Bonding material, method for producing bonding material, and method for producing bonding body
A tailored silver particle blend with controlled exothermic properties forms a robust, crack-free joint by drying and firing, addressing bonding defects and resinless cracking in silver-based bonding materials.
Patent Information
- Application Number
- JP2023071346
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Existing bonding materials using silver nanoparticles face issues such as rapid sintering leading to bonding defects like peeling, or high exothermic peak temperatures causing cracking without resin, which are not effectively addressed by current technologies.
A bonding material composed of specific size and exothermic peak temperature ranges of silver particles, blended in a particular ratio, and optionally with a solvent, is dried and fired to form a joint, suppressing cracking and bonding defects without substantial resin content.
The method ensures that the bonding material forms a strong, crack-free joint with improved bonding integrity, even under thermal stress, by controlling the sintering process effectively.
Smart Images

Figure 2024157172000010 
Figure 2024157172000011 
Figure 2024157172000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a bonding material, a method for manufacturing a bonding material, and a method for manufacturing a bonded body. [Background technology]
[0002] Silver has high thermal conductivity and a high melting point, so it is considered a promising raw material for a bonding material to replace solder when bonding conductive parts together. When using such a bonding material, the conductive parts to be bonded are stacked together via a bonding material containing silver, and the bonding material is fired to bond these conductive parts together. When fired, the bonding material forms a bond whose main component is sintered silver.
[0003] For example, a known bonding material contains silver particles and resin. However, resin functions as a binder and disappears during firing, so it is a component that should not be used. Despite this, resin is used in order to increase the bonding strength at the joint.
[0004] In contrast, as a bonding material that can be formed without containing resin, a bonding material containing silver nanoparticles having an average particle size of 200 to 600 nm and an exothermic peak temperature observed by simultaneous thermogravimetry and differential thermal analysis (TG / DTA) of less than 175°C has been disclosed (see Patent Document 1). Also disclosed is a bonding material containing sintered silver particles having an average particle size of 0.1 to 10 μm and an exothermic peak temperature observed by simultaneous thermogravimetry and differential thermal analysis of 175°C to 235°C (see Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 7120314 [Patent Document 2] Patent No. 6713182 Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the bonding material described in Patent Document 1 is used, the heat peak temperature of the silver nanoparticles is relatively low, which tends to cause the sintering of the silver nanoparticles to proceed rapidly, and the resulting bond (in other words, the silver sintered body) can suffer from bonding defects such as peeling off from the objects to be bonded. On the other hand, when the bonding material described in Patent Document 2 was used, the heat peak temperature of the silver nanoparticles was relatively high, and the bonding material was easily affected by the fact that it did not contain resin, and cracks sometimes occurred in the dried bonding material (dried bonding material).
[0007] The present invention provides a bonding material for forming a joint that joins conductive parts together and a manufacturing method thereof, in which the bonding material is dried and then fired to form the joint, thereby suppressing cracking of the dried bonding material and suppressing poor bonding at the joint, even if the bonding material does not substantially contain resin, and a manufacturing method thereof. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention employs the following configuration. [1] A method for manufacturing a bonding material for bonding conductive parts, comprising: The production method includes a blending step of blending silver particles (A) and silver particles (B), the silver particles (A) have a 50% cumulative particle size on a volume basis of 0.2 to 0.5 μm, as measured by a laser diffraction / scattering particle size distribution analyzer; when an exothermic peak of the silver particles (A) is observed by simultaneous differential thermal and thermogravimetric analysis, if only one exothermic peak is observed, the temperature of the exothermic peak is 210 to 225°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 210 to 225°C, the silver particles (B) have a volume-based 50% cumulative particle size of 0.2 to 0.7 μm, as measured by a laser diffraction / scattering particle size distribution analyzer; when an exothermic peak of the silver particles (B) is observed by simultaneous differential thermal and thermogravimetric analysis, if only one exothermic peak is observed, the temperature of the exothermic peak is 168 to 180°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 168 to 180°C, a temperature of the exothermic peak is 183 to 224°C when only one exothermic peak is observed, and a maximum temperature of the exothermic peak is 183 to 224°C when two or more exothermic peaks are observed, when an exothermic peak of a mixture of silver particles (A) and silver particles (B) in the same amounts as those in the blending step is observed by simultaneous differential thermal and thermogravimetry measurement.
[0009] [2] The method for producing a bonding material according to [1], wherein a ratio of a blending amount of the silver particles (B) to a total blending amount of the silver particles (A) and the silver particles (B) is 20 to 50 mass %. [3] A bonding material for bonding conductive parts together, the bonding material comprising silver particles and a solvent, the silver particles having a particle size at 50% cumulative volume of 0.2 to 0.7 μm as measured by laser diffraction / scattering particle size distribution measurement, an exothermic peak of the silver particles is observed by simultaneous differential thermal and thermogravimetric measurement, and when only one exothermic peak is observed, the temperature of the exothermic peak is 183 to 224° C., and when two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 183 to 224° C., and the solvent is one or more selected from the group consisting of ethylene glycol mono(2-ethylhexyl) ether, ethylene glycol monohexyl ether, and Texanol.
[0010] [4] A method for producing a bonded body, comprising the steps of: the joined body is configured by joining a conductive first component and a conductive second component via a conductive joint, The manufacturing method includes a step of attaching a bonding material manufactured by the manufacturing method described in [1] or [2] to a surface of one of the first component and the second component; drying the applied bonding material to form a dried bonding material; laminating the first component and the second component with the dried bonding material interposed therebetween to produce a laminate; and forming the bonded portion from the dried bonding material by firing the dried bonding material in the laminate at a temperature higher than a temperature at which the bonding material was dried. Effect of the Invention
[0011] According to the present invention, there is provided a bonding material for forming a joint that joins conductive parts together and a manufacturing method thereof, in which the bonding material is dried and then fired, so that when the joint is formed, cracking of the dried bonding material is suppressed even if the bonding material does not substantially contain resin, and poor bonding at the joint is suppressed. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view showing a schematic example of a bonded body to which a manufacturing method according to an embodiment of the present invention is applied; [Diagram 2] 1A to 1C are cross-sectional views for illustrating an example of a method for producing a bonded body according to an embodiment of the present invention. [Diagram 3] 5A to 5C are cross-sectional views for illustrating a schematic diagram of another example of the method for producing a bonded body according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] ◇ Manufacturing method of bonding material A method for producing a bonding material according to one embodiment of the present invention is a method for producing a bonding material for bonding conductive parts together, the method including a blending step of blending silver particles (A) and silver particles (B), the silver particles (A) have a 50% cumulative volumetric particle diameter (sometimes referred to as "D50" in this specification) of 0.2 to 0.5 μm, as measured by a laser diffraction / scattering particle size distribution analyzer; when an exothermic peak of the silver particles (A) is observed by simultaneous differential thermal and thermogravimetric analysis (sometimes referred to herein as "TG / DTA"), if only one exothermic peak is observed, the temperature of the exothermic peak is 210 to 225°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 210 to 225°C, the silver particles (B) have a 50% cumulative volume particle size (D50) of 0.2 to 0.7 μm, as measured by a laser diffraction / scattering particle size distribution analyzer; when an exothermic peak of the silver particles (B) is observed by simultaneous thermogravimetry and differential thermal analysis (TG / DTA), if only one exothermic peak is observed, the temperature of the exothermic peak is 168 to 180°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 168 to 180°C; When an exothermic peak of a mixture of silver particles (A) and silver particles (B) in the same amount as the blending amount in the blending step (sometimes referred to in this specification as a "silver particle mixture") is observed by simultaneous differential thermal and thermogravimetry (TG / DTA), if only one exothermic peak is observed, the temperature of the exothermic peak is 183 to 224°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 183 to 224°C.
[0014] According to the manufacturing method of this embodiment, by blending silver particles (A) and silver particles (B) whose D50 and exothermic peak temperature are both within specific ranges, a bonding material is obtained, which is dried and then fired, and thus a bonding material is obtained that suppresses cracking of the dried bonding material when a bond is formed, even if the bonding material does not substantially contain resin, and thus suppresses bonding failure at the bond.
[0015] In this specification, the bonding material being substantially free of resin means that the bonding material does not contain any resin at all, or that although it contains resin, the amount of resin is so small that the effect of the resin inclusion is not noticeable in the bonding material.
[0016] In the blending step of the production method of this embodiment, the ratio of the total blend amount of one or more blend components described below to the total mass of the blended components does not exceed 100 mass %.
[0017] ◎Blending process <<Silver particles (A)>> The D50 of the silver particles (A) is 0.2 to 0.5 μm, and may be, for example, any one of 0.2 to 0.4 μm, 0.4 to 0.5 μm, and 0.35 to 0.45 μm. When the D50 of the silver particles (A) is in such a range, cracks in the dried bonding material are further suppressed, and a bonding material in which bonding defects at the bonded parts are further suppressed can be obtained.
[0018] The particle size at 90% cumulative volume of the silver particles (A) measured by laser diffraction / scattering particle size distribution measurement (sometimes referred to as "D90" in this specification) is not particularly limited, but is preferably 1 μm or less, and may be, for example, any one of 0.95 μm or less, 0.85 μm or less, 0.75 μm or less, and 0.65 μm or less. When the D90 of the silver particles (A) is in such a range, cracking of the dried bonding material is further suppressed. On the other hand, the D90 of the silver particles (A) is preferably 0.45 μm or more, and may be, for example, 0.7 μm or more. Such silver particles (A) can be more easily prepared or obtained. In one embodiment, the D90 of the silver particles (A) may be, for example, any one of 0.45 to 1 μm, 0.45 to 0.95 μm, 0.45 to 0.85 μm, 0.45 to 0.75 μm, and 0.45 to 0.65 μm, or any one of 0.7 to 1 μm, 0.7 to 0.95 μm, and 0.7 to 0.85 μm, although these are only examples of the D90 of the silver particles (A).
[0019] The particle size of the silver particles (A) at 10% cumulative volume measured by laser diffraction / scattering particle size distribution measurement (sometimes referred to as "D10" in this specification) is not particularly limited, but is preferably 0.08 μm or more, and may be, for example, any of 0.2 μm or more and 0.25 μm or more. When the D10 of the silver particles (A) is in such a range, cracking of the dried bonding material is further suppressed. On the other hand, D10 of the silver particles (A) is preferably 0.3 μm or less, and may be, for example, 0.27 μm or less. Such silver particles (A) can be more easily prepared or obtained. In one embodiment, D10 of the silver particles (A) may be, for example, any one of 0.08 to 0.3 μm, 0.2 to 0.3 μm, and 0.25 to 0.3 μm, or any one of 0.08 to 0.27 μm and 0.2 to 0.27 μm, although these are just examples of D10 of the silver particles (A).
