Carbon dioxide fixation method
By forming and peeling off carbon dioxide films on minerals containing calcium and/or magnesium, the method addresses slow reaction rates and high costs in existing technologies, achieving efficient and cost-effective carbon dioxide immobilization with stable carbonate films.
Patent Information
- Application Number
- JP2023072041
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
Existing carbon dioxide fixation technologies using mineral carbonation are limited by slow reaction rates and the need for expensive chelating agents, and silicate minerals do not react effectively due to surface film formation, leading to incomplete carbon dioxide immobilization.
A method involving the formation of a carbon dioxide film on minerals containing calcium and/or magnesium in the presence of water, followed by peeling off the film using an external force, with alternating or simultaneous immobilization and peeling steps, without the use of expensive chemicals.
This method allows for efficient carbon dioxide immobilization on minerals, regenerating the fixation ability, and reduces the risk of re-emission by forming stable carbonate films at room temperature and pressure, enhancing productivity and reducing costs.
Smart Images

Figure 2024157607000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for fixation of carbon dioxide, and more particularly to a method for fixation of carbon dioxide in the atmosphere or exhaust gases, thereby enabling sequestration underground or in the sea. [Background technology]
[0002] In recent years, global warming has become a major issue, and there is a worldwide demand to reduce emissions of carbon dioxide, a greenhouse gas. Reducing carbon dioxide emissions requires technology to reduce the amount of emissions themselves, as well as technology to capture and capture carbon dioxide and sequester it underground or in the sea. Regarding the latter fixation technology, a method called mineral carbonation, in which carbon dioxide is fixed in minerals, is attracting attention.
[0003] Mineral carbonation is a method of artificially reacting metal elements such as calcium and magnesium in minerals with carbon dioxide to produce carbon dioxide. Carbonates such as calcium carbonate (CaCO3) and magnesium carbonate (MgCO3) are stable at room temperature and pressure, and the possibility of emitting carbon dioxide after immobilization is lower than with geological storage. In addition, there are fewer geological constraints compared to geological storage, and it can be applied to low concentrations of carbon dioxide, so mineral carbonation can be said to be one of the most effective methods for furnaces and boilers with carbon dioxide concentrations of 10 to 20% and generating tens of thousands to hundreds of thousands of tons of carbon dioxide.
[0004] Known techniques for mineral carbonation use silicate minerals (CaSiO3, Mg3Si2O5(OH)4) in natural rocks, quicklime (CaO) in steelmaking slag, and quicklime (CaO) in fly ash.
[0005] Patent Document 1 describes a method for producing carbonated slag from steelmaking slag by immersing steelmaking slag in water in a reaction tank and blowing a carbon dioxide-containing gas into the water. Patent Document 2 describes a method for treating fly ash that also fixes carbon dioxide, comprising: [1] a step of washing fly ash in a liquid having a pulp concentration of 5 to 100 g / L while blowing in CO2 gas to dissolve the Ca content as Ca(HCO3)2 (washing step); and [2] a step of recovering Ca(HCO3)2 in the post-washing liquid by performing solid-liquid separation of the slurry obtained in the washing step, and recovering the solid content as a washing residue. Patent Document 3 describes a method for fixing carbon dioxide and a method for recovering carbon dioxide, in which an alkaline aqueous solution containing a raw material containing a metal element capable of combining with carbonate ions to form a carbonate mineral and a chelating agent is formed in an aqueous solution formation step, the metal element is reacted with the chelating agent in the aqueous solution to separate the metal element from the raw material as metal ions in a separation step, and a compound capable of generating carbonate ions is added to the aqueous solution, and the carbonate ions generated from the compound are reacted with the metal ions to form a carbonate mineral in a mineral formation step.
[0006] Incidentally, it is known that calcium in steelmaking slag and fly ash, which contain a few percent of free lime, reacts with carbon dioxide and easily becomes carbonated. On the other hand, silicate minerals in natural ores have a slower reaction rate than free lime (CaO) in slag, so it is not practical to directly apply the conventional techniques described in Patent Documents 1 and 2 to mineral carbonation. Furthermore, Patent Document 3 improves the reaction rate by using a chelating agent, but such chelating agents are generally expensive and are not practical from an economic standpoint.
