Coating filler, coating composition, method for producing coating composition, coating film, article and method for producing article having coating film

Flat glass fibers with specific dimensions address the issue of hardness and gloss loss in paint films by enhancing both properties simultaneously.

JP2024158212APending Publication Date: 2024-11-08CENT GLASS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023073219
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The use of glass fibers in paint compositions improves hardness but leads to a decrease in appearance and gloss due to the fibers protruding on the surface of the paint film.

Method used

Employing flat glass fibers with a specific median fiber length and cross-sectional shape, measured by the Coulter Counter method, to enhance hardness while minimizing the deterioration in appearance and gloss.

Benefits of technology

The use of flat glass fibers with controlled dimensions maintains paint film hardness while preserving gloss and appearance, achieving a smoother and more durable coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158212000001_ABST
    Figure 2024158212000001_ABST
Patent Text Reader

Abstract

To provide a coating filler capable of improving hardness while suppressing lowering of appearance and glossiness of a coating film, a coating composition using the coating filler, a method for producing the coating composition, a coating film formed by the coating composition, an article having the coating film and a method for producing the article having the coating film.SOLUTION: A coating filler includes glass fiber, and the glass fiber has a flat cross-sectional shape in a cross section perpendicular to a longitudinal direction, and the median fiber length of the glass fiber determined by the Coulter Counter method, is 0.025 mm-0.24 mm.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a paint filler, a paint composition using the paint filler, a method for producing the paint composition, a coating film formed from the paint composition, an article having the coating film, and a method for producing an article having the coating film. [Background technology]

[0002] It is known that the strength, hardness, scratch resistance, etc. of the coating film can be improved by adding an inorganic filler to the coating, and glass fiber in particular is considered to have a large reinforcing effect (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 50-25485 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of the investigations by the present inventors, it has become clear that, although the hardness of the coating film is improved when glass fibers are added to a paint, the glass fibers protrude to the surface of the coating film, causing problems such as a poor appearance of the coating film and a decrease in gloss of the coating film. Thus, as a result of the investigations by the present inventors, it has been newly discovered that, although the hardness is improved when glass fibers are used as a paint filler, the appearance and gloss of the coating film are decreased.

[0005] The present disclosure aims to solve the above-mentioned problems newly discovered by the present inventors, and to provide a paint filler that can improve hardness while suppressing deterioration in the appearance and gloss of a coating film, a coating composition using the paint filler, a method for producing the coating composition, a coating film formed from the coating composition, an article having the coating film, and a method for producing an article having the coating film. [Means for solving the problem]

[0006] As the glass fiber, as described in Patent Document 1, a glass fiber (also referred to as a normal glass fiber) having a circular cross-sectional shape perpendicular to the longitudinal direction is usually used. As a result of intensive research, the present inventors have found that by using a glass fiber (also referred to as a flat glass fiber) having a flat cross-sectional shape perpendicular to the longitudinal direction instead of a normal glass fiber, and further by using milled fiber (MF) obtained by pulverizing the flat glass fiber, the hardness can be improved while suppressing the deterioration of the appearance and gloss of the coating film. As a result of further intensive research on the use of MF, the present inventors have found that the above problem can be solved by a flat glass fiber having a median fiber length in a specific range as measured by the Coulter Counter method. That is, the present disclosure (1) relates to a paint filler, the filler containing glass fiber, the glass fiber having a flat cross-sectional shape perpendicular to the longitudinal direction, and the median fiber length of the glass fiber as measured by the Coulter Counter method being 0.025 mm to 0.24 mm.

[0007] The present disclosure (2) relates to the paint filler according to the present disclosure (1), wherein the cross-sectional shape has an average flattening ratio of 2.0 to 8.0 and an average circular equivalent fiber diameter of 0.0045 mm to 0.034 mm.

[0008] The present disclosure (3) relates to the paint filler according to the present disclosure (2), wherein the average flattening ratio of the cross-sectional shape is 3.0 to 6.0.

[0009] The present disclosure (4) relates to the paint filler according to any one of the present disclosures (1) to (3), in which the coefficient of variation of the circular equivalent fiber diameter of the cross-sectional shape is 10% or less.

[0010] The present disclosure (5) relates to the paint filler according to any one of the present disclosures (1) to (4), wherein the coefficient of variation of the flattening of the cross-sectional shape is 20% or less.

[0011] The present disclosure (6) relates to the paint filler according to any one of the present disclosures (1) to (5), in which the content of the glass fibers is 30 mass % or more.

[0012] The present disclosure (7) relates to the paint filler according to any one of the present disclosures (1) to (6), in which the glass fibers are pulverized glass fibers.

[0013] The present disclosure (8) also relates to a coating composition comprising the coating filler according to any one of the present disclosures (1) to (7) and a coating film-forming resin.

[0014] The present disclosure (9) further relates to a coating composition according to the present disclosure (8) comprising a medium.

[0015] The present disclosure (10) relates to a method for producing a coating composition, comprising a step of mixing, in a medium, a coating film-forming resin and a paint filler according to any one of the present disclosures (1) to (7).

[0016] The present disclosure (11) also relates to a coating film formed from the coating composition according to the present disclosure (8) or (9).

[0017] The present disclosure (12) also relates to an article having the coating film according to the present disclosure (11).

[0018] The present disclosure (13) also relates to a method for producing an article having a coating film, comprising the steps of: mixing, in a medium, a coating film-forming resin and a paint filler according to any one of the present disclosures (1) to (7) to form a coating composition; applying the coating composition to an article; and drying the applied coating composition and removing the medium to obtain a coating film. Effect of the Invention

[0019] According to the paint filler of the present disclosure, the filler contains glass fibers, and the glass fibers have a flat cross-sectional shape in a cross section perpendicular to the longitudinal direction, and the median fiber length of the glass fibers as measured by the Coulter Counter method is 0.025 mm to 0.24 mm. Therefore, it is possible to provide a paint filler that can improve hardness while suppressing deterioration in the appearance and gloss of a coating film, a coating composition using the paint filler, a method for producing the coating composition, a coating film formed from the coating composition, an article having the coating film, and a method for producing an article having a coating film. [Brief description of the drawings]

[0020] [Figure 1] Fig. 1(a) is an example of an electron microscope photograph of a normal glass fiber, and Fig. 1(b) is an example of an electron microscope photograph of a flat glass fiber. [Diagram 2] Fig. 2(a) is an example of an electron microscope photograph and a schematic diagram of normal glass fibers in a coating film, and Fig. 2(b) is an example of an electron microscope photograph and a schematic diagram of flat glass fibers in a coating film. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a rectangle circumscribing a fiber cross section. [Figure 4] FIG. 4 is a diagram showing the relationship between the median fiber length and the gloss level as measured by the Coulter Counter method in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present disclosure will be described in detail below, but the following description of the constituent elements is an example of an embodiment of the present disclosure, and the present disclosure is not limited to these specific contents. Various modifications can be made within the scope of the gist of the disclosure.

