Photosensitive resin composition, cured product, substrate with partition and method for producing the same, and image display device and method for producing the same
The photosensitive resin composition with a specific alkali-soluble binder polymer and liquid repellent addresses the issue of reduced reliability in partition walls by enhancing moisture and heat resistance, maintaining wall thickness and width in image display devices.
Patent Information
- Application Number
- JP2023071360
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing photosensitive resin compositions used for forming partition walls in image display devices suffer from reduced moisture and heat resistance reliability under high temperature and humidity conditions, leading to a decrease in thickness and width of the partition walls.
A photosensitive resin composition comprising an alkali-soluble binder polymer with a specific double bond equivalent weight, a photopolymerizable monomer, a photopolymerization initiator, and a liquid repellent, which reacts and cures to firmly fix the liquid repellent in the partition wall, enhancing its moisture and heat resistance.
The composition improves the moisture and heat resistance reliability of partition walls, preventing elution of components and maintaining the thickness and width of the partition walls even in high-temperature, high-humidity environments, ensuring stable retention of color filters.
Smart Images

Figure 2024157181000020 
Figure 2024157181000021 
Figure 2024157181000022
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a photosensitive resin composition, a cured product, a substrate with partition walls and a method for producing the same, and an image display device and a method for producing the same. [Background technology]
[0002] Image display devices such as televisions, signage, smart watches, smartphones, AR devices, and VR devices enable color display by arranging color filters of different colors as necessary opposite each of a number of light-emitting elements arranged in a matrix. Color filters are formed by filling openings in a photosensitive partition (also called a "bank material") with ink, such as quantum dot (QD) ink. In this case, the partition may be required to have ink repellency (liquid repellency) to prevent insufficient filling of the ink in the openings.
[0003] For example, Patent Document 1 listed below proposes imparting sufficient liquid repellency to partition walls by using a photosensitive resin composition containing an ethylenically unsaturated compound, a photopolymerization initiator, an alkali-soluble resin, and a liquid repellent agent, the liquid repellent agent containing a resin having a repeating unit including a polycyclic aliphatic hydrocarbon skeleton having a fluorine-containing organic group as a substituent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-51235 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the photosensitive resin composition described in Patent Document 1 has the following problems. That is, the photosensitive resin composition described in Patent Document 1 has room for improvement in terms of preventing a reduction in thickness and width of the partition walls obtained by curing the composition under high temperature and high humidity conditions, that is, in terms of imparting reliable moisture and heat resistance to the partition walls.
[0006] The present disclosure has been made in consideration of the above-mentioned problems, and aims to provide a photosensitive resin composition that can improve the moist heat resistance reliability of partition walls obtained by curing, a cured product, a substrate with partition walls and a method for producing the same, and an image display device and a method for producing the same. [Means for solving the problem]
[0007] In order to solve the above problems, the present disclosure provides a photosensitive resin composition, a cured product, a substrate with partition walls and a method for producing the same, and an image display device and a method for producing the same, as described in the following [1] to
[12] . [1] A photosensitive resin composition comprising an alkali-soluble binder polymer, a photopolymerizable monomer having an ethylenically unsaturated group, a liquid repellent agent having a photocurable group, and a photopolymerization initiator, wherein the alkali-soluble binder polymer has a double bond equivalent of 250 to 440 g / mol. [2] The photosensitive resin composition according to [1], wherein the alkali-soluble binder polymer has a double bond equivalent of 250 to 400 g / mol. [3] The photosensitive resin composition according to [1] or [2], wherein the alkali-soluble binder polymer contains a structural unit (a) represented by the following formula (1), a structural unit (b) represented by the following formula (2), a structural unit (c) represented by the following formula (3), and a structural unit (d) represented by the following formula (4): [ka] (In the above formula (1), R 1 represents a hydrogen atom or a methyl group, and X represents an alicyclic hydrocarbon group which may have a substituent. [ka] (In the above formula (2), R2 represents a hydrogen atom or a methyl group, and Y represents an aromatic group which may have a substituent. [ka] (In the above formula (3), R 3 represents a hydrogen atom or a methyl group. [ka] (In the above formula (4), R 4 and R 5 each independently represents a hydrogen atom or a methyl group. [4] The photosensitive resin composition according to any one of [1] to [3], further comprising a polyfunctional thiol compound, the polyfunctional thiol compound having three or more mercapto groups in one molecule. [5] The photosensitive resin composition according to any one of [1] to [4], wherein the photopolymerizable monomer has three or more functional groups in one molecule, and the three or more functional groups include the ethylenically unsaturated group and a hydroxyl group. [6] The photosensitive resin composition according to any one of [1] to [5], further comprising a colorant, wherein the colorant is an organic pigment. [7] The photosensitive resin composition according to any one of [1] to [6], wherein the photopolymerization initiator includes an acylphosphine oxide-based photopolymerization initiator. [8] A cured product obtained by curing the photosensitive resin composition according to any one of [1] to [7]. [9] A method for producing a substrate with partition walls, comprising: a photosensitive resin layer forming step of forming a photosensitive resin layer on a substrate using the photosensitive resin composition according to any one of [1] to [7]; an exposure step of partially exposing the photosensitive resin layer provided on the substrate to light to form a partially cured layer; a heating step of heating the partially cured layer; and a development step of forming a partition wall having at least one opening by alkaline development of the partially cured layer.
[10] A substrate with partition walls obtained by the method for producing a substrate with partition walls according to [9].
[11] An image display device comprising: a first structure; and a second structure laminated on the first structure, the first structure having the partition-equipped substrate described in
[10] and a color filter provided in at least one of the openings of the partition of the partition-equipped substrate, and the second structure comprising a light-emitting element positioned opposite the opening of the partition of the first structure.
[12] A method for manufacturing an image display device, comprising: a lamination step of laminating a first structure and a second structure, the first structure having a substrate with partition wall described in
[10] and a color filter filled in at least a part of the opening of the partition wall of the substrate with partition wall, the second structure having a light-emitting element, and in the lamination step, the light-emitting element of the second structure is positioned so as to face the opening of the partition wall of the first structure.
[0008] According to the photosensitive resin composition [1] above, the moisture and heat resistance reliability of the partition walls obtained by curing can be improved.
[0009] The reason why the above-mentioned effects are obtained by the photosensitive resin composition [1] above is presumed to be as follows. That is, when the photosensitive resin composition of the present disclosure, which includes an alkali-soluble binder polymer, a photopolymerizable monomer having an ethylenically unsaturated group, a photopolymerization initiator, and a liquid repellent agent, is applied onto a substrate to form a photosensitive resin layer, and the photosensitive resin layer is exposed to light, the alkali-soluble binder polymer has a double bond equivalent of 250 to 440 g / mol, and in the presence of the photopolymerization initiator, the alkali-soluble binder polymer, the photopolymerizable monomer, and the liquid repellent agent react with each other by light and are sufficiently cured. Therefore, the liquid repellent agent is firmly fixed in the cured product. As a result, even if the partition wall is placed in a high-temperature and high-humidity environment, the liquid repellent agent, the photopolymerizable monomer, and the like are prevented from eluting from the partition wall, and the thickness and width of the partition wall are prevented from decreasing. From the above, it is speculated that the photosensitive resin composition of the present disclosure can provide the above-mentioned effects.
[0010] According to the cured product of the above [8], when the cured product is used as a partition wall, the reliability of the moisture and heat resistance can be improved.
[0011] According to the method for producing a substrate with partition walls described above in [9], the reliability of moisture and heat resistance of the resulting partition walls can be improved.
[0012] According to the substrate with partition walls
[10] , the moisture and heat resistance reliability of the partition walls can be improved.
[0013] According to the image display device of the above
[11] , the manufacturing method of the partition-formed substrate can improve the moisture and heat resistance reliability of the partition walls. Therefore, even in a high-temperature and high-humidity environment, it is possible to suppress a decrease in the thickness and width of the partition walls, and the color filter can be stably held in the opening of the partition walls. As a result, in the image display device, replacement of the partition-formed substrate is not required for a long period of time.
[0014] According to the manufacturing method of the image display device
[12] above, the moisture and heat resistance reliability of the partition walls can be improved by the manufacturing method of the partition wall-equipped substrate. Therefore, in the obtained image display device, even in a high-temperature and high-humidity environment, the reduction in the thickness and width of the partition walls can be suppressed, and the color filters can be stably held in the openings of the partition walls. As a result, replacement of the partition wall-equipped substrate becomes unnecessary for a long period of time. Effect of the Invention
[0015] According to the present disclosure, there are provided a photosensitive resin composition capable of improving the moisture and heat resistance reliability of partition walls obtained by curing, a cured product, a substrate with partition walls and a method for producing the same, and an image display device and a method for producing the same. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a partial cross-sectional view showing an embodiment of a substrate with partition walls according to the present disclosure. [Diagram 2] FIG. 2 is a plan view showing the partition-formed substrate of FIG. [Diagram 3] FIG. 2 is a partial cross-sectional view showing a photosensitive resin layer forming step in an embodiment of a method for producing a substrate with partition walls according to the present disclosure. [Figure 4]FIG. 2 is a partial cross-sectional view showing an exposure step in an embodiment of a method for producing a substrate with partition walls according to the present disclosure. [Diagram 5] 5 is a partial cross-sectional view showing a second laminate obtained in the exposure step of FIG. 4. [Figure 6] FIG. 2 is a partial cross-sectional view showing a heating step in an embodiment of a method for producing a substrate with partition walls according to the present disclosure. [Figure 7] 1 is a partial cross-sectional view showing an embodiment of an image display device according to the present disclosure. [Figure 8] 4 is a partial cross-sectional view showing a color filter forming step in the embodiment of the manufacturing method for an image display device according to the present disclosure. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the embodiments for carrying out the present disclosure will be described in detail with reference to the drawings as needed. However, the present disclosure is not limited to the following embodiments. In this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid, and "(meth)acrylate" means acrylate or the corresponding methacrylate.
