Laminate, packaging body, and method for producing laminate

A laminate with a polyolefin resin film, metal/inorganic compound, and polyvinyl alcohol-siloxane coating addresses the barrier property deficiencies of polyolefin films, enhancing packaging performance and environmental sustainability.

JP2024157608AInactive Publication Date: 2024-11-08TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023072047
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional polyolefin resin films lack sufficient oxygen and water vapor barrier properties, making them unsuitable for packaging applications, and existing methods to enhance these properties are either costly or result in structural issues like wrinkles and cracks.

Method used

A laminate structure is developed with a metal and/or inorganic compound layer laminated on a polyolefin resin film, featuring a coating layer composed of polyvinyl alcohol resin and a siloxane compound, optimized for a specific Raman band area ratio and peak intensity ratio to create a dense and stable barrier.

Benefits of technology

The laminate achieves improved oxygen and water vapor barrier properties while maintaining flexibility and recyclability, reducing environmental impact by allowing low-temperature processing and minimizing structural defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157608000004
    Figure 2024157608000004
  • Figure 2024157608000001
    Figure 2024157608000001
  • Figure 2024157608000002
    Figure 2024157608000002
Patent Text Reader

Abstract

To provide a laminate having a good barrier property, in which a metal layer and / or an inorganic compound layer and a coating layer are laminated on a polyolefin-based resin film, a package body, and a method for producing the laminate.SOLUTION: There is provided a laminate having a metal layer and / or an inorganic compound layer and a coating layer in this order on at least one surface of a resin film, wherein the resin film is a polyolefin-based resin film, the coating layer contains a polyvinyl alcohol-based resin and a siloxane compound, and an area ratio A1 / (A1+A2) of a random network structure in a total value of an area A1 of a Raman band indicating a random network structure derived from a siloxane compound and a peak intensity A2 of the Raman band indicating a linear polysiloxane structure and a cyclic siloxane, both of which are obtained by measuring the coating layer by laser Raman spectroscopy, is 0.50 or more and 0.85 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate having excellent barrier properties using a polyolefin resin substrate, a package, and a method for producing the laminate. [Background technology]

[0002] Packaging materials for foods, medicines, daily necessities, etc., are required to have oxygen barrier properties and water vapor barrier properties to prevent deterioration of the contents. As such barrier packaging materials, barrier films have been used in which a metal layer such as aluminum, a metal oxide layer, or even a protective layer is laminated onto a resin film such as polyester. In particular, when a metal oxide layer is laminated, it becomes a transparent film, so it has good visibility, and in the case of packaging food, it is widely used because it is highly convenient, such as being able to be heated in a microwave oven.

[0003] On the other hand, plastic packaging materials are of concern because they do not decompose in soil even if they are buried after use, and they generate a lot of heat when incinerated. Furthermore, marine pollution caused by outflowing plastic waste has become a major problem in recent years, and there is a growing momentum worldwide to reduce the use of plastic materials and reuse them. Therefore, the recovery and recycling of packaging materials has been advocated from the perspective of environmental conservation.

[0004] The base film of the barrier film used in the conventional packaging material has been made of polyester resins, such as polyethylene terephthalate, which has high heat resistance and transparency, or polyamide resins, which have excellent mechanical strength. These films do not have the heat sealability required for bag-making processing of packaging materials, and are therefore laminated with polypropylene resins, which are heat-sealable, for use in packaging materials. However, since it is difficult to separate laminates of different materials when recycling, attempts have been made to make the packaging material mono-material by using the same material to improve recyclability, that is, to use an olefin material similar to polypropylene resins, which have heat sealability, as the base material of the barrier film. However, the olefin material has a problem that the oxygen barrier property of the base material itself is poor compared to polyester resins and polyamide resins. Therefore, in order to improve the oxygen barrier property and improve the storage stability of the contents as a packaging material, a method of improving the barrier property by forming a coating layer has been considered (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4784039 [Patent Document 2] Patent No. 4972951 Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Document 1 discloses a gas barrier film having a vapor-deposited film of inorganic oxide and a gas barrier coating film on a substrate, but the processing conditions are high, at 150°C or higher, and when applied to a polyolefin resin film that has lower heat resistance than polyester resin, there is a problem that wrinkles and cracks occur. Patent Document 2 discloses a vapor-deposited film that can be used as a packaging material by laminating a vapor-deposited layer and a composite coating on a polypropylene film, but the film is not densely cured enough to suppress deterioration of the contents, so it is not sufficient to obtain barrier properties and there is room for improvement.

[0007] An object of the present invention is to provide a laminate, a package, and a method for producing a laminate having good barrier properties, which have a metal layer and / or an inorganic compound layer and a coating layer laminated on a polyolefin resin film. [Means for solving the problem]

[0008] A preferred embodiment of the present invention is as follows. (1) A laminate having a metal layer and / or an inorganic compound layer, and a coating layer in this order on at least one surface of a resin film, The resin film is a polyolefin-based resin film, the coating layer contains a polyvinyl alcohol-based resin and a siloxane compound, A laminate in which the area ratio A1 / (A1+A2) of the random network structure to the sum of the area A1 of the Raman band indicative of a random network structure derived from a siloxane compound and the peak intensity A2 of the Raman band indicative of a linear polysiloxane structure and a cyclic siloxane, obtained by measuring the coating layer by laser Raman spectroscopy, is 0.50 or more and 0.85 or less. (2) The stress at 121°C along the main orientation axis measured by thermomechanical analysis (TMA) is defined as SF 121℃ , the stress at 145°C in the main orientation axis direction is SF 145℃ When SF 145℃ -SCIENCE FICTION 121℃ The laminate according to (1), wherein the elastic modulus is ≦2.50 MPa. (3) The laminate according to (1) or (2), wherein tan δ at 145° C. in the main orientation axis direction is 0.25 or less. (4) The elongation at break in the main axis direction is defined as T0, and the elongation at break in the main axis direction measured after heat-treating the laminate at 130° C. for 10 minutes is defined as T 130 Then, T0 / T 130 The laminate according to any one of (1) to (3), wherein the value is 1.20 or less. (5) The laminate according to any one of (1) to (4), wherein the ratio P1 / P2 of the following peak intensities P1 and P2 detected by measuring the coating layer by an FT-IR-ATR method (attenuated total reflection Fourier transform infrared spectroscopy) is 3.5 or more and 8.0 or less. P1: 1,050~1,080cm -1 Intensity of the largest peak present in P2: 920~970cm -1 Intensity of the largest peak present in (6) The laminate according to any one of (1) to (5), wherein the polyvinyl alcohol-based resin is a polyvinyl alcohol-based resin having one or more functional groups selected from a vinyl ester group, an alkyl group, a carbonyl group, a carboxy group, an acetoacetyl group, a vinyl ether group, an alkyl group, an ethylene group, and a lactone ring. (7) The laminate according to any one of (1) to (6), wherein the coating layer has a thickness of 200 nm or more and 600 nm or less. (8) The laminate according to any one of (1) to (7), wherein the metal layer or the inorganic compound layer contains aluminum. (9) The laminate has a water vapor permeability of 1.0 g / m 2 / 24hr or less, and oxygen permeability is 1.0cc / m 2 The laminate according to any one of (1) to (8), wherein the thermal expansion coefficient is 1 / 24 hr or less. (10) The laminate according to any one of (1) to (9), wherein the metal layer or the inorganic compound layer is in direct contact with the resin film. (11) A packaging material having the laminate according to any one of (1) to (10). (12) At least one surface of the resin film, A method for producing a laminate having a metal layer and / or an inorganic compound layer, and a coating layer in this order, comprising the steps of: the resin film is a polyolefin resin, and the coating layer is obtained by applying a liquid containing a polyvinyl alcohol resin and a siloxane compound and drying the liquid at 120°C or less; A method for producing a laminate, in which the area ratio A1 / (A1+A2) of the random network structure to the total value of the area A1 of the Raman band indicating a random network structure derived from a siloxane compound, obtained by measuring a coating layer by laser Raman spectroscopy, and the peak intensity A2 of the Raman band indicating a linear polysiloxane structure and a cyclic siloxane, is 0.50 or more and 0.85 or less. (13) The method for producing a laminate according to (12), wherein the siloxane compound includes at least one selected from the group consisting of alkoxysilanes and siloxane compounds having a pentamer or less of alkoxysilanes. Effect of the Invention

[0009] According to the present invention, it is possible to provide a dense laminate having good barrier properties, a package, and a method for producing a laminate, which have a metal layer and / or an inorganic compound layer and a coating layer on a polyolefin resin film. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view showing a configuration of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] A preferred embodiment of the laminate, package, and method for producing the laminate of the present invention will be described in more detail below.

