Thermal transfer recording medium

The thermal transfer recording medium with a compatible polyester and acid-modified polyolefin resin adhesive layer addresses the issue of pressure contamination on tubes, enabling high-quality printing on both vinyl chloride and non-vinyl chloride tubes.

JP2024157480APending Publication Date: 2024-11-07FUJI COPIAN
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023071892
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing thermal transfer recording media fail to achieve good printing on both vinyl chloride and non-vinyl chloride tubes, and often result in pressure contamination on the tube end surface due to strong pressure applied by the thermal head.

Method used

A thermal transfer recording medium with a colored layer containing a polyester resin and a colorant, and an adhesive layer composed of acid-modified polyolefin resin and polyester resin that are compatible with each other, with specific ratios and components to ensure adhesion and prevent pressure stains.

Benefits of technology

Enables high-quality thermal transfer printing on various tubes without pressure contamination, allowing fine images to be formed on both vinyl chloride and non-vinyl chloride tubes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157480000001_ABST
    Figure 2024157480000001_ABST
Patent Text Reader

Abstract

To provide a thermofusion transfer type thermal transfer recording medium for tube printing which enables good printing on various tubes such as a vinyl chloride-made tube and a non-vinyl chloride-made tube, and prevents pressure-contacting stains during thermal transfer printing.SOLUTION: A thermal transfer recording medium for tube printing in which a colored layer and an adhesive layer are laminated in this order on one surface of a base material contains at least a polyester resin and a coloring agent in the colored layer, and contains at least an acid-modified polyolefin resin and a polyester resin that are compatible with each other in the adhesive layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermal transfer recording medium for tube printing, which is used for printing on various tubes by a thermal melt transfer method. [Background technology]

[0002] 2. Description of the Related Art Conventionally, at work sites such as electrical construction sites and factory equipment maintenance sites, in order to identify and mark electric wires connected to terminal blocks on control panels, switchboards, control boxes, and the like, various types of tubes on which printed images such as wire numbers and symbols are formed using a tube printing printer that uses a thermal transfer recording medium are attached to the electric wires.

[0003] As tubes to be thermally transferred printed by a tube printing printer, various types of tubes such as polyvinyl chloride tubes and non-polyvinyl chloride tubes are used.

[0004] Until now, thermal transfer recording media for tube printing have been able to print well on polyvinyl chloride tubes but not on non-polyvinyl chloride tubes, or, even if they were able to print on various types of tubes, when printing on various types of tubes that are elastic and hollow inside, problems such as the occurrence of pressure-contact stains on the end surface of the tube that is crushed by the thermal head (the thermal transfer recording medium and the tube are pressed together by the thermal head, and on the end surface of the tube where strong pressure is applied, part of the thermal transfer layer in the unheated part of the thermal transfer recording medium is pressure-sensitively transferred to the tube by pressure alone, causing stains) (shown in Figure 2) have been encountered, and there has not been a thermal transfer recording medium that can print well on various types of tubes.

[0005] Patent Document 1 discloses a thermal transfer recording medium comprising a substrate, a colored layer, and an adhesive layer in this order, the colored layer containing a colorant and a specific polyester resin, and the adhesive layer containing a polyester resin. However, when the thermal transfer recording medium was used in a printer for tube printing, good character printing was not obtained on non-vinyl chloride tubes, and pressing stains occurred on the end face of the tube when characters were printed on vinyl chloride tubes.

[0006] Patent Document 2 discloses a thermal transfer recording medium comprising a substrate, a colored layer, and an adhesive layer in this order, the colored layer containing a colorant and a polyester resin, and the adhesive layer containing a propylene-based polyolefin resin. However, when the thermal transfer recording medium was used in a printer for tube printing, good character printing was not obtained on polyvinyl chloride tubes. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2017-121734 [Patent Document 2] Patent Publication No. 2017-154393 Summary of the Invention [Problem to be solved by the invention]

[0008] The problem that the present invention aims to solve is to provide a thermal transfer recording medium for tube printing used for printing on various tubes by a thermal melt transfer method, which enables good thermal transfer printing on various tubes such as polyvinyl chloride tubes and non-polyvinyl chloride tubes, and which does not cause pressure stains on the end face of the tube during thermal transfer printing. [Means for solving the problem]

[0009] The first invention is a thermal transfer recording medium for tube printing, which has a colored layer and an adhesive layer laminated in that order on one side of a substrate, and is characterized in that the colored layer contains at least a polyester resin and a colorant, and the adhesive layer contains at least an acid-modified polyolefin resin and a polyester resin that are compatible with each other.

