Heat-conductive silicone composition and method for producing heat-conductive silicone composition
The thermally conductive silicone composition addresses caking and viscosity issues by using a compatible base polymer and fillers, ensuring effective thermal conductivity and discharge performance.
Patent Information
- Application Number
- JP2023072886
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-27
AI Technical Summary
Existing thermally conductive silicone compositions face issues with caking during discharge, which affects adhesion and thermal conductivity, and require high filler content to maintain thermal conductivity, leading to increased viscosity and dischargeability problems.
A thermally conductive silicone composition using a highly compatible base polymer with adjusted viscosity, incorporating diorganopolysiloxanes and thermally conductive fillers, along with a coupling agent, to prevent caking and ensure high thermal conductivity and discharge performance.
The composition achieves good adhesion, high thermal conductivity, and flexibility while preventing caking, maintaining dischargeability and flexibility under pressure, with improved thermal dissipation properties.
Smart Images

Figure 2024158046000001 
Figure 2024158046000002 
Figure 2024158046000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a thermally conductive silicone composition and a method for making the thermally conductive silicone composition. [Background technology]
[0002] Thermally conductive silicone compositions, for example gap fillers, are applied directly to heat generating or heat dissipating bodies such as batteries for electric vehicles and semiconductors for electronic devices, and have the function of transferring heat generated from them to heat dissipating members such as heat sinks. In order to transfer heat efficiently at the interface formed by application, adhesion is required at the contact interface between the heat generating body and the gap filler. For example, gap filler for electronic devices is applied in small amounts with high precision and pinpoint accuracy onto a circuit board. In this case, it is required that the amount of application is consistent. One of the factors that causes variation in the amount of application is a phenomenon called caking. In this disclosure, caking refers to a phenomenon in which the filler and the polymer separate when the gap filler is discharged from a discharge device, and only the filler components aggregate within the flow path. It is important to prevent this caking from occurring in terms of both quality and productivity.
[0003] Generally, in order to obtain sufficient thermal conductivity, it is necessary to mix a high content of thermally conductive filler in the composition, but mixing a high content of filler increases the viscosity of the gap filler, which leads to deterioration of dischargeability. If a low-viscosity polymer is used to ensure dischargeability, the proportion of organic functional groups in the polymer increases, which deteriorates compatibility with the filler, raising concerns about the occurrence of caking during discharge. One method for suppressing caking is, for example, surface treatment of the filler with a coupling agent. However, even if the amount of the coupling agent is increased, it is difficult to completely treat the filler surface, and compatibility cannot be significantly improved. Furthermore, if a high viscosity polymer having a high molecular chain that is highly compatible with the filler is used, the viscosity of the gap filler increases, making it difficult to discharge.
[0004] Patent Document 1 discloses a method for preventing sedimentation and separation of a silicone composition, which involves blending a condensation reaction product of D-sorbitol and benzaldehyde to produce a silicone composition that prevents sedimentation and separation. However, the blending amount of the condensation reaction product relative to the filler is large, and there is a problem that high thermal conductivity cannot be maintained. Patent Document 1 also concerns the issue of long-term storage stability by suppressing separation of the polymer and filler. Patent Document 2 discloses a resin composition in which aluminum nitride powder can be uniformly dispersed in the resin without forming aggregates, and which has excellent thermal conductivity. The flowability is improved by mixing a flowability modifier. However, although Patent Document 2 improves the flowability, it does not disclose caking during long-term discharge under pressure. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 2946104 [Patent Document 2] Japanese Patent Application Publication No. 10-204300 Summary of the Invention [Problem to be solved by the invention]
[0006] The present disclosure provides a thermally conductive silicone composition that exhibits good adhesion and bonding properties to substrates such as heat generating bodies and heat dissipating bodies, has excellent heat dissipation properties due to its high thermal conductivity, and is resistant to caking due to discharge pressure while retaining its flexibility, as well as a method for producing the same. [Means for solving the problem]
[0007] The thermally conductive silicone composition of the present disclosure uses a highly compatible base polymer, introduces a separation-inhibiting polymer, adjusts viscosity with diorganopolysiloxane, and adds an appropriate amount of thermally conductive filler, thereby endowing the composition with high thermal conductivity, high dischargeability, and caking resistance against discharge pressure.
[0008] The thermally conductive silicone composition of the present disclosure comprises: (A) 1.0 part by mass or more and 9.0 parts by mass or less (based on 100 parts by mass of the total composition) of an alkenyl group-containing diorganopolysiloxane having a viscosity of 500 mPa s or more and 7,000 mPa s or less at 25°C, (B) 0.05 parts by mass or more and 1.0 parts by mass or less (based on 100 parts by mass of the total composition) of an organopolysiloxane having a viscosity of 10,000 mPa s or more and 200,000 mPa s or less at 25°C; (C) an organopolysiloxane having two or more hydrosilyl groups per molecule; (D) a diorganopolysiloxane having no alkenyl groups and having a viscosity of 500 mPa·S or less at 25°C; (E) an addition catalyst; (F) at least one or more thermally conductive fillers selected from metals, metal oxides, metal hydroxides, metal nitrides, and metal carbides; A thermally conductive silicone composition comprising: the thermally conductive silicone composition contains 85 parts by mass or more of the component (F) relative to 100 parts by mass of the entire composition, The thermally conductive silicone composition has a mixed viscosity of 250 Pa·s or less at 25° C. The thermally conductive silicone composition may further contain (G) a coupling agent. The thermally conductive silicone composition may further contain (H) a silanol group-containing polydimethylsiloxane.
[0009] The alkenyl-containing diorganopolysiloxane (A) may have a Vi (vinyl group) in the side chain, or may have at least one Vi (vinyl group) at each of its two terminals. The alkenyl-containing diorganopolysiloxane (A) is preferably a linear dimethylpolysiloxane having one Vi group at each of its two terminals, and has a viscosity at 25°C of 1,000 mPa s or more and 1,200 mPa s or less.
[0010] The (B) may be a non-functional dimethylpolysiloxane, and preferably has a viscosity at 25°C of 80,000 mPa·s or more and 120,000 mPa·s or less.
[0011] The above-mentioned (C) is preferably a dimethylpolysiloxane having 12 to 18 hydrogen atoms bonded to silicon atoms only in the side chains and having a viscosity at 25° C. of 150 mPa·s or more and 300 mPa·s or less.
[0012] The diorganopolysiloxane not having an alkenyl group of component (D) is a non-functional siloxane, which may have a trimethylsilyl group at its terminal. The component (D) is preferably a non-functional dimethylpolysiloxane having a viscosity at 25°C of 30 mPa s or more and 60 mPa s or less.
[0013] The addition catalyst (E) is preferably a platinum-divinyltetramethyldisiloxane complex.
[0014] The thermally conductive filler (F) is preferably zinc oxide, amorphous aluminum oxide, or spherical aluminum oxide.
[0015] The above-mentioned (H) is preferably a linear dimethylpolysiloxane having one silanol group at each end and a viscosity at 25° C. of 30 mPa·s or more and 60 mPa·s or less.
[0016] The thermally conductive silicone composition comprises: A two-part thermally conductive silicone composition comprising a first liquid and a second liquid packaged separately from each other, the first liquid and the second liquid being mixed (for example, under pressure in a discharge device) at the time of use to form a thermally conductive silicone composition, The first liquid may contain (A), (B), (D), (E) and (F); The second liquid may contain (B), (C), (D), and (F), but does not contain (E). The second liquid may further contain (A). The first liquid and / or the second liquid may further contain a coupling agent (G). The first liquid and / or the second liquid may further contain (H) a silanol group-containing polydimethylsiloxane.