[0020] When the exothermic peak of silver particles (A) is observed by simultaneous thermogravimetry and differential thermal analysis (TG / DTA), there are cases where only one exothermic peak is observed, and cases where two or more exothermic peaks are observed. In this embodiment, when only one exothermic peak is observed for silver particles (A), silver particles (A) having a temperature showing the exothermic peak (exothermic peak temperature) of 210 to 225°C are used, and when two or more exothermic peaks are observed for silver particles (A), silver particles (A) having the highest temperature among the temperatures showing the exothermic peaks (exothermic peak temperatures) of 210 to 225°C are used. By using such silver particles (A) in combination with silver particles (B) described later, the bonding material becomes equivalent to one containing silver particles having an exothermic peak temperature of 183 to 224°C described later.
[0021] The exothermic peak temperature of the silver particles (A) may be, for example, any one of 217 to 225°C and 210 to 218°C.
[0022] The exothermic peak temperature of the silver particles (A) can be adjusted, for example, by adjusting the type and amount of a surface treatment agent for the silver particles (A) described below, the specific surface area of the silver particles (A), etc.
[0023] The specific surface area of the silver particles (A) is not particularly limited, but is preferably 1.15 to 3.6 m 2 / g, for example, 1.15 to 3.2 m 2 / g, and 1.15 to 2m 2 / g or 1.2 to 3.6 m 2 / g, and 2 to 3.6 m 2 / g or 1.2 to 3.2 m 2 When the specific surface area of the silver particles (A) is within this range, cracks in the dried bonding material are further suppressed, and a bonding material in which bonding defects at the bonded portion are further suppressed can be obtained.
[0024] The specific surface area of particles, including that of silver particles (A), can be measured by known methods such as a permeation method or a gas adsorption method using gas molecules such as nitrogen.
[0025] The silver particles (A) preferably have a substantially spherical shape. As the approximately spherical silver particles (A), any commercially available product having a spherical or approximately spherical shape can be used as long as it satisfies the above-mentioned conditions of D50 and exothermic peak temperature.
[0026] In this specification, the term "approximately spherical" refers not only to silver particles (A) but also to a shape that is spherical or can be considered as spherical, and more specifically, refers to a particle shape in which the aspect ratio calculated by [major axis of particle] / [minor axis of particle] is 2 or less. The aspect ratio is preferably 1.6 or less, and more preferably 1.3 or less. The surface of a particle that is approximately spherical may be composed of only curved surfaces, or may have flat surfaces, or may have corners formed by two flat surfaces connected to each other at a predetermined angle. The surface of a particle that is approximately spherical may be smooth or may have uneven portions.
[0027] The silver particles (A) preferably satisfy one or more of the above-mentioned conditions, and more preferably satisfy all of them. An example of a more preferred silver particle (A) is one in which D50 is 0.4 to 0.5 μm, D90 is 0.7 to 1 μm, and D10 is 0.2 to 0.27 μm; if only one exothermic peak is observed for the silver particles (A), the temperature showing the exothermic peak (exothermic peak temperature) is 210 to 225° C.; if two or more exothermic peaks are observed for the silver particles (A), the highest temperature among the temperatures showing the exothermic peaks (exothermic peak temperatures) is 210 to 225° C.; and the specific surface area is 1.15 to 3.2 m. 2 / g and has a substantially spherical shape.
[0028] Examples of the silver particles (A) include silver particles obtained by a reduction method and silver particles obtained by an atomization method. The silver particles (A) may be surface-treated products whose surfaces have been chemically treated (treated with a chemical substance), or they may be surface-untreated products whose surfaces have not been chemically treated. Generally, silver particles (A) obtained by the reduction method are surface-treated, while silver particles (A) obtained by the atomization method are surface-untreated.
[0029] Examples of the surface treatment agent (the chemical substance) for the silver particles (A) include lubricants such as 2-ethylhexylamine, and surface protective agents such as saturated fatty acids and saturated fatty acid salts. The saturated fatty acids may be, for example, low-molecular-weight saturated fatty acids.
[0030] In the blending step, the ratio of the amount of silver particles (A) to the total amount of components other than the solvent ([amount of silver particles (A) in the blending step (parts by mass)] / [total amount of components other than the solvent in the blending step (parts by mass)] × 100) is preferably 45 to 85 mass%, and may be, for example, any of 55 to 85 mass% and 65 to 85 mass%, any of 45 to 75 mass% and 45 to 65 mass%, or may be 55 to 75 mass%. When the ratio is in such a range, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonded portion are further suppressed can be obtained.
[0031] <<Silver particles (B)>> The D50 of the silver particles (B) is 0.2 to 0.7 μm, preferably 0.2 to 0.68 μm, and may be, for example, any one of 0.2 to 0.55 μm, 0.45 to 0.68 μm, and 0.4 to 0.6 μm. When the D50 of the silver particles (B) is in such a range, cracks in the dried bonding material are further suppressed, and a bonding material in which bonding defects at the bonded parts are further suppressed can be obtained.
[0032] The D90 of the silver particles (B) is not particularly limited, but is preferably 1.05 μm or less, and may be, for example, either 0.85 μm or less or 0.65 μm or less. When the D90 of the silver particles (B) is in such a range, cracks in the dried bonding material are further suppressed. On the other hand, D90 of silver particles (B) is preferably 0.4 μm or more, and may be, for example, 0.7 μm or more. Such silver particles (B) can be more easily prepared or obtained. In one embodiment, D90 of silver particles (B) may be, for example, any one of 0.4 to 1.05 μm, 0.4 to 0.85 μm, and 0.4 to 0.65 μm, or any one of 0.7 to 1.05 μm and 0.7 to 0.85 μm, although these are only examples of D90 of silver particles (B).
[0033] D10 of the silver particles (B) is not particularly limited, but is preferably 0.1 μm or more, and may be, for example, 0.2 μm or more or 0.3 μm or more. When D10 of the silver particles (B) is in such a range, cracking of the dried bonding material is further suppressed. On the other hand, D10 of silver particles (B) is preferably 0.45 μm or less, and may be, for example, 0.35 μm or less. Such silver particles (B) can be more easily prepared or obtained. In one embodiment, D10 of silver particles (B) may be, for example, any one of 0.1 to 0.45 μm, 0.2 to 0.45 μm, and 0.3 to 0.45 μm, or any one of 0.1 to 0.35 μm and 0.2 to 0.35 μm, although these are only examples of D10 of silver particles (B).
[0034] When the exothermic peak of silver particles (B) is observed by simultaneous thermogravimetry and differential thermal analysis (TG / DTA), there are cases where only one exothermic peak is observed, and cases where two or more exothermic peaks are observed. In this embodiment, when only one exothermic peak of silver particles (B) is observed, silver particles (B) having a temperature showing the exothermic peak (exothermic peak temperature) of 168 to 180°C are used, and when two or more exothermic peaks of silver particles (B) are observed, silver particles (B) having the highest temperature among the temperatures showing the exothermic peaks (exothermic peak temperatures) of 168 to 180°C are used. By using such silver particles (B) in combination with silver particles (A), the bonding material becomes equivalent to one containing silver particles having an exothermic peak temperature of 183 to 224°C, which will be described later.
[0035] The exothermic peak temperature of the silver particles (B) may be, for example, any one of 168 to 174°C and 173 to 180°C.
[0036] The exothermic peak temperature of silver particles (B) can be adjusted, for example, by adjusting the type and amount of a surface treatment agent for silver particles (B) described below, the specific surface area of silver particles (B), etc.
[0037] The specific surface area of the silver particles (B) is not particularly limited, but is preferably 1.1 to 3 m 2 / g, for example, 1.1 to 2.5 m 2 / g, and 1.1 to 1.9 m 2 / g or 1.5 to 3m 2 / g, and 2.2 to 3 m 2 When the specific surface area of the silver particles (B) is in this range, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonding portion are further suppressed can be obtained.
[0038] The shape of the silver particles (B) is preferably approximately spherical, that is, the shape of the silver particles (B) is preferably spherical or can be regarded as spherical. As the approximately spherical silver particles (B), any commercially available product having a spherical or approximately spherical shape can be used as long as it satisfies the above-mentioned conditions of D50 and exothermic peak temperature.
[0039] The silver particles (B) preferably satisfy one or more of the above-mentioned conditions, and more preferably satisfy all of them. An example of a more preferable silver particle (B) is one in which D50 is 0.2 to 0.68 μm, D90 is 0.4 to 1.05 μm, and D10 is 0.1 to 0.45 μm, and when only one exothermic peak is observed for silver particles (B), the temperature showing the exothermic peak (exothermic peak temperature) is 168 to 180° C., and when two or more exothermic peaks are observed for silver particles (B), the highest temperature among the temperatures showing the exothermic peaks (exothermic peak temperatures) is 168 to 180° C., and the specific surface area is 1.1 to 3 m. 2 / g and has a substantially spherical shape.
[0040] As in the case of the silver particles (A), examples of the silver particles (B) include silver particles obtained by a reduction method and silver particles obtained by an atomization method. The silver particles (B), like the silver particles (A), may be surface-treated or surface-untreated. Usually, silver particles (B) obtained by the reduction method are surface-treated, while silver particles (B) obtained by the atomization method are surface-untreated.
[0041] Examples of the surface treatment agent (the above-mentioned chemical substance) for the silver particles (B) include surface protective agents such as polycyclic fatty acids (in other words, branched-chain fatty acids).
[0042] In the blending step, the ratio of the amount of silver particles (B) to the total amount of silver particles (A) and silver particles (B) ([amount of silver particles (B) in the blending step (parts by mass)] / ([amount of silver particles (A) in the blending step (parts by mass)]+[amount of silver particles (B) in the blending step (parts by mass)])×100) is preferably 20 to 50 mass%, and may be, for example, any of 20 to 45 mass%, 20 to 37 mass%, and 20 to 32 mass%, any of 25 to 50 mass%, 33 to 50 mass%, and 38 to 50 mass%, or any of 25 to 45 mass% and 33 to 37 mass%. When the ratio is in such a range, it becomes easier to adjust the exothermic peak temperature of the silver particle mixture to 183 to 224° C. For example, when the ratio is equal to or more than the lower limit, the exothermic peak temperature of the silver particle mixture is lowered, making it easier for the silver particles (silver particles (A) and silver particles (B)) to be sintered.