[0012] The polyolefin resin film in the present invention is a film mainly composed of a resin having an olefin hydrocarbon as a main constituent unit. The main constituent unit refers to the monomer unit contained in the resin that has the highest content (unit number), and the main component refers to the monomer unit contained in the resin that has the highest content (mass%) of all the constituent components. Examples of polyolefin resins include polymers of α-olefins having alkyl groups on the side chain such as ethylene, propylene, and 4-methyl-1-pentene, and copolymers thereof, copolymers obtained by copolymerizing α-olefins with acrylic acid, C=C bond-containing carboxylic acid, C=C bond-containing carboxylate, C=C bond-containing carboxylate alkyl ester, etc., polymers of norbornene and cyclodiene, and polymers thereof, which may be single-layered or multi-layered. Among these, it is preferable to include polyethylene or polypropylene because they are relatively inexpensive, and it is more preferable to include polypropylene in terms of heat resistance, and it is even more preferable to use polypropylene as the main component from the same viewpoint. In addition, the film may be unstretched or stretched, but it is preferable to be biaxially stretched from the viewpoint of thermal dimensional stability. That is, it is preferable to be a biaxially stretched polyolefin resin film. The polyolefin resin film preferably has a melting point of 150°C or higher. By setting the melting point to 150°C or higher, heat damage due to heat during the process of forming a metal oxide or processing into a packaging material configuration can be prevented, and the heat resistance after processing is also increased, so that the deterioration of the barrier property can be suppressed. The melting point of the film can be measured by the following method using DSC (differential scanning calorimetry). Using a differential scanning calorimeter (EXSTAR DSC6220 manufactured by Seiko Instruments Inc.), a 3 mg sample is heated from 30°C to 260°C at a heating rate of 20°C / min in a nitrogen atmosphere, and then held at 260°C for 5 minutes, and then cooled to 30°C at a rate of 20°C / min. Furthermore, after holding at 30°C for 5 minutes, the temperature is raised again from 30°C to 260°C at a rate of 20°C / min, and the peak temperature of the endothermic curve obtained during this reheating is taken as the melting point. When multiple peak temperatures are observed, the highest temperature is taken as the melting point.

[0013] The glass transition temperature (Tg) of the polyolefin resin film is preferably not higher than 50° C. In this embodiment, the flexibility of the film is high even at low temperatures, and the film does not harden even at low temperatures when used as a package, enabling stable use over a wide temperature range.

[0014] The thickness of the polyolefin resin film is preferably 3 μm or more and 100 μm or less, more preferably 5 μm or more and 50 μm or less, and even more preferably 8 μm or more and 30 μm or less. By making the film thickness 3 μm or more, the rigidity as a support can be maintained, and by making it 100 μm or less, the flexibility as a packaging material is maintained and the followability is improved, which is preferable. The thickness of the polyolefin resin film is determined by the method described in the examples.

[0015] In addition, it is preferable that the polyolefin resin film has a smooth surface. The surface smoothness can be expressed by the arithmetic mean height Sa defined in ISO25178 (2012), and Sa is preferably 50 nm or less, more preferably 30 nm or less. Sa can be measured with a non-contact surface observation device, for example, a scanning white light interference microscope manufactured by Hitachi High-Tech Science Corporation. The measurement is performed using a 10x objective lens, a 1x lens barrel, and a 1x zoom lens, with the wavelength filter set to 530 nm·white, and an area of ​​0.561 mm×0.561 mm is measured in the measurement mode wave. The measurement software used was VS-Measure Version 10.0.4.0, and the analysis software used was VS-Viewer Version 10.0.3.0. In the analysis, the waviness component of the captured image is removed by polynomial 4th order approximation surface correction, and then the image is processed with a median (3×3) filter, followed by an interpolation process (a process in which pixels for which height data could not be obtained are supplemented with height data calculated from surrounding pixels), and then Sa is calculated. By smoothing the surface, defects in the inorganic oxide layer laminated on the surface can be reduced, making it possible to form a good inorganic oxide layer and improving the barrier properties.

[0016] The laminate in the present invention is a laminate having an inorganic layer on at least one surface of a polyolefin resin film, and the inorganic layer preferably has a metal layer and / or an inorganic compound layer.

[0017] The metal layer and / or the inorganic compound layer preferably contains one or more elements selected from Groups 2 to 14 (excluding carbon) of the periodic table, and the inorganic compound layer further contains at least one of oxygen and nitrogen. Among these, from the viewpoint of processing cost and gas barrier properties, the metal layer preferably contains aluminum, and more preferably contains aluminum as the main component. From the same viewpoint, the inorganic compound layer preferably contains at least one element selected from aluminum, magnesium, titanium, tin, indium, and silicon, and more preferably contains silicon or aluminum. Examples of preferable inorganic compound layers include silicon oxide, silicon oxynitride, and aluminum oxide. Furthermore, in the inorganic oxide layer, the ratio of aluminum to the total of elements from Groups 2 to 14 (excluding carbon) of the periodic table is preferably 50 atomic % or more.

[0018] When a metal layer is provided, the thickness of the metal layer is preferably 5 nm to 500 nm, more preferably 10 nm to 100 nm. By making the thickness 5 nm or more, the barrier property can be improved, and by making the thickness 500 nm or less, the substrate can be prevented from being damaged by heat during film formation, which is preferable.

[0019] When an inorganic compound layer is provided, the thickness of the inorganic compound layer is preferably 2 nm to 50 nm, more preferably 2 nm to 20 nm, and even more preferably 4 nm to 10 nm. By making the thickness 1 nm or more, defects such as pinholes in the inorganic compound layer can be reduced, and by making the thickness 50 nm or less, cracks can be suppressed, which is preferable. The thickness of the metal layer or the inorganic compound layer is determined by the method described in the examples.

[0020] In the laminate of the present invention, it is preferable that the metal layer and / or the inorganic oxide layer are in direct contact with the surface of the polyolefin resin film. In the present invention, "in direct contact" refers to an embodiment in which no other layer exists between the polyolefin resin film and the inorganic layer. By adopting such an embodiment, the manufacturing cost and recyclability of the laminate are improved.

[0021] The coating layer in the present invention refers to at least one outermost layer of the laminate, which is a layer laminated on the surface of the metal layer and / or inorganic compound layer opposite to the polyolefin resin, and is a layer containing a polyvinyl alcohol resin and a siloxane compound. Examples of polyvinyl alcohol resins include polyvinyl alcohol, ethylene-vinyl alcohol copolymers, modified polyvinyl alcohol, etc., and these resins may be used alone or in a mixture of two or more kinds. The average molecular weight of the polyvinyl alcohol resin (based on JIS K 6726 (1994)) is preferably 500 or more and 3,000 or less. If the molecular weight is small, the polymer is difficult to fix in the layer, and the barrier property may be reduced.

[0022] Polyvinyl alcohol resins are generally obtained by saponifying polyvinyl acetate, and may be partially saponified by saponifying a portion of the acetate groups, or may be completely saponified, but a higher degree of saponification is preferable. The degree of saponification (based on JISK 6727 (1994)) is preferably 90 mol% or more, more preferably 95 mol% or more. A higher degree of saponification is preferable because it reduces the number of acetate groups with large steric hindrance, reduces the free volume of the coating layer, and increases the crystallinity of the resin, which is advantageous for improving the barrier properties.

[0023] The modified polyvinyl alcohol resin of the present invention refers to a polyvinyl alcohol obtained by chemically reacting a monomer having a different chemical structure with the polyvinyl alcohol, or a monomer having a different chemical structure is copolymerized. Examples of modified polyvinyl alcohol resins include vinyl esters such as propiono vinyl, carboxylic acids, methacrylic acid esters, vinyl ethers such as methyl vinyl ether, and glycols. The modified site of the polyvinyl alcohol resin may be present in either the main chain, side chain, or crosslinked chain of the polyvinyl alcohol resin, but main chain modification is preferable. When the side chain has a functional group with large steric hindrance, the free volume of the coating layer increases, which may reduce the barrier properties, but when the main chain has a modified structure, the steric hindrance can be reduced and the free volume of the coating layer also decreases, which is advantageous for improving the barrier properties and is preferable.

[0024] The detailed structure of the polyvinyl alcohol resin contained in the coating layer can be analyzed by NMR (nuclear magnetic resonance analysis). A piece of film is immersed in deuterated isopropanol, and the coating layer composition is dissolved in the solvent, or the coating layer is physically scraped off using a spatula or the like. Whether the coating layer has dissolved or been scraped off can be confirmed by measuring the film thickness of the coating layer in the same manner as the film thickness evaluation method described below. Next, the sample dissolved in the solvent is analyzed by liquid NMR, or the scraped-off sample is analyzed by solid-state NMR. 13 The structure can be confirmed by analyzing C and protons and assigning each peak. Furthermore, information about the structure can be obtained by combining the analysis of the coating layer obtained in the same manner with the diffuse reflectance method of FT-IR.

[0025] The siloxane compound contained in the coating layer is preferably one or more selected from silicon alkoxides represented by Si(OR)4, hydrolysates of silicon alkoxides, and polycondensates of hydrolysates of silicon alkoxides. Here, R is an alkyl group, and a lower alkyl group having 1 to 4 carbon atoms is particularly preferred. In particular, from the viewpoints of reactivity, stability, and cost, for example, tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane can be preferably used, and these may be used alone or in a mixture of two or more kinds. These silicon alkoxides may be hydrolyzed or polycondensed to form a network.