[0010] The second invention is a thermal transfer recording medium for tube printing described in the first invention, characterized in that the acid-modified polyolefin resin in the adhesive layer is a copolymer containing ethylene and / or propylene as an olefin component and maleic anhydride and / or acrylic acid as an unsaturated carboxylic acid component.

[0011] The third invention is a thermal transfer recording medium for tube printing according to the first invention, characterized in that the acid-modified polyolefin resin in the adhesive layer is a copolymer containing ethylene and / or propylene as an olefin component, maleic anhydride and / or acrylic acid as an unsaturated carboxylic acid component, and any one or more of methyl acrylate, ethyl acrylate, dimethyl maleate, and diethyl maleate as an ester component.

[0012] A fourth invention is the thermal transfer recording medium for tube printing according to the first invention, characterized in that the mass ratio of the acid-modified polyolefin resin / polyester resin in the adhesive layer is in the range of 20 / 80 to 90 / 10.

[0013] A fifth invention is the thermal transfer recording medium for tube printing according to the first invention, characterized in that the acid value of the acid-modified polyolefin resin in the adhesive layer is in the range of 12 to 30 mgKOH / g. Effect of the Invention

[0014] In the present invention, in a thermal transfer recording medium for tube printing, a colored layer and an adhesive layer are laminated in this order on one side of a substrate, the colored layer contains at least a polyester resin and a colorant, and the adhesive layer contains at least an acid-modified polyolefin resin and a polyester resin that are compatible with each other. This makes it possible to provide a thermal transfer recording medium for tube printing that enables good thermal transfer printing on various tubes such as polyvinyl chloride tubes and non-polyvinyl chloride tubes, and that does not cause pressure stains on the end face of the tube during thermal transfer printing. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a thermal transfer recording medium of the present invention. [Diagram 2] FIG. 13 is a diagram showing pressure stains that occur during thermal transfer printing with a printer for tube printing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the thermal transfer recording medium of the present invention will be described in detail.

[0017] The thermal transfer recording medium of the present invention has a thermal transfer layer structure in which a colored layer and an adhesive layer are laminated in this order on one side of a substrate, as shown in Figure 1. It is preferable to provide a heat-resistant slip layer on the other side of the substrate.

[0018] (base material) The substrate used in the thermal transfer recording medium of the present invention may be a polyester film such as a polyethylene terephthalate film or a polyethylene naphthalate film, a polycarbonate film, a polyimide film, a polyamide film, an aramid film, or any other plastic film generally used as a substrate film for this type of thermal transfer recording medium. Among these, it is preferable to use a polyethylene terephthalate film from the viewpoints of physical properties, processability, cost, etc. The thickness of the substrate is usually about 2 to 12 μm, and in order to improve heat transfer, it is preferably in the range of 2 to 6 μm.

[0019] The surface of the substrate may be subjected to a surface treatment, if necessary, to improve adhesion with adjacent layers. Examples of the surface treatment include conventionally known surface treatment techniques such as corona discharge treatment, ultraviolet irradiation treatment, plasma treatment, and primer treatment.

[0020] (colored layer) The colored layer is a layer composed of at least a polyester resin and a colorant. By containing the polyester resin, good printed images can be formed on various tubes and the formed printed images have good abrasion resistance and solvent resistance.

[0021] The polyester resin refers to a polymer containing an ester group obtained by polycondensation of a polycarboxylic acid and a polyhydric alcohol.

[0022] Examples of polyvalent carboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, and biphenyldicarboxylic acid; saturated dicarboxylic acids such as oxalic acid, succinic acid, succinic anhydride, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, eicosane diacid, and hydrogenated dimer acid; unsaturated aliphatic dicarboxylic acids such as fumaric acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, citraconic acid, citraconic anhydride, and dimer acid; and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 2,5-norbornenedicarboxylic acid and anhydrides thereof, and tetrahydrophthalic acid and anhydride thereof.

