Film-shaped sealant and circuit device
A film-like sealant with specific viscosity properties allows simultaneous chip mounting and sealing in reflow soldering, addressing inefficiencies in existing methods by ensuring complete coverage and alignment without solder washaway or misalignment, thus enhancing bonding and thermal resistance.
Patent Information
- Application Number
- JP2024063029
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-09
- Publication Date
- 2024-11-07
AI Technical Summary
Existing methods for chip mounting and sealing in reflow soldering processes require separate steps for solder mounting and sealing, which are inefficient and do not allow for simultaneous sealing of the entire chip, especially in narrow areas, and often result in poor bonding or misalignment of components.
A film-like sealant with a melt viscosity of 25 to 70 Pa·s at 220°C is used, allowing simultaneous mounting and sealing of electronic components by adjusting reflow conditions to ensure proper alignment and coverage of the chip periphery without hindering the soldering process.
The film-like sealant enables the entire electronic component to be sealed at once during the reflow solder mounting process, preventing solder washaway and misalignment, while maintaining strong bonding and thermal resistance.
Smart Images

Figure 2024157525000001_ABST
Abstract
Description
[Technical field]
[0001] The present technology relates to a film sealant and a circuit device. [Background technology]
[0002] Conventionally, in surface mounting of chips by reflow soldering using solder paste, etc., the chip (e.g., semiconductor element) is sealed after the solder connection by reflow in order to prevent corrosion of the solder and to improve the soldering strength, vibration resistance, and thermal shock resistance. For example, when flip chip mounting, etc. is performed, the lower part of the chip is sealed, and the entire chip including the lower part may be sealed.
[0003] On the other hand, there is a demand for shorter mounting conditions due to the demand for shorter takt time in mounting and for reasons such as the miniaturization of chips. Regarding sealing, there is also a demand for sealing in a smaller area, particularly for the lower part of the chip components. For example, a method using an underfill film can be cited as a technique for simultaneously performing solder mounting and sealing the lower part of the chip (see, for example, Patent Documents 1 and 2). In addition, there are methods described in Patent Documents 3 and 4 as techniques for sealing the entire chip, including the lower part, after mounting.
[0004] The techniques described in Patent Documents 1 and 2 simultaneously perform solder mounting and sealing of the bottom of the chip, but do not seal the entire chip, so if the entire chip is to be sealed, a separate sealing process is required. Also, the techniques described in Patent Documents 3 and 4 can seal the entire chip, but they do so after solder mounting, so a sealing process is required in addition to the reflow process. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-184605 A [Patent Document 2] JP 2020-065063 A [Patent Document 3] JP 2012-054363 A [Patent Document 4] JP 2015-216229 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present technology has been proposed in light of the above-mentioned conventional situation, and provides a film-like sealant that can simultaneously seal the entire electronic component, such as a chip, on a substrate at the same time as mounting the electronic component on the substrate during the reflow step of a reflow solder mounting process. [Means for solving the problem]
[0007] As a result of extensive investigations, the inventors of the present application focused on the viscosity of the film-shaped sealant at the melting point of the bonding material that bonds the substrate and the electronic component, and discovered that the above-mentioned problems can be solved by using a film-shaped sealant whose melt viscosity at the melting point of the bonding material that bonds the substrate and the electronic component (e.g., the liquidus temperature of the solder) is within a predetermined range.
[0008] The film-like sealant according to the present technology contains a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity at 220°C of 25 to 70 Pa·s.
[0009] The film-like sealant according to the present technology includes a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity of 25 to 70 Pa s at 220°C. A second resin layer is laminated on a first resin layer made of the film-like sealant.
[0010] The present technology relates to a film-like sealant for sealing electronic components mounted on a substrate, the film-like sealant containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and having a melt viscosity of 25 to 70 Pa s at the melting point of a bonding material that bonds the substrate and the electronic components.
[0011] The present technology relates to a film-like sealant for sealing an electronic component mounted on a substrate, the film-like sealant comprising a first resin layer made of a film-like sealant that contains a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity of 25 to 70 Pa s at the melting point of a bonding material that bonds the substrate and the electronic component, and a second resin layer laminated on a surface of the first resin layer opposite to the surface that contacts the electronic component.
[0012] In the circuit device according to the present technology, electronic components mounted on a substrate are sealed with the cured product of the film sealant described above. Effect of the Invention
[0013] According to the present technology, it is possible to provide a film sealant that can simultaneously mount electronic components such as chips on a substrate and seal the entire electronic component at the same time in the reflow step of a solder mounting process using reflow.
[0014] Furthermore, according to the present technology, when a film-type sealant is formed by laminating a first resin layer and a second resin layer, even if a substrate carries a mixture of multiple components of different sizes, such as chips (semiconductor elements) and electronic components (chip resistors, etc.) that are smaller than chips, these components can be collectively sealed at the same time as they are mounted during reflow. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a circuit device in which electronic components mounted on a substrate are encapsulated with a cured product of the film sealant according to the present technology. [Diagram 2] FIG. 2 is a graph showing the relationship between time and temperature for explaining an example of a reflow condition. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of the film sealant according to the second embodiment. [Figure 4] FIG. 4 is a cross-sectional view illustrating a method of placing mounting components on a circuit board in an example of a method for manufacturing a circuit device. [Diagram 5] FIG. 5 is a cross-sectional view illustrating a method of applying a film sealant to the periphery of a mounting component in an example of a method for manufacturing a circuit device. [Figure 6] FIG. 6 is a cross-sectional view illustrating a method of applying a film sealant to the periphery of a mounting component in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed and mounted on a circuit board. [Figure 7] FIG. 7 is a cross-sectional view illustrating a method of performing a reflow process on a circuit board on which mounting components of different sizes are mounted, in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed and mounted on a circuit board. [Figure 8] FIG. 8 is a cross-sectional view for explaining a method of performing a reflow process on a circuit board on which mounting components of different sizes are placed. [Figure 9] FIG. 9 is a cross-sectional view for explaining a method of performing a reflow process on a circuit board on which mounting components of different sizes are placed. [Figure 10] FIG. 10(A) is a cross-sectional view illustrating a method of applying a film sealant having a first resin layer and a second resin layer laminated to the periphery of a plurality of mounting components of different sizes in an example of a manufacturing method for a circuit device in which mounting components of different sizes are mixed on a circuit board. FIG. 10(B) is a cross-sectional view illustrating a method of performing a reflow process on a circuit board on which mounting components of different sizes are placed. FIG. 10(C) is a cross-sectional view showing a state in which the mounting components are all sealed together at the same time as the mounting components are mounted on the circuit board. [Figure 11] FIG. 11 is a plan view showing an example of the configuration of the test mounting component used in the sealing performance evaluation (2). [Figure 12] FIG. 12 is a cross-sectional view showing an example of a state in which a film sealant was placed on a test mounting component used in the sealing property evaluation (2). [Figure 13] Figure 13(A) is a plan view showing an example of a test circuit device after sealing evaluation (2) was performed using a film sealant (1), and Figure 13(B) is a cross-sectional view along A-A' in Figure 13(A). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] <Film-type sealant> A film-like sealant according to the present technology, as a first embodiment, is a film-like sealant for sealing electronic components mounted on a substrate, which contains a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity of 25 to 70 Pa s at the melting point of the bonding material that bonds the substrate and the electronic components. By using such a film-like sealant, the entire electronic components can be encapsulated simultaneously with the mounting of electronic components such as chips on a substrate in the reflow step of a solder mounting process by reflow.
[0017] As described later, in a second embodiment of the film sealant according to the present technology, a second resin layer may be laminated on a first resin layer made of a film sealant containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator and having a melt viscosity of 25 to 70 Pa s at 220° C. For example, the second resin layer may be laminated on the surface of the first resin layer opposite to the surface in contact with the electronic component.
[0018] [First embodiment] FIG. 1 is a cross-sectional view showing an example of a circuit device in which an electronic component mounted on a substrate is sealed with a cured product of the film-like sealant according to the present technology. In the circuit device 10, a circuit board 1 as a substrate and a mounting component 2 as an electronic component are joined by a solder joint 3A derived from a solder paste 3. The solder joint 3A is provided between an electrode pad 1a of the circuit board 1 and an electrode bump 2a of the mounting component 2. In the circuit device 10, the periphery of the mounting component 2 is sealed with a sealing part 4A formed by curing the film-like sealant 4 according to the present technology. The periphery of the mounting component 2 includes the periphery of the solder joint 3A (including the side of the solder joint 3A, and the space S surrounded by the space between the solder joints 3A and the mounting component 2 and the circuit board 1), the periphery (side) of the electrode bump 2a, and the periphery of the mounting component 2 (upper surface 2b, side surface 2c, lower surface 2d). In this manner, in the circuit device 10, the periphery of the mounting component 2 is covered with the sealing portion 4A so that there is substantially no gap between the circuit board 1 and the mounting component 2.