[0018] <Photosensitive resin composition and its cured product> The photosensitive resin composition of the present disclosure contains (A) an alkali-soluble binder polymer (hereinafter sometimes referred to as component (A)), (B) a photopolymerizable monomer having an ethylenically unsaturated group (hereinafter sometimes referred to as component (B)), (C) a photopolymerization initiator (hereinafter sometimes referred to as component (C)), and (D) a liquid repellent having a photocurable group. Here, the double bond equivalent of the binder polymer is 250 to 440 g / mol. The photosensitive resin composition may contain (E) a polyfunctional thiol compound (hereinafter, sometimes referred to as component (E)) and a colorant (hereinafter, sometimes referred to as component (F)).
[0019] According to the photosensitive resin composition of the present disclosure, the moisture and heat resistance reliability of the partition walls obtained by curing can be improved.
[0020] The cured product of the present disclosure is obtained by curing the above-mentioned photosensitive resin composition. According to the cured product of the present disclosure, when the cured product is used as a partition wall, the reliability of the moisture and heat resistance can be improved.
[0021] (A) Alkali-soluble binder polymer The double bond equivalent of the alkali-soluble binder polymer is 250 to 440 g / mol. When the double bond equivalent of the alkali-soluble binder polymer is 250 g / mol or more, the photosensitive resin composition is less likely to become sticky than when the double bond equivalent is less than 250 g / mol, and a useful alkali-soluble binder polymer is more likely to be obtained. When the double bond equivalent of the alkali-soluble binder polymer is 440 g / mol or less, the moisture and heat resistance reliability of the partition wall obtained by curing can be improved compared to when the double bond equivalent is more than 440 g / mol.
[0022] The double bond equivalent of the alkali-soluble binder polymer may be 260 g / mol or more, 270 g / mol or more, or 280 g / mol or more. The double bond equivalent of the alkali-soluble binder polymer may be 400 g / mol or less, or may be 380 g / mol or less. When the double bond equivalent of the alkali-soluble binder polymer is 400 g / mol or less, the moisture and heat resistance reliability of the partition wall obtained by curing can be further improved compared to when the double bond equivalent of the alkali-soluble binder polymer exceeds 400 g / mol. The double bond equivalent of the alkali-soluble binder polymer is the mass of the polymer per mole of polymerizable unsaturated bonds, and is calculated based on the amount of monomer used.
[0023] The binder polymer may contain a structural unit (a) represented by the following formula (1), a structural unit (b) represented by the following formula (2), a structural unit (c) represented by the following formula (3), and a structural unit (d) represented by the following formula (4). In this case, the moisture and heat resistance reliability of the partition wall obtained by curing the photosensitive resin composition can be further improved. In addition, the water repellency of the partition wall obtained by curing the photosensitive resin composition can be further improved. Furthermore, if the partition wall obtained is left under high humidity for a long time, the water repellency is further improved. Although the reason for this is unclear, it is thought that the liquid repellency is improved because some kind of reaction occurs between the moisture and the surface layer of the partition wall when the partition wall is exposed to high humidity for a long time. Alternatively, it is thought that the liquid repellency is improved because the layer of the outermost layer of the partition wall in which the liquid repellent agent is hardly segregated is dissolved at first, and the layer in which the liquid repellent agent is slightly segregated gradually comes to the surface layer. [ka] (In the above formula (1), R 1 represents a hydrogen atom or a methyl group, and X represents an alicyclic hydrocarbon group which may have a substituent. [ka] (In the above formula (2), R 2 represents a hydrogen atom or a methyl group, and Y represents an aromatic group which may have a substituent. [ka] (In the above formula (3), R 3 represents a hydrogen atom or a methyl group. [ka] (In the above formula (4), R 4 and R 5 each independently represents a hydrogen atom or a methyl group.
[0024] X in the formula (1) representing the structural unit (a) represents an alicyclic hydrocarbon group which may have a substituent. The alicyclic hydrocarbon group may have 7 to 20 carbon atoms. Examples of the substituent include halogen atoms such as fluoro, chloro and bromo, and hydroxy groups. Examples of the alicyclic hydrocarbon group include an adamantyl group, a tricyclodecyl group, an isobornyl group, and a cyclohexyl group. The structural unit (a) can be introduced by using an alicyclic hydrocarbon group-containing polymerizable monomer as the polymerizable monomer used when producing an alkali-soluble binder polymer by copolymerization. The alicyclic hydrocarbon group-containing polymerizable monomer is represented, for example, by the following general formula (1A). CH2=C(R 1 )-COOX…(1A)
[0025] Examples of the alicyclic hydrocarbon group-containing polymerizable monomer represented by the above general formula (1A) include adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, etc. These alicyclic hydrocarbon group-containing polymerizable monomers may be used alone or in combination of two or more.
[0026] In the formula (2) representing the structural unit (b), Y represents an aromatic group which may have a substituent. The aromatic group may have an aromatic ring, and is represented, for example, by -PQ. Here, P represents a single bond or -COO-, and Q represents an aromatic hydrocarbon group which may have a substituent. Examples of the aromatic hydrocarbon group include aryl groups such as a phenyl group and a naphthyl group, aralkyl groups such as a benzyl group, and a styryl group. The structural unit (b) can be introduced by using an aromatic hydrocarbon group-containing polymerizable monomer as the polymerizable monomer used when producing an alkali-soluble binder polymer by copolymerization. The aromatic hydrocarbon group-containing polymerizable monomer is represented by the following general formula (2A). CH2=C(R 2 )-Y …(2A)
[0027] Examples of the aromatic hydrocarbon group-containing polymerizable monomer represented by the general formula (2A) include aromatic hydrocarbon group-containing (meth)acrylates such as benzyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, etc., and aromatic vinyl compounds such as styrene, etc. These aromatic hydrocarbon group-containing polymerizable monomers may be used alone or in combination of two or more.
[0028] The structural unit (c) can be introduced by using (meth)acrylic acid as a polymerizable monomer when producing an alkali-soluble binder polymer by copolymerization. (Meth)acrylic acid is highly reactive and easily available.
[0029] The structural unit (d) can be introduced, for example, by using a polymerizable monomer represented by the following formula (4A) as a polymerizable monomer used when producing an alkali-soluble binder polymer. [ka] The structural unit (d) can also be introduced by adding glycidyl (meth)acrylate to some of the carboxy groups of the structural unit (c).
[0030] The above-mentioned alkali-soluble binder polymer has an ethylenically unsaturated group. Therefore, during exposure, the alkali-soluble binder polymer reacts with the photopolymerizable monomer and the liquid repellent agent, and the curing proceeds more sufficiently. In addition, during heating of the partially cured layer obtained after the exposure of the photosensitive resin layer, the alkali-soluble binder polymer reacts with the photopolymerizable monomer and the liquid repellent agent, and the curing proceeds more sufficiently.
[0031] In the alkali-soluble binder polymer, when the total of the above-mentioned structural units (a), (b), (c) and (d) is taken as 100 mol%, the proportion of the structural unit (a) is not particularly limited as long as it is greater than 0 mol%, and may be 0.1 mol% or more, 0.5 mol% or more, or 1 mol% or more. The proportion of the structural unit (a) may be 30 mol% or less, 29 mol% or less, or 28 mol% or less.
[0032] In the alkali-soluble binder polymer, the ratio of the structural unit (b) is not particularly limited as long as it is greater than 0 mol%, based on the total of the structural unit (a), the structural unit (b), the structural unit (c) and the structural unit (d) (100 mol%), and may be 0.1 mol% or more, 0.5 mol% or more, or 1.0 mol% or more. The ratio of the structural unit (b) may be less than 20 mol%, 19 mol% or less, or 18 mol% or less. If the ratio of the structural unit (b) is less than 20 mol%, there is a tendency that the reduction in the line width can be suppressed even when the partition wall is left in a high-temperature and high-humidity environment.
[0033] In the alkali-soluble binder polymer, when the total of the above-mentioned structural units (a), (b), (c) and (d) is taken as 100 mol%, the proportion of the structural unit (c) is not particularly limited as long as it is greater than 0 mol%, and may be 1 mol% or more, 2 mol% or more, or 3 mol% or more. The proportion of the structural unit (c) may be 35 mol% or less, 34 mol% or less, or 33 mol% or less.
[0034] In the alkali-soluble binder polymer, when the total of the above-mentioned structural units (a), (b), (c) and (d) is taken as 100 mol%, the proportion of the structural unit (d) is not particularly limited as long as it is within a range that allows the double bond equivalent to be in the range of 250 to 440 g / mol, and may be 45 mol% or more, 47 mol% or more, or 49 mol% or more. The proportion of the structural unit (d) may be 85 mol% or less, 83 mol% or less, or 81 mol% or less.
[0035] The acid value of the solid content of the alkali-soluble binder polymer is not particularly limited, but may be 25 mgKOH / g or more, or may be 30 mgKOH / g or more. When the acid value of the solid content of the alkali-soluble binder polymer is 25 mgKOH / g or more, the resolution of the partition walls can be improved even if the exposure dose during exposure is low. The alkali-soluble binder polymer may have an acid value of 125 mgKOH / g or less, or may have an acid value of 120 mgKOH / g or less. When the alkali-soluble binder polymer has an acid value of 125 mgKOH / g or less, the resolution of the partition walls can be further improved. The solid content acid value means the number of milligrams of potassium hydroxide required to neutralize the acid present in 1 g of the alkali-soluble binder polymer.