[0023] Examples of polyhydric alcohols include aliphatic glycols such as ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, and 2-ethyl-2-butylpropanediol; alicyclic glycols such as 1,4-cyclohexanedimethanol; diethylene glycol, triethylene glycol, and dipropylene glycol; and glycols obtained by adding 1 to several moles of ethylene oxide or propylene oxide to two phenolic hydroxyl groups of bisphenols, such as ether bond-containing glycols such as 2,2-bis(4-hydroxyethoxyphenyl)propane.

[0024] One or more of these polyester resins can be used. The glass transition temperature (Tg) of the polyester resin is preferably in the range of 50 to 90°C, more preferably in the range of 60 to 80°C. When Tg is within the above range, the thermal transfer recording medium has good blocking resistance when stored in a rolled state, and a fine thermal transfer printed image can be formed on various tubes without a decrease in thermal transfer sensitivity. The Tg described in this specification is a value determined by differential scanning calorimetry (DSC) in accordance with JIS K 7121. The number average molecular weight (Mn) of the polyester resin is preferably in the range of 1500 to 30000. When Mn is within the above range, the formed thermal transfer printed image has good abrasion resistance and solvent resistance, and a fine thermal transfer printed image can be formed on various tubes without a decrease in thermal transfer sensitivity. The Mn described in this specification is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0025] The content of the polyester resin in the colored layer is preferably within a range of 45 to 85% by mass of the solid content of the colored layer. When the content of the polyester resin is within this range, the formed thermal transfer printed image has good abrasion resistance and solvent resistance.

[0026] As the binder for the colored layer, thermoplastic resins, waxes, etc. can be added in addition to polyester resins, within the range in which the effects of the present invention are not reduced. Examples of thermoplastic resins include acrylic resins, epoxy resins, styrene resins, petroleum resins, ketone resins, acetophenone formaldehyde resins, etc. Examples of waxes include polyethylene wax, oxidized polyethylene wax, carnauba wax, montan wax, etc. The thermoplastic resins and waxes are not necessarily limited to these, and can be used alone or in a mixture of two or more kinds.

[0027] As the colorant, for example, an appropriate one such as an organic or inorganic pigment, metal powder, etc. Specific examples thereof include organic pigments such as azo pigments, phthalocyanine pigments, triphenylmethane pigments, metal complex pigments, vat dye pigments, quinacridone pigments, and isoindolinone pigments. Examples of inorganic pigments include black materials such as carbon black, titanium black, chromium oxide, cobalt oxide, iron oxide, manganese oxide, chromates, and permanganates; red materials such as manganese oxide-alumina, chromium oxide-tin oxide, iron oxide, cadmium sulfide, and selenium sulfide; blue materials such as cobalt oxide, zirconia-vanadium oxide, chromium oxide-divanadium pentoxide; yellow materials such as zirconium-silicon-praseodymium, vanadium-tin, chromium-titanium-antimony; green materials such as chromium oxide, cobalt-chromium, and alumina-chromium; and pink materials such as aluminum-manganese, iron-silicon-zirconium.

[0028] In addition, the colored layer may contain various known additives such as a dispersant, a leveling agent, and a filler, if necessary.

[0029] The content of the colorant in the colored layer is preferably in the range of 15 to 55% by mass of the solid content of the colored layer. In particular, when carbon black is used as the colorant, the content is more preferably in the range of 30 to 50% by mass. When the content of the colorant is within the above range, the density of the thermal transfer printed image of various tubes is sufficient, pressure stains do not occur on the end face of the tube during thermal transfer printing, and the abrasion resistance and solvent resistance of the formed thermal transfer printed image are also good.

[0030] The thickness of the colored layer (thickness after drying, the same applies below) is desirably in the range of 0.5 to 3.0 μm from the viewpoint of the density of the thermal transfer printing image and the thermal transfer sensitivity.

[0031] The colored layer can be formed by dispersing or dissolving the above-mentioned materials in a suitable solvent such as methyl ethyl ketone, toluene, xylene, water, etc. to prepare a coating liquid for the colored layer, and coating the coating liquid on the substrate by a known means such as roll coating, reverse roll coating, gravure coating, reverse gravure coating, bar coating, or rod coating to form a coating film, which is then dried.