[0026] The hydrolysis and / or polycondensation of silicon alkoxides can be carried out in the presence of water, a catalyst, and an organic solvent. The water used in the reaction is Si(OR)4 and / or M(OR) n The amount of water is preferably 0.8 equivalents or more and 5 equivalents or less relative to the alkoxy group. By making the amount of water 0.8 equivalents or more, it is preferable that the hydrolysis can be sufficiently advanced to form a network. By making the amount of water 5 equivalents or less, it is preferable that the degree of hydrolysis can be adjusted to suppress random network formation, and the free volume of the film can be reduced to improve the barrier property.

[0027] The catalyst used for the reaction of silicon alkoxide is preferably an acid catalyst. Examples of acid catalysts include hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, acetic acid, tartaric acid, etc., but are not particularly limited. Usually, the hydrolysis and polycondensation reaction of silicon alkoxide can be carried out with either an acid catalyst or a base catalyst. When an acid catalyst is used, the monomers in the system are easily hydrolyzed on average, and condensation is likely to proceed in a linear or network structure. On the other hand, when a base catalyst is used, the reaction mechanism is such that the hydrolysis and polycondensation reaction of alkoxides bonded to the same molecule is easily promoted, so the reaction product tends to be granular with a large free volume and many voids. Since the voids in the film become a permeation path for water vapor and oxygen, it is preferable to use an acid catalyst.

[0028] The organic solvent used in the reaction of silicon alkoxide may be water or an alcohol that is miscible with silicon alkoxide, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, or n-butyl alcohol.

[0029] In addition, commercially available silicate oligomers and polysiloxanes can also be used as polycondensates of silicon alkoxides. Although silicate oligomers and polysiloxanes can be used alone or mixed with low molecular weight silicon alkoxides, it is preferable to use them mixed with low molecular weight silicon alkoxides in order to suppress cracks caused by excessive crosslinking. In addition, even when using silicate oligomers and polysiloxanes, it is preferable to select those with linear or network structure, because the free volume of the film is small and the barrier property is easily improved.

[0030] The coating layer may contain a leveling agent, a crosslinking agent, a curing agent, an adhesion agent, a stabilizer, an ultraviolet absorber, an antistatic agent, etc., within the range that does not impair the gas barrier property. Examples of the crosslinking agent include metal alkoxides of aluminum, titanium, zirconium, etc., and complexes thereof, and examples of the adhesion agent include various silane coupling agents.

[0031] The coating layer of the present invention can be obtained by coating and drying a coating agent obtained by mixing the polyvinyl alcohol resin and the polysiloxane compound on a metal layer and / or an inorganic compound layer. The ratio of the resin and the siloxane compound contained in the coating layer is the ratio of the mass (converted mass of SiO2) when the silicon of the siloxane compound is completely oxidized to the mass of the resin, and the resin / converted mass of silicon oxide is preferably in the range of 15 / 85 to 85 / 15, more preferably in the range of 20 / 80 to 65 / 35, further preferably in the range of 20 / 80 to 40 / 60, and particularly preferably in the range of 20 / 80 to 50 / 50. If this ratio is 15 / 85 or more, it is preferable because it is possible to suppress the film from being weakened by an excess amount of the siloxane compound and the occurrence of cracks. If this ratio is 85 / 15 or less, it is preferable because it is possible to fix the resin with the network of the siloxane compound and suppress the deterioration of the water vapor barrier property. The ratio of resin to silicon oxide can be determined by the ratio c / s of the peak intensity c of fragment ions derived from carbon and the peak intensity s of fragment ions derived from a segment having an Si-O bond, measured at the center of the thickness of the coating layer by a time-of-flight secondary ion mass spectrometer (TOF-SIMS), and it is preferable that c / s is 0.015 or more and 0.650 or less. If the coating layer is exposed on the outermost surface, no pretreatment is required, but if other layers are formed on the coating layer, each layer can be etched by various ions such as an argon ion beam or removed by chemical treatment before analysis. The measurement can be performed, for example, by the following method. The measurement was performed using a time-of-flight secondary ion mass spectrometer TOF-SIMS5 manufactured by ION TOF under the following conditions. The sample after analysis is measured using a stylus-type step gauge (Dektak XTL manufactured by BRUKER) to determine the actual crater depth, and the depth is converted using the average etching rate obtained by dividing the depth by the etching time, and the value at the center is read. If there is no TOF-SIMS measurement data for the part that is exactly half the thickness, the TOF-SIMS measurement data for the measurement point closest to the part that is half the thickness will be used. If there is not a single measurement point closest to the part that is half the thickness, the average value of c / s obtained from the measurement data for each measurement point will be used as c / s for the part that is half the thickness.The analysis will be carried out by reading the raw data using the software SURFACE LAB 7.1 provided with the measuring device, and reading the peaks attributable to various ions from the mass spectrum.

[0032] <Measurement conditions> Primary ion species: Bi + (2pA, 50μs) Accelerating voltage: 25kV Detected ion polarity: positive Measurement range: 100μm×100μm Resolution: 128×128 Etching ion species: O 2+ (2keV, 170nA) Etching area: 300μm×300μm Etching rate: 1sec / cycle.

[0033] In the coating layer of the present invention, the area ratio A1 / (A1+A2) of the random network structure to the total value of the area A1 of the Raman band showing the random network structure derived from the siloxane compound measured by laser Raman spectroscopy and the peak intensity A2 of the Raman band showing the linear polysiloxane structure and the cyclic siloxane is preferably 0.50 or more and 0.85 or less. Note that A1 / (A1+A2) is determined by the method described in the examples, and if a layer is formed on the coating layer, it is polished to expose the coating layer and then measured. The siloxane compound contained in the coating layer can be obtained by hydrolysis and polycondensation of silicon alkoxide. Silicon alkoxide is represented by the general formula Si(OR)4, and becomes a compound having a siloxane bond of Si-O-Si through oxygen bonded to silicon atom by hydrolysis and polycondensation. In this case, the four bonds of silicon are not all uniformly siloxane bonds, but can take various bond states such as three-membered ring or four-membered ring structures, straight-chain structures, and even network structures in which part of the straight chain is cross-linked. After extensive research, the inventors discovered that by increasing the ratio of network structures among these siloxane structures, the structure becomes like a mesh, which can suppress the molecular motion of the polyvinyl alcohol resin and improve the barrier properties. The bond state of siloxane can be analyzed by laser Raman spectroscopy, and the network structure can be analyzed by laser Raman spectroscopy at a wave number of 425 cm. -1 The linear structure has a 4-membered ring structure that contributes little to the immobilization of polyvinyl alcohol resins, and the linear structure has a 490 cm -1 The signal indicating the network structure is detected around the wave number of 415 to 430 cm. The ratio of the network structure to the peak area can be calculated by waveform separation of these spectra. -1 The four-membered ring and linear chain structures, which have a small contribution to the network, have a peak in the range of 480–500 cm -1In the Raman spectrum of the coating layer, these peaks are separated, and the area of ​​the peak showing the network structure is A1, and the area of ​​the peak showing the four-membered ring and linear structure is A2. The value of A1 / (A1+A2) indicates the ratio of the network structure to the main siloxane bonds. The value of A1 / (A1+A2) is preferably 0.50 to 0.85, more preferably 0.60 to 0.80. When A1 / (A1+A2) is 0.50 or more, there is a lot of siloxane with a network structure, and the coating layer can be fixed in a mesh-like structure, so that stable barrier properties can be obtained, which is preferable. When A1 / (A1+A2) is 0.85 or less, it is preferable because it is possible to avoid embrittlement due to an excessive amount of siloxane network structure and maintain flexibility.

[0034] One of the preferred embodiments for obtaining a siloxane compound having a network structure is to use a polyvinyl alcohol resin having a hydrophobic modified group. In general, both polyvinyl alcohol resins and siloxane compounds have hydroxyl groups, and can form hydrogen bonds during coating and drying to form a coating film. However, hydrogen bonds are weaker than siloxane bonds, which are covalent bonds, and are dissociated by heat or moisture, etc., and the molecular motion of the resin cannot be suppressed, resulting in the formation of gas permeation paths, which has been a factor in making it difficult to obtain stable barrier properties. If alkoxysilanes are polycondensed to reduce terminal silanols and form networked siloxane bonds, dissociation of hydrogen bonds can be suppressed and polyvinyl alcohol can be fixed by the siloxane network structure, so that stabilization of barrier properties can be expected. Therefore, the inventors have conducted extensive research and found that by increasing the hydrophobicity of polyvinyl alcohol resins, the barrier properties can be improved even at relatively low temperatures of 120°C or less. It is considered that when a highly hydrophobic polyvinyl alcohol resin is used, the interaction between the polyvinyl alcohol resin and the hydroxyl group of the alkoxysilane is reduced, and the interaction between the silanol groups is strengthened and the siloxane network structure is increased. By bringing the raw materials forming the siloxane network structure into close proximity to each other, the reaction is facilitated, so that the thermal energy required for the formation of the siloxane network can be reduced, and a sufficient network structure can be formed even at low temperature processing. Furthermore, since the polyolefin resin film constituting the laminate of the present invention has a lower water absorption rate than conventional polyester resins, it has been found that by making the coating layer hydrophobic, the deformation difference due to the water absorption of the resin film and the coating layer is reduced, and the laminate is less likely to curl.

