Rubber composition for grip and golf club grip
The use of thiuram and sulfenamide vulcanization accelerators in a hydrogenated carboxy-modified acrylonitrile-butadiene rubber composition addresses slow vulcanization rates, enabling high-temperature processing with enhanced mechanical strength and productivity.
Patent Information
- Application Number
- JP2023072362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
Hydrogenated carboxy-modified acrylonitrile-butadiene rubber exhibits slow vulcanization rates due to low unsaturated bonds, which hinders crosslinking and reduces mechanical strength when high temperatures are used for vulcanization, leading to poor rubber productivity and mechanical properties.
A rubber composition containing hydrogenated carboxy-modified acrylonitrile-butadiene rubber with specific amounts of thiuram and sulfenamide vulcanization accelerators, allowing for high-temperature vulcanization without compromising mechanical strength.
The composition enables rapid vulcanization at high temperatures, resulting in crosslinked rubber with excellent mechanical strength and improved productivity.
Smart Images

Figure 2024157785000003 
Figure 2024157785000004 
Figure 2024157785000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for a grip used in the manufacture of a grip. [Background technology]
[0002] Rubber grips are often used as grips (anti-slip members) attached to sporting goods, etc. It has been proposed to use hydrogenated carboxy-modified acrylonitrile-butadiene rubber as the base rubber for such grips.
[0003] For example, Patent Document 1 describes a grip for sporting goods, characterized in that the outermost layer is formed from a surface layer rubber composition containing (A) a base rubber and (B) a resin having a softening point of 5°C to 120°C, the (A) base rubber containing an acrylonitrile-butadiene rubber, and the (B) resin being at least one selected from the group consisting of hydrogenated rosin ester, disproportionated rosin ester, ethylene-vinyl acetate copolymer, coumarone resin, phenolic resin, xylene resin, and styrene resin (see Patent Document 1 (Claim 1, paragraphs 0013 and 0019)). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-113388 A Summary of the Invention [Problem to be solved by the invention]
[0005] Hydrogenated carboxy-modified acrylonitrile-butadiene rubber has low unsaturated bond content, which gives it excellent weather resistance and ozone resistance, but on the other hand, it has problems such as slow vulcanization speed and poor productivity of crosslinked rubber due to the low unsaturated bond content. In addition, when using hydrogenated carboxy-modified acrylonitrile-butadiene rubber for grips, resins are added to improve the friction coefficient of the crosslinked rubber, but these resins also slow down the vulcanization speed. A common method for accelerating the vulcanization rate of a rubber composition is to increase the vulcanization temperature, but vulcanization at high temperatures tends to reduce the mechanical strength of the resulting crosslinked rubber.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a rubber composition containing a hydrogenated carboxyl-modified acrylonitrile-butadiene rubber as a base rubber, which is capable of giving a crosslinked rubber having excellent mechanical strength even when vulcanized at high temperatures. [Means for solving the problem]
[0007] The rubber composition for grips of the present invention, which is able to solve the above-mentioned problems, contains a base rubber, a vulcanizing agent, and a vulcanization accelerator, wherein the base rubber contains hydrogenated carboxy-modified acrylonitrile-butadiene rubber, the vulcanization accelerator contains a thiuram-based vulcanization accelerator and a sulfenamide-based vulcanization accelerator, the content of the thiuram-based vulcanization accelerator is 4 parts by mass or more per 100 parts by mass of the base rubber, and the content of the sulfenamide-based vulcanization accelerator is 0.3 parts by mass or more per 100 parts by mass of the base rubber. Effect of the Invention
[0008] The rubber composition for grips of the present invention has excellent mechanical strength even when vulcanized at high temperatures. Therefore, the vulcanization temperature during grip molding can be set high and the vulcanization time can be shortened, improving the productivity of grips. [Brief description of the drawings]
[0009] [Figure 1] 1 is a perspective view showing an example of a golf club grip of the present invention. [Diagram 2] 1 is a perspective view showing an example of a golf club equipped with a golf club grip of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Rubber composition] The rubber composition for a grip of the present invention (hereinafter sometimes simply referred to as "rubber composition") is used for molding a grip. The rubber composition contains a base rubber, a vulcanizing agent, and a vulcanization accelerator, the base rubber contains hydrogenated carboxy-modified acrylonitrile-butadiene rubber, the vulcanization accelerator contains a thiuram-based vulcanization accelerator and a sulfenamide-based vulcanization accelerator, the content of the thiuram-based vulcanization accelerator is 4 parts by mass or more per 100 parts by mass of the base rubber, and the content of the sulfenamide-based vulcanization accelerator is 0.3 parts by mass or more per 100 parts by mass of the base rubber.
[0011] In a rubber composition containing hydrogenated carboxy-modified acrylonitrile-butadiene rubber as a base rubber, by blending a predetermined amount of a thiuram-based vulcanization accelerator and a sulfenamide-based vulcanization accelerator as a vulcanization accelerator, it is possible to obtain a crosslinked rubber having excellent mechanical strength even when vulcanized at high temperatures.
[0012] The reason why the mechanical strength of the crosslinked rubber obtained even at high temperature vulcanization does not decrease is not necessarily clear, but it is considered as follows. When vulcanization temperature is increased in vulcanization of hydrogenated carboxy-modified acrylonitrile-butadiene rubber with a small amount of unsaturated bonds, intramolecular crosslinking and the formation of so-called pendants, in which the crosslinking precursor of the vulcanization accelerator remains hanging from the rubber chain and does not become a crosslinking point, increase. It is therefore considered that the crosslink density decreases and the strength of the crosslinked rubber decreases. In the rubber composition for grips of the present invention, a predetermined amount of a basic thiuram-based vulcanization accelerator and an acidic sulfenamide-based vulcanization accelerator are blended, and these vulcanization accelerators are activated by each other, and the vulcanization speed is increased. As a result, it is possible to reduce intramolecular crosslinking and pendant formation, which cause a decrease in crosslink density and strength, even under high temperature vulcanization, and it is considered that the decrease in mechanical strength due to the decrease in crosslink density can be prevented.