[0032] (adhesive layer) The adhesive layer is a layer disposed on the colored layer, and is a layer made of an acid-modified polyolefin resin and a polyester resin that are compatible with each other. Since the adhesive layer is made of an acid-modified polyolefin resin and a polyester resin that are compatible with each other, the coating surface of the adhesive layer after coating and drying becomes a uniform surface. This makes it possible to form a fine thermal transfer printing image without chipping even when printing a fine image such as a thin line of 1 dot (width 0.085 mm, the minimum line width drawn by a dot at a printing resolution of 300 dpi) on various tubes such as polyvinyl chloride tubes and non-polyvinyl chloride tubes, and also to eliminate pressure contact stains on the end surface of the tube during thermal transfer printing. The total content of the acid-modified polyolefin resin and the polyester resin in the adhesive layer is preferably 70% by mass or more in the solid content of the adhesive layer. When the total content of the acid-modified polyolefin resin and the polyester resin is within the above range, it is easy to form a fine thermal transfer printing image on various tubes. In addition, when the acid-modified polyolefin resin and the polyester resin are combined in a mutually incompatible manner, the coating surface of the adhesive layer after coating and drying will be a phase-separated, uneven, and uneven surface, such as a sea-island structure, and the acid-modified polyolefin resin parts and polyester resin parts will be scattered, causing transfer defects when printing fine images such as one-dot thin lines.

[0033] The acid-modified polyolefin resin is a resin modified by polymerizing a polyolefin resin such as polyethylene or polypropylene with an acid component such as carboxylic acid, and one or more kinds of acid-modified polyolefin resins can be used.

[0034] As the olefin component of the acid-modified polyolefin resin, from the viewpoint of adhesion to various tubes, alkenes having 2 to 6 carbon atoms such as ethylene, propylene, isobutylene, 2-butene, 1-butene, 1-pentene, and 1-hexene are preferred, and one or more of these can be used. Among these, ethylene and propylene are more preferred.

[0035] The acid-modified polyolefin resin preferably contains an unsaturated carboxylic acid component. Examples of the unsaturated carboxylic acid component include acrylic acid, methacrylic acid, maleic acid or maleic anhydride, itaconic acid or itaconic anhydride, fumaric acid, and crotonic acid. Among them, acrylic acid, methacrylic acid, maleic acid, or maleic anhydride are preferred from the viewpoint of adhesion to various tubes, and acrylic acid and maleic anhydride are particularly preferred. In addition, the unsaturated carboxylic acid component may be copolymerized in the acid-modified polyolefin resin, and the form is not limited. Examples of the copolymerization state include random copolymerization, block copolymerization, and graft copolymerization.

[0036] The acid-modified polyolefin resin may contain an ester component such as a (meth)acrylic acid ester or a maleic acid ester. By containing the ester component, the adhesiveness to a polyvinyl chloride tube is improved, and the compatibility with a polyester resin is also improved. As the (meth)acrylic acid ester, an ester of (meth)acrylic acid and an alcohol having 1 to 20 carbon atoms is preferable. Incidentally, "(meth)acrylic acid" means "acrylic acid or methacrylic acid". Specific examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate, and examples of the maleic acid ester include dimethyl maleate, diethyl maleate, and dibutyl maleate. These can be used alone or in combination. Among them, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl acrylate, octyl acrylate, dimethyl maleate, and diethyl maleate are preferred, and methyl acrylate, ethyl acrylate, dimethyl maleate, and diethyl maleate are particularly preferred. The ester component may be copolymerized in the acid-modified polyolefin resin, and the form is not limited. Examples of the copolymerization state include random copolymerization, block copolymerization, and graft copolymerization.

[0037] The blending of the acid-modified polyolefin resin and polyester resin constituting the adhesive layer of the present invention is preferably such that the mass ratio of the acid-modified polyolefin resin / polyester resin is in the range of 20 / 80 to 90 / 10, more preferably in the range of 50 / 50 to 70 / 30. If the mass ratio is less than 20 / 80, the thermal transfer printing suitability for non-vinyl chloride tubes may decrease, or pressure stains may occur on the end surface of the tube during thermal transfer printing of vinyl chloride tubes. On the other hand, if the mass ratio exceeds 90 / 10, the thermal transfer printing suitability for vinyl chloride tubes is likely to decrease.