[0035] Examples of polyvinyl alcohol resins having hydrophobic modified groups include vinyl esters such as propionyl vinyl, carboxylic acids, methacrylic acid esters, vinyl ethers such as methyl vinyl ether, glycols, saturated / unsaturated alkyls, and hydrocarbons having a cyclic structure. In other words, it is preferable that the polyvinyl alcohol resin is a polyvinyl alcohol resin having one or more functional groups selected from vinyl ester groups, alkyl groups, carbonyl groups, carboxy groups, acetoacetyl groups, vinyl ether groups, alkyl groups, ethylene groups, and lactone rings. The modified site may be in either the main chain or the side chain. Among these modified structures, main chain modification with alkyl groups or cyclic structures is preferable from the viewpoint of being able to uniformly mix with hydrolysates and polycondensates of alkoxysilanes while suppressing the expansion of free volume that serves as a gas permeation path due to the presence of hydrophobic groups with large steric hindrance. On the other hand, from the viewpoint of increasing hydrophobicity, a method of lowering the saponification degree of polyvinyl alcohol resins may be considered, but a lower saponification degree may be undesirable because it causes the crystallization of polyvinyl alcohol resins to decrease and the barrier properties to deteriorate. The degree of saponification is preferably 90 mol % or more, and more preferably 95 mol % or more. Specific examples of preferred resins include modified poval D polymer and Z polymer manufactured by Nippon Vinyl Acetate & Poval Corporation, "Gosenex" (registered trademark) Z series manufactured by Nippon Synthetic Chemical Industry Co., Ltd., and modified polyvinyl alcohol resin "Exceval" (registered trademark) manufactured by Kuraray Co., Ltd.

[0036] Another preferred embodiment of obtaining a siloxane compound with a network structure includes an example in which the raw material of the siloxane compound contains an alkoxysilane or a siloxane compound with a short chain length of alkoxysilane pentamer or less. If a polymer in which polycondensation has already progressed is used as the siloxane compound, the amount of silanol residue is limited, so that polycondensation between molecular chains is difficult to proceed, and the network structure cannot be formed sufficiently. It is preferable to have a low molecular weight component as a crosslinking agent for bonding between molecular chains, because a dense network structure can be formed.

[0037] In the coating layer of the present invention, the ratio P1 / P2 of the peak intensities P1 and P2 detected by the FT-IR-ATR method is preferably 3.5 or more and 8.0 or less, more preferably 4.0 or more and 6.5 or less (however, P1: 1,050 to 1,080 cm -1 Intensity of the maximum peak present at 920-970 cm -1 It indicates the intensity of the maximum peak present in the. Note that peak intensity is the absorbance (unitless) at the peak position). The FT-IR-ATR method can capture the characteristics of the surface coating layer, where P1 indicates the reaction product Si-O-Si, and P2 indicates the amount of the reaction raw material Si-OH. Therefore, the ratio of peak intensity P1 to P2, P1 / P2, increases as the polycondensation of alkoxysilane proceeds. As the polycondensation reaction of alkoxysilane proceeds, the terminal OH is reduced to form a strong film, improving the barrier properties and improving the moist heat resistance when retorted as a packaging material. If P1 / P2 is 3.5 or more, the terminal OH is reduced to form a strong film, which can be a layer with excellent barrier properties and moist heat resistance. It is preferable to set P1 / P2 to 8.0 or less, as this can suppress cracks and embrittlement due to shrinkage of the film. Note that P1 and P2 are determined by the method described in the examples, and if a layer is formed on the coating layer, the coating layer is polished to expose it before measurement.

[0038] In order to set the ratio P1 / P2 of the peak intensities P1 and P2 detected by the FT-IR-ATR method to a preferred range, it is necessary to sufficiently proceed with the reaction of alkoxysilane. Since the polycondensation of alkoxysilane is a dehydration reaction, it can be proceeded by heating, but since the polyolefin resin film constituting the laminate of the present invention has a lower heat resistance than conventional polyester resins, it is difficult to sufficiently proceed with the reaction. As a result of intensive research, the inventors have found that by using a polyvinyl alcohol resin having a hydrophobic modifying group, the hydrolysis of alkoxysilane and the interaction between the polycondensate and the resin are reduced, and by increasing the interaction between the hydrolysis of alkoxysilane and the polycondensate, these reactions are easily promoted and a network can be formed at a low temperature. In addition, it has been found that the deterioration of the barrier property in the subsequent process can be suppressed by adjusting P1 / P2 to 3.5 or more and 8.0 or less. When the laminate of the present invention is used as a packaging material, it is heated and pressure is applied because it goes through printing and bag making processes. In this case, a coating that has an appropriate network structure is preferable because it can also function as a protective film. On the other hand, if P1 / P2 is less than 3.5, for example, there is a lot of unreacted metal alkoxide, so the coating layer does not harden and is easily scratched, which deteriorates the barrier properties, or the unreacted metal alkoxide cures and shrinks depending on the processing conditions, which deteriorates the barrier properties. On the other hand, if P1 / P2 is more than 8.0, the coating layer becomes brittle, and cracks are likely to occur due to the pressure and transport tension during lamination, which can deteriorate the barrier properties.

[0039] In the coating layer of the present invention, the free volume radius of the vacancies determined by the positron annihilation method is preferably 0.260 nm or less. The positron beam method is one of the positron annihilation lifetime measurement methods, and is a technique for non-destructively evaluating information on the size, number concentration, and size distribution of vacancies of about 0.1 to 10 nm from the annihilation lifetime by measuring the time (on the order of several hundred ps to several tens of ns) from when a positron is incident on a sample to when it annihilates. A radioisotope ( 22This method differs significantly from the usual positron annihilation method in that it uses a positron beam instead of Na), making it possible to measure thin films of about several hundred nm thick formed on silicon or quartz substrates. The free volume radius can be measured, for example, by the following procedure. The laminate is attached to a 15 mm x 15 mm silicon wafer, and the positron annihilation lifetime is measured under the following conditions using a sample that has been vacuum degassed at 25°C.

[0040] Measurement equipment: Fuji Invac small positron annihilation generator PALS-200A Positron source: 22 Na-based positron annihilation Gamma-ray detector: BaF2 scintillator and photomultiplier tube Beam intensity: 3keV Measurement temperature: 25℃ Measurement atmosphere: Vacuum Total count: Approximately 5,000,000 counts.

[0041] The obtained positron annihilation lifetime curves were subjected to three-component analysis using the nonlinear least squares program POSITRONFIT, and the annihilation lifetimes were designated τ1, τ2, and τ3 in ascending order of annihilation lifetime. The free volume radius R3 (nm) of the vacancy was calculated from the longest average annihilation lifetime τ3 using the following formula.

[0042] τ3=(1 / 2)[1-{R3 / (R3+0.166)}+(1 / 2π)sin{2πR3 / (R3+0.166)}] -1 .

[0043] When the free volume radius of the coating layer is 0.260 nm or less, the pore size of the coating layer is small and the layer is dense, so that the barrier property is good. Although the lower limit of the free volume radius is not particularly limited, it is preferably 0.240 nm or more from the viewpoint of cracking.

[0044] As a method for reducing the free volume radius, it is preferable to control the bonding mode of the silicon alkoxide described above or to increase the reaction progress. It is known that the structure of silicon alkoxide changes depending on the hydrolysis conditions during the preparation of the coating material, and it is preferable to use an acid as a hydrolysis catalyst because the cyclic structure is reduced and the free volume radius can be reduced. In addition, when the reaction progress is low, unreacted hydroxyl groups with a high degree of freedom of movement are present and the free volume increases, so it is preferable to fix it by polycondensation. Furthermore, reducing the branching of the modified group of the polyvinyl alcohol resin is also effective in reducing the free volume. When the steric hindrance of the modified group of the polyvinyl alcohol resin is large, or when the saponification degree is low and the steric hindrance is large, the free volume also increases, and the barrier property may deteriorate.

[0045] The coating layer of the present invention preferably has a thickness of 200 nm or more and 600 nm or less, more preferably 320 nm or more and 500 nm or less. By making the thickness 200 nm or more, the metal layer and / or metal compound layer can be coated without defects and the barrier property can be improved. By making the thickness 600 nm or less, cracks due to thermal shrinkage during curing and insufficient curing can be prevented, which is preferable. The thickness of the coating layer is determined by the method described in the examples.