[0013] (Base rubber) The rubber composition contains a base rubber, and the content of the base rubber in the rubber composition is preferably 50% by mass or more, and more preferably 55% by mass or more.
[0014] The base rubber contains hydrogenated carboxy-modified acrylonitrile-butadiene rubber (hereinafter, sometimes referred to as "HXNBR"). The HXNBR is a hydrogenated copolymer of a monomer having a carboxy group, acrylonitrile, and butadiene. The HXNBR may be used alone or in combination of two or more types.
[0015] The acrylonitrile content of the HXNBR is preferably 15% by mass or more, more preferably 18% by mass or more, and even more preferably 21% by mass or more, and is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. If the acrylonitrile content is 15% by mass or more, the wear resistance of the grip is good, and if it is 50% by mass or less, the tactile feel of the grip in cold regions or in winter is good.
[0016] In the HXNBR, examples of the monomer having a carboxy group include acrylic acid, methacrylic acid, fumaric acid, and maleic acid. In the HXNBR, the content of the monomer containing a carboxy group is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and even more preferably 3.5% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. If the content of the monomer containing a carboxy group is 1.0% by mass or more, the wear resistance of the grip is improved, and if it is 30% by mass or less, the tactile feel of the grip in cold regions and winter is improved.
[0017] In the HXNBR, the carboxyl group content is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and even more preferably 3.5% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. If the carboxyl group content is 1.0% by mass or more, the wear resistance of the grip becomes better, and if it is 30% by mass or less, the tactile feel of the grip in cold regions or in winter becomes good.
[0018] The double bond content of the HXNBR is preferably 0.09 mmol / g or more, more preferably 0.2 mmol / g or more, and is preferably 2.5 mmol / g or less, more preferably 2.0 mmol / g or less, and even more preferably 1.5 mmol / g or less. If the double bond content is 0.09 mmol / g or more, vulcanization during molding is facilitated and the tensile strength of the grip is improved, and if it is 2.5 mmol / g or less, the durability (weather resistance) and tensile strength of the grip are improved. The double bond content can be adjusted by the butadiene content in the copolymer and the amount of hydrogen added to the copolymer.
[0019] The content of HXNBR in the base rubber is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. It is also preferable that the rubber composition contains only HXNBR as the base rubber. The higher the content of HXNBR in the base rubber, the better the abrasion resistance, durability (weather resistance) and tensile strength of the obtained grip.
[0020] The base rubber may contain other rubber components than HXNBR to the extent that the effect of the present invention is not impaired. Examples of the other rubber components include natural rubber (NR), ethylene-propylene-diene rubber (EPDM), butyl rubber (IIR), acrylonitrile-butadiene rubber (NBR), hydrogenated acrylonitrile-butadiene rubber (HNBR), carboxy-modified acrylonitrile-butadiene rubber (XNBR), butadiene rubber (BR), styrene-butadiene rubber (SBR), polyurethane rubber (PU), isoprene rubber (IR), chloroprene rubber (CR), and ethylene-propylene rubber (EPM). These base rubbers may be used alone or in combination of two or more.
[0021] (Vulcanizing agent) The vulcanizing agent may be a sulfur-based vulcanizing agent or an organic peroxide. The vulcanizing agents may be used alone or in combination of two or more kinds. The sulfur-based vulcanizing agent includes elemental sulfur and sulfur donor type compounds. The elemental sulfur includes powdered sulfur, precipitated sulfur, colloidal sulfur, and insoluble sulfur. The sulfur donor type compound includes 4,4'-dithiobismorpholine, etc. Examples of the organic peroxide include dicumyl peroxide, α,α'-bis(t-butylperoxy-m-diisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, etc. As the vulcanizing agent, a sulfur-based vulcanizing agent is preferable, and elemental sulfur is more preferable.
[0022] The content of the vulcanizing agent is preferably 0.2 parts by mass or more, more preferably 0.4 parts by mass or more, and even more preferably 0.6 parts by mass or more, and is preferably 4.0 parts by mass or less, more preferably 3.5 parts by mass or less, and even more preferably 3.0 parts by mass or less, per 100 parts by mass of the base rubber. If the content of the vulcanizing agent is 0.2 parts by mass or more, vulcanization will proceed more easily, and if it is 4.0 parts by mass or less, the occurrence of scorch can be reduced.
[0023] (Vulcanization accelerator) The rubber composition contains a thiuram vulcanization accelerator and a sulfenamide vulcanization accelerator as vulcanization accelerators. By containing the thiuram vulcanization accelerator and the sulfenamide vulcanization accelerator, it is possible to obtain a crosslinked rubber having excellent mechanical strength even when vulcanized at high temperatures.
[0024] Thiuram vulcanization accelerator Examples of the thiuram vulcanization accelerator include tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), tetramethylthiuram monosulfide (TMTM), dipentamethylenethiuram tetrasulfide, tetrakis(2-ethylhexyl)thiuram disulfide, etc. The thiuram vulcanization accelerator may be used alone, but from the viewpoint of preventing blooming, it is preferable to use two or more kinds in combination.
[0025] The amount of the thiuram vulcanization accelerator per 100 parts by mass of the base rubber is preferably at least 4 parts by mass, more preferably at least 5 parts by mass, and even more preferably at least 6 parts by mass, and is preferably at most 9 parts by mass, more preferably at most 8 parts by mass, and even more preferably at most 7 parts by mass. If the amount of the thiuram vulcanization accelerator is within the above range, even in a base rubber having a small amount of double bonds, even higher speed vulcanization can be achieved while maintaining scorch resistance.
[0026] Sulfenamide vulcanization accelerator Examples of the sulfenamide vulcanization accelerator include N-cyclohexyl-2-benzothiazolylsulfenamide (CBS), N-(tert-butyl)-2-benzothiazolylsulfenamide (BBS), etc. The sulfenamide vulcanization accelerator may be used alone or in combination of two or more kinds.
[0027] The amount of the sulfenamide vulcanization accelerator is preferably at least 0.3 parts by mass, more preferably at least 0.5 parts by mass, and even more preferably at least 0.7 parts by mass, and is preferably at most 2.5 parts by mass, more preferably at most 2.0 parts by mass, and even more preferably at most 1.5 parts by mass, per 100 parts by mass of the base rubber. If the amount of the sulfenamide vulcanization accelerator is within the above range, the occurrence of blooming can be further reduced.