[0017] When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of the component (A) is preferably 2.5 parts by mass or more and 3.0 parts by mass or less. When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of the component (B) is preferably 0.2 parts by mass or more and 0.4 parts by mass or less. When the total amount of the second liquid is taken as 100 parts by mass, the amount of the component (C) is preferably 0.3 part by mass or more and 0.5 part by mass or less. When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of the component (D) is preferably 4.5 parts by mass or more and 5.5 parts by mass or less. When the total amount of the first liquid is taken as 100 parts by mass, the amount of the component (E) is preferably 0.15 part by mass or more and 0.25 part by mass or less. When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of zinc oxide as the component (F) is preferably 4.0 parts by mass or more and 8.0 parts by mass or less. When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of amorphous aluminum oxide, which is the component (F), is preferably 20.0 parts by mass or more and 40.0 parts by mass or less. When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of spherical aluminum oxide, which is the component (F), is preferably 45.0 parts by mass or more and 65.0 parts by mass or less. When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of the component (G) is preferably 0.4 parts by mass or more and 0.5 parts by mass or less. When the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass, the amount of the component (H) is preferably 0.25 parts by mass or more and 0.35 parts by mass or less.
[0018] The thermally conductive silicone composition comprises: It is preferable that no aggregates are observed in any of the first liquid, the second liquid, and the thermally conductive silicone composition in the caking evaluation described below. (Caking evaluation) Using a dispenser (e.g., MPP-3 manufactured by Musashi Engineering), dispense 0.03 cc and wait for 0.20 seconds repeatedly to dispense 1.0 kg of material. After that, disassemble the dispenser and visually check for any agglomerates.
[0019] The method for producing the thermally conductive silicone composition of the present disclosure includes the steps of: a first liquid producing step of mixing (A) 1.0 part by mass or more and 9.0 parts by mass or less (based on 100 parts by mass of the total composition) of an alkenyl group-containing diorganopolysiloxane having a viscosity of 500 mPa·s or more and 7,000 mPa·s or less at 25°C, (B) 0.05 part by mass or more and 1.0 part by mass of an organopolysiloxane having a viscosity of 10,000 mPa·s or more and 200,000 mPa·s or less at 25°C, (D) an alkenyl group-free diorganopolysiloxane having a viscosity of 500 mPa·s or less at 25°C, and (E) an addition catalyst, and then mixing (F) at least one or two or more types of thermally conductive filler selected from metals, metal oxides, metal hydroxides, metal nitrides, and metal carbides to obtain a first liquid; a second liquid producing step of mixing (B) 0.05 part by mass or more and 1.0 part by mass or less of an organopolysiloxane having a viscosity of 10,000 mPa s or more and 200,000 mPa s or less at 25°C, (C) an organopolysiloxane having two or more hydrosilyl groups in one molecule, and (D) a diorganopolysiloxane having no alkenyl groups and having a viscosity of 500 mPa s or less at 25°C, and then mixing (F) at least one or two or more types of thermally conductive filler selected from metals, metal oxides, metal hydroxides, metal nitrides, and metal carbides to obtain a second liquid; Includes. In the second liquid preparation step, prior to adding component (F), 1.0 part by mass or more and 9.0 parts by mass or less of (A) an alkenyl group-containing diorganopolysiloxane having a viscosity of 500 mPa s or more and 7,000 mPa s or less at 25°C may be mixed with other components. In the first liquid preparation step and / or the second liquid preparation step, a coupling agent (G) may be mixed with other components before the component (F) is added. In the first liquid preparation step and / or the second liquid preparation step, (H) silanol group-containing polydimethylsiloxane may be mixed with other components before the addition of the component (F). The method for producing the thermally conductive silicone composition includes the steps of: a first liquid packaging step of filling the first liquid obtained in the first liquid production step into a predetermined first packaging material; a second liquid packaging step of filling the second liquid obtained in the second liquid production step into a predetermined second packaging material; may also include
[0020] The method for discharging the thermally conductive silicone composition of the present disclosure includes the steps of: The first liquid is introduced from the first packaging material into a first liquid flow path of the dispenser; The second liquid is introduced from the second packaging material into a second liquid flow path of the dispenser; The first liquid and the second liquid are introduced at a predetermined ratio into a joining flow path where the first liquid flow path and the second liquid flow path join together; The method may include a step of discharging a mixture of the first liquid and the second liquid that have been brought into contact with each other in the junction flow path from a nozzle of a dispenser onto a substrate. The "predetermined ratio" is the mixing ratio of the first liquid to the second liquid, and is set according to the specifications of the thermally conductive silicone composition.
[0021] A method for producing a thermally conductive member according to the present disclosure includes the steps of: discharging the first liquid from a first liquid storage section to a mixing section; discharging the second liquid from a second liquid storage section to the mixing section; mixing the first liquid and the second liquid in the mixing section to obtain a thermally conductive silicone composition; applying the thermally conductive silicone composition to a substrate by discharging; and curing the thermally conductive silicone composition applied to the substrate to obtain a thermally conductive member.
[0022] In the method for producing a thermally conductive member and the method for discharging a thermally conductive silicone composition, the discharge pressure at which the first liquid, the second liquid, and the thermally conductive silicone composition are discharged onto a substrate varies depending on the dispenser, but for example, the lower limit is 0.1 MPa, and preferably 0.2 MPa to 0.8 MPa.
[0023] The heat dissipation member of the present disclosure may have a substrate and a heat conductive member provided on the surface of the substrate, the heat conductive member being obtained by curing the heat conductive silicone composition described above.
[0024] The electric or electronic device of the present disclosure may include the heat dissipation member.
[0025] (Action and effect) (1) The thermally conductive gap filler composition has good adhesion and bonding properties to substrates such as heat sinks, and has excellent heat dissipation properties due to its high thermal conductivity. Furthermore, the composition is useful as a gap filler that suppresses caking while maintaining high dischargeability. (2) It is useful as a thermally conductive silicone composition that is less susceptible to clogging of flow paths even during long-term dispensing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The thermally conductive silicone composition, the method for producing the thermally conductive silicone composition, the method for producing a thermally conductive member, and the heat dissipating member according to the present invention will be described in detail below.
[0027] (Thermal conductive silicone composition) The thermally conductive silicone composition may be any composition that can be used to form a thermally conductive member. Examples of thermally conductive members include those that are cured and formed into heat-generating bodies such as car batteries, gap fillers and heat dissipation sheets that are applied to films that cover heat-generating bodies, base materials for electric or electronic devices, circuit chips, heat dissipation members, etc. The thermally conductive silicone composition may be applied to a substrate in a liquid state before curing and then cured to provide a thermally conductive member, or the cured thermally conductive member obtained may be applied to a substrate.
[0028] The temperature and procedure for curing the thermally conductive silicone composition are not limited and can be appropriately selected depending on the application of the resulting cured product. The present invention is characterized by being able to provide a thermally conductive silicone composition that exhibits sufficient performance, i.e., sufficient curability, adhesion to substrates under discharge pressure, and caking resistance, even when it can only be used in a room temperature environment, but when a high-temperature environment is acceptable, curing in such an environment is not prevented.
[0029] The curing method of the thermally conductive silicone composition is preferably an addition reaction type. The main reasons are that the curing can be controlled in various temperature ranges from room temperature to about 150°C, there is little volume change or gas release, and compatibility with the thermally conductive filler is generally good. Generally, the higher the curing temperature, the faster the curing, but the present invention assumes that due to various constraints depending on the application, the process of applying the thermally conductive silicone composition, the curing process, and further, some or all of the subsequent processes must be performed at room temperature, and an appropriate curing temperature can be set accordingly.
[0030] When the curing method of the thermally conductive silicone composition according to the present invention is an addition reaction type, each component of the thermally conductive silicone composition will be described in detail below.