[0046] The laminate of the present invention has a stress at 121°C in the main orientation direction measured by thermomechanical analysis (TMA) of SF 121℃ , the stress at 145°C in the main orientation axis direction is SF 145℃ When SF 145℃ -SCIENCE FICTION 121℃ It is preferable that the stress satisfies ≦2.50 MPa. Each stress is determined by the method described in the Examples. The main orientation axis direction of the laminate refers to the direction in which the stress of the maximum point strength is greatest when a rectangular sample of 50 mm in length (measurement direction) × 10 mm in width is pulled in the measurement direction at room temperature at a tensile speed of 300 mm / min until breakage occurs, and the details of the method of determining the stress are as described in the Examples. SF 145℃ -SCIENCE FICTION 121℃By satisfying the condition of ≦2.50 MPa, when the laminate of the present invention is subjected to post-processing including high-temperature treatment such as heat sealing, the laminate is prevented from being deformed by heat, and defects such as pinholes and cracks are prevented from being generated in the inorganic oxide layer, which makes it possible for the laminate to maintain excellent water vapor barrier properties.

[0047] science fiction 145℃ -SCIENCE FICTION 121℃ Meeting ≦2.50 MPa means that the shrinkage stress is small in the high temperature range of 121°C or higher. When the shrinkage stress is small in the high temperature range of 121°C or higher, the shrinkage stress becomes even smaller in the temperature range from below 121°C to room temperature, and the dimensional change over time becomes extremely small. Therefore, when the laminate of the present invention is used for bag manufacturing, the dimensional stability is good, so that the deterioration of quality due to deformation during printing, lamination, and bag manufacturing can be reduced. In particular, during heat sealing in bag manufacturing, wrinkles and shrinkage in the heated parts are suppressed, and the yield of the final product is also high, which is preferable. In addition, when the laminate of the present invention is stored in a roll for a long period of time, it is expected that deformation of the roll, such as the occurrence of wrinkles (tightening of the roll), can be suppressed.

[0048] From the above perspective, SF 145℃ -SCIENCE FICTION 121℃ The upper limit of SF is preferably 2.00 MPa, more preferably 1.80 MPa, and further preferably 1.50 MPa. 145℃ -SCIENCE FICTION 121℃ The smaller the value, the more preferable it is, and the lower limit is not particularly limited, but is substantially about 0.05 MPa.

[0049] science fiction 145℃ or Sci-Fi 121℃ can be read from the thermal shrinkage stress curve obtained by performing a thermomechanical analysis under the temperature and load conditions shown in the Examples. The thermomechanical analyzer is not particularly limited and can be appropriately selected as long as it is capable of performing the measurement. For example, TMA / SS6000 manufactured by Seiko Instruments Inc. can be used.

[0050] Laminated SF 145℃ -SCIENCE FICTION 121℃The method of controlling the stress to 2.50 MPa or less or to the above-mentioned preferred range is not particularly limited, but may be, for example, a method of adjusting the conditions of a tenter device during the film formation of a polypropylene-based resin film constituting a laminate. More specifically, a method of setting the lower limit of the heat treatment temperature of the tenter to 140°C, more preferably 150°C, even more preferably 155°C, and particularly preferably 161°C, and the upper limit to 167°C, more preferably 166°C, and even more preferably 165°C, a method of setting the lower limit of the relaxation rate to 2%, more preferably 5%, even more preferably 7%, and particularly preferably 9%, and the upper limit to 20%, more preferably 18%, even more preferably 17%, and particularly preferably 15%, and the like. When the heat treatment temperature of the tenter is set to 168°C or more, the molecular chains that were strongly oriented in the main orientation axis direction are loosened, and the SF 145℃ -SCIENCE FICTION 121℃ It may be difficult to control the molecular weight distribution Mz / Mw to 2.50 MPa or less. In addition, there are also methods for controlling the molecular weight distribution Mz / Mw of the polypropylene resin composition constituting the polypropylene resin film to 1.5 to 4.5, and methods for controlling the differential distribution value when the logarithmic molecular weight Log(M) is 6.5 to 1.0% to 10%. Note that none of these methods is essential, and they can be combined as appropriate. Note that Mz is the Z-average molecular weight, and Mw is the weight-average molecular weight. The logarithmic molecular weight Log(M) is the common logarithm of the polymer molecular weight M.

[0051] The laminate of the present invention preferably has a tan δ in the main orientation axis direction at 145°C of 0.25 or less. Tan δ is also called loss tangent, and correlates with the degree of mobility of the molecular chains of the resin constituting the laminate, and generally increases with increasing temperature in the region of 100°C or higher. Tan δ in the main orientation axis direction at 145°C is an index that correlates with the degree of mobility of the molecular chains in the film at around 145°C. By reducing this value, in other words by suppressing the movement of the molecular chains at high temperatures, the heat shrinkage stress of the laminate at high temperatures can be suppressed, and the stress at 121°C in the main orientation axis direction of the laminate measured by thermomechanical analysis (TMA) can be reduced to SF 121℃ , the stress at 145°C in the main orientation axis direction is SF 145℃ When SF 145℃-SCIENCE FICTION 121℃ ≦2.50MPa. From the above viewpoint, tan δ in the main orientation axis direction at 145°C is preferably 0.23 or less, more preferably 0.21 or less, and even more preferably 0.19 or less. The smaller tan δ in the main orientation axis direction at 145°C is preferable, and the lower limit is not particularly limited, but is substantially about 0.01. Tan δ can be obtained by cooling to a low temperature of -100°C, and then measuring the viscoelasticity-temperature curve from -100°C to 180°C after starting to heat up, and the details of the measurement method are as described in the Examples.

[0052] The method for making the tan δ of the laminate in the main orientation axis direction at 145° C. 0.25 or less is not particularly limited, but examples thereof include a method of reducing the molecular weight distribution Mz / Mw of the resin composition constituting the polypropylene-based film, a method of performing a heat relaxation treatment after uniaxial stretching in the film-forming process of the polypropylene-based resin film, a method of increasing the heat treatment temperature of the tenter, a method of increasing the relaxation rate of the tenter, etc. By using these methods alone or in appropriate combination, it is possible to reduce tan δ.

[0053] The laminate of the present invention is characterized in that the elongation at break in the main orientation axis is defined as T0, and the elongation at break in the main orientation axis direction measured after the laminate is heat-treated at 130° C. for 10 minutes is defined as T 130 Then, T0 / T 130 It is preferable that the value of T0 / T0 is 1.20 or less. The elongation at break is the maximum elongation at break when a rectangular sample of 150 mm length x 10 mm width with the long side in the main orientation axis direction is prepared and pulled in the measurement direction at room temperature at a tensile speed of 300 mm / min, and is specifically determined by the method described in the Examples. The elongation at break is determined by (l-l0) / l0 x 100, where l0 is the length of the sample before the test and l is the length at break. In the present invention, T0 / T 130A value of 1.20 or less indicates that even after 10 minutes of heat treatment at 130°C, there is little change from before the heat treatment, and that the heat damage during manufacturing is small. Heat treatment at 130°C for 10 minutes means that the material is placed in an oven (such as Espec Corporation's SPHH-201 thermostatic oven with safety door) that has been kept stable at a set temperature of 130°C for 10 minutes or more in a laboratory environment of 23°C and 50% RH, and then removed after 10 minutes. T----0 / T 130 By making T0 / T 1.20 or less, it is possible to suppress heat damage during the production of the laminate, and to exhibit good barrier properties. In addition, it is possible to suppress the winding tightness of the polyolefin resin film, and to suppress the deterioration of the barrier properties. 130 The lower limit is effectively 0.5.

[0054] The ratio T0 / T of the elongation at break in the main orientation axis direction of the laminate of the present invention before and after heat treatment at 130° C. for 10 minutes 130 In order to keep T to 1.20 or less, it is preferable not to expose to high temperatures during the manufacturing process. For example, when a polypropylene resin is used as the polyolefin resin film that serves as the base film, it is easily affected by heat, and exposure to high temperatures causes the crystal structure to collapse and the orientation to relax, resulting in a decrease in the elongation at break. Once the polymer structure collapses due to exposure to high temperatures, the elongation at break will further decrease when exposed to high temperatures again. In other words, in the case of a laminate manufactured without exposure to high temperatures, T 130 The decrease in T0 / T 130 The value of T is 1.20 or less for the laminates produced at high temperatures, while the value of T 130 The decrease in T0 / T 130is a value exceeding 1.20. In the production of the laminate of the present invention, the process exposed to high temperatures includes a process of laminating a metal layer or a metal oxide layer and a process of laminating a coating layer. As described later, the process of laminating a metal layer or a metal oxide layer can be performed by a known method such as a vapor deposition method. In this process, the main roll can be cooled to suppress damage to the substrate, and since the processing is performed at a very high speed, the thermal effect can be relatively suppressed. On the other hand, the process of laminating the coating layer and promoting its reaction cannot avoid heating for drying the coating agent and promoting the reaction of the coating layer, so the effect on the substrate is large. In terms of thermal damage, the preferred temperature range for the drying process of the coating layer is, for example, 120°C or less, more preferably 110°C or less. In order to improve the barrier properties of the coating layer, even if further heat treatment is performed after drying, the treatment temperature is preferably 80°C or less, more preferably 60°C or less, in order to suppress thermal damage as much as possible. In addition, if the treatment time is 14 days or less, thermal damage can be suppressed, which is also preferable in terms of production efficiency.