[0007] Furthermore, in each of the above conventional techniques, silicate minerals tend to react with carbon dioxide on the particle surface to form a carbonate film or a metal oxide film (e.g., FeOOH), which can cause the reaction to stop with the calcium and magnesium inside the particle remaining unreacted, resulting in a slowdown in the reaction rate. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2013-147370 A [Patent Document 2] JP 2005-246225 A [Patent Document 3] Patent Publication No. 2022-102786 Summary of the Invention [Problem to be solved by the invention]
[0009] In view of the above circumstances, an object of the present invention is to provide a method for immobilizing carbon dioxide in a mineral containing calcium and / or magnesium without using expensive chemicals. [Means for solving the problem]
[0010] The carbon dioxide fixation method of the first invention is characterized by comprising a fixation step of reacting a treated solid containing calcium and / or magnesium with carbon dioxide in the presence of water to produce a coating and fixing it to the treated solid, and a peeling step of applying an external force to the treated solid with the fixed coating to peel off the coating and regenerate the carbon dioxide fixation capacity. The carbon dioxide fixation method of the second invention is characterized in that in the first invention, the fixation step and the peeling step are alternately repeated. The carbon dioxide fixation method of the third invention is characterized in that, in the first invention, the fixation step and the peeling step are carried out simultaneously. The method for fixation of carbon dioxide of a fourth invention is characterized in that, in the first invention, the solid to be treated comprises one or more of minerals containing calcium silicate and / or magnesium silicate obtained by mining, and slag, clinker, dust, and incineration ash generated in the process of smelting the minerals. The carbon dioxide fixation method of the fifth invention is characterized in that, in the first invention, the solid to be treated is pulverized to 64 μm or less and supplied to the fixation step. The carbon dioxide fixation method of the sixth invention is characterized in that in the first invention, the weight ratio of the water to the solid to be treated in the fixation step is 0.01-10. The carbon dioxide fixation method of the seventh invention is characterized in that in the fixation step, the solid to be treated is reacted with the carbon dioxide while adjusting the partial pressure of carbon dioxide to 0.1 atm to 5 atm. The method for fixation of carbon dioxide of the eighth invention is characterized in that in the first invention, when the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, sodium bicarbonate and / or potassium bicarbonate are further added in the fixation step. The method for fixing carbon dioxide of the ninth invention is characterized in that in the first invention, when the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, one or more of sulfide, sulfur, sulfate, and sulfite are further added in the fixation step. The method for fixation of carbon dioxide according to a tenth aspect of the present invention is characterized in that in the fixation step, the reaction with carbon dioxide is carried out while maintaining a reaction temperature of 5°C to 90°C in the first aspect of the present invention. The carbon dioxide fixation method of an eleventh invention is characterized in that, in the first invention, the iron content in the solid to be treated in the fixation step is 25% by weight or less. The method for fixation of carbon dioxide of the 12th invention is characterized in that in the fixation step, the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, and the fixation step further comprises a preheating step of heating the treated solid to 600°C or higher. Effect of the Invention
[0011] According to the first invention, in the immobilization step, when carbon dioxide is reacted with a treated solid containing calcium and / or magnesium coexisting with water, a coating can be formed on the surface of the treated solid, and when the coating is peeled off in the peeling step, the treated solid and the coating can be separated. Therefore, carbon dioxide can be immobilized in the coating without using expensive chemicals, and its industrial value is extremely great. According to the second aspect of the present invention, the immobilization step and the peeling step are separately performed and are repeated alternately, so that the coating is sufficiently formed before the coating is peeled off, thereby improving the productivity of the immobilization method as a whole. According to the third aspect of the present invention, the fixing step and the peeling step are carried out simultaneously, so that the fixing process can be carried out even in a short operation time. According