[0043] <<Silver particle mixture>> When the exothermic peak of a mixture of the silver particles (A) in the same amount as that in the blending step and the silver particles (B) in the same amount as that in the blending step (i.e., the silver particle mixture) is observed by simultaneous differential thermal analysis / thermogravimetry (TG / DTA), only one exothermic peak is observed, or two or more exothermic peaks are observed. In this embodiment, when only one exothermic peak is observed for the silver particle mixture, the temperature showing the exothermic peak (exothermic peak temperature) is 183 to 224°C, and when two or more exothermic peaks are observed for the silver particle mixture, the highest temperature among the temperatures showing the exothermic peaks (exothermic peak temperatures) is 183 to 224°C. When the exothermic peak temperature of the silver particle mixture is within this range, cracking of the dried bonding material is suppressed, and a bonding material in which bonding defects at the bonded portion are suppressed can be obtained.
[0044] The exothermic peak temperature of the silver particle mixture may be, for example, any one of 183 to 198°C, 196 to 211°C, and 209 to 224°C. The lower the exothermic peak temperature of the silver particle mixture, the easier it is to sinter the silver particles (silver particles (A) and silver particles (B)).
[0045] The exothermic peak pattern of the silver particle mixture does not necessarily result from the sum of the exothermic peak pattern of silver particles (A) and the exothermic peak pattern of silver particles (B), but depends on the respective amounts of silver particles (A) and silver particles (B) mixed. In the blending step, the blending amounts of silver particles (A) and silver particles (B) can be adjusted so that the exothermic peak temperature of the silver particle mixture is 183 to 224°C.
[0046] The D50 of the silver particles in the silver particle mixture is preferably 0.2 to 0.7 μm, and may be, for example, any one of 0.2 to 0.4 μm, 0.35 to 0.55 μm, and 0.5 to 0.7 μm. When the D50 of the silver particles in the silver particle mixture is in such a range, cracks in the dried bonding material are further suppressed, and bonding defects at the bonding portion are further suppressed.
[0047] The D90 of the silver particles in the silver particle mixture is not particularly limited, but is preferably 1.05 μm or less, and may be, for example, either 0.85 μm or less or 0.65 μm or less. When the D90 of the silver particles in the silver particle mixture is in such a range, cracking of the dried bonding material is further suppressed. On the other hand, the D90 of the silver particles in the silver particle mixture is preferably 0.4 μm or more, and may be, for example, 0.7 μm or more. Such a silver particle mixture can be more easily prepared or obtained. In one embodiment, the D90 of the silver particles in the silver particle mixture may be, for example, any one of 0.4 to 1.05 μm, 0.4 to 0.85 μm, and 0.4 to 0.65 μm, or any one of 0.7 to 1.05 μm and 0.7 to 0.85 μm, although these are only examples of the D90 of the silver particles in the silver particle mixture.
[0048] The D10 of the silver particles in the silver particle mixture is not particularly limited, but is preferably 0.08 μm or more, and may be, for example, 0.2 μm or more or 0.3 μm or more. When the D10 of the silver particles in the silver particle mixture is in such a range, cracking of the dried bonding material is further suppressed. On the other hand, the D10 of the silver particles in the silver particle mixture is preferably 0.45 μm or less, and may be, for example, 0.35 μm or less. Such a silver particle mixture can be more easily prepared or obtained. In one embodiment, the D10 of the silver particles in the silver particle mixture may be, for example, any one of 0.08 to 0.45 μm and 0.08 to 0.35 μm, or any one of 0.2 to 0.45 μm and 0.2 to 0.35 μm, although these are only examples of the D10 of the silver particles in the silver particle mixture.
[0049] The specific surface area of the silver particles in the silver particle mixture is not particularly limited, but is preferably 1.1 to 3.6 m 2 / g, for example, 1.1 to 3.2 m 2 / g, and 1.1 to 2 m 2 / g or 1.2 to 3.6 m 2 / g, and 2 to 3.6 m 2 / g or 1.2 to 3.2 m 2 When the specific surface area of the silver particles in the silver particle mixture is in this range, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonding portion are further suppressed can be obtained.
[0050] <<Solvent (S)>> In the blending step, it is preferable to further blend a solvent (S). The bonding material obtained by blending the solvent (S) has fluidity and good handleability due to the inclusion of the solvent (S). The bonding material is typically in a paste or liquid form.
[0051] In this specification, the term "solvent" is not limited to the solvent (S), and unless otherwise specified, is a concept that encompasses both a component that is liquid at room temperature and that dissolves a solute, and a component that is liquid at room temperature and that functions as a dispersion medium for dispersing a dispersoid. In this specification, "room temperature" means a temperature that is neither particularly cooled nor heated, that is, an ordinary temperature, and examples thereof include temperatures of 15 to 25°C.
[0052] The solvent (S) is not particularly limited as long as it can be removed (vaporized) under heating conditions, but it is preferable that the solvent has a boiling point of 200 to 265° C. A solvent (S) having a boiling point of 200° C. or more is difficult to vaporize when handled at room temperature, and therefore the composition of a bonding material containing such a solvent (S) is stabilized. On the other hand, a solvent (S) having a boiling point of 265° C. or less can be relatively easily removed under heating conditions, and therefore, by using a bonding material containing such a solvent (S), a dried bonding material can be more easily formed.
[0053] Preferred examples of the solvent (S) include alcohol ethers having a boiling point of 200 to 265° C. (i.e., compounds having both a hydroxyl group (-OH) and an ether bond (-O-) in one molecule); and alcohol esters having a boiling point of 200 to 265° C. (i.e., compounds having both a hydroxyl group (-OH) and an ester bond in one molecule). The alcohol ester is preferably an alcohol carboxylate (that is, a compound having both a hydroxyl group (-OH) and a carboxylate bond (-C(=O)-O-) in one molecule). Preferred examples of the alcohol ether include ethylene glycol mono(2-ethylhexyl) ether (boiling point: about 228.6° C.) and ethylene glycol monohexyl ether (boiling point: about 208.3° C.). A preferred example of the alcohol ester is texanol (boiling point: about 255 to 260° C.).
[0054] The solvent (S) to be blended in the blending step may be one type only, or two or more types may be blended. When two or more types are blended, the combination and ratio thereof can be selected arbitrarily.
[0055] The solvent (S) to be blended in the blending step is preferably one or more selected from the group consisting of ethylene glycol mono(2-ethylhexyl) ether, ethylene glycol monohexyl ether, and Texanol.
[0056] When a solvent (S) is blended in the blending step, the ratio of the blending amount of the solvent (S) to the total blending amount of silver particles (A) and silver particles (B) ([blend amount of solvent (S) in the blending step (parts by mass)] / ([blend amount of silver particles (A) in the blending step (parts by mass)]+[blend amount of silver particles (B) in the blending step (parts by mass)])×100) is preferably 10 to 17% by mass, and may be, for example, any one of 10 to 14.5% by mass, 10 to 13.5% by mass, and 10 to 12.5% by mass, any one of 12.5 to 17% by mass, 13.5 to 17% by mass, and 14.5 to 17% by mass, or may be 12.5 to 14.5% by mass. When the ratio is equal to or more than the lower limit, the effect obtained by using the solvent (S) is enhanced. When the ratio is equal to or less than the upper limit, excessive use of the solvent (S) is suppressed.
[0057] <<Other Ingredients>> In the blending step, a component other than silver particles (A), silver particles (B), or a solvent (S) may or may not be blended within a range that does not impair the effects of the present invention. The other components are not particularly limited as long as they do not impair the effects of the present invention, and can be arbitrarily selected depending on the purpose.
[0058] The other components to be blended in the blending step may be one type only, or two or more types. When two or more types are used, the combination and ratio thereof can be selected arbitrarily.
[0059] Examples of the other component to be blended in the blending step include silver particles (C) that do not fall into the category of silver particles (A) or silver particles (B) and additive (Z).
[0060] <Silver particles (C)> The silver particles (C) are not particularly limited as long as they are not classified as silver particles (A) or silver particles (B). Examples of the silver particles (C) include: Silver particles having at least a D50 outside the range of 0.2 to 0.7 μm (less than 0.2 μm or more than 0.7 μm); silver particles in which, when at least one exothermic peak is observed by simultaneous thermogravimetry and differential thermal analysis (TG / DTA), the temperature of the exothermic peak is outside the ranges of 168 to 180°C and 210 to 225°C (less than 168°C, more than 180°C and less than 210°C, or more than 225°C), and, when two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is outside the ranges of 168 to 180°C and 210 to 225°C (less than 168°C, more than 180°C and less than 210°C, or more than 225°C); etc.
[0061] In the blending step, the ratio of the blending amount of silver particles (C) to the total blending amount of silver particles (A) and silver particles (B) ([blend amount (parts by mass) of silver particles (C) in the blending step)] / ([blend amount (parts by mass) of silver particles (A) in the blending step)]+[blend amount (parts by mass) of silver particles (B) in the blending step)])×100) is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less. When the ratio is equal to or less than the upper limit, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonded parts are further suppressed can be obtained. On the other hand, the ratio is 0% by mass or more.
[0062] <Additives (Z)> Examples of the additive (Z) include branched carboxylic acids (i.e., carboxylic acids having a branched hydrocarbon group), acetylene alcohols (i.e., compounds having both a hydroxyl group (-OH) and a triple bond between carbon atoms (-C≡C-) in one molecule, provided that the hydroxyl group is not bonded to the carbon atom forming the triple bond), and the like.
[0063] The branched carboxylic acid may be either a monobasic carboxylic acid or a dibasic or higher polybasic carboxylic acid, but is preferably a monobasic carboxylic acid. The branched carboxylic acid preferably has 7 to 9 carbon atoms. The branched carboxylic acid is preferably 3,5,5-trimethylhexanoic acid.
[0064] The acetylene alcohol may be either a monohydric alcohol (alcohol having one hydroxyl group) or a dihydric or higher polyhydric alcohol (alcohol having two hydroxyl groups), but is preferably a monohydric alcohol. The acetylene alcohol preferably has 8 to 10 carbon atoms. The acetylenic alcohol is preferably 4-ethyl-1-octyn-3-ol or 3,5-dimethyl-1-hexyn-3-ol.
[0065] The additive (Z) to be blended in the blending step may be one type only, or may be two or more types. When two or more types are used, the combination and ratio thereof can be selected arbitrarily.
[0066] When additive (Z) is blended in the blending step, the ratio of the blending amount of additive (Z) to the total blending amount of silver particles (A) and silver particles (B) ([blend amount of additive (Z) in the blending step (parts by mass)] / ([blend amount of silver particles (A) in the blending step (parts by mass)]+[blend amount of silver particles (B) in the blending step (parts by mass)])×100) is preferably 0.5 to 8 mass%, and may be, for example, any of 0.5 to 4 mass% and 0.5 to 2 mass%, or may be 2 to 8 mass%. When the ratio is equal to or more than the lower limit, the effect obtained by using additive (Z) is enhanced. When the ratio is equal to or less than the upper limit, excessive use of additive (Z) is suppressed.