[0036] The weight average molecular weight of the alkali-soluble binder polymer may be 3,000 to 30,000, 3,500 to 25,000, or 4,000 to 20,000 from the viewpoint of balancing mechanical strength and alkali developability. In terms of excellent developer resistance after exposure, the weight average molecular weight may be 4,000 or more. In terms of development time, the weight average molecular weight may be 20,000 or less. However, since the developability is also greatly affected by the solid acid value, hydroxyl value, and resin skeleton, the weight average molecular weight of the alkali-soluble binder polymer is not particularly limited to the above range. The weight average molecular weight is a value measured by gel permeation chromatography (GPC) and converted using a calibration curve prepared using standard polystyrene.
[0037] The alkali-soluble binder polymers can be used alone or in combination of two or more.
[0038] (B) Photopolymerizable monomer The photopolymerizable monomer has an ethylenically unsaturated group, such as a (meth)acryloyloxy group, a vinyl group, or an allyl group.
[0039] Examples of photopolymerizable monomers having an ethylenically unsaturated group include compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid, bisphenol A-based (meth)acrylate compounds such as 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolypropoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloxypolyethoxypolypropoxy)phenyl)propane, compounds obtained by reacting a glycidyl group-containing compound with an α,β-unsaturated carboxylic acid, urethane monomers such as (meth)acrylate compounds having a urethane bond, γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, β-hydroxyethyl-β'-(meth)acryloyloxyethyl-o-phthalate, β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, and (meth)acrylic acid alkyl esters.
[0040] Examples of compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid include polyethylene glycol di(meth)acrylate having 2 to 14 ethylene groups, polypropylene glycol di(meth)acrylate having 2 to 14 propylene groups, polyethylene polypropylene glycol di(meth)acrylate having 2 to 14 ethylene groups and 2 to 14 propylene groups, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethoxy tri(meth)acrylate, trimethylolpropane diethoxy tri(meth)acrylate, and trimethylolpropane diethoxy tri(meth)acrylate. acrylate, trimethylolpropane triethoxy tri(meth)acrylate, trimethylolpropane tetraethoxy tri(meth)acrylate, trimethylolpropane pentaethoxy tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, polypropylene glycol di(meth)acrylate having 2 to 14 propylene groups, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0041] Examples of the urethane monomer include addition reaction products of a (meth)acrylic monomer having a hydroxyl group at the β-position with a diisocyanate compound such as isophorone diisocyanate, 2,6-toluene diisocyanate, 2,4-toluene diisocyanate, or 1,6-hexamethylene diisocyanate; tris[(meth)acryloxytetraethylene glycol isocyanate]hexamethylene isocyanurate; EO-modified urethane di(meth)acrylate; and EO,PO-modified urethane di(meth)acrylate. In addition, "EO" stands for ethylene oxide, and EO-modified compounds have a block structure of ethylene oxide groups. Also, "PO" stands for propylene oxide, and PO-modified compounds have a block structure of propylene oxide groups.
[0042] The number of functional groups in one molecule of the photopolymerizable monomer may be 2 or more, or 3 or more. Two or more types of photopolymerizable monomers, a photopolymerizable monomer having 2 or more functional groups and a photopolymerizable monomer having 3 or more functional groups, may be used in combination.
[0043] In the case where the number of functional groups in one molecule of the photopolymerizable monomer is 3 or more, all of the 3 or more functional groups may be ethylenically unsaturated groups, but the 3 or more functional groups may further include a hydroxyl group in addition to the ethylenically unsaturated group. In this case, the developability of the partially cured layer obtained after the exposure of the photosensitive resin layer is further improved. In addition, the swelling of the cured part due to the exposure of the partially cured layer during development by the developer can be suppressed, and the resolution of the photosensitive resin composition can be further improved.
[0044] The number of functional groups in one molecule may be 26 or less, or 5 or less.
[0045] As the photopolymerizable monomer, the above-mentioned compounds can be used alone or in combination of two or more kinds.
[0046] The content of the photopolymerizable monomer in the photosensitive resin composition may be 5 to 50 parts by mass or 5 to 30 parts by mass relative to 100 parts by mass of the total amount of the alkali-soluble binder polymer and the photopolymerizable monomer. When the content of the photopolymerizable monomer is 5 parts by mass or more, the photocurability of the photosensitive resin layer tends to be good, and when it is 50 parts by mass or less, when a photosensitive resin layer is formed on a substrate using the photosensitive resin composition, the photosensitive resin layer tends to have excellent shape retention before exposure.
[0047] (C) Photopolymerization initiator The photopolymerization initiator is a compound that initiates the reaction between the alkali-soluble binder polymer, the photopolymerizable monomer, and the liquid repellent agent, and the reaction between the photopolymerizable monomers themselves, and the photopolymerization initiator can be appropriately selected depending on the light wavelength of the exposure machine used, and known initiators such as photoradical polymerization initiators and photocationic polymerization initiators can be used. The photopolymerization initiator can be used alone or in combination of two or more types.
[0048] Examples of the photoradical polymerization initiator include aromatic ketones such as benzophenone, N,N'-tetraalkyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, 4,4'-bis(dimethylamino)benzophenone (Michler's ketone), 4,4'-bis(diethylamino)benzophenone, and 4-methoxy-4'-dimethylaminobenzophenone; quinones such as alkylanthraquinone and phenanthrenequinone; benzoin compounds such as benzoin and alkylbenzoin; benzoin ether compounds such as benzoin alkyl ether and benzoin phenyl ether; benzoin ether compounds such as benzoin alkyl ether and benzoin phenyl ether; benzyl derivatives such as aryl dimethyl ketal; 2,4,5-triarylimidazole dimers such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,4-di(p-methoxyphenyl)-5-phenylimidazole dimer, and 2-(2,4-dimethoxyphenyl)-4,5-diphenylimidazole dimer; N-phenylglycine, N-phenylglycine derivatives, and acridine derivatives such as 9-phenylacridine; 1-[4-(phenylthio)phenyl]-1,2-octanedione. Examples of such compounds include oxime esters such as 2-(O-benzoyloxime), coumarin compounds such as 7-diethylamino-4-methylcoumarin, thioxanthone compounds such as 2,4-diethylthioxanthone, and acylphosphine oxide compounds such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide.
[0049] Among them, an acylphosphine oxide-based photopolymerization initiator made of an acylphosphine oxide-based compound has a photobleaching function, and therefore becomes less likely to absorb light after being decomposed by exposure. Therefore, during exposure, light can be allowed to reach a sufficiently deep position from the surface of the photosensitive resin layer over time, so that insufficient curing of the exposed portion can be suppressed even if the photosensitive resin composition contains a colorant. Therefore, dissolution or swelling of the cured portion due to exposure during development can be suppressed, and the resolution of the partition wall can be further improved. The acylphosphine oxide photopolymerization initiator has an acylphosphine oxide group (>P(=O)-C(=O)- group), and examples thereof include (2,6-dimethoxybenzoyl)-2,4,6-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (product name: IRGACURE-TPO, manufactured by BASF), ethyl-2,4,6-trimethylbenzoylphenylphosphinenate, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (product name: IRGACURE-819, manufactured by BASF), (2,5-dihydroxyphenyl)diphenylphosphine oxide, (p-hydroxyphenyl)diphenylphosphine oxide, bis(p-hydroxyphenyl)phenylphosphine oxide, and tris(p-hydroxyphenyl)phosphine oxide.
[0050] As the photocationic polymerization initiator, an onium salt that releases a Lewis acid when irradiated with active energy rays may be used. Examples of such onium salts include aromatic sulfonium salts of Group VIIa elements, aromatic onium salts of Group VIa elements, and aromatic onium salts of Group Va elements. Specific examples include triarylsulfonium hexafluoroantimonate, triphenylphenacylphosphonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, bis-[4-(diphenylsulfonio)phenyl]sulfide bisdihexafluoroantimonate, bis-[4-(di-4'-hydroxyethoxyphenylsulfonio)phenyl]sulfide bisdihexafluoroantimonate, bis-[4-(diphenylsulfonio)phenyl]sulfide bisdihexafluorophosphate, and diphenyliodonium tetrafluoroborate.
[0051] From the viewpoint of achieving both photosensitivity and internal photocurability, the content of the photopolymerization initiator in the photosensitive resin composition may be 2.0 to 15.0 parts by mass, 3.0 to 12.0 parts by mass, or 4.0 to 10.0 parts by mass relative to 100 parts by mass of the total amount of the alkali-soluble binder polymer and the photopolymerizable monomer.
[0052] (D) Liquid repellent The liquid repellent agent is used to impart liquid repellency to the ink that fills the openings formed in the partition walls, and has a photocurable group. Examples of the photocurable group include ultraviolet-curable groups such as an acryloyl group, a methacryloyl group, and a vinyl group. The liquid repellent agent may contain two or more, three or more, or four or more photocurable groups in one molecule. The number of photocurable groups in one molecule may be up to 5 or up to 6. In this case, the film remaining property of the partition wall and the pattern width are easily controlled.
[0053] The liquid repellent may be a fluorine-based liquid repellent. A fluorine-based liquid repellent refers to a liquid repellent containing a fluorine atom. In this case, the liquid repellency of the cured product of the photosensitive resin composition against ink (e.g., QD ink) can be further increased.