[0055] The laminate of the present invention has a water vapor transmission rate of 1.0 g / m 2 / 24hr or less is preferable, and 0.5g / m 2 / 24hr or less. The oxygen permeability is more preferably 1.0cc / m 2 / 24hr or less is preferable, and 0.3cc / m 2 The smaller the water vapor permeability and oxygen permeability, the more preferable. There is no particular lower limit, but the water vapor permeability is substantially 0.01 g / m 2 / 24hr, oxygen permeability is 0.01cc / m 2 / 24hr. Water vapor transmission rate is 1.0g / m 2 / 24hr or less, oxygen permeability 1.0cc / m 2 By setting the storage time to 24 hours or less, deterioration of the contents due to moisture absorption and oxidation can be prevented when the contents are packaged, which is preferable. The water vapor transmission rate and oxygen transmission rate are determined by the method described in the Examples.

[0056] The laminate of the present invention can be obtained by forming a metal layer and / or an inorganic compound layer on at least one surface of a polyolefin resin film, and then laminating a coating layer. The metal layer and / or the inorganic compound layer can be formed by using known methods such as vacuum deposition, sputtering, ion plating, and plasma vapor phase growth, but the deposition method can be preferably used because it can form a film at high speed with good productivity. The deposition method of the vacuum deposition method includes, but is not limited to, electron beam (EB) deposition, resistance heating, and induction heating. In addition, when forming a metal layer and / or an inorganic compound layer on a long resin film roll pair, it is preferable to cool the main roll for deposition to prevent heat damage of the film, and the temperature is preferably 20°C or less, more preferably 0°C or less. As a method for obtaining a metal layer, an example can be given of deposition using a target metal as a raw material. As a method for obtaining an inorganic compound layer, in addition to deposition using a compound of a target composition as a raw material, a method can be exemplified in which a metal is used as a raw material and a reactive gas is introduced into the deposited metal vapor to obtain an inorganic compound. For example, when obtaining an aluminum oxide layer, aluminum is used as a deposition material, and a gas containing oxygen is introduced into the evaporated aluminum vapor to form an inorganic oxide layer on the film. The gas introduced may contain a gas having a composition that reacts with the evaporated metal and is incorporated into the layer, and may contain an inert gas or the like to control the film quality. The surface of the resin film on which the metal layer and / or inorganic compound layer is formed may be subjected to a surface modification treatment in order to improve interlayer adhesion. The surface modification treatment may be in-line or off-line, and the modification treatment method is not particularly limited, but examples thereof include known methods such as corona treatment, plasma treatment, ion beam treatment, and flame treatment. These surface modification treatments may be performed using air, as well as argon, nitrogen, oxygen, carbon dioxide, hydrogen, ammonia, hydrocarbons (C n H 2n+2The treatment may be performed under an atmosphere of various gases such as argon, nitrogen, etc., where n is an integer of 1 to 4, or a mixed gas of these. The gas used for the surface modification treatment can be selected depending on the ease of discharge, the energy of the active species obtained, and the type of functional group to be introduced, but it is preferable that the gas contains carbon dioxide gas or oxygen gas for introducing the functional group, and argon or nitrogen gas which easily generates a stable discharge.

[0057] The laminate of the present invention is preferably produced by a production method including a step of applying a coating agent containing a polyvinyl alcohol resin and a siloxane compound to the inorganic layer of a laminate having a metal layer and / or an inorganic compound layer on at least one side of a polyolefin resin film, and a step of drying. By adopting this embodiment, a dense laminate with good barrier properties can be obtained. In addition, a laminate with high water vapor barrier properties and oxygen barrier properties can be obtained while suppressing the environmental load during production. In particular, by adopting this embodiment, the environmental load during production can be reduced because it can be sufficiently cured even at low temperatures, and can be sufficiently cured even at high temperatures in a short time, which is preferable.

[0058] In addition, from the viewpoint of water vapor barrier properties and oxygen barrier properties, the mass ratio of the polyvinyl alcohol resin in the coating agent to the SiO2 equivalent mass when the silicon of the siloxane compound is completely oxidized is preferably in the range of resin / SiO2 equivalent mass=15 / 85 to 85 / 15, more preferably in the range of 20 / 80 to 65 / 35, even more preferably in the range of 20 / 80 to 40 / 60, and particularly preferably in the range of 20 / 80 to 50 / 50.

[0059] In addition, in the method for producing the laminate, it is preferable that the above-mentioned A1 / (A1+A2) is 0.50 or more and 0.85 or less for the film obtained through the process of applying the coating agent and the process of drying. This embodiment indicates that the siloxane compound has a network structure as the main structure, and this fixes the polyvinyl alcohol resin and reduces its mobility, thereby improving the barrier property.

[0060] The coating method of the coating agent containing the polyvinyl alcohol resin and the siloxane compound is not particularly limited, and known methods can be used, such as direct gravure, reverse gravure, microgravure, rod coat, bar coat, die coat, and spray coat. The drying temperature after coating is preferably 70°C or higher and 120°C or lower, and more preferably 80°C or higher and 110°C or lower. The drying temperature refers to the maximum temperature reached on the film surface. By setting the temperature at 70°C or higher, the solvent can be removed to form a layer, and by setting the temperature at 120°C or lower, the thermal shrinkage and deformation of the polyolefin resin film can be suppressed. After coating and drying, the laminate of the present invention may be further heat-treated to promote the polycondensation reaction of silicon alkoxide and improve the barrier property. The atmospheric temperature when heat-treating is preferably 30°C or higher and 80°C or lower, and more preferably 30°C or higher and 60°C or lower. The heat treatment time is preferably 1 day or higher and 14 days or lower, and more preferably 3 days or higher and 7 days or lower. By setting the heat treatment temperature to 30°C or higher, crosslinking of the coating layer can be promoted to improve the barrier properties, and by setting the temperature to 60°C or lower, curling and shrinkage of the film due to heat treatment can be suppressed.

[0061] The packaging body of the present invention has the laminate. The packaging body may be laminated with another resin film for printing or a heat seal layer for bag making, or for improving rigidity. The heat seal layer or the resin film for improving rigidity is preferably a polyolefin resin in order to improve recyclability. By including the laminate in the packaging body, it is preferable that the packaging body has good and stable water vapor barrier properties and oxygen barrier properties, and deterioration of the contents can be suppressed. EXAMPLES

[0062] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention. [Evaluation method] (1) Thickness of the base film The thickness of ten randomly selected points was measured in an atmosphere of 23°C and 65% RH using an electronic micrometer (K-312A type) manufactured by Anritsu Corp. The arithmetic mean value of the thicknesses obtained at the ten points was regarded as the thickness of the substrate film (unit: μm).

[0063] (2) Thickness of the metal layer and / or inorganic compound layer The thickness was measured by cross-sectional observation using a transmission electron microscope (TEM). Using a microsampling system FB-2000A manufactured by Hitachi, Ltd., a sample for observation was prepared by the FIB method (specifically, based on the method described in "Polymer Surface Processing Science" (by Akira Iwamori) p.118-119). Next, the cross-section of the sample for observation was observed using a transmission electron microscope H-9000UHRII manufactured by Hitachi, Ltd., at an acceleration voltage of 300 kV, and the thickness of the metal layer and / or inorganic compound layer was confirmed at any 10 points. The arithmetic average value of these values ​​was taken as the thickness of the metal layer and / or inorganic compound layer (unit: nm).

[0064] (3) Thickness of the coating layer The laminate was cut perpendicular to the film surface with a microtome, and the cross section of the laminate was observed and measured with a scanning electron microscope. Observation was performed using a STEM (scanning transmission electron microscope / H-9000UHRII) manufactured by Hitachi, Ltd., and images were taken at three points at a magnification of 100,000 times. The thickness of the coating layer was measured in the three images obtained, and the average value was taken as the thickness of the coating layer.

[0065] (4) Laser Raman spectroscopy The coating layer of the laminate was separated by cutting, and the Raman spectrum of the coating layer was obtained by measurement under the following conditions. Equipment: Laser Raman microscope RAMANtouch (Nano Photon Corporation) Measurement mode: Microscopic Raman, point mode Objective lens: x10 Laser wavelength: 532nm Laser power: 100mW Diffraction grating: Single 600gr / mm Slit: 100μm Detector: CCD 400×1,340 The obtained spectrum was analyzed using the analysis software RAMAN Viewer manufactured by Nano Photon. The spectrum was smoothed by the moving average method, the baseline was corrected with a spline curve, and the 600-250 cm -1 With a peak wave number of 425 cm -1 , 485cm -1 The area A1 of the separated two components (peak position 425 cm) was calculated by autofitting the Lorentzian function approximation. -1 ), area A2 (peak wave number 485 cm -1 ) the area ratio A1 / (A1+A2) was calculated.