[0067] <Other components (Y) that do not fall under either silver particles (C) or additives (Z)> When a component (Y) other than silver particles (C) or additive (Z) is blended in the blending step, the component (Y) to be blended may be one type, or two or more types. When the component (Y) is two or more types, the combination and ratio thereof can be selected arbitrarily. In the blending step, the ratio of the blending amount of the other component (Y) to the total blending amount of the silver particles (A) and the silver particles (B) ([blend amount (parts by mass) of the other component (Y) in the blending step)] / ([blend amount (parts by mass) of the silver particles (A) in the blending step)]+[blend amount (parts by mass) of the silver particles (B) in the blending step)])×100) is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less. When the ratio is equal to or less than the upper limit, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonded parts are further suppressed can be obtained. On the other hand, the ratio is 0% by mass or more.
[0068] In the blending step, the ratio of the total amount of silver particles (A), silver particles (B), solvent (S), and additive (Z) to the total mass of the blended components ((([amount of silver particles (A) in the blending step (parts by mass)]+[amount of silver particles (B) in the blending step (parts by mass)]+[amount of solvent (S) in the blending step (parts by mass)]+[amount of additive (Z) in the blending step (parts by mass)]) / [total mass of components in the blending step (parts by mass)]×100) is preferably 95% by mass or more, more preferably 97% by mass or more, and even more preferably 99% by mass or more. The higher the ratio, the more cracks are suppressed in the dried bonding material, and the more a bonding material in which bonding defects at the bonded parts are suppressed can be obtained. On the other hand, the proportion is 100% by mass or less.
[0069] In the blending step, the ratio of the total amount of silver particles (A) and silver particles (B) to the total mass of the components other than the solvent (S) (([amount of silver particles (A) in the blending step (parts by mass)]+[amount of silver particles (B) in the blending step (parts by mass)]) / [total mass of components other than the solvent (S) in the blending step (parts by mass)]×100) is preferably 90 to 100 mass%, and may be, for example, any one of 93 to 100 mass%, 96 to 100 mass%, and 98 to 100 mass%. When the ratio is in such a range, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonded parts are further suppressed can be obtained.
[0070] <<Other conditions for the compounding process>> In the blending step, the order in which the silver particles (A), the silver particles (B), and, if necessary, the other components are blended is not particularly limited. For example, when silver particles (A) and silver particles (B) are blended, they may be blended separately, or a mixture obtained by mixing them may be blended.
[0071] The method for mixing the blend is not particularly limited, and may be appropriately selected from known methods such as a method for mixing by rotating a stirrer or agitator blades, etc.; a method for mixing using a mixer, a three-roll mill, a kneader, a bead mill, etc.; a method for mixing by applying ultrasonic waves, etc.
[0072] The temperature at which each component is mixed is not particularly limited as long as the components do not deteriorate, but a temperature of 0 to 40°C is preferable. The blending time of each component is not particularly limited as long as each blended component does not deteriorate, but it is preferably 10 minutes to 12 hours.
[0073] ◎Other processes The manufacturing method of this embodiment may include other steps in addition to the blending step, as long as the effects of the present invention are not impaired. The other steps may be one type only, or two or more types, and when there are two or more types, the combination thereof can be arbitrarily selected. The timing of performing the other steps can be arbitrarily selected depending on the type of the other steps.
[0074] The bonding material obtained by the manufacturing method of this embodiment is dried, and the dried bonding material thus obtained is fired in a state where the conductive parts are in contact with each other separately, thereby forming a conductive bonding part, which can bond the conductive parts together. At this time, even if the bonding material does not substantially contain resin, cracking of the dried bonding material is suppressed, and bonding failure at the bonding part is suppressed.
[0075] ◇Joining material A bonding material according to one embodiment of the present invention is a bonding material for bonding conductive parts together, the bonding material containing silver particles (X) and a solvent, the silver particles (X) have a 50% cumulative volume particle size (D50) of 0.2 to 0.7 μm, as measured by a laser diffraction / scattering particle size distribution measurement; when an exothermic peak of the silver particles (X) is observed by simultaneous thermogravimetry and differential thermal analysis (TG / DTA), if only one exothermic peak is observed, the temperature of the exothermic peak is 183 to 224°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 183 to 224°C; The solvent is one or more selected from the group consisting of ethylene glycol mono(2-ethylhexyl) ether, ethylene glycol monohexyl ether, and Texanol.
[0076] By using the bonding material of this embodiment and drying and then firing it, cracking of the dried bonding material is suppressed when forming the joint, even if the bonding material does not substantially contain resin, and poor bonding at the joint is suppressed.
[0077] <<Silver particles (X)>> The silver particles (X) contained in the bonding material of the present embodiment are not particularly limited as long as their D50 and exothermic peak temperature satisfy the above conditions. For example, the silver particles (X) may be a single particle or a mixture of two or more kinds of silver particles. The mixture of two or more kinds of silver particles may be a mixture of silver particles (A) and silver particles (B) used in the manufacturing method of a bonding material according to one embodiment of the present invention (i.e., the silver particle mixture).
[0078] The bonding material of this embodiment may include the bonding material obtained by the manufacturing method according to one embodiment of the present invention described above.
[0079] In the bonding material, the ratio of the total content of one or more of the components contained in the bonding material, which will be described later, to the total mass of the bonding material does not exceed 100 mass %.
[0080] The silver particles (X) have a D50 of 0.2 to 0.7 μm, and may be, for example, any one of 0.2 to 0.4 μm, 0.35 to 0.55 μm, and 0.5 to 0.7 μm. When the silver particles (X) have a D50 in such a range, cracks in the dried bonding material are further suppressed, and bonding defects at the bonded parts are further suppressed.
[0081] The D90 of the silver particles (X) is not particularly limited, but is preferably 1.05 μm or less, and may be, for example, either 0.85 μm or less or 0.65 μm or less. When the D90 of the silver particles (X) is in such a range, cracks in the dried bonding material are further suppressed. On the other hand, the D90 of the silver particles (X) is preferably 0.4 μm or more, and may be, for example, 0.7 μm or more. Such silver particles (X) can be more easily prepared or obtained. In one embodiment, the D90 of the silver particles (X) may be, for example, any one of 0.4 to 1.05 μm, 0.4 to 0.85 μm, and 0.4 to 0.65 μm, or any one of 0.7 to 1.05 μm and 0.7 to 0.85 μm, although these are only examples of the D90 of the silver particles (X).
[0082] D10 of the silver particles (X) is not particularly limited, but is preferably 0.08 μm or more, and may be, for example, 0.2 μm or more or 0.3 μm or more. When D10 of the silver particles (X) is in such a range, cracking of the dried bonding material is further suppressed. On the other hand, D10 of silver particles (X) is preferably 0.45 μm or less, and may be, for example, 0.35 μm or less. Such silver particles (X) can be more easily prepared or obtained. In one embodiment, D10 of silver particles (X) may be, for example, any of 0.08 to 0.45 μm and 0.08 to 0.35 μm, or any of 0.2 to 0.45 μm and 0.2 to 0.35 μm, although these are only examples of D10 of silver particles (X).
[0083] When the exothermic peak of silver particles (X) is observed by simultaneous differential thermal analysis / thermogravimetry (TG / DTA), there are cases where only one exothermic peak is observed, and cases where two or more exothermic peaks are observed. In this embodiment, when only one exothermic peak of silver particles (X) is observed, the temperature showing the exothermic peak (exothermic peak temperature) is 183 to 224°C, and when two or more exothermic peaks of silver particles (X) are observed, the highest temperature among the temperatures showing the exothermic peaks (exothermic peak temperatures) is 183 to 224°C. When the exothermic peak temperature of the silver particles (X) is within this range, cracking of the dried bonding material is suppressed, and bonding defects at the bonded portion are suppressed.
[0084] The exothermic peak temperature of the silver particles (X) may be, for example, any one of 183 to 198°C, 196 to 211°C, and 209 to 224°C. The lower the exothermic peak temperature of the silver particles (X), the easier it is for the silver particles (X) to be sintered.
[0085] The exothermic peak temperature of silver particles (X) can be adjusted, for example, by adjusting the type and amount of a surface treatment agent for silver particles (X) described below, and the specific surface area of silver particles (X).
[0086] The specific surface area of the silver particles (X) is not particularly limited, but is preferably 1.1 to 3.6 m 2 / g, for example, 1.1 to 3.2 m 2 / g, and 1.1 to 2 m 2 / g or 1.2 to 3.6 m 2 / g, and 2 to 3.6 m 2 / g or 1.2 to 3.2 m 2 When the specific surface area of the silver particles (X) is within this range, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonded portion are further suppressed can be obtained.
[0087] The shape of the silver particles (X) may be the same as the shape of the silver particles (A) or silver particles (B). As in the case of the silver particles (A) or silver particles (B), examples of the silver particles (X) include silver particles obtained by a reduction method and silver particles obtained by an atomization method. The silver particles (X), like the silver particles (A) or silver particles (B), may be surface-treated or surface-untreated. Examples of the surface treatment agent for silver particles (X) include the same surface treatment agents as those for silver particles (A) or silver particles (B).
[0088] <<Solvent>> The bonding material of the present embodiment contains one or more solvents selected from the group consisting of ethylene glycol mono(2-ethylhexyl)ether, ethylene glycol monohexyl ether, and texanol. By using the bonding material containing such a solvent, cracking of the dried bonding material is suppressed, and bonding defects at the bonding portion are suppressed.
[0089] In this specification, unless otherwise specified, the mere mention of "solvent" does not mean the solvent (S) but means one or more solvents selected from the group consisting of ethylene glycol mono(2-ethylhexyl) ether, ethylene glycol monohexyl ether, and Texanol.
[0090] In the bonding material, the ratio of the content of the solvent to the content of silver particles (X) ([content of solvent in bonding material (parts by mass)] / [content of silver particles (X) in bonding material (parts by mass)]×100) is preferably 10 to 17% by mass, and may be, for example, any one of 10 to 14.5% by mass, 10 to 13.5% by mass, and 10 to 12.5% by mass, any one of 12.5 to 17% by mass, 13.5 to 17% by mass, and 14.5 to 17% by mass, or may be 12.5 to 14.5% by mass. When the ratio is equal to or greater than the lower limit, the effect obtained by using the solvent is enhanced. When the ratio is equal to or less than the upper limit, excessive use of the solvent is suppressed.
[0091] <<Other Ingredients>> The bonding material may or may not contain other components that do not fall into the category of either silver particles (X) or the solvent, as long as the effects of the present invention are not impaired. The other components are not particularly limited as long as they do not impair the effects of the present invention, and can be arbitrarily selected depending on the purpose.
[0092] The bonding material may contain only one type of other component, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.
