Antifouling treatment agent and antifouling laminate

A laminate structure with specific layers using a fluorine-free solvent and catalyst addresses the environmental and cost issues of existing treatments, providing effective antifouling and antiglare properties with reduced environmental impact.

JP2024158204APending Publication Date: 2024-11-08HONNY CHEM
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023073195
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing antifouling and antiglare treatments for displays involve fluorine-based silane coupling agents that require fluorine-based solvents, leading to environmental impact and high costs, and often require complex etching processes.

Method used

A laminate structure with specific layers, including a base material, a first anti-reflective layer, and a second anti-reflective layer, using a hydrolyzed condensate oligomer and a fluorine-free solvent, along with a catalyst, to form an antifouling layer with balanced properties.

Benefits of technology

The laminate achieves excellent transparency, antiglare properties, low reflectivity, scratch resistance, and abrasion resistance with reduced environmental impact, using simple manufacturing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158204000001_ABST
    Figure 2024158204000001_ABST
Patent Text Reader

Abstract

To provide a method for producing an antifouling laminate that is free of fluorine-based solvents, contributing to reduced environmental load, offers superior manufacturability, and features an excellent combination of fouling prevention, glare reduction, low reflectivity, scratch resistance, and wear resistance.MEANS FOR SOLVING THE PROBLEM: An antifouling treatment agent, designed for forming an antifouling layer on a substrate layer, includes a hydrolytic condensate oligomer (A), an acid or base catalyst (J), and a solvent substantially free of fluorine (H). The hydrolytic condensate oligomer (A) is a hydrolytic condensate oligomer of an alkoxysilane compound (D) that contains a tetraalkoxysilane compound (E) and a fluorinated silane coupling agent compound (G).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antifouling laminate which has a small environmental load, excellent manufacturability, and a simple layer structure while having an excellent balance of antifouling property, antiglare property, low reflectivity, scratch resistance, and abrasion resistance, and to an antifouling treatment agent which has a small environmental load for producing the antifouling laminate. [Background technology]

[0002] 2. Description of the Related Art Displays for personal computers and the like are generally provided with an anti-stain layer and an anti-glare layer to prevent stains and light reflection. Anti-glare treatment for forming an anti-glare layer often involves etching the glass with hydrofluoric acid or the like to create irregularities, but this places a heavy burden on the environment as it produces fluorine-based waste liquid. Antifouling layers are generally formed on an antiglare layer or an antireflection layer by spraying a treatment agent that contains a fluorine-based silane coupling agent to adhere to the substrate and to impart water repellency. However, since fluorine-based silane coupling agents are poorly compatible with general solvents, they must be diluted with a fluorine-based solvent before use, which places a heavy burden on the environment and is very expensive (Patent Documents 1 to 4). Some anti-glare treatments involve forming unevenness by spray coating, and an anti-reflection layer or anti-fouling layer is often formed on top of this (Patent Document 5). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3449070 [Patent Document 2] Patent No. 5655215 [Patent Document 3] Patent No. 3876961 [Patent Document 4] WO2006-046643 [Patent Document 5] JP 2018-097379 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention aims to provide an antifouling laminate which contains a fluorine compound but does not contain a fluorine-based solvent, has a small environmental impact, is excellent in manufacturability, and has a simple layer structure while having an excellent balance of transparency, antifouling property, antiglare property, low reflectivity, scratch resistance and abrasion resistance, and an antifouling treatment agent which imposes a small environmental impact when used to produce the antifouling laminate. [Means for solving the problem]

[0005] As a result of extensive investigations, the inventors have found that the above-mentioned object can be achieved by a low-reflection laminate comprising at least a specific substrate layer, a specific first antireflection layer, and a specific second antireflection layer laminated adjacent to each other in this order, in which the first antireflection layer and the second antireflection layer have specific refractive indexes, layer thicknesses, hardness, and minimum reflectance. That is, the present invention is characterized in the following points. 1. An antifouling treatment agent for forming an antifouling layer on a substrate layer, comprising: The stain-proofing agent contains a hydrolysis condensation product oligomer (A), an acid or base catalyst (J), and a solvent (H1), The hydrolysis condensation product oligomer (A) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D) and is soluble in the solvent (H1); The alkoxysilane compound (D) contains a tetraalkoxysilane compound (E) and a fluorine-containing silane coupling agent compound (G), The solvent (H1) is substantially free of fluorine, the content of the hydrolysis-condensation product oligomer (A) in the soil-proofing agent is 1 to 50 mass%; The content of the acid or base catalyst (J1) in the stain-proofing agent is 0.05 to 7 mass %. 2. The stain-proofing agent according to the above item 1, characterized in that the mass ratio of the tetraalkoxysilane compound (E) / the fluorine-containing silane coupling agent compound (G) is 1 / 1 to 1000 / 1. 3. The stain-proofing agent according to 1 or 2 above, wherein the solvent (H1) is an alcohol-based solvent and / or a glycol-based solvent. 4. An antifouling laminate having at least a base layer and an antifouling layer, The substrate layer is made of a metal oxide or a resin, the antifouling layer is made of a dried and cured product of the antifouling treatment agent according to any one of 1 to 3 above, has a layer thickness of 50 to 1000 nm, and has a surface roughness Ra of 0.1 to 20 nm; The haze of the antifouling laminate is 0.1 to 10%. 1. An antifouling laminate comprising: 5. The antifouling laminate according to the above item 4, wherein the antifouling layer is a multi-coated layer formed by applying the antifouling treatment agent two or more times. 6. An antifouling laminate further comprising a high refractive index layer between the substrate layer and the antifouling layer, the high refractive index layer is a layer formed from a high refractive index treatment agent, The high refractive index treatment agent contains an alkoxy titanium compound (C) and a solvent (H2), The solvent (H2) is substantially free of fluorine. The content of the alkoxytitanium compound (C) in the high refractive index treatment agent is 5 to 80 mass %, the high refractive index layer is adjacent to the antifouling layer and has a layer thickness of 50 to 1000 nm; The refractive index of the high refractive index layer is 1.5 to 1.9, The refractive index of the antifouling layer is 1.2 to 1.5, The difference in refractive index between the high refractive index layer and the antifouling layer is 0.2 to 0.5. 6. The antifouling laminate according to claim 4 or 5, Effect of the Invention