[0038] The acid-modified polyolefin resin of the present invention is preferably an acid-modified polyolefin resin having an acid value in the range of 12 to 30 mgKOH / g. If the acid value is less than the above range, the compatibility with polyester resin decreases, or sufficient adhesion with a polyvinyl chloride tube is not obtained, making it difficult to form a fine thermal transfer printed image. On the other hand, if the acid value exceeds the above range, it becomes difficult to form a fine thermal transfer printed image in a non-polyvinyl chloride tube, or the solvent resistance is likely to decrease. The acid value described in this specification is a value measured by a method conforming to JIS K0070. The melting point or Tg of the acid-modified polyolefin resin of the present invention is preferably in the range of 50 to 100°C, more preferably in the range of 70 to 90°C. If the melting point or Tg is within the above range, the blocking resistance when the thermal transfer recording medium is stored in a roll form is good, and a fine thermal transfer printed image can be formed in various tubes without decreasing the thermal transfer sensitivity.

[0039] The polyester resin contained in the adhesive layer of the present invention may be one or more of the same polyester resins contained in the colored layer.

[0040] Furthermore, various known additives such as dispersants, leveling agents, and fillers may be appropriately blended into the adhesive layer as necessary within the range in which the effects of the present invention are not impaired.

[0041] The thickness of the adhesive layer (thickness after drying, the same applies below) is preferably in the range of 0.05 to 1.0 μm, more preferably in the range of 0.1 to 0.3 μm. When the thickness of the adhesive layer is within the above range, the adhesiveness to various tubes is good, and a fine thermal transfer printing image can be formed on various tubes without decreasing the thermal transfer sensitivity.

[0042] The adhesive layer can be formed by dispersing or dissolving the above-mentioned material in a suitable solvent such as methyl ethyl ketone, toluene, xylene, water, etc. to prepare a coating liquid for the adhesive layer, and coating the coating liquid on the substrate by known means such as roll coating, reverse roll coating, gravure coating, reverse gravure coating, bar coating, and rod coating to form a coating film, which is then dried.

[0043] (Release layer) In the thermal transfer recording medium of the present invention, a release layer may be provided between the substrate and the colored layer. The release layer is a layer that is transferred onto a transfer recipient together with the colored layer during thermal transfer.

[0044] The release layer may be, for example, a layer containing wax or a thermoplastic resin. As waxes, polyethylene wax, carnauba wax, paraffin wax, microcrystalline wax, montan wax, oxidized wax, synthetic wax, etc. may be used, and these may be mixed in two or more kinds as necessary. As thermoplastic resins, polyester resins, polyamide resins, polyurethane resins, ethylene vinyl acetate copolymers, rosin resins, terpene resins, phenolic resins, styrene butadiene rubber, etc. may be used. In addition, various known additives such as dispersants, leveling agents, and fillers may be appropriately blended as necessary within a range that does not impair the effects of the present invention.

[0045] The thickness of the release layer (thickness after drying, the same applies below) is preferably in the range of 0.1 to 2.0 μm. When the thickness of the release layer is within the above range, the release performance is good, and fine thermal transfer printing images can be formed on various tubes.

[0046] The release layer can be formed by dispersing or dissolving the above-mentioned material in a suitable solvent such as methyl ethyl ketone, toluene, xylene, water, etc. to prepare a coating liquid for the release layer, and coating the coating liquid on the substrate by a known means such as roll coating, reverse roll coating, gravure coating, reverse gravure coating, bar coating, or rod coating to form a coating film, which is then dried.

[0047] (Heat-resistant slip layer) In the thermal transfer recording medium for tube printing of the present invention, it is preferable to provide a heat-resistant slipping layer on the substrate surface opposite to the surface on which the colored layer, adhesive layer, and optionally the release layer are provided. By providing a heat-resistant slipping layer, it is possible to reduce thermal damage to the substrate of the thermal transfer recording medium caused by a thermal head during thermal transfer printing on various tubes. If the substrate is thermally damaged, the thermal head may stick to the substrate during thermal transfer printing, making it impossible to perform thermal transfer printing smoothly, which is known as sticking. By providing a heat-resistant slipping layer, it is possible to prevent such sticking.

[0048] The material of the heat-resistant slipping layer may be any material that has been conventionally used in thermal transfer recording media without any particular limitations. In consideration of heat resistance to thermal heads, low dynamic friction coefficient at high temperatures, and cost, silicone-modified urethane resins, silicone-modified acrylic resins, and cured silicone resins are particularly preferred as the material of the heat-resistant slipping layer.

[0049] The heat-resistant slipping layer may contain various conventionally known additives such as particles, lubricants, and antistatic agents.