[0093] The other components contained in the bonding material include the same components as those blended in the blending step of the manufacturing method, such as silver particles (C), additives (Z), etc.
[0094] In the bonding material, the ratio of the content of silver particles (C) to the content of silver particles (X) ([content of silver particles (C) in bonding material (parts by mass)] / [content of silver particles (X) in bonding material (parts by mass)]×100) is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less. When the ratio is equal to or less than the upper limit, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonding portion are further suppressed can be obtained. On the other hand, the ratio is 0% by mass or more.
[0095] The bonding material may contain only one type of additive (Z), or may contain two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.
[0096] When the bonding material contains an additive (Z), the ratio of the content of the additive (Z) to the content of the silver particles (X) in the bonding material ([content of additive (Z) in the bonding material (parts by mass)] / [content of silver particles (X) in the bonding material (parts by mass)]×100) is preferably 0.5 to 8 mass%, and may be, for example, any one of 0.5 to 4 mass% and 0.5 to 2 mass%, or may be 2 to 8 mass%. When the ratio is equal to or more than the lower limit, the effect obtained by using the additive (Z) is enhanced. When the ratio is equal to or less than the upper limit, excessive use of the additive (Z) is suppressed.
[0097] When the bonding material contains another component (Y) that does not fall into either the silver particles (C) or the additive (Z), the other component (Y) contained may be one type or two or more types. When the other component (Y) is two or more types, the combination and ratio thereof can be selected arbitrarily. In the bonding material, the ratio of the content of the other component (Y) to the content of the silver particles ([content of the other component (Y) in the bonding material (parts by mass)] / [content of the silver particles in the bonding material (parts by mass)]×100) is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less. When the ratio is equal to or less than the upper limit, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonding portion are further suppressed can be obtained. On the other hand, the ratio is 0% by mass or more.
[0098] In the bonding material, the ratio of the total content of silver particles (X), solvent, and additive (Z) to the total mass of the bonding material (([content of silver particles (X) in the bonding material (parts by mass)] + [content of solvent in the bonding material (parts by mass)] + [content of additive (Z) in the bonding material (parts by mass)]) / [total mass of the bonding material (parts by mass)] × 100) is preferably 95 mass% or more, more preferably 97 mass% or more, and even more preferably 99 mass% or more. The higher the ratio, the more cracks in the dried bonding material are suppressed, and the more a bonding material in which poor bonding at the bonded joint is suppressed can be obtained. On the other hand, the proportion is 100% by mass or less.
[0099] In the bonding material, the ratio of the content of silver particles (X) to the total mass of the bonding material ([content of silver particles (X) in bonding material (parts by mass)] / [total mass of bonding material (parts by mass)]×100) is preferably 90 to 100 mass%, and may be, for example, any one of 93 to 100 mass%, 96 to 100 mass%, and 98 to 100 mass%. When the ratio is in such a range, cracking of the dried bonding material is further suppressed, and a bonding material in which bonding defects at the bonded portion are further suppressed can be obtained.
[0100] <<Method of manufacturing bonding material>> The bonding material can be produced by mixing silver particles (X), the solvent, and, if necessary, the other components. The order in which the components are mixed is not particularly limited. The method for mixing the blend is not particularly limited, and may be appropriately selected from known methods such as a method for mixing by rotating a stirrer or agitator blades, etc.; a method for mixing using a mixer, a three-roll mill, a kneader, a bead mill, etc.; a method for mixing by applying ultrasonic waves, etc.
[0101] The temperature at which each component is mixed is not particularly limited as long as the components do not deteriorate, but a temperature of 0 to 40°C is preferable. The blending time of each component is not particularly limited as long as each blended component does not deteriorate, but it is preferably 10 minutes to 12 hours.
[0102] The method for producing a bonding material containing silver particles (X) can be included in the method for producing a bonding material according to one embodiment of the present invention, in which a mixture obtained by mixing silver particles (A) and silver particles (B) is blended.
[0103] ◇ Manufacturing method of the joint A method for producing a bonded body according to one embodiment of the present invention is a method for producing a bonded body in which a conductive first part (sometimes simply referred to as a "first part" in this specification) and a conductive second part (sometimes simply referred to as a "second part" in this specification) are bonded to each other via a conductive bonding part (sometimes simply referred to as a "bonding part" in this specification), The manufacturing method includes a step of attaching a bonding material manufactured by the manufacturing method according to one embodiment of the present invention or a bonding material according to one embodiment of the present invention to a surface of one of the first component and the second component (sometimes referred to as an "attaching step" in this specification); A step of forming a dried bonding material by drying the applied bonding material (sometimes referred to as a "drying step" in this specification); a step of laminating the first component and the second component with the dried bonding material interposed therebetween to produce a laminate (sometimes referred to as a "lamination step" in this specification); and a step of forming the joint from the dried bonding material by firing the dried bonding material in the laminate at a temperature higher than the temperature at which the bonding material was dried (sometimes referred to as a "firing step" in this specification).
[0104] The conductive parts such as the first part and the second part are not particularly limited as long as they are conductive. Examples of the conductive parts include metal parts (metal members). The metal parts may be, for example, metal layers provided on the surface of a semiconductor chip or semiconductor element such as a silicon chip by a sputtering method or a plating method, or may be metal layers such as electrodes provided on a resin substrate or a ceramic substrate.
[0105] The joint is formed using a joint material manufactured by the manufacturing method according to one embodiment of the present invention described above, or a joint material according to one embodiment of the present invention described above, and is a silver sintered body. The joint is electrically and thermally conductive, making it a useful alternative to solder.
[0106] In the above-mentioned production method, any of the steps can be carried out under atmospheric conditions. When the constituent material of either or both of the first and second components to be joined is a metal that is easily oxidized (e.g., copper, etc.), any of the steps in the manufacturing method may be performed in an inert gas atmosphere, such as nitrogen gas or helium gas.
[0107] Hereinafter, the method for producing the bonded body of the present embodiment will be described with reference to the drawings. In addition, the figures used in the following explanation may show key parts enlarged for convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones. First, a bonded body to which the manufacturing method of this embodiment is applied will be described.
[0108] <<zygote>> FIG. 1 is a cross-sectional view showing a schematic example of the bonded body. The bonded body 1 shown here is configured by bonding a conductive first component 11 and a conductive second component 12 via a conductive bonding portion 13. The first component 11 is in contact with the joint portion 13 on one surface 11a thereof. The second component 12 is in contact with the joint portion 13 at one surface 12a thereof. The bonded body 1 is configured by laminating a first component 11, a bonding portion 13, and a second component 12 in this order in the thickness direction.
[0109] The area of one surface 11 a of the first component 11 is equal to or larger than the area of one surface 12 a of the second component 12 .
[0110] The first component 11 has a sheet, plate or block shape.
[0111] The first component 11 is preferably configured to contain a metal, and more preferably is made of metal. Examples of metals that form the first component 11 include silver, copper, aluminum, gold, and nickel.
[0112] The first component 11 may be made of one layer (single layer) or may be made of two or more layers. When the first component 11 is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited. In this specification, not only in the case of the first part, "multiple layers may be the same or different" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different" means "at least one of the constituent materials and thicknesses of each layer is different from each other".
[0113] When the first component 11 is made up of a plurality of layers, for example, one or more layers on the bonding portion 13 side of the first component 11 may be layers that improve adhesion to the bonding portion 13 .
[0114] The thickness of the first component 11 can be set arbitrarily depending on the purpose of the joined body 1, and is not particularly limited. The thickness of the first component 11 may be, for example, 10 to 10,000 μm.
[0115] When the first component 11 is made up of a plurality of layers, the total thickness of the layers is preferably the thickness of the first component 11 described above.
[0116] Here, the first part 11 is shown to be in a sheet shape, a plate shape, or a block shape, but the first part 11 may be in a shape other than these, and the shape of the first part 11 can be selected arbitrarily depending on the purpose.
[0117] The second part 12 has a sheet, plate or block shape.
[0118] The second component 12 is preferably composed of a metal, and more preferably made of metal, and examples of metals constituting the second component 12 include the same metals as those constituting the first component 11 described above.
[0119] The second component 12 may be made of one layer (single layer) or may be made of two or more layers. When the second component 12 is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.
[0120] When the second component 12 is made up of multiple layers, for example, one or more layers on the bonding portion 13 side of the second component 12 may be layers that improve adhesion to the bonding portion 13.
[0121] The thickness of the second component 12 can be set arbitrarily depending on the purpose of the joined body 1, and is not particularly limited. The thickness of the second component 12 is preferably 0.05 to 10,000 μm, and may be, for example, 0.05 to 500 μm, or may be more than 500 μm and not more than 10,000 μm. When the second component 12 is made up of a plurality of layers, the total thickness of the layers is preferably the thickness of the second component 12 described above.
[0122] The area of one surface 11a of the first component 11 is preferably equal to or larger than the area of one surface 12a of the second component 12.
[0123] Here, the second part 12 is shown to be in a sheet shape, a plate shape, or a block shape, but the second part 12 may be in a shape other than these, and the shape of the second part 12 can be selected arbitrarily depending on the purpose.
[0124] The joint 13 is in the form of a sheet, a plate or a block. The bonding portion 13 may be made of one layer (single layer) or may be made of two or more layers. When the bonding portion 13 is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.
[0125] It is preferable that the entire surface of the joint portion 13 on the first component 11 side be in contact with one surface 11 a of the first component 11 .
[0126] The thickness of the joint 13 may be, for example, any one of 10 μm or more and less than 100 μm, 45 μm or more and less than 100 μm, and 80 μm or more and less than 100 μm, but is preferably 100 μm or more, and may be, for example, any one of 120 μm or more and 140 μm or more. When the thickness of the joint 13 is as thick as 100 μm or more, the thickness of the dried bonding material also needs to be 100 μm or more. When the thickness of the dried bonding material is thus thickened, the effect of the present invention, that is, cracking of the dried bonding material can be suppressed, is more significantly obtained by using the bonding material of this embodiment. On the other hand, the thickness of the joint 13 is preferably 170 μm or less in that the joint 13 can be formed more easily.
[0127] Here, the joint 13 is shown to be in a sheet, plate or block shape, but the joint 13 may be in any other shape, and the shape of the joint 13 can be selected arbitrarily depending on the purpose.
[0128] The area of the contact region of the joint 13 with the first component 11 (more specifically, one surface 11a) and the area of the contact region with the second component 12 (more specifically, one surface 12a) may be the same or different, and may be within a range of 9 to 2500 mm 2 It is preferable that the length is 9 to 1225 mm. 2 More preferably, for example, 9 to 576 mm 2 , and 9 to 144 mm 2 It may be either 225 to 1225 mm 2 , and 625~1225mm2 It may be either 225 to 576 mm 2 However, these are just examples of the area of the contact region.