[0006] The antifouling laminate of the present invention has a simple layer structure, yet has an excellent balance of transparency, antifouling property, antiglare property, low reflectivity, scratch resistance, and abrasion resistance. In addition, the antifouling treatment agent of the present invention can be applied by a simple method to transparent substrates other than glass, such as resins, and does not substantially contain fluorine-based solvents, so that the environmental load is small and the antifouling laminate can be produced by simple equipment and methods. [Brief description of the drawings]

[0007] [Figure 1] 1 is a cross-sectional view of an antifouling laminate of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of another embodiment of an antifouling laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Antifouling treatment agent The antifouling treatment agent of the present invention is a treatment agent for forming an antifouling layer on the substrate layer in the antifouling laminate of the present invention. The stain-proofing agent of the present invention contains a hydrolysis-condensation oligomer (A) and a solvent (H1) that is substantially free of fluorine, and may further contain an acid or base catalyst (J) to promote the hydrolysis-condensation reaction. Furthermore, the antifouling treatment agent may contain, as necessary, a wetting agent, a viscous material (thickener), a surface conditioning material, a coloring material (pigment, dye), an antistatic material, a conductivity imparting agent, an antibacterial and antiviral material, a filler such as hollow, chain-like, or porous solid silica particles, metal fine particles, and the like, within a range that does not adversely affect the properties of the antifouling laminate. The antifouling treatment agent preferably has excellent storage stability. For example, when stored at 40°C for 3 months in a stationary state, it is preferable that there is no change in appearance and that the increase in molecular weight is 0 to 100%, and more preferably 0 to 50%.

[0009] 1-1. Hydrolysis condensation product oligomer (A) This hydrolysis condensation oligomer (A) is a hydrolysis condensation oligomer of the alkoxysilane compound (D) and is soluble in the solvent (H1). The content of the hydrolysis condensate oligomer (A) in the soil-proofing agent is preferably from 1 to 80 mass %, more preferably from 2 to 40 mass %.

[0010] 1-2. Alkoxysilane compounds (D) The alkoxysilane compound (D) contains a tetraalkoxysilane compound (E) and a fluorine-containing silane coupling agent compound (G). The fluorine-containing silane coupling agent compound (G) is poorly compatible with organic components such as other resins and solvents, but by forming a hydrolysis condensation oligomer with the tetraalkoxysilane compound (E), it becomes easier to make it compatible with organic components such as other resins and solvents.

[0011] The mass ratio of the tetraalkoxysilane compound (E) / fluorine-containing silane coupling agent compound (G) is preferably 1 / 1 to 1000 / 1, more preferably 4 / 1 to 50 / 1. If it is smaller than the above range, the hardness is likely to be inferior, and if it is larger than the above range, the water contact angle is likely to be inferior.

[0012] 1-3. Tetraalkoxysilane compounds (E) The tetraalkoxysilane compound (E) is a silane compound having four alkoxy groups. The alkoxy group undergoes a hydrolysis reaction and a dehydration condensation reaction to form a crosslinked structure.

[0013] Specific examples of the tetraalkoxysilane compound (E) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, and oligomers thereof. Among these, tetraethoxysilane and its oligomers are preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the tetraalkoxysilane compound (E).

[0014] 1-4. Fluorine-containing silane coupling agent compounds (G) The fluorine-containing silane coupling agent compound (G) is a silane compound having a functional group capable of reacting with an organic component, a fluorine group and an alkoxy group. The functional group capable of reacting with an organic component has the effect of adjusting the refractive index.