[0066] (5) Science fiction 145℃ -SCIENCE FICTION 121℃ <Identifying the main orientation axis of the laminate> Cut the laminate into a rectangular sample measuring 50 mm in length and 10 mm in width with the long side facing in any direction. <1> In this case, the rectangular sample <1> The direction in which the long side of the sample faces was defined as 0°. Next, a sample of the same size was placed so that the long side direction was rotated 15° to the right from the 0° direction. <2> Similarly, the rectangular sample was rotated 15° in the long side direction and the sample was taken. <3> ~ <12> Next, each rectangular sample was set in a tensile tester (Orientec Co., Ltd. "Tensilon" (registered trademark) UCT-100) with an initial chuck distance of 20 mm so that the long side direction was the tensile direction, and a tensile test was performed at a tensile speed of 300 mm / min in a room temperature atmosphere. The maximum load until the sample broke was read at this time, and the value divided by the cross-sectional area (film thickness x width) of the sample before the test was calculated as the stress of the maximum point strength. The same measurement was performed five times for each sample to determine the average value of the stress of the maximum point strength, and the long side direction of the sample with the largest average value was set as the main orientation axis of the laminate. <Measurement of thermal shrinkage stress by thermomechanical analysis (TMA)> The laminate was cut into a rectangular sample with a width of 4 mm and a length of 50 mm, with the long side being the "main orientation axis direction" defined as above, and clamped in a metal chuck so that the sample length was 20 mm. It was then set in the thermomechanical analyzer described below, and the thermal shrinkage stress curve in the main orientation axis direction of the laminate with the sample length kept constant under the temperature and load conditions described below was obtained. Equipment: TMA / SS6000 (Seiko Instruments Inc.) Temperature range: 23~200℃ Heating rate: 10℃ / min ·Hold: 10 minutes Sampling time: 10 seconds / time Nitrogen cooling: No Control mode: L Upper limit displacement during standby: 0μm Starting Displacement: 0μm Load rate: 0.1μm / min ·Holding: 600 minutes Measurement atmosphere: Nitrogen Measurement thickness: The sum of the thickness of the substrate film, the thickness of the metal layer and / or inorganic compound layer, and the thickness of the coating layer.

[0067] <SF 145℃ -SCIENCE FICTION 121℃ Calculation of > From the heat shrinkage stress curve obtained by the above measurement method, the shrinkage stress value at the temperature closest to 25°C is set as the zero point, and then the following values ​​are read and calculated. SF 145℃ -SCIENCE FICTION 121℃ was calculated. science fiction 145℃ : Heat shrinkage stress (MPa) at 145°C in the main orientation direction of the laminate science fiction 121℃ : Heat shrinkage stress (MPa) at 121°C in the main orientation axis direction of the laminate.

[0068] (6) Tangent delta at 145°C along the main orientation axis The measurement direction was the main orientation axis direction of the laminate determined in (5), and a test piece (width 5 mm x length 20 mm) cut with the measurement direction as the long side was attached to the chuck of the device in a 23°C atmosphere, cooled to -100°C, and tan δ was measured from -100°C to 180°C after the start of heating. A viscoelasticity-temperature curve was drawn using the dynamic viscoelasticity method, and tan δ at each temperature was calculated. The test was performed with n=3, and the average of the obtained values ​​was taken as tan δ in the measurement direction. The measurement device and conditions are as follows. Equipment: Rheogel-E4000 (UBM) Geometry: Tensile Chuck distance: 10mm Frequency: 10Hz Distortion: 0.1~0.2% Temperature range: -100~180℃ Heating rate: 5℃ / min Measurement atmosphere: Nitrogen.

[0069] (7) Elongation ratio at break (T0 / T 130 ) <Measurement of elongation at break> The laminate was sampled in a rectangle of length 150 mm x width 10 mm with the main orientation axis direction of the laminate determined in (5) as the measurement direction and the main orientation axis direction of the laminate as the long side. Using a universal testing machine RTG-1210 "Tensilon" (registered trademark) manufactured by Orientec Co., Ltd., the initial chuck distance was set to 120 mm so that the long side direction was the tensile direction, and the elongation at break was calculated from the length at break when pulled in the measurement direction at room temperature at a pulling speed of 300 mm / min. The elongation at break is (l-l0) / l0 x 100, where l0 is the sample length before the test and l is the length at break. The elongation at break T-0 was measured without prior heat treatment. Elongation at break T 130 The samples were placed in an oven (ESP Corporation, SPHH-201, incubator with safety door, safety oven) that had been kept stable at a set temperature of 130°C for at least 10 minutes in a laboratory environment of 23°C and 50% RH, then removed after 10 minutes and allowed to return to room temperature before being measured.

[0070] (8) FT-IR-ATR analysis: P1 / P2 The spectrum was measured using a laminate sampled to 30 mm x 30 mm, and the specified peaks P1 and P2 were detected using the peak detection mode of the analysis software. P1 / P2 was calculated from the obtained values ​​of P1 and P2.

[0071] P1 / P2 was calculated at three different positions, and the values ​​at the three points were averaged to determine P1 / P2 for that sample. Equipment: Fourier transform infrared spectrophotometer FT / IR-6100 (JASCO Corporation) Light source: High brightness ceramic light source Detector: TGS Beam splitter: Ge / KBr Measurement mode: ATR method (Ge prism, incident angle 45°) Measurement wave number range: 4,000 cm -1 ~600cm -1 ·Resolution: 4cm -1 Number of times: 32 Analysis: Peaks were detected using Spectra Manager Version 2 spectrum analysis program.

[0072] (9) Water vapor permeability According to JIS K7129 (2008) Method B, measurements were taken at a temperature of 40°C and a humidity of 90% RH using a water vapor transmission rate measuring device ("PERMATRAN" (registered trademark) W3 / 31) manufactured by MOCON / Modern Controls. Measurements were taken twice for two test pieces, and the average of the four measured values ​​was calculated to determine the water vapor transmission rate.

[0073] (10) Oxygen permeability According to the isobaric method of JIS K7126-2 (2006), the measurement was performed using an oxygen transmission rate measuring device ("OXTRAN" (registered trademark) 2 / 20) manufactured by MOCON / Modern Controls under conditions of temperature 23°C and humidity 90% RH. The measurement was performed twice for each of two test pieces, and the average of the four measured values ​​was calculated as the oxygen transmission rate.

[0074] [Example 1] (Formation of metal layer or inorganic compound layer) An aluminum oxide layer of 7 nm was formed as an inorganic compound layer on one side of a 12 μm-thick biaxially oriented polypropylene film (polypropylene film manufactured by Toray Industries, Inc., melting point 170°C, Sa 21 nm). The aluminum oxide layer was deposited by reactive deposition, in which aluminum is evaporated and then oxidized by introducing oxygen into the deposition area.

[0075] (Formation of coating layer) As a polyvinyl alcohol-based resin, modified polyvinyl alcohol (hereinafter sometimes abbreviated as modified PVA, ZF-15 long-chain alkyl modified, saponification degree 98.5 mol% or more manufactured by Nippon Vinyl Acetate & Poval Co., Ltd.) was added to a solvent of water / isopropyl alcohol = 97 / 3 by mass ratio, and heated and stirred at 90 ° C to obtain a water-soluble polymer solution with a solid content of 5 mass%. Next, a solution of 6.7 g of tetraethoxysilane (hereinafter sometimes abbreviated as TEOS) and 2.7 g of methanol was mixed, and 10.6 g of 0.02 N hydrochloric acid solution was added dropwise while stirring to obtain a TEOS hydrolyzed solution. The water-soluble polymer solution and the TEOS hydrolyzed solution were mixed so that the ratio of the PVA solid content of the water-soluble polymer solution to the SiO2 equivalent mass of TEOS was PVA solid content / SiO2 equivalent mass = 35 / 65. The mixture was diluted with water to a total solid content of 13 mass% to obtain a coating agent, which was applied on the above-mentioned aluminum oxide layer and dried at 100 ° C to obtain a laminate.

[0076] [Example 2] A laminate was obtained in the same manner as in Example 1, except that after the coating agent was applied and dried, it was heat-treated at 40°C for 3 days.

[0077] [Example 3] A laminate was obtained in the same manner as in Example 2, except that the modified polyvinyl alcohol of the coating layer was a special modified polyvinyl alcohol resin "Exceval" (registered trademark) RS-1717 manufactured by Kuraray Co., Ltd. (PVA modified with γ-butyrolactone having a carbonyl group in the ring structure, saponification degree 92.0 to 94.0 mol%).

[0078] [Example 4] A laminate was obtained in the same manner as in Example 2, except that the modified polyvinyl alcohol of the coating layer was a special modified polyvinyl alcohol resin "EXCEVAL" (registered trademark) HR-3010 manufactured by Kuraray Co., Ltd. (PVA modified with γ-butyrolactone having a carbonyl group in the ring structure, saponification degree 99.0 to 99.4 mol%).

[0079] [Example 5] A laminate was obtained in the same manner as in Example 2, except that the modified polyvinyl alcohol for the coating layer was DF-20 (carbonyl group modified, saponification degree 98.0 to 99.0 mol%) manufactured by Japan Vinyl Acetate & Poval Co., Ltd.