[0054] The liquid repellent agent may have an alicyclic skeleton, which can enhance the liquid repellency of the cured product of the photosensitive resin composition against ink (e.g., QD ink). The number of ring members in the alicyclic skeleton may be 5 to 20, 5 to 18, 6 to 18, 6 to 14, or 6 to 12, from the viewpoint of improving photocurability. From the same viewpoint, the number of rings in the alicyclic skeleton contained in the liquid repellent agent may be 2 or more, or may be 3 or more. In this case, the liquid repellency against ink of the partition wall obtained by curing the photosensitive resin composition can be further improved. The number of rings in the alicyclic skeleton contained in the liquid repellent agent may be 4 or less. Examples of alicyclic skeletons having one ring include a cyclohexane skeleton and a cyclohexene skeleton, and examples of alicyclic skeletons having two or more rings include a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton, and a saturated dicyclopentadiene skeleton.
[0055] Examples of liquid repellents include Megafac RS-72-A (manufactured by DIC Corporation), F-563 (manufactured by DIC Corporation), pentafluorocyclopentene, Viscoat 13F (manufactured by Osaka Organic Industry Co., Ltd.), pentafluorobenzyl methacrylate, octafluorohexanediol diacrylate, pentafluorotoluene, etc. These can be used alone or in combination of two or more.
[0056] The content of the liquid repellent agent relative to the total amount of 100 parts by mass of the alkali-soluble binder polymer and the photopolymerizable monomer may be 0.05 to 10.0 parts by mass, 0.1 to 8.0 parts by mass, or 0.2 to 6.0 parts by mass. When the content of the liquid repellent agent is 0.05 to 10.0 parts by mass, it becomes easier to achieve both photosensitivity and internal photocurability.
[0057] The content of the liquid repellent agent relative to 100 parts by mass of the total amount of the photopolymerizable monomer and the liquid repellent agent may be 1.0 part by mass or more, 3.0 parts by mass or more, or 5.0 parts by mass or more. In this case, even if the exposure dose during exposure is low, the resolution of the partition walls can be effectively improved. The content of the liquid repellent agent relative to 100 parts by mass of the total amount of the photopolymerizable monomer and the liquid repellent agent may be 60.0 parts by mass or less, 50.0 parts by mass or less, or 30.0 parts by mass or less, in which case the resolution of the partition wall can be further improved and the spread of the pattern width can be suppressed.
[0058] (E) Polyfunctional thiol compound When the photosensitive resin layer obtained by exposing the photosensitive resin composition to light is heated, the polyfunctional thiol compound causes a radical chain reaction, and the reaction between the photopolymerizable monomers and between the photopolymerizable monomers and the mercapto group of the polyfunctional thiol compound proceeds moderately even after exposure, making it easier to harden the photosensitive resin layer. The polyfunctional thiol compound also forms a sufficient crosslinked structure in the exposed part of the partially cured layer, relieves the stress applied between the partition wall and the substrate, and maintains the adhesion of the partition wall to the substrate, thereby improving reliability. The polyfunctional thiol compound may contain two or more mercapto groups in one molecule, may contain three or more mercapto groups, or may contain four or more mercapto groups. When the polyfunctional thiol compound contains three or more mercapto groups in one molecule, the resolution of the partition wall can be further improved even if the exposure amount during exposure is low. The number of mercapto groups in one molecule may be up to 6. In this case, the film remaining property and pattern width of the partition wall can be easily controlled.
[0059] Examples of the polyfunctional thiol compound include primary polyfunctional thiols and secondary polyfunctional thiols. Among them, secondary polyfunctional thiols have high storage stability and can suppress odors.
[0060] Examples of secondary polyfunctional thiols include pentaerythritol tetrakis(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptobutyrate), and 1,3,5-tris[2-(3-mercaptobutanoyloxy)ethyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.
[0061] Examples of primary polyfunctional thiols include trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), and dipentaerythritol hexakis(3-mercaptopropionate).
[0062] The polyfunctional thiol compounds can be used alone or in combination of two or more.
[0063] The content ratio of the polyfunctional thiol compound relative to the total amount of 100 parts by mass of the alkali-soluble binder polymer and the photopolymerizable monomer may be 0.05 to 10.0 parts by mass, 0.1 to 8.0 parts by mass, or 0.2 to 6.0 parts by mass. When the content ratio of the polyfunctional thiol compound is 0.05 to 10.0 parts by mass, it becomes easier to achieve both photosensitivity and internal photocurability.
[0064] The content ratio of the polyfunctional thiol compound relative to 100 parts by mass of the total amount of the photopolymerizable monomer and the polyfunctional thiol compound may be 1.0 part by mass or more, 3.0 parts by mass or more, or 5.0 parts by mass or more. In this case, even if the exposure dose during exposure is low, the resolution of the partition wall can be effectively improved. The content of the polyfunctional thiol compound may be 60.0 parts by mass or less, 50.0 parts by mass or less, or 30.0 parts by mass or less. In this case, the resolution of the partition wall can be further improved, and the spread of the pattern width can also be suppressed.
[0065] (F) Coloring agent Examples of the colorant include pigments and dyes. The pigment may be either an organic pigment or an inorganic pigment, but may be an organic pigment. When the pigment is an organic pigment, the organic pigment can transmit ultraviolet light, so that light can reach a sufficiently deep position from the surface of the photosensitive resin layer during exposure, compared to the case where an inorganic pigment is used, and insufficient curing of the exposed part can be further suppressed. Therefore, dissolution or swelling of the cured part due to exposure during development can be further suppressed, and the resolution of the partition wall can be further improved. The photosensitive resin composition may contain two or more colorants.
[0066] Examples of organic pigments include lactam black, perylene black, and aniline black.
[0067] Examples of inorganic pigments include carbon black and titanium black.
[0068] The dyes include leuco dyes.
[0069] The content of the colorant in the total solid content is not particularly limited as long as it is greater than 0% by mass, but may be 4% by mass or more, or 6% by mass or more from the viewpoint of improving the light-shielding property of the partition wall to be formed. However, the content of the colorant in the total solid content may be 15% by mass or less, 12% by mass or less, or 4% by mass or less. When the content of the colorant in the total solid content is 15% by mass or less, the depth of light reaching from the surface can be increased during exposure of the photosensitive resin layer formed using the photosensitive resin composition, and insufficient curing of the exposed part can be suppressed. Therefore, dissolution or swelling of the cured part due to exposure during development with a developer is sufficiently suppressed. In particular, when the content of the colorant in the total solid content is 4% by mass or less, there is a tendency that the reduction in the thickness and width of the partition wall can be suppressed even after the partition wall is left under high temperature and high humidity.
[0070] (Other Ingredients) The photosensitive resin composition may further contain a solvent such as methanol, ethanol, acetone, methyl ethyl ketone, methyl cellosolve, ethyl cellosolve, toluene, N,N-dimethylformamide, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, etc., as necessary. These may be used alone or in combination of two or more. The amount of the solvent may be appropriately determined so that the total solid content concentration in the photosensitive resin composition is, for example, about 10 to 60 mass%.
[0071] The photosensitive resin composition may further contain additives such as plasticizers, fillers, defoamers, flame retardants, stabilizers, adhesion promoters, leveling agents, peeling promoters, antioxidants, fragrances, and thermal crosslinking agents, as necessary. Each of these may be used alone or in combination of two or more. The amount of each of these additives may be 0.01 to 20 parts by mass per 100 parts by mass of the total of the alkali-soluble binder polymer and the photopolymerizable monomer.
[0072] <Substrate with partition walls and its manufacturing method> Next, an embodiment of a substrate with partition walls according to another aspect of the present disclosure will be described with reference to Fig. 1 and Fig. 2. Fig. 1 is a partial cross-sectional view showing a substrate with partition walls obtained in a development step of an embodiment of a method for producing a substrate with partition walls according to the present disclosure, and Fig. 2 is a plan view showing the substrate with partition walls of Fig. 1.
[0073] 1 and 2, a partition-formed substrate 120 of this embodiment includes a substrate 10 and partitions 21 provided on the substrate 10. The partitions 21 have a plurality of openings 21a.
[0074] Next, an embodiment of a method for producing a substrate with partition walls according to the present disclosure will be described with reference to Fig. 3 to Fig. 6. Fig. 3 is a partial cross-sectional view showing a photosensitive resin layer formation step in the embodiment of the method for producing a substrate with partition walls according to the present disclosure, Fig. 4 is a partial cross-sectional view showing an exposure step in the embodiment of the method for producing a substrate with partition walls according to the present disclosure, Fig. 5 is a partial cross-sectional view showing a second laminate obtained in the exposure step of Fig. 4, and Fig. 6 is a partial cross-sectional view showing a heating step in the embodiment of the method for producing a substrate with partition walls according to the present disclosure.
[0075] The method for producing a substrate with partition walls of this embodiment includes a photosensitive resin layer formation step (see FIG. 3) of forming a photosensitive resin layer 20 on the substrate 10 using the photosensitive resin composition of this embodiment described above to obtain a first laminate 100, an exposure step (see FIGS. 4 and 5) of partially exposing the photosensitive resin layer 20 provided on the substrate 10 (partially irradiating the photosensitive resin layer 2 with light L) to form a partially cured layer 30 and obtain a second laminate 110, a heating step (see FIG. 6) of heating the partially cured layer 30 of the second laminate 110, and a development step (see FIG. 1) of alkaline-developing the partially cured layer 30 of the second laminate 110 and performing a post-curing step as necessary to form partition walls 21 and obtain a substrate with partition walls 120.
[0076] (Photosensitive resin layer formation process) Examples of the substrate 10 in the photosensitive resin layer forming step include a glass substrate, a sapphire substrate, and a plastic substrate such as polycarbonate or cycloolefin polymer.