[0015] Specific examples of the fluorine-containing silane coupling agent compound (G) include trifluoropropyltrimethoxysilane, dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, trimethoxy(1H,1H,2H,2H-perfluorohexyl)silane, triethoxy(1H,1H,2H,2H-perfluorohexyl)silane, trimethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane, triethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane, triethoxy[5,5,6,6,7,7,7-heptafluoro-4,4-bis(trifluoromethyl)heptyl]silane, trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane, and triethoxy-1H,1H,2H,2H-heptadecafluorodecylsilane. Among these, trimethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane and triethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane are preferable. In the present invention, the above compounds can be used alone or in combination of two or more as the fluorine-containing silane coupling agent compound (G).

[0016] 1-5. Acid or base catalyst (J) The acid or base catalyst (J) is a component that promotes the hydrolysis reaction and dehydration condensation reaction of the alkoxysilane compound (D), the fluorine-containing silane coupling agent compound (G) and the hydrolysis condensate oligomer (A). The content of the acid or base catalyst (J) in the stain-proofing agent is preferably 0.05 to 10 mass%, more preferably 0.1 to 5.0 mass%. If it is less than the above range, the promotion effect is likely to be insufficient, and if it is more than the above range, it is likely to be difficult to ensure uniform reaction progress.

[0017] Specific examples of the acid catalyst include hydrochloric acid, sulfuric acid, nitric acid, p-toluenesulfonic acid, benzenesulfonic acid, 10-camphorsulfonic acid, formic acid, oxalic acid, acetic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, and lactic acid. Specific examples of the base catalyst include triethyleneamine, dimethylaminoethanol, and aqueous ammonia. Of these, nitric acid is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the acid or base catalyst (J).

[0018] 1-6. Solvent (H1) The solvent (H1) is not particularly limited as long as it can dissolve the hydrolysis condensate oligomer (A) and the acid or base catalyst (J), but it is preferable that the solvent (H1) contains an alcohol-based solvent and / or a glycol-based solvent, and is preferably a non-fluorine-based solvent.

[0019] The solvent (H1) not only serves as a solvent for the hydrolysis condensation product oligomer (A) and the acid or base catalyst (J), but also plays an important role in forming a coating film having an uneven shape during application, particularly during spray application.

[0020] The stain-proofing agent forms a concave-convex shape due to the evaporation of the solvent (H1) that accompanies application of the agent to the base layer. Therefore, if the solvent (H1) evaporates quickly, the film formation condition deteriorates and a coating film with large projections and recesses is formed. Conversely, if the evaporation rate of the solvent (H1) is slow, the film will be in good condition, but the unevenness will be too small, and sufficient antiglare properties will not be achieved. Furthermore, during the main curing, the residual solvent (H1) evaporates, which may cause the stain-resistant layer to shrink significantly and crack.

[0021] When using a solvent that evaporates slowly, it is effective to mix a large amount of a solvent with a low boiling point or to reduce the spray discharge amount, coating speed, atomization pressure, etc. To speed up the evaporation, the substrate may be preheated to about 100°C.

[0022] Specific examples of alcohol-based solvents include methanol (carbon number 1, boiling point 65°C), ethanol (carbon number 2, boiling point 78°C), normal propanol (carbon number 3, boiling point 97°C), isopropyl alcohol (carbon number 3, boiling point 82°C), tertiary butanol (carbon number 4, boiling point 82°C), normal butanol (carbon number 4, boiling point 118°C), isobutanol (carbon number 4, boiling point 108°C), and secondary butanol. Examples of the alcohol include ethanol (carbon number: 4, boiling point: 100° C.), 1-pentanol (carbon number: 5, boiling point: 138° C.), 2-methyl-1-butanol (carbon number: 5, boiling point: 128° C.), 3-methyl-1-butanol (carbon number: 5, boiling point: 131° C.), 2-pentanol (carbon number: 5, boiling point: 119° C.), 1-ethyl-1-propanol (carbon number: 5, boiling point: 116° C.), and 2-methyl-2-butanol (carbon number: 5, boiling point: 102° C.). Among these, ethanol is preferred.

[0023] Specific examples of glycol-based solvents include alkylene glycols and alkylene glycol ethers. Specific examples of alkylene glycols include ethylene glycol (carbon number 2, boiling point 197°C), propylene glycol (carbon number 3, boiling point 189°C), butylene glycol (carbon number 4, boiling point 207°C), hexylene glycol (carbon number 6, boiling point 197°C), and octylene glycol (carbon number 8, boiling point 175°C).

[0024] Specific examples of alkylene glycol ethers include ethylene glycol monomethyl ether (carbon number 3, boiling point 124°C), ethylene glycol monoethyl ether (carbon number 4, boiling point 135°C), ethylene glycol diethyl ether (carbon number 6, boiling point 121°C), ethylene glycol monoisopropyl ether (carbon number 5, boiling point 141°C), ethylene glycol monobutyl ether (carbon number 6, boiling point 171°C), propylene glycol monomethyl ether (carbon number 4, boiling point 120°C), propylene glycol monoethyl ether (carbon number 5, boiling point 132°C), propylene glycol mono-normal propyl ether (carbon number 6, boiling point 149°C), and propylene glycol mono-normal butyl ether (carbon number 7, boiling point 171°C). Among these, propylene glycol monomethyl ether is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the solvent (H1).

