The larger this index, the better the wet performance. In addition, the results of tan δ at 60°C were calculated by calculating the reciprocal of each, and shown in the "low rolling resistance" column of Tables 1 to 2 as an index with the value of Reference Example 1 set to 100. The larger this index, the better the low rolling resistance.
[0048] Chipping resistance A pneumatic tire (tire size: 265 / 60R18) was vulcanized using the obtained rubber composition for tires as a cap tread. The obtained pneumatic tire was mounted on a standard rim (rim size: 265 / 60R18), inflated to an air pressure of 250 kPa, mounted on a test vehicle, and driven 1000 km on an unpaved test road, after which the number of chippings that occurred in the tread was measured. The evaluation results were expressed as an index using the reciprocal of the measured value, with the value of Reference Example 1 being 100. The larger the index value, the fewer the number of chippings and the better the chipping resistance.
[0049] [Table 1]
[0050] [Table 2]
[0051] The types of raw materials used in Tables 1 and 2 are shown below. NR: Natural rubber, TSR20 (glass transition temperature Tg A :-75℃) SBR: Styrene butadiene rubber, Zeon Nipol NS612 (glass transition temperature Tg: -63℃) Silica: Solvay ZEOSIL 1165MP Thermoplastic resin 1: Aromatic modified terpene resin, YS Resin TO-125 manufactured by Yasuhara Chemical Co., Ltd., with an aromatic proton content of 12% Thermoplastic resin 2: C9 / hydrogenated DCPD resin, ENEOS T-REZ HA125, aromatic proton content 1% Thermoplastic resin 3: C9 petroleum resin, RT-95B manufactured by Shanghai Xuanda Processing Co., Ltd., aromatic proton content is 15% Thermoplastic resin 4: Hydrogenated DCPD resin, Hanwha HS-130, aromatic proton content 0% Thermoplastic resin 5: Rosin ester resin, Kraton Sylvatraxx 2097, aromatic proton content 4% Thermoplastic resin 6: C9 petroleum resin, ENEOS Neopolymer S100, aromatic proton content 37% Coupling agent: Silane coupling agent, Evonik Si69 Oil: Showa Shell Sekiyu Extract No. 4 S Ester plasticizer 1: Phosphate ester plasticizer, tris(2-ethylhexyl)phosphate, manufactured by Daihachi Chemical Industry Co., Ltd. Ester plasticizer 2: Aliphatic dibasic acid ester, bis(2-ethylhexyl) adipate, DOA manufactured by Daihachi Chemical Industry Co., Ltd. Ester plasticizer 3: Phthalate ester, di(2-ethylhexyl) phthalate, manufactured by New Japan Chemical Co., Ltd. Ester plasticizer 4: Trimellitic acid ester, trimellitic acid isononyl ester, manufactured by ADEKA Ether plasticizer: Ether plasticizer, Sofval P-0403N, NOF Corporation
[0052] [Table 3]
[0053] The types of raw materials used in Table 3 are shown below. Anti-aging agent: LANXESS VULKANOX 4020 Wax: NIPPON SEIRO OZOACE-0015A Sulfur: Sulfax 5 manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator: Noccela TOT-N manufactured by Ouchi Shinko Chemical Co., Ltd.
[0054] As is clear from Table 2, it was confirmed that the tire rubber compositions of Examples 1 to 14 maintain or improve wet performance, low rolling resistance, chipping resistance and processability compared to Reference Example 1, and achieve a good balance between these performance properties.
[0055] As is clear from Table 1, the rubber composition of Comparative Example 1 has a small amount of thermoplastic resin and does not contain ester-based plasticizer, and therefore has insufficient chipping resistance. The rubber composition of Comparative Example 2 contains a large amount of thermoplastic resin and does not contain ester-based plasticizer, and therefore the low rolling resistance is deteriorated. The rubber composition of Comparative Example 3 has a small amount of silica mixed therein, and therefore is deficient in wet performance. The rubber composition of Comparative Example 4 has a large amount of silica blended therein, and therefore the low rolling resistance is deteriorated. The rubber composition of Comparative Example 5 has insufficient chipping resistance due to the small amount of isoprene-based rubber. The rubber composition of Comparative Example 6 is insufficient in low rolling resistance and wet performance because the blending amount of the ester-based plasticizer is large. The rubber composition of Comparative Example 7, in which an ether-based plasticizer was blended in place of an ester-based plasticizer, did not sufficiently exhibit the effects of improving low rolling resistance and wet performance.
[0056] The present disclosure includes the following inventions. Invention [1] A rubber composition for tires, characterized by blending 100 parts by mass of diene rubber containing 50% by mass or more of isoprene-based rubber with 50 parts by mass or more and 150 parts by mass or less of silica, 16 parts by mass or more and 200 parts by mass or less of thermoplastic resin, and 10 parts by mass or less of an ester-based plasticizer. Invention [2] The rubber composition for tires according to invention [1], characterized in that the isoprene-based rubber is natural rubber. Invention [3] The rubber composition for tires according to invention [1] or [2], characterized in that the ester-based plasticizer is at least one selected from the group consisting of aliphatic dibasic acid esters, phosphate esters, phthalic acid esters, and trimellitic acid esters. Invention [4] The rubber composition for tires according to any one of inventions [1] to [3], characterized in that the thermoplastic resin is at least one selected from the group consisting of C5 petroleum resins, C9 petroleum resins, C5 / C9 petroleum resins, dicyclopentadiene resins, C5 / dicyclopentadiene resins, C9 / dicyclopentadiene resins, terpene resins, aromatic modified terpene resins, rosin resins, and hydrogenated resins thereof. Invention [5] A rubber composition for tires according to any one of inventions [1] to [4], characterized in that the thermoplastic resin is composed of units derived from aliphatic monomers and / or units derived from aromatic monomers, and has an aromatic proton content of 30% or less. [Explanation of symbols]
[0057] 1 Tread section 2 Sidewall 3 Bead section 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Belt cover layer 10 Tread rubber layer 11 Cap Tread 12 Undertread 20 Side rubber layer 30 Rim cushion rubber layer CL Tire Equator
Claims
1. A rubber composition for tires, comprising 100 parts by mass of diene rubber containing 50% by mass or more of isoprene-based rubber, 50 parts by mass or more and 150 parts by mass or less of silica, 16 parts by mass or more and 200 parts by mass or less of a thermoplastic resin, and 10 parts by mass or less of an ester-based plasticizer.
2. 2. The rubber composition for tires according to claim 1, wherein the isoprene-based rubber is a natural rubber.
3. 3. The rubber composition for tires according to claim 1, wherein the ester-based plasticizer is at least one selected from the group consisting of an aliphatic dibasic acid ester, a phosphate ester, a phthalate ester, and a trimellitate ester. Satisfying the relationship
4. 3. The rubber composition for tires according to claim 1, wherein the thermoplastic resin is at least one selected from the group consisting of C5 petroleum resins, C9 petroleum resins, C5 / C9 petroleum resins, dicyclopentadiene resins, C5 / dicyclopentadiene resins, C9 / dicyclopentadiene resins, terpene resins, aromatic modified terpene resins, rosin resins, and hydrogenated resins thereof.
5. 3. The rubber composition for tires according to claim 1, wherein the thermoplastic resin is composed of units derived from aliphatic monomers and / or units derived from aromatic monomers, and has an aromatic proton content of 30% or less.
Citation Information
Patent Citations
Steer-lock apparatus used for car
JP1985092986A
Cited By
Rubber compositions and articles thereof
EP4834600A1