[0028] The total content of the thiuram vulcanization accelerator and the sulfenamide vulcanization accelerator in the rubber composition is preferably 4.5 parts by mass or more, more preferably 5.5 parts by mass or more, even more preferably 6.5 parts by mass or more, and is preferably 11.5 parts by mass or less, more preferably 10.0 parts by mass or less, and even more preferably 8.5 parts by mass or less, per 100 parts by mass of the base rubber. If the total content is 4.5 parts by mass or more, the vulcanization rate can be increased even in a base rubber having a small amount of double bonds, and if it is 11.5 parts by mass or less, the scorch resistance of rubber having a small amount of double bonds is improved.
[0029] The mass ratio of the thiuram vulcanization accelerator to the sulfenamide vulcanization accelerator in the rubber composition (thiuram vulcanization accelerator / sulfenamide vulcanization accelerator) is preferably 1.5 or more, more preferably 3.0 or more, even more preferably 4.5 or more, and is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less. When the mass ratio (thiuram vulcanization accelerator / sulfenamide vulcanization accelerator) is 1.5 or more, the vulcanization rate can be increased even for a base rubber with a small amount of double bonds, and when it is 30 or less, a decrease in the strength of the crosslinked rubber obtained during vulcanization at high temperature and high speed can be further suppressed.
[0030] Thiourea vulcanization accelerator The rubber composition preferably further contains a thiourea vulcanization accelerator as a vulcanization accelerator. By containing the thiourea vulcanization accelerator, the thiuram vulcanization accelerator can be activated, and the vulcanization time can be further shortened. Examples of the thiourea-based vulcanization accelerator include trimethylthiourea, N,N'-diethylthiourea, etc. The thiourea-based vulcanization accelerators may be used alone or in combination of two or more kinds.
[0031] When the rubber composition contains a thiourea-based vulcanization accelerator, the mass ratio of the thiuram-based vulcanization accelerator to the thiourea-based vulcanization accelerator in the rubber composition (thiuram-based vulcanization accelerator / thiourea-based vulcanization accelerator) is preferably 4 or more, more preferably 6 or more, even more preferably 8 or more, and is preferably 20 or less, more preferably 18 or less, and even more preferably 16 or less. When the mass ratio (thiuram-based vulcanization accelerator / thiourea-based vulcanization accelerator) is 4 or more, the strength of the obtained crosslinked rubber is further improved, and when it is 20 or less, the activation of the thiuram-based accelerator by the thiourea-based accelerator is further improved.
[0032] The rubber composition may contain other vulcanization accelerators to the extent that the effect of the present invention is not impaired. Examples of other vulcanization accelerators include thiazole-based accelerators such as mercaptobenzothiazole (MBT) and benzothiazole disulfide, guanidine-based accelerators such as diphenylguanidine (DPG), and dithiocarbamate-based accelerators such as zinc dimethyldithiocarbamate (ZnPDC) and zinc dibutyldithiocarbamate.
[0033] The total content of the vulcanization accelerator in the base rubber is, per 100 parts by mass of the base rubber, preferably at least 4.3 parts by mass, more preferably at least 5.0 parts by mass, even more preferably at least 6.0 parts by mass, and is preferably at most 12 parts by mass, more preferably at most 11.5 parts by mass, even more preferably at most 10 parts by mass. If the total content of the vulcanization accelerator is within the above range, the occurrence of blooming and the like can be further suppressed.
[0034] (Vulcanization activator) The rubber composition may further contain a vulcanization activator. Examples of the vulcanization activator include metal oxides, metal peroxides, and fatty acids. Examples of the metal oxides include zinc oxide, magnesium oxide, and lead oxide. Examples of the metal peroxides include zinc peroxide, chromium peroxide, magnesium peroxide, and calcium peroxide. Examples of the fatty acids include stearic acid, oleic acid, and palmitic acid. These vulcanization activators may be used alone or in combination of two or more.
[0035] The total amount of the vulcanization activators used, per 100 parts by mass of the base rubber, is preferably at least 0.5 parts by mass, more preferably at least 0.6 parts by mass, and even more preferably at least 0.7 parts by mass, and is preferably at most 10.0 parts by mass, more preferably at most 9.5 parts by mass, and even more preferably at most 9.0 parts by mass.
[0036] (resin) The rubber composition may further contain a resin having a softening point of 120°C or less (hereinafter, may be simply referred to as "resin"). By containing a resin having a softening point of 120°C or less, the obtained crosslinked rubber becomes softer and the stress during deformation is reduced. Incidentally, when the resin is blended, the time required for vulcanization tends to be longer. However, the rubber composition of the present invention contains a predetermined amount of a thiuram vulcanization accelerator and a sulfenamide vulcanization accelerator as vulcanization accelerators, so that vulcanization in a short time is possible even when a resin is blended.
[0037] Examples of the resin include ethylene-vinyl acetate copolymer, rosin ester, coumarone resin, phenol resin, terpene resin, terpene phenol resin, and styrene-based resin.
[0038] The vinyl acetate content of the ethylene-vinyl acetate copolymer is preferably 10% by mass or more, more preferably 12% by mass or more, and even more preferably 15% by mass or more, and is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. If the vinyl acetate content is 10% by mass or more, the grip feeling becomes better, and if it is 80% by mass or less, the wear resistance of the grip is further improved.
[0039] The rosin ester is an ester compound obtained by reacting the rosin with alcohols. Rosin is a natural resin containing abietic acid, neoabietic acid, palustric acid, pimaric acid, isopimaric acid, and dehydroabietic acid. Examples of the alcohols include monohydric alcohols such as n-octyl alcohol, 2-ethylhexyl alcohol, decyl alcohol, lauryl alcohol, and stearyl alcohol; dihydric alcohols such as ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, and neopentyl glycol; trihydric alcohols such as glycerin and trimethylolpropane; tetrahydric alcohols such as pentaerythritol and diglycerin; and hexahydric alcohols such as dipentaerythritol and sorbitol. Among these, dihydric or higher polyhydric alcohols are preferred, and glycerin is more preferred.