[0077] The height of the photosensitive resin layer 20 from the substrate 10 varies depending on the application, but from the viewpoint of achieving both coatability and photocurability, the thickness after drying may be 1 μm or more, 5 μm or more, or 10 μm or more. The height of the photosensitive resin layer 20 from the substrate 10 may be, for example, 200 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less.
[0078] The photosensitive resin layer 20 can be formed by applying a solution of the above-mentioned photosensitive resin composition (coating liquid for forming a photosensitive resin layer) onto the substrate 10 and drying it. In this case, however, the amount of the organic solvent remaining in the photosensitive resin layer 20 may be 2 mass % or less in order to prevent the organic solvent from diffusing in a later step.
[0079] Coating can be performed by a known method such as roll coating, comma coating, gravure coating, air knife coating, die coating, bar coating, spray coating, spin coating, etc. After coating, drying to remove the organic solvent and the like can be performed at 70 to 150° C. for about 1 to 30 minutes using a hot air convection dryer or the like.
[0080] (Exposure process) The exposure method in the exposure step includes a method (mask exposure method) in which light (active light rays) are irradiated imagewise through a mask M having a plurality of openings in order to irradiate a predetermined portion of the photosensitive resin layer 20 with light (active light rays) (see FIG. 4). As a light source of the active light rays, known light sources, for example, carbon arc lamps, mercury vapor arc lamps, ultra-high pressure mercury lamps, high pressure mercury lamps, xenon lamps, and other light sources that effectively radiate ultraviolet light, visible light, and the like, can be used. In addition, Ar ion lasers, semiconductor lasers, and other light sources that effectively radiate ultraviolet light, visible light, and the like can also be used. Furthermore, photographic flood lamps, sun lamps, and other light sources that effectively radiate visible light can also be used. In addition, a method of irradiating active light rays imagewise by a direct drawing method using a laser exposure method or the like may be adopted. In this case, the mask M is not necessary.
[0081] The exposure dose in the exposure step varies depending on the apparatus used and the composition of the photosensitive resin layer 20, but from the viewpoint of excellent photocuring properties, a dose of 30 mJ / cm 2 or more than 50 mJ / cm 2 The exposure amount in the exposure step is preferably 500 mJ / cm or more in terms of resolution. 2 or less than 400 mJ / cm 2 It may be the following:
[0082] The exposure can be carried out in air, in vacuum, or the like, and the atmosphere for the exposure is not particularly limited.
[0083] After exposure, the photosensitive resin layer 20 becomes a partially cured layer 30. Specifically, the exposed portion of the photosensitive resin layer 20 becomes a cured portion, and the unexposed portion of the photosensitive resin layer 20 becomes a non-cured portion 22 (see FIG. 3).
[0084] (Heating process) The heating step is a step for appropriately proceeding the curing reaction between photopolymerizable monomers or between the photopolymerizable monomer and the photocurable group of the liquid repellent agent in the portion of the partition wall 21 on the substrate 10 side by heating the partially cured layer 30. By heating the partially cured layer 30, the polyfunctional thiol compound causes a radical chain reaction, so that the reaction between the photopolymerizable monomers and between the photopolymerizable monomer and the ultraviolet curable group of the liquid repellent agent proceeds appropriately and is easily cured, even after exposure.
[0085] In the heating step, when the partially cured layer 30 is heated, a hot plate H (see FIG. 4), a box-type dryer, a reflow furnace, a clean oven, or the like can be used as the heating means.
[0086] In the heating step, the temperature may be from 70 to 150° C., or from 85 to 130° C. The heating time may be from 1 to 30 minutes, or from 2 to 20 minutes.
[0087] (Development process) The developing step is a step of alkaline developing the partially cured layer 30 of the second laminate 110, and optionally performing a post-curing step to form the partition walls 21 to obtain the partition-wall-attached substrate 120. In the developing step, the non-cured portions 22 are removed, and the cured portions are left on the substrate 10, and these cured portions become the partition walls 21. The alkaline development in the development step is carried out by a known method such as spraying, shaking immersion, brushing, scrubbing, etc., using a developer such as an alkaline aqueous solution.
[0088] The developer may be any solution capable of dissolving an alkali-soluble binder polymer, and may be, for example, an alkaline aqueous solution that is safe, stable, and easy to handle. Examples of the base in the alkaline aqueous solution include alkali hydroxides such as hydroxides of lithium, sodium, potassium, or ammonium, alkali carbonates such as carbonates or bicarbonates of lithium, sodium, potassium, or ammonium, alkali metal phosphates such as potassium phosphate and sodium phosphate, and alkali metal pyrophosphates such as sodium pyrophosphate and potassium pyrophosphate.
[0089] The alkaline aqueous solution used for development may be a 0.1 to 5 mass% tetramethylammonium hydroxide (TMAH) aqueous solution, a 0.1 to 5 mass% sodium carbonate aqueous solution, a 0.1 to 5 mass% potassium carbonate aqueous solution, a 0.1 to 5 mass% sodium hydroxide aqueous solution, a 0.1 to 5 mass% sodium tetraborate aqueous solution, or the like. The pH of the alkaline aqueous solution used for development may be in the range of 9 to 11, and the temperature is adjusted according to the developability of the photosensitive resin layer 20. The alkaline aqueous solution may contain a surfactant, an antifoaming agent, a small amount of an organic solvent for promoting development, or the like.
[0090] Alternatively, an aqueous developer consisting of an alkaline aqueous solution and one or more organic solvents may be used. In this case, examples of the base contained in the alkaline aqueous solution include, in addition to the above-mentioned bases, borax, sodium metasilicate, ethanolamine, ethylenediamine, diethylenetriamine, 2-amino-2-hydroxymethyl-1,3-propanediol, 1,3-diaminopropanol-2, and morpholine. Examples of organic solvents include diacetone alcohol, acetone, ethyl acetate, alkoxyethanol having an alkoxy group having 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether. These may be used alone or in combination of two or more.
[0091] The above-mentioned developers may be used in combination of two or more kinds, if necessary.
[0092] Examples of the developing method include a dipping method, a paddle method, a spray method, brushing, scrubbing, etc. Among these, when the high pressure spray method is used, the resolution of the partition walls is improved. The development time is not particularly limited, and may be, for example, 3 seconds or more, or 5 seconds or more. When the development time is 5 seconds or more, overdevelopment is unlikely to occur, and manufacturing variations in the line width and thickness of the partition wall are reduced. The development time may be 300 seconds or less, or 200 seconds or less.
[0093] (Post-curing process) The post-curing step is a step of curing the cured portion after development. The exposure method in the post-curing step includes a method of irradiating the cured portion with light (actinic rays). The light source of the actinic rays can be the same as the light source used in the exposure step.
[0094] The exposure dose in the post-curing step varies depending on the equipment used and the composition of the curing part, but in terms of excellent photocuring properties, 100 mJ / cm 2 or more than 300mJ / cm 2 The exposure dose in the post-curing step may be 10,000 mJ / cm or more. 2 or less than 5000mJ / cm 2 It may be the following:
[0095] The post-curing step can be carried out in air, in vacuum, or the like, and the atmosphere for the post-curing step is not particularly limited.
[0096] When the post-curing step is carried out, the hardened portion which is further hardened by the post-curing step finally becomes the partition wall 21.
[0097] <Image display device> Next, an embodiment of an image display device according to the present disclosure will be described with reference to Fig. 7. Fig. 7 is a partial cross-sectional view showing an embodiment of an image display device according to the present disclosure.
[0098] As shown in FIG. 7, an image display device 400 of this embodiment includes a first structure 200 and a second structure 300. The first structure 200 and the second structure 300 are arranged in a row and a column. The first structure 200 includes a partition-equipped substrate 120 and a color filter 23 that fills at least a part of the opening 21a of the partition-equipped substrate 120. The second structure 300 includes a base material 310, a partition wall 31 provided on the base material 310 and having an opening 31a, and a micro LED 40 accommodated in the opening 31a of the partition wall 31 as a light-emitting element. The first structure 200 is provided on the partition 31 of the second structure 300, and the opening 31a of the partition 31 and the opening 21a of the partition 21 are arranged to overlap in the thickness direction of the first structure 200. Therefore, the light from the micro LED 40 passes through the base material 10 and then passes through the opening 21a of the partition 21 to be emitted.
[0099] According to the image display device 400, the manufacturing method of the partition-equipped substrate can improve the moisture and heat resistance reliability of the partition 21. Therefore, even in a high-temperature and high-humidity environment, it is possible to suppress a decrease in the thickness and width of the partition 21, and the color filter 23 can be stably held in the opening 21a of the partition 21. As a result, in the image display device 400, replacement of the partition-equipped substrate 120 is not required for a long period of time.
[0100] Micro LED 40 refers to a minute LED (semiconductor light emitting diode), an element for manufacturing an LED, a member for manufacturing an LED, a part incorporating an LED, an LED wafer, etc. Examples include LED elements using gallium nitride, indium gallium nitride, silicon, etc. The shape of the micro LED 40 is not particularly limited, and examples thereof include shapes in which the shape of the main surface is a square, a rectangle, a rhombus, a trapezoid, a polygon, and a shape having a curved surface such as a circle, an ellipse, and an arc. The micro LED 40 may also have a shape with projections and recesses in the thickness direction. The size of the micro LED 40 may be, for example, when the shape of the main surface is a square, the length of one side is 0.1 to 2000 μm, and when the shape of the main surface is a rectangle, the length of the long side is 0.2 μm to 2000 μm and the length of the short side is 0.1 to 1500 μm. The thickness of the micro LED 40 is, for example, 0.1 to 20 μm.
