Manufacturing method of antifouling laminate
The method for forming an antifouling laminate using controlled spray coating of a specific treatment agent addresses environmental concerns and enhances durability, achieving balanced antifouling and antiglare performance.
Patent Information
- Application Number
- JP2023073196
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing antifouling and antiglare treatments for displays involve the use of hydrofluoric acid and fluorine-based solvents, leading to environmental impact, high costs, and complex layer structures, while lacking in scratch resistance and abrasion resistance.
A manufacturing method for an antifouling laminate involving a base material layer and an antifouling layer formed by spray coating a specific antifouling treatment agent under controlled conditions, using a hydrolyzed condensate oligomer, alkoxysilane compound, and solvent without fluorine, with precise adjustments for surface roughness and haze.
The method produces a laminate with a simple structure, excellent antifouling and antiglare properties, low reflectivity, and high scratch and abrasion resistance, while minimizing environmental impact.
Smart Images

Figure 2024158205000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an antifouling laminate which has a small environmental load, excellent manufacturability, and a simple layer structure while having an excellent balance of antifouling properties, antiglare properties, low reflectivity, scratch resistance, and abrasion resistance. [Background technology]
[0002] 2. Description of the Related Art Displays for personal computers and the like are generally provided with an anti-stain layer and an anti-glare layer to prevent stains and light reflection. Anti-glare treatment for forming an anti-glare layer often involves etching the glass with hydrofluoric acid or the like to create irregularities, but this places a heavy burden on the environment as it produces fluorine-based waste liquid. Antifouling layers are generally formed on an antiglare layer or an antireflection layer by spraying a treatment agent that contains a fluorine-based silane coupling agent to adhere to the substrate and to impart water repellency. However, since fluorine-based silane coupling agents are poorly compatible with general solvents, they must be diluted with a fluorine-based solvent before use, which places a heavy burden on the environment and is very expensive (Patent Documents 1 to 4). Anti-glare treatment may involve forming unevenness by spray coating, and an anti-reflection layer or an anti-fouling layer is often formed on top of this (Patent Document 5). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3449070 [Patent Document 2] Patent No. 5655215 [Patent Document 3] Patent No. 3876961 [Patent Document 4] WO2006-046643 [Patent Document 5] JP 2018-097379 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention aims to provide a method for producing an antifouling laminate which does not use hydrofluoric acid or a fluorine-based solvent, has a small environmental impact, is excellent in manufacturability, and has a simple layer structure while having an excellent balance of antifouling properties, antiglare properties, low reflectivity, scratch resistance, and abrasion resistance. [Means for solving the problem]
[0005] As a result of various investigations, the inventors have found that the above-mentioned object can be achieved by a manufacturing method in which an antifouling layer is formed by spray coating a specific antifouling treatment agent under specific conditions, thereby producing an antifouling laminate having at least a base layer and an antifouling layer. That is, the present invention is characterized in the following points. 1. A method for producing an antifouling laminate having at least a substrate layer and an antifouling layer, comprising the steps of: The production method includes the following antifouling layer-forming step, adjusting the surface roughness Ra of the antifouling layer to 0.1 to 20 nm and the haze of the antifouling laminate to 0.3 to 10%, antifouling layer forming step: a step of applying an antifouling treatment agent onto the base layer, drying and heat curing the agent to form the antifouling layer; Base material layer temperature: 0~120℃, Antifouling treatment agent application method: spray coat, Antifouling treatment agent application conditions Nozzle diameter: 0.1 to 10 mm Atomization pressure: 150~700kPa Discharge amount: 0.5~20ml / min Spray distance: 10~200mm Head speed: 50~500mm / sec Pitch: 0.5~10mm Pre-drying and heat curing conditions for the stain-resistant layer: 10 to 100°C, 30 to 90 minutes, Drying and heat curing conditions for the stain-resistant layer: 120 to 180°C, 10 to 60 minutes, Antifouling layer thickness: 50-1000 nm, The stain-proofing agent contains a hydrolysis-condensation product oligomer (A), an acid or base catalyst (J), and a solvent (H), The hydrolysis condensation product oligomer (A) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D) and is soluble in the solvent (H1); The alkoxysilane compound (D) contains a tetraalkoxysilane compound (E) and a fluorine-containing silane coupling agent compound (G), The solvent (H) is substantially free of fluorine, the content of the hydrolysis-condensation product oligomer (A) in the soil-proofing agent is 1 to 50 mass%; The content of the acid or base catalyst (J) in the stain-proofing agent is 0.05 to 7 mass%. A manufacturing method comprising the steps of: 2. The method according to the above item 1, wherein the mass ratio of the tetraalkoxysilane compound (E) / fluorine-containing silane coupling agent compound (G) is 1 / 1 to 1000 / 1. 