[0025] 1-7. Manufacturing method of antifouling treatment agent The stain-proofing agent of the present invention can be prepared, for example, by the following method. 1) Preparation of silane compound solution The alkoxysilane compound (D) and the fluorine-containing silane coupling agent compound (G) are dissolved in a solvent (H1) to obtain a silane compound solution. 2) Preparation of catalyst solution Also, an acid or base catalyst (J) is added dropwise to the solvent (H1) and mixed to obtain a catalyst solution. 3) Preparation of antifouling agent The catalyst solution obtained above is added dropwise to the silane compound solution obtained above while stirring and mixing to produce a hydrolysis condensation oligomer (A). The temperature of the mixture is preferably adjusted to between 10 and 60° C. in order to suppress the hydrolysis condensation reaction. After the dropwise addition is completed, the mixture is left to stand at a constant temperature of 20 to 40° C. to allow the hydrolysis and condensation reaction to proceed to a desired reaction rate. The obtained reaction liquid is diluted with a solvent (H1) to a concentration and viscosity appropriate for the desired coating method and coating conditions to obtain an antifouling treatment agent. The antifouling treatment agent may be filtered, for example, through a filter having a mesh size of 0.5 to 2 μm.

[0026] 2. Antifouling laminate The antifouling laminate of the present invention is a laminate having at least a substrate layer and an antifouling layer, and while having a simple layer structure, has an excellent balance of transparency, antifouling properties, antiglare properties, low reflectivity, scratch resistance, and abrasion resistance. In order for the antifouling laminate of the present invention to have excellent transparency, the haze of the antifouling laminate is preferably from 0.1 to 10%, more preferably from 0.3 to 5.0%.

[0027] The antifouling laminate of the present invention may further have a high refractive index layer between the substrate layer and the antifouling layer. The antifouling laminate of the present invention can have improved antireflection properties by making the difference in refractive index between the high refractive index layer and the antifouling layer preferably 0.2 to 0.5, more preferably 0.2 to 0.4. If the difference in refractive index is smaller than the above range, the antireflection properties are likely to be inferior, and if the difference in refractive index is larger than the above range, the transparency is likely to be inferior.

[0028] The minimum reflectance of the antifouling layer side surface of the antifouling laminate of the present invention at a wavelength of 380 to 780 nm is preferably 0.5 to 2%, more preferably 0.5 to 1.5%. It is difficult to obtain a minimum reflectance smaller than the above range, and if the minimum reflectance is larger than the above range, the antireflection properties are likely to be inferior.

[0029] 2-1. Base material layer The substrate layer is an object to be coated with the stain-proofing agent of the present invention. The substrate layer is preferably made of a metal oxide or a resin, and in order for the antifouling laminate to have transparency, it is more preferably made of a highly transparent metal oxide or resin, and even more preferably made of a transparent metal oxide such as soda glass.

[0030] The metal oxide contained in the substrate layer may be ceramic, glass, or the like. Examples of the substrate that uses glass include a glass plate and a glass cloth. Specific examples of the resin contained in the substrate layer include PMMA, PC, PET, etc. Among these, PMMA is preferable.

[0031] The thickness of the substrate layer is not particularly limited, but is preferably 0.1 to 5.0 mm. The surface of the base layer may be subjected to an antiglare treatment (AG treatment), and the surface roughness Ra is preferably 0.5 to 20 nm as a result of the antiglare treatment. In order to set the haze of the antifouling laminate to 0.1 to 10%, the haze of the base layer is preferably 0.1 to 10%.

[0032] 2-2.Anti-stain layer The stain-proofing layer in the present invention is a layer formed from the stain-proofing agent of the present invention, and is preferably made of a cured product of the hydrolysis condensation product oligomer (A).

[0033] The refractive index of the antifouling layer is preferably from 1.2 to 1.5, and more preferably from 1.3 to 1.5. The thickness of the antifouling layer is preferably 50 to 1000 nm, more preferably 70 to 800 nm. If the thickness is thinner than the above range, the effect of providing the antifouling layer is not easily obtained, and if the thickness is thicker than the above range, cracks are easily generated. The surface roughness Ra of the antifouling layer is preferably 0.1 to 20 nm, more preferably 0.5 to 1.5 nm. If it is smaller than the above range, it is difficult to obtain Ra, and if it is larger than the above range, the haze tends to increase.

[0034] In addition, when it is desired to enhance antiglare properties, the antifouling layer is preferably a multi-coated layer formed by applying an antifouling treatment agent two or more times. The multi-coated layer is preferably a layer in which the same stain-proofing agent is multiply coated. In addition, a drying step or a heat curing step may or may not be included between coating steps. There is no particular limitation on the thickness of the antifouling layer formed by a single coating, and it is sufficient that the above-mentioned thickness is finally achieved by two or more multiple coatings.