to the fourth invention, calcium and / or magnesium contained in the treated solid, which is a mineral obtained by mining, dissolves in water and reacts with carbon dioxide to produce a coating made of carbonates, etc., so that carbon dioxide can be fixed in the coating. Furthermore, when the coating is made of carbonate, it is stable under normal temperature and pressure, so the risk of emitting carbon dioxide is reduced. According to the fifth aspect of the present invention, the solid to be treated is pulverized to a size of 64 μm or less, so that the specific surface area of the solid to be treated is increased, and a larger amount of carbon dioxide can be fixed. According to the sixth aspect of the present invention, the amount of water coexisting with the solid to be treated is in the range of 0.01 to 10 by weight relative to the solid to be treated, so that the dissolution reaction can be carried out sufficiently. According to the seventh invention, the partial pressure of carbon dioxide is set in the range of 0.1 atm to 5 atm, so that the reaction can be made sufficiently fast and the carbon dioxide introduction equipment can be simple. According to the eighth aspect of the present invention, sodium hydrogen carbonate and / or potassium hydrogen carbonate is added, so that the carbonation of silicate can be promoted. According to the ninth aspect of the present invention, one or more of sulfide, sulfur, sulfate, and sulfite are added, so that the elution of calcium and / or magnesium into water can be promoted by sulfate ions and / or sulfite ions. According to the tenth aspect of the present invention, the reaction temperature is set in the range of 5° C. to 90° C., so that the reaction proceeds smoothly and the amount of heat required is not excessive. According to the eleventh aspect of the present invention, the iron content in the treated solid is 25% by weight or less, so that the carbonation of calcium and / or magnesium is not easily inhibited and the fixation of carbon dioxide proceeds efficiently. According to the twelfth aspect of the present invention, by preheating the treated solid to 600°C or higher, the crystal structure of the mineral can be partially rendered amorphous, and a larger amount of calcium and / or magnesium in the treated solid can be dissolved into water. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a process diagram of a carbon dioxide fixation method according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of an implementation facility used in the process shown in FIG. 1. [Diagram 3] FIG. 4 is a process diagram of a carbon dioxide fixation method according to a second embodiment of the present invention. [Figure 4] FIG. 4 is an explanatory diagram of an implementation facility used in the process shown in FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (Basic principle of the present invention) As shown in FIG. 1, the carbon dioxide fixation method according to the present invention comprises a fixation step I in which a coating 2 formed by reacting a treated solid 1 containing calcium and / or magnesium with carbon dioxide in the presence of water is fixed to the surface of the treated solid 1, and a peeling step II in which an external force is applied to the treated solid 1 with the fixed coating 2 to peel off the coating 2 and regenerate the carbon dioxide fixation capacity. The immobilization method of the present invention includes a method in which the immobilization step I and the peeling step II are alternately repeated, and a method in which the immobilization step I and the peeling step II are simultaneously performed.
[0014] According to the method for fixing carbon dioxide of the present invention, in fixation step I, a coating 2 containing carbon dioxide can be formed on the surface of a treated solid 1 containing calcium and / or magnesium coexisting with water, and in peeling step II, the coating 2 is peeled off to separate the treated solid 1 from the coating 2 containing carbon dioxide. When the coating 2 is separated, the surface of the treated solid 1 is exposed, and the carbon dioxide fixation capacity is restored.
[0015] According to the immobilization method of the present invention, carbon dioxide can be immobilized in the film without using expensive chemicals. A typical example of the film that can be formed is carbonate, which is stable at room temperature and pressure and has the advantage of being less risky in releasing carbon dioxide after fixation compared to conventional methods such as underground storage, making it extremely valuable industrially.
[0016] The solid to be treated 1 in the present invention refers to one or more of minerals containing calcium silicate and / or magnesium silicate obtained by mining, and slag, clinker, dust, and incineration ash generated in the process of smelting the minerals. These are fixation bodies suitable for fixing carbon dioxide.