[0129] The area of one surface 12a of the second component 12 is preferably 50 to 150% of the area of the surface of the joint 13 on the second component 12 side. The area of the contact region with the joint portion 13 on one surface 12a of the second component 12 is preferably 50 to 100% of the entire area of the one surface 12a. In joint 13, it is preferable that the entire surface on the first component 11 side is in contact with first component 11.
[0130] In the joined body 1, one first component 11 and one second component 12 are joined by one joint 13, but the joining form is not limited to this. In the joined body, for example, one first part and two or more second parts may be joined by one joint, in which case the two or more second parts may all be the same, all be different, or only partly different. In addition, in the joined body, for example, one first part and two or more second parts may be joined by two or more joining parts. In this case, the number of second parts and the number of joining parts may be the same or different. Furthermore, the two or more second parts may all be the same, all be different, or only some may be different. The numbers of first components and second components exemplified here may be reversed.
[0131] The bonded body to which the manufacturing method of the present embodiment is applied is not limited to that shown in FIG. 1. For example, the bonded body 1 shown in FIG. 1 may have some components changed, deleted, or added thereto without departing from the spirit of the present invention. Next, the manufacturing method of this embodiment will be described by taking as an example the case of manufacturing the bonded body shown in FIG.
[0132] ◎Manufacturing method (1) FIG. 2 is a cross-sectional view for illustrating a schematic example of a method for producing a bonded body according to this embodiment (sometimes referred to as "production method (1)" in this specification). In FIG. 2 and subsequent figures, the same components as those shown in the figures already described are given the same reference numerals as in the figures already described, and detailed description thereof will be omitted.
[0133] <<Attachment process>> In the attaching step of the manufacturing method (1), the bonding material 130 is attached to one surface 11a of the first component 11, as shown in FIG. 2(a). The bonding material 130 may be attached to the first component 11 by known methods such as printing and coating.
[0134] Examples of the printing method include screen printing, flexographic printing, offset printing, dip printing, inkjet printing, dispenser printing, jet dispenser printing, gravure printing, gravure offset printing, and pad printing.
[0135] Examples of the coating method include methods using various coaters such as a spin coater, an air knife coater, a curtain coater, a die coater, a blade coater, a roll coater, a gate roll coater, a bar coater, a rod coater, and a gravure coater; methods using a wire bar; and methods using a coating device such as a slot die.
[0136] When bonding material 130 is applied to first component 11, a mask such as a metal mask plate may be used to apply bonding material 130 only to desired locations.
[0137] <<Drying process>> After the adhesion step of the manufacturing method (1), in the drying step, the adhered bonding material 130 is dried to form a dried bonding material 130', as shown in FIG. 2(b). The drying process causes the solvent in the bonding material 130 to volatilize, so that in the dried bonding material 130 ′, there is no solvent or the amount of solvent contained is significantly reduced compared to the bonding material 130 .
[0138] The dried bonding material 130' is not a silver sintered body, and typically does not have the luster characteristic of metal. This external appearance characteristic also makes it possible to distinguish the dried bonding material 130' from the target silver sintered body.
[0139] The bonding material 130 can be dried by a known method, and is preferably dried by heating under normal pressure.
[0140] The heating temperature (drying temperature) of the bonding material 130 in the drying step can be appropriately adjusted depending on the type of solvent, but is preferably 90° C. or higher, and may be, for example, 120° C. or higher or 130° C. or higher. When the heating temperature is equal to or higher than the lower limit, the drying of the bonding material 130 proceeds more quickly. On the other hand, the heating temperature is preferably equal to or lower than 160° C. By setting the heating temperature equal to or lower than the upper limit, deterioration of the dried bonding material 130′ and sintering of silver particles (e.g., silver particles (A) and silver particles (B)) in the dried bonding material 130′ are suppressed.
[0141] The heating time (drying time) of the bonding material 130 in the drying step can be appropriately adjusted depending on the heating temperature, but is preferably 1 to 40 minutes, and may be, for example, either 3 to 30 minutes or 5 to 20 minutes. By keeping the heating time in such a range, the desired dried bonding material 130' can be formed more efficiently.
[0142] The thickness of the dried bonding material 130' may be, for example, any of 10 μm or more and less than 100 μm, 45 μm or more and less than 100 μm, and 80 μm or more and less than 100 μm, but is preferably 100 μm or more, and may be, for example, any of 120 μm or more and 140 μm or more. A dried product of a normal bonding material is prone to cracking, especially when it is thick. In contrast, the dried bonding material 130' uses the bonding material 130, and thus cracking is suppressed not only when the thickness is thin, but also when the thickness is thick, such as 100 μm or more. On the other hand, the thickness of the dried bonding material 130' is preferably 170 μm or less in that the dried bonding material 130' is easier to form.
[0143] <<Lamination process>> 2(c), in the lamination step after the drying step of manufacturing method (1), the first component 11 and the second component 12 are laminated with the dried bonding material 130' interposed therebetween to produce the laminated body 101. That is, the laminated body 101 is configured by laminating the first component 11, the dried bonding material 130', and the second component 12 in this order in the thickness direction, and the dried bonding material 130' is in close contact with the first component 11. The first component 11 is in contact with the dried bonding material 130' on one surface 11a thereof. The second component 12 is in contact with the dried bonding material 130' on one surface 12a thereof.
[0144] <<Firing process>> After the lamination step of manufacturing method (1), in the firing step, the dried bonding material 130' in the laminate 101 is fired at a temperature (sometimes referred to as the "firing temperature" in this specification) higher than the temperature at which the bonding material 130 was dried, as shown in FIG. 2(d). When the bonding material 130 is dried by heating, the baking temperature of the dried bonding material 130' (the baking temperature) is set higher than the heating temperature of the bonding material 130 (the drying temperature).
[0145] The temperature rise rate of the dried bonding material 130' during heating when the dried bonding material 130' is fired is not particularly limited, but is preferably 30 to 70° C. / min, and may be, for example, 40 to 60° C. / min. When the temperature rise rate is in such a range, a silver sintered body (bonding portion 13) having the desired characteristics can be more efficiently manufactured.
[0146] The firing temperature of the dried bonding material 130′ (e.g., the temperature at which silver particles (A) and silver particles (B) are sintered) is preferably 180° C. or higher, and may be, for example, any one of 200° C. or higher, 220° C. or higher, and 240° C. or higher. When the firing temperature is equal to or higher than the lower limit, a silver sintered body (bonding portion 13) with higher purity can be obtained. On the other hand, the firing temperature of the dried bonding material 130' is preferably 320°C or less, in order to prevent excessive heating and obtain a silver sintered body (bonding portion 13) with good characteristics, and may be, for example, either 300°C or less or 280°C or less.
[0147] The firing time of the dried bonding material 130' (e.g., the time for sintering the silver particles (A) and the silver particles (B)) is preferably 3 to 120 minutes, and may be, for example, any one of 3 to 60 minutes, 50 to 90 minutes, and 80 to 120 minutes. When the firing time (sintering time) is within such a range, a silver sintered body having the desired characteristics can be produced more efficiently. In the firing step, it is preferable to fire the dried bonding material 130' at a firing temperature within the above-mentioned range and for a firing time within the above-mentioned range.
[0148] In the firing step, it is preferable to fire the dried bonding material 130' (sometimes referred to as "pressure firing" in this specification) while pressurizing the laminate 101 in its thickness direction (in other words, the stacking direction of the first component 11, the dried bonding material 130', and the second component 12). By firing the dried bonding material 130' under pressure in this manner, a bonded portion with few voids can be formed.
[0149] When pressurizing the laminate 101 in its thickness direction (in other words, the stacking direction of the first component 11, the dried bonding material 130', and the second component 12), the pressure applied to the laminate 101 can be either or both of a pressure P1 applied from the first component 11 side and a pressure P2 applied from the second component 12 side, as shown in FIG. 2(d). In this specification, "pressurization" means increasing the pressure applied to an object by actively applying force to the object, and does not mean, for example, that the object is only supported (just applying normal force) and no operation of actively applying force is performed. In the case of pressurization, for example, the position of the pressurizing means changes by itself with acceleration.
[0150] During pressurized firing, heating for firing the dried bonding material 130' (laminate 101) and pressurizing the dried bonding material 130' (laminate 101) may be started simultaneously, heating for firing the dried bonding material 130' may be started before pressurizing the dried bonding material 130' is started, or heating for firing the dried bonding material 130' may be started before pressurizing the dried bonding material 130' is started.
[0151] The pressure applied to the dried bonding material 130′ during the pressure firing is preferably 20 MPa or less, and may be, for example, 16 MPa or less. When the pressure is equal to or less than the upper limit, damage such as cracks and deformation of the first component 11 or the second component 12 are further suppressed. On the other hand, the pressure during the pressurized sintering is preferably, for example, 3 MPa or more in order to effectively obtain the effect of the pressurization. Here, the pressure applied to the dried bonding material 130' (the pressure during pressure firing) is the load applied to the laminate 101 when pressure is applied, divided by the area of the region of the dried bonding material 130' that is subjected to this load.
[0152] 2(e), the bonding part 13 is formed from the dried bonding material 130', and the desired bonded body 1 is obtained. The bonding part 13 is a silver sintered body formed from the bonding material 130 via the dried bonding material 130'.
[0153] By using the bonding material 130, bonding defects at the bonding portion 13 in the bonded body 1 are suppressed. For example, peeling between the surface of the bonding portion 13 on the first component 11 side and one surface 11a of the first component 11 is suppressed, and peeling between the surface of the bonding portion 13 on the second component 12 side and one surface 12a of the second component 12 is suppressed. Such suppression of bonding defects at the bonding portion 13 is observed not only immediately after the manufacture of the bonded body 1, but also when the bonded body 1 is subjected to thermal shock by repeatedly heating and cooling it.
[0154] So far, a manufacturing method for a bonded body (manufacturing method (1)) has been described in which the bonding material is adhered to one surface of a first component and a bonded joint is formed from this bonding material. However, the manufacturing method of this embodiment may also be a manufacturing method for a bonded body (sometimes referred to in this specification as "manufacturing method (2)") in which the bonding material is adhered to one surface of a second component and a bonded joint is formed from this bonding material.
[0155] ◎Manufacturing method (2) FIG. 3 is a cross-sectional view for illustrating another example of the method for producing a bonded body of the present embodiment, that is, the production method (2).
[0156] <<Attachment process>> In the attaching step of the manufacturing method (2), the bonding material 130 is attached to one surface 12a of the second component 12, as shown in FIG. 3(a). The adhesion step in manufacturing method (2) can be performed in the same manner as the adhesion step in manufacturing method (1), except that the target to which the bonding material 130 is to be adhered is one surface 12a of the second component 12, rather than one surface 11a of the first component 11.