[0019] Generally, there are reflow conditions recommended for each bonding material. For example, there are a method of adjusting the reflow conditions according to the melting point of the bonding material, and a method of not changing the reflow conditions regardless of the melting point of the bonding material. First, when adjusting the reflow conditions according to the melting point of the bonding material, if the melting point of the bonding material is too low, the reflow conditions become lower, so that melting of the film-like sealant 4 is difficult to proceed, and there is a risk that sealing cannot be performed sufficiently. On the other hand, if the melting point of the bonding material is too high, the reflow conditions become higher, and the film-like sealant 4 with a lower viscosity may push the bonding material (for example, the solder particles of the solder paste 3) away, which may hinder bonding or cause the solder particles to scatter. Next, when the reflow conditions are not changed regardless of the melting point of the bonding material, if the melting point of the bonding material is too low, more heat than necessary may be applied, which may reduce the thermal fatigue resistance of the bonding material and reduce the long-term durability of the bonded portion. On the other hand, if the melting point of the bonding material is too high, bonding tends to be difficult.
[0020] In the present technology, the temperature at which the film-like sealant 4 exhibits a melt viscosity of 25 to 70 Pa·s preferably coincides with the melting point of the bonding material (for example, the solder in the solder paste 3) that bonds the circuit board 1 and the mounting component 2. When using the film-like sealant 4 according to the present technology, it is preferable to use a bonding material having a melting point (liquid phase temperature) of about 220°C as the bonding material that bonds the circuit board 1 and the mounting component 2. As a specific example, it is preferable to use a solder paste 3 using a solder having a liquid phase temperature of 220°C (for example, SAC-305 (Ag3.0%-Cu0.5%-Sn (balance))). On the premise of using such a bonding material, it is preferable to use a film-like sealant 4 according to the present technology that contains a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator and has a melt viscosity of 25 to 70 Pa·s at 220°C.
[0021] Hereinafter, assuming the use of a solder paste 3 using solder with a liquidus temperature of 220°C, a film-like sealant that contains a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator and has a melt viscosity of 25 to 70 Pa s at 220°C will be described as an example of the film-like sealant 4 according to the present technology.
[0022] FIG. 2 is a graph showing the relationship between time and temperature to explain an example of reflow conditions. The area within the frame indicated by P in FIG. 2 represents a preheat area (hereinafter referred to as the preheat area P). Solder paste 3 usually contains a solvent and flux as volatile components. The preheat area P refers to a process in which the solvent in the solder paste 3 is volatilized and the flux cleans the oxide film on the solder surface and the member to be joined. The area within the frame indicated by R in FIG. 2 represents a reflow area (hereinafter referred to as the reflow area R). The reflow area R refers to a process in which the flux removes the oxide film on the solder particle surface, and the solder paste 3 melts, and the electrode pads 1a of the circuit board 1 and the electrode pads 2a of the mounting component 2 are self-aligned and joined. A in FIG. 2 represents a preheat start point (for example, 150 to 180° C.). B in FIG. 2 represents a preheat end point (for example, 170 to 200° C.). In the region a in FIG. 2, the temperature is preferably increased at a rate of 2 to 4° C. / sec. The period between A and B in FIG. 2 is preferably 90±30 seconds. In the region b in FIG. 2, the temperature is preferably increased at a rate of 2 to 3° C. / sec. C in FIG. 2 represents a peak temperature (e.g., 230 to 250° C.). D in FIG. 2 represents a holding time of 220° C. or more, and this holding time is preferably 30 to 60 seconds. The horizontal dashed line between 220° C. and 250° C. in FIG. 2 represents the heat resistance temperature of general substrates and electronic components.
[0023] In the preheat region P in FIG. 2, the solvent in the solder paste 3 starts to volatilize. On the other hand, since the melt viscosity of the film sealant 4 at 220°C is 25 to 70 Pa·s, in the preheat region P, the film sealant 4 remains in a film form or becomes liquid but maintains its film form. In particular, in the low temperature region near A in the preheat region P, the film sealant 4 does not melt and remains in a film form, so most of the volatilized solvent escapes through the gaps in the film sealant 4, but it may also escape through the film sealant 4. In this way, in the preheat region P, the solvent in the solder paste 3 volatilizes, and the volatilized solvent is discharged from the inside to the outside of the film sealant 4 through the gap between the circuit board 1 and the film sealant 4, or through the film sealant 4.
[0024] 2, the solder in the solder paste 3 starts to melt, and the circuit board 1 and the mounting component 2 are self-aligned. In the reflow region R, the flux in the solder paste 3 starts to volatilize, and the volatilized flux is discharged from the inside of the liquid film-like sealant 4 to the outside. Then, in the reflow region R, the film-like sealant 4 starts to melt, and the periphery of the mounting component 2 is covered with a sealing portion 4A as shown in FIG.
[0025] In this way, since the film-shaped sealant 4 has a melt viscosity of 25 to 70 Pa s at 220°C, the melting of the solder paste 3 and the alignment of the circuit board 1 and the mounting components 2 occur first, followed by the melting of the film-shaped sealant 4, so that the alignment of the circuit board 1 and the mounting components 2 is less likely to be hindered by the film-shaped sealant 4. Therefore, by using the film-shaped sealant 4 according to the present technology, the entire mounting components 2 can be encapsulated simultaneously with the mounting of the mounting components 2 in the reflow step of the solder mounting process by reflow.
[0026] Since the film-shaped sealant 4 has a melt viscosity of 70 Pa·s or less at 220°C, the viscosity of the film-shaped sealant 4 can be sufficiently reduced, and the film-shaped sealant 4 can be prevented from clinging to the circuit board 1 or the mounting component 2 and making it difficult to enter the lower part of the mounting component 2 (space S shown in Figure 1).As a result, the periphery of the mounting component 2 can be sealed at the same time as the mounting component 2 is mounted.
[0027] Furthermore, since the film sealant 4 has a melt viscosity of 25 Pa·s or more at 220°C, it is possible, for example, to prevent the particulate solder that constitutes the solder paste 3 from being washed away before the solder paste 3 melts, and to prevent a shortage of solder particles necessary for connecting the circuit board 1 and the mounting components 2. As a result, it is possible to seal the periphery of the mounting components 2 at the same time as mounting the mounting components 2.
[0028] The film-like sealant 4 has a melt viscosity at 220°C of 25 to 70 Pa·s, and may be 26 Pa·s or more, 31 Pa·s or more, 41 Pa·s or more, 43 Pa·s or more, 44 Pa·s or more, 56 Pa·s or more, 64 Pa·s or more, or may be 26 to 64 Pa·s. The melt viscosity of the film-like sealant at 220°C can be adjusted by, for example, the contents of the film-forming component and the thermosetting monomer.
[0029] <Film-forming components> The film-forming component is appropriately selected so that the film-like sealing agent 4 melts and becomes liquid at about 220°C and has a melt viscosity of 25 to 70 Pa·s at 220°C. The film-forming component may have a melt viscosity of 30 Pa·s or more, 40 Pa·s or more, or 45 Pa·s or more at 220°C. The film-forming component may have a melt viscosity of 300 Pa·s or less, 200 Pa·s or less, 100 Pa·s or less, 80 Pa·s or less, or 70 Pa·s or less at 220°C. The film-forming component may have a melt viscosity of 25 to 70 Pa·s, or 30 to 50 Pa·s at 220°C.
[0030] As the film-forming component, various resins such as a thermoplastic elastomer having a styrene-ethylene-propylene-styrene structure, a thermoplastic elastomer having a styrene-ethylene-ethylene-propylene-styrene structure, a thermoplastic elastomer having a styrene-ethylene-butylene-styrene structure, an acrylic polymer, a phenoxy resin, an epoxy resin, and a urethane resin can be used. Specific examples include Clarity LA2250, LA4285 (methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, manufactured by Kuraray), Nanostrength M51 (methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, manufactured by Arkema), Nanostrength D51N (modified methyl methacrylate-polybutyl acrylate block copolymer, manufactured by Arkema), Septon 2000 series (elastomer having a styrene-ethylene-propylene-styrene structure), and Septon 4000 series (elastomer having a styrene-ethylene-ethylene-propylene-styrene structure, manufactured by Kuraray).