[0022] The paint filler of the present disclosure is a paint filler, the filler containing glass fibers, the cross-sectional shape of the glass fibers perpendicular to the longitudinal direction being flat, and the median fiber length of the glass fibers as measured by the Coulter Counter method being 0.025 mm to 0.24 mm. This makes it possible to provide a paint filler that can improve hardness (coating strength) while suppressing deterioration in the appearance (surface smoothness) and gloss of a coating film, a coating composition using the paint filler, a method for producing the coating composition, a coating film formed from the coating composition, an article having the coating film, and a method for producing an article having the coating film.

[0023] The reason why the above-mentioned effect is obtained is not entirely clear, but it is presumed to be due to the following mechanism. As described above, glass fibers having a circular cross-sectional shape in a cross section perpendicular to the longitudinal direction (normal glass fibers) are usually used (see FIG. 1(a)). On the other hand, in the present disclosure, glass fibers having a flat cross-sectional shape in a cross section perpendicular to the longitudinal direction (flat glass fibers) are used instead of normal glass fibers (see FIG. 1(b)). Furthermore, the median fiber length of the flat glass fibers used is within a specific range as measured by the Coulter Counter method. When ordinary glass fibers are used as a paint filler, when the paint is dried to form a coating, the ordinary glass fibers 10 in the coating film 1 tend to overlap each other while facing in various directions due to their cross-sectional shape, as shown in Figure 2(a), and therefore the ordinary glass fibers 10 tend to be exposed on the surface of the coating film, which can reduce the appearance and gloss of the coating film. On the other hand, when flat glass fibers having a specific range of median fiber length by the Coulter Counter method are used as a paint filler as in the present disclosure, when the paint is dried to form a coating film, the flat glass fibers 20 in the coating film 1 tend to pile up in a state where they are arranged in a relatively similar direction due to their cross-sectional shape when applied, as shown in Fig. 2(b), and the flat glass fibers contained in the coating film 1, whose long axes are not parallel to the surface of the coating film 1, tend to become parallel to the surface of the coating film 1 due to the surface tension and gravity of the paint (leveling) after application, so that the flat glass fibers 20 are unlikely to be exposed on the coating film surface, and the coating film surface tends to become smooth, and the hardness can be improved while suppressing the deterioration of the appearance and glossiness of the coating film. In this way, in the present disclosure, the "appearance and glossiness of the coating film" and the "hardness of the coating film", which are in a trade-off relationship, can be achieved at the same time. It is said that when flat glass fibers are mixed as a reinforcing material into a thermoplastic resin and then injection molded, a molded product without surface irregularities or roughness can be obtained. This is because the fluid dynamic effect of the shape increases the fluidity of the thermoplastic resin in the injection molding machine, and at the same time, the flat surface of the flat glass fibers flows along the mold, and the flat surface of the flat glass fibers is aligned (oriented) with respect to the surface that contacts the mold, so that the glass fibers near the surface are buried (hidden) in the resin and tend to harden as is, and the action and function are different from the mechanism presumed in the present disclosure. Therefore, it is considered that the preferred shape and fiber length of the glass fibers are different between the case where the flat glass fibers are heated to a high temperature and mixed into a fluid thermoplastic resin, and are oriented in an injection molding machine that flows at high pressure and high speed, and the case where the flat glass fibers are mixed into a fluid paint at room temperature and slowly leveled at normal pressure. In addition, it is considered that the preferred shape and fiber length of the glass fibers are different between the thermoplastic resin molded by injection molding, which places more importance on strength, and the paint, which places more importance on appearance and glossiness.

[0024] <Paint filler> The paint filler of the present disclosure contains glass fibers, the cross-sectional shape of the glass fibers being perpendicular to the longitudinal direction is flat, and the median fiber length of the glass fibers, as measured by the Coulter Counter method, is 0.025 mm to 0.24 mm.

[0025] In this specification, paint refers to a material that is applied to the surface of an article. In this specification, paint filler means a filler used in paint, preferably a filler that can be used in paint to improve the hardness, elastic modulus and / or tactile feel of the coating film formed by the paint. In this specification, glass fiber means a fibrous glass material.

[0026] In this specification, the flat shape means that when a rectangle with all interior angles of 90° is circumscribed on a plane, the rectangle is not a square but a rectangle with long and short sides. Therefore, in this specification, when the cross-sectional shape of a cross section perpendicular to the longitudinal direction is a flat shape, it means that when a rectangle with all interior angles of 90° is circumscribed on a cross section perpendicular to the longitudinal direction, the rectangle is not a square but a rectangle with long and short sides. In the following, a cross section that is a flat shape is also referred to as a flat cross section.

[0027] In this specification, the long axis of a flat cross section means the central axis parallel to the long side of a rectangle circumscribing the cross section, and the short axis of a flat cross section means the central axis parallel to the short side of a rectangle circumscribing the cross section. In this specification, the length of the long axis of the flat cross section means the length of the long side of the rectangle circumscribing the cross section, and the length of the short axis of the flat cross section means the length of the short side of the rectangle circumscribing the cross section. For example, in Fig. 3, the length of the long side of the rectangle 22 circumscribing the fiber cross section 21 is represented by L, the length of the short side is represented by S, the length of the long axis of the fiber cross section 21 is represented by L, and the length of the short axis of the fiber cross section 21 is represented by S.