[0157] <<Drying process>> After the adhesion step of the manufacturing method (2), in the drying step, the adhered bonding material 130 is dried to form a dried bonding material 130', as shown in FIG. 3(b). The drying step in manufacturing method (2) can be performed in the same manner as the drying step in manufacturing method (1), except that a second part 12 having bonding material 130 attached thereto is used instead of a first part 11 having bonding material 130 attached thereto. The dried bonding material 130' formed by manufacturing method (2) is the same as the dried bonding material 130' formed by manufacturing method (1), except that it is in contact with the second component 12 instead of the first component 11. In the manufacturing method (2), the dried bonding material 130' also uses the bonding material 130, and thus cracks are suppressed not only when the bonding material is thin, but also when the bonding material is thick, such as 100 μm or more.
[0158] <<Lamination process>> 3(c), in the lamination step after the drying step of manufacturing method (2), the first component 11 and the second component 12 are laminated with the dried bonding material 130' interposed therebetween to produce a laminate 102. That is, the laminate 102 is configured by laminating the first component 11, the dried bonding material 130', and the second component 12 in this order in the thickness direction, and the dried bonding material 130' is in close contact with the second component 12. Laminate 102 is the same as laminate 101, except that dried bonding material 130' is in contact with second component 12 instead of first component 11. The lamination step in manufacturing method (2) can be performed in the same manner as the lamination step in manufacturing method (1), except that the first part 11 having the dried bonding material 130' is replaced with the second part 12 having the dried bonding material 130', and the first part 11 not having the dried bonding material 130' is replaced with the second part 12 not having the dried bonding material 130'.
[0159] <<Firing process>> After the lamination step of the manufacturing method (2), in the firing step, the dried bonding material 130' in the laminate 102 is fired at a temperature higher than the temperature at which the bonding material 130 was dried, as shown in FIG. 3(d). The firing step in the manufacturing method (2) can be performed in the same manner as the firing step in the manufacturing method (1). In the firing step in the manufacturing method (2), it is also preferable to pressurize and fire the dried bonding material 130'.
[0160] By carrying out the firing step of manufacturing method (2), as shown in Fig. 3(e), a joint 13 is formed from the dried bonding material 130', and the desired bonded body 1 is obtained. The joint 13 is a silver sintered body formed from the bonding material 130 via the dried bonding material 130'. The bonded body 1 obtained by manufacturing method (2) is the same as the bonded body 1 obtained by manufacturing method (1).
[0161] In the case of manufacturing method (2), as in the case of manufacturing method (1), by using the bonding material 130, bonding defects at the bonding portion 13 in the bonded body 1 are suppressed. For example, peeling between the surface of the bonding portion 13 on the first component 11 side and one surface 11a of the first component 11 is suppressed, and peeling between the surface of the bonding portion 13 on the second component 12 side and one surface 12a of the second component 12 is suppressed. Such suppression of bonding defects at the bonding portion 13 is observed not only immediately after the manufacturing of the bonded body 1, but also when the bonded body 1 is subjected to thermal shock by repeatedly heating and cooling it. EXAMPLES
[0162] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the examples shown below.
[0163] The silver particles (A), silver particles (B), and silver particles (C) used in the following examples and comparative examples are shown in Table 1. All of these silver particles are dry powders. The D50, D10 and D90 of these silver particles are actual measured values. The exothermic peak temperatures of these silver particles were measured by TG / DTA. The tap density and specific surface area of these silver particles are actually measured values.
[0164] [Table 1]
[0165] The solvent (S) used in each of the following Examples and Comparative Examples is shown in Table 2.
[0166] [Table 2]
[0167] The additives (Z) used in the following Examples and Comparative Examples are shown in Table 3.
[0168] [Table 3]
[0169] [Example 1] << Manufacturing of bonding materials >> Silver particles (A)-1 (80 parts by mass), silver particles (B)-1 (20 parts by mass), additive (Z)-1 (1 part by mass), and solvent (S)-1 (13.9 parts by mass) were kneaded at room temperature for 15 minutes. Next, the obtained kneaded material was passed through a triple roll three times to obtain the desired paste-like bonding material.
[0170] <<Measurement of heat peak temperature of total silver particles (silver particle mixture)>> Silver particles (A)-1 (80 parts by mass) and silver particles (B)-1 (20 parts by mass) were mixed at room temperature to prepare a silver particle mixture. The exothermic peak temperature of this silver particle mixture was measured by TG / DTA, and the results are shown in Table 4. In the examples and comparative examples described below, there are cases where only one type of silver particles is blended, so in Table 4 and subsequent tables, the column showing the exothermic peak temperature is given the title "Exothermic peak temperature of all silver particles (°C)."
[0171] <<Manufacturing of joints>> <Formation of dried joint material and evaluation of its crack suppression effect> A silver-plated copper plate having a size of 20 mm×20 mm and a thickness of 2 mm and having a silver-plated layer of 5 μm on its surface was prepared. A metal mask plate with a thickness of 300 μm was placed on one side of the silver-plated copper plate (the surface of the silver-plated layer), and the bonding material was used to print a square shape measuring 7 mm x 7 mm, thereby adhering the bonding material in this shape to the surface of the silver-plated copper plate (adhering process). Next, the silver-plated copper plate with this bonding material attached was heated at 125°C for 15 minutes using a hot air oven to volatilize the solvent (S)-1 in the bonding material, thereby drying it and forming a film-like dried bonding material with a rectangular planar shape (drying process). The dried bonded material was then visually observed and evaluated for crack suppression effect according to the following criteria. The results are shown in Table 1. [Evaluation Criteria] A: There are no cracks or only slight cracks in the dried bonding material, and the crack suppression effect is high. B: The dried joint material had some cracks that were not small, and the crack suppression effect was poor. C: Numerous cracks are clearly observed in the dried joint material, and no or only a small crack suppression effect is observed.
[0172] <Production of Joint> A back-side film-formed silicon carbide (SiC) chip was prepared, measuring 4.7 mm x 4.7 mm and 0.3 mm in thickness, with a 50 nm thick titanium film and a 100 nm thick silver film laminated in that order on one side (i.e. the back side) by sputtering. The entire exposed surface of the silver film in the silicon carbide chip having a film formed on its back side was overlapped on the side of the dried bonding material formed above opposite the silver-plated copper plate (i.e., the exposed surface), to produce a laminate in which the silver-plated copper plate, the dried bonding material, and the silicon carbide chip having a film formed on its back side were stacked in this order in the thickness direction (stacking process). Furthermore, in the laminate, a carbon sheet ("PERMA-FOIL (registered trademark)" manufactured by Toyo Tanso Co., Ltd.) was placed as a cushioning material on the surface of the silicon carbide chip in the silicon carbide chip having a film formed on its back surface.
[0173] Next, the laminate with the carbon sheet obtained above was pressed in its thickness direction (in other words, the lamination direction of the dried bonding material, etc.) using a servo press, and the pressure of the dried bonding material was started at a pressure of 15 MPa, and at the same time, heating was started at a temperature increase rate of about 50 ° C. / min. At this time, the laminate with the carbon sheet was placed between a pair of press plates in the servo press, and one of the press plates on the back surface-coated silicon carbide chip side in the laminate with the carbon sheet was fixed. Then, the other press plate on the silver-plated copper plate side in the laminate with the carbon sheet was moved to the side of the one press plate, and pressure was applied to the laminate with the carbon sheet from its silver-plated copper plate side while the laminate with the carbon sheet was supported by the one press plate. That is, the pressure was applied to the laminate with the carbon sheet at this time from the silver-plated copper plate side. Then, after the heating temperature (in other words, the temperature of the laminate) reached 250°C, this temperature was maintained for 5 minutes (i.e., heating and pressurizing were performed at a temperature of 250°C and a pressure of 15 MPa for 5 minutes), and the dried bonding material was pressurized and fired to form a bond from the dried bonding material (firing process). Next, cooling was started by running cooling water inside the servo press, and when the temperature of the laminate reached 60° C., the pressure was released. In this way, the desired bonded body was obtained. The thickness of the bonded portion in the bonded body was 128 μm.
[0174] <<Evaluation of zygotes>> <Evaluation of initial bonding rate> Using an ultrasonic testing instrument (SAT), the interface between the silver film provided on the silicon carbide chip via the titanium film and the joint (silver sintered body) in the bonded body obtained above was observed. When the interface was viewed from above the silicon carbide chip side in a plan view, it was determined that the black area in the area on the silver sintered body side from the silicon carbide chip was the silver sintered body in close contact with the silver film on the silicon carbide chip. Therefore, the ratio of the area of the above-mentioned black area to the area of the surface of the silver sintered body on the silicon carbide chip side ([area of the area of the black area in the area on the silver sintered body side from the silicon carbide chip] / [area of the surface of the silver sintered body on the silicon carbide chip side]×100) was calculated, and this was adopted as the initial bonding rate of the chip side (backside film-formed silicon carbide chip side) of the bonded body. The results are shown in Table 4.
[0175] Similarly, the interface between the silver-plated layer in the silver-plated copper plate and the joint (silver sintered body) in the joint was observed. That is, when the interface was viewed from above the silver-plated copper plate side in a plan view, it was determined that the black area in the area closer to the silver sintered body than the silver-plated copper plate was the silver sintered body in close contact with the silver-plated layer in the silver-plated copper plate. Therefore, the ratio of the area of the above-mentioned black area to the area of the silver-plated copper plate side of the silver sintered body ([area of the area of the black area in the area closer to the silver sintered body than the silver-plated copper plate] / [area of the silver sintered body on the silver-plated copper plate side]×100) was calculated, and this was used as the initial bonding rate of the substrate side (silver-plated copper plate side) of the joint. The results are shown in Table 4.
[0176] In this example and in the other examples and comparative examples that follow, if the initial bonding rate of the bonded body was 90% or more on both the substrate side and the chip side, the initial bonding property of the bonded body was judged to be pass, and otherwise it was judged to be fail.
[0177] <Evaluation of bonding rate after thermal shock (after 300 cycles)> The bonded body for which the initial bonding rate was calculated was placed in a thermal shock tester, and left to stand for 30 minutes under a heating condition of 150°C, and then left to stand for 30 minutes under a cooling condition of -40°C from 2 minutes after that, which constituted one cycle. From 2 minutes after that, the heat-cooling cycle of leaving under the same heating condition and leaving under the cooling condition was repeated 299 times, and this heat-cooling cycle was repeated 300 times in total, to perform a thermal shock test. The bonded body was then removed from the thermal shock tester. As in the case of the initial bonding rate (%) described above, the bonding rate (bonding rate after 300 cycles) of the substrate side (silver-plated copper plate side) and the bonding rate (bonding rate after 300 cycles) of the chip side (backside silicon carbide chip side) were calculated for the bonded body after this thermal shock test. The results are shown in Table 4.