[0017] (First embodiment) The immobilization method of the first embodiment will be described below with reference to the process diagram of FIG. 1 and the equipment explanatory diagram of FIG. The immobilization method of the first embodiment is a method in which an immobilization step I and a peeling step II are alternately repeated.
[0018] (Immobilization step I) In the immobilization step I shown in FIG. 1, the treated individual 1 is allowed to coexist with water, so that the calcium and / or magnesium contained therein can be dissolved in the water. When calcium and / or magnesium dissolved in water is reacted with carbon dioxide (specifically, carbonate ions) in the water, carbonates (i.e., calcium carbonate and / or magnesium carbonate) and iron oxide (FeOOH) are produced.
[0019] Representative reaction formulas for producing carbonates include the following formulas 1, 2, and 3. CaO + CO2→ CaCO3...(Formula 1) MgO + CO2→ MgCO3...(Formula 2) Mg3Si2O5(OH)4+ 3CO2→ 3MgCO3+ 2SiO2+2H2O...(Formula 3) Through these reactions, carbon dioxide (CO2) is fixed in these carbonates (CaCO3, MgCO3, 3MgCO3). The produced carbonates and iron oxide are formed as a film 2 on the surface of the treated solid 1.
[0020] The immobilization step I can be carried out using equipment as shown in Fig. 2. Reference numeral 10 denotes a reaction vessel, which is made up of a vessel body 11 and a lid 12 and is capable of being sealed. Inside the reaction tank 10, the object 1 can be supplied by a supply device 13 (for example, a chute), water can be supplied by a water conduit 14, and carbon dioxide gas can be introduced by an introduction pipe 15. When water 4 is stored in the tank body 11 of the reaction tank 10, the objects to be treated 1 are present in the water, and carbon dioxide is also dissolved in the water, a reaction for producing carbonates and the like can be carried out.
[0021] However, the equipment used in the immobilization step I is not limited to that shown in FIG. 2, and any equipment may be used as long as the treated individual 1 can be reacted with carbon dioxide in water. Although not shown, the reaction tank 10 in FIG. 2 may be provided with an agitation device for agitating the treated object 1 and water in the tank body 11, in which case carbonates are efficiently produced.
[0022] In the fixation step I, the treated solid 1 to be supplied is preferably pulverized to make it fine. This increases the specific surface area, making it possible to fix a larger amount of carbon dioxide. A general ball mill or vibration mill can be used for the pulverization. The particle size after the pulverization is preferably 64 μm or less, and more preferably 32 μm or less. The lower limit of the pulverization is 1 μm, and it is preferable to make it 1 μm or more. If the particle size is less than 1 μm, an extremely large amount of energy is required for pulverization, and the pulverization equipment must be enlarged.
[0023] The reaction tank 10 shown in FIG. 2 may be provided with an agitator as necessary so that all of the objects to be treated 1 are brought into contact with the water 4, and the objects to be treated 1 and the water may be agitated. In FIG. 2, the treated individual 1 is shown as a sphere and the coating 2 is shown as having a uniform thickness; however, in reality, the treated individual 1 is irregular in shape and the coating 2 is also non-uniform in thickness, with some coatings partially covering the treated individual 1.
[0024] The weight ratio of water 4 to the treated individual 1 in the tank body 11 in the immobilization step I is preferably 0.01 to 10. In other words, anything from a small proportion of water that only wets the surface of the treated individual 1 to a slurry-like state with a high proportion of water is acceptable. In the immobilization step I, the lower limit of the amount of water coexisting with the treated individual 1 is 0.01 or more by weight ratio. This amount of water allows the dissolution reaction of the treated individual 1 to occur. If the amount of water added is less than 1% by weight, there is a concern that the reaction will be insufficient, and handling will be difficult due to the tendency for dust to be generated. The upper limit of the amount of water coexisting with the treated solid 1 is adjusted so that the weight ratio of water to the treated solid 1 is not more than 10, more preferably not more than 5. If the amount of water added is excessive, it becomes necessary to enlarge the treatment equipment, and it is also undesirable from the viewpoint of conserving water resources.