[0040] The rosin ester includes hydrogenated rosin ester and disproportionated rosin ester. The hydrogenated rosin ester and disproportionated rosin ester are so-called stabilized rosin esters.
[0041] The hydrogenated rosin ester is an ester compound in which the portion of a rosin ester derived from rosin is hydrogenated. The hydrogenated rosin ester can be obtained by hydrogenating rosin and then reacting the hydrogenated rosin with an alcohol, or by reacting rosin with an alcohol and then hydrogenating the resulting rosin ester.
[0042] The disproportionated rosin ester is an ester compound in which the portion of the rosin ester derived from rosin has been disproportionated. The disproportionated rosin ester can be obtained by disproportionating rosin, and then reacting the disproportionated rosin with an alcohol, or by reacting rosin with an alcohol and then disproportionating the resulting rosin ester.
[0043] The coumarone resin is a resin containing coumarones as monomer components. The coumarone resin is preferably a coumarone-indene resin. The coumarone-indene resin is a copolymer containing coumarones and indenes as monomer components, and the total content of coumarones and indenes in the total monomer components is 50% by mass or more. Examples of the coumarones include coumarones and methylcoumarones. The content of coumarones in the total monomer components is preferably 1% by mass to 20% by mass. Examples of the indenes include indene and methylindene. The content of indenes in the total monomer components is preferably 40% by mass to 95% by mass. The coumaron-indene resin may contain other monomer components other than coumarones and indenes. Examples of the other monomer components include styrene, vinyltoluene, dicyclopentadiene, etc.
[0044] The phenolic resin may be, for example, a condensate of a phenol and formaldehyde. Examples of the phenol include phenol, m-cresol, etc. The phenolic resin may also include resol obtained by addition reaction of a phenol and formaldehyde with an alkali catalyst; novolac obtained by condensation reaction with an acid catalyst, etc. The phenolic resin may also include rosin phenolic resin obtained by adding a phenol to rosin with an acid catalyst and thermally polymerizing the mixture.
[0045] When the rubber composition contains a resin, the amount of the resin is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 30 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less, per 100 parts by mass of the base rubber. If the amount of the resin is 10 parts by mass or more, the feeling of the obtained grip becomes better, and if it is 50 parts by mass or less, the wear resistance of the grip is further improved.
[0046] (Processing aids) The rubber composition preferably contains a processing aid, such as an internal lubricant or an external lubricant. The internal lubricant may be a mineral oil or a plasticizer. The mineral oil may be paraffin oil, naphthenic oil, aromatic oil, etc. The plasticizer may be dioctyl phthalate, dibutyl phthalate, dioctyl sebacate, dioctyl adipate, etc. Examples of the external lubricant include phosphate compounds and long-chain alkylamine compounds. The rubber composition preferably contains a phosphate ester-based compound as an external lubricant. By containing a phosphate ester-based compound as an external lubricant, adhesion to the inside of a kneading device can be prevented even with a small amount of addition, and a homogeneous rubber composition can be obtained.
[0047] When the rubber composition contains an external lubricant, the content of the external lubricant is preferably at least 0.1 part by mass, more preferably at least 0.15 parts by mass, and even more preferably at least 0.25 parts by mass, and is preferably at most 1.0 part by mass, more preferably at most 0.75 parts by mass, and even more preferably at most 0.5 parts by mass, per 100 parts by mass of the base rubber. If the content of the external lubricant is within the above range, the effect as a lubricant is high, and the occurrence of blooming can be suppressed.
[0048] The rubber composition may further contain reinforcing agents, antioxidants, scorch inhibitors, colorants, etc., as required.
[0049] Examples of the reinforcing material include carbon black and silica. When the rubber composition contains a reinforcing material, the content of the reinforcing material is preferably 2.0 parts by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 4.0 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less, relative to 100 parts by mass of the base rubber. If the content of the reinforcing material is 2.0 parts by mass or more, the coloring of the rubber after vulcanization can be concealed, and if it is 50 parts by mass or less, the feeling of the obtained grip is good.
[0050] Examples of the antiaging agents include imidazoles, amines, phenols, and thioureas. Examples of the imidazoles include nickel dibutyldithiocarbamate (NDIBC), 2-mercaptobenzimidazole, and zinc salt of 2-mercaptobenzimidazole. Examples of the amines include phenyl-α-naphthylamine. Examples of the phenols include 2,2'-methylenebis(4-methyl-6-t-butylphenol) (MBMBP), and 2,6-di-tert-butyl-4-methylphenol. Examples of the thioureas include tributylthiourea and 1,3-bis(dimethylaminopropyl)-2-thiourea. These antiaging agents may be used alone or in combination of two or more.
[0051] When the rubber composition contains an antioxidant, the amount of the antioxidant per 100 parts by mass of the base rubber is preferably at least 0.2 parts by mass, more preferably at least 0.3 parts by mass, and even more preferably at least 0.4 parts by mass, and is preferably at most 5.0 parts by mass, more preferably at most 4.8 parts by mass, and even more preferably at most 4.6 parts by mass.
[0052] Examples of the scorch inhibitor include organic acids, nitroso compounds, etc. Examples of the organic acids include phthalic anhydride, pyromellitic anhydride, trimellitic anhydride, benzoic acid, salicylic acid, malic acid, etc. Examples of the nitroso compounds include N-nitroso diphenylamine, N-(cyclohexylthio)phthalimide, sulfonamide derivatives, diphenylurea, bis(tridecyl)pentaerythritol diphosphite, 2-mercaptobenzimidazole, etc.
[0053] The rubber composition may contain microballoons. By blending the microballoons in the rubber composition, a grip with a porous structure can be obtained. As the microballoons, either organic microballoons or inorganic microballoons can be used. Examples of organic microballoons include hollow particles made of a thermoplastic resin, and resin capsules in which low-boiling point hydrocarbons are encapsulated in a shell of a thermoplastic resin.