[0028] In this specification, the longitudinal direction means the length direction of the glass fiber, for example, the direction into the paper in Fig. 3. Therefore, in this specification, the cross section perpendicular to the longitudinal direction means the cross section perpendicular to the length direction of the glass fiber. In this specification, the fiber length of a glass fiber means the length of the glass fiber in the longitudinal direction. In this specification, the cross-sectional shape of a cross section perpendicular to the longitudinal direction of a glass fiber means the shape of a surface cut perpendicular to the longitudinal direction of the glass fiber.

[0029] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass."

[0030] In the present disclosure, since the structure of the glass fiber, such as its shape, is important, the composition of the glass fiber is not particularly limited. Examples of the composition of the glass fiber include E glass (composition SiO 2 52~56% by mass, Al 2 O 3 12-16% by mass, CaO 15-25% by mass, MgO 0-6% by mass, B 2 O 3 5~13% by mass, Na 2 O+K 2 O 0-2% by mass), C glass (composition SiO 2 64~68% by mass, Al 2 O 3 3~5% by mass, CaO 11~15% by mass, MgO 2~4% by mass, B 2 O 3 4~6% by mass, Na 2 O+K 2 O 7-10% by mass), S-glass, D-glass, ECR-glass, A-glass, AR-glass, etc. are included. Among them, E-glass composition is preferable. E-glass is preferable because it has a composition with a small amount of alkaline components in the glass, so that alkali elution is unlikely to occur and it has little effect on the coating film formed by the coating composition. In addition, C-glass is an acid-resistant composition, and is preferable when acid resistance is particularly desired for the coating material.

[0031] The flat shape is not particularly limited, and examples thereof include a rectangle formed by joining flat portions to each other, an oval formed by joining an arc portion to a flat portion, a gourd shape, an ellipse, a trapezoid, a dumbbell shape, a triangle, etc. Among these, a rectangle and an oval having a flat portion in a part of the shape are more preferable.

[0032] The median fiber length (D50) of the glass fibers as measured by the Coulter Counter method is 0.025 mm to 0.24 mm, preferably 0.025 mm to 0.20 mm, and more preferably 0.030 mm to 0.10 mm, whereby the effect can be more suitably obtained. In the measurement of particle size distribution by the Coulter counter method, the volume change is calculated from the electrical resistance that changes when particles in an electrolyte solution pass through a fine hole, and the particle size distribution is measured. When the measured particles are fibers as in the present disclosure, the fiber length is calculated by dividing the calculated volume by the fiber cross-sectional area. Since the calculation result is not affected by the cross-sectional shape, comparison based on the fiber length is possible. Note that, since it may be difficult to measure the fiber cross-sectional area after crushing, it is preferable to measure the fiber cross-sectional area before crushing. In this specification, the median fiber length as determined by the Coulter Counter method refers to a value that is in the middle when fiber lengths are arranged in ascending order in a volume-based cumulative distribution, in other words, a fiber length at which, when a fiber length distribution is divided into two parts with a certain fiber length as a boundary, the amount of fibers belonging to a group having a fiber length shorter than the certain fiber length is equal to the amount of fibers belonging to a group having a fiber length longer than the certain fiber length, and is a value measured by the method described in the Examples.

[0033] The average flattening of the cross-sectional shape of the glass fiber in a cross section perpendicular to the longitudinal direction is preferably 2.0 to 8.0, more preferably 3.0 to 6.0, and more preferably 3.5 to 5.0, whereby the effect can be more suitably obtained. Here, the flattening ratio is calculated by dividing the length of the long axis by the length of the short axis, and the average flattening ratio is the average value of the flattening ratios. In this specification, the average flattening ratio of the cross-sectional shape of a cross section perpendicular to the longitudinal direction is synonymous with the average flattening ratio of a cross section perpendicular to the longitudinal direction, and is also synonymous with other similar descriptions such as the average circular equivalent fiber diameter unless otherwise specified. In this specification, the average value is an average value based on the number of pieces, unless otherwise specified.

[0034] The coefficient of variation of the flatness of the cross-sectional shape of the cross-section perpendicular to the longitudinal direction of the glass fiber is preferably 20% or less, more preferably 15% or less, and even more preferably 12% or less, and the smaller the better, so there is no particular lower limit. This allows the effect to be more suitably obtained. In this specification, the coefficient of variation of the flattening is a ratio of the standard deviation of the flattening to the average value of the flattening, expressed as a percentage.

[0035] The average length of the minor axis of the cross section perpendicular to the longitudinal direction of the glass fiber is preferably 0.0025 mm to 0.013 mm, and more preferably 0.0055 mm to 0.010 mm, whereby the effect can be more suitably obtained.

[0036] The average length of the major axis of the cross section perpendicular to the longitudinal direction of the glass fiber is preferably 0.0050 mm to 0.074 mm, and more preferably 0.015 mm to 0.044 mm, whereby the effect can be more suitably obtained. In this specification, the average minor axis length is the average value of the minor axis lengths, and the average major axis length is the average value of the major axis lengths.

[0037] The average circular fiber diameter of the cross section perpendicular to the longitudinal direction of the glass fibers is preferably 0.0045 mm to 0.034 mm, more preferably 0.0050 mm to 0.024 mm, and even more preferably 0.013 mm to 0.018 mm, whereby the effect can be more suitably obtained. Here, the circular equivalent fiber diameter is the diameter of a fiber calculated based on the cross-sectional area when the cross-sectional shape is assumed to be a circle, and the average circular equivalent fiber diameter is the average value of the circular equivalent fiber diameters.

[0038] The coefficient of variation of the equivalent circular fiber diameter of the cross section perpendicular to the longitudinal direction of the glass fiber is preferably 10% or less, more preferably 8.0% or less, and the smaller the better, so there is no particular lower limit. This allows the effect to be more suitably obtained. In this specification, the coefficient of variation of the equivalent circular fiber diameter is the ratio of the standard deviation of the equivalent circular fiber diameter to the average value of the equivalent circular fiber diameter, expressed as a percentage.