3. The manufacturing method according to 1 or 2 above, wherein the solvent (H) is an alcohol-based solvent and / or a glycol-based solvent. 4. The method according to any one of 1 to 3 above, wherein the antifouling layer is formed by applying the antifouling treatment agent two or more times. 5. The method according to any one of 1 to 3 above, wherein the base layer is a layer made of a metal oxide or a resin film having a haze of 0 to 0.3%. 6. The method according to 4 above, wherein the substrate layer is a layer made of a metal oxide or a resin film having a haze of 0 to 0.3%. Effect of the Invention
[0006] The manufacturing method of the present invention makes it possible to produce an antifouling laminate that has a simple layer structure, excellent manufacturability, and an excellent balance of transparency, antifouling property, antiglare property, low reflectivity, scratch resistance, and abrasion resistance, without using a fluorine-based solvent or hydrofluoric acid, and with a small environmental impact. [Brief description of the drawings]
[0007] [Figure 1] 1 is a cross-sectional view of an antifouling laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1. Manufacturing method of antifouling laminate The production method of the present invention is a production method for an antifouling laminate having at least a substrate layer and an antifouling layer, and is a production method including a step of forming an antifouling layer. According to the production method of the present invention, it is possible to obtain an antifouling laminate in which the thickness of the antifouling layer is adjusted to 50 to 1000 nm, the surface roughness Ra of the antifouling layer is adjusted to 0.1 to 20 nm, and the haze of the antifouling laminate is adjusted to 0.3 to 10%. The antifouling layer forming step is a step in which an antifouling treatment agent is applied onto a base layer, and then dried and heat-cured to form an antifouling layer.
[0009] In the production method of the present invention, the antifouling layer may be formed by single-layer coating in which the antifouling treatment agent is applied only once, or by multiple coating in which the antifouling treatment agent is applied two or more times. By forming the antifouling layer by multiple coating, the antiglare property of the antifouling laminate is improved. There is no particular limitation on the thickness of the film formed by each coating in the multiple coating process, as long as the film finally has the above-mentioned thickness by two or more multiple coating processes.
[0010] In the case of multiple coating, it is preferable to coat the same antifouling treatment agent multiple times. Furthermore, a drying step or a heat curing step may or may not be performed between each of the multiple coatings. Each application is preferably performed with the same nozzle. By applying multiple coats of the same soil-repellent treatment agent using the same nozzle, with only the machine settings changed, and without drying between coats, loss of raw materials and time due to liquid changes, nozzle changes, and drying is reduced, improving productivity.
[0011] 1-2. When forming an antifouling layer by single layer coating When the antifouling treatment agent is applied in a single layer, the temperature of the substrate layer is preferably 0 to 120° C., and more preferably 20 to 100° C. If the temperature is higher than the above range, the haze tends to decrease, and if the temperature is higher than the above range, the contact angle tends to decrease.
[0012] The method of applying the stain-proofing agent is preferably spray coating, spin coating, or roll coating, with spray coating being more preferred in that the surface roughness Ra can be easily adjusted. Since the antiglare properties can be improved by adjusting the surface roughness Ra through adjustment of the coating conditions, there is no need to etch the base layer with hydrofluoric acid. The conditions for applying the stain-proofing agent by spray coating include the nozzle diameter, atomization pressure, discharge amount, spray distance, head speed, pitch, and the like.
[0013] The nozzle diameter is preferably 0.1 to 10 mm, and more preferably 0.1 to 2.0 mm. If it is smaller than the above range, the ejection stability decreases, and if it is larger than the above range, the ejection stability decreases.
[0014] The atomization pressure is preferably 150 to 700 kPa, and more preferably 400 to 600 kPa. If it is lower than the above range, glare is likely to occur, and if it is higher than the above range, the ejection stability decreases.
[0015] The discharge amount is preferably 0.5 to 20 ml / min, more preferably 0.5 to 5 ml / min. If it is less than the above range, the discharge stability decreases, and if it is more than the above range, coating unevenness is likely to occur.