[0054] The rubber composition can be prepared by a conventional method. For example, it can be prepared by kneading each raw material using a kneading machine such as a Banbury mixer, a kneader, or an open roll. When the rubber composition contains microballoons, it is preferable to knead the components other than the microballoons in advance, and then knead the kneaded mixture with the microballoons. The material temperature when kneading the kneaded mixture with the microballoons is preferably set to a temperature lower than the expansion start temperature of the microballoons.
[0055] (Vulcanization characteristics) The rubber composition has a 90% vulcanization time (t90) of 8 minutes or less in a vulcanization curve measured at a vulcanization temperature of 185°C, more preferably 7 minutes or less, even more preferably 6 minutes or less, and particularly preferably 5 minutes or less. If the 90% vulcanization time is 8 minutes or less, grips can be manufactured in the same cycle as base rubbers having many unsaturated bonds such as natural rubber, and productivity is increased. The lower limit of the 90% vulcanization time is not particularly limited, but is usually 3 minutes.
[0056] The rubber composition has a 5% vulcanization time (t5) of 0.5 min or more in a vulcanization curve measured at a vulcanization temperature of 185° C., more preferably 0.7 min or more, and even more preferably 0.9 min or more. If the 5% vulcanization time is 0.5 min or more, scorching during charging of the rubber composition into a mold is more suppressed. The upper limit of the 5% vulcanization time is not particularly limited, but is usually 2 min.
[0057] The rubber composition has a maximum torque (MH) in a vulcanization curve measured at a vulcanization temperature of 185° C. of preferably 0.76 N·m or more, more preferably 0.78 N·m or more, even more preferably 0.80 N·m or more, and preferably 2.0 N·m or less, more preferably 1.8 N·m or less, even more preferably 1.6 N·m or less. If the maximum torque (MH) is within the above range, a good grip feeling and strength can be obtained.
[0058] The 90% vulcanization time and the 5% vulcanization time were determined from a vulcanization curve measured at a vulcanization temperature of 185° C. Specifically, the minimum torque value in the vulcanization curve was defined as ML, the maximum torque value as MH, and the difference between them as ME. The times required for the torque to reach ML+90%ME and ML+5%ME were defined as the 90% vulcanization time and the 5% vulcanization time, respectively.
[0059] (Crosslinked rubber) The rubber composition preferably has the physical properties described below when cured at a vulcanization temperature of 185° C. The vulcanization time for vulcanizing the rubber composition was set to 2 minutes added to the 90% vulcanization time (t90) in the vulcanization curve.
[0060] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. preferably has a tensile strength at break of 23 MPa or more, more preferably 24 MPa or more, and even more preferably 25 MPa or more. If the tensile strength at break is 23 MPa or more, the wear resistance of the grip is better. The upper limit of the tensile strength at break of the crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. is not particularly limited, but is usually 40 MPa.
[0061] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185°C has a density of 1.00 g / cm 3 It is preferable that the content is equal to or more than 1.02 g / cm. 3 More preferably, 1.04 g / cm 3 More than 1.3g / cm 3 Preferably less than 1.25 g / cm 3 More preferably, 1.2 g / cm 3 If the density is within the above range, the weight of the resulting grip will be approximately the same as that of a conventional grip, and the grip can be easily replaced with the conventional grip.
[0062] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. has a swelling ratio of preferably 200% or more, more preferably 210% or more, even more preferably 220% or more, and preferably 250% or less, more preferably 245% or less, and even more preferably 240% or less, when immersed in toluene at 40° C. for 24 hours. If the swelling ratio is 200% or more, the adhesiveness to the shaft is improved by absorbing the insertion liquid when the shaft is inserted into the grip, and if it is 250% or less, the crosslink density of the crosslinked rubber is better. The swelling ratio is measured by the measurement method described later.
[0063] The hardness (Shore A hardness) of the crosslinked rubber is preferably 30 or more, more preferably 40 or more, and even more preferably 45 or more, and is preferably 80 or less, more preferably 70 or less, and even more preferably 60 or less. If the hardness (Shore A hardness) of the crosslinked rubber is 30 or more, the mechanical strength of the grip is further improved, and if it is 80 or less, the grip does not become too hard, and the feeling when held is better.
[0064] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. had a loss tangent (tanδ) at 40° C., measured using a dynamic viscoelasticity device under the measurement conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode. 40) is preferably 0.154 or less, more preferably 0.153 or less, and further preferably 0.152 or less. 40 If the loss tangent (tan δ) is 0.154 or less, the crosslink density of the crosslinked rubber is better. 40 The lower limit of ) is not particularly limited, but is preferably 0.100 or more, and more preferably 0.120 or more.
[0065] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. had a storage modulus (E') at 40° C., measured using a dynamic viscoelasticity device under the measurement conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode. 40 The storage elastic modulus (E') is preferably 4.20 MPa or more, more preferably 4.22 MPa or more, and even more preferably 4.24 MPa or more, and is preferably 6.00 MPa or less, more preferably 5.50 MPa or less, and even more preferably 5.00 MPa or less. 40 If the elastic modulus is 4.20 MPa or more, the crosslinking progresses more smoothly, and if it is 6.00 MPa or less, the grip feeling obtained is better.
[0066] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. had a loss tangent (tanδ) at 25° C., measured using a dynamic viscoelasticity device under the measurement conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode. 25 ) is preferably 0.201 or more, more preferably 0.202 or more, and further preferably 0.203 or more. 25 If the loss tangent (tan δ) is 0.201 or more, the anti-slip performance of the obtained grip will be better. 25 The lower limit of ) is not particularly limited, but is preferably 0.300 or less, and more preferably 0.250 or less.
[0067] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. had a storage modulus at 25° C. (E′ 25The storage elastic modulus (E') is preferably 4.72 MPa or more, more preferably 4.73 MPa or more, and even more preferably 4.74 MPa or more, and is preferably 7.00 MPa or less, more preferably 6.50 MPa or less, and even more preferably 6.00 MPa or less. 25 If the crosslinking coefficient is 4.72 MPa or more, the crosslinking density of the crosslinked rubber will be better, and if the crosslinking coefficient is 7.00 MPa or less, the grip feeling obtained will be better.