[0101] The micro LED 40 is disposed in an opening 31a formed in the partition 31 and electrically connected to the substrate 310. The micro LED 40 may be a micro LED formed on another substrate such as a sapphire substrate and cut out individually. The micro LED 40 may be appropriately selected from micro LEDs emitting blue light, micro LEDs emitting red light, and micro LEDs emitting green light. In this case, the height of the micro LED 40 from the substrate 310 may be equal to or less than the height of the partition 31 from the substrate 310. In this case, crosstalk caused by light from adjacent micro LEDs 40 can be further suppressed.
[0102] When a colorant is contained in the photosensitive resin composition used to form the partition walls 21, the colorant may be black from the viewpoint of further suppressing crosstalk.
[0103] A circuit board is used as the base material 310. The circuit board is configured to mount the micro LEDs 40 and to electrically connect the micro LEDs 40 to enable the micro LEDs 40 to be turned on and off.
[0104] The partition 31 may be made of a cured product of the photosensitive resin composition from which the liquid repellent agent is removed from the partition 21, but may be made of a material different from such a cured product. The partition 31 may contain a colorant. When the partition 31 contains a colorant, crosstalk between adjacent micro LEDs 40 can be suppressed.
[0105] <Manufacturing method for image display device> Next, an embodiment of a method for manufacturing an image display device according to the present disclosure will be described with reference to Fig. 8. Fig. 8 is a partial cross-sectional view showing a color filter formation step in the embodiment of a method for manufacturing an image display device according to the present disclosure.
[0106] The manufacturing method of the image display device of this embodiment includes a lamination process of laminating the first structure 200 and the second structure 300. In the lamination process, the micro LEDs 40 as light-emitting elements of the second structure 300 are disposed so as to face the openings 21a of the partition walls 21 of the first structure 200. The image display device 400 is obtained by laminating the first laminate 200 and the second structure 300 together.
[0107] According to the method for manufacturing the image display device 400, the moisture and heat resistance reliability of the partition walls 21 can be improved by the method for manufacturing the partition wall-equipped substrate. Therefore, in the obtained image display device 400, even in a high-temperature and high-humidity environment, the reduction in thickness and width of the partition walls 21 can be suppressed, and the color filters 23 can be stably held in the openings 21a of the partition walls 21. As a result, replacement of the partition wall-equipped substrate 120 becomes unnecessary for a long period of time.
[0108] The first structure 200 can be obtained by forming a substrate 120 with partition walls by the manufacturing method for a substrate with partition walls described above, and then filling at least one of the openings 21a of the partition walls 21 with ink and forming a color filter 23.
[0109] The second structure 300 can be obtained by forming a partition 31 having an opening 31a on a substrate 310 and accommodating the micro LED 40 in the opening 31a. The partition wall 31 can be obtained, for example, in the same manner as the partition wall 21. That is, the partition wall 31 can be obtained by applying a photosensitive resin composition onto a base material 310 to form a photosensitive resin layer, partially exposing the photosensitive resin composition to light to form a partially cured layer, and then developing the photosensitive resin layer.
[0110] In the above embodiment, the image display device according to the present disclosure is an image display device in which the light-emitting elements are micro LEDs. However, the light-emitting elements may be organic light-emitting elements or quantum dot light-emitting elements. EXAMPLES
[0111] The present disclosure will be described more specifically below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0112] <Preparation of alkali-soluble binder polymer solution> Alkali-soluble binder polymer solutions (hereinafter sometimes simply referred to as "binder polymer solutions") 1 to 7 were prepared as follows. The constituent units 1 to 8 of the alkali-soluble binder polymer (hereinafter sometimes simply referred to as "binder polymer") are as follows. Here, the constituent unit 1 is included in the constituent unit (a), the constituent unit 2 is included in the constituent unit (b), the constituent unit 3 is included in the constituent unit (c), and the constituent units 4 and 6 are included in the constituent unit (d). [ka] [ka]
[0113] (Binder polymer solution 1) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 180.1 g of propylene glycol monomethyl ether (PGME) was added as a solvent, and the mixture was stirred while replacing the gas in the flask with nitrogen gas and heated to 120°C. Next, a monomer mixture consisting of 39.6 g (0.18 mol) of tricyclodecanyl methacrylate, 3.52 g (0.02 mol) of benzyl methacrylate, and 68.8 g (0.80 mol) of methacrylic acid was prepared by adding 5.93 g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropping was completed, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a precursor solution of binder polymer 1 was synthesized. Thereafter, the gas in the flask was replaced with air, and 88.1 g (0.62 mol) of glycidyl methacrylate, 0.6 g of triphenylphosphine (catalyst), and 0.6 g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of binder polymer 1. Thereafter, the reaction was continued at 110° C. for 10 hours to obtain a resin solution. The binder polymer 1 contained in this resin solution had a weight average molecular weight of 13,100, a double bond equivalent of 340 g / mol, and a glass transition temperature (Tg) of 59° C. The proportions of the structural units 1 to 8 in the binder polymer 1 were as shown in Table 1, with the total of all the structural units 1 to 8 being taken as the standard (100 mol%). PGME was further added to this resin solution to prepare a binder polymer solution 1 (solid concentration 49.1% by mass) as a binder polymer solution. At this time, the binder polymer solution 1 was prepared so that the binder polymer 1 and PGME were mixed in the mass ratio shown in Table 2. The solid content means the heating residue when the binder polymer solution is heated at 130° C. for 2 hours, and the binder polymer 1 is the main component of the solid content.
[0114] (Binder polymer solution 2) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 180.1 g of propylene glycol monomethyl ether (PGME) was added as a solvent, and the mixture was stirred while replacing the gas in the flask with nitrogen gas and heated to 120°C. Next, a monomer mixture consisting of 2.20g (0.01 mol) of tricyclodecanyl methacrylate, 1.76g (0.01 mol) of benzyl methacrylate, and 84.3g (0.98 mol) of methacrylic acid was prepared by adding 7.77g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropping was completed, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a precursor solution of binder polymer 2 was synthesized. Thereafter, the gas in the flask was replaced with air, and 113.7g (0.80 mol) of glycidyl methacrylate, 0.6g of triphenylphosphine (catalyst), and 0.6g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of binder polymer 2. Thereafter, the reaction was continued at 110° C. for 10 hours to obtain a resin solution. The binder polymer 2 contained in this resin solution had a weight average molecular weight of 16,500, a double bond equivalent of 260 g / mol, and a glass transition temperature (Tg) of 37° C. The proportions of the structural units 1 to 8 in the binder polymer 2 were as shown in Table 1, with the total of all the structural units 1 to 8 being taken as the standard (100 mol%). PGME was further added to this resin solution to prepare a binder polymer solution 2 (solid content concentration: 44.1% by mass) as a binder polymer solution. At this time, the binder polymer solution 2 was prepared so that the binder polymer 2 and PGME were mixed in the mass ratio shown in Table 2. The solid content means the heating residue when the binder polymer solution 2 is heated at 130° C. for 2 hours, and the binder polymer 2 is the main component of the solid content.
[0115] (Binder polymer solution 3) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 180.1 g of PGME was added as a solvent, and the mixture was stirred while replacing the gas in the flask with nitrogen gas, and the temperature was raised to 120°C. Next, a monomer mixture consisting of 61.6 g (0.28 mol) of tricyclodecanyl methacrylate, 3.52 g (0.02 mol) of benzyl methacrylate, and 60.2 g (0.70 mol) of methacrylic acid was prepared by adding 5.64 g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropping was completed, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a precursor solution of binder polymer 3 was synthesized. Thereafter, the gas in the flask was replaced with air, and 73.9 g (0.52 mol) of glycidyl methacrylate, 0.6 g of triphenylphosphine (catalyst), and 0.6 g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of binder polymer 3. Thereafter, the reaction was continued at 110° C. for 10 hours to obtain a resin solution. The binder polymer 3 contained in this resin solution had a weight average molecular weight of 14,600, a double bond equivalent of 400 g / mol, and a glass transition temperature (Tg) of 73° C. The proportions of the structural units 1 to 8 in the binder polymer were as shown in Table 1, with the total of all structural units 1 to 8 being taken as the standard (100 mol%). PGME was further added to this resin solution to prepare a binder polymer solution 3 (solid content concentration: 46.0% by mass) as a binder polymer solution. At this time, the binder polymer solution 3 was prepared so that the binder polymer 3 and PGME were mixed in the mass ratio shown in Table 2.
[0116] (Binder polymer solution 4) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 152.5 g of PGMEA was added as a solvent, and the mixture was heated to 120°C with stirring while replacing the gas in the flask with nitrogen gas. Next, 6.60 g (0.03 moles) of tricyclodecanyl methacrylate and 7 g of styrene were added. A monomer mixture consisting of 127.9g (0.90 mol) of glycidyl methacrylate and 25.8g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, Perbutyl (registered trademark) O, manufactured by NOF Corporation) was separately prepared. This mixture of monomer and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropwise addition, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a precursor of binder polymer 4 was generated. Thereafter, the gas in the flask was replaced with air, and 64.8g (0.90 mol) of acrylic acid, 0.61g of triphenylphosphine (catalyst), and 0.31g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of binder polymer 4. Then, the reaction was continued at 110°C for 10 hours. Next, 60.0 g (0.60 mol) of succinic anhydride was added to the flask, and the reaction was continued for 3 hours at 110° C. to obtain a resin solution. The weight average molecular weight of binder polymer 4 contained in this resin solution was 6800, the double bond equivalent was 330 g / mol, and the glass transition temperature (Tg) of binder polymer 4 was 15° C. Furthermore, the proportions of each of the structural units 1 to 8 in binder polymer 4 were as shown in Table 1, with the total of all structural units 1 to 8 being taken as the standard (100 mol%). PGMEA was further added to this resin solution to prepare a binder polymer solution 4 (solid content concentration: 43.2% by mass) as a binder polymer solution. At this time, the binder polymer solution 4 was prepared so that the binder polymer 4 and PGMEA were mixed in the mass ratio shown in Table 2.