[0035] 2-4. High refractive index layer The high refractive index layer is a layer formed from a high refractive index treatment agent, and is a layer contained between the substrate layer and the antifouling layer, and is preferably adjacent to the antifouling layer. The refractive index of the high refractive index layer is preferably from 1.6 to 1.9, and more preferably from 1.6 to 1.8. The thickness of the high refractive index layer is preferably 50 to 250 nm, more preferably 70 to 200. If the thickness is smaller than the above range, the effect of providing the reflective layer is less likely to be obtained, whereas if the thickness is larger than the above range, the reflectance is likely to increase.

[0036] 3. High refractive index treatment agent The high refractive index treatment agent is a treatment agent for forming a high refractive index layer in the antifouling laminate of the present invention. The high refractive index treatment agent contains an alkoxytitanium compound (C) and a solvent (H2). Furthermore, the high refractive treatment agent may contain, as necessary, a wetting agent, a viscous material (thickener), a surface adjustment material, a coloring material (pigment, dye), an antistatic material, a conductivity imparting agent, an antibacterial and antiviral material, a filler such as hollow, chain-like, or porous solid silica particles, metal fine particles, etc., within a range that does not adversely affect the properties of the antifouling laminate.

[0037] The content of the alkoxytitanium compound (C) in the high refractive index treatment agent is preferably 5 to 80 mass %, more preferably 5 to 40 mass %. If it is less than the above range, the effect of providing the reflective layer is difficult to be obtained, and if it is more than the above range, cracks are likely to occur.

[0038] 3-1. Alkoxy titanium compounds (C) The alkoxytitanium compound (C) is a titanium compound having an alkoxy group. The alkoxy group can undergo hydrolysis and dehydration condensation to form a crosslinked structure.

[0039] Specific examples of the alkoxy titanium compound (C1) include tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetraoctyl titanate, titanium acetylacetonate, titanium tetraacetylacetonate, titanium ethylacetoacetate, dodecylbenzenesulfonic acid titanium compound, phosphate titanium complex, titanium octylene glycolate, titanium ethylacetoacetate, titanium lactate ammonium salt, titanium lactate, etc., or may be a compound synthesized with an oligomer or an organic monomer. Among these, tetra-n-butyl titanate or a compound similar thereto is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the alkoxytitanium compound (C).

[0040] 3-2. Solvent (H2) The solvent (H2) is not particularly limited as long as it can dissolve the alkoxytitanium compound (C), but it is preferable that it contains an alcohol-based solvent and / or a glycol-based solvent. It is also preferable that it is a non-fluorine-based solvent and does not substantially contain fluorine.

[0041] Specific examples of alcohol-based solvents include methanol (carbon number 1, boiling point 65°C), ethanol (carbon number 2, boiling point 78°C), normal propanol (carbon number 3, boiling point 97°C), isopropyl alcohol (carbon number 3, boiling point 82°C), tertiary butanol (carbon number 4, boiling point 82°C), normal butanol (carbon number 4, boiling point 118°C), isobutanol (carbon number 4, boiling point 108°C), and secondary butanol. Examples of such alcohols include n-butanol (carbon number: 4, boiling point: 100° C.), 1-pentanol (carbon number: 5, boiling point: 138° C.), 2-methyl-1-butanol (carbon number: 5, boiling point: 128° C.), 3-methyl-1-butanol (carbon number: 5, boiling point: 131° C.), 2-pentanol (carbon number: 5, boiling point: 119° C.), 1-ethyl-1-propanol (carbon number: 5, boiling point: 116° C.), and 2-methyl-2-butanol (carbon number: 5, boiling point: 102° C.). Among these, n-butanol is preferred.

[0042] Specific examples of glycol-based solvents include alkylene glycols and alkylene glycol ethers. Specific examples of alkylene glycols include ethylene glycol (carbon number 2, boiling point 197°C), propylene glycol (carbon number 3, boiling point 189°C), butylene glycol (carbon number 4, boiling point 207°C), hexylene glycol (carbon number 6, boiling point 197°C), and octylene glycol (carbon number 8, boiling point 175°C).

[0043] Specific examples of alkylene glycol ethers include ethylene glycol monomethyl ether (carbon number 3, boiling point 124°C), ethylene glycol monoethyl ether (carbon number 4, boiling point 135°C), ethylene glycol diethyl ether (carbon number 6, boiling point 121°C), ethylene glycol monoisopropyl ether (carbon number 5, boiling point 141°C), ethylene glycol monobutyl ether (carbon number 6, boiling point 171°C), propylene glycol monomethyl ether (carbon number 4, boiling point 120°C), propylene glycol monoethyl ether (carbon number 5, boiling point 132°C), propylene glycol mononormal propyl ether (carbon number 6, boiling point 149°C), and propylene glycol mononormal butyl ether (carbon number 7, boiling point 171°C). Among these, propylene glycol mononormal propyl ether is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the solvent (H2).