[0031] The content of the film-forming component in the film-shaped sealant 4 can be appropriately selected within a range in which the melt viscosity of the film-shaped sealant 4 is 25 to 70 Pa·s at 220°C, and can be, for example, 40% by weight or more, 50% by weight or more, 60% by weight or more, 70% by weight or more, or 75% by weight or more. The content of the film-forming component in the film-shaped sealant 4 can be 90% by weight or less, 85% by weight or less, or can be 80% by weight or less. The content of the film-forming component in the film-shaped sealant 4 can be, for example, in the range of 65 to 85% by weight, or can be in the range of 70 to 80% by weight.
[0032] The film-forming component may be used alone or in combination of two or more. When two or more film-forming components are used in combination, it is preferable that the total amount thereof satisfies the above range. When two or more film-forming components are used in combination, it is preferable that the film-forming component having a melt viscosity of 30 to 50 Pa·s at 220°C is included. For example, the content of the film-forming component having a melt viscosity of 30 to 50 Pa·s at 220°C relative to the total amount of the film-forming components in the film-like sealant is preferably 50% by weight or more, may be 60% by weight or more, may be 70% by weight or more, may be 80% by weight or more, may be 90% by weight or more, may be 95% by weight or more, may be 99% by weight or more, or may be 100% by weight.
[0033] <Thermosetting monomer> The thermosetting monomer is appropriately selected so that the film sealant 4 melts and becomes liquid at about 220°C, and has a melt viscosity of 25 to 70 Pa·s at 220°C. As the thermosetting monomer, various thermosetting monomers such as acrylic resin and epoxy resin can be used. As the thermosetting monomer, a (meth)acrylate-based monomer is preferable from the viewpoint that the viscosity reduction effect is large when a small amount is added, and the crosslinking density can be increased by increasing the number of functional groups, thereby improving the heat resistance. In addition, as described above, when the solder paste 3 using the solder having a liquidus temperature of 220°C is used as the joining material, if the curing temperature is too low, the viscosity of the resin when the solder paste 3 melts becomes higher, making it more difficult for the mounting component 2 to move, and the alignment between the circuit board 1 and the mounting component 2 tends to be difficult, so it is preferable to use an acrylic resin, which has a higher curing temperature than the epoxy resin.
[0034] As the (meth)acrylate monomer, it is preferable to use at least one of a bifunctional (meth)acrylate monomer and a polyfunctional (meth)acrylate monomer, because crosslinking easily proceeds even in a small amount. Specific examples of the (meth)acrylate monomer include 1,6-hexanediol diacrylate and trimethylolpropane triacrylate.
[0035] The content of the (meth)acrylate monomer in the film-shaped sealant 4 can be appropriately selected within a range in which the melt viscosity of the film-shaped sealant 4 is 25 to 70 Pa·s at 220°C, and can be, for example, 1 wt% or more, 2 wt% or more, 3 wt% or more, 4 wt% or more, or 5 wt% or more. The content of the (meth)acrylate monomer in the film-shaped sealant can be, for example, 10 wt% or less, 8 wt% or less, 7 wt% or less, or 6 wt% or less. The content of the (meth)acrylate monomer in the film-shaped sealant can be, for example, in the range of 1 to 10 wt%, or in the range of 3 to 6 wt%.
[0036] The (meth)acrylate monomer may be used alone or in combination of two or more. When two or more (meth)acrylate monomers are used in combination, it is preferable that the total amount thereof falls within the above range.
[0037] <Curing agent or polymerization initiator> The film-like sealant 4 includes a curing agent for a thermosetting monomer, or a polymerization initiator for initiating a reaction between thermosetting monomers. The curing agent or polymerization initiator can be appropriately selected according to the type of thermosetting monomer. For example, when an acrylic resin is used as the thermosetting monomer, it is preferable to use a thermal radical polymerization initiator as the polymerization initiator. Also, when an epoxy resin is used as the thermosetting monomer, it is preferable to use, for example, a phenolic resin or an acid anhydride as the curing agent. For example, an imidazole compound or a tertiary amine compound that mainly acts as a curing catalyst can also be used as the curing agent for the epoxy resin.
[0038] The thermal radical polymerization initiator generates radicals by heating and initiates polymerization of the (meth)acrylate monomer. For example, in a solder mounting process by reflow, it is preferable that the curing of the thermosetting monomer does not start as much as possible while the temperature is raised from room temperature to about 200 to 220°C at a rate of 2 to 3°C / min, and it is also preferable that the curing reaction of the thermosetting monomer starts at 250 to 260°C thereafter. In the reflow step of the solder mounting process by reflow, for example, if the thermosetting monomer starts curing in the preheat region P shown in FIG. 2, the viscosity of the molten film-like sealant 4 becomes higher, and the mounting component 2 becomes difficult to move, making self-alignment impossible, and there is a risk that the solder connection between the circuit board 1 and the mounting component 2 is hindered.
[0039] Therefore, it is preferable that the thermal radical polymerization initiator has a reaction initiation temperature as high as possible, for example, a 10-hour half-life temperature of 140°C to 170°C. Examples of the thermal radical polymerization initiator include peroxides having a 10-hour half-life temperature of 140°C to 170°C. Specific examples include aromatic hydroperoxides and aliphatic hydroperoxides having a 10-hour half-life temperature of 140°C to 170°C. Examples of products of the thermal radical polymerization initiator include Perbutyl H (10-hour half-life temperature: 166.5°C), Percumyl H (10-hour half-life temperature: 157.9°C), Perocta H (10-hour half-life temperature: 152.9°C), and Percumyl P (10-hour half-life temperature: 145.1°C, all manufactured by NOF Corporation).
[0040] The curing agent or polymerization initiator may be used alone or in combination of two or more. For example, when the film sealant 4 contains an acrylic resin as a thermosetting monomer, it is preferable to contain a thermal radical polymerization initiator as a polymerization initiator, and a thermal radical polymerization initiator and a photopolymerization initiator may be used in combination, or a thermal radical polymerization initiator may be used alone.
[0041] The content of the curing agent or polymerization initiator in the film-shaped sealant 4 can be, for example, 0.01% by weight or more based on the total amount of the film-forming components and the thermosetting monomer in the film-shaped sealant 4. The content of the curing agent or polymerization initiator in the film-shaped sealant 4 can be, for example, 2% by weight or less based on the total amount of the film-forming components and the thermosetting monomer in the film-shaped sealant 4. For example, when the film-shaped sealant 4 contains an acrylic resin as a thermosetting monomer, the content of the polymerization initiator based on the total amount of the film-forming components and the thermosetting monomer can be in the range of 0.1 to 1% by weight. When two or more types of curing agents or polymerization initiators are used in combination, it is preferable that the total amount satisfies the above range.
[0042] <Surfactant> The film-shaped sealant 4 may further contain other components than the above-mentioned components within a range that does not impair the effect of the present technology. For example, the film-shaped sealant 4 may further contain a surfactant in order to more efficiently break bubbles generated by outgassing due to the solvent in the solder paste 3 during reflow, to adjust the permeability of the film-shaped sealant 4 around the mounting component 2, particularly to the lower part of the mounting component 2 (space S shown in FIG. 1), and to further increase the adhesive strength. The surfactant can be appropriately selected in consideration of heat resistance, reactivity with the thermosetting monomer, defoaming property, and the like. As the surfactant, for example, BYK354 and BYK322 (both manufactured by BYK Japan) can be used.
[0043] When the film-shaped sealant 4 contains a surfactant, the content of the surfactant in the film-shaped sealant 4 can be, for example, 1 wt % or more, and may be 10 wt % or more. The content of the surfactant in the film-shaped sealant 4 can be, for example, 30 wt % or less, and may be 20 wt % or less. The surfactant may be used alone or in combination of two or more types. When two or more types of surfactants are used in combination, it is preferable that the total amount thereof satisfies the above range.
[0044] <Other resins> The film-shaped sealant 4 may further contain a resin (hereinafter also referred to as other resin) different from the film-forming component and the thermosetting monomer, depending on the purpose of adjusting the viscosity of the film-forming component, adjusting the elastic modulus of the film-shaped sealant 4, and further increasing the adhesive strength of the film-shaped sealant 4. The other resin may be any material that melts and becomes liquid at about 220°C and has a melt viscosity of 25 to 70 Pa·s at 220°C, and is not particularly limited in structure. For example, from the viewpoint of increasing the elastic modulus of the film-shaped sealant 4 at room temperature, a styrene-based or terpene phenol-based resin may be used. An example of a product of the other resin is YS Polystar T160 (terpene phenol resin, softening point: 160°C, manufactured by Yasuhara Chemical Co., Ltd.).