[0016] The spray distance is preferably 10 to 200 mm, more preferably 40 to 120 mm. If it is closer than the above range, uneven coating is likely to occur, and if it is farther than the above range, uneven coating is likely to occur.
[0017] The head speed is preferably 50 to 500 mm / sec, more preferably 100 to 400 mm / sec. If it is slower than the above range, the productivity decreases, and if it is faster than the above range, uneven coating tends to occur.
[0018] The pitch is preferably 0.5 to 10 mm, more preferably 1.0 to 5.0 mm. If it is smaller than the above range, the productivity decreases, and if it is larger than the above range, uneven coating tends to occur.
[0019] The applied antifouling layer is pre-dried and heat-cured at a low temperature, and then fully dried and heat-cured at a high temperature. The pre-drying and heat-curing conditions are preferably 10 to 100°C for 30 to 90 minutes, and more preferably 15 to 50°C for 30 to 60 minutes. If the temperature is lower than the above range, the hardness is likely to decrease, and if the temperature is higher than the above range, the durability is likely to decrease. Also, if the temperature is shorter than the above range, the durability is likely to decrease, and if the temperature is longer than the above range, the hardness is likely to decrease. The main drying and heat curing conditions are preferably 100-200°C for 10-60 minutes, and more preferably 120-180°C for 20-40 minutes. If the temperature is lower than the above range, the hardness is likely to decrease, and if the temperature is higher than the above range, the contact angle is likely to decrease. Also, if the temperature is shorter than the above range, the hardness is likely to decrease, and if the temperature is longer than the above range, the contact angle is likely to decrease.
[0020] 1-2. When antifouling layer is formed by multiple coating When the antifouling treatment agent is applied in multiple layers, the temperature of the substrate layer is preferably 0 to 120° C., and more preferably 20 to 100° C. If the temperature is higher than the above range, the haze tends to decrease, and if the temperature is higher than the above range, the contact angle tends to decrease.
[0021] When the stain-proofing agent is applied in multiple layers, the application method is preferably spray coating, spin coating, or roll coating, and spray coating is more preferable in that the surface roughness Ra can be easily adjusted. The conditions for multiple application of the stain-proofing agent by spray coating include the nozzle diameter, atomization pressure, discharge amount, spray distance, head speed, pitch, and the like.
[0022] The nozzle diameter is preferably 0.1 to 10 mm, and more preferably 0.1 to 2.0 mm. If it is smaller than the above range, the ejection stability decreases, and if it is larger than the above range, the ejection stability decreases.
[0023] The atomization pressure is preferably 150 to 700 kPa, and more preferably 400 to 600 kPa. If it is lower than the above range, glare is likely to occur, and if it is higher than the above range, the ejection stability decreases.
[0024] The discharge amount is preferably 0.5 to 20 ml / min, more preferably 0.5 to 5 ml / min. If it is less than the above range, the discharge stability decreases, and if it is more than the above range, coating unevenness is likely to occur.
[0025] The spray distance is preferably 10 to 200 mm, more preferably 40 to 120 mm. If it is closer than the above range, uneven coating is likely to occur, and if it is farther than the above range, uneven coating is likely to occur.
[0026] The head speed is preferably 50 to 500 mm / sec, more preferably 100 to 400 mm / sec. If it is slower than the above range, the productivity decreases, and if it is faster than the above range, uneven coating tends to occur.
[0027] The pitch is preferably 0.5 to 10 mm, more preferably 1.0 to 5.0 mm. If it is smaller than the above range, the productivity decreases, and if it is larger than the above range, uneven coating tends to occur.
[0028] The applied antifouling layer is pre-dried and heat-cured at a low temperature, and then fully dried and heat-cured at a high temperature. The pre-drying and heat-curing conditions are preferably 10 to 100°C for 30 to 90 minutes, and more preferably 15 to 50°C for 30 to 60 minutes. If the temperature is lower than the above range, the hardness is likely to decrease, and if the temperature is higher than the above range, the durability is likely to decrease. Also, if the temperature is shorter than the above range, the durability is likely to decrease, and if the temperature is longer than the above range, the hardness is likely to decrease. The main drying and heat curing conditions are preferably 100-200°C for 10-60 minutes, and more preferably 120-180°C for 20-40 minutes. If the temperature is lower than the above range, the hardness is likely to decrease, and if the temperature is higher than the above range, the contact angle is likely to decrease. Also, if the temperature is shorter than the above range, the hardness is likely to decrease, and if the temperature is longer than the above range, the contact angle is likely to decrease.