[0178] In this example and the other examples and comparative examples, when the bonding rate of the bonded body after 300 cycles was 90% or more on both the substrate side and the chip side, it was rated as A, which means a high bonding rate. When the bonding rate of the bonded body after 300 cycles was 80% or more and less than 90% on either or both the substrate side and the chip side, and was not less than 80% on either or both the substrate side and the chip side, it was rated as B, which means a medium bonding rate. When the bonding rate of the bonded body after 300 cycles was less than 80% on either or both the substrate side and the chip side, it was rated as C, which means a low bonding rate.
[0179] <Comprehensive assessment of zygotes> When the result of the above "evaluation of initial bonding rate" was a pass judgment and the result of the above "evaluation of bonding rate after thermal shock (after 300 cycles)" was an A or B judgment, the bonding quality of the bonded body was judged to be pass. On the other hand, when at least the result of the "evaluation of initial bonding rate" was a fail judgment or the result of the "evaluation of bonding rate after thermal shock (after 300 cycles)" was a C judgment, the bonding quality of the bonded body was judged to be fail. The results are shown in Table 4. Note that when at least the "evaluation of bonding rate after thermal shock (after 300 cycles)" was not performed, this overall judgment could not be made, so in such cases, "-" was entered in the corresponding column in Table 4.
[0180] <<Production of bonding material, measurement of heat peak temperature of all silver particles, production and evaluation of bonded body>> [Examples 2 to 22, Comparative Examples 1 to 21] A bonding material was produced in the same manner as in Example 1, except that either or both of the types and amounts of the blended components were changed so that the types and contents of the components contained in the bonding material were as shown in Tables 4 to 8. If necessary, the exothermic peak temperatures of all the silver particles were measured, and a bonded body was produced and evaluated. However, in Examples 2, 4 to 6, 9, 10, 12, 13, 15, 17 to 22 and Comparative Examples 2, 9, 12, and 19, the drying temperature of the bonding material was set to 115°C instead of 125°C. In Comparative Examples 3 to 8, 10, 11, and 14 to 18, the drying temperature of the bonding material was set to 145°C instead of 125°C. In Comparative Examples 3 to 5 and 16 to 19, the intended bonding materials were obtained without passing the kneaded mixture through a triple roll. The results are shown in Tables 4 to 8.
[0181] [Examples 23 to 31, Comparative Examples 22 to 24] The silver-plated copper plate was replaced with a silver-plated aluminum plate having a size of 20 mm x 20 mm, a thickness of 1 mm, and a silver-plated layer having a thickness of 5 μm on the surface, and the silicon carbide chip having a film on the back side was replaced with a silver-plated copper (Cu) chip having a size of 5 mm x 5 mm, a thickness of 2 mm, and a silver-plated layer having a thickness of 5 μm on the surface, and, if necessary, either one or both of the types and amounts of the blended components were changed so that the types and contents of the components contained in the bonding material were as shown in Tables 8 to 9. Except for this, a bonding material was produced in the same manner as in Example 1, and the exothermic peak temperature of all silver particles was measured as necessary, and a bonding body was produced and evaluated. However, in Examples 29 to 31, the drying temperature of the bonding material was changed to 145°C instead of 125°C. The results are shown in Tables 8 and 9.
[0182] [Examples 32 to 34] The bonding materials were manufactured and the bonded bodies were manufactured and evaluated in the same manner as in Example 1, except that either or both of the types and amounts of the blended components were changed so that the types and contents of the components in the bonding materials were as shown in Table 9, and the kneaded materials were not passed through the triple roll. However, in Example 32, the drying temperature of the bonding material was changed from 125° C. to 115° C. In Example 34, the drying temperature of the bonding material was further changed to 145°C instead of 125°C. The results are shown in Table 9.
[0183] [Table 4]
[0184] [Table 5]
[0185] [Table 6]
[0186] [Table 7]
[0187] [Table 8]
[0188] [Table 9]
[0189] As is clear from the above results, in Examples 1 to 34, even though the bonding material did not contain resin, cracking of the dried bonding material was suppressed, and bonding defects at the bonded portion were suppressed.
[0190] In the bonding materials of Examples 1 to 34, the exothermic peak temperature of all the silver particles (silver particle mixture) was 183 to 223° C., and the D50 of the silver particles contained in the bonding materials was 0.25 to 0.66 μm. Among these Examples, in Examples 1 to 28 in which bonding materials were produced through a blending step of blending silver particles (A) and silver particles (B), the silver particles (A) had a D50 of 0.25 to 0.46 μm and a peak exothermic temperature of 210 to 225° C., and the silver particles (B) had a D50 of 0.25 to 0.66 μm and a peak exothermic temperature of 168 to 179° C. Among these Examples, in Examples 29 to 34 in which bonding materials were produced without using silver particles (A) and silver particles (B) in combination, the silver particles (silver particles (A)-1, silver particles (A)-3, and silver particles (A)-4) had a D50 of about 0.42 to 0.46 μm and an exothermic peak temperature of 210 to 223° C., and the bonding materials contained ethylene glycol mono(2-ethylhexyl) ether, ethylene glycol monohexyl ether, or Texanol as the solvent (S).
[0191] In contrast to this, in Comparative Examples 1 to 24, at least cracking of the dried bonding material was not suppressed, and bonding failure at the bonded portion was not suppressed.
[0192] More specifically, in Comparative Examples 1 to 17, cracking of the dried bonding material was not suppressed. Among these, in Comparative Examples 1, 4, 9 to 13, and 16, the initial bonding rate of the bonded body was further low, and in Comparative Examples 16 to 17, the bonding rate of the bonded body after 300 cycles was further low, and bonding failure at the bonded portion was not suppressed. In Comparative Examples 5 to 8 and 14 to 15, the degree of cracking of the dried bonding material was large, so the initial bonding rate was not evaluated, and the thermal shock test and the bonding rate after 300 cycles were not evaluated. In Comparative Examples 4 and 9 to 13, only the initial bonding rate was evaluated. In Comparative Examples 1 to 15, the exothermic peak temperatures of all the silver particles were relatively low, being 182° C. or lower (168 to 182° C.). In Comparative Examples 16 to 17, only silver particles (C)-1 or (C)-2 were used as the silver particles during production of the bonding material, and the firing temperature was higher than the exothermic peak temperature of all the silver particles, but the difference was small. From the results of Comparative Examples 1 to 10, it was confirmed that when the exothermic peak temperature of all the silver particles is relatively low, the dried bonding material tends to crack easily.
[0193] In Comparative Examples 18 to 19 and 22 to 24, the bonding rate of the bonded bodies after 300 cycles was low, and bonding defects at the bonded portions were not suppressed. In Comparative Examples 18 to 19, only silver particles (A)-2 were used as the silver particles during production of the bonding material, and the firing temperature was higher than the exothermic peak temperature of all the silver particles, but the difference was small. In Comparative Examples 22 to 24, the firing temperatures were lower than those of the other Comparative Examples and were approximately equal to the exothermic peak temperatures of all the silver particles.
[0194] In Comparative Examples 20 and 21, the printing suitability of the bonding material was poor, so that the adhesion step could not be performed and the production of the bonded body was abandoned. In particular, in Comparative Example 20, the fluidity of the bonding material was low. In Comparative Examples 20 to 21, only silver particles (C)-3 or (C)-4 were used as the silver particles during production of the bonding material. [Industrial Applicability]
[0195] The present invention can be used in the manufacture of conductive junctions, particularly semiconductor devices. [Explanation of symbols]
[0196] 1...zygote, 11: a conductive first part; 11a: one surface of the conductive first part; 12: a conductive second part; 12a: one surface of the conductive second part; 13... conductive joint, 130... joint material, 130'... dried joint material, 101, 102...Laminate
Claims
1. A method for manufacturing a bonding material for bonding conductive parts, comprising the steps of: The production method includes a blending step of blending silver particles (A) and silver particles (B), the silver particles (A) have a particle size at 50% cumulative volume of 0.2 to 0.5 μm, as measured by laser diffraction / scattering particle size distribution measurement, when an exothermic peak of the silver particles (A) is observed by simultaneous differential thermal and thermogravimetric analysis, if only one exothermic peak is observed, the temperature of the exothermic peak is 210 to 225°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 210 to 225°C, the silver particles (B) have a particle size at 50% cumulative volume of 0.2 to 0.7 μm, as measured by laser diffraction / scattering particle size distribution measurement; when an exothermic peak of the silver particles (B) is observed by simultaneous differential thermal and thermogravimetric analysis, if only one exothermic peak is observed, the temperature of the exothermic peak is 168 to 180°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 168 to 180°C, a temperature of the exothermic peak is 183 to 224°C when only one exothermic peak is observed, and a maximum temperature of the exothermic peak is 183 to 224°C when two or more exothermic peaks are observed, when an exothermic peak of a mixture of silver particles (A) and silver particles (B) in the same amounts as those in the blending step is observed by simultaneous differential thermal and thermogravimetry measurement.
2. 2. The method for producing a bonding material according to claim 1, wherein a ratio of a blending amount of the silver particles (B) to a total blending amount of the silver particles (A) and the silver particles (B) is 20 to 50 mass%.
3. A bonding material for bonding conductive parts together, The bonding material contains silver particles (X) and a solvent, the silver particles (X) have a particle size at 50% cumulative volume of 0.2 to 0.7 μm, as measured by laser diffraction / scattering particle size distribution measurement; when an exothermic peak of the silver particles (X) is observed by simultaneous differential thermal and thermogravimetric analysis, if only one exothermic peak is observed, the temperature of the exothermic peak is 183 to 224°C, and if two or more exothermic peaks are observed, the maximum temperature of the exothermic peak is 183 to 224°C, The bonding material, wherein the solvent is one or more selected from the group consisting of ethylene glycol mono(2-ethylhexyl) ether, ethylene glycol monohexyl ether, and Texanol.
4. A method for producing a bonded body, comprising the steps of: the joined body is configured by joining a conductive first part and a conductive second part via a conductive joint, The manufacturing method includes a step of attaching a bonding material manufactured by the manufacturing method according to claim 1 or 2 to a surface of one of the first component and the second component; drying the applied bonding material to form a dried bonding material; laminating the first component and the second component with the dried bonding material interposed therebetween to produce a laminate; and forming the bonded portion from the dried bonding material by firing the dried bonding material in the laminate at a temperature higher than a temperature at which the bonding material was dried.
Citation Information
Patent Citations
How to select sinterable silver particles and volatile dispersion media
JP6713182B1
Silver nanoparticles
JP7120314B2