[0080] [Example 6] A laminate was obtained in the same manner as in Example 2, except that the modified polyvinyl alcohol for the coating layer was "GOSENEX" (registered trademark) Z-300 (acetoacetyl group modified, saponification degree 98.0 to 99.0 mol%) manufactured by Mitsubishi Chemical Corporation.

[0081] [Example 7] A laminate was obtained in the same manner as in Example 2, except that the heat treatment after coating and drying was carried out at 60°C for 3 days.

[0082] [Example 8] A laminate was obtained in the same manner as in Example 2, except that an aluminum layer having a thickness of 50 nm was formed as a metal layer by vacuum deposition on one side of a biaxially oriented polypropylene film.

[0083] [Examples 9 and 10] Laminates were obtained in the same manner as in Example 4, except that the coating thickness of the coating layer was changed.

[0084] [Examples 11 and 12] Laminates were obtained in the same manner as in Example 2, except that in the coating formulation for the covering layer, the ratio of the modified PVA solid content to the TEOS hydrolyzed solution in terms of SiO2 mass was changed.

[0085] [Examples 13 and 14] Laminates were obtained in the same manner as in Example 2, except that the drying temperature for the coating layer was changed.

[0086] [Example 15] A laminate was obtained in the same manner as in Example 2, except that the tetraethoxysilane hydrolyzed liquid used in preparing the coating agent for the coating agent was changed to a mixed liquid with ethyl silicate hydrolyzed liquid. The coating agent used was prepared in the following manner. As a polyvinyl alcohol-based resin, modified polyvinyl alcohol (long-chain alkyl modified, saponification degree 98.5 mol% or more) was added to a solvent of water / isopropyl alcohol = 97 / 3 by mass ratio, and heated and stirred at 90 ° C to obtain a water-soluble polymer solution with a solid content of 5 mass%. Next, 10.6 g of 0.02N hydrochloric acid solution was added dropwise to a solution mixed with 6.7 g of tetraethoxysilane and 2.7 g of methanol, and stirred to obtain a TEOS hydrolyzed solution. Furthermore, 7.0 g of 0.06N hydrochloric acid solution was added dropwise to a solution of 11.2 g of Ethyl Silicate 40 (ethyl silicate oligomer with an average of 5-mer) manufactured by Colcoat Co., Ltd. and 16.9 g of methanol to obtain an ethyl silicate hydrolyzed liquid. Tetraethoxysilane hydrolyzed liquid and ethyl silicate hydrolyzed liquid were mixed so that the SiO2 equivalent mass ratio of TEOS hydrolyzed liquid / ethyl silicate hydrolyzed liquid was 40 / 60 to obtain a hydrolyzed mixed liquid. Finally, the water-soluble polymer liquid and the hydrolyzed liquid were mixed so that the SiO2 equivalent mass ratio of the PVA solid content and the hydrolyzed mixed liquid was PVA solid content / SiO2 equivalent mass = 35 / 65 to obtain a coating agent.

[0087] [Example 16] A laminate was obtained in the same manner as in Example 2, except that the biaxially oriented polypropylene film was changed to a biaxially oriented polypropylene film having a melting point of 168°C and Sa of 14 nm.

[0088] [Example 17] A laminate was obtained in the same manner as in Example 2, except that an undercoat layer was formed on one side of a biaxially oriented polypropylene film, and then an inorganic compound layer was formed. The undercoat layer was formed by the following procedure. To 100 parts by mass of "Hydran" (registered trademark) AP-201 (manufactured by DIC Corporation, solid content concentration 23% by mass), which is a polyester urethane-based water-dispersible resin, 6 parts by mass of a melamine compound "Amidea" (registered trademark) APM (manufactured by DIC Corporation) was added as a crosslinking agent, and 1 part by mass of "Catalyst" PTS (manufactured by DIC Corporation), which is a water-soluble acidic compound, was added as a crosslinking catalyst. Pure water was then added, and the total solid content concentration was adjusted to 10% by mass, to obtain a mixed coating agent. This mixed coating liquid was applied to one side of a biaxially oriented polypropylene film, and dried at 100°C to form an undercoat layer with a thickness of 700 nm.

[0089] Comparative Example 1 A laminate was obtained in the same manner as in Example 1, except that the metal layer or inorganic compound layer was not formed.

[0090] Comparative Example 2 A laminate was obtained in the same manner as in Example 1, except that the polyvinyl alcohol resin was unmodified polyvinyl alcohol "Kuraray Poval" (registered trademark) 28-98 (saponification degree 98.0 to 99.0 mol%) manufactured by Kuraray Co., Ltd.

[0091] Comparative Example 3 A laminate was obtained in the same manner as in Example 2, except that the polyvinyl alcohol resin was unmodified polyvinyl alcohol "Kuraray Poval" (registered trademark) 28-98 (saponification degree 98.0 to 99.0 mol%) manufactured by Kuraray Co., Ltd.

[0092] Comparative Examples 4 and 5 Laminates were obtained in the same manner as in Comparative Example 3, except that the heat treatment conditions after coating and drying were changed.

[0093] Comparative Example 6 A laminate was obtained in the same manner as in Comparative Example 2, except that the coating drying temperature during coating layer formation was 160°C.

[0094] [Table 1]

[0095] [Table 2]

[0096] [Table 3] [Explanation of symbols]

[0097] 1 Resin film 2 Metal layer and / or inorganic oxide layer 3 Covering layer

Claims

1. A laminate having a metal layer and / or an inorganic compound layer, and a coating layer in this order on at least one surface of a resin film, The resin film is a polyolefin-based resin film, the coating layer contains a polyvinyl alcohol-based resin and a siloxane compound, A laminate in which the area ratio A1 / (A1+A2) of the random network structure to the sum of the area A1 of the Raman band indicating a random network structure derived from a siloxane compound, obtained by measuring the coating layer by laser Raman spectroscopy, and the peak intensity A2 of the Raman band indicating a linear polysiloxane structure and a cyclic siloxane, is 0.50 or more and 0.85 or less.

2. The stress at 121° C. in the direction of the main orientation axis measured by thermomechanical analysis (TMA) is represented as SF 121℃ , the stress at 145° C. in the main orientation axis direction is SF 145℃ When this is done, SF 145℃ - Sci-Fi 121℃ 2. The laminate of claim 1, wherein the modulus is ≦2.50 MPa.

3. 3. The laminate according to claim 1, wherein tan δ at 145° C. in the main orientation axis direction is 0.25 or less.

4. The elongation at break in the main orientation direction is T 0 The laminate was heat-treated at 130° C. for 10 minutes, and the elongation at break in the main orientation direction was measured as T 130 Then, T 0 / T 130 3. The laminate according to claim 1, wherein the value of is 1.20 or less.

5. The laminate according to claim 1 or 2, wherein the ratio P1 / P2 of the following peak intensities P1 and P2 detected by measuring the coating layer by an FT-IR-ATR method (total reflection Fourier transform infrared spectroscopy) is 3.5 or more and 8.0 or less. P1: 1,050-1,080cm -1 Intensity of the largest peak present in P2: 920-970cm -1 Intensity of the largest peak present in

6. 3. The laminate according to claim 1, wherein the polyvinyl alcohol-based resin has one or more functional groups selected from a vinyl ester group, an alkyl group, a carbonyl group, a carboxy group, an acetoacetyl group, a vinyl ether group, an alkyl group, an ethylene group, and a lactone ring.

7. 3. The laminate according to claim 1, wherein the coating layer has a thickness of 200 nm or more and 600 nm or less.

8. 3. The laminate according to claim 1, wherein the metal layer or the inorganic compound layer contains aluminum.

9. The laminate has a water vapor permeability of 1.0 g / m 2 / 24hr or less, and oxygen permeability is 1.0cc / m 2 3. The laminate according to claim 1, wherein the heat resistance is 24 hr or less.

10. 3. The laminate according to claim 1, wherein the metal layer or the inorganic compound layer is in direct contact with the resin film.

11. A packaging material comprising the laminate according to claim 1 or 2.

12. At least one surface of the resin film is A method for producing a laminate having a metal layer and / or an inorganic compound layer, and a coating layer in this order, comprising the steps of: the resin film is a polyolefin-based resin, and the coating layer is obtained by applying a liquid containing a polyvinyl alcohol-based resin and a siloxane compound and drying the liquid at 120° C. or less; A method for producing a laminate, in which the area ratio A1 / (A1+A2) of the random network structure to the total value of the area A1 of the Raman band indicating a random network structure derived from a siloxane compound, obtained by measuring a coating layer by laser Raman spectroscopy, and the peak intensity A2 of the Raman band indicating a linear polysiloxane structure and a cyclic siloxane, is 0.50 or more and 0.85 or less.

13. The method for producing a laminate according to claim 12, wherein the siloxane compound comprises at least one selected from the group consisting of alkoxysilanes and siloxane compounds having pentamer or less of alkoxysilanes.

Citation Information

Patent Citations

  • JP1974072951A

  • High-adhesion vapor-deposited film with antistatic properties

    JP4784039B2