[0031] (Component (A)) Component (A) is the main component of the thermally conductive silicone composition and is an alkenyl-containing diorganopolysiloxane. The alkenyl-containing diorganopolysiloxane preferably has a terminal Vi (vinyl group) in order to have an appropriate hardness after curing. The alkenyl-containing diorganopolysiloxane may have an OH group at the terminal. The viscosity and degree of polymerization of component (A) are not particularly limited and can be selected depending on the required mixed viscosity of the thermally conductive composition, etc. For example, the viscosity at 25°C may be 500 mPa s or more and 7,000 mPa s or less. The diorganopolysiloxane may be used alone or in appropriate combination of two or more. This is the main component of the thermally conductive composition and has at least 2, preferably 2 to 50, and more preferably 2 to 20 alkenyl groups bonded to silicon atoms on average in one molecule. When the entire thermally conductive silicone composition is taken as 100 parts by mass, the amount of component A is in the range of 1.0 part by mass to 9.0 parts by mass, and preferably 2 parts by mass to 4 parts by mass. Component A is preferably contained in both the first liquid and the second liquid.
[0032] The molecular structure of component (A) is not particularly limited, and may be, for example, a linear structure, a linear structure having some branching, a branched structure, a cyclic structure, or a cyclic structure having branching. Of these, component (A) is preferably a substantially linear organopolysiloxane, and specifically may be a linear diorganopolysiloxane whose molecular chain is mainly composed of repeating diorganosiloxane units and whose both molecular chain terminals are blocked with triorganosiloxy groups. Some or all of the molecular chain terminals, or some of the side chains, may be silanol groups.
[0033] The position of the alkenyl group bonded to the silicon atom in component (A) is not particularly limited, and component (A) may be a diorganopolysiloxane having an alkenyl group bonded to a silicon atom at both ends of the molecular chain. An organopolysiloxane having one alkenyl group at each end of the molecular chain has the advantage that it has a low content of alkenyl groups that serve as reaction sites for the crosslinking reaction, and the flexibility of the gap filler obtained after curing is increased.
[0034] The alkenyl group may be bonded to either a silicon atom at a molecular chain terminal or a silicon atom at a non-terminal position (in the middle of the molecular chain), or may be bonded to both. Furthermore, the component (A) may be a polymer made up of a single siloxane unit, or a copolymer made up of two or more types of siloxane units.
[0035] The viscosity of component (A) at 25°C is from 500 mPa·s to 7,000 mPa·s, preferably from 1,000 mPa·s to 5,000 mPa·s, more preferably from 1,000 mPa·s to 4,000 mPa·s, and even more preferably from 1,000 mPa·s to 2,000 mPa·s. When the viscosity is within the above range, the resulting thermally conductive composition has an appropriate fluidity, which makes it possible to improve the dischargeability and productivity, and also makes it possible to improve the flexibility of the thermally conductive member obtained by curing the thermally conductive composition.
[0036] In order to adjust the viscosity (mixed viscosity) before curing of the thermally conductive composition obtained by mixing the liquid compositions, two or more types of alkenyl-containing diorganopolysiloxanes having different viscosities can also be used.
[0037] Specifically, the average composition formula of the component (A) is represented by the following general formula (1). R 1 a SiO (4-a) / 2 (1) (In formula (1), R 1are the same or different, unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms. a is 1.7 to 2.1. Also, a is preferably 1.8 to 2.5, more preferably 1.95 to 2.05.
[0038] In one embodiment, the R 1 At least two of the monovalent hydrocarbon groups represented by the formula (I) are selected from alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, isobutenyl, hexenyl, and cyclohexenyl, and the remaining groups are substituted or unsubstituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, specifically alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, 2-ethylhexyl, heptyl, octyl, nonyl, decyl, and dodecyl, cyclohexyl, and the like. They are selected from cycloalkyl groups such as cyclopentyl, cyclohexyl and cycloheptyl; aryl groups such as phenyl, tolyl, xylyl, biphenyl and naphthyl; aralkyl groups such as benzyl, phenylethyl, phenylpropyl and methylbenzyl; and halogen-substituted or cyano-substituted alkyl groups in which some or all of the hydrogen atoms in these hydrocarbon groups have been replaced with halogen atoms, cyano groups or the like, such as chloromethyl, 2-bromoethyl, 3,3,3-trifluoropropyl, 3-chloropropyl and cyanoethyl.
[0039] R 1 In selecting R, the alkenyl groups required in the number of two or more are preferably vinyl, allyl, propenyl, isopropenyl, 2-methyl-1-propenyl, 2-methylallyl, and 2-butenyl, with vinyl being particularly preferred. As R other than the alkenyl group, methyl and phenyl groups are preferred, with methyl being particularly preferred. In addition, when the total number of R 1 It is preferable that 70 mol % or more of the copolymer contains methyl groups in terms of the physical properties of the cured product and economic efficiency, and generally, copolymers containing 80 mol % or more of methyl groups are used.
[0040] The molecular structure of component (A) may be dimethylpolysiloxane terminated at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylsiloxane-methylphenylsiloxane copolymer terminated at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymer terminated at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymer terminated at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymer terminated at both molecular chain terminals with trimethylsiloxy groups, or a compound represented by the formula: (CH 3 ) 2 ViSiO 1 / 2 Siloxane units represented by the formula: (CH 3 ) 3 SiO 1 / 2 Siloxane units represented by the formula: SiO 4 / 2 (wherein Vi represents a vinyl group); organopolysiloxanes in which some or all of the methyl groups of these organopolysiloxanes have been substituted with alkyl groups such as ethyl groups, propyl groups, etc.; aryl groups such as phenyl groups, tolyl groups, etc.; or halogenated alkyl groups such as 3,3,3-trifluoropropyl groups, etc.; and mixtures of two or more of these organopolysiloxanes. From the viewpoint of increasing the elongation until breakage of the cured product by increasing the molecular chain length, however, linear diorganopolysiloxanes having vinyl groups at both molecular chain terminals are preferred.
[0041] At least 1.0 part by mass but no more than 9.0 parts by mass of component (A) may be an alkenyl-containing diorganopolysiloxane that has at least one silanol group at a molecular chain terminal. When the thermally conductive silicone composition of the present invention is stored as a two-part type, the alkenyl-containing diorganopolysiloxane having silanol groups may be blended into the first part and / or the second part.
[0042] These diorganopolysiloxanes may be commercially available products, or may be produced by methods known to those skilled in the art.
[0043] ((B) component) Component (B) is an organopolysiloxane. The viscosity and degree of polymerization of component (B) are not particularly limited and can be selected according to the required mixed viscosity of the thermally conductive composition, etc. For example, the viscosity at 25°C may be 10,000 mPa s or more and 200,000 mPa s or less. Component (B) is an organopolysiloxane that acts as a separation inhibitor to inhibit separation of the polymer and filler under discharge pressure.
[0044] Component (B) may be any organohydrogenpolysiloxane, and may, for example, have the same structure as component (A), or may be a diorganopolysiloxane that does not contain vinyl groups.
[0045] The viscosity of component (B) at 25°C is from 10,000 mPa·s to 200,000 mPa·s, preferably from 10,000 mPa·s to 150,000 mPa·s, and more preferably from 15,000 mPa·s to 100,000 mPa·s.
[0046] ((C) component) Component (C) is an organopolysiloxane having two or more hydrosilyl groups in each molecule. Component (C) functions as a crosslinking agent. There are no particular limitations on the viscosity or degree of polymerization of component (C) and these can be selected according to the required mixed viscosity and other factors of the thermally conductive composition; for example, the viscosity at 25°C may be 10 mPa s or more and 10,000 mPa s or less. Component (C) may be a diorganopolysiloxane that contains three or more hydrosilyl groups bonded to silicon atoms in each molecule, and is a component that functions as a crosslinking agent to cure the thermally conductive silicone composition.