[0039] The cross-sectional shape characteristics such as the flattening ratio, the minor axis length, the major axis length, and the circular equivalent fiber diameter of the cross section perpendicular to the longitudinal direction of the glass fiber are measured as follows. First, the glass fibers are embedded in resin (embedded in resin). Next, the resin with the embedded glass fibers is cut using a device capable of cutting resin. Here, the cut surface is polished. Then, the resin surface is observed, and fibers whose cut surface and the longitudinal direction of the glass fibers are perpendicular to each other are identified. The cut surface of the identified fiber corresponds to a cross section perpendicular to the longitudinal direction of the glass fibers. The above-mentioned characteristics are measured for the cross section perpendicular to the longitudinal direction of the glass fibers thus identified. Specifically, the above-mentioned characteristics are measured by the method described in the examples. When glass fibers are used as a paint and are present in the coating film, the coating film may be used for the measurement instead of the resin in which the glass fibers are embedded.

[0040] Next, a method for producing the glass fiber used in the present disclosure will be described. If the shape, fiber length, etc. of the glass fiber are determined, a person skilled in the art can easily produce the glass fiber by a known method or the like.

[0041] The manufacturing process for flat glass fibers is basically the same as that for normal glass fibers, but in order to make the cross section flat, a bushing for glass fiber manufacturing (hereinafter also referred to as a nozzle plate) with an array of multiple nozzles having a special structure is required to draw out the molten glass as glass fibers.

[0042] For example, International Publication No. 99 / 028543, Japanese Patent Application Publication No. 2003-048742, and Japanese Patent Application Publication No. 2010-163342 disclose a nozzle for producing glass fibers having a flat cross section, the nozzle tip having a notch at the tip of the long side wall of the nozzle wall consisting of a long side wall and a short side wall, and a nozzle plate in which a plurality of such nozzle tips are arranged. In order to produce glass fibers having a flat cross section, it is necessary to draw out and discharge the molten glass from a nozzle having a flat cross section at the end for discharging the molten glass, and to rapidly cool the molten glass to form the glass fiber. When forming the molten glass into a fiber, the surface tension of the molten glass is high and the molten glass tends to become round, so countering this is a key point in producing glass fibers having a flat cross section.

[0043] In order to mass-produce glass fibers, it is effective to use a bushing equipped with many nozzles on a base plate. In a bushing equipped with many nozzles, the area of ​​the base plate needs to be large. If the area of ​​the base plate is large, temperature unevenness is likely to occur in the base plate, which may cause variations in the flattening ratio and cross-sectional area of ​​the glass fiber, and thus the cross-sectional shape of the glass fiber may vary. The reason for this is that if temperature unevenness occurs in the base plate, the viscosity of the molten glass passing through the inside of each nozzle is different, so that the magnitude of the force that opposes the force (surface tension) that makes the glass round at the nozzle outlet is different, and thus the flattening ratio of the obtained glass fiber is thought to vary. Furthermore, the flow of the molten glass is likely to pulsate in a nozzle with a relatively low temperature, which is likely to cause problems such as glass fibers not having a uniform cross-sectional shape being obtained.

[0044] Furthermore, when the area of ​​the base plate is large, if the drawn molten glass is spun so as to converge at the center of the base plate, the angle of the molten glass drawn from each nozzle (hereinafter also referred to as the pulling angle of the glass fiber) differs between the nozzles at the center and the nozzles at the ends of the base plate, which causes variations in the flattening and cross-sectional area of ​​the glass fiber, and may result in large variations in the cross-sectional shape of the glass fiber.

[0045] With the nozzle shapes disclosed in WO 99 / 028543, JP 2003-048742 A, and JP 2010-163342 A, glass fibers with a flat cross-section can be produced, but there is a risk that the flattening ratio and cross-sectional area of ​​the glass fibers will vary due to the temperature unevenness of the base plate described above and differences in the pulling angle of the glass fibers, resulting in large variation in the cross-sectional shape of the glass fibers.

[0046] In contrast, a bushing for producing glass fibers as disclosed in WO 2020 / 040033, specifically, a bushing for producing glass fibers comprising a base plate and a plurality of nozzles arranged on the base plate for discharging molten glass, wherein the base plate has a base hole having a flat horizontal cross section, and the nozzle has a nozzle wall protruding from the base plate along the contour of the base hole, and a nozzle hole penetrating from the base hole toward the tip of the nozzle wall while maintaining the shape of the base hole, and the nozzle wall is By manufacturing glass fibers using a bushing for manufacturing glass fibers, which has a pair of notches that do not protrude from the base plate, the pair of notches facing each other via the central axis in the longitudinal direction of the nozzle hole, and the width of the notches is 10% or more and 95% or less of the length of the central axis in the longitudinal direction of the nozzle hole, it is possible to reduce the variation in the cross-sectional shape of the glass fiber caused by the temperature unevenness of the base plate and the difference in the pulling angle of the glass fiber, and it is possible to manufacture glass fibers having a flat cross section and small variation in the cross-sectional shape. This makes it possible to suitably manufacture flat glass fibers having a small coefficient of variation in the flatness of the cross-sectional shape and a small coefficient of variation in the circular equivalent fiber diameter of the cross-sectional shape. The size of the cross section of the glass fiber is appropriately designed depending on the size of the base hole and the nozzle hole, the temperature of the glass melt and the nozzle, and the pulling speed of the winder, etc.

[0047] In the present disclosure, since the median fiber length of the glass fiber measured by the Coulter Counter method is 0.025 mm to 0.24 mm, the glass fiber produced by the bushing for producing glass fiber must usually be pulverized to form milled fiber (MF). Thus, the glass fiber is preferably a pulverized product of glass fiber.

[0048] The method of producing MF by pulverizing glass fibers is not particularly limited, and may be produced by a known method. For example, known pulverizing means such as a ball mill, a planetary ball mill, a hammer mill, a jet mill, a cutter mill, etc. may be selected according to the desired fiber length. In addition, the pulverization does not change the cross-sectional shape of the glass fibers, and the cross-sectional shape of the glass fibers when spun is maintained as it is.