[0117] (Binder polymer solution 5) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 167.1 g of PGMEA was added as a solvent, and the mixture was heated to 120°C with stirring while replacing the gas in the flask with nitrogen gas. Next, a monomer mixture consisting of 66.0 g (0.30 mol) of tricyclodecanyl methacrylate, 10.4 g (0.10 mol) of styrene, and 85.2 g (0.60 mol) of glycidyl methacrylate was prepared by adding 34.2 g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropping was completed, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a precursor of binder polymer 5 was generated. Thereafter, the gas in the flask was replaced with air, and 43.2 g (0.60 mol) of acrylic acid, 0.61 g of triphenylphosphine (catalyst), and 0.31 g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of binder polymer 5. Then, the reaction was continued at 110°C for 10 hours. Next, 16.0 g (0.16 mol) of succinic anhydride was added to the flask, and the reaction was continued for 3 hours at 110° C. to obtain a resin solution. The binder polymer 5 contained in this resin solution had a weight average molecular weight of 7,300, a double bond equivalent of 410 g / mol, and a glass transition temperature (Tg) of 56° C. The proportions of the structural units 1 to 8 in the binder polymer 5 were as shown in Table 1, assuming the total of all the structural units 1 to 8 as the standard (100 mol%). PGMEA was further added to this resin solution to prepare a binder polymer solution 5 (solid content concentration: 56.6% by mass) as a binder polymer solution. At this time, binder polymer solution 5 was prepared so that binder polymer 5 and PGMEA were mixed in the mass ratio shown in Table 2.
[0118] (Binder polymer solution 6) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 167.1 g of PGMEA was added as a solvent, and the mixture was heated to 120°C with stirring while replacing the gas in the flask with nitrogen gas. Next, a monomer mixture consisting of 66.0 g (0.30 mol) of tricyclodecanyl methacrylate, 10.4 g (0.10 mol) of styrene, and 85.2 g (0.60 mol) of glycidyl methacrylate was prepared by adding 10.3 g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropping was completed, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a precursor of binder polymer 6 was generated. Thereafter, the gas in the flask was replaced with air, and 43.2 g (0.60 mol) of acrylic acid, 0.61 g of triphenylphosphine (catalyst), and 0.31 g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of binder polymer 6. Then, the reaction was continued at 110°C for 10 hours. Next, 33.0 g (0.33 mol) of succinic anhydride was added to the flask, and the reaction was continued for 3 hours at 110° C. to obtain a resin solution. The weight average molecular weight of binder polymer 6 contained in this resin solution was 8700, the double bond equivalent was 440 g / mol, and the glass transition temperature (Tg) of binder polymer 6 was 48° C. Furthermore, the proportions of each of the structural units 1 to 8 in binder polymer 6 were as shown in Table 1, with the total of all structural units 1 to 8 being taken as the standard (100 mol%). PGMEA was further added to this resin solution to prepare a binder polymer solution 6 (solid concentration: 57.6% by mass) as a binder polymer solution. At this time, the binder polymer solution 6 was prepared so that the binder polymer 6 and PGMEA were mixed in the mass ratio shown in Table 2.
[0119] (Binder polymer solution 7) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 167.1 g of PGMEA was added as a solvent, and the mixture was heated to 120°C with stirring while replacing the gas in the flask with nitrogen gas. Next, a monomer mixture consisting of 66.0 g (0.30 mol) of tricyclodecanyl methacrylate, 10.4 g (0.10 mol) of styrene, and 85.2 g (0.60 mol) of glycidyl methacrylate was prepared by adding 19.4 g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropwise addition, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a precursor of binder polymer 7 was produced. Thereafter, the gas in the flask was replaced with air, and 41.9 g (0.58 mol) of acrylic acid, 0.61 g of triphenylphosphine (catalyst), and 0.31 g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of binder polymer 7. Then, the reaction was continued at 110°C for 10 hours. Next, 68.4 g (0.45 mol) of tetrahydrophthalic anhydride was added to the flask, and the reaction was continued for 3 hours at 110° C. to obtain a resin solution. The binder polymer 7 contained in this resin solution had a weight average molecular weight of 8,300, a double bond equivalent of 500 g / mol, and a glass transition temperature (Tg) of 39° C. The proportions of the structural units 1 to 8 in the binder polymer 7 were as shown in Table 1, assuming the total of all the structural units 1 to 8 as the standard (100 mol%). PGMEA was further added to this resin solution to prepare a binder polymer solution 7 (solid concentration: 57.6% by mass) as a binder polymer solution. At this time, the binder polymer solution 7 was prepared so that the binder polymer 7 and PGMEA were mixed in the mass ratios shown in Tables 2 to 4.
[0120] <Method of measuring physical properties> The above double bond equivalent, weight average molecular weight and glass transition temperature are values obtained by the methods described below. (1) Double bond equivalent The double bond equivalent is the mass of a polymer per mole of a polymerizable unsaturated bond, and is a calculated value calculated based on the amount of monomer used. (2) Weight average molecular weight (Mw) The weight average molecular weight means a weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions and converted into standard polystyrene. Column: Showdex (registered trademark) LF-804 + LF-804 (manufactured by Showa Denko K.K.) Column temperature: 40℃ Sample: 0.2% solution of copolymer in tetrahydrofuran Developing solvent: Tetrahydrofuran Detector: Differential refractometer (Shodex (registered trademark) RI-71S) (manufactured by Showa Denko K.K.) Flow rate: 1mL / min (3) Glass transition temperature (Tg) The Tg of the binder polymer was measured using a differential scanning calorimeter (DSC7000X, manufactured by Hitachi High-Tech Science Corporation). Specifically, 1 g of each binder polymer solution was collected, dried at 130°C for 120 minutes to volatilize the solvent, and 10 mg of each sample was collected from each solid obtained. Then, using a differential scanning calorimeter (DSC), the temperature of the sample was changed from -0°C to 200°C at a heating rate of 10°C / min to perform differential scanning calorimetry, and the endothermic start temperature due to the observed glass transition was taken as the glass transition temperature (Tg). When two Tgs were observed, the average value of the two Tgs was taken as the Tg of the binder polymer.
[0121] [Table 1]
[0122] <Examples 1 to 12 and Comparative Examples 1 to 3> [Preparation of photosensitive resin composition] The components (A), (B), (C), (D), (E), (F) and (G) shown in Table 2, Table 3 or Table 4 were blended to obtain the content ratios (unit: parts by mass) shown in the same table, and mixed for 15 minutes using a stirrer to prepare a coating liquid for forming a photosensitive resin layer as a photosensitive resin composition.
[0123] [Table 2]
[0124] [Table 3]
[0125] [Table 4]
[0126] In Table 2, Table 3 or Table 4, details of the components (A), (B), (C), (D), (E), (F) and (G) are as follows: Component (A) Solutions 1 to 7: Binder polymer solutions 1 to 7 prepared by the above-mentioned method
[0127] (B) Component Photopolymerizable monomer: Pentaerythritol tri- and tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "A-TMM-3")
[0128] (C) Component Photopolymerization initiator: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (product name: "Lunacure TPO", manufactured by DKSH Japan Co., Ltd.)
[0129] (D) Component Liquid repellent 1: Megafac RS-72-A, manufactured by DIC Corporation Liquid repellent 2: Viscoat 13F (1H,1H,2H,2H-tridecafluorooctyl acrylate), manufactured by Osaka Organic Industry Co., Ltd. Liquid repellent 3: Pentafluorotoluene
[0130] (E) Component Multifunctional thiol compound: pentaerythritol tetrakis(3-mercaptobutyrate) (KarenzMT (registered trademark) PE1 (number of SH groups = 4), manufactured by Showa Denko K.K.)
[0131] Ingredient (F) A mixture of lactam black (solid content) represented by the following structural formula as a pigment, a non-amine-based dispersant (solid content) as a dispersant, and PGMEA in a ratio of 15.0:4.5:80.5 (mass ratio) (lactam black organic pigment dispersion (product name "SF BLACK BJ4379", Sanyo Pigment Co., Ltd., solid content: 19.5 mass%, lactam black organic pigment: 15 mass%))
[0132] (G) Component Adhesion aid: Si coupling agent (product name "KBM-803", manufactured by Shin-Etsu Chemical Co., Ltd.)
[0133] [Formation of bulkhead] The photosensitive resin layer forming coating solution obtained as described above was dropped onto a glass plate having a thickness of 3.0 mm, and a coating film was formed by spin coating to obtain a laminate having a coating film on the glass plate. Then, this laminate was placed on a hot plate and heated at 120°C for 2 minutes to remove the solvent, and a first laminate having a photosensitive resin layer was produced. When obtaining the first laminate, the thickness of the coating film was adjusted by adjusting the rotation speed in the spin coating method so that the thickness of the photosensitive resin layer was 20±1 μm. Next, the first laminate was partially exposed to ultraviolet light using an ultraviolet exposure machine (product name "MA-20", manufactured by Mikasa Co., Ltd.) through a grid-shaped glass mask (manufactured by Shin-ei Co., Ltd.) as a photomask, to obtain a second laminate having a partially cured layer. At this time, the glass mask used had a space width (S) of 40 μm and a line width (L) of 40 μm. The ultraviolet light exposure amount (UV exposure amount) was the value shown in Table 2, Table 3, or Table 4 (unit: mJ / cm2). 2 ) was decided. Next, the second laminate was placed on a hot plate and heated (post-baked) at 100° C. for 1 minute as shown in Table 2, Table 3 or Table 4. Next, the second laminate was placed on an adsorption stage, and spray development was performed using a developing machine (product name "AD-1200", manufactured by Mikasa Co., Ltd.), followed by washing to obtain a third laminate having only the cured portion on the glass plate. In this case, spray development was performed using a 2.38% TMAH (tetramethylammonium hydroxide) aqueous solution as the developing solution at 23°C for the developing time shown in Table 2, Table 3 or Table 4. Here, the developing time is the minimum time required for the uncured portion of the partially cured layer to completely dissolve in the developing solution. In addition, water washing was performed for 30 seconds using pure water at 23°C. Thereafter, the third laminate was exposed to ultraviolet light over the entire surface using an ultraviolet light exposure machine (product name "MA-20", manufactured by Mikasa Co., Ltd.). At this time, the exposure dose was 1000 mJ / cm 2 It was decided. In this manner, a substrate with partition walls having a thickness of 20 μm was formed on the glass plate.