[0047] As long as the number of hydrosilyl groups bonded to a silicon atom is two or more, the bonding sites are not particularly limited. There are no particular limitations on the hydrogen content (H content) of component (C), but in order to impart practically sufficient elongation to the thermally conductive member obtained by curing the thermally conductive silicone composition, the hydrogen content (H content) of component (C) is preferably from 0.01 mmol / g to 4.0 mmol / g, more preferably from 0.3 mmol / g to 3.0 mmol / g, and even more preferably from 1.0 mmol / g to 2.0 mmol / g.
[0048] Organohydrogenpolysiloxane can be used as component (C). Component (C) forms a cured product by addition reaction with an alkenyl group and may have at least one hydrogen atom bonded to a silicon atom (hydrosilyl group) in a side chain in the molecule. The (C) component may function as a crosslinking agent. The crosslinking agent may preferably have 3 or more hydrosilyl groups in one molecule and at least one hydrosilyl group in a side chain in the molecule. The crosslinking agent is more preferably an organohydrogenpolysiloxane having 5 or more hydrosilyl groups, and may have 10 to 18 hydrosilyl groups. The organohydrogenpolysiloxane as the crosslinking agent has at least two hydrosilyl groups in its side chain. The number of hydrosilyl groups at the molecular chain terminal may be 0 to 2, but it is economically preferable that the number is 2. The molecular structure of the organohydrogenpolysiloxane may be any of linear, cyclic, branched, and three-dimensional network structures. There is no particular restriction on the position of the silicon atom to which the hydrogen atom is bonded, and it may be the terminal or non-terminal of the molecular chain, or the side chain. There are no particular limitations on other conditions, organic groups other than the hydrosilyl groups, bonding positions, degree of polymerization, structure, etc., and two or more types of organohydrogenpolysiloxanes may be used.
[0049] The content of component (C) in the silicone composition is preferably in a range such that the ratio of the number of hydrosilyl groups in component (C) to the number of alkenyl groups in components (A) and (B) is 2 / 5 to 7, more preferably 1 / 2 to 2, and even more preferably 2 / 5 to 5 / 4. Within the above ranges, the thermally conductive silicone composition cures sufficiently, the hardness of the entire thermally conductive composition falls within a more suitable range, and when used as a gap filler, cracks are less likely to occur, and the composition has the advantages of both flexibility and adhesiveness.
[0050] The hydrosilyl groups in component (C) may be located at the molecular terminals, in side chains, or both at the molecular terminals and in side chains. An organohydrogenpolysiloxane having hydrosilyl groups only at the molecular terminals and an organohydrogenpolysiloxane having hydrosilyl groups only in side chains may be mixed and used.
[0051] From the viewpoint of improving heat resistance, component (C) may also contain an organohydrogenpolysiloxane containing at least one aromatic group in the molecule. For economic reasons, the aromatic group is preferably a phenyl group. A mixture of an aromatic group-containing organohydrogenpolysiloxane and an aromatic group-free organohydrogenpolysiloxane may also be used.
[0052] The viscosity of component (C) at 25°C is from 10 mPa·s to 10,000 mPa·s, preferably from 20 mPa·s to 5,000 mPa·s, and more preferably from 30 mPa·s to 2,000 mPa·s. In order to adjust the viscosity of the final product, the thermally conductive composition, two or more types of hydrogen-containing diorganopolysiloxanes with different viscosities can be used. The mixed viscosity of the gap filler composition may be in the range of 10 Pa·s to 1,000 Pa·s, more preferably in the range of 20 Pa·s to 500 Pa·s, and even more preferably in the range of 30 Pa·s to 250 Pa·s.
[0053] The amount of component (C) contained in the thermally conductive silicone composition of the present invention can be set so that the ratio of the number of hydrosilyl groups in component (C) to the number of alkenyl groups in components (A) and (B) is in the range of 1 / 5 to 7. Within the above range, the thermally conductive composition can have an appropriate hardness after curing.
[0054] ((D) component) Component (D) is a diorganopolysiloxane that does not contain alkenyl groups. Component (D) functions to control the viscosity of the thermally conductive silicone composition. Component (D) has a viscosity of 500 mPa·s or less at 25°C.
[0055] There are no particular limitations on the molecular structure of component (D), and it can be, for example, a linear, branched or cyclic diorganopolysiloxane, with linear diorganopolysiloxane being preferred.
[0056] Specific examples of component (D) include linear dimethylpolysiloxanes blocked at both ends with trimethylsilyl groups and linear diethylpolysiloxanes blocked at both ends with triethylsilyl groups. Linear dimethylpolysiloxanes blocked at both ends with trimethylsilyl groups are particularly preferred.
[0057] ((E) component) Component (E) is an addition catalyst that promotes the addition curing reaction between alkenyl groups bonded to silicon atoms in component (A) described above and hydrogen atoms bonded to silicon atoms in component (C) described above. The addition catalyst is a catalyst known to those skilled in the art. Component (E) includes platinum group metals such as platinum, rhodium, palladium, osmium, iridium, and ruthenium, or metals thereof immobilized on a fine particle support material (e.g., activated carbon, aluminum oxide, and silicon oxide). Further examples of the component (E) include platinum compounds such as platinum halides, platinum-olefin complexes, platinum-alcohol complexes, platinum-alcoholate complexes, platinum-vinylsiloxane complexes, dicyclopentadiene-platinum dichloride, cyclooctadiene-platinum dichloride, and cyclopentadiene-platinum dichloride.
[0058] From an economical point of view, metal compound catalysts other than the platinum group metals as mentioned above may be used as component (E).For example, the hydrosilylation iron catalyst includes an iron-carbonyl complex catalyst, an iron catalyst having a cyclopentadienyl group as a ligand, an iron catalyst having a terpyridine-based ligand, an iron catalyst having a terpyridine-based ligand and a bistrimethylsilylmethyl group, an iron catalyst having a bisiminopyridine ligand, an iron catalyst having a bisiminoquinoline ligand, an iron catalyst having an aryl group as a ligand, an iron catalyst having a cyclic or non-cyclic olefin group having an unsaturated group, and an iron catalyst having a cyclic or non-cyclic olefin group having an unsaturated group.Other examples include hydrosilylation cobalt catalysts, vanadium catalysts, ruthenium catalysts, iridium catalysts, samarium catalysts, nickel catalysts, and manganese catalysts.
[0059] The amount of component (E) used is an effective amount depending on the desired curing temperature and curing time depending on the application, but typically the concentration of the catalytic metal element relative to the total mass of the thermally conductive silicone composition is preferably in the range of 0.5 ppm to 1,000 ppm, more preferably 1 ppm to 500 ppm, and even more preferably 1 ppm to 100 ppm. If the amount is less than 0.5 ppm, the addition reaction will be significantly slower, while if the amount exceeds 1,000 ppm, costs will increase and this is economically undesirable.
[0060] (Component (F)) The thermally conductive filler of component (F) is a filler component for improving the thermal conductivity of the thermally conductive composition. Component (F) is at least one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, metal nitrides, and metal carbides. In order to obtain a gap filler with high insulating properties for application to electronic substrates and the like, it is preferable to use a material that has excellent insulating properties as well as thermal conductivity as the thermally conductive filler (F).
[0061] Examples of the (F) thermally conductive filler include metal oxides such as aluminum oxide, zinc oxide, magnesium oxide, titanium oxide, silicon oxide, and beryllium oxide, metal hydroxides such as aluminum hydroxide and magnesium hydroxide, nitrides such as aluminum nitride, silicon nitride, and boron nitride, carbides such as boron carbide, titanium carbide, and silicon carbide, graphite and other graphite, metals such as aluminum, copper, nickel, and silver, and mixtures thereof. In particular, when the silicone composition requires electrical insulation, it is preferable to use a metal oxide, metal hydroxide, nitride, or a mixture thereof, and it may be an amphoteric hydroxide or amphoteric oxide, and specifically, it is preferable to use one or more selected from the group consisting of aluminum hydroxide, boron nitride, aluminum nitride, zinc oxide, aluminum oxide, magnesium oxide, and magnesium hydroxide.