[0049] The glass fiber may be a glass fiber bundle. The glass fiber may be coated with a sizing agent or may be surface-treated. The sizing agent is not particularly limited, and known treatment agents including silane coupling agents, resin emulsions, surfactants, acidic and alkaline components, etc. may be used. The surface treatment is not particularly limited, and examples thereof include treatment with a silane coupling agent, treatment with a surfactant or chemicals, plating treatment, etc. These may be used alone or in combination of two or more.

[0050] The content of the glass fiber in the paint filler of the present disclosure is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and may be 100% by mass, whereby the effect can be more suitably obtained. In this specification, the content ratio of the glass fiber in the paint filler of the present disclosure means the content ratio of the glass fiber in 100 mass% of the paint filler of the present disclosure, and the same applies to other similar descriptions.

[0051] The paint filler of the present disclosure is a filler containing the glass fiber, but may contain other components other than the glass fiber. The other components are not particularly limited, and examples thereof include glass fibers other than the glass fibers, such as ordinary glass fibers, processing aids, etc. These may be used alone or in combination of two or more.

[0052] The paint filler of the present disclosure is suitable for use in paints because it can improve hardness while suppressing deterioration in the appearance and gloss of the coating film.

[0053] <Paint composition> The coating composition of the present disclosure contains the coating filler of the present disclosure and a coating film-forming resin, which may be used alone or in combination of two or more kinds.

[0054] In the coating composition of the present disclosure, the content of the coating filler of the present disclosure is preferably 1 to 30 mass%, more preferably 2 to 20 mass%, and even more preferably 5 to 17 mass%, whereby the effects can be more suitably obtained.

[0055] The film-forming resin is not particularly limited as long as it is a resin capable of forming a film, and examples thereof include thermoplastic resins, thermosetting resins, photocurable resins, moisture-curable resins, and electron beam-curable resins. These may be used alone or in combination of two or more. Specific examples of the film-forming resin are not particularly limited, and examples thereof include acrylic resins and modified products thereof (such as silicone-modified acrylic resins); urethane resins and modified products thereof (ester-based urethane resins; ether-based urethane resins; carbonate-based urethane resins; epoxy-based urethane resins); acrylic urethane resins; polyester resins and modified products thereof (urethane-modified polyester resins; epoxy-modified polyester resins; silicone-modified polyester resins); polyamide resins; melamine resins; phenolic resins and modified products thereof (acrylic-modified phenolic resins; epoxy-modified phenolic resins); alkyd resins; epoxy resins; vinyl chloride resins; vinyl ester resins; fluororesins; silicone resins; acrylic silicone resins; phenoxy resins; alkyd resins and modified products thereof (urethane-modified alkyd resins, acrylic-modified alkyd resins, etc.); and the like. In this specification, the term "acrylic resin" refers to a resin whose main component is acrylic, and the same applies to other resins.

[0056] The coating resin can be selected from the above-mentioned resins or one or more other resins according to the desired characteristics and applications. For example, acrylic resins, acrylic urethane resins, and urethane resins are suitable for coating applications that require aesthetics, and epoxy resins and acrylic resins are suitable for applications that require strength to prevent peeling. For applications that require weather resistance and chemical resistance, fluororesins can be used. Among these, fluororesins and silicone resins are preferred, and fluororesins are more preferred.

[0057] In the coating composition of the present disclosure, the content of the film-forming resin is preferably 1 to 85% by mass, and more preferably 20 to 60% by mass, whereby the effect can be more suitably obtained.

[0058] The coating composition of the present disclosure preferably contains, in addition to the coating filler of the present disclosure and the film-forming resin, a crosslinking agent capable of reacting with the film-forming resin to form a cured coating film.

[0059] The crosslinking agent is not particularly limited as long as it can react with the coating film-forming resin to form a cured coating film, and examples thereof include polyisocyanate compounds, blocked polyisocyanate compounds in which the isocyanate groups of polyisocyanate compounds are blocked with active hydrogen-containing compounds, amino resins such as urea resins, etc. These may be used alone or in combination of two or more kinds.

[0060] The content (solid content) of the crosslinking agent is preferably 5 to 70 parts by mass, more preferably 10 to 30 parts by mass, per 100 parts by mass of the resin solid content of the coating film-forming resin, which allows the crosslinking reaction between the coating film-forming resin and the crosslinking agent to proceed smoothly, and tends to improve the appearance of the resulting coating film.

[0061] The coating composition of the present disclosure may be colored by including a colorant such as a pigment or dye in addition to the coating filler of the present disclosure and the coating film-forming resin. The present disclosure believes that the coating filler of the present disclosure has a higher gloss when the coating composition or the coating film formed by the coating composition is dark in color, and particularly when the coating film is black, the gloss is even higher. Therefore, the present disclosure believes that the coating composition of the present disclosure preferably includes a colorant that exhibits a dark color, and more preferably includes a colorant that exhibits a black color, in addition to the coating filler of the present disclosure and the coating film-forming resin. In this specification, a dark color is a color with a brightness of 5 or less in the Munsell color system, and each color has a low degree of brightness and a dark feeling, and is not limited to a specific color. Specific examples of dark colors include black, brown, dark brown, navy blue, and dark gray.

[0062] The colorant is not particularly limited, and examples thereof include color pigments, color dyes, etc. These may be used alone or in combination of two or more kinds.

[0063] The color pigment is not particularly limited, and examples thereof include color inorganic pigments such as titanium dioxide, carbon black, graphite, iron oxide, and coal dust; color organic pigments such as phthalocyanine blue, phthalocyanine green, quinacridone, perylene, anthrapyrimidine, carbazole violet, anthrapyridine, azo orange, flavanthrone yellow, isoindoline yellow, azo yellow, industhrone blue, dibromoanthathrone red, perylene red, azo red, and anthraquinone red; aluminum powder, alumina powder, bronze powder, copper powder, tin powder, zinc powder, iron phosphide, and fine titanium powder. Of these, carbon black is preferred.

[0064] The coloring dye is not particularly limited, and examples thereof include monoazo-based, disazo-based, metal complex monoazo-based, anthraquinone-based, methine-based, phthalocyanine-based, and triarylmethane-based dyes.

[0065] In the coating composition of the present disclosure, the content of the colorant is preferably 0.01 to 30% by mass, and more preferably 0.1 to 10% by mass, whereby the effect can be more suitably obtained.