[0068] The crosslinked rubber obtained by curing the rubber composition at a vulcanization temperature of 185° C. has a storage modulus (E' 40 ) (MPa) and the storage modulus at 25°C (E' 25 ) (MPa) and the ratio (E' 40 / E' 25 The ratio (E') is preferably 0.888 or more, more preferably 0.889 or more, even more preferably 0.890 or more, and particularly preferably 0.891 or more, and is preferably 0.900 or less, more preferably 0.898 or less, and even more preferably 0.896 or less. 40 / E' 25 When the value is 0.889 or more, the crosslink density of the crosslinked rubber becomes better, and when the value is 0.900 or less, the grip feeling obtained becomes better.
[0069] The rubber composition for grips of the present invention is used for molding grips. The rubber composition for grips has excellent abrasion resistance and tensile strength after curing, and therefore can be suitably used for golf club grips.
[0070] [Golf club grips] The golf club grip of the present invention has a cylindrical portion, at least a portion of which is formed from the rubber composition for grips, i.e., at least a portion of the cylindrical portion is made of a crosslinked rubber obtained by vulcanizing the rubber composition for grips.
[0071] The golf club grip has a cylindrical portion into which a shaft is inserted. The cylindrical portion may have a single-layer structure, a two-layer structure, a three-layer structure, or the like. When the cylindrical portion has a single-layer structure, the entire cylindrical portion is formed from the rubber composition. When the cylindrical portion has a multi-layer structure, at least one layer is formed from the rubber composition. When the cylindrical portion has a multi-layer structure, it is preferable that at least the outermost layer is formed from the rubber composition.
[0072] The cylindrical portion of the golf club grip is preferably a single-layer structure. Since the rubber composition for grips can be vulcanized at high temperatures, even thick members can be molded in a short time. Therefore, if a cylindrical portion of a single layer structure is manufactured using the rubber composition for grips, the structure is simple and the vulcanization time can be shortened, which further improves the productivity of the grip.
[0073] The cylindrical portion may have a solid structure or a porous structure. If the cylindrical portion has a solid structure, the mechanical strength of the grip is increased, and if the cylindrical portion has a porous structure, the weight of the grip can be reduced.
[0074] The golf club grip is obtained by molding the rubber composition in a mold. Examples of molding methods include press molding and injection molding. A golf club grip having an inner layer and an outer layer is obtained, for example, by press molding a laminate of an unvulcanized rubber sheet formed from the outer layer rubber composition and an unvulcanized rubber sheet formed from the inner layer rubber composition in a mold.
[0075] [Golf clubs] The present invention also includes a golf club using the golf club grip. The golf club includes a shaft, a head attached to one end of the shaft, and a grip attached to the other end of the shaft, the grip being the golf club grip. The shaft can be made of stainless steel or carbon fiber reinforced resin. Examples of the head include wood type, utility type, and iron type. The material constituting the head is not particularly limited, and examples thereof include titanium, titanium alloy, carbon fiber reinforced plastic, stainless steel, maraging steel, and soft iron.
[0076] Hereinafter, a golf club grip and a golf club will be described with reference to the drawings. FIG. 1 is a perspective view showing an example of a golf club grip. The grip 1 has a cylindrical portion 2 into which a shaft is inserted, and a cap portion 3 integrally formed so as to cover an opening at the rear end of the cylindrical portion. The cylindrical portion 2 has a single-layer structure. The cylindrical portion 2 is formed so that its thickness gradually increases from the front end toward the rear end. In the grip 1 shown in FIG. 1, the cap portion 3 is formed from the same rubber composition as the cylindrical portion 2.
[0077] 2 is a perspective view showing an example of a golf club equipped with the golf club grip of the present invention. The golf club 4 includes a shaft 5, a head 6 attached to one end of the shaft 5, and a grip 1 attached to the other end of the shaft 4. The rear end of the shaft 5 is fitted into the cylindrical portion 2 of the grip 1. EXAMPLES
[0078] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.
[0079] [Evaluation method] (1) Acrylonitrile content The acrylonitrile content was measured according to ISO 24698-1(2008) on the acrylonitrile-butadiene rubber before hydrogenation.
[0080] (2) Double bond content (mmol / g) The double bond content was calculated from the butadiene content (mass%) and the amount of remaining double bonds (%) in the copolymer. The amount of remaining double bonds is the mass ratio of the double bonds in the copolymer before hydrogenation to the double bonds in the copolymer after hydrogenation (amount of double bonds after hydrogenation / amount of double bonds before hydrogenation), and can be measured by infrared spectroscopy. When the acrylonitrile-butadiene rubber is an acrylonitrile-butadiene binary copolymer, the butadiene content in the copolymer can be calculated by subtracting the acrylonitrile content (mass%) from 100. Amount of double bonds = {butadiene content / 54} x amount of remaining double bonds x 10
[0081] (3) Content of monomers containing carboxyl groups 1 g of hydrogenated acrylonitrile-butadiene rubber was weighed out and dissolved in 50 mL of chloroform, to which thymol blue indicator was added dropwise. While stirring this solution, a 0.05 mol / L methanol solution of sodium hydroxide was added dropwise, and the amount of dripping (V mL) until the first color change was recorded. As a blank, 50 mL of chloroform containing no hydrogenated acrylonitrile-butadiene rubber was also dripped with a 0.05 mol / L methanol solution of sodium hydroxide using thymol blue as an indicator, and the amount of dripping (B mL) until the first color change was recorded. The carboxyl group content was calculated using the following formula. Carboxylic group-containing monomer content = {0.05 × (VB) × PM} / (10 × X) (In the formula, V is the amount of sodium hydroxide solution dropped as the test solution (mL), B is the amount of sodium hydroxide solution dropped as the blank (mL), PM is the molecular weight of the carboxyl group-containing monomer, and X is the valence of the carboxyl group-containing monomer.)