[0062] Incidentally, aluminum oxide, aluminum hydroxide, magnesium oxide, magnesium hydroxide, zinc oxide, aluminum nitride, and boron nitride are insulating materials, have relatively good compatibility with components (A) and (B), are available in a wide industrial range of particle sizes, are easily available, and are relatively inexpensive, and therefore are suitable as thermally conductive inorganic fillers.
[0063] In the thermally conductive silicone composition of the present invention, it is more preferable to use at least one selected from aluminum oxide, aluminum hydroxide, magnesium oxide, magnesium hydroxide, zinc oxide, aluminum nitride, and boron nitride as component (F). When only one type is used as component (F), it is preferable to select aluminum oxide, aluminum hydroxide, or zinc oxide, and it is more preferable to select aluminum oxide. Even when only one type is used, it is more preferable to combine two or more types with different shapes. For example, spherical aluminum oxide and amorphous aluminum oxide may be combined, or spherical zinc oxide and amorphous zinc oxide may be combined. As the component (F), it is more preferable to use at least two selected from aluminum oxide, aluminum hydroxide, magnesium oxide, magnesium hydroxide, zinc oxide, aluminum nitride, and boron nitride. For example, spherical aluminum oxide, amorphous aluminum oxide, and amorphous zinc oxide are combined.
[0064] The shape of the thermally conductive filler is not particularly limited, and may be, for example, spherical, amorphous, fine powder, fibrous, scaly, etc. In order to blend a necessary amount of thermally conductive filler to increase the thermal conductivity of the thermally conductive member, the shape of the thermally conductive filler is preferably spherical, and the average particle size may be 1 to 100 μm. The spherical shape referred to here may be not only a perfect sphere, but also a round shape. When spherical aluminum oxide is used as component (F), α-alumina obtained by high-temperature spraying or by hydrothermal treatment of alumina hydrate may be used.
[0065] In order to improve the filling rate of the thermally conductive filler, it is more preferable to use a spherical thermally conductive filler and a non-spherical thermally conductive filler. By using at least two or more types of thermally conductive fillers with different shapes in combination, it is possible to fill them in a state close to the closest packing, and the effect of increasing the thermal conductivity is obtained. By using a spherical thermally conductive filler in combination with a non-spherical thermally conductive filler (for example, an amorphous thermally conductive filler), it is possible to further increase the thermal conductivity.
[0066] The thermally conductive filler preferably has a thermal conductivity of at least 10 W / m·K. If the thermal conductivity is less than 10 W / m·K, the thermal conductivity of the thermally conductive silicone composition itself may be low. In particular, when the thermally conductive member needs to have electrical insulation properties, it may be possible to select a non-conductive thermally conductive filler.
[0067] The thermally conductive filler needs to be blended in an amount necessary to increase the thermal conductivity of the thermally conductive member (for example, 2.0 W / m K or more). For example, when the entire thermally conductive silicone composition is taken as 100 parts by mass, the content of component (F) may be from 70 parts by mass to 95 parts by mass. Within the above range, the thermally conductive composition as a whole has sufficient thermal conductivity, is easy to mix during compounding, maintains flexibility after curing, and does not have an excessively large specific gravity, making it more suitable as a thermally conductive composition for forming a thermally conductive member that requires thermal conductivity and light weight. If the content of component (F) is too low, it becomes difficult to sufficiently increase the thermal conductivity of the cured product of the thermally conductive composition obtained, while if the content of component (F) is too high, the silicone composition becomes highly viscous, which may make it difficult to apply the thermally conductive composition uniformly, and problems such as an increase in the thermal resistance value of the cured composition and a decrease in flexibility may occur.
[0068] The average particle size of component (F) is not particularly limited and may be in the range of 1 μm to 100 μm. If the average particle size is too small, the fluidity of the silicone composition decreases, and if the average particle size is too large, the particles may get caught in the sliding parts of the coating device, causing problems such as scraping of the device. The average particle size of component (F) is D50 (or median size), which is the 50% particle size in the volume-based cumulative particle size distribution measured with a laser diffraction particle size measuring device.
[0069] ((G) component) The coupling agent of the component (G) may, for example, be a silane coupling agent. Examples of the silane coupling agent include organosilicon compounds or organosiloxanes having an organic group having 3 or more carbon atoms in one molecule, such as an epoxy group, an alkyl group, an aryl group, a vinyl group, a styryl group, a methacryl group, an acrylic group, an amino group, an isocyanurate group, a ureido group, a mercapto group, an isocyanate group, or an acid anhydride, and an alkoxy group bonded to a silicon atom. Examples of silane coupling agents include silane compounds such as octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, vinyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-isocyanatepropyltriethoxysilane, and 3-trimethoxysilylpropylsuccinic anhydride. The silane compounds may be compounds that do not have a hydrosilyl group, and may be used alone or in combination of two or more. By treating the surface of the thermally conductive filler with the silane coupling agent, the affinity with the silicone polymer is improved, the viscosity of the composition can be reduced, and the filling property of the thermally conductive filler can be improved. Therefore, by blending more thermally conductive filler, it is possible to improve the thermal conductivity.
[0070] The amount of silane coupling agent to be blended with the thermally conductive filler is an effective amount depending on the curing temperature and curing time desired for the application. Usually, the optimum amount is 0.5 wt% to 2 wt% of the thermally conductive filler. However, as a guideline for the required amount, the following formula is used, and 1 to 3 times the amount may be blended. Required amount of silane coupling agent (g) = Thermally conductive filler mass (g) × specific surface area of thermally conductive filler (m 2 / g) ÷ specific minimum coverage area of silane coupling agent (m2 / g)
[0071] ((H) component) Component (H) is a silanol group-containing polydimethylsiloxane. The component (H) exhibits the function of improving the thread breakability of the discharged liquid. The viscosity of component (H) is 10 mPa·s or greater and 1,000 mPa·s or less at 25°C.
[0072] Component (H), a silanol group-containing organopolysiloxane with a viscosity of 10 mPa s or greater and 500 mPa s or less at 25°C, is blended in to improve the storage stability of the thermally conductive silicone composition, and to improve the flexibility and pump-out resistance of the thermally conductive component obtained by curing the composition. Component (H) may be a compound that does not have an alkenyl group or a hydrogen atom (hydrosilyl group) bonded to a silicon atom. It may also be a linear organopolysiloxane that has at least one silanol group at each end of the molecular chain. If component (H) has such a structure, this results in improved resistance to thread breakage.
[0073] Specific examples of component (H) include linear dimethylpolysiloxanes blocked at both ends with dimethylhydroxysilyl groups and linear diethylpolysiloxanes blocked at both ends with diethylhydroxysilyl groups. Linear dimethylpolysiloxanes blocked at both ends with dimethylhydroxysilyl groups are particularly preferred.
[0074] Incidentally, other components (for example, (D)) may contain silanol groups at an impurity level (for example, 0.001 parts by mass or less relative to the total amount of the component), and in such cases they are not included in the blending amount of component H.
[0075] In the thermally conductive silicone composition, further, as an optional component other than the above components (A) to (G), conventionally known additives for silicone rubber and gel can be used, provided that the purpose of the present disclosure is not impaired. Examples of such additives include organosilicon compounds, crosslinking agents, adhesive assistants, pigments, dyes, curing inhibitors, heat resistance imparting agents, flame retardants, antistatic agents, conductivity imparting agents, airtightness improvers, radiation shielding agents, electromagnetic wave shielding agents, preservatives, stabilizers, organic solvents, plasticizers, and fungicides, or organopolysiloxanes that contain one silicon-bonded hydrogen atom or alkenyl group in one molecule and do not contain other functional groups, and silicon-bonded hydrogen atoms. These optional components may be used alone or in combination of two or more. The thermally conductive silicone composition of the present invention may contain one or more of octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), dodecamethylcyclohexasiloxane (D6), tetradecamethylcycloheptasiloxane (D7), and hexadecamethylcyclooctasiloxane (D8). The total content of each of the above (D4), (D5), (D6), (D7), and (D8) may be less than 0.1 parts by mass (i.e., less than 1,000 ppm) when the total amount of the first liquid and / or the total amount of the second liquid is taken as 100 parts by mass.