[0134] <Performance evaluation> The partition walls of the substrate with partition walls were evaluated for their reliability in terms of moisture and heat resistance, and the water repellency of the photosensitive resin composition after curing was also evaluated, as described below.
[0135] (1) Moisture and heat resistance reliability The substrate with partition walls prepared as described above was left to stand in an environment of 85° C. and 85% RH for 500 hours. The remaining film ratio (%) in the thickness direction of the partition wall was calculated based on the following formula. The results are shown in Tables 2, 3 and 4. Remaining film rate (%)=100×a1 / a0 (In the above formula, a0 represents the initial partition wall thickness (μm), and a1 represents the partition wall thickness (μm) after being left in an environment of 85° C. and 85% RH for 500 hours.) The increase rate (%) of the bank width was calculated based on the following formula, taking the distance between the opposing partition walls as the bank width. The results are shown in Tables 2, 3, and 4. Note that the larger the increase rate of the bank width, the higher the decrease rate of the partition wall width. Bank width increase rate (%) = 100 × (b1-b0) / b0 (In the above formula, b0 represents the initial bank width (μm), and b1 represents the bank width (μm) after being left in an environment of 85°C and 85% RH for 500 hours.)
[0136] (2) Water repellency after curing of the photosensitive resin composition The photosensitive resin layer forming coating solution obtained as described above was dropped onto a glass plate having a thickness of 3.0 mm, and a coating film was formed by spin coating to obtain a laminate having a coating film on the glass plate. Then, this laminate was placed on a hot plate and heated at 120°C for 2 minutes to remove the solvent, and a first laminate having a photosensitive resin layer was produced. When obtaining the first laminate, the thickness of the coating film was adjusted by adjusting the rotation speed in the spin coating method so that the thickness of the photosensitive resin layer was 20±1 μm. Next, the first laminate was exposed to ultraviolet light over the entire surface using an ultraviolet exposure machine (product name "MA-20", manufactured by Mikasa Co., Ltd.) to obtain a second laminate having a cured layer. At this time, the exposure dose was the value (unit: mJ / cm2) shown in Table 2, Table 3 or Table 4. 2 ) was decided. Next, the second laminate was placed on a hot plate and heated (post-baked) at 100° C. for 1 minute as shown in Table 2, Table 3 or Table 4. Next, the entire surface of the second laminate was exposed to ultraviolet light using an ultraviolet light exposure machine (product name "MA-20", manufactured by Mikasa Co., Ltd.). At this time, the exposure dose was 1000 mJ / cm 2 It was decided. In this way, a substrate for contact angle measurement was obtained, which had a cured portion having a thickness of 20 μm formed on the glass plate. Next, 2.0 μL of PGMEA was dropped onto the surface of the contact angle measurement substrate obtained as described above under conditions of 23° C. and 50% humidity using a Drop Master 500 (contact angle measurement device) manufactured by Kyowa Interface Science Co., Ltd., and the contact angle (against PGMEA) after 1 second was measured as the initial contact angle. The results are shown in Tables 2, 3, and 4. In addition, after 500 hours had passed, 2.0 μL of PGMEA was dropped onto the surface of the contact angle measurement substrate obtained as described above under conditions of 23° C. and 50% humidity, and the contact angle (vs. PGMEA) after 1 second was measured as the contact angle after 500 hours in the same manner as described above. The results are shown in Tables 2, 3, and 4. Similarly, 2.0 μL of QD ink (containing a (meth)acrylate compound) was dropped onto the surface of the contact angle measurement substrate obtained as described above, and the contact angle (with respect to the QD ink) was measured 1 second later. The results are shown in Tables 2, 3, and 4. In addition, after 500 hours had passed, 2.0 μL of QD ink (containing a (meth)acrylate compound) was dropped onto the surface of the contact angle measurement substrate obtained as described above under conditions of 23° C. and 50% humidity in the same manner as described above, and the contact angle (against PGMEA) after 1 second was measured as the contact angle after 500 hours. The results are shown in Tables 2, 3, and 4.
[0137] The results shown in Table 2 show that the photosensitive resin compositions of Examples 1 to 6 suppressed the decrease in the residual film rate and suppressed the increase in the bank width to a small extent compared to the photosensitive resin composition of Comparative Example 1, and therefore were able to improve the moist heat resistance reliability of the partition walls obtained by curing. Furthermore, from the results shown in Table 3, it was found that the photosensitive resin compositions of Examples 7 to 9, which used liquid repellents different from those of Examples 1 to 6 and Comparative Example 1, suppressed the decrease in the residual film rate and reduced the increase rate of the bank width compared to the photosensitive resin composition of Comparative Example 2, and therefore were able to improve the moist heat resistance reliability of the partition walls obtained by curing. Furthermore, from the results shown in Table 4, it was found that the photosensitive resin compositions of Examples 10 to 12, which used liquid repellents different from those of Examples 1 to 9 and Comparative Examples 1 and 2, suppressed the decrease in the residual film rate and reduced the increase rate of the bank width compared to the photosensitive resin composition of Comparative Example 3, thereby improving the moist heat resistance reliability of the partition walls obtained by curing.
[0138] From the above, it was confirmed that the photosensitive resin composition of the present disclosure can improve the moisture and heat resistance reliability of the partition walls obtained by curing. [Explanation of symbols]
[0139] Reference Signs List 10: substrate, 20: photosensitive resin layer, 21: partition wall, 21a: opening, 23: color filter, 30: partially cured layer, 40: micro LED (light-emitting element), 120: substrate with partition wall, 200: first structure, 300: second structure, 400: image display device.
Claims
1. An alkali-soluble binder polymer; a photopolymerizable monomer having an ethylenically unsaturated group; A liquid repellent agent containing a photocurable group; A photopolymerization initiator is included, The alkali-soluble binder polymer has a double bond equivalent of 250 to 440 g / mol.
2. 2. The photosensitive resin composition according to claim 1, wherein the alkali-soluble binder polymer has a double bond equivalent of 250 to 400 g / mol.
3. The photosensitive resin composition according to claim 1, wherein the alkali-soluble binder polymer comprises a structural unit (a) represented by the following formula (1), a structural unit (b) represented by the following formula (2), a structural unit (c) represented by the following formula (3), and a structural unit (d) represented by the following formula (4): 【Chemistry 1】 (In the above formula (1), R 1 represents a hydrogen atom or a methyl group, and X represents an alicyclic hydrocarbon group which may have a substituent. 【Chemistry 2】 (In the above formula (2), R 2 represents a hydrogen atom or a methyl group, and Y represents an aromatic group which may have a substituent. 【Chemistry 3】 (In the above formula (3), R 3 represents a hydrogen atom or a methyl group. 【Chemistry 4】 (In the above formula (4), R 4 and R 5 each independently represents a hydrogen atom or a methyl group.
4. The photosensitive resin composition according to claim 1 , further comprising a polyfunctional thiol compound, the polyfunctional thiol compound having three or more mercapto groups in one molecule.
5. 2. The photosensitive resin composition according to claim 1, wherein the photopolymerizable monomer has three or more functional groups in one molecule, and the three or more functional groups include the ethylenically unsaturated group and a hydroxyl group.
6. The photosensitive resin composition according to claim 1 , further comprising a colorant, the colorant being an organic pigment.
7. The photosensitive resin composition according to claim 1 , wherein the photopolymerization initiator comprises an acylphosphine oxide-based photopolymerization initiator.
8. A cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 7.
9. A photosensitive resin layer forming step of forming a photosensitive resin layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 7; an exposure step of partially exposing the photosensitive resin layer provided on the base material to light to form a partially cured layer; a heating step of heating the partially cured layer; a developing step of forming a partition wall having at least one opening by performing alkali development on the partially cured layer; A method for manufacturing a substrate with partition walls, comprising:
10. A substrate with partition walls, obtained by the method for producing a substrate with partition walls according to claim 9 .
11. A first structure; a second structure laminated on the first structure, The first structure is The partition wall-equipped substrate according to claim 10 , a color filter provided in at least one of the openings of the partition wall of the partition wall-formed substrate, The second structure includes a light-emitting element at a position facing the opening of the partition wall of the first structure.
12. A lamination step of laminating a first structure and a second structure, The first structure is The partition wall-equipped substrate according to claim 10 , a color filter that is filled in at least a part of the opening of the partition wall of the partition wall-formed substrate, the second structure has a light emitting element; In the laminating step, the light emitting element of the second structure is disposed so as to face the opening of the partition wall of the first structure.
Citation Information
Patent Citations
Photosensitive resin composition, cured product, and image display device
JP2021051235A