[0045] When the film-shaped sealant 4 contains other resins, the content of the other resins in the film-shaped sealant 4 can be, for example, 1% by weight or more, and may be 20% by weight or more. The content of the other resins in the film-shaped sealant 4 can be, for example, 50% by weight or less, and may be 40% by weight or less. The other resins may be used alone or in combination of two or more types. When two or more types of other resins are used in combination, it is preferable that the total amount thereof satisfies the above range.
[0046] Moreover, the film sealant 4 may further contain a filler, a lubricant, an antioxidant, and the like within a range that does not impair the effects of the present technology.
[0047] The thickness of the film-shaped sealant 4 is not particularly limited and can be appropriately selected depending on the purpose, and can be, for example, in the range of 50 to 200 μm. Also, the thickness of the film-shaped sealant 4 can be, for example, in the range of 50 to 300 μm, or can be in the range of 200 to 300 μm.
[0048] In the above description, an example of the film-like sealant 4 in which a solder paste 3 using a solder with a liquidus temperature of 220° C. is used has been described, but the present invention is not limited to this example, and various modifications can be made depending on the liquidus temperature of the solder paste 3. For example, when a solder paste 3 using a solder with a liquidus temperature lower than 220° C. is used, an epoxy resin may be used as the thermosetting monomer, or a thermal radical polymerization initiator with a low reaction initiation temperature (for example, a 10-hour half-life temperature lower than 140° C. to 170° C.) may be used.
[0049] [Second embodiment] 3 is a cross-sectional view showing an example of a film-like sealant according to the second embodiment. In the film-like sealant 20 according to the second embodiment, a second resin layer 22 is laminated on a first resin layer 21 made of the film-like sealant according to the first embodiment described above, and as described later in detail, it is preferable that the product of the rigidity of the first resin layer 21 and a predetermined coefficient is smaller than the rigidity of the second resin layer 22. By using such a film-like sealant 20, as described later in detail, for a circuit board on which relatively large components such as chips (e.g., semiconductor elements) and relatively small components such as chip resistors are mixed, the components to be mounted that need to be sealed can be sealed together without the small components such as chip resistors being displaced due to the shape change of the film-like sealant during reflow.
[0050] The first resin layer 21 has the same preferred ranges as those of the above-mentioned film-like sealant 4, except for the shear modulus G' at 150° C. and the film thickness, which will be described later.
[0051] The resin constituting the second resin layer 22 can be selected from any resin, and examples of the resin include epoxy resin, acrylic resin, polyimide resin, etc. When an epoxy resin or an acrylic resin is used as the resin constituting the second resin layer 22, a cured product obtained by curing a resin composition containing a monomer of each resin by irradiating it with ultraviolet light or by thermally curing the resin composition can be used.
[0052] Examples of the epoxy resin include epoxy resins having a naphthalene skeleton, bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins (e.g., dicyclopentadiene type epoxy resins, 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate), siloxane type epoxy resins, biphenyl type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, and the like. These may be used alone or in combination of two or more.
[0053] As the acrylic resin, for example, a monofunctional (meth)acrylate monomer, a polyfunctional (meth)acrylate monomer, or a (meth)acrylate resin may be used alone or in combination of two or more of them. The monofunctional (meth)acrylate monomer refers to a (meth)acrylate monomer having one (meth)acryloyl group. The polyfunctional (meth)acrylate monomer refers to a (meth)acrylate monomer having two or more (meth)acryloyl groups. The (meth)acrylate resin may be a polymer or an oligomer. Specific examples of the monofunctional (meth)acrylate monomer include isobornyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. Specific examples of the polyfunctional (meth)acrylate monomer include tricyclodecane dimethanol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. Specific examples of the (meth)acrylate resin include (meth)acrylates having a polyurethane skeleton and (meth)acrylates having a polyisoprene skeleton.
[0054] The second resin layer 22 may further contain other components as necessary in addition to the epoxy resin, acrylic resin, and polyimide resin, such as plasticizers and rubbers that are not directly involved in the reaction.
[0055] The first resin layer 21 and the second resin layer 22 constituting the film sealant 20 preferably satisfy the following formula 1. Equation 1: (shear modulus G' (Pa) of the first resin layer 21 at 150°C) x (film thickness (µm) of the first resin layer 21) x 9 < (tensile modulus E' (Pa) of the second resin layer 22 at 150°C) x (film thickness (µm) of the second resin layer 22)
[0056] The film-shaped sealant 20 satisfies formula 1; in other words, the product of the rigidity of the first resin layer 21 and a predetermined coefficient is smaller than the rigidity of the second resin 22. Therefore, in mounting and sealing using the film-shaped sealant 20, even in a circuit board on which relatively large components such as chips and relatively small components such as chip resistors are mixed, the tiny components such as chip resistors do not shift in position due to changes in shape of the film-shaped sealant during reflow, and the mounting components that require sealing can be sealed all at once.
[0057] In formula 1, the reason for focusing on the shear modulus G' of the first resin layer 21 and the tensile modulus E' of the second resin layer 22 at a specific temperature (150°C) is as follows. The reason why minute components (components for mounting having a relatively small size) mixed on a circuit board are displaced due to the flow of the film-shaped sealant during reflow is considered to be caused by, for example, a change in the modulus of elasticity of the film-shaped sealant up to the vicinity of the preheating start point A (for example, 150 to 180°C) in the preheating region P in FIG. 2. Therefore, the focus was on 150°C, which corresponds to the preheating start point. In addition, the tensile modulus E' is difficult to measure when the measurement target has low elasticity (approximately 1.0E+04 Pa or less), whereas the shear modulus G' can be measured at low elasticity but is difficult to measure at high elasticity. Therefore, the shear modulus G' of the first resin layer 21 and the tensile modulus E' of the second resin layer 22, which can be measured at 150° C., were compared.
[0058] The shear modulus G' of the first resin layer 21 at 150°C is not particularly limited as long as it satisfies formula 1, depending on the thickness of the first resin layer 21 or the second resin layer 22, and can be, for example, 3.8E+03 Pa or more and 2.9+04 Pa or less. The shear modulus G' of the first resin layer 21 at 150°C can be measured by the method described in the Examples below. The film thickness of the first resin layer 21 is not particularly limited as long as it satisfies formula 1, and can be, for example, in the range of 200 to 300 µm.
[0059] The tensile modulus E' of the second resin layer 22 at 150°C is not particularly limited as long as it satisfies the formula 1, depending on the thickness of the first resin layer 21 or the second resin layer 22, and may be, for example, 6.0E+05 Pa or more and 4.0E+09 Pa or less, from the viewpoint of more effectively suppressing the fluidity of the first resin layer 21 during reflow. The tensile modulus E' of the second resin layer 22 can be measured by the method described in the examples below. The film thickness of the second resin layer 22 is not particularly limited as long as it satisfies the formula 1, and may be, for example, in the range of 50 to 100 μm.
[0060] <Method of manufacturing film sealant> [First embodiment] Next, a method for producing the film-like sealant 4 according to the present technology will be described. The method for producing the film-like sealant 4 is not particularly limited, and for example, the film-like sealant 4 can be obtained by weighing out predetermined components (for example, the above-mentioned film-forming components, thermosetting monomer, curing agent or polymerization initiator, organic solvent), dissolving or dispersing them by stirring, mixing, kneading, or the like to prepare a resin varnish, applying the resin varnish onto a base film that has been subjected to a release treatment, and removing the organic solvent by heating.
[0061] The organic solvent is preferably one that has the property of being able to uniformly dissolve or disperse each component. For example, dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, dimethylsulfoxide, diethylene glycol dimethyl ether, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate, butyl cellosolve, dioxane, cyclohexanone, ethyl acetate, etc. The organic solvent may be used alone or in combination of two or more kinds.
[0062] The stirring, mixing or kneading in preparing the resin varnish can be carried out using, for example, a stirrer, a grinding machine, a three-roll mill, a ball mill, a bead mill or a homodisper. The application of the resin varnish onto the substrate film can be carried out using, for example, a knife coater, a roll coater, an applicator or the like.
[0063] The substrate film to which the resin varnish is applied is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent. For example, the substrate film may be a polyolefin film such as a polypropylene film or a polymethylpentene film, a polyester film such as a polyethylene terephthalate film or a polyethylene naphthalate film, a polyimide film, or a polyetherimide film. The substrate film may be a single-layer film or a multilayer film. When the substrate film is a multilayer film, each layer may be made of different materials or the same material.