[0076] (base material) The substrate may be one or more selected from glass, metal, ceramics, and resin. The metal substrate to which the thermally conductive silicone composition is adhered is preferably a metal substrate selected from aluminum, magnesium, iron, nickel, titanium, stainless steel, copper, lead, zinc, molybdenum, and silicon. The ceramic substrate to which the thermally conductive silicone composition is adhered is preferably aluminum oxide, aluminum nitride, alumina zirconia, zirconium oxide, zinc oxide, barium titanate, lead zirconate titanate, beryllium oxide, silicon nitride, silicon carbide, or other oxides, carbides, or nitrides. The resin substrate to which the thermally conductive silicone composition cures and adheres is preferably a resin substrate selected from polyester, epoxy, polyamide, polyimide, ester, polyacrylamide, acrylonitrile-butadiene-styrene (ABS), styrene, polypropylene, polyacetal, acrylic, polycarbonate (PC), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyether ether ketone (PEEK), polymethyl methacrylate (PMMA), and silicone. When the thermally conductive member obtained by curing the thermally conductive silicone composition is a gap filler for a battery unit, the battery unit housing, which is the substrate to be adhered, may have an iron surface at least partially coated with cationic electrodeposition coating, or the heat sink may have an aluminum surface. The thermally conductive silicone composition is injected so as to fill the gap between the iron surface and the aluminum surface that have been coated by cathodic electrodeposition coating, and is cured to provide a gap filler.
[0077] The electric and electronic devices are not particularly limited, and examples thereof include mobile phones, smartphones, tablets, smartwatches, computers, semiconductor package substrates, electronic circuit substrates, LED package substrates, sensor substrates, imaging element substrates, liquid crystal substrates, and organic EL substrates.
[0078] (Method of producing thermally conductive silicone composition) The first manufacturing method is a method for obtaining a cured product of a two-part mixture type thermally conductive silicone composition. The first liquid contains the above-mentioned components (A), (B), (D), (E) and (F). The second liquid contains the above-mentioned components (B), (C), (D) and (F). The second liquid may further contain component (A). The first liquid and / or the second liquid may further contain the above-mentioned component (G). The first liquid and / or the second liquid may further contain the above-mentioned component (H).
[0079] In the first liquid preparation process, components (A), (B), (D), and (E) are mixed together, and then component (F) is mixed therein. Component (A): Alkenyl-containing diorganopolysiloxane Viscosity at 25℃: 500mPa·s to 7,000mPa·s 1.0 to 9.0 parts by mass per 100 parts by mass of the first liquid total composition Ingredient (B): Organopolysiloxane Viscosity at 25℃: 10,000 mPa s or more and 200,000 mPa s or less 0.05 to 1.0 parts by mass per 100 parts by mass of the total composition of the first liquid Ingredients (D): Diorganopolysiloxane not containing alkenyl groups Viscosity 500mPa s or less at 25℃ 0.1 to 9.0 parts by mass per 100 parts by mass of the first liquid total composition Ingredients (E): Addition Catalyst 0.01 to 1.0 parts by weight per 100 parts by weight of the first liquid total composition Ingredient(F): Thermally conductive filler 70.0 to 95.0 parts by mass per 100 parts by mass of the total composition of the first liquid In the first liquid preparation process, components (A), (B), (D), (E), (G), and (H) may be mixed together. In this case, components (G) and (H) are as follows: Ingredients (G): Coupling agent (WACKER SILANE 25013 VP) 0.01 to 2.0 parts by weight per 100 parts by weight of the first liquid total composition Ingredients (H): Silanol-containing polydimethylsiloxane Viscosity at 25℃: 10 mPa s to 1,000 mPa s 0.01 to 2.0 parts by weight per 100 parts by weight of the first liquid total composition
[0080] In the second liquid preparation process, components (A), (B), (C), and (D) are mixed together, and then component (F) is mixed therein. Component (A): Alkenyl-containing diorganopolysiloxane Viscosity at 25℃: 500mPa·s to 7,000mPa·s 1.0 to 9.0 parts by mass per 100 parts by mass of the second liquid total composition Ingredient (B): Organopolysiloxane Viscosity at 25℃: 10,000 mPa s or more and 200,000 mPa s or less 0.05 to 1.0 parts by weight per 100 parts by weight of the total composition of the second liquid Ingredients (C): Organopolysiloxane with two or more hydrosilyl groups per molecule Viscosity at 25°C: 10 mPa·s to 10,000 mPa·s 0.01 to 10.0 parts by mass per 100 parts by mass of the total composition of the second liquid Ingredients (D): Diorganopolysiloxane not containing alkenyl groups Viscosity 500mPa s or less at 25℃ 0.1 to 9.0 parts by weight per 100 parts by weight of the second liquid total composition Ingredient(F): Thermally conductive filler 70.0 to 95.0 parts by mass per 100 parts by mass of the total composition of the second liquid In the second liquid preparation process, components (A), (B), (C), (D), (G), and (H) may be mixed together. In this case, components (G) and (H) are as follows: Ingredients (G): Coupling Agent 0.01 to 2.0 parts by weight per 100 parts by weight of the total composition of the second liquid Ingredients (H): Silanol-containing polydimethylsiloxane Viscosity at 25℃: 10 mPa s to 1,000 mPa s 0.01 to 2.0 parts by weight per 100 parts by weight of the total composition of the second liquid
[0081] (Method of manufacturing thermally conductive member) The manufacturing method for thermally conductive members involves placing the first and second liquids in a two-liquid internal mixing dispenser, applying a predetermined pressure to each of the first and second liquids to mix the first and second liquids in a predetermined ratio, and ejecting a predetermined amount of the mixed liquid toward the substrate. The manufacturing method is Discharging the first liquid from the first liquid storage section to a mixing section; discharging the second liquid from a second liquid storage section into the mixing section; a step of mixing the first liquid and the second liquid in a mixing section to obtain a thermally conductive silicone composition (mixed liquid); A step of discharging and applying the thermally conductive silicone composition to a substrate; and curing the thermally conductive silicone composition (mixed liquid) applied to a substrate to obtain a thermally conductive member. By using the first and second liquids, no caking occurs under discharge pressure from the first liquid storage section, the second liquid storage section, the mixing section, and until the liquid is discharged from the nozzle.
[0082] <Example> Examples will be described below, but the present invention is not limited to the following examples. Table 1 shows the compounding ratio of each component in the examples, and Table 3 shows the evaluation results. Table 2 shows the compounding ratio of each component in the comparative examples, and Table 4 shows the evaluation results. The numerical values of the compounding ratios shown in Tables 1 and 2 indicate parts by mass. The viscosity described in this specification is a value measured using a rotational viscometer (JIS K7117-2) at 25°C and a shear rate of 10 / s.
[0083] First and second liquids shown in the examples and comparative examples were prepared, respectively. The first and second liquids are loaded into a dispenser (e.g., MPP-3 manufactured by Musashi Engineering Co., Ltd.) and discharged onto the substrate. In the dispenser, the mixture ratio of the first and second liquids is set to 1:1. The discharge pressure of the dispenser is set to 0.5 MPa.
[0084] <Method of measuring mixed viscosity> The mixed liquid discharged from the dispenser was measured at 25° C. and a shear rate of 10 / s using a rotational viscometer (JIS K7117-2). The viscosity is preferably 250 kPa or less.