[0066] The coating composition of the present disclosure is not particularly limited, and any of water-based coatings containing water as a medium, organic solvent-based coatings containing an organic solvent as a medium, and solvent-free coatings containing no medium can be used, but it is preferable that the coating composition is a composition in which the film-forming resin is dispersed and / or dissolved in a medium. That is, the coating composition of the present disclosure preferably further contains a medium in addition to the paint filler and film-forming resin of the present disclosure. This improves the applicability to the substrate, and furthermore, the flat glass fiber is more likely to level during the process of drying and hardening after application, which tends to improve the appearance of the resulting coating film.

[0067] The medium is not particularly limited, and examples thereof include water; glycol-based organic solvents such as ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol monobutyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate; alcohol-based organic solvents such as methanol, ethanol, isopropyl alcohol, and Solfit (manufactured by Kuraray); ether-based organic solvents such as dioxane and tetrahydrofuran; ester-based organic solvents such as 3-methoxybutyl acetate, ethyl acetate, isopropyl acetate, and butyl acetate; ketone-based organic solvents such as methyl ethyl ketone, acetone, methyl isobutyl ketone, cyclohexanone, and isophorone; toluene, xylene, pentane, iso-pentane, hexane, iso-hexane, cyclohexane, solvent naphtha, mineral spirits, T-SOL 100, T-SOL 150 (all aromatic hydrocarbon solvents, manufactured by JXTG Energy Corporation); as well as N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, etc. These may be used alone or in combination of two or more. Among them, water, glycol organic solvents, alcohol organic solvents, ester organic solvents, and hydrocarbon organic solvents are preferred.

[0068] Examples of solvent-free paints include powder paints and liquid resin paints. Powder paints are powdered paint compositions containing film-forming resins, and are divided into thermoplastic resins and thermosetting resins. In the case of thermoplastic resins, a coating film can be formed by attaching the resin to a coating object, heating and melting the resin, and then cooling and solidifying the resin. Liquid resin paints are coating compositions containing liquid film-forming resins, and examples of such coatings include ultraviolet-curing paints. In the case of ultraviolet-curing paints, a coating film can be formed by photopolymerization reaction by applying ultraviolet light to a coating object after application.

[0069] When the coating composition of the present disclosure contains a medium, the content of the medium in the coating composition is preferably 10 to 70% by mass, more preferably 20 to 65% by mass. When the coating composition contains a medium, the content of the film-forming resin in the coating composition is preferably 10 to 80% by mass, more preferably 25 to 75% by mass, and the content of the paint filler in the coating composition is preferably 1 to 30% by mass, more preferably 2 to 20% by mass, and even more preferably 5 to 17% by mass. This allows the effect to be more suitably obtained.

[0070] The coating composition of the present disclosure may further contain other additives in addition to the above components. The other additives are not particularly limited, and examples thereof include surface conditioners, extender pigments, waxes, heat-shielding pigments, luster pigments, ultraviolet absorbers (benzophenone-based ultraviolet absorbers, etc.), antioxidants (phenol-based, sulfoid-based, hindered amine-based antioxidants, etc.), plasticizers, coupling agents (silane-based, titanium-based, zirconium-based coupling agents, etc.), anti-sagging agents, thickeners, pigment dispersants, pigment wetting agents, leveling agents, color separation inhibitors, precipitation inhibitors, antifoaming agents, antifreezing agents, emulsifiers, preservatives, fungicides, antibacterial agents, stabilizers, etc. These may be used alone or in combination of two or more.

[0071] The method for producing the coating composition of the present disclosure is not particularly limited. For example, the coating composition can be prepared by selecting and using a mixer, disperser, kneader, etc., such as a sand grind mill, a ball mill, a blender, a paint shaker, or a disperser, and mixing each component. The method for producing the coating composition of the present disclosure preferably includes a step of mixing the coating film-forming resin and the coating filler of the present disclosure in a medium. This improves the applicability to the substrate, and further, the flat glass fiber is more likely to level during the process of drying and hardening after coating, which tends to improve the appearance of the resulting coating film.

[0072] <Coating film> The coating film of the present disclosure is a coating film formed by the coating composition of the present disclosure. The thickness of the coating film is not particularly limited, and is, for example, 0.020 to 0.10 mm. The coating film of the present disclosure is preferably a topcoat coating film (protective coating film, outermost coating film) because the hardness is improved while suppressing the deterioration of the appearance and gloss of the coating film. Of course, the coating film of the present disclosure has excellent surface smoothness, so it may be used as an intermediate coating paint or an undercoat paint for the purpose of smoothing the surface of the coated object.

[0073] The coating method of the coating composition of the present disclosure is not particularly limited, and examples thereof include spray coating, roller coating, brush coating, trowel coating, spatula coating, electrostatic coating, immersion, electrodeposition coating, curtain coating, shower coat coating, and roll coater coating. These may be used alone or in combination of two or more. By these methods, the coating composition of the present disclosure can be applied to a substrate to be coated and dried to form a coating film.

[0074] The substrate to be coated with the coating composition of the present disclosure is not particularly limited, and examples thereof include metal substrates such as steel, galvanized steel (e.g., galvanized iron sheet), tin-plated steel (e.g., tin plate), stainless steel, magnesium alloy, aluminum, and aluminum alloy; inorganic substrates such as gypsum, calcium silicate, glass, ceramic, concrete, cement, mortar, and slate; plastic substrates such as acrylic resin, polyvinyl chloride resin, polycarbonate resin, acrylonitrile-butadiene-styrene (ABS) resin, polyethylene terephthalate resin, and polyolefin resin; fiber substrates such as paper and cloth; and wood. In addition, composite substrates such as wood fiber reinforced cement board, fiber reinforced cement board, and fiber reinforced cement-calcium silicate board can also be exemplified. Metal substrates include substrates that have been subjected to various surface treatments, such as oxidation treatment. Plastic substrates whose surfaces are coated with inorganic substances (e.g., plastic substrates coated with glass) are included in inorganic substrates. The substrate may have a surface treatment such as degreasing with a detergent or solvent, phosphate treatment, chromate treatment, composite oxide treatment, cleaning, polishing, etc., and may further have an undercoat coating film formed thereon. An old coating film (a coating film already formed) may be present on at least a part of the substrate surface. Among these, metal substrates are preferred.