[0029] 2. Antifouling laminate The antifouling laminate produced by the manufacturing method of the present invention is a laminate having at least a base layer and an antifouling layer, and while having a simple layer structure, has an excellent balance of transparency, antifouling properties, antiglare properties, low reflectivity, scratch resistance, and abrasion resistance. In order for the antifouling laminate of the present invention to have excellent transparency, the haze of the antifouling laminate is preferably from 0.1 to 10%, more preferably from 0.3 to 5.0%.
[0030] 2-1. Base material layer The substrate layer is an object to be coated with the stain-proofing agent of the present invention. The substrate layer is preferably made of a metal oxide or a resin, and in order for the antifouling laminate to have transparency, it is more preferably made of a highly transparent metal oxide or resin, and even more preferably made of a transparent metal oxide such as soda glass.
[0031] The metal oxide contained in the substrate layer may be ceramic, glass, or the like. Examples of the substrate that uses glass include a glass plate and a glass cloth. Specific examples of the resin contained in the substrate layer include PMMA, PC, PET, etc. Among these, PMMA is preferable.
[0032] The thickness of the substrate layer is not particularly limited, but is preferably 0.1 to 5.0 mm. The surface of the base layer may be subjected to an antiglare treatment (AG treatment), and the surface roughness Ra is preferably 0.5 to 20 nm as a result of the antiglare treatment. In order to set the haze of the antifouling laminate to 0.1 to 10%, the haze of the base layer is preferably 0.1 to 10%.
[0033] 2-2.Anti-stain layer The stain-proofing layer in the present invention is a layer formed from the stain-proofing agent of the present invention, and is preferably made of a cured product of the hydrolysis condensation product oligomer (A).
[0034] The thickness of the antifouling layer is preferably 50 to 1000 nm, more preferably 70 to 800 nm. If the thickness is thinner than the above range, the effect of providing the antifouling layer is not easily obtained, and if the thickness is thicker than the above range, cracks are easily generated. The surface roughness Ra of the antifouling layer is preferably 0.1 to 20 nm, more preferably 0.5 to 1.5 nm. If it is smaller than the above range, it is difficult to obtain Ra, and if it is larger than the above range, the haze tends to increase.
[0035] The antifouling layer is preferably a multi-coated layer formed by applying an antifouling treatment agent two or more times. The antifouling layer being a multi-coated layer improves antiglare properties. The antifouling layer is preferably a layer in which the same antifouling treatment agent is applied in multiple layers. In addition, a drying step or a heat curing step may or may not be included between the coating steps. There is no particular limitation on the thickness of the antifouling layer formed by a single coating, and it is sufficient that the above-mentioned thickness is finally achieved by two or more multiple coatings.
[0036] 3. Antifouling agent The antifouling treatment agent of the present invention is a treatment agent for forming an antifouling layer on the substrate layer in the antifouling laminate of the present invention. The stain-proofing agent of the present invention contains a hydrolysis-condensation oligomer (A) and a solvent (H) that is substantially free of fluorine, and may further contain an acid or base catalyst (J1) to promote the hydrolysis-condensation reaction. Furthermore, the antifouling treatment agent may contain, as necessary, a wetting agent, a viscous material (thickener), a surface conditioning material, a coloring material (pigment, dye), an antistatic material, a conductivity imparting agent, an antibacterial and antiviral material, a filler such as hollow, chain-like, or porous solid silica particles, metal fine particles, and the like, within a range that does not adversely affect the properties of the antifouling laminate. The antifouling treatment agent preferably has excellent storage stability. For example, when stored at 40°C for 3 months in a stationary state, it is preferable that there is no change in appearance and that the increase in molecular weight is 0 to 100%, and more preferably 0 to 50%.
[0037] 3-1. Hydrolysis condensation product oligomer (A) This hydrolysis condensation oligomer (A) is a hydrolysis condensation oligomer of an alkoxysilane compound (D) and is soluble in a solvent (H). The content of the hydrolysis condensate oligomer (A) in the soil-proofing agent is preferably from 1 to 80 mass %, more preferably from 2 to 40 mass %.