[0025] The carbon dioxide introduced in fixation process I is contained in the atmosphere and exhaust gases, and using this carbon dioxide can contribute to reducing CO2 emissions on earth. The method of introducing carbon dioxide (gas) is not particularly limited. For example, any method may be used as long as the treated object 1 is placed in a sealed container together with water and carbon dioxide is introduced therein. The reaction tank 10 in FIG. 2 uses an introduction pipe 15, but this is only one example.
[0026] It is preferable to adjust the introduction pressure of carbon dioxide into the reaction tank 10 so that the partial pressure of carbon dioxide is 0.1 atm to 5 atm. This pressure range allows simple introduction equipment to be used. If the partial pressure of carbon dioxide is lower than 0.1 atm, the reaction tends to be slow, and if it is higher than 5 atm, the introduction equipment tends to be expensive.
[0027] In the immobilization step I, when the treated solid 1 is a mineral containing calcium silicate and / or magnesium silicate, sodium hydrogen carbonate and / or potassium hydrogen carbonate can be further added. This can promote the carbonation of the silicate. That is, potassium hydrogen carbonate can carbonate the magnesium silicate by the reaction shown in the following formula 4. Mg3Si2O5(OH)4+ 6KHCO3→ 3MgCO3+ 2SiO2+5H2O+3K2CO3...(Formula 4)
[0028] When magnesium silicate is carbonated, potassium carbonate is produced. However, the produced potassium carbonate is regenerated as potassium bicarbonate through the reaction shown in the following formula 5. Therefore, after a specified amount of potassium bicarbonate has been added, it is no longer necessary to add new potassium bicarbonate. K2CO3+CO2+H2O → 2KHCO3(regenerated with CO2) (Equation 5)
[0029] In the immobilization step I, when the treated solid 1 is a mineral containing calcium silicate and / or magnesium silicate, one or more of sulfide, sulfur, sulfate, and sulfite can be further added. This can promote the dissolution of calcium and / or magnesium into water by the sulfate ions and / or sulfite ions generated. Note that a gas containing sulfur oxide (SOX) may be introduced instead of sulfide, sulfur, sulfate, and sulfite.
[0030] In the immobilization step I, the reaction between calcium and / or magnesium and carbon dioxide proceeds better at higher temperatures. For example, the reaction can be carried out in a temperature range of 5°C to 90°C. In particular, the reaction is preferably carried out in a temperature range of 20°C or higher, and more preferably in a temperature range of 50°C or higher. In this case, the reaction proceeds well and the amount of heat does not need to be excessive. However, at temperatures above 90°C, more heat is required, which tends to be uneconomical.
[0031] The iron content in the treated solid 1 is preferably 25% by weight or less, and more preferably 10% by weight or less. In other words, the lower the iron content in the treated solid 1, the more efficient the fixation of carbon dioxide and the more advantageous it is. The reason for this is that the iron in the treated solid 1 dissolves into the water in the presence of water and deposits as hydroxide on the particle surface of the treated solid 1, forming a coating of iron hydroxide, which tends to inhibit the carbonation of calcium and / or magnesium.
[0032] (Peeling process II) As shown in FIG. 1, in the peeling step II, an external force F is applied to the coating 2 made of carbonate or the like obtained in the fixing step I, and the coating 2 is peeled off. As shown in Fig. 2, the applied external force F should be sufficient to crack or peel off the coating 2. Therefore, it is not necessary to apply a large external force F that would destroy the particles of the treated individual 1, and it can be done by applying a relatively small external force.
[0033] The application of the external force can be performed, for example, by using a device such as a homogenizer (atomizer), an agitator (mixer), or a wet scrubber (wet dust collector), or it can be performed by lightly mixing the material using a pestle and mortar. Therefore, the device is not limited to the above-mentioned devices, and an ultrasonic vibration device that applies a smaller external force F may be used. Furthermore, the peeling process may be performed by applying an external force using thermal stress.