[0075] As described above, examples of objects to be painted include substrates made of various materials. Specific examples of objects to be painted include, but are not limited to, structures such as buildings and structures, vehicles, furniture, fixtures, electronic devices, ships, road surfaces, and parts thereof. In this specification, a building refers to a structure constructed for the purpose of human habitation or stay, such as a house (particularly a detached house or an apartment building), a building, or a factory, and a structure refers to a structure constructed for purposes other than human habitation or stay, such as a bridge, a tank, a plant piping, or a chimney. Furthermore, the members of the structure are not particularly limited, and examples thereof include roofs and walls (inner walls, outer walls, and the like, particularly curtain walls). Furthermore, the vehicles are not particularly limited, and examples thereof include passenger cars, trucks, motorcycles, buses, and the like. Furthermore, the electronic devices are not particularly limited, and examples thereof include home appliances such as mobile phones and audio equipment.

[0076] <Goods> The article of the present disclosure has a coating of the present disclosure. The article of the present disclosure is a coated article having a coating film formed by the coating composition of the present disclosure, and is preferably a coated article having the coating film on the surface of a substrate. Here, the thickness of the coating film is not particularly limited, and is, for example, 0.020 to 0.10 mm.

[0077] In the article of the present disclosure, the details of the substrate are as described in the coating film of the present disclosure. The article of the present disclosure is not particularly limited, and examples thereof include those having a coating film on the surface of an article such as those described as the object to be painted in the coating film of the present disclosure.

[0078] <Method of manufacturing an article having a coating film> A method for producing an article having a coating film of the present disclosure includes the steps of mixing a film-forming resin and a coating filler of the present disclosure in a medium to form a coating composition; applying the coating composition to an article; and drying the applied coating composition to remove the medium to obtain a coating film.

[0079] The process of mixing the film-forming resin and the paint filler of the present disclosure in a medium to form a paint composition is as described in the <Paint Composition> section. The process for applying the coating composition to an article is as described in the <Coating> section. The step of drying the applied coating composition and removing the medium to obtain a coating film is as described in the <Coating Film> section, and the drying method is not particularly limited. The method for producing an article having a coating film according to the present disclosure may also include other steps in addition to those described above. EXAMPLES

[0080] EXAMPLES Hereinafter, examples will be given that more specifically disclose embodiments of the present disclosure, but the present disclosure is not limited to these examples.

[0081] The glass fibers obtained in each production example were evaluated by the following methods.

[0082] (Measurement of median fiber length (D50) of glass fibers using the Coulter Counter method) Here, we measure glass fibers that are added to paint and crushed using the method described in the manufacturing example. The measurement device used was a precision particle size distribution measurement device using the electrical detection zone method (Multisizer3, Beckman Coulter, manufactured in 2007). The sample solution was prepared by adding glass fibers to an electrolyte solution and mixing with a medicine spoon to thoroughly disperse the glass fibers. A beaker containing the electrolyte solution was placed on the sample stand, and the sample solution was dropped into it using a pipette to perform the measurement. From the obtained cumulative distribution based on volume, the volume was divided by the cross-sectional area of ​​the fiber to calculate the median fiber length (D50).

[0083] (Preparation of samples for cross-sectional observation) Since the cross section perpendicular to the longitudinal direction of the glass fibers does not change before and after crushing, the evaluation was performed using the fibers before crushing. First, a glass fiber bundle in which multiple glass fibers were bundled was aligned in one direction and embedded in resin, and hardened by heating or the like (embedded in resin). Next, the resin in which the glass fibers were embedded was cut at a plane perpendicular to the longitudinal direction of the aligned glass fibers using a device capable of cutting resin, and the cut surface was polished and ground.

[0084] Next, a cross section perpendicular to the longitudinal direction of the glass fiber was observed by a scanning electron microscope, and each characteristic was measured. (Measurement of the length of the long axis and the length of the short axis) The length of the major axis and the length of the minor axis of the cross-sectional shape of the cross section perpendicular to the longitudinal direction of the glass fiber were measured. (Calculation of the above aspect ratio) Based on the measurement results of the major axis length and the minor axis length, the flattening of the cross-sectional shape of the cross section perpendicular to the longitudinal direction of the glass fiber was calculated by dividing the major axis length by the minor axis length. (Calculation of the circular equivalent fiber diameter) The cross-sectional shape of the glass fiber perpendicular to the longitudinal direction is assumed to be two semicircles with the diameter equal to the length of the short axis, and a rectangle between the two semicircles with the length of the long axis minus the radius of the two semicircles as its horizontal axis and the length of the short axis as its vertical axis. Then, the area of ​​the cross-sectional shape of the cross section perpendicular to the longitudinal direction of the glass fiber is: Based on the measurement results of the major axis length and the minor axis length, it is calculated by the following formula (1). (S / 2)^2×π+((LS)×S) (1) Then, based on the calculated area of ​​the cross-sectional shape, a circular equivalent fiber diameter, which is the diameter of the fiber when the cross-sectional shape is assumed to be a circle, was calculated to calculate the circular equivalent fiber diameter of the cross-sectional shape of the cross section perpendicular to the longitudinal direction of the glass fiber. (Calculation of average value and coefficient of variation) The length of the long axis, the length of the short axis, the flatness, and the equivalent circular fiber diameter were measured for 50 glass fibers, and the average values ​​were calculated. The coefficients of variation of the flatness and the equivalent circular fiber diameter were also calculated.

[0085] (Production Example 1) Production of flat glass fibers A bushing for producing glass fibers, as disclosed in International Publication No. 2020 / 040033, comprising a base plate and a plurality of nozzles arranged on the base plate for discharging molten glass, wherein the base plate comprises a base hole having a flat horizontal cross section, the nozzle comprises a nozzle wall protruding from the base plate along the contour of the base hole, and a nozzle hole penetrating from the base hole to the tip of the nozzle wall while maintaining the shape of the base hole, the nozzle wall has a pair of notches that do not protrude from the base plate, the pair of notches face each other through the central axis in the longitudinal direction of the nozzle hole, and the width of the notches is 10% or more and 95% or less of the length of the central axis in the longitudinal direction of the nozzle hole. Glass fibers having a flat (oval) cross section were produced using the bushing for producing glass fibers. The obtained glass fibers were first cut to 50 mm, and then pulverized using a ball mill to obtain flat glass fibers 1 to 6 (E glass composition). The evaluation results of the flat glass fibers 1 to 6 are shown in Table 1.