[0064] The drying conditions for volatilizing the organic solvent from the resin varnish applied to the substrate film are preferably conditions under which the organic solvent is sufficiently volatilized, and can be, for example, conditions of 50 to 200° C. and 0.1 to 90 minutes.
[0065] [Second embodiment] Next, a description will be given of a manufacturing method of the film-shaped sealant 20. The manufacturing method of the film-shaped sealant 20 includes, for example, a step of preparing a first resin layer 21, a step of preparing a second resin layer 22, and a step of bonding the first resin layer 21 and the second resin layer 22 together to obtain the film-shaped sealant 20.
[0066] In the step of preparing the first resin layer 21, for example, the film sealant 4 (first resin layer 21) is obtained by the same method as in the above-mentioned first embodiment.
[0067] In the step of preparing the second resin layer 22, a resin composition for the second resin layer 22 is prepared, and the prepared resin composition is applied onto a base film that has been subjected to a release treatment, and cured with light (ultraviolet rays) to obtain the second resin layer 22. Alternatively, a commercially available resin film may be used as it is as the second resin layer 22. When a commercially available resin film is used as the second resin layer 22, the step of preparing the second resin layer 22 can be omitted.
[0068] The resin composition for the second resin layer 22 includes, for example, the above-mentioned epoxy resin or acrylic resin precursor, a photopolymerization initiator, and a plasticizer. Specific examples of the resin composition for the second resin layer 22 mainly composed of an acrylic resin include a resin composition including a (meth)acrylate resin having a polyurethane skeleton, isobornyl (meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, and a photopolymerization initiator, and a resin composition including a (meth)acrylate resin having a polyisoprene skeleton, isobornyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and a photopolymerization initiator. Specific examples of the resin composition for the second resin layer 22 mainly composed of an epoxy resin include a resin composition including a bisphenol A type epoxy resin and a photoacid generator, and a resin composition including a bisphenol A type epoxy resin, an alicyclic epoxy resin, and a photoacid generator.
[0069] The resin composition can be applied onto the base film, for example, by using a bar coater. The base film may be any of those listed in the first embodiment.
[0070] In the step of laminating the first resin layer 21 and the second resin layer 22 to obtain the film-like sealant 20, for example, a laminator can be used to laminate the first resin layer 21 and the second resin layer 22. Note that the step of preparing the first resin layer 21 and the step of preparing the second resin layer 22 may be performed in either order, or may be performed in parallel.
[0071] <Circuit device> 1, a circuit device 10 according to the present technology includes a circuit board 1 as a substrate and a mounting component 2 as an electronic component, which are joined at a solder joint 3A derived from a solder paste. The mounting component 2 is surrounded by a sealing portion 4A formed by hardening a film sealant 4.
[0072] Examples of the circuit board 1 include known boards such as a semiconductor board, a flexible circuit board, a rigid wiring board, and a printed wiring board. Known electrode pads such as copper pads and aluminum pads can be used as the electrode pads 1a of the circuit board 1. The electrode pads 1a can also be replaced with electrodes of other shapes, such as electrode bumps.
[0073] The mounting component 2 may be any of various known surface mounting components, such as a semiconductor chip, a light-emitting diode, a capacitor chip, a resistor element, etc. The electrode bump 2a of the mounting component 2 may be any known electrode bump, such as a gold bump or a solder bump. The electrode bump 2a may be replaced by an electrode of another form, such as an electrode pad.
[0074] The solder joints 3A are formed by reflow processing of the solder paste 3, and provide electrical continuity between the electrode bumps 2a of the mounting component 2 and the electrode pads 1a of the circuit board 1.
[0075] The sealing portion 4A is formed by curing the film-like sealant 4. As described above, the sealing portion 4A covers the periphery of the mounting component 2, the periphery of the electrode bumps 2a, and the periphery of the solder joint portions 3A, and also covers a part of the surface of the circuit board 1.
[0076] In addition, in the circuit device according to the present technology, electronic components mounted on the substrate may be sealed with the cured product of the film sealant 20 .
[0077] <Manufacturing method of circuit device> [First embodiment] Next, an example of a manufacturing method for the circuit device 10 according to the present technology will be described. First, the solder paste 3 is applied to the electrode pads 1a of the circuit board 1. The solder paste can be applied to the electrode pads 1a by a known method, and can be applied using, for example, a precision dispenser or a screen printer.
[0078] FIG. 4 is a cross-sectional view for explaining a method of placing a mounting component 2 on a circuit board 1 in an example of a manufacturing method of a circuit device 10. After applying a solder paste 3 to the electrode pads 1a of the circuit board 1, the mounting component 2 is placed on the circuit board 1 as shown in FIG. 4. Specifically, the electrode bumps 2a of the mounting component 2 are aligned with the electrode pads 1a of the circuit board 1, and may be lightly pressed as necessary. This brings the electrode bumps 2a of the mounting component 2 into contact with the solder paste 3. The height of the gap between the electrode pads 1a and the electrode bumps 2a is not particularly limited, and may be, for example, about 10 to 100 μm, or about 80 μm.
[0079] FIG. 5 is a cross-sectional view for explaining a method of applying the film-shaped sealant 4 to the periphery of the mounting component 2 in an example of a manufacturing method of the circuit device 10. For example, after mounting the mounting component 2 on the circuit board 1, as shown in FIG. 5, a method of placing the film-shaped sealant 4 on the mounting component 2 so as to cover the mounting component 2 can be mentioned. Since the film-shaped sealant 4 placed on the mounting component 2 does not follow the shape of the mounting component 2, etc., as shown in FIG. 5, for example, there are spaces between the film-shaped sealant 4 and the upper surface 2b of the mounting component 2, between the film-shaped sealant 4 and the side surface 2c, and between the film-shaped sealant 4 and the surface of the circuit board 1. Therefore, as described above, in the preheat region P, the volatilized solvent is likely to escape from the inside to the outside of the film-shaped sealant 4.
[0080] Next, a reflow process is performed on the solder paste 3 sandwiched between the electrode pad 1a of the circuit board 1 and the electrode bump 2a of the mounting component 2. In the reflow process, the solder paste 3 is heated to a temperature higher than the melting temperature of the solder particles, the oxide film on the surface of the solder particles is removed by the flux, and the solder paste 3 is wetted and spread between the electrode pad 1a and the electrode bump 2a to form a solder joint 3A, and the film sealant 4 is hardened by heating during the reflow process to form a sealing portion 4A. During the reflow process of the solder paste 3, the solder paste 3 does not spread beyond the periphery of the electrode pad 1a but tends to remain on the surface of the electrode pad 1a, so that the mounting component 2 can be self-aligned with the circuit board 1. The reflow process can be performed at normal pressure. In other words, as described above, the reflow process includes the steps of volatilizing the solvent in the solder paste 3 and discharging the volatilized solvent from the inside of the liquefied film-like sealant 4 to the outside, melting the solder in the solder paste 3 to self-align the circuit board 1 and the mounting component 2, volatilizing the flux in the solder paste 3 and discharging the volatilized flux from the inside of the liquefied film-like sealant 4 to the outside, and melting the film-like sealant 4 to seal the periphery of the mounting component 2 with the sealing portion 4A.
[0081] With this manufacturing method, in the reflow step of the solder mounting process by reflow, the mounting components 2 can be mounted on the circuit board 1 and the entire mounting components 2 can be sealed at the same time. As a result, as shown in Fig. 1, a circuit device 10 in which the mounting components 2 are sealed with a sealing portion 4A is obtained. In this manner, in the manufacturing method for the circuit device 10 according to the present technology, the reflow treatment of the solder paste 3 and the hardening treatment of the film sealant 4 can be performed simultaneously.
[0082] Furthermore, in the manufacturing method for the circuit device 10 according to the present technology, in the reflow step of the solder mounting process by reflow, the mounting components 2 can be entirely sealed at the same time as mounting the mounting components 2 without the need for pressure with a tool. Furthermore, in the manufacturing method for the circuit device 10 according to the present technology, in the solder mounting process by reflow, scattering of solder balls can be suppressed and the solvent (volatile components) of the solder paste 3 can be discharged.
[0083] [Second embodiment] FIG. 6 is a cross-sectional view illustrating a method of applying a film sealant to the periphery of a mounting component in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed and mounted on a circuit board.