[0034] Although the treated individual 1 and the coating 2 separated in the peeling step II are separated, they remain mixed in the reaction tank 10. Therefore, after the immobilization step I and the peeling step II are repeated several times (for example, three times), the treated individual 1 and the coating 2 can be collected together.
[0035] When the coating 2 obtained in the above-described manner is a carbonate, it is stable at room temperature and pressure. Therefore, if the coating is immobilized and then isolated underground or in the sea, the risk of emitting carbon dioxide can be reduced compared to conventional underground storage. Furthermore, from the treated solid 1 from which carbon dioxide has been separated, new surfaces are exposed as shown in Figure 2. Therefore, even if the fixation of carbon dioxide becomes saturated, the fixation ability can be easily regenerated, and the treated solid 1 can be supplied again to the fixation step I as shown in Figure 1.
[0036] In the above first embodiment, the immobilization step I and the peeling step II are separated and alternately repeated, so that the coating 2 is sufficiently formed before the coating 2 is peeled off, thereby increasing the productivity of the entire immobilization method.
[0037] Second embodiment The immobilization method of the second embodiment will be described with reference to the process diagram of FIG. 3 and the equipment explanatory diagram of FIG. The immobilization method of the second embodiment is a method in which the immobilization step I and the peeling step II are carried out simultaneously.
[0038] In the immobilization method of the second embodiment, as shown in Fig. 3, the immobilization step I and the peeling step II are carried out simultaneously. To carry out this second embodiment, as shown in Fig. 4, a stirring device 20 is provided in a reaction vessel 10, and an external force F is applied to peel off the coating 2 while a coating 2 made of carbonate or the like is being formed.
[0039] There are no particular limitations on the structure or function of the stirring device 20 used, and an example is one in which the stirring blades 21 are rotated by a motor or the like 22. By stirring, the treated individuals 1 collide with each other in the water, or the treated individuals 1 collide with the stirring blades 21, which applies an external force F, causing the coating 2 to peel off from the treated individuals 1. By simultaneously generating and peeling off the coating 2 made of carbonates or the like in this way, the coating 2 is generated while exposing a new surface on the surface of the treated individuals 1, and carbon dioxide can be fixed in this coating 2, so that carbon dioxide can be fixed efficiently. In addition, the carbon dioxide fixation ability of the treated individuals 1 can be regenerated.
[0040] In the second embodiment described above, since the fixing step I and the peeling step II are carried out simultaneously, the fixing process can be performed even in a short operation time. Furthermore, the regenerated individual 1 can be supplied again to the immobilization step I as shown in FIG.
[0041] (Other embodiments) In the carbon dioxide fixation method of the present invention, a preheating step may be provided prior to fixation step I. When the treated solid 1 is a mineral containing calcium silicate and / or magnesium silicate, the crystal structure of these minerals can be partially amorphized by providing such a preheating step. This allows a larger amount of calcium and / or magnesium in the treated solid 1 to be eluted into water. Specifically, it is preferable to heat to 600°C or higher, which allows for good elution. This activates the reaction in fixation step I, enabling efficient fixation of carbon dioxide. EXAMPLES
[0042] [Example 1] The immobilization method shown in FIG. 1 was tested as follows. (Immobilization step I) As the treated object 1, waste ore mainly composed of lizardite and containing 23% Fe, 13% Si, and 14% Mg was used. The waste ore was crushed to 64 μm or less using a mortar and pestle. 15 mL of pure water was added to 3 g of crushed waste ore to prepare a slurry. The prepared slurry was filled into a sample container (a jar-type sample container made of fluororesin (trade name "Teflon (registered trademark)")), and stirred while supplying carbon dioxide so that the pressure inside the sealed container was 5 atm, and the container was kept for one week. The sample container was not heated and the test was performed at room temperature. The slurry taken out of the sample container was separated into solid and liquid, the solid side was dried, and the amount of carbon dioxide absorbed (weight) was calculated by measuring the total carbon. As a result of the calculation, the amount of carbon dioxide absorbed was 0.85% by weight of the waste ore.