[0082] (4) Vulcanization test The rubber composition was subjected to a vulcanization test at the vulcanization temperature shown in Table 2 using a vulcanization tester (Curastometer (registered trademark) Type 7, manufactured by JSR Trading Co., Ltd.). According to "9. Die vulcanization test A" of "Method of determining vulcanization characteristics using a vibration vulcanization tester" of JIS K6300-2 (2001), a sine wave vibration of a low amplitude that does not break the rubber test piece was applied from the lower die, and the torque transmitted from the test piece to the upper die was measured from unvulcanized to overvulcanized. The measurement conditions were a torsional vibration frequency of 100 times per minute, an amplitude angle of 1°, and a measurement time of 30 minutes. From the obtained vulcanization curve, the minimum (ML) and maximum (MH) torque values, as well as the 5% vulcanization time (t5) and the 90% vulcanization time (t90) were obtained.
[0083] (5) Hardness (Shore A hardness) The rubber composition was vulcanized under the conditions shown in Table 2 to prepare a sheet having a thickness of 2 mm. The sheet was stored at 23°C for 2 weeks, and the hardness was measured using an automatic hardness tester (Digitest II, manufactured by H. Burleith Co.) in a state where three sheets were stacked so as not to be affected by the measurement substrate, etc. The detector used was "Shore A".
[0084] (6) Density (g / cm 3 ) The rubber composition was vulcanized under the conditions shown in Table 2 to prepare a sheet having a size of 13 cm square and a thickness of 2 mm. A test piece was prepared by punching out a 2 cm square from this sheet. The density of the obtained test piece was measured using an automatic specific gravity meter (MS Tech Co., Ltd., SP-GR1, Archimedes' principle).
[0085] (7) Swelling rate The rubber composition was vulcanized under the conditions shown in Table 2 to prepare a sheet having a thickness of 2 mm and a square of 13 cm. A test piece was prepared by punching out a square of 2 cm from the sheet. The swelling ratio of the obtained test piece was measured by immersing it in toluene at 40°C for 24 hours using an automatic specific gravity meter (MS Tech Co., Ltd., SP-GR1, Archimedes' principle). The swelling ratio is calculated by the following formula. Swelling ratio (%) = {(volume after swelling - volume before swelling) / volume before swelling} x 100
[0086] (8) Tensile strength at break (MPa) The tensile strength at break was measured in accordance with JIS K 6251 (2017). Specifically, the rubber composition was vulcanized under the conditions shown in Table 2 to prepare a sheet having a thickness of 1 mm, which was then punched into a dumbbell shape (dumbbell shape No. 3) to prepare a test specimen. The physical properties were measured using a tensile test measuring device (Shimadzu Corporation, Autograph AGS-D) (measurement temperature 23°C, tensile speed 500 mm / min). The tensile strength at break was calculated by dividing the tensile force recorded when the test specimen was broken by the cross-sectional area of the test specimen before the test.
[0087] (9) Viscoelasticity Loss tangent (tan δ) and storage modulus (E') were measured using a dynamic viscoelasticity measuring device (UBM Corporation). The measurements were performed using a Rheogel-E4000 manufactured by Epson. The test samples were prepared by slicing the grips in the thickness direction to a thickness of 2 mm and punching them to a specified size. The measurement conditions were: temperature; -100°C to 100°C, heating rate; 3°C / min, measurement interval; 3°C, frequency; 10Hz, strain amplitude; 10%, jig; tension, sample shape; width 4mm, thickness 2mm, length 40mm. Tan δ and E' at 25°C and 40°C were obtained from the viscoelasticity spectrum obtained by dynamic viscoelasticity measurement.
[0088] [Preparation of Rubber Composition] A rubber composition was prepared by kneading the raw materials according to the composition shown in Table 1. All the raw materials for the rubber composition were kneaded in an internal kneader.
[0089] [Table 1]
[0090] The materials used in Table 1 are as follows: HXNBR: Hydrogenated carboxy-modified acrylonitrile-butadiene rubber (ARANXEO, Therban XT VPKA 8889 (residual double bond amount 3.5%, acrylonitrile content 33.0% by mass, double bond content 0.40 mmol / g, carboxy group-containing monomer content 5.0% by mass) Sulfur: Tsurumi Chemical Industry Co., Ltd., 5% oil-filled fine sulfur (200 mesh) Suncerer (registered trademark) TBzTD: Tetrabenzyl thiuram disulfide, manufactured by Sanshin Chemical Industry Co., Ltd. Noccela (registered trademark) TOT-N: Tetrakis(2-ethylhexyl)thiuram disulfide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Noccela EUR: N,N'-diethylthiourea, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Suncerer NS: Sanshin Chemical Industry Co., Ltd., N-(tert-butyl)-2-benzothiazole sulfenamide Zinc peroxide: Struktol ZP 1014 (zinc peroxide content 29% by mass) manufactured by Struktol EVA: Ethylene-vinyl acetate copolymer (ARANXEO, Levapren 500 (vinyl acetate content 50% by mass, softening point 100±5°C, Mooney viscosity (ML 1+4 (100℃))27) SYLVATAC RE-5S: Made by Arizona Chemical, rosin ester (melting point below 25°C) Carbon black: SEAST (registered trademark) 3, manufactured by Tokai Carbon Co., Ltd. vanfre VAM: Polyoxyethylene-octadecyl ether-phosphate, manufactured by Vanderbilt Chemicals
[0091] [Grip Creation] The rubber composition was poured into a mold having a groove pattern on the cavity surface. The rubber was then vulcanized under the conditions shown in Table 2 to cause a crosslinking reaction, thereby obtaining a golf club grip. The grip was evaluated for viscoelastic properties, and the results are shown in Table 2.
[0092] [Table 2]
[0093] Rubber composition No. A contains a thiuram vulcanization accelerator and a thiourea vulcanization accelerator as vulcanization accelerators, but does not contain a sulfenamide vulcanization accelerator. When this rubber composition No. A is used, crosslinked rubbers No. 1 and 2 vulcanized at a vulcanization temperature of 165°C and a vulcanization temperature of 175°C have tensile strengths at break of 26 MPa or more, and are excellent in mechanical properties. However, the 90% vulcanization time at a vulcanization temperature of 165°C is 11 minutes, and the 90% vulcanization time at a vulcanization temperature of 175°C is 5.9 minutes, which is a long time for vulcanization. In addition, this rubber composition No. A has a 90% vulcanization time at a vulcanization temperature of 185°C of 3.5 minutes, and the vulcanization speed is fast. However, crosslinked rubber No. 3 vulcanized at a vulcanization temperature of 185°C from rubber composition No. A has a tensile strength at break of 21 MPa, and is inferior in mechanical properties.