[0085] <Method of measuring thermal conductivity> The mixture discharged from the dispenser was poured into a cylindrical press mold with a diameter of 30 mm and a height of 6 mm, and cured at 23°C for 24 hours to produce a cylindrical cured product. The thermal conductivity of the cured product was measured using a machine [TPS-500, Kyoto Electronics Manufacturing Co., Ltd.] that measures by the hot disk method in accordance with ISO 22007-2. A sensor was placed between the two cylindrical cured products prepared above, and the thermal conductivity was measured using the above device. The thermal conductivity is preferably 2.0 W / m·K or higher.
[0086] <How to measure hardness (Shore 00)> The mixture discharged from the dispenser was poured into a cylindrical press mold with a diameter of 30 mm and a height of 6 mm, and cured at 23°C for 24 hours to produce a cylindrical cured product. The hardness of the cured product was measured using a Techlock Co., Ltd. Shore 00 hardness tester, which measures the hardness according to the method of JIS K 6253-3. The hardness (Shore 00) is preferably between 30 and 80.
[0087] <Method of measuring caking> Using a dispenser (MPP-3 manufactured by Musashi Engineering), dispense 0.03cc and wait for 0.20 seconds repeatedly, and dispense 1.0kg of material. After that, disassemble the dispenser and check for caking. The criteria for judgment are A, B, and C below. A: No agglomerates were observed, B: Agglomerates of several mm were observed, but there was no blockage in the passage, C: A blockage occurred in the passage.
[0088] <Method for measuring initial ejection properties> Using a dispenser (MPP-3 manufactured by Musashi Engineering Co., Ltd.), the discharge pressure is set to 0.5 MPa, the material is discharged for 10 seconds, the amount of material discharged is confirmed, and the amount discharged per hour is calculated. The criteria for judgment are A, B, and C below. A: 0.2cc / sec or more, B: less than 0.2cc / sec, 0.1cc / sec or more, C: less than 0.1cc / sec
[0089] <Method for measuring thread breakage> The thermally conductive composition is filled and applied as a bead from a dispenser (MPP3 manufactured by Musashi Engineering) to an aluminum plate at a height of 2.5 mm, width of 10 mm, and length of 20 mm. It is dispensed at five locations spaced 10 mm apart, and the bead spacing at four locations is measured. The closer the average value is to 10 mm, the better the stringiness is, and the closer it is to 0 mm, the worse the stringiness is. The evaluation results were graded on a three-point scale: A=good, B=average, and C=poor. A:6mm or more B: 2 or more and less than 6 mm C: Less than 2 mm
[0090] [1st liquid] Components (A), (B), (D), (E), (G), and (H) were weighed and added based on the compounding ratios in Tables 1 and 2, and mixed at room temperature for 30 minutes using a planetary mixer. Then, component (F) was added, and mixed at room temperature for 15 minutes using a planetary mixer.
[0091] [Second liquid] Components (A), (B), (C), (D), (G), and (H) were weighed and added based on the mixing ratios in Tables 1 and 2, and mixed at room temperature for 30 minutes using a planetary mixer. Then, component (F) was added, and mixed at room temperature for 15 minutes using a planetary mixer.
[0092] [Table 1]
[0093] [Table 2]
[0094] <Ingredients> (A-1) A linear dimethylpolysiloxane having one alkenyl group at each end and a viscosity of 1,000 mPa s. (A-2) A linear dimethylpolysiloxane having one alkenyl group at each end and a viscosity of 500 mPa s. (A-3) A linear dimethylpolysiloxane having one alkenyl group at each end and a viscosity of 7,000 mPa s. (A-4) A linear dimethylpolysiloxane having one alkenyl group at each end and a viscosity of 100 mPa s. (B-1) A linear organopolysiloxane having a viscosity of 100,000 mPa·s (B-2) A linear organopolysiloxane having a viscosity of 200,000 mPa·s (B-3) A linear organopolysiloxane having a viscosity of 1,000,000 mPa·s (B-4) A linear organopolysiloxane having a viscosity of 10,000 mPa·s (C) A dimethylpolysiloxane with a viscosity of 200 mPa s having 12 to 18 hydrogen atoms bonded to silicon atoms in the side chains. (D-1) A linear dimethylpolysiloxane that does not contain an alkenyl group and has a viscosity of 50 mPa s (D-2) A linear dimethylpolysiloxane that does not contain an alkenyl group and has a viscosity of 500 mPa·s (E) Platinum-divinyltetramethyldisiloxane complex (F-1) Irregular zinc oxide (average particle size (D50) 0.6 μm, BET specific surface area 4.1 m 2 / g) was used. (F-2) Irregular aluminum oxide (average particle size (D50) 3.9 μm, BET specific surface area 0.9 m 2 / g) was used. (F-3) Spherical aluminum oxide (average particle size (D50) 40 μm, BET specific surface area 0.12 m2 / g) was used. (G) SILANE 25013 VP manufactured by Wacker Chemie AG. (H) A linear diorganopolysiloxane having one silanol group at each end and a viscosity of 50 mPa·s.
[0095] (evaluation) Table 3 shows the evaluation results of Examples 1 to 15. In Example 1, a polymer with an appropriate viscosity was used as the base polymer, and a polymer with an appropriate viscosity for suppressing separation was introduced to suppress caking, and the dischargeability and thread breakage resistance were good, and the thermal conductivity was also high. In Example 2, although the amount of the separation-suppressing polymer was smaller than in Example 1, caking was somewhat suppressed (to an extent that did not substantially cause problems in use), and the other items were good. In Example 3, a polymer with a slightly high viscosity was used as the base polymer, and a polymer with an appropriate viscosity for suppressing separation was introduced to suppress caking, and the dischargeability was somewhat good, the thread breakage resistance was good, and the thermal conductivity was also high. In Example 4, a polymer with a relatively low viscosity was used as the base polymer, and a polymer with an appropriate viscosity for suppressing separation was introduced, thereby slightly suppressing caking, and the dischargeability and thread breakage resistance were good, and the thermal conductivity was also high. In Example 5, a polymer with an appropriate viscosity was used as the base polymer, and a polymer with a slightly higher viscosity was introduced to suppress separation, thereby suppressing caking, and the dischargeability was also somewhat good, the thread breakage resistance was good, and the thermal conductivity was also high. In Example 6, a polymer with an appropriate viscosity was used as the base polymer, and a polymer with a slightly lower viscosity for suppressing separation was introduced, thereby slightly suppressing caking. The dischargeability and thread-snipping properties were also good, and the thermal conductivity was also high. In Example 7, a polymer with an appropriate viscosity was used as the base polymer, a polymer with an appropriate viscosity for suppressing separation was introduced, and the amount of base polymer was increased, thereby suppressing caking, providing somewhat good dischargeability, good thread breakage resistance, and high thermal conductivity. In Example 8, a polymer with an appropriate viscosity was used as the base polymer, a polymer with an appropriate viscosity for suppressing separation was introduced, and the amount of base polymer was reduced, thereby slightly suppressing caking, and the dischargeability and thread-snipping properties were also good, and the thermal conductivity was also high. In Example 9, a polymer with an appropriate viscosity was used as the base polymer, a polymer with an appropriate viscosity for inhibiting separation was introduced, and the amount of the separation-inhibiting polymer was increased, thereby inhibiting caking, providing somewhat good dischargeability, good resistance to thread breakage, and high thermal conductivity. In Example 10, a polymer with an appropriate viscosity was used for the base polymer, a polymer with an appropriate viscosity for inhibiting separation was introduced, and the amount of the separation-inhibiting polymer was reduced, thereby inhibiting caking, providing somewhat good dischargeability, good thread breakage resistance, and high thermal conductivity. In Example 11, a polymer with an appropriate viscosity was used as the base polymer, and a polymer with an appropriate viscosity for suppressing separation was introduced. By using a dimethyl oil with a slightly high viscosity (500 mPa s) for viscosity adjustment, caking was suppressed, the dischargeability was also somewhat good, the thread breakage resistance was good, and the thermal conductivity was also high. In Example 12, a polymer with an appropriate viscosity was used as the base polymer, a polymer with an appropriate viscosity for suppressing separation was introduced, and the thermally conductive filler was set at 85%, thereby suppressing caking, and the extrusion and thread cutting properties were also good, and the thermal conductivity was also high. In Example 13, no base polymer was used in the second liquid, and the amount of base polymer introduced in the first liquid was large. However, by using a polymer with an appropriate viscosity for the base polymer and introducing a polymer with an appropriate viscosity for suppressing separation, caking was suppressed, the dischargeability was somewhat good, the thread breakage resistance was good, and the thermal conductivity was high. In Example 14, a polymer with an appropriate viscosity was used as the base polymer, and a polymer with an appropriate viscosity for suppressing separation was introduced, which suppressed caking and had good dischargeability, but the thread breakage was poor because component H was not used. The thermal conductivity was high. In Example 15, a polymer with an appropriate viscosity was used as the base polymer, and a polymer with an appropriate viscosity for suppressing separation was introduced, which suppressed caking and improved thread breakage resistance, but the dischargeability was somewhat good because component G was not used. The thermal conductivity was high.