[0043] (Peeling process II) Next, after drying, the sample was lightly stirred in a mortar for peeling. After that, 1.5 g was taken out and 7.5 mL of water was added to prepare a slurry again. The prepared slurry was filled into the sample container in the same way as the first time, and stirred while supplying carbon dioxide so that the pressure inside the sealed container was 5 atm, and kept for one week.
[0044] According to the experimental results, the amount of carbon dioxide absorbed (weight) was 1.68% by weight relative to the mineral, and it was confirmed that the amount of carbon dioxide absorbed continued to increase even two weeks after the start of the test.
[0045] [Comparative Example 1] Except for not carrying out the peeling treatment II, the experiment was carried out in the same manner as in Example 1. According to the experimental results, the amount of carbon dioxide absorbed by the mineral after 4 weeks from the start of the test was 0.8% by weight, and no increase in the amount of carbon dioxide absorbed was observed.
[0046] (summary) As described above, it has been confirmed that by carrying out the carbon dioxide fixation method of the present invention, carbon dioxide can be absorbed into a coating formed on the surface of a mineral containing calcium and / or magnesium, without the addition of expensive chemicals. [Industrial Applicability]
[0047] According to the present invention, carbon dioxide can be fixed in a film made of carbonate or the like, and then isolated underground or in the sea, thereby enabling the reduction of carbon dioxide in the atmosphere. [Explanation of symbols]
[0048] 1. Treated specimen 2 Coating 4 water 10 Reactor 11 Tank body 20 Mixing device 21 Mixing blade
Claims
1. an immobilization step of reacting a treated solid containing calcium and / or magnesium with carbon dioxide in the presence of water to form a coating on the treated solid; a peeling step of applying an external force to the treated solid body to which the coating is fixed, peeling off the coating, and regenerating the carbon dioxide fixation capacity. A method for fixation of carbon dioxide, comprising:
2. The fixing step and the peeling step are repeated alternately.
2. The method for fixation of carbon dioxide according to claim 1.
3. The immobilization step and the peeling step are carried out simultaneously.
2. The method for fixation of carbon dioxide according to claim 1.
4. The solid to be treated is one or more of minerals containing calcium silicate and / or magnesium silicate obtained by mining, and slag, clinker, dust, and incineration ash produced during the smelting of the minerals.
2. The method for fixation of carbon dioxide according to claim 1.
5. The treated solid is crushed to 64 μm or less and supplied to the immobilization step.
2. The method for fixation of carbon dioxide according to claim 1.
6. The weight ratio of the water to the solid to be treated in the immobilization step is 0.01 to 10.
2. The method for fixation of carbon dioxide according to claim 1.
7. In the immobilization step, the solid to be treated is reacted with carbon dioxide while adjusting the partial pressure of carbon dioxide to 0.1 atm to 5 atm.
2. The method for fixation of carbon dioxide according to claim 1.
8. In the immobilization step, when the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, sodium hydrogen carbonate and / or potassium hydrogen carbonate is further added.
2. The method for fixation of carbon dioxide according to claim 1.
9. In the immobilization step, when the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, one or more of sulfide, sulfur, sulfate, and sulfite are further added.
2. The method for fixation of carbon dioxide according to claim 1.
10. In the immobilization step, the reaction with carbon dioxide is carried out while maintaining the reaction temperature at 5°C to 90°C.
2. The method for fixation of carbon dioxide according to claim 1.
11. The iron content in the treated solid in the immobilization step is 25% by weight or less.
2. The method for fixation of carbon dioxide according to claim 1.
12. In the immobilization step, the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, The method includes a preheating step of heating the treated solid to 600° C. or higher prior to the fixation step.
2. The method for fixation of carbon dioxide according to claim 1.
Citation Information
Patent Citations
Treating method for fly ash combined with fixation of carbon dioxide
JP2005246225A
Method for manufacturing carbonated slag
JP2013147370A
Carbon dioxide fixing method, recovery method of carbon dioxide, carbon dioxide fixation apparatus, and environment-oriented industrial apparatus
JP2022102786A