[0044] 3-3. Manufacturing method of high refractive index treatment agent The high refractive index treatment agent in the present invention can be prepared, for example, by the following method. The alkoxytitanium compound (C) is mixed with the solvent (H2) by stirring to dissolve it. The resulting mixture is diluted with a solvent (H2) to a concentration and viscosity appropriate for the desired coating method and coating conditions to obtain a high refractive index treatment agent. The high refractive index treatment agent may be filtered, for example, through a filter with a mesh size of 0.5 to 2 μm.

[0045] 4. Manufacturing method of antifouling laminate The stain-proof laminate of the present invention is produced by applying a stain-proofing agent onto a substrate layer, drying it, and curing it by heating. When the antifouling laminate has a high refractive index layer, it is produced by applying a high refractive index treatment agent onto a base layer, drying, and heat curing, and then applying an antifouling treatment agent onto the high refractive index layer, drying, and heat curing. An example of the application method is spray coating. In the case of spray coating, it is easy to control the surface roughness Ra of the layer formed by adjusting the coating conditions. Since the antiglare properties can be improved by adjusting the surface roughness Ra through adjustment of the coating conditions, there is no need to etch the base layer with hydrofluoric acid. EXAMPLES

[0046] <Ingredients> Tetraalkoxysilane compound 1: Silicate 40 manufactured by Tama Chemicals Co., Ltd. A mixture of ethyl polysilicate and tetraethoxysilane. Ethyl polysilicate 60-70% by mass. Fluorine-containing silane coupling agent compound 1: Triethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane. Fluorine-containing silane coupling agent compound 2: Trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane. · Alkoxy titanium compound hydrolysis condensate oligomer solution 1: Orgatics PC-200 manufactured by Matsumoto Fine Chemical Co., Ltd. Organotitanium compound solid content 31%. 90% lactic acid aqueous solution: 90% by mass L-lactic acid aqueous solution manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. PGM1: Propylene glycol monomethyl ether Fluorine-containing coating material 1: NB06-04 manufactured by Katsurayama Technology Co., Ltd. Contains fluorine-based resin and fluorine-based solvent. Degreased glass 1: A soda glass plate degreased with an alkaline detergent. 50 mm x 100 mm x 2 m thick. A commercially available soda glass plate was cleaned with a glass detergent solution (Semiclean LGL, Yokohama Resin Industries Co., Ltd.), then rinsed with water three times, water droplets on the surface were removed with an air blower, and the plate was dried in a dryer at 50°C for at least 5 minutes. Acrylic substrate 1: Acrylic resin plate, Acrylite, manufactured by Mitsubishi Chemical Corporation. 50mm x 100mm x 2m thick.

[0047] [Example 1] (Preparation of antifouling agent) The following was mixed to obtain a silane compound / ethanol solution. Tetraalkoxysilane compound 1 7.7 parts by mass Fluorine-containing silane coupling agent compound 1 0.3 parts by mass Ethanol 30 parts by weight Next, the following was mixed to obtain a nitric acid solution: 10% nitric acid aqueous solution 1.0 parts by mass Water 3.0 parts by mass Ethanol 30 parts by weight The nitric acid solution obtained above was added dropwise to the silane compound / ethanol solution obtained above, and the mixture was stirred and mixed at 40° C. for 1 hour. Next, the following was further added and mixed with stirring to obtain an antifouling treatment agent. PGM1 28.0 parts by mass

[0048] (Formation of antifouling layer) The antifouling treatment agent obtained above was spray-coated on one side of degreased glass 1 at 20°C using a precision coating machine manufactured by Apiros Co., Ltd. under the conditions described below. After preliminary drying at 20°C for 60 minutes, the glass was dried at 150°C for 30 minutes to form an antifouling layer with a thickness of 200 nm, and an antifouling laminate was obtained. The obtained antifouling laminate was subjected to various evaluations. Nozzle diameter: 0.4mm Atomization pressure: 600kPa Discharge amount: 1.0ml / min Spray distance: 40mm Head speed: 200mm / sec Pitch: 3mm

[0049] [Examples 2 to 7, Comparative Examples 1 to 4] According to the descriptions in Tables 1 to 3, antifouling treatment agents were prepared and antifouling layers were formed in the same manner as in Example 1 to obtain antifouling laminates.

[0050] [Example 8] (Preparation of antifouling agent) According to the description in Table 2, the same procedure as in Example 1 was carried out to prepare an antifouling treatment agent.