[0084] As shown in FIG. 6, when components of different sizes that require sealing, specifically, a relatively large mounting component 30 (hereinafter simply referred to as mounting component 30) and a relatively small mounting component 31 (hereinafter simply referred to as mounting component 31) are mixed and mounted on a circuit board 32, if the mounting components that require sealing are all sealed with a film-like sealant (for example, film-like sealant 4), there is a risk that a minute component (mounting component 31) with a size of, for example, 1 mm square or less may be displaced due to the flow of the film-like sealant 4 during reflow processing. In FIG. 6, a component 35 that is not to be sealed, in other words, a component that is not preferably sealed with a film-like sealant, is a component that may affect the original function or performance if sealed. Examples of the component 35 that is not to be sealed include a type of protective element that cuts off an element by heat generation, an electrode provided on a substrate, and a light-emitting element.
[0085] 7 is a cross-sectional view for explaining a method of performing a reflow process on a circuit board on which mounting components of different sizes are placed, in an example of a manufacturing method of a circuit device in which mounting components of different sizes are mixed and mounted on the circuit board. As shown in FIG. 7, when a reflow process is performed on a solder paste 34a sandwiched between an electrode pad 32a of a circuit board 33 and an electrode bump 30a of a mounting component 30, and a solder paste 34b sandwiched between an electrode pad 32b and an electrode bump 31a of a mounting component 31 using a film-shaped sealant 4, the elastic modulus of the film-shaped sealant 4 changes due to a temperature rise during the reflow process, causing the film-shaped sealant 4 to bend, and the mounting component 31 is moved by the bent film-shaped sealant 4, which may cause a component misalignment (misalignment of the mounting component 31) in the direction of the arrow shown in FIG. 7. It is difficult to adjust such a component misalignment by self-alignment even if the solder paste 34b melts.
[0086] Such misalignment of tiny components tends to be particularly noticeable when tiny components are mounted on the ends of a circuit board, or even if not on the ends of the circuit board, when the mounting portion of the tiny components abuts the ends of the film-type sealant, or when there are no areas on the ends of the film-type sealant where components are not mounted and the components are mounted at a very narrow pitch.
[0087] 8 and 9 are cross-sectional views for explaining a method of performing a reflow process on a circuit board on which mounting components of different sizes are placed. As shown in Fig. 8, when there is no part at the end of the film-shaped sealant 4 where components are not mounted and components (mounting components 30, 31) are mounted at a narrow pitch, the elastic modulus of the film-shaped sealant 4 changes due to the temperature rise during the reflow process, causing the film-shaped sealant 4 to bend, and the mounting component 31 is moved by the bent film-shaped sealant 4, which may cause a component misalignment (misalignment of the mounting component 31) in the direction of the arrow shown in Fig. 8.
[0088] On the other hand, as shown in FIG. 9, if there are portions at the ends of the film-shaped sealant 4 where components (mounting components 30, 31) are not mounted, the elastic modulus of the film-shaped sealant 4 changes due to the rise in temperature during the reflow process, causing the film-shaped sealant 4 to bend. However, before the film-shaped sealant 4 comes into contact with the mounting components 30, 31, it comes into contact with the circuit board 33, and when it comes into contact with the circuit board 32, the film-shaped sealant 4 does not move any further, so no component misalignment occurs.
[0089] From the above viewpoints, when components (mounting components 30, 31) of different sizes that require sealing are mixed and mounted on circuit board 32, film sealant 20 is preferably used.
[0090] FIG. 10(A) is a cross-sectional view illustrating a method for applying a film sealant having a first resin layer and a second resin layer laminated to the periphery of a plurality of mounting components of different sizes in an example of a manufacturing method for a circuit device in which mounting components of different sizes are mixed and mounted on a circuit board.
[0091] First, solder pastes 34a and 34b are applied to electrode pads 32a and 32b of a circuit board 32, and then mounting components 30 and 31 are placed on the circuit board 32. Specifically, electrode bumps 30a (not shown) of the mounting components 30 are aligned with electrode pads 32a of the circuit board 32, and electrode bumps 31a (not shown) of the mounting components 31 are aligned with electrode pads 32a of the circuit board 32, and may be lightly pressed as necessary. Next, for example, after mounting components 30 and 31 are placed on the circuit board 32, as shown in FIG. 10(A), a film-like sealant 20 is placed on the mounting components 30 and 31 so as to cover the mounting components 30 and 31. The film-like sealant 20 is placed on the mounting components 30 and 31 so that the first resin layer 21 faces the mounting components 30 and 31.
[0092] Fig. 10(B) is a cross-sectional view for explaining a method of performing a reflow process on a circuit board on which mounting components of different sizes are placed in an example of a manufacturing method for a circuit device in which mounting components of different sizes are mixedly mounted on the circuit board, and Fig. 10(C) is a cross-sectional view showing a state in which all of the mounting components are collectively sealed at the same time as mounting a plurality of mounting components on the circuit board in an example of a manufacturing method for a circuit device in which mounting components of different sizes are mixedly mounted on the circuit board.
[0093] A reflow process is performed on the solder pastes 34a, 34b sandwiched between the electrode pads 32a of the circuit board 32 and the electrode bumps 30a, 31a of the mounting components 30, 31. The reflow process heats the solder pastes 34a, 34b to a temperature higher than the melting temperature of the solder particles, removes the oxide film on the surfaces of the solder particles with flux, and causes the solder pastes 34a, 34b to wet and spread between the electrode pads 32a, 32b and the electrode bumps 30a, 31a to form the solder joints 34a, 34b, and hardens the film sealant 20 by heating during the reflow process to form a sealing portion.
[0094] During the reflow process of the solder pastes 34a and 34b, as shown in Fig. 10(B), the movement of the first resin layer 21 in the film-like sealant 20 is suppressed by the second resin layer 22, and the curvature of the first resin layer 21 in the film-like sealant 20 is suppressed by the temperature rise during the reflow process, so that the occurrence of misalignment of the mounting components 30 and 31 (particularly the mounting components 31) due to the curvature of the first resin layer 21 is suppressed. In addition, the first resin layer 21 flows after it has a sufficiently low viscosity, and the entire mounting components 30 and 31 are sealed by the flowing first resin layer 21. The reflow process can be performed in the same manner as in the first embodiment of the manufacturing method for a circuit device. During the reflow process, the solvent in the solder pastes 34a, 34b evaporates in the preheat region P shown in FIG. 2, and the volatilized solvent is discharged through the gap between the circuit board 32 and the film-shaped sealant 20, or through the film-shaped sealant 20 from the inside to the outside of the film-shaped sealant 20.
[0095] With this manufacturing method, in the reflow step of the solder mounting process by reflow, the mounting components 30, 31 can be mounted on the circuit board 32 and the entire mounting components 30, 31 can be sealed at the same time. As a result, as shown in FIG. 10(C), a circuit device 33 in which the mounting components 30, 31 are sealed at the sealing portion can be obtained. In this manner, in the manufacturing method of the circuit device, the reflow process of the solder paste 34 and the hardening process of the film sealant 20 can be performed simultaneously. Furthermore, in the manufacturing method of the circuit device, even in the case of a circuit board 32 on which a plurality of mounting components of different sizes, such as the mounting components 30 and the mounting components 31, are mixed, the components on the entire surface of the circuit board 32 can be sealed without causing the minute components (mounting components 31) to shift positions. EXAMPLES
[0096] Examples of the present technology will be described below. Note that the present technology is not limited to these examples. The components of the film-like sealant used in the examples and comparative examples are as follows.
[0097] [First resin layer] <Film-forming components> Kuraray LA2250: Methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, viscosity at 220°C: 47 Pa·s, manufactured by Kuraray Nanostrength M51: Methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, viscosity at 220°C: 46 Pa·s, Arkema Nanostrength D51N: Modified methyl methacrylate-polybutyl acrylate block copolymer, viscosity at 220°C: 33 Pa·s, manufactured by Arkema KuraRity LA4285: Methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, viscosity at 220°C: 590 Pa·s, manufactured by Kuraray Co., Ltd. Septon 2002: Elastomer with a styrene-ethylene-propylene-styrene structure, viscosity at 220°C: 350 Pa·s, manufactured by Kuraray Co., Ltd.
[0098] <Thermosetting monomer> NK Ester A-TMPT: Trimethylolpropane triacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd. HDDA: 1,6-hexanediol diacrylate, manufactured by Daicel-Allnex Corporation
[0099] <Thermal radical polymerization initiator> Perocta H: 1,1,3,3-tetramethylbutyl hydroperoxide, NOF Corporation
[0100] <Other resins> YS Polyster T160: Terpene phenol resin, softening point: 160°C, manufactured by Yasuhara Chemical Co., Ltd.