[0050] The thickness of the heat-resistant slipping layer (thickness after drying, the same applies below) is preferably in the range of 0.05 to 0.8 μm in order to achieve a good sticking prevention effect and to prevent a decrease in thermal conductivity.

[0051] The heat-resistant slipping layer can be formed by dispersing or dissolving the above-mentioned material in a suitable solvent such as methyl ethyl ketone, toluene, xylene, water, etc. to prepare a coating liquid for the heat-resistant slipping layer, applying the coating liquid to a substrate by a known means such as roll coating, reverse roll coating, gravure coating, reverse gravure coating, bar coating, or rod coating to form a coating film, and then drying the coating film. EXAMPLES

[0052] The thermal transfer recording medium of the present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0053] <Preparation of coating solution for colored layer> A colored layer coating solution 1 for use in a thermal transfer recording medium for tube printing was prepared according to the following formulation. (Colored layer coating liquid 1) Polyester resin A (Tg60℃, Mn8000) 6.0 parts by mass Carbon black 6.0 parts by weight Pigment dispersant 0.6 parts by weight Methyl ethyl ketone 70.0 parts by mass Toluene 17.4 parts by mass

[0054] <Preparation of coating fluid for adhesive layer> An adhesive layer coating liquid for use in a thermal transfer recording medium for tube printing was prepared according to the following formulation. (Adhesive layer coating liquid 1) Acid-modified polyolefin resin A 6.0 parts by mass (Propylene-maleic anhydride copolymer resin, melting point 80℃, acid value 22mgKOH / g) Polyester resin A (Tg 60°C, Mn 8000) 4.0 parts by mass Methyl ethyl ketone 18.0 parts by mass Toluene 72.0 parts by mass (Adhesive layer coating liquid 2) Acid-modified polyolefin resin B 2.0 parts by mass (Propylene-maleic anhydride copolymer resin, melting point 95℃, acid value 17mgKOH / g) Polyester resin A (Tg 60°C, Mn 8000) 8.0 parts by mass Methyl ethyl ketone 18.0 parts by mass Toluene 72.0 parts by mass (Adhesive layer coating liquid 3) Acid-modified polyolefin resin B 9.0 parts by mass (Propylene-maleic anhydride copolymer resin, melting point 95℃, acid value 17mgKOH / g) Polyester resin A (Tg 60°C, Mn 8000) 1.0 part by mass Methyl ethyl ketone 18.0 parts by mass Toluene 72.0 parts by mass (Adhesive layer coating liquid 4) Acid-modified polyolefin resin C aqueous dispersion 20.0 parts by mass (Ethylene-maleic anhydride-acrylic ester copolymer resin, solid content 25%, melting point 85℃, acid value 22mgKOH / g) Polyester resin B aqueous dispersion 16.7 parts by mass (Solid content 30%, Tg 80℃, Mn 8000) Leveling agent 0.1 parts by weight Water 15.8 parts by mass Methanol 47.4 parts by mass (Adhesive layer coating liquid 5) Acid-modified polyolefin resin C aqueous dispersion 28.0 parts by mass (Ethylene-maleic anhydride-acrylic ester copolymer resin, solid content 25%, melting point 85℃, acid value 22mgKOH / g) Polyester resin B aqueous dispersion 10.0 parts by mass (Solid content 30%, Tg 80℃, Mn 8000) Leveling agent 0.1 parts by weight Water 15.5 parts by mass Methanol 46.4 parts by mass (Adhesive layer coating liquid 6) Acid-modified polyolefin resin D 6.0 parts by mass (Propylene-maleic anhydride copolymer resin, melting point 80℃, acid value 12mgKOH / g) Polyester resin A (Tg 60°C, Mn 8000) 4.0 parts by mass Methyl ethyl ketone 18.0 parts by mass Toluene 72.0 parts by mass (Adhesive layer coating liquid 7) Acid-modified polyolefin resin E aqueous dispersion 24.0 parts by mass (Propylene-maleic anhydride-acrylic ester copolymer resin, solid content 25%, melting point 65℃, acid value 30mgKOH / g) Polyester resin B aqueous dispersion 13.3 parts by mass (Solid content 30%, Tg 80℃, Mn 8000) Leveling agent 0.1 parts by weight Water 15.6 parts by mass Methanol 47.0 parts by mass (Adhesive layer coating liquid 8) Polyester resin B aqueous dispersion 33.3 parts by weight (Solid content 30%, Tg 80℃, Mn 8000) Leveling agent 0.1 parts by weight Water 16.7 parts by mass Methanol 49.9 parts by mass (Adhesive layer coating liquid 9) Acid-modified polyolefin resin E aqueous dispersion 40.0 parts by mass (Propylene-maleic anhydride-acrylic ester copolymer resin, solid content 25%, melting point 65℃, acid value 30mgKOH / g) Leveling agent 0.1 parts by weight Water 15.0 parts by mass Methanol 44.9 parts by mass