[0051] (Formation of antifouling layer 1) The stain-proofing agent obtained above was spray-coated on one side of degreased glass 1 at 20° C. under the following conditions using a precision coating machine manufactured by Apiros Co., Ltd., and no heating or drying treatment was performed. Nozzle diameter: 0.4mm Atomization pressure: 600kPa Discharge amount: 0.5ml / min Spray distance: 100mm Head speed: 200mm / sec Pitch: 3mm

[0052] (Formation of antifouling layer 2) The same antifouling treatment agent was spray-coated on the layer formed by spray coating above under the following conditions, pre-dried at 20°C for 60 minutes, and then heated and baked at 150°C for 30 minutes to form an antifouling layer with a total thickness of 550 nm, to obtain an antifouling laminate. The laminate was then evaluated in the same manner as in Example 1. Nozzle diameter: 0.4mm Atomization pressure: 600kPa Discharge amount: 1.0ml / min Spray distance: 40mm Head speed: 200mm / sec Pitch: 3mm

[0053] [Example 9] (Preparation of high refractive index treatment agent) The following were mixed to obtain a high refractive index treatment agent. Alkoxytitanium compound hydrolysis condensate oligomer solution 1 33 parts by mass PGM1 67 parts by mass

[0054] (Preparation of antifouling agent) The stain-proofing agent obtained in Example 1 was used.

[0055] (Formation of high refractive layer) The high refractive treatment agent obtained above was spray-coated on one side of degreased glass 1 at 20° C. under the following conditions using a precision coating machine manufactured by Apiros Co., Ltd., and dried at 100° C. for 30 minutes to form a high refractive layer with a thickness of 200 nm. Nozzle diameter: 1.2mm Atomization pressure: 400kPa Discharge amount: 4.0ml / min Spray distance: 60mm Head speed: 500mm / sec Pitch: 7mm

[0056] (Formation of antifouling layer) Next, the antifouling treatment agent obtained above was spray-coated on the high refractive index layer formed above using a precision coating machine manufactured by Apiros Co., Ltd. under the following conditions, and the antifouling layer was baked at 150°C for 30 minutes to form an antifouling layer with a thickness of 200 nm, thereby obtaining an antifouling laminate. The laminate was then evaluated in the same manner as in Example 1. Nozzle diameter: 0.4mm Atomization pressure: 600kPa Discharge amount: 1.0ml / min Spray distance: 40mm Head speed: 200mm / sec Pitch: 3mm

[0057] [Example 10] Except for changing the material of the substrate layer to the acrylic substrate 1, the same procedure as in Example 9 was carried out to obtain an antifouling laminate, which was then evaluated in the same manner.

[0058] <Evaluation items> [Appearance of antifouling laminate] The appearance of the prepared antifouling laminate was visually observed for the presence or absence of abnormalities. The symbols in the table have the following meanings. Passed: No abnormalities Fail: Abnormal

[0059] [Surface hardness] The surface hardness of the antifouling layer side of the prepared antifouling laminate was measured in accordance with JIS K5600-5-4:1999 "Scratch hardness (pencil method)". A hardness of 6H or more was considered to be acceptable.

[0060] [Minimum reflectance] The side of the substrate layer of the prepared antifouling laminate was painted black, and black tape was attached to prevent light from passing through the antifouling laminate. The reflectance of the surface on the antifouling layer side was measured using an ultraviolet-visible spectrophotometer (UV-2600, manufactured by Shimadzu Corporation). A reflectance of 1.5% or less was considered to be acceptable.

[0061] [Haze of antifouling laminate] The haze value of the prepared antifouling laminate was measured in accordance with JIS K7136:2000 using a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) A value of 10 or less was considered to be acceptable.

[0062] [Surface roughness Ra] The surface roughness Ra of the antifouling layer side of the prepared antifouling laminate was measured using a laser microscope LEXT OLS4100 (manufactured by Olympus Corporation). A roughness of 20 nm or less was considered to be acceptable.

[0063] [Contact angle] The contact angle with water on the surface of the antifouling layer side of the prepared antifouling laminate was measured using PCA-11 (manufactured by Kyowa Interface Science Co., Ltd.) in accordance with JIS R3257. The antifouling layer was subjected to the following abrasion treatment, and then the contact angle with water was measured in the same manner. A passing grade was 100 degrees or above. Abrasive material: Steel wool #0000 Load: 10gf Load area: 2.25cm 2 Travel width: 40mm Speed: 100mm / sec

[0064] [Refractive index] The high refractive index treatment agent was spin-coated onto a soda glass plate (refractive index 1.53), dried at 150°C for 30 minutes, and heat-cured to form a 100 nm treatment layer. The refractive index was measured using a high-speed automatic ellipsometer DVA-36L3 (manufactured by Mizojiri Optical Co., Ltd.) to obtain the refractive index of the high refractive index layer. The same procedure was carried out using an antifouling treatment agent to obtain the refractive index of the antifouling layer. Each layer was judged to pass the following criteria: Refractive index of antifouling layer: 1.2 to 1.5 Refractive index of high refractive layer: 1.5 to 1.9 Difference in refractive index between antifouling layer and high refractive index layer: 0.2 to 0.5