[0101] <Surfactant> BYK354: Polyacrylate surfactant, manufactured by BYK Japan BYK322: Silicone surfactant, manufactured by BYK Japan
[0102] [Second resin layer] CN9014NS: Bifunctional urethane acrylate, manufactured by Arkema Acryester IBX: Isobornyl methacrylate, manufactured by Mitsubishi Chemical Corporation NK Ester DCP: Tricyclodecane dimethanol dimethacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd. UC-203M: Isoprene methacrylate, manufactured by Kuraray LBR-307: Polybutadiene, manufactured by Kuraray Alcon M-100: alicyclic saturated hydrocarbon resin, manufactured by Arakawa Chemical Industries, Ltd. PI-184: Aal Chem EXA-850CRP: Bisphenol A type epoxy resin, manufactured by DIC CELLOXIDE 2021P: 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, manufactured by Daicel Corporation EPICLON HP7200L: Dicyclopentadiene type epoxy resin, manufactured by DIC CPI-200K: San-Apro Kapton 200H: Toray DuPont (polyimide resin film)
[0103] <Preparation of Composition for Film-like Sealant> The components shown in Table 1 were uniformly mixed in the blending ratios (parts by weight) shown in Table 1 to prepare compositions for film-like sealants (first resin layer).
[0104] <Preparation of composition for second resin layer> A composition for a film-like sealant (second resin layer) was prepared by uniformly mixing the components shown in Table 2 in the blending ratios (parts by weight) shown in Table 2. In Example 15, a commercially available film was used as is.
[0105] <Preparation of film sealant (1)> A resin varnish was prepared by mixing a composition for a film-like sealant (first resin layer) with an organic solvent (a mixed solvent of 80% toluene and 20% methyl ethyl ketone), and the resin varnish was applied to a base film (polyethylene terephthalate film) that had been subjected to a release treatment using a bar coater. The organic solvent was removed by heating at 100°C for 5 minutes to obtain a primary film-like sealant having a thickness of 50 μm, and then the resin varnish was applied and dried again from the primary film-like sealant to obtain a film-like sealant having a thickness of 100 μm. Hereinafter, this film-like sealant is referred to as film-like sealant (1). Film-like sealant (1) was used in the sealing property evaluation (1) described below.
[0106] <Preparation of film sealant (2)> The first resin layer was obtained in the same manner as in the preparation of the film-like sealant (1) described above. In addition, in Examples 8 to 18, except for Example 15, a resin composition for the second resin layer containing each component shown in Table 2 was applied onto a peel-treated film using a bar coater and cured with ultraviolet light. In Example 15, a commercially available polyimide resin film was used as is. The obtained first resin layer and second resin layer were bonded together with a laminator to obtain a film-like sealant in which the second resin layer was laminated on the first resin layer. The thickness of each layer is as shown in Table 1. Hereinafter, this film-like sealant is referred to as film-like sealant (2). The film-like sealant (2) was used in the sealability evaluation (2) described later. In Examples 1 to 7 and Comparative Examples 1 to 4, the film-like sealant (1) was also used in the sealability evaluation (2).
[0107] <Melt viscosity of film-forming components and film-type sealant> The melt viscosity at 220° C. of the film-forming component and the film-like sealant was measured using a rheometer (AR-G2 (manufactured by TA Instruments)). The results are shown in Table 1.
[0108] <Shear modulus G' of first resin layer> The shear modulus G' of the first resin layer at 150° C. was measured using a rheometer (AR-G2 (manufactured by TA instruments) at a frequency of 1 Hz and a heating rate of 10° C. / min. The results are shown in Table 1.
[0109] <Tensile modulus E' of second resin layer> The tensile modulus E' of the second resin layer at 150° C. was measured using a viscoelasticity measuring device (DMA7100, Hitachi High-Tech Science Corporation) at a frequency of 1 Hz and a heating rate of 10° C. / min. The results are shown in Table 1.
[0110] <Sealability evaluation (1)> <Fabrication of circuit device> A test circuit device was fabricated using the following FR-4 grade circuit board as the test circuit board and the following semiconductor element as the test mounting component. Specifically, solder paste ("M705-GRN360-K2-V" (solder particles: Ag3.0%-Cu0.5%-Sn (balance)) manufactured by Senju Metal Industry Co., Ltd. was applied to the electrode pads of the test circuit board with a precision dispenser to a thickness of 150 μm, and the electrode bumps of the test mounting component were aligned with the electrode pads of the test circuit board to which the solder paste had been applied, and the test mounting component was mounted on the test circuit board by lightly pressing it. Next, the above-mentioned film sealant (1) was applied to the pads on which the test mounting components were placed. The test circuit board was placed on a test circuit board, heated from room temperature to 170°C at 3°C / sec in air, and held at 170°C for 90 seconds. After that, the temperature was raised to 250°C at 2°C / sec, and then cooled to room temperature at 2°C / sec, in a reflow process under normal pressure. This soldered the test mounting component to the test circuit board, and sealed the top, sides, and bottom of the test mounting component. As a result, a circuit device 10 sealed with a cured product 4A of the film sealant 4 was obtained, as shown in Figure 1. A UNI-5016A (manufactured by Antom Co., Ltd.) was used as the reflow furnace.
[0111] The test circuit board used was an FR-4 grade circuit board (20 x 40 x 0.6 mm) with gold-plated copper wiring (1.0 x 7.2 mm) on the surface. The test mounting component used was a semiconductor element (5 x 9.5 x 1 mm) with electrode bumps (1.0 x 7.2 mm). The film sealant was cut to 22 mm x 42 mm.
[0112] An evaluation was made as to whether the periphery (outer periphery and bottom) of the semiconductor element, which was a mounting component for testing, was sealed with the film sealant. The appearance of the top and side parts of the semiconductor element was observed with a microscope and visually evaluated. For the bottom part of the semiconductor element, the encapsulated semiconductor element was polished from the top until the internal solder paste part was revealed, and then observed with a microscope. Those in which the periphery of the semiconductor element was sealed were evaluated as ○ (OK), and those in which there was an unsealed part around the semiconductor element were evaluated as × (NG). The results are shown in Table 1.
[0113] [Table 1]
[0114] [Table 2]
[0115] <Sealability evaluation (2)> FIG. 11 is a plan view showing an example of the configuration of the test mounting component and the test circuit board used in the sealability evaluation (2). FIG. 12 is a cross-sectional view showing an example of the state in which the film sealant is placed on the test mounting component used in the sealability evaluation (2). As the test circuit board 41, an FR-4 grade circuit board (5 mm×20 mm×0.6 mm) having gold-plated copper wiring 41a, 41b on the surface was used. The mounting portion of the component on the test circuit board 41 has a copper wiring (semiconductor element 43 mounting portion) of 2 mm×1 mm and a copper wiring (chip component 42 mounting portion) of 0.1 mm×0.2 mm. As the test mounting component, in addition to the semiconductor element 43 (4 mm×4 mm×1 mm) having an electrode bump (2 mm×1 mm), a chip resistor 42 of 0402 (0.4 mm×0.2 mm×0.2 mm) size was arranged at the end of the board 41 as shown in FIG. 11. The distance from the end of the test circuit board 41 to the chip resistor 42 on the end side of the test circuit board 41 was 1 mm, the distance between the chip resistors 42 was 0.5 mm, and the distance from the chip resistor 42 on the semiconductor element 43 side to the end of the semiconductor element 43 was 6.1 mm. The method of mounting the test mounting components on the test circuit board 41 was the same as in the sealing evaluation (1). The solder paste and its application method were also the same as in the sealing evaluation (1).
[0116] As shown in Fig. 12, the film sealant was placed on a test circuit board 41 on which a test mounting component was placed. After that, the test mounting component and the test circuit board 41 were soldered together under the same reflow conditions as in the sealing evaluation (1), and the top, sides, and bottom of the test mounting component were sealed. The film sealant was cut to a size of 7 mm x 22 mm and used.
[0117] Then, whether the periphery of the test mounting component, i.e., the periphery (outer periphery and bottom) of the chip resistor 42 and the semiconductor element 43, was sealed by the film-like sealant was evaluated in the same manner as in the sealability evaluation (1). Specifically, the case where the periphery of the test mounting component was sealed was evaluated as ○ (OK), the case where the film-like sealant spread onto the test circuit board 41 and around the test mounting component but the test mounting component (especially the chip resistor 42) was misaligned was evaluated as △ (NG), and the case where the film-like sealant did not spread and there were unsealed parts on the test circuit board 41 or around the test mounting component was evaluated as × (NG). The results are shown in Table 1.