[0055] <Preparation of coating solution for release layer> A release layer coating solution 1 for use in a thermal transfer recording medium for tube printing was prepared according to the following formulation. (Release layer coating solution 1) Ethylene-vinyl acetate copolymer resin (melting point 73°C) 1.0 part by mass Polyethylene wax (melting point 99°C) 5.0 parts by weight Toluene 94.0 parts by mass

[0056] <Preparation of coating solution for heat-resistant slip layer> A heat-resistant slipping layer coating solution 1 for use in a thermal transfer recording medium for tube printing was prepared according to the following formulation. (Heat-resistant slip layer coating solution 1) Silicone modified acrylic resin (20% solids) 12.5 parts by weight Isocyanate (TDI) 1.5 parts by weight Methyl ethyl ketone 74.0 parts by mass Toluene 12.0 parts by mass

[0057] Example 1 <Preparation of thermal transfer recording medium> [Formation of heat-resistant slip layer] The heat-resistant slipping layer coating solution 1 was applied to one surface of a 6 μm-thick polyethylene terephthalate film by gravure coating so that the coating thickness after drying would be 0.1 μm, and then dried by heating to form a heat-resistant slipping layer. [Formation of colored layer] The colored layer coating solution 1 was applied by gravure coating to the side of the polyethylene terephthalate film opposite the side on which the heat-resistant slipping layer was formed, so that the coating thickness after drying would be 0.6 μm, and then the film was heated and dried to form a colored layer. [Formation of adhesive layer] On the surface on which the colored layer was formed, adhesive layer coating solution 1 was coated by gravure coating so that the coating thickness after drying would be 0.15 μm, and then heated and dried to obtain the thermal transfer recording medium of Example 1.

[0058] Example 2 [Formation of peeling layer] The release layer coating solution 1 was applied by bar coating to the side opposite to the side on which a heat-resistant slipping layer was formed in the same manner as in Example 1 of a 6 μm-thick polyethylene terephthalate film so that the coating thickness after drying would be 0.3 μm, and the film was heated and dried to form a release layer. [Formation of colored layer] As in Example 1, the colored layer coating solution 1 was layered on the surface on which the release layer was formed by gravure coating so that the coating thickness after drying was 0.6 μm, and then heated and dried to form a colored layer. [Formation of adhesive layer] As in Example 1, adhesive layer coating solution 1 was layered on the surface on which the colored layer was formed by gravure coating so that the coating thickness after drying would be 0.15 μm, and then heated and dried to obtain the thermal transfer recording medium of Example 2.

[0059] Example 3 A thermal transfer recording medium of Example 3 was obtained in the same manner as in Example 2, except that adhesive layer coating solution 1 in Example 2 was changed to adhesive layer coating solution 2.

[0060] Example 4 A thermal transfer recording medium of Example 4 was obtained in the same manner as in Example 2, except that the adhesive layer coating solution 1 in Example 2 was changed to the adhesive layer coating solution 3.

[0061] Example 5 A thermal transfer recording medium of Example 5 was obtained in the same manner as in Example 2, except that the adhesive layer coating solution 1 in Example 2 was changed to the adhesive layer coating solution 4.

[0062] Example 6 A thermal transfer recording medium of Example 6 was obtained in the same manner as in Example 2, except that the adhesive layer coating solution 1 in Example 2 was changed to the adhesive layer coating solution 5.

[0063] Example 7 A thermal transfer recording medium of Example 7 was obtained in the same manner as in Example 2, except that the adhesive layer coating solution 1 in Example 2 was changed to the adhesive layer coating solution 6.

[0064] Example 8 A thermal transfer recording medium of Example 8 was obtained in the same manner as in Example 2, except that the adhesive layer coating solution 1 in Example 2 was changed to the adhesive layer coating solution 7.