[0065] [Adhesion of the anti-soiling layer or high refractive layer to the substrate layer] The same antifouling treatment agent or high refractive index treatment agent as used in preparing the antifouling laminate was spray-coated on one side of the same substrate layer at 20°C as used in preparing the antifouling laminate using a precision coating machine manufactured by Apiros Co., Ltd. under the same conditions as used in preparing the antifouling laminate, and then dried at 100°C for 30 minutes to form an antifouling layer or high refractive index layer having a thickness of 200 nm. Next, a 10 x 10 grid-shaped cut (1 square is 1.0 x 1.0 mm) was made in the antifouling layer or the high refractive index layer with a utility knife, Nichiban tape was attached and peeled off, and the number of peeled squares was counted. The symbols in the table have the following meanings. Passed: No peeling Failed: Peeling occurred

[0066] [Table 1]

[0067] [Table 2]

[0068] [Table 3]

[0069] <Summary of results> The low reflection laminates of all the Examples exhibited an excellent balance of surface hardness, low reflectance, low haze, and high contact angle. In contrast, the laminates of the comparative examples showed poor results in any one of surface hardness, low reflectance, low haze, and high contact angle. For example, Comparative Example 1, in which the antifouling treatment agent reaction liquid did not contain the tetraalkoxysilane compound (E), exhibited an excessively low surface hardness. Comparative Example 2, in which the antifouling treatment reaction liquid did not contain the fluorine-containing silane coupling agent compound (G), showed a too small contact angle. Comparative Example 3, in which the antifouling treatment agent reaction liquid contained a fluorine-based solvent and the antifouling layer was too thin, showed too small haze and Ra. Comparative Example 4, in which the content of the acid or base catalyst (J) in the antifouling treatment agent reaction liquid was too low, showed too small a contact angle and surface hardness. [Industrial Applicability]

[0070] The antifouling treatment agent of the present invention can be used for transparent glass or resin used in displays, showcases, partitions, etc. for personal computers, etc., and the antifouling laminate of the present invention can be used for displays, showcases, partitions, etc. for personal computers, etc. [Explanation of symbols]

[0071] 1 Antifouling laminate 2 Base material layer 3 High refractive index layer 4. Antifouling layer

Claims

1. An antifouling treatment agent for forming an antifouling layer on a substrate layer, comprising: The stain-proofing agent contains a hydrolysis condensation product oligomer (A), an acid or base catalyst (J), and a solvent (H1), The hydrolysis condensation product oligomer (A) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D) and is soluble in the solvent (H1); The alkoxysilane compound (D) contains a tetraalkoxysilane compound (E) and a fluorine-containing silane coupling agent compound (G), The solvent (H1) is substantially free of fluorine, the content of the hydrolysis-condensation product oligomer (A) in the soil-proofing agent is 1 to 50 mass%; The content of the acid or base catalyst (J1) in the stain-proofing agent is 0.05 to 7 mass %.

2. 2. The stain-proofing treatment agent according to claim 1, wherein the mass ratio of the tetraalkoxysilane compound (E) to the fluorine-containing silane coupling agent compound (G) is 1 / 1 to 1000 / 1.

3. The stain-proofing treatment agent according to claim 1, wherein the solvent (H1) is an alcohol-based solvent and / or a glycol-based solvent.

4. An antifouling laminate having at least a base layer and an antifouling layer, The substrate layer is made of a metal oxide or a resin, The antifouling layer is made of a dried and cured product of the antifouling treatment agent according to any one of claims 1 to 3, has a layer thickness of 50 to 1000 nm, and has a surface roughness Ra of 0.1 to 20 nm; The haze of the antifouling laminate is 0.1 to 10%.

1. An antifouling laminate comprising:

5. 5. The antifouling laminate according to claim 4, wherein the antifouling layer is a multi-coated layer formed by applying the antifouling treatment agent two or more times.

6. An antifouling laminate further comprising a high refractive index layer between the substrate layer and the antifouling layer, the high refractive index layer is a layer formed from a high refractive index treatment agent, The high refractive index treatment agent contains an alkoxy titanium compound (C) and a solvent (H2), The solvent (H2) is substantially free of fluorine. The content of the alkoxy titanium compound (C) in the high refractive index treatment agent is 5 to 80 mass %, the high refractive index layer is adjacent to the antifouling layer and has a layer thickness of 50 to 1000 nm; The refractive index of the high refractive index layer is 1.5 to 1.9, The refractive index of the antifouling layer is 1.2 to 1.5, The difference in refractive index between the high refractive index layer and the antifouling layer is 0.2 to 0.

5. The stain-resistant laminate according to claim 4 .

Citation Information

Patent Citations

  • Manufacturing device for cement tile

    JP1981055215A

  • Method of manufacturing Anti-glare, Anti-reflection member

    JP2018097379A

  • Antifouling treatment method

    JP3449070B2

  • Surface treatment agents and water- and oil-repellent articles

    JP3876961B2

  • Fluorine-containing treatment composition

    WO2006046643A1