[0118] FIG. 13(A) is a plan view showing an example of a test circuit device after performing a sealing evaluation (2) using a film-like sealant (1), and FIG. 13(B) is a cross-sectional view of A-A' in FIG. 13(A). For example, when performing a sealing evaluation (2) using a film-like sealant (film-like sealant (1)) that does not have a second resin layer, as shown in FIG. 8, the elastic modulus of the film-like sealant 4 changes due to the temperature rise during the reflow process, and the film-like sealant 4 is curved, and the curved film-like sealant 4 causes a shift in the chip resistor 42. Thereafter, as shown in FIGS. 13(A) and (B), the film-like sealant 4 spreads over the test circuit board 41 and around the test mounting component, but the chip resistor 42 is shifted. Thus, a sealability evaluation (2) of Δ (NG) refers to, for example, a state in which chip resistor 42 is misaligned, chip resistor 42 is not connected to test circuit board 41, and the hardened film-like sealant (sealing portion 4B) covers the periphery of the test mounting component. In this case, test circuit board 41 and semiconductor element 43 are joined by solder joint 44A derived from solder paste 44a, but chip resistor 42 is misaligned from position 42P (the position of chip resistor 42 when connected correctly), and test circuit board 41 and chip resistor 42 are not sufficiently joined by solder joint 44B derived from solder paste 44b, so that chip resistor 42 does not function on test circuit board 41.
[0119] [Sealability evaluation (1) results] From the results of Examples 1 to 18, it was found that the sealing property evaluation was good when using a film-like sealant (1) containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator and having a melt viscosity of 25 to 70 Pa s at 220° C. That is, it was found that in Examples 1 to 18, in the reflow step of the solder mounting process by reflow, the entire electronic components such as chips (semiconductor elements) can be encapsulated at the same time as mounting the electronic components on the substrate.
[0120] Moreover, from the results of Comparative Examples 1 to 4, it was found that even in the case of a film-like sealant (1) containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, if the melt viscosity at 220°C does not satisfy 25 to 70 Pa s, the sealability evaluation is not good. That is, it was found that in Comparative Examples 1 to 4, it is difficult to simultaneously seal the entire electronic components, such as chips, on the board at the same time as mounting the electronic components on the board in the reflow step of the solder mounting process by reflow.
[0121] For example, in Comparative Example 3, a film-shaped sealant (1) with a melt viscosity of 102 Pa s at 220°C was used. Although the film-shaped sealant (1) melted during the reflow treatment, the viscosity did not decrease sufficiently, and the film-shaped sealant (1) clung to the components (the test circuit board and the test mounting components) and was difficult to penetrate into the lower parts of the test mounting components.
[0122] [Sealability evaluation (2) results] From the results of Examples 8, 10, 12 to 15, 17, and 18, it was found that by using the film sealant (2) satisfying the above-mentioned formula 1, even if multiple components of different sizes are placed on a circuit board, they can be sealed all at once at the same time as reflow, and in addition, tiny components are not displaced due to changes in shape of the film sealant (2) during reflow.
[0123] In Example 9, the thickness of the first resin layer in Example 8 was increased, so that formula 1 was not satisfied, and the chip resistor 42 was misaligned, but the semiconductor element 43 could be mounted.
[0124] In Example 11, the tensile elastic modulus E' of the second resin layer was reduced, so that the formula 1 was not satisfied, and the chip resistor 42 was displaced, but the semiconductor element 43 could be mounted.
[0125] In Example 16, the formula 1 was not satisfied due to the large shear modulus G' of the first resin layer, and the chip resistor 42 was displaced, but the semiconductor element 43 could be mounted.
[0126] In Examples 1 to 7, the sealability evaluation (2) was performed using a film-like sealant (1) that contained a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator and had a melt viscosity of 25 to 70 Pa·s at 220°C, so that the chip resistor 42 was misaligned, but it was possible to mount the semiconductor element 43. In Comparative Examples 1 to 4, the sealability evaluation (2) was performed using a film-like sealant (1) that did not satisfy the melt viscosity of 25 to 70 Pa·s at 220°C, so that the film-like sealant did not spread, and there were unsealed areas on the test circuit board 41 and around the test mounting components. [Explanation of symbols]
[0127] 1 Circuit Board, 1a electrode pad, 2 Mounting parts, 2a electrode pump, 2b top surface, 2c side, 2d bottom surface, 3 solder paste, 3A solder joints, 4 Film-type sealant, 4A sealing part, 4B Sealing part, 10 circuit equipment; 20 Film-type sealant, 20A sealing part, 21 first resin layer, 22 second resin layer, 30 Relatively large mounting components, 30a electrode pump, 31 Relatively small mounting components, 31a Electrode pump, 32 circuit boards, 32a electrode pad, 32b electrode pad, 33 circuit devices; 34a solder paste, 34b solder paste, 34A solder joints, 34B Solder joint 35 Unsealed parts, 41 Test circuit board, 41a copper wiring, 41b copper wiring, 42 Chip resistor, 42P: The position of the chip resistor when connected correctly. 43 Semiconductor elements, 44a solder paste, 44b solder paste 44A solder joints, 44B solder joint
Claims
1. A film-forming component; A thermosetting monomer; A curing agent or a polymerization initiator, A film-like sealant having a melt viscosity at 220°C of 25 to 70 Pa·s.
2. The film sealant according to claim 1 , wherein the thermosetting monomer is a (meth)acrylate monomer.
3. The polymerization initiator includes a thermal radical polymerization initiator, 3. The film-like sealing material according to claim 1, wherein the thermal radical polymerization initiator has a 10-hour half-life temperature of 140° C. to 170° C.
4. The film-like sealing agent according to claim 1 or 2, comprising a film-forming component having a melt viscosity at 220° C. of 30 to 50 Pa·s.
5. The film-like sealant according to claim 1 or 2, wherein the film-forming component contains at least one selected from the group consisting of a methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, a modified methyl methacrylate-polybutyl acrylate block copolymer, an elastomer having a styrene-ethylene-propylene-styrene structure, and an elastomer having a styrene-ethylene-ethylene-propylene-styrene structure.
6. The film-like sealant according to claim 1 or 2, wherein the thermosetting monomer is a difunctional (meth)acrylate monomer or a polyfunctional (meth)acrylate monomer.
7. The film sealant according to claim 1 or 2, further comprising a surfactant.
8. The film sealant according to claim 1 , further comprising a resin other than the film-forming component and the thermosetting monomer.
9. A film sealant comprising a first resin layer made of the film sealant according to claim 1 or 2 and a second resin layer laminated on the first resin layer.
10. The film sealant according to claim 9 , wherein the first resin layer and the second resin layer satisfy the following formula 1: Equation 1: (shear modulus G' (Pa) of the first resin layer at 150°C) x (film thickness (µm) of the first resin layer) x 9 < (tensile modulus E' (Pa) of the second resin layer at 150°C) x (film thickness (µm) of the second resin layer)
11. A film-like sealant for sealing electronic components mounted on a substrate, comprising: A film-forming component; A thermosetting monomer; A curing agent or a polymerization initiator, A film-like sealant having a melt viscosity at a melting point of 25 to 70 Pa·s for bonding the substrate and the electronic component.
12. A film-like sealant comprising: a first resin layer made of the film-like sealant according to claim 11; and a second resin layer laminated on a surface of the first resin layer opposite to a surface in contact with the electronic component.
13. The film sealant according to claim 12 , wherein the first resin layer and the second resin layer satisfy the following formula 1: Equation 1: (shear modulus G' (Pa) of the first resin layer at 150°C) x (film thickness (µm) of the first resin layer) x 9 < (tensile modulus E' (Pa) of the second resin layer at 150°C) x (film thickness (µm) of the second resin layer)
14. The film sealant according to claim 11 , wherein the bonding material is a solder paste.
15. A circuit device, comprising an electronic component mounted on a substrate and sealed with the cured film sealant according to claim 1 .
16. A circuit device, comprising an electronic component mounted on a substrate and sealed with the cured film sealant according to claim 9.
17. A circuit device, comprising an electronic component mounted on a substrate and sealed with the cured film sealant according to claim 12.
18. 16. The circuit device according to claim 15, wherein the substrate and the electronic component having an electrode bump are joined by a solder joint, and the periphery of the solder joint, the periphery of the electrode bump, the top surface of the electronic component, the side surface of the electronic component, and the bottom surface of the electronic component are covered with a hardened product of the film-shaped sealant.
Citation Information
Patent Citations
Sealing method of electronic component
JP2012054363A
Method for manufacturing semiconductor device, and thermosetting resin sheet
JP2015216229A
Prior-supply type underfill material, electronic component device and method for producing electronic component device
JP2018184605A
Pre-supply type underfill material, cured product of pre-supply type underfill material, electronic component device, and manufacturing method of electronic component device
JP2020065063A