[0094] Rubber compositions No. B to E contain a predetermined amount of a thiuram vulcanization accelerator and a sulfenamide vulcanization accelerator as vulcanization accelerators. These rubber compositions No. B to E have a 90% vulcanization time of 4.1 minutes or less at a vulcanization temperature of 185°C, and have a fast vulcanization speed. Furthermore, crosslinked rubbers No. 4 to 7 vulcanized at a vulcanization temperature of 185°C from these rubber compositions No. B to E had a tensile strength at break of 24 MPa or more and excellent mechanical properties. Among these, rubber compositions No. C to E, crosslinked rubbers No. 5 to 7 vulcanized at a vulcanization temperature of 185°C had a tensile strength at break of 25 MPa or more and were even more excellent in mechanical properties.
[0095] The present invention (1) is a rubber composition for a grip, comprising a base rubber, a vulcanizing agent, and a vulcanization accelerator, wherein the base rubber comprises hydrogenated carboxy-modified acrylonitrile-butadiene rubber, the vulcanization accelerator comprises a thiuram-based vulcanization accelerator and a sulfenamide-based vulcanization accelerator, the content of the thiuram-based vulcanization accelerator being 4 parts by mass or more per 100 parts by mass of the base rubber, and the content of the sulfenamide-based vulcanization accelerator being 0.3 parts by mass or more per 100 parts by mass of the base rubber.
[0096] The present invention (2) is a rubber composition for grips according to the present invention (1), wherein the crosslinked rubber obtained by curing the rubber composition for grips at a vulcanization temperature of 185°C has a tensile strength at break of 23 MPa or more.
[0097] The present invention (3) is a rubber composition for grips according to the present invention (1) or (2), in which the 90% vulcanization time (t90) in a vulcanization curve measured at a vulcanization temperature of 185°C is 8 minutes or less.
[0098] The present invention (4) is a rubber composition for grips according to any one of the present inventions (1) to (3), wherein a crosslinked rubber obtained by curing the rubber composition for grips at a vulcanization temperature of 185°C has a swelling rate of 200% to 250% when immersed in toluene at 40°C for 24 hours.
[0099] The present invention (5) is directed to a crosslinked rubber obtained by curing the rubber composition for grips at a vulcanization temperature of 185°C, and the storage modulus (E') at 40°C is measured using a dynamic viscoelasticity device under the measurement conditions of a vibration frequency of 10Hz, a strain amplitude of 0.05%, and a tensile mode. 40 ) and storage modulus at 25°C (E' 25 ) and the ratio (E' 40 / E' 25 ) is 0.888 to 0.900.
[0100] The present invention (6) is the rubber composition for a grip according to any one of the present inventions (1) to (5), wherein the rubber composition for a grip contains a resin having a softening point of 120° C. or lower.
[0101] The present invention (7) is a rubber composition for a grip according to any one of the present inventions (1) to (6), wherein the rubber composition for a grip contains a phosphate ester-based compound as an external lubricant.
[0102] The present invention (8) is the rubber composition for a grip according to any one of the present inventions (1) to (7), wherein the vulcanization accelerator contains a thiourea-based vulcanization accelerator.
[0103] The present invention (9) is a golf club grip having a cylindrical portion, at least a portion of which is formed from the rubber composition for a grip according to any one of the present inventions (1) to (8). [Explanation of symbols]
[0104] 1: Grip, 2: Cylinder, 3: Cap, 4: Golf club, 5: Shaft, 6: Head
Claims
1. Contains base rubber, vulcanizing agent and vulcanization accelerator, the base rubber contains a hydrogenated carboxy-modified acrylonitrile-butadiene rubber, The vulcanization accelerator contains a thiuram vulcanization accelerator and a sulfenamide vulcanization accelerator, the amount of the thiuram vulcanization accelerator is 4 parts by mass or more per 100 parts by mass of the base rubber, A rubber composition for a grip, wherein the content of the sulfenamide vulcanization accelerator is 0.3 parts by mass or more per 100 parts by mass of the base rubber.
2. 2. The rubber composition for grips according to claim 1, wherein the crosslinked rubber obtained by curing the rubber composition for grips at a vulcanization temperature of 185°C has a tensile strength at break of 23 MPa or more.
3. 2. The rubber composition for a grip according to claim 1, wherein the 90% vulcanization time (t90) in a vulcanization curve measured at a vulcanization temperature of 185° C. is 8 minutes or less.
4. The rubber composition for grips according to claim 1, wherein the crosslinked rubber obtained by curing the rubber composition for grips at a vulcanization temperature of 185°C has a swelling rate of 200% to 250% when immersed in toluene at 40°C for 24 hours.
5. The rubber composition for grips was cured at a vulcanization temperature of 185° C. to obtain a crosslinked rubber. The storage modulus at 40° C. (E′) was measured using a dynamic viscoelasticity device under the measurement conditions of a vibration frequency of 10 Hz, a strain amplitude of 0.05%, and a tensile mode. 40 ) (MPa) and storage modulus at 25° C. (E′ 25 ) (MPa) 40 / E' 25 2. The rubber composition for a grip according to claim 1, wherein the coefficient of friction coefficient is 0.888 to 0.
900.
6. 2. The rubber composition for a grip according to claim 1, which contains a resin having a softening point of 120° C. or lower.
7. 2. The rubber composition for a grip according to claim 1, further comprising a phosphoric acid ester compound as an external lubricant.
8. The rubber composition for a grip according to claim 1, wherein the vulcanization accelerator contains a thiourea-based vulcanization accelerator.
9. A golf club grip having a cylindrical portion, at least a portion of the cylindrical portion being formed from the rubber composition for grips according to any one of claims 1 to 8.
Citation Information
Patent Citations
Grip for sport gear and golf club
JP2017113388A