[0038] 3-2. Alkoxysilane compounds (D) The alkoxysilane compound (D) contains a tetraalkoxysilane compound (E) and a fluorine-containing silane coupling agent compound (G). The fluorine-containing silane coupling agent compound (G) is poorly compatible with organic components such as other resins and solvents, but by forming a hydrolysis condensation oligomer with the tetraalkoxysilane compound (E), it becomes easier to make it compatible with organic components such as other resins and solvents.
[0039] The mass ratio of the tetraalkoxysilane compound (E) / fluorine-containing silane coupling agent compound (G) is preferably 1 / 1 to 1000 / 1, more preferably 4 / 1 to 50 / 1. If it is smaller than the above range, the hardness is likely to be inferior, and if it is larger than the above range, the water contact angle is likely to be inferior.
[0040] 3-3. Tetraalkoxysilane compounds (E) The tetraalkoxysilane compound (E) is a silane compound having four alkoxy groups. The alkoxy group undergoes a hydrolysis reaction and a dehydration condensation reaction to form a crosslinked structure.
[0041] Specific examples of the tetraalkoxysilane compound (E) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, and oligomers thereof. Among these, tetraethoxysilane and its oligomers are preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the tetraalkoxysilane compound (E).
[0042] 3-4. Fluorine-containing silane coupling agent compounds (G) The fluorine-containing silane coupling agent compound (G) is a silane compound having a functional group capable of reacting with an organic component, a fluorine group and an alkoxy group. The functional group capable of reacting with an organic component has the effect of adjusting the refractive index.
[0043] Specific examples of the fluorine-containing silane coupling agent compound (G) include trifluoropropyltrimethoxysilane, dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, trimethoxy(1H,1H,2H,2H-perfluorohexyl)silane, triethoxy(1H,1H,2H,2H-perfluorohexyl)silane, trimethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane, triethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane, triethoxy[5,5,6,6,7,7,7-heptafluoro-4,4-bis(trifluoromethyl)heptyl]silane, trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane, and triethoxy-1H,1H,2H,2H-heptadecafluorodecylsilane. Of these, trimethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the fluorine-containing silane coupling agent compound (G).
[0044] 3-5. Acid or Base Catalysts (J) The acid or base catalyst (J) is a component that promotes the hydrolysis reaction and dehydration condensation reaction of the alkoxysilane compound (D) and the hydrolysis condensate oligomer (A). The content of the acid or base catalyst (J) in the stain-proofing agent is preferably 0.05 to 10 mass%, more preferably 0.1 to 5.0 mass%. If it is less than the above range, the promotion effect is likely to be insufficient, and if it is more than the above range, it is likely to be difficult to ensure uniform reaction progress.
[0045] Specific examples of the acid catalyst include hydrochloric acid, sulfuric acid, nitric acid, p-toluenesulfonic acid, benzenesulfonic acid, 10-camphorsulfonic acid, formic acid, oxalic acid, acetic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, and lactic acid. Specific examples of the base catalyst include triethyleneamine, dimethylaminoethanol, and aqueous ammonia. Of these, nitric acid is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the acid or base catalyst (J).
[0046] 3-6. Solvent (H) The solvent (H1) is not particularly limited as long as it can dissolve the hydrolysis condensation product oligomer (A), but it is preferable that the solvent (H1) contains an alcohol-based solvent and / or a glycol-based solvent, and is preferably a non-fluorine-based solvent.
[0047] The solvent (H) not only serves as a solvent for the hydrolysis condensate oligomer (A), but also plays an important role in forming a coating film having an uneven shape during application, particularly during spray application.
[0048] The stain-proofing agent forms a roughened shape due to the evaporation of the solvent (H) that accompanies application to the base layer. Therefore, if the solvent (H) evaporates quickly, the film formation state will be poor and a coating film with large irregularities will be formed. Conversely, if the evaporation rate of the solvent (H) is slow, the film will be in a good condition, but the unevenness will be too small, and sufficient antiglare properties will not be achieved. Furthermore, during the main curing, the residual solvent (H) evaporates, which may cause the stain-resistant layer to shrink significantly and crack.
[0049] When using a solvent that evaporates slowly, it is effective to mix a large amount of a solvent with a low boiling point or to reduce the spray discharge amount, coating speed, atomization pressure, etc. To speed up the evaporation, the substrate may be preheated to about 100°C.
[0050] Specific examples of alcohol-based solvents include methanol (carbon number 1, boiling point 65°C), ethanol (carbon number 2, boiling point 78°C), normal propanol (carbon number 3, boiling point 97°C), isopropyl alcohol (carbon number 3, boiling point 82°C), tertiary butanol (carbon number 4, boiling point 82°C), normal butanol (carbon number 4, boiling point 118°C), isobutanol (carbon number 4, boiling point 108°C), and secondary butanol. Examples of the alcohol include ethanol (carbon number: 4, boiling point: 100° C.), 1-pentanol (carbon number: 5, boiling point: 138° C.), 2-methyl-1-butanol (carbon number: 5, boiling point: 128° C.), 3-methyl-1-butanol (carbon number: 5, boiling point: 131° C.), 2-pentanol (carbon number: 5, boiling point: 119° C.), 1-ethyl-1-propanol (carbon number: 5, boiling point: 116° C.), and 2-methyl-2-butanol (carbon number: 5, boiling point: 102° C.). Among these, ethanol is preferred.
[0051] Specific examples of glycol-based solvents include alkylene glycols and alkylene glycol ethers. Specific examples of alkylene glycols include ethylene glycol (carbon number 2, boiling point 197°C), propylene glycol (carbon number 3, boiling point 189°C), butylene glycol (carbon number 4, boiling point 207°C), hexylene glycol (carbon number 6, boiling point 197°C), and octylene glycol (carbon number 8, boiling point 175°C).
[0052] Specific examples of alkylene glycol ethers include ethylene glycol monomethyl ether (carbon number 3, boiling point 124°C), ethylene glycol monoethyl ether (carbon number 4, boiling point 135°C), ethylene glycol diethyl ether (carbon number 6, boiling point 121°C), ethylene glycol monoisopropyl ether (carbon number 5, boiling point 141°C), ethylene glycol monobutyl ether (carbon number 6, boiling point 171°C), propylene glycol monomethyl ether (carbon number 4, boiling point 120°C), propylene glycol monoethyl ether (carbon number 5, boiling point 132°C), propylene glycol mono-normal propyl ether (carbon number 6, boiling point 149°C), and propylene glycol mono-normal butyl ether (carbon number 7, boiling point 171°C). Among these, propylene glycol monomethyl ether is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the solvent (H).
[0053] 3-7. Manufacturing method of antifouling agent The stain-proofing agent of the present invention can be prepared, for example, by the following method. 1) Preparation of silane compound solution The alkoxysilane compound (D) and the fluorine-containing silane coupling agent compound (G) are dissolved in a solvent (H) to obtain a silane compound solution. 2) Preparation of catalyst solution Also, an acid or base catalyst (J) is added dropwise to the solvent (H) and mixed to obtain a catalyst solution. 3) Preparation of antifouling agent The catalyst solution obtained above is added dropwise to the silane compound solution obtained above while stirring and mixing to produce a hydrolysis condensation oligomer (A). The temperature of the mixture is preferably adjusted to between 10 and 60° C. in order to suppress the hydrolysis condensation reaction. After the dropwise addition is completed, the mixture is left to stand at a constant temperature of 20 to 40° C. to allow the hydrolysis and condensation reaction to proceed to a desired reaction rate. The obtained reaction liquid is diluted with a solvent (H) to a concentration and viscosity appropriate for the desired coating method and coating conditions to obtain an antifouling treatment agent. The antifouling treatment agent may be filtered, for example, through a filter having a mesh size of 0.5 to 2 μm. EXAMPLES
[0054] <Ingredients> Tetraalkoxysilane compound 1: Silicate 40 manufactured by Tama Chemicals Co., Ltd. A mixture of ethyl polysilicate and tetraethoxysilane. Ethyl polysilicate 60-70% by mass. Fluorine-containing silane coupling agent compound 1: Triethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane. Fluorine-containing silane coupling agent compound 2: Trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane. 90% lactic acid aqueous solution: 90% by mass L-lactic acid aqueous solution manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. PGM1: Propylene glycol monomethyl ether Fluorine-containing coating material 1: NB06-04 manufactured by Katsurayama Technology Co., Ltd. Contains fluorine-based resin and fluorine-based solvent. Degreased glass 1: A soda glass plate degreased with an alkaline detergent. 50 mm x 100 mm x 2 m thick. A commercially available soda glass plate was cleaned with a glass detergent solution (Semiclean LGL, Yokohama Resin Industries Co., Ltd.), then rinsed with water three times, water droplets on the surface were removed with an air blower, and the plate was dried in a dryer at 50°C for at least 5 minutes.
[0055] [Example 1] (Preparation of antifouling agent) The following was mixed to obtain a silane compound / ethanol solution. Tetraalkoxysilane compound 1 7.7 parts by mass Fluorine-containing silane coupling agent compound 1 0.3 parts by mass Ethanol 30 parts by weight Next, the following was mixed to obtain a nitric acid solution: 10% nitric acid aqueous solution 1.0 parts by mass Water 3.0 parts by mass Ethanol 30 parts by weight The nitric acid solution obtained above was added dropwise to the silane compound / ethanol solution obtained above, while stirring and mixing at 40° C. for 1.5 hours. Next, the following was further added and mixed with stirring to obtain an antifouling treatment agent. PGM1 28.0 parts by mass
[0056] (Formation of antifouling layer) The antifouling treatment agent obtained above was spray-coated on one side of degreased glass 1 at 20°C using a precision coating machine manufactured by Apiros Co., Ltd. under the conditions described below. After pre-drying at 20°C for 60 minutes, the glass was dried at 150°C for 30 minutes to form an antifouling layer having a thickness of 200 nm. Nozzle diameter: 0.4mm Atomization pressure: 600kPa Discharge amount: 0.5ml / min Spray distance: 100mm Head speed: 200mm / sec Pitch: 3mm
[0057] [Examples 2 to 5, Comparative Examples 1 to 5] According to the descriptions in Tables 1 and 2, antifouling treatment agents were prepared in the same manner as in Example 1, and antifouling layers were formed to prepare antifouling laminates.
[0058] [Example 6] (Preparation of antifouling agent) According to the description in Table 1, the same procedure as in Example 1 was carried out to prepare an antifouling treatment agent.
[0059] (Formation of antifouling layer 1) The stain-proofing agent obtained above was spray-coated on one side of degreased glass 1 at 20° C. under the following conditions using a precision coating machine manufactured by Apiros Co., Ltd., and no heating or drying treatment was performed. Nozzle diameter: 0.4mm Atomization pressure: 600kPa Discharge amount: 0.5ml / min Spray distance: 100mm Head speed: 200mm / sec Pitch: 3mm
[0060] (Formation of antifouling layer 2) The same antifouling treatment agent was then spray-coated on the layer formed by spray coating above under the conditions described below, and after pre-drying at 20°C for 60 minutes, it was heated and baked at 150°C for 30 minutes to form an antifouling layer with a total thickness of 550 nm. Nozzle diameter: 0.4mm Atomization pressure: 600kPa Discharge amount: 1.0ml / min Spray distance: 40mm Head speed: 200mm / sec Pitch: 3mm
[0061] <Evaluation items> [Appearance of antifouling laminate] The appearance of the prepared antifouling laminate was visually observed for the presence or absence of abnormalities. The symbols in the table have the following meanings. 〇: No abnormalities ×: Abnormal
[0062] [Surface hardness] The surface hardness of the antifouling layer side of the prepared antifouling laminate was measured in accordance with "4.4 Scratch hardness (pencil method)" of JIS K5600 general coating test method. A hardness of 6H or more was considered to be acceptable.
[0063] [Haze of antifouling laminate] The haze value of the prepared antifouling laminate was measured in accordance with JIS K7136:2000 using a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) A haze value of 10% or less was considered to be acceptable.
[0064] [Surface roughness Ra] The surface roughness Ra of the antifouling layer side of the prepared antifouling laminate was measured using a laser microscope LEXT OLS4100 (manufactured by Olympus Corporation). A roughness of 20 nm or less was considered to be acceptable.
[0065] [Contact angle] The contact angle with water on the surface of the antifouling layer side of the prepared antifouling laminate was measured using PCA-11 (manufactured by Kyowa Interface Science Co., Ltd.) in accordance with JIS R3257. The antifouling layer was subjected to the following abrasion treatment, and then the contact angle with water was measured in the same manner. A passing grade was 100 degrees or above. Abrasive material: Steel wool #0000 Load: 10gf Load area: 2.25cm 2 Travel width: 40mm Speed: 100mm / sec
[0066] [Table 1]
[0067] [Table 2]
[0068] <Summary of Results> The antifouling laminates of all the Examples exhibited an excellent balance of surface hardness, low haze, and high contact angle. For example, in Example 6, compared with Example 1, the haze increased and the antiglare properties improved. In contrast, the laminates of the comparative examples showed poor results in any one of surface hardness, low haze, and high contact angle. For example, Comparative Example 1, in which the antifouling treatment agent reaction liquid did not contain the tetraalkoxysilane compound (E), exhibited an excessively low surface hardness. Comparative Example 2, in which the antifouling treatment reaction liquid did not contain the fluorine-containing silane coupling agent compound (G), showed a too small contact angle. Comparative Example 3, in which the coating conditions were not suitable, showed too small a haze and Ra because the discharge amount was too small. Comparative Example 4, in which the antifouling treatment agent reaction liquid contained a fluorine-based solvent and the antifouling layer was too thin, showed too small haze and Ra. Comparative Example 5, in which the content of the acid or base catalyst (J) in the antifouling treatment agent reaction liquid was too low, showed too small a contact angle and surface hardness. [Industrial Applicability]
[0069] The manufacturing method of the present invention makes it possible to produce an antifouling laminate having an excellent balance of antifouling properties, antiglare properties, low reflectivity, scratch resistance, and abrasion resistance in a short period of time without using fluorinated solvents or hydrofluoric acid, with little environmental impact, and is therefore extremely useful industrially in terms of both performance and the environment. [Explanation of symbols]
[0070] 1 Antifouling laminate 2 Base material layer 3. Antifouling layer
Claims
1. A method for producing an antifouling laminate having at least a substrate layer and an antifouling layer, comprising the steps of: The production method includes the following antifouling layer-forming step, which adjusts the surface roughness Ra of the antifouling layer to 0.1 to 20 nm and the haze of the antifouling laminate to 0.3 to 10%, antifouling layer forming step: a step of applying an antifouling treatment agent onto the base layer, drying and heat curing the agent to form the antifouling layer; Base material layer temperature: 0 to 120°C, Antifouling treatment agent application method: spray coat, Antifouling treatment agent application conditions Nozzle diameter: 0.1 to 10 mm Atomization pressure: 150 to 700 kPa Discharge amount: 0.5-20ml / min Spray distance: 10-200mm Head speed: 50 to 500 mm / sec Pitch: 0.5 to 10 mm Pre-drying and heat curing conditions for the stain-resistant layer: 10 to 100°C, 30 to 90 minutes, Drying and heat curing conditions for the stain-resistant layer: 120 to 180°C, 10 to 60 minutes, Antifouling layer thickness: 50 to 1000 nm, The stain-proofing agent contains a hydrolysis-condensation product oligomer (A), an acid or base catalyst (J), and a solvent (H), The hydrolysis condensation product oligomer (A) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D) and is soluble in the solvent (H1); The alkoxysilane compound (D) contains a tetraalkoxysilane compound (E) and a fluorine-containing silane coupling agent compound (G), The solvent (H) is substantially free of fluorine, the content of the hydrolysis-condensation product oligomer (A) in the soil-proofing agent is 1 to 50 mass%; The content of the acid or base catalyst (J) in the stain-proofing agent is 0.05 to 7 mass%. A manufacturing method comprising the steps of:
2. The method according to claim 1, characterized in that the mass ratio of the tetraalkoxysilane compound (E) to the fluorine-containing silane coupling agent compound (G) is 1 / 1 to 1000 / 1.
3. The method according to claim 1 , wherein the solvent (H) is an alcohol-based solvent and / or a glycol-based solvent.
4. The method according to any one of claims 1 to 3, wherein the antifouling layer is formed by applying the antifouling treatment agent two or more times.
5. 4. The method according to claim 1, wherein the substrate layer is a layer made of a metal oxide or a resin film having a haze of 0 to 0.3%.
6. 5. The method according to claim 4, wherein the substrate layer is a layer made of a metal oxide or a resin film having a haze of 0 to 0.3%.
Citation Information
Patent Citations
Manufacturing device for cement tile
JP1981055215A
Method of manufacturing Anti-glare, Anti-reflection member
JP2018097379A
Antifouling treatment method
JP3449070B2
Surface treatment agents and water- and oil-repellent articles
JP3876961B2
Fluorine-containing treatment composition
WO2006046643A1