[0065] Comparative Example 1 A thermal transfer recording medium of Comparative Example 1 was obtained in the same manner as in Example 2, except that adhesive layer coating solution 1 in Example 2 was changed to adhesive layer coating solution 8.

[0066] Comparative Example 2 A thermal transfer recording medium of Comparative Example 2 was obtained in the same manner as in Example 2, except that the adhesive layer coating solution 1 in Example 2 was changed to the adhesive layer coating solution 9.

[0067] <Printing evaluation conditions> Using the thermal transfer recording media of Examples 1 to 8 and Comparative Examples 1 and 2, printing was carried out on each tube under the following conditions to produce printed matter. Printing Conditions Printer: Max Corporation Letatwin LM-550W2 Print resolution: 300dpi Printing speed: 40mm / sec Print density: 8 Transfer target: PVC tube (Max genuine drum-type round tube LM-TU452L: inner diameter 5.2 mm) Non-vinyl chloride tubing (Panduit HSTT25-48-Q10: inner diameter 6.4 mm)

[0068] (Print quality evaluation) The print quality of the print was confirmed using a 5x magnifying lens and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 1. (If it is rated ○ or higher, there is no problem in practical use.) Evaluation criteria ◎: Thin lines 0.085 mm wide (the smallest line width possible with a print resolution of 300 dpi) and small letters 1.3 mm high are printed precisely and without any missing parts. ◯: For thin lines with a width of 0.085 mm and small letters with a character height of 1.3 mm, there are slight defects in the printing, but the printing is still legible. ×: For thin lines with a width of 0.085 mm and small letters with a character height of 1.3 mm, the printing is chipped or crushed, making the characters illegible.

[0069] (Pressure Welding Contamination Evaluation) The printed matter was visually inspected and examined using a 5x magnifying lens for pressure stains, and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 1. (If the result is ◯ or higher, there is no problem in practical use.) Evaluation criteria ◎: No pressure stains. ◯: Slight pressure stains are visible through a magnifying lens, but are not noticeable to the naked eye. ×: Pressure stains easily visible to the naked eye were observed.

[0070] (Evaluation of compatibility between acid-modified polyolefin resin and polyester resin) Regarding the compatibility of the acid-modified polyolefin resin and polyester resin in the adhesive layer, only the adhesive layer was coated on one side of a 6 μm-thick polyethylene terephthalate film and dried, and then the coating surface of the adhesive layer was observed at 500 times using a digital microscope and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 1. Evaluation criteria ⊚: No phase separation structure was observed on the surface of the adhesive layer, and the surface was uniform. ×: A phase separation structure such as a sea-island structure is observed on the surface of the adhesive layer.

[0071] [Table 1] [Explanation of symbols]

[0072] 1: Thermal transfer recording medium 2: Adhesive layer 3: Colored layer 4: Thermal transfer layer 5: Base material 6: Heat-resistant slippery layer

Claims

1. A thermal transfer recording medium for tube printing, comprising a colored layer and an adhesive layer laminated in that order on one side of a substrate, the colored layer containing at least a polyester resin and a colorant, and the adhesive layer containing at least an acid-modified polyolefin resin and a polyester resin that are compatible with each other.

2. 2. A thermal transfer recording medium for tube printing as described in claim 1, characterized in that the acid-modified polyolefin resin in the adhesive layer is a copolymer containing ethylene and / or propylene as an olefin component and maleic anhydride and / or acrylic acid as an unsaturated carboxylic acid component.

3. The thermal transfer recording medium for tube printing according to claim 1, characterized in that the acid-modified polyolefin resin in the adhesive layer is a copolymer containing ethylene and / or propylene as an olefin component, maleic anhydride and / or acrylic acid as an unsaturated carboxylic acid component, and any one or more of methyl acrylate, ethyl acrylate, dimethyl maleate, and diethyl maleate as an ester component.

4. 2. The thermal transfer recording medium for tube printing according to claim 1, wherein a mass ratio of the acid-modified polyolefin resin to the polyester resin in the adhesive layer is in the range of 20 / 80 to 90 / 10.

5. 2. The thermal transfer recording medium for tube printing according to claim 1, wherein the acid value of the acid-modified polyolefin resin in the adhesive layer is in the range of 12 to 30 mgKOH / g.

Citation Information

Patent Citations

  • Thermal transfer sheet

    JP2017121734A

  • Thermal transfer sheet

    JP2017154393A