[0096] Table 4 shows the evaluation results of Comparative Examples 1 to 3. In Comparative Example 1, a low-viscosity polymer was used as the base polymer, and a polymer with an appropriate viscosity for suppressing separation was introduced, which caused caking. The dischargeability was good, and the thermal conductivity was also high. In Comparative Example 2, a polymer with an appropriate viscosity was used as the base polymer, and a high-viscosity polymer for suppressing separation was introduced to suppress caking, but the dischargeability and thread breakage resistance were poor, and the thermal conductivity was high. In Comparative Example 3, a low-viscosity polymer was used as the base polymer, but the amount of filler was reduced and a polymer with an appropriate viscosity for suppressing separation was introduced, thereby suppressing caking. The dischargeability and thread breakage resistance were good, but the thermal conductivity was low.
[0097] [Table 3]
[0098] [Table 4]
Claims
1. (A) 1.0 part by mass or more and 9.0 parts by mass or less of an alkenyl group-containing diorganopolysiloxane having a viscosity of 500 mPa·s or more and 7,000 mPa·s or less at 25°C, (B) 0.05 parts by mass or more and 1.0 parts by mass or less of an organopolysiloxane having a viscosity of 10,000 mPa·s or more and 200,000 mPa·s or less at 25°C; (C) an organopolysiloxane having two or more hydrosilyl groups per molecule; (D) a diorganopolysiloxane having no alkenyl group and having a viscosity of 500 mPa·s or less at 25° C.; (E) an addition catalyst; and (F) at least one or more thermally conductive fillers selected from metals, metal oxides, metal hydroxides, metal nitrides, and metal carbides; A thermally conductive silicone composition comprising: the thermally conductive silicone composition contains 85 parts by mass or more of the component (F) based on 100 parts by mass of the entire composition, The mixed viscosity of the thermally conductive silicone composition is 250 Pa·s or less at 25° C.; A thermally conductive silicone composition.
2. The thermally conductive silicone composition further contains (H) a silanol group-containing polydimethylsiloxane. The thermally conductive silicone composition according to claim 1 .
3. The thermally conductive silicone composition comprises: A two-part thermally conductive silicone composition comprising a first liquid and a second liquid packaged separately from each other, the first liquid and the second liquid being mixed together at the time of use to form a thermally conductive silicone composition, the first liquid contains the components (A), (B), (D), (E) and (F); the second liquid contains the components (B), (C), (D), and (F) but does not contain the component (E); The thermally conductive silicone composition according to claim 1 .
4. The thermally conductive silicone composition according to claim 3 , wherein the first liquid and / or the second liquid further comprises (H) a silanol group-containing polydimethylsiloxane.
5. The thermally conductive silicone composition comprises:
5. The thermally conductive silicone composition according to claim 3, wherein no aggregates are observed in any of the first liquid, the second liquid, and the thermally conductive silicone composition in the caking evaluation described below. (Caking Evaluation) The dispenser is used to repeatedly dispense 0.03 cc and wait for 0.20 seconds, until 1.0 kg of material is dispensed. The dispenser is then disassembled and visually inspected for the presence of aggregates.
6. A method for producing a thermally conductive silicone composition, comprising the steps of: a first liquid producing step of mixing (A) 1.0 part by mass or more and 9.0 parts by mass or less of an alkenyl group-containing diorganopolysiloxane having a viscosity of 500 mPa·s or more and 7,000 mPa·s or less at 25°C, (B) 0.05 part by mass or more and 1.0 parts by mass or less of an organopolysiloxane having a viscosity of 10,000 mPa·s or more and 200,000 mPa·s or less at 25°C, (D) an alkenyl group-free diorganopolysiloxane having a viscosity of 500 mPa·s or less at 25°C, and (E) an addition catalyst, and then mixing (F) at least one or two or more types of thermally conductive filler selected from metals, metal oxides, metal hydroxides, metal nitrides, and metal carbides to obtain a first liquid; a second liquid producing step of mixing (B) 0.05 part by mass or more and 1.0 part by mass or less of an organopolysiloxane having a viscosity of 10,000 mPa·s or more and 200,000 mPa·s or less at 25°C, (C) an organopolysiloxane having two or more hydrosilyl groups in one molecule, and (D) a diorganopolysiloxane having no alkenyl groups and having a viscosity of 500 mPa·s or less at 25°C, and then mixing (F) at least one or two or more types of thermally conductive filler selected from metals, metal oxides, metal hydroxides, metal nitrides, and metal carbides to obtain a second liquid; Including, A method for producing a thermally conductive silicone composition.
7. In the second liquid preparation step, before the addition of the component (F), 1.0 part by mass or more and 9.0 parts by mass or less of an alkenyl group-containing diorganopolysiloxane (A) having a viscosity of 500 mPa·s or more and 7,000 mPa·s or less at 25° C. is mixed with other components; A method for producing the thermally conductive silicone composition according to claim 6.
8. In the first liquid preparation step and / or the second liquid preparation step, (H) silanol group-containing polydimethylsiloxane is mixed with other components before the addition of the component (F). A method for producing the thermally conductive silicone composition according to claim 6 or 7. A method for manufacturing a thermally conductive member.
9. A method for manufacturing a thermally conductive member, comprising the steps of: A step of discharging the first liquid according to claim 3 from a first liquid storage section to a mixing section; A step of discharging the second liquid according to claim 3 from a second liquid storage section to the mixing section; mixing the first liquid and the second liquid in the mixing section to obtain a thermally conductive silicone composition; applying the thermally conductive silicone composition to a substrate by discharging; and curing the thermally conductive silicone composition applied to the substrate to obtain a thermally conductive member. A method for manufacturing a thermally conductive member.
10. A thermally conductive member provided on a surface of the substrate, the thermally conductive member being obtained by curing the thermally conductive silicone composition according to claim 1 or 2, the thermally conductive member being obtained by curing the thermally conductive silicone composition obtained by the method for producing a thermally conductive silicone composition according to claim 6 or 7, or the thermally conductive member being obtained by the method for producing a thermally conductive member according to claim 9. Heat dissipation material.
11. An electric or electronic device comprising the heat dissipation member according to claim 10.
Citation Information
Patent Citations
Polyorganosiloxane and thermally conductive silicone composition thereof
JP2022531875A
Thermally conductive silicone composition and cured product thereof, and manufacturing method
WO2018088416A1
Thermally conductive silicone composition and cured product thereof, and manufacturing method
WO2018088417A1
Thermally conductive silicone composition and method for producing gap filler using said composition
WO2023053760A1
Highly heat-conductive resin composition
JP1998204300A