[0086] (Production Example 2) Production of normal glass fiber The nozzle of the bushing for producing the glass fiber was changed to a nozzle with a circular cross section, and the rest of the process was the same as for the flat glass fiber, to obtain ordinary glass fibers 1 to 3 (E glass composition). The evaluation results of ordinary glass fibers 1 to 3 are shown in Table 2. The ordinary glass fiber had a circular cross section and a cross-sectional diameter of 0.011 mm.

[0087] (Examples and Comparative Examples) The base paint for the primer (Mighty All-Purpose Water-Based Sealer (containing water, titanium oxide, zinc oxide, etc.) manufactured by Nippon Toryo Co., Ltd.) was mixed with the accompanying hardener and left to mature for 30 minutes. The mixture was then applied with a brush to a 10cm x 10cm galvanized steel plate and allowed to dry at room temperature to form a primer coating film 0.015mm thick. Next, the glass fibers obtained in Production Examples 1 and 2 were added to the base of a weak solvent-based fluororesin paint (Sunflon UV manufactured by Rock Paint Co., Ltd. (brown paint containing fluororesin, pigment, mineral spirits, solvent naphtha, etc.) according to the composition shown in Tables 1 and 2, and mixed using a medicine spoon. Furthermore, the attached hardener was added and further mixed to prepare a brown topcoat paint. The content of the medium in the topcoat paint (the paint composition of the present disclosure) was 35 mass%. Next, the prepared topcoat paint was applied with a brush to the surface of the undercoat film formed on the galvanized steel sheet, and dried at room temperature to form a coating film with a thickness of 0.040 mm.

[0088] The resulting coating film was evaluated by the following test methods, and the results are shown in Tables 1 and 2.

[0089] (Appearance of the coating) The appearance of the coating film was visually evaluated according to the following criteria. ×: Poor (overall unevenness is strong) △: Slightly poor (some unevenness) 〇: Good ◎: Very good

[0090] (Glossiness of coating film) The specular gloss (Gs(60°)) of the coating film at 60° was measured using a HORIBA handheld gloss meter Gloss Checker IG-331 and evaluated according to the following criteria. The gloss is preferably 40 or more. ×: Glossiness 0~30 △: Glossiness 31~45 〇: Glossiness 46~60 ◎: Glossiness 61~

[0091] (Pencil hardness of coating film) The pencil hardness of the coating film was determined in accordance with JIS K 5600-5-4:1999, by judging plastic deformation under a load of 750 g, and was evaluated according to the following criteria: The pencil hardness is preferably 4B or higher. ×: Pencil hardness less than 6B △:Pencil hardness 6B~5B (improved by 1~2 steps) 〇: Pencil hardness 4B~2B (improved by 3~5 levels) ◎:Pencil hardness B~ (improved to 6 levels)

[0092] [Table 1]

[0093] [Table 2]

[0094] From Tables 1 and 2, it can be seen that the paint filler of the present disclosure, which contains glass fibers, the cross-sectional shape of the glass fibers being flat in a cross section perpendicular to the longitudinal direction, and the median fiber length of the glass fibers as measured by the Coulter Counter method being 0.025 mm to 0.24 mm, can improve hardness while suppressing deterioration in the appearance and gloss of the coating film.

[0095] Figure 4 shows a graph plotting gloss against median fiber length for the results in Tables 1 and 2. Figure 4 shows that regular glass fiber not only has a lower gloss than flat glass fiber, but also shows a large drop in gloss as the median fiber length increases, whereas flat glass fiber not only has a higher gloss than regular glass fiber, but also shows a small drop in gloss even as the median fiber length increases, meaning that gloss can be maintained over a wide range of median fiber lengths. Thus, it was found that with flat glass fiber, there is a tendency for gloss to be maintained even when the median fiber length is changed. [Explanation of symbols]

[0096] 1 Coating 10 Normal glass fiber 20 Flat glass fiber 21 Fiber cross section 22 Rectangle circumscribing the fiber cross section L Length of the long side S Length of the short side

Claims

1. A paint filler comprising: The filler includes glass fibers, The glass fiber has a flat cross-sectional shape perpendicular to the longitudinal direction, The paint filler, wherein the median fiber length of the glass fiber, as measured by the Coulter Counter method, is 0.025 mm to 0.24 mm.

2. 2. The paint filler according to claim 1, wherein the cross-sectional shape has an average flattening ratio of 2.0 to 8.0 and an average circular equivalent fiber diameter of 0.0045 mm to 0.034 mm.

3. 3. The paint filler according to claim 2, wherein the average flatness of the cross-sectional shape is 3.0 to 6.

0.

4. 3. The paint filler according to claim 1, wherein the coefficient of variation of the circular equivalent fiber diameter of the cross-sectional shape is 10% or less.

5. 3. The paint filler according to claim 1, wherein the coefficient of variation of the flatness of the cross-sectional shape is 20% or less.

6. 3. The paint filler according to claim 1, wherein the content of the glass fibers is 30% by mass or more.

7. 3. The paint filler according to claim 1, wherein the glass fiber is a ground glass fiber.

8. A coating composition comprising the coating filler according to claim 1 or 2 and a film-forming resin.

9. The coating composition of claim 8 further comprising a medium.

10. A method for producing a coating composition, comprising the step of mixing in a medium a film-forming resin and the coating filler according to claim 1 or 2.

11. A coating film formed from the coating composition according to claim 8.

12. An article having the coating of claim 11.

13. A step of mixing a film-forming resin and the paint filler according to claim 1 or 2 in a medium to form a paint composition; applying the coating composition to an article; and drying the applied coating composition to remove the medium to obtain a coating film. A method for producing an article having a coating.

Citation Information

Patent